Shaft body for pencils or cosmetics
The use of a naturally derived extender, binder, and pigment composition for pencil and cosmetic shafts addresses environmental concerns and aesthetic challenges, offering easy cutting, drop resistance, and water resistance, while enabling customizable appearances without painting, thus improving upon conventional methods.
Patent Information
- Application Number
- PCT/JP2024/014086
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-14
- Filing Date
- 2024-04-05
- Publication Date
- 2024-10-17
AI Technical Summary
Conventional methods for producing pencil and cosmetic shafts face environmental burdens due to high energy requirements, dye waste, and difficulties in achieving desired aesthetic appearances, especially in cutting and coloring, while also struggling with the scarcity of natural wood materials like red cedar.
A shaft material composition comprising a naturally derived extender, binder, and pigment, with a natural origin index of 75% or more, is used to coat pencil leads or rod-shaped cosmetics, providing ease of cutting, drop resistance, and water resistance similar to conventional wooden shafts without the need for painting.
The solution allows for pencils and cosmetics with easy cutting, drop resistance, and water resistance, while reducing environmental impact and enabling customization of the appearance, including the cut cross-section, without painting, thus addressing the limitations of existing methods.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Pencil or cosmetic barrel
[0001] This specification relates to a pencil lead or cosmetic shaft that has the same ease of sharpening, drop resistance, and water resistance as conventional wooden shafts, has a low environmental impact, and can have any color in appearance, including the cut cross section, without painting.
[0002] Conventionally, natural wood, particularly natural wood such as American red cedar, has been used for the shafts of pencils, stick-shaped cosmetics, and the like, because it provides a pleasant feel to the user and is soft and easy to sharpen with a knife or pencil sharpener. However, in recent years, forests have been declining due to deforestation and other indiscriminate harvesting, and this situation has drawn attention to the problem of environmental destruction. As a result, red cedar and other woods have become difficult to obtain, and alternative materials have been developed. Furthermore, when coloring shafts made of the above-mentioned natural wood, the two most common methods are to impregnate the natural wood itself with a dye-containing liquid, or to apply a paint to the surface after the shaft has been formed. However, the former method requires a large amount of energy during impregnation and generates waste dye liquid, which places a heavy burden on the environment. Meanwhile, the latter method leaves the cross section of the wood that has been cut to expose the pencil lead or stick-shaped cosmetic unchanged in its normal wood color.
[0003] Conventionally, techniques for substitute materials for the shafts of pencils, stick-shaped cosmetics, etc., and techniques for coloring these shafts include, for example, the following techniques 1) to 7): 1) A method for producing a pencil shaft plate, which comprises adding caustic soda or a soluble substance with the same effect to old newspapers, pulp wood chips, sawdust, or other plant fibrous materials, boiling and dissolving the mixture in water to form a liquid, molding the resulting material into a plate, drying it, and then uniformly infiltrating one or more of cellulose acetate, stearin, lacquer, urea resin, etc., into the interior of the material, and applying appropriate pressure to form the material into a plate (see, for example, Patent Document 1);
[0004] 2) A pencil characterized in that convex and concave stripes are alternately and continuously formed along the axial direction on the rod-shaped outer peripheral surface of a core material containing a thermoplastic resin, a lubricant, and graphite or a pigment, and a shaft material containing a thermoplastic resin, cellulose fibers, and a foaming agent is formed on the outside of the core material so as to closely contact the concave and convex surfaces of the stone, and a part of the cellulose fibers in the shaft material is mixed in and bites into the concave and convex portions of the rod-shaped outer peripheral surface of the core material (see, for example, Patent Document 2).
[0005] 3) A pencil in which a lead is inserted into a pencil shaft obtained by mixing fine cellulose powder particles obtained by grinding with a resin, molding the mixture by extrusion or injection molding, and forming the molded body into the shape of a pencil shaft, in order to provide a pencil that can be sharpened without any problems and that can be manufactured inexpensively because the shaft is easy to process (see, for example, Patent Document 3).
[0006] 4) A method for producing a substantially rod-shaped composite from a core surrounded by at least one polymer obtained by plasticizing a polymer and extruding it onto a continuous core, characterized in that at least one natural polymer based on lignin is used and a slip agent based on natural oils and / or waxes is added to the plasticized polymer before or during extrusion, and further a method for adding natural fibers to the plasticized polymer before or during extrusion, which method is used to produce writing implements such as pencils or colored pencils, cosmetic pencils, composites that are coated by applying paints or the like (see, for example, Patent Document 4);
[0007] 5) A wood substitute material for a wooden-barrel pencil, comprising at least one polymer binder, at least one organic filler, at least one inorganic filler, at least one compatibilizer, at least one wax, at least one color pigment, and at least one additive, wherein the at least one compatibilizer forms a chemical bond between the at least one polymer binder and the at least one organic filler, the ratio of the at least one compatibilizer to the at least one wax is in the range of 1:2 to 1:6, and the total of the organic filler and the inorganic filler is 80% by weight or less (see, for example, Patent Document 5).
