Method for producing cured composite resin, curable resin composition, ink, ink set, and cured object
The method of curing composite resin products with specific polyurethane resin compositions ensures accurate molding and stable mechanical properties by controlling elastic moduli and preventing plasticizer migration, addressing the challenge of maintaining accuracy and tack in multi-component resin products.
Patent Information
- Application Number
- PCT/JP2024/014161
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-12
- Filing Date
- 2024-04-05
- Publication Date
- 2024-10-17
AI Technical Summary
The challenge is to produce a composite resin cured product with multiple resin components having different mechanical properties that are adjacent to each other, while maintaining excellent molding accuracy and preventing changes in mechanical properties and surface tack due to plasticizer migration.
A method involving two resin compositions cured with active energy rays, where the first resin composition contains a curable polyurethane resin with a monovalent high molecular weight alcohol and the second with a polyhydric high molecular weight alcohol, ensuring a high elastic modulus ratio and suppressing plasticizer migration.
The method produces a composite resin product with excellent molding accuracy and stable mechanical properties, preventing changes in surface tack and maintaining the desired elastic moduli of the resin components.
Smart Images

Figure JP2024014161_17102024_PF_FP_ABST
Abstract
Description
Method for producing cured composite resin product, curable resin composition, ink, ink set, and cured product
[0001] The present invention relates to a method for producing a cured composite resin product, a curable resin composition, an ink, an ink set, and a cured product.
[0002] It has been proposed to three-dimensionally mold a photocurable resin composition to obtain a cured resin product. For example, the following method for producing a photocurable three-dimensional object has been proposed. In this method, a non-contact dispenser is used to dispense and place the photocurable resin composition. A urethane (meth)acrylate resin is used as the photocurable resin composition. The photocurable resin composition can also contain a plasticizer to adjust the mechanical properties of the object (see, for example, Patent Document 1).
[0003] International Publication No. 2017 / 018525
[0004] In recent years, there has been a demand for a composite cured resin product that is an integral product of a plurality of cured resin products. More specifically, there has been a demand for a cured resin product that is an integral product of a plurality of cured resin products that have different mechanical properties (e.g., elastic modulus) and are arranged adjacent to (in contact with) each other.
[0005] Therefore, in order to obtain a composite cured resin product, it has been considered to prepare two or more types of photocurable resin compositions, and to add a plasticizer to one or more types of photocurable resin compositions in order to obtain cured resin products having different mechanical properties.
[0006] However, in such cases, if multiple cured resins are placed adjacent to (in contact with) each other, migration of the plasticizer may occur between the cured resins. In such cases, each cured resin may swell and / or shrink over time. As a result, the volume of the cured composite resin may change, resulting in a problem of reduced molding accuracy.
[0007] Furthermore, if migration of the plasticizer occurs, there is a problem in that the mechanical properties and surface tackiness of each of the composite resin cured products change over time.
[0008] The present invention provides a method for producing a cured composite resin product, which is a cured composite resin product that includes a plurality of cured resin products that have different elastic moduli and are arranged adjacent to one another, has excellent molding precision, and is capable of suppressing changes in mechanical properties and surface tack, and a curable resin composition, ink, ink set, and cured product that are used in the production method.
[0009] The present invention [1] relates to a method for producing a cured composite resin product comprising a first cured resin product and a second cured resin product adjacent to each other, the method comprising: a first step of curing a first resin composition with active energy rays to form the first cured resin product; and a second step of curing a second resin composition with active energy rays to form the second cured resin product, wherein the ratio (M2 / M1) of the modulus of elasticity M2 (MPa) of the second cured resin product to the modulus of elasticity M1 (MPa) of the first cured resin product is 10 or more, the first resin composition contains a first curable polyurethane resin, and the first curable polyurethane resin contains a reaction product of a first polyisocyanate component, a first alcohol component, and a first active energy ray-curable group-containing component, and the first alcohol component is a monohydric high-molecular-weight alcohol.
[0010] The present invention [2] includes the method for producing a cured composite resin product described in the above [1], in which the first resin composition further contains a second curable polyurethane resin, the second curable polyurethane resin contains a reaction product of a second polyisocyanate component, a second alcohol component, and a second active energy ray-curable group-containing component, and the second alcohol component is a polyhydric high-molecular-weight alcohol.
[0011] The present invention [3] includes the method for producing a cured composite resin product according to the above [2], in which the content of the second curable polyurethane resin is 10% by mass or more and 95% by mass or less relative to the total amount of the first curable component.
[0012] The present invention [4] is a method for producing a composite resin cured product according to any one of the above [1] to [3], wherein the viscosity of the first resin composition at 25°C is 0.