[0008] 6) A rigid fiberboard used as a pencil shaft, the fiberboard comprising fibers selected from the group consisting of natural fibers, synthetic fibers, and mixtures thereof, a binder, a filler, a lubricant, and a waterproofing agent; the natural fibers being cellulose fibers obtained from a source selected from the group consisting of wood pulp, linters, denim fibers, newspapers, cardboard boxes, kraft paper bags, bleached paper, kraft paper, cotton waste, and mixtures thereof; the binder being selected from the group consisting of thermosetting resin binders, water-soluble gums, and mixtures thereof, the water-soluble gums being selected from the group consisting of guar gum, carboxymethyl cellulose, hydroxyethyl cellulose, and mixtures thereof; the filler being an inorganic particulate material selected from the group consisting of perlite, vermiculite, glass microbubbles, and mixtures thereof; and at least one dye; a pencil comprising a marking lead and a shaft enclosing the lead, the shaft being molded from the fiberboard comprising fibers, a binder, a filler, a lubricant, and a waterproofing agent (see, for example, Patent Document 6).
[0009] 7) To provide a synthetic biodegradable pencil-shaped cosmetic barrel that can replace a wooden barrel and has excellent physical properties such as rigidity, machinability, and resistance to oil and grease penetration, as well as a good feel when used, and that is easily decomposed after disposal, can be burned with a low amount of heat, and does not generate harmful substances when incinerated, and a method for producing the same, a hollow cylindrical biodegradable pencil-shaped synthetic cosmetic barrel is known, which is molded using a biodegradable thermoplastic material as a base material that consists of a starch ester in which the hydrogen atoms of the reactive hydroxyl groups of the same starch molecule are substituted with short-chain acyl groups and long-chain acyl groups, and a reinforcing filler (see, for example, Patent Document 7).
[0010] However, in Patent Document 1, the plant fiber material needs to be dissolved by boiling, and in Patent Documents 2 to 5, thermoplastic or thermosetting resins are used, which necessitate heating during coloring, molding, or curing, and therefore the current situation is that there is still a problem of a heavy burden on the environment. Also, Patent Documents 6 and 7 use natural fibers or starch esters, but still have the problem of a heavy burden on the environment, and furthermore, the aesthetic treatment of the appearance, including the cut cross section, is still not sufficient.
[0011] Japanese Patent Publication No. 37-2728 (Claims, etc.) Japanese Patent Application Laid-Open No. 60-204399 (Claims, etc.) Japanese Patent Application Laid-Open No. 6-255296 (Claims, etc.) Japanese Patent Publication No. 2002-529273 (Claims, etc.) Japanese Patent Application Laid-Open No. 2011-528046 (Claims, etc.) Japanese Patent Application Laid-Open No. 5-96899 (Claims, etc.) Japanese Patent Application Laid-Open No. 2001-192502 (Claims, etc.)
[0012] The present disclosure seeks to solve the above-mentioned conventional problems, and aims to provide a pencil lead or cosmetic shaft or the like that has the same ease of sharpening, drop resistance, and water resistance as conventional wooden shafts, has a low environmental impact, and furthermore, the appearance, including the cut cross section, can be made any color without painting.
[0013] As a result of intensive research into the above-mentioned conventional problems, the present inventors have discovered that the above-mentioned desired pencil or cosmetic shaft can be obtained by coating a pencil lead or a stick-shaped cosmetic with a shaft material composition, and that the shaft material composition contains at least an extender with specific physical properties, a binder, and a pigment, thereby completing the present disclosure.
[0014] That is, the shaft of a pencil or cosmetic product according to the present disclosure is a shaft of a pencil or cosmetic product formed by coating a pencil lead or a stick-shaped cosmetic product with a shaft material composition, characterized in that the shaft material composition contains at least a naturally derived filler, a naturally derived binder, and a pigment. The shaft material composition preferably has a natural origin index (excluding water) of 75% or more. The pencil according to the present disclosure is a pencil comprising at least a pencil lead and a shaft formed by coating and molding the pencil lead, characterized in that the shaft has the above-described configuration. Furthermore, the stick-shaped cosmetic product according to the present disclosure is a stick-shaped cosmetic product comprising at least a stick-shaped cosmetic product and a shaft formed by coating and molding the stick-shaped cosmetic product, characterized in that the shaft has the above-described configuration.
[0015] According to the present disclosure, it is possible to provide a pencil lead or cosmetic barrel that has the same ease of sharpening, drop resistance, and water resistance as conventional wooden barrels, is environmentally friendly, and allows the appearance, including the cut cross section, to be any color without painting, as well as a pencil, stick-shaped cosmetic, etc., equipped with this barrel. The objects and advantages of the present disclosure will be realized and attained by use of the elements and combinations particularly pointed out in the claims. Both the foregoing general description and the following detailed description are exemplary and explanatory and do not limit the present disclosure, which is set forth in the claims.
[0016] The following describes in detail the embodiments of the present disclosure. However, please note that the technical scope of the present disclosure is not limited to the embodiments described in detail below, but extends to the inventions set forth in the claims and their equivalents. Furthermore, the present disclosure can be implemented based on the contents disclosed in this specification and common general technical knowledge in the relevant field (including design matters and obvious matters).
[0017] The pencil or cosmetic barrel of the present disclosure is a pencil or cosmetic barrel formed by coating a pencil lead or a stick-shaped cosmetic with a barrel material composition, and is characterized in that the barrel material composition contains at least a naturally-derived filler, a naturally-derived binder, and a pigment.
[0018] Examples of natural body materials used in the present disclosure include sawdust, wood flour, powdered cellulose, and naturally occurring inorganic powders obtained from natural wood. The sawdust that can be used is not particularly limited, and may be derived from either hardwood or softwood. Specific tree species of sawdust used in the present disclosure include cedar, pine, larch, red pine, Abies sachalinensis, cypress, beech, horse chestnut, oak, Japanese oak, linden, birch, Japanese elm, lauan, and western hemlock. Cedar, cypress sapwood, beech, horse chestnut, and Japanese oak are particularly suitable. Furthermore, waste generated during the production of these woods may be effectively utilized. Furthermore, at least one type of sawdust (either one type or a combination of two or more types, the same applies below) can be used. The size of the sawdust is preferably an average particle size of 10 mesh or more in terms of dispersibility and moldability, and more preferably 200 mesh or less in terms of the energy cost required for crushing.
[0019] Examples of wood flour that can be used include at least one of wood flours obtained from the various tree species exemplified above for sawdust, wood flour obtained from the above sawdust or waste wood, and sander dust. To further improve dispersibility and moldability, the upper limit of the average particle size of the wood flour is preferably, for example, 2000 μm or less, and the lower limit is preferably, for example, 100 μm or more, although microfibrillated fibrous wood is also acceptable. The average particle size in the present disclosure can be a value measured in accordance with a laser diffraction / scattering method.
[0020] The powdered cellulose that can be used is preferably a cellulose powder obtained by finely pulverizing cellulose fibers derived from natural plants, and has an average particle size of 100 μm or less, preferably in the range of 10 to 50 μm. As the powdered cellulose, for example, a crystalline cellulose powder having a certain particle size distribution produced by a method such as purifying and drying the undecomposed residue obtained after acid hydrolysis of selected pulp, followed by pulverization and sieving, may be used, or a commercially available product such as "KC Flock" (manufactured by Nippon Paper Chemicals Co., Ltd.), "Ceolas" (manufactured by Asahi Kasei Chemicals Corporation), or "Avicel" (manufactured by FMC Corporation) may be used.
[0021] Usable naturally occurring inorganic powders include at least one of talc, calcium carbonate, huntite, kaolin, sericite, bentonite, titanium oxide, etc. The upper limit of the average particle size of these inorganic powders is preferably, for example, 50 μm or less, and the lower limit is preferably, for example, 1 μm.
[0022] The content of these naturally derived fillers is preferably 60 to 90% by mass, and more preferably 70 to 80% by mass, of the total amount of the shaft material composition. By setting the content of these naturally derived fillers to 60% by mass or more, usable cutting ability can be achieved, and by setting it to 90% by mass or less, usable strength can be achieved. Furthermore, by keeping the proportion of inorganic powders within these naturally derived fillers to 60% by mass or less, the drop resistance of the shaft can be improved, and when used as a pencil or cosmetic, it becomes possible to prevent breakage inside the pencil lead or stick-shaped cosmetic.
[0023] The naturally occurring binder used in the present disclosure may be at least one of cellulose fibers (including nanofibers), methylcellulose or its salts, carboxymethylcellulose or its salts, hydroxymethylpropylcellulose or its salts, cellulose acetate or its salts, sodium alginate, etc. Examples of the above-mentioned cellulose salts include sodium, ammonium, and calcium. These binders are preferably water-soluble, and from the viewpoint of imparting water resistance, carboxymethylcellulose ammonium is preferred.
[0024] The content of these naturally occurring binders is preferably 10 to 40% by mass, more preferably 20 to 30% by mass, based on the total amount of the shaft material composition. By setting the content of these naturally occurring binders to 10% by mass or more, usable strength can be achieved, and by setting it to 40% by mass or less, usable machinability can be achieved.
[0025] In addition to the naturally-derived filler and naturally-derived binder, the shaft material composition of the present disclosure may further contain a crosslinking agent that crosslinks the binder to further enhance the effects of the present disclosure and to impart water resistance. The crosslinking agent that crosslinks the binder is preferably one having a carboxylic acid group that forms an ester crosslink with the binder, and specific examples include succinic acid, malic acid, maleic acid, tartaric acid, citric acid, and polyacrylic acid. The content of these crosslinking agents is preferably 0.1 to 5% by mass, more preferably 0.5 to 2% by mass, of the total shaft material composition to achieve water resistance, prevent strength loss due to moisture absorption, and prevent discoloration of the material.
[0026] The pigments used in the present disclosure include inorganic pigments and organic pigments. In the present disclosure, the pencil or cosmetic barrel is formed using the above-mentioned natural fillers and natural binders, which have a low environmental impact, so it is preferable to use pigments that also have a low environmental impact. Therefore, it is not preferable to use pigment-containing resin particle pigments, white plastic pigments, hollow resin particles, thermochromic pigments, photochromic particles, or composite particles thereof.
[0027] Examples of inorganic pigments that can be used include at least one of carbon black, titanium black, zinc white, red iron oxide, aluminum, chromium oxide, iron black, cobalt blue, iron oxide yellow, viridian, zinc sulfide, lithopone, cadmium yellow, vermilion, cadmium red, yellow lead, molybdate orange, zinc chromate, strontium chromate, white carbon, clay, talc, ultramarine, precipitated barium sulfate, baryte powder, calcium carbonate, white lead, dark blue, iron blue, manganese violet, aluminum powder, brass powder, titanium oxide, zinc oxide, silica powder, and lithopone.
[0028] Usable organic pigments include, for example, azo lakes, insoluble azo pigments, chelate azo pigments, phthalocyanine pigments, perylene and perinone pigments, nitroso pigments, etc. More specifically, C.I. Pigment Blue 15, C.I. Pigment Blue 17, C.I. Pigment Blue 27, C.I. Pigment Red 5, C.I. Pigment Red 22, C.I. Pigment Red 38, C.I. Pigment Red 48, C.I. Pigment Red 49, C.I. Pigment Red 53, C.I. Pigment Red 57, C.I. Pigment Red 81, C.I. Pigment Red 104, C.I. Pigment Red 146, C.I. Pigment Red 245, C.I. Pigment Yellow 1, C.I. Pigment Yellow 3, C.I. Pigment Yellow 12, C.I. Pigment Yellow 13, C.I. Pigment Yellow 14, C.I. Pigment Yellow 17, C.I. Pigment Yellow 34, C.I. Pigment Yellow 55, C.I. Pigment Yellow 74, C.I. Pigment Yellow 95, C.I. Pigment Yellow 166, C.I. Pigment Yellow 167, C.I. Pigment Orange 5, C.I. Pigment Orange 13, C.I. Pigment Orange 16, C.I. Pigment Violet 1, C.I. Pigment Violet 3, C.I. Pigment Violet 19, C.I. Pigment Violet 23, C.I. Examples of pigments that can be used include at least one of C.I. Pigment Violet 50, C.I. Pigment Green 7, etc. Among these pigments, inorganic pigments, particularly iron black, iron oxide yellow, red iron oxide, titanium oxide, etc., are preferred in terms of light resistance and heat resistance. Furthermore, the average particle size of these pigments is preferably 0.1 to 2 μm in terms of preventing a decrease in strength and achieving sufficient coloring power. In this disclosure (including examples), the "average particle size" refers to the D50 value measured using a particle size analyzer [Microtrac HRA9320-X100 (manufactured by Nikkiso Co., Ltd.)].
[0029] The content of these pigments is preferably 0.2 to 5 mass %, more preferably 0.5 to 2 mass %, relative to the total amount of the shaft material composition, from the viewpoints of not causing a decrease in strength and obtaining good color development. Furthermore, the shaft material composition of the present disclosure can contain, as necessary, an antibacterial agent, a preservative, a fragrance, and the like, in addition to the above-mentioned naturally-derived fillers, naturally-derived binders, crosslinking agents, and pigments.
[0030] These shaft material compositions preferably have a natural origin index (excluding water) of 75% or more, from the viewpoint of further enhancing the effects of the present disclosure and reducing the burden on the environment. This "natural origin index (excluding water)" refers to an index indication according to ISO 16128, and by making this natural origin index (excluding water) 75% or more, more preferably 85% or more, it is possible to obtain pencil leads or cosmetic shafts that have an even smaller burden on the environment. A shaft material composition with a natural origin index (excluding water) of 75% or more can be achieved by appropriately selecting the above-mentioned natural extenders, natural binders, and pigments.
[0031] The shaft of the pencil or cosmetic product of the present disclosure is prepared by dry-mixing a blended composition comprising the above-mentioned naturally-derived fillers, naturally-derived binders, pigments, etc., using a kneading machine such as a Henschel mixer, planetary mixer, or kneader, then adding water (purified water, distilled water, etc.) so that the moisture content is 40 to 80%, and kneading to obtain a slurry. This slurry is further kneaded while heating and degassing to obtain a clay-like mixture with a moisture content of approximately 30 to 60%, and this mixture is extruded using a die of a predetermined diameter to coat the outer periphery of the pencil lead or cosmetic product to be coated with the above material, and then drying to obtain the pencil or cosmetic product. Alternatively, the kneaded mixture can be molded into a round or plate shape using a die of a predetermined diameter or a T-die using an extruder or the like, and dried to produce a molded product, which can then be processed to insert the pencil lead or cosmetic product. Furthermore, the physical properties of the barrel can be controlled over a wide range by combining the pressing pressure, moisture content, naturally derived fillers and binders during extrusion molding, etc., so that it is possible to obtain a barrel that is suitable for pencils or cosmetics and that satisfies the desired texture, strength, moldability, and color appearance including the cut cross section.
[0032] In the present disclosure, the composition and form of the pencil lead coated with the shaft material composition are not particularly limited, and examples thereof include baked pencil leads (including baked colored pencil leads) and non-baked pencil leads (including non-baked colored pencil leads). Examples of baked pencil leads include baked pencil leads obtained by mixing, dispersing, and kneading materials such as coloring components such as graphite, organic binders such as vinyl chloride resin, vinylidene chloride resin, vinyl acetate resin, chlorinated polyethylene, polyvinyl alcohol, acrylamide resin, chlorinated paraffin resin, phenolic resin, furan resin, urea resin, and butyl rubber, plasticizers such as phthalates, solvents such as methyl ethyl ketone and water, stabilizers such as stearates, lubricants such as stearic acid, and fillers such as carbon black, and then extruding and molding the resulting material into a thin wire, which is then heat-treated to a baking temperature to obtain a core, which is then impregnated with oils or waxes such as silicone oil, liquid paraffin, spindle oil, squalane, and α-olefin oligomers.
[0033] Furthermore, the composition and form of the stick-shaped cosmetic to be coated with the shaft material composition are not particularly limited, and examples include various blend compositions used for applications such as eyeliner, eyebrow, lip liner, concealer pencil, eyeshadow pencil, etc., such as cosmetics obtained by kneading waxes or clays, such as fats and oils, waxes, fatty acids, hydrocarbons, etc., as binders, with colorants and fillers, and then shaping the mixture into a stick shape; these may be baked stick-shaped cosmetics or non-baked stick-shaped cosmetics.
[0034] The pencil lead or cosmetic barrel of the present disclosure configured in this manner has the same ease of sharpening, drop resistance, and water resistance as conventional wooden barrels, the appearance including the cut cross section can be made any color, it has a low environmental impact, and can be used without modifying molding machines used in molding conventional pencils or cosmetics, so a pencil lead or cosmetic barrel that can be easily manufactured is obtained.
[0035] The pencil of the present disclosure is characterized in that at least the shaft is formed by covering and molding the pencil lead described above, and the stick-shaped cosmetic of the present disclosure is characterized in that at least the shaft is formed by covering and molding the stick-shaped cosmetic material described above, and the stick-shaped cosmetic material of the present disclosure is characterized in that the shaft is formed by covering and molding the stick-shaped cosmetic material described above. In the present disclosure, the pencil lead and stick-shaped cosmetic material can be formed into any shape, for example, a cross-sectional shape that is circular (including oval), a polygonal shape such as a triangular or hexagonal shape, or a tubular shape, and therefore pencils and stick-shaped cosmetics of various shapes can be made into such shapes by various processing methods such as covering and molding and cutting.
[0036] The present disclosure will be described below using examples and comparative examples, but the present disclosure is not limited to these examples. The pencils of Examples 1 to 9 and Comparative Examples 1 to 3 used pencil leads obtained by the following manufacturing method. 60% by mass of graphite and 40% by mass of clay were dry-mixed in a Henschel mixer, and then purified water was added to a moisture content of 40%, followed by kneading. The resulting slurry was kneaded while heating and degassing to obtain a clay-like mixture with a moisture content of approximately 30%. This was molded in a 2.5 mm diameter die using a hydraulic plunger extrusion molding machine, and the molded body was dried in a 60°C environment and then fired at 800 to 1400°C for 12 to 24 hours to obtain a lead body with a diameter of 2.0 mm. The obtained lead body was impregnated with an α-olefin oligomer to obtain a pencil lead with a diameter of 2.0 mm and a hardness of HB.
[0037] Example 1: Cedar wood sawdust (16 mesh) 69% by mass, black iron oxide 1% by mass, carboxymethylcellulose ammonium 30% by mass. The natural origin index (water-free) of this shaft material composition was 91.5%. The above blended composition was dry-mixed in a Henschel mixer, and then purified water was added to a moisture content of 50% and kneaded. The resulting slurry was kneaded while heating and degassing to obtain a clay-like mixture with a moisture content of approximately 40%. This material was extruded into a 9.0 mm diameter die using a hydraulic plunger extrusion molding machine to coat the outer periphery of a pencil lead with a diameter of 2.0 mm and a hardness of HB. The molded body was dried in a 60°C environment and heated at 180°C to render the binder insoluble in water, resulting in a pencil with a black appearance.
[0038] Example 2 Hunt's stone powder (average particle size 2 μm) 89% by mass Black iron oxide 1% by mass Cellulose powder (average particle size 45 μm) 10% by mass The natural origin index (excluding water) of this shaft material composition was 99.0%. The above blended composition was dry-mixed in a Henschel mixer, and then purified water was added to a moisture content of 50% and kneaded. The resulting slurry was kneaded while heating and degassing to obtain a clay-like mixture with a moisture content of approximately 40%. This was extruded into a 9.0 mm diameter die using a hydraulic plunger extrusion molding machine, and the material was coated onto the outer periphery of a pencil lead with a diameter of 2.0 mm and a hardness of HB. The molded body was dried in an environment of 60°C to obtain a pencil with a black appearance.
[0039] Example 3: Talc (average particle size 8 μm) 29% by mass, Cellulose powder (average particle size 45 μm) 60% by mass, Black iron oxide 1% by mass, Carboxymethylcellulose ammonium 10% by mass. The natural origin index (water-free) of this shaft material composition was 96.5%. The above blended composition was dry-mixed in a Henschel mixer, and then purified water was added to a moisture content of 50% and kneaded. The resulting slurry was kneaded while heating and degassing to obtain a clay-like mixture with a moisture content of approximately 40%. This material was extruded into a 9.0 mm diameter die using a hydraulic plunger extrusion molding machine to coat the outer periphery of a pencil lead with a diameter of 2.0 mm and a hardness of HB. The molded product was dried in a 60°C environment and heated at 180°C to render the binder insoluble in water, resulting in a pencil with a black appearance.
[0040] Example 4: Talc (average particle size 8 μm) 28.5% by mass, Cellulose powder (average particle size 45 μm) 60% by mass, C.I. Pigment Red 245 1.5% by mass, Carboxymethylcellulose ammonium 10% by mass. The natural origin index (water-free) of this shaft material composition was 97.0%. The above blended composition was dry-mixed in a Henschel mixer, and then purified water was added to a moisture content of 50%, followed by kneading. The resulting slurry was kneaded while heating and degassing to obtain a clay-like mixture with a moisture content of approximately 50%. This was extruded into a 9.0 mm diameter die using a hydraulic plunger extrusion molding machine, and the material was coated onto the outer periphery of a pencil lead with a diameter of 2.0 mm and a hardness of HB. The molded product was dried in a 60°C environment and heated at 180°C to render the binder insoluble in water, resulting in a pencil with a red appearance.
[0041] Example 5: Talc (average particle size 8 μm) 28% by mass, Cellulose powder (average particle size 45 μm) 60% by mass, Iron oxide yellow 2% by mass, Carboxymethylcellulose ammonium 10% by mass. The natural origin index (water-free) of this shaft material composition was 95.5%. The above blended composition was dry-mixed in a Henschel mixer, and then purified water was added to a moisture content of 50% and kneaded. The resulting slurry was kneaded while heating and degassing to obtain a clay-like mixture with a moisture content of approximately 40%. This material was extruded into a 9.0 mm diameter die using a hydraulic plunger extrusion molding machine to coat the outer periphery of a pencil lead with a diameter of 2.0 mm and a hardness of HB. The molded product was dried in a 60°C environment and heated at 180°C to render the binder insoluble in water, resulting in a pencil with a yellow appearance.
[0042] Example 6: Talc (average particle size 8 μm) 28% by mass, Cellulose powder (average particle size 45 μm) 60% by mass, C.I. Pigment Yellow 3 0.5% by mass, C.I. Pigment Red 22 0.4% by mass, Red iron oxide 1.1% by mass, Carboxymethylcellulose ammonium 10% by mass. The natural origin index (water-free) of this shaft material composition was 95.5%. The above blended composition was dry-mixed using a Henschel mixer, and then purified water was added to a moisture content of 50%, followed by kneading. The resulting slurry was kneaded while heating and degassing to obtain a clay-like mixture with a moisture content of approximately 40%. This was extruded into a 9.0 mm diameter die using a hydraulic plunger extrusion molding machine, and the material was coated onto the outer periphery of a pencil lead with a diameter of 2.0 mm and a hardness of HB. The molded product was dried in a 60°C environment and heated at 180°C to render the binder insoluble in water, resulting in a pencil with a brown appearance.
[0043] Example 7: Talc (average particle size 8 μm) 29% by mass, Cellulose powder (average particle size 45 μm) 60% by mass, Iron oxide black 1% by mass, Sodium carboxymethylcellulose 10% by mass. The natural origin index (water-free) of this shaft material composition was 94.1%. The above blended composition was dry-mixed in a Henschel mixer, and then a 5% aqueous succinic acid solution was added to achieve a moisture content of 50%, followed by kneading. The resulting slurry was kneaded while heating and degassing to obtain a clay-like mixture with a moisture content of approximately 40%. This material was extruded into a 9.0 mm diameter die using a hydraulic plunger extrusion molding machine, and the material was coated onto the outer periphery of a pencil lead with a diameter of 2.0 mm and a hardness of HB. The molded body was dried in a 60°C environment and then heated at 180°C to crosslink the binder, resulting in a pencil with a black appearance.
[0044] Example 8: Talc (average particle size 8 μm) 29% by mass, Cellulose powder (average particle size 45 μm) 60% by mass, Iron oxide black 1% by mass, Methylcellulose 10% by mass. The natural origin index (excluding water) of this shaft material composition was 96.5%. The above blended composition was dry-mixed in a Henschel mixer, and then purified water was added to a moisture content of 50%, followed by kneading. The resulting slurry was kneaded while heating and degassing, yielding a clay-like mixture with a moisture content of approximately 40%. This was extruded into a 9.0 mm diameter die using a hydraulic plunger extrusion molding machine, and the material was coated onto the outer periphery of a pencil lead with a diameter of 2.0 mm and a hardness of HB. The molded product was dried in a 60°C environment to obtain a pencil with a black appearance.
[0045] Example 9: Talc (average particle size 8 μm) 29% by mass, Cellulose powder (average particle size 45 μm) 60% by mass, Black iron oxide 1% by mass, Methylcellulose 10% by mass. The natural origin index (water-free) of this shaft material composition was 94.1%. The above blended composition was dry-mixed in a Henschel mixer, and then a 5% aqueous succinic acid solution was added to achieve a moisture content of 50%, followed by kneading. The resulting slurry was kneaded while heating and degassing to obtain a clay-like mixture with a moisture content of approximately 40%. This material was extruded into a 9.0 mm diameter die using a hydraulic plunger extrusion molding machine, and the material was coated onto the outer periphery of a pencil lead with a diameter of 2.0 mm and a hardness of HB. The molded body was dried in a 60°C environment and then heated at 180°C to crosslink the binder, resulting in a pencil with a black appearance.
[0046] (Example 10) <Preparation of solid cosmetic preparation> Beeswax 20 parts Ozokerite 10 parts Microcrystalline wax 10 parts Carnauba wax 8 parts Vaseline 7 parts Lanolin 5 parts Liquid paraffin 7 parts Isopropyl myristate 4 parts The above ingredients were dissolved, and to this was added 10 parts of iron oxide and 19 parts of red iron oxide. After stirring and dispersing, the mixture was kneaded in a mixer, cooled to room temperature, and then extruded to obtain a 2.0 mm brown solid cosmetic preparation.
[0047] (Preparation of stick-shaped cosmetic product) Talc (average particle size 8 μm) 29% by mass Cellulose powder (average particle size 45 μm) 60% by mass Black iron oxide 1% by mass Methylcellulose 10% by mass The natural origin index (water-free) of the above shaft material composition was 96.5%. The above blended composition was dry-mixed using a Henschel mixer, and then purified water was added to a moisture content of 50% and kneaded. The resulting slurry was kneaded while heating and degassing to obtain a clay-like mixture with a moisture content of approximately 40%. This was then extruded using a hydraulic plunger extrusion molding machine with a 9.0 mm diameter die to coat the above solid cosmetic product with a diameter of 2.0 mm. The molded product was dried in an environment of 60°C to obtain a stick-shaped cosmetic product with a black appearance.
[0048] (Comparative Example 1) Pencil (a pencil made by cutting an incense cedar board impregnated with 2% by weight of paraffin wax and coating the pencil lead with the above-mentioned diameter of 2.0 mm and hardness of HB. The surface of the shaft was colored with a paint containing iron oxide black.)
[0049] (Comparative Example 2) This is a pencil made from known recycled natural materials. Since a thermoplastic resin is used as the binder, a non-natural material is used, and the barrel surface is coated with a thermoplastic resin containing a colorant. The barrel has the following composition, and the natural origin index is 70.0%: Polypropylene (PP) 20% by mass, Wood flour 70% by mass, Maleic anhydride grafted polypropylene 1% by mass, Amide wax 3% by mass, Stearic acid 1% by mass, Boron nitride 5% by mass.
[0050] Comparative Example 3: Talc (average particle size 8 μm) 30% by mass, Cellulose powder (average particle size 45 μm) 60% by mass, Carboxymethylcellulose ammonium 10% by mass. The natural origin index (water-free) of this shaft material composition was 97.5%. The above blended composition was dry-mixed in a Henschel mixer, and then purified water was added to a moisture content of 50% and kneaded. The resulting slurry was kneaded while heating and degassing to obtain a clay-like mixture with a moisture content of approximately 40%. This was extruded into a 9.0 mm diameter die using a hydraulic plunger extrusion molding machine, and the material was coated onto the outer periphery of a pencil lead with a diameter of 2.0 mm and a hardness of HB. The molded body was dried in a 60°C environment and heated at 180°C to render the binder insoluble in water, resulting in a pencil with a white appearance.
[0051] The pencils and stick-type cosmetics of Examples 1 to 10 and Comparative Examples 1 to 3 obtained above were evaluated for their natural origin index by the following method, and their sharpening properties and appearance, including the cut cross section, were evaluated by the following evaluation methods. These results are shown in Table 1 below.
[0052] (Method of calculating the natural origin index) The natural origin index (excluding water) of the shaft bodies of Examples 1 to 10 and Comparative Examples 1 to 3 was determined by calculating the composition ratio as a percentage using the weight ratio of the raw materials blended into the shaft material excluding the core, of the natural raw materials and the naturally derived portions of the naturally derived raw materials, as defined in ISO 16128, excluding water. The higher this value, the higher the proportion of animal- and plant-derived materials and the less petroleum-derived materials used, which indicates a smaller burden on the environment.
[0053] (Method for evaluating ease of sharpening) For the pencils and stick-shaped cosmetics of Examples 1 to 10 and Comparative Examples 1 to 3, the tips were trimmed to a diameter of 2 mm using a pencil sharpener, and then the pencil was sharpened by manually rotating the side opposite the sharpener using a pencil sharpener installed in a fixture connected to a rotation moment measuring device until the lead was sharpened. The peak value of the rotation moment during this period was measured, and the ease of sharpening (cuttability) was evaluated according to the following evaluation criteria. If this value is less than 0.1 N, it can be easily cut, and if it exceeds 0.2 N·m, it can be said to be hard and difficult to cut. Evaluation criteria: A: Easily sharpened (less than 0.1 N·m) B: Sharpened (0.1 N·m or more but less than 0.2 N·m) C: Difficult to sharpen (0.2 N·m or more)
[0054] (Method for evaluating appearance including cut cross section) For the pencils and stick-shaped cosmetics of Examples 1 to 10 and Comparative Examples 1 to 3, a pencil sharpener was used to expose the cut surface, and the colors of the shaft and the cut surface were observed, and the appearance including the cut cross section was evaluated according to the following evaluation criteria. Evaluation criteria: A: Both the shaft and the cut surface are of the desired color B: The surface of the shaft is of the desired color, but the cut surface is not colored C: Not colored and not of the desired color
[0055]
[0056] Considering the evaluation results in Table 1 above, it was confirmed that Examples 1 to 10, which fall within the scope of the present disclosure, have the same easy-to-sharpen properties as Comparative Examples 1 to 3, but are environmentally friendly, and allow for easy production of any desired color for the appearance, including the cut cross section. Furthermore, Examples 3 to 10 maintain a high natural origin index while reducing the inorganic powder ratio in the filler to 60% or less. When evaluated by free-falling 10 times from a height of 75 cm onto a concrete floor, no damage was observed in the pencil or cosmetic product itself, pencil lead, or stick-shaped cosmetic product, confirming sufficient drop resistance. Furthermore, the pencils in Examples 1, 3 to 7, which were made water-insoluble by using carboxymethylcellulose ammonium as the natural binder, and the pencils in Example 9, which were crosslinked with a crosslinking agent having a carboxylic acid group that forms ester bridges, were evaluated for water resistance (water resistance after immersion of the manufactured pencil in purified water for 24 hours), and were confirmed to exhibit sufficient water resistance.
[0057] It is possible to obtain pencil or cosmetic shafts suitable for pencil leads (including colored pencil leads) and stick-type cosmetics such as eyeliners, eyebrow pencils, and eyeshadows.
Claims
1. A pencil or cosmetic barrel formed by covering a pencil lead or a stick-shaped cosmetic with a barrel material composition, characterized in that the barrel material composition contains at least a naturally derived filler, a naturally derived binder, and a pigment.
2. The pencil or cosmetic barrel according to claim 1, characterized in that the barrel material composition has a natural origin index (excluding water) of 75% or more.
3. A pencil comprising at least a pencil lead and a shaft body formed by covering the pencil lead, said shaft body being the shaft body described in claim 1 or 2.
4. A stick-shaped cosmetic comprising at least a stick-shaped cosmetic material and a shaft body formed by covering the stick-shaped cosmetic material, characterized in that the shaft body is the shaft body described in claim 1 or 2.
Citation Information
Patent Citations
pencil
JP1985204399A
Pencil
JP1994255296A
Synthetic shaft for biodegradable pencil-shaped cosmetic and method for manufacturing the same
JP2001192502A
Rigid fiberboard
JP1993096899A
Pencil plant-growing vessel
JP2001320914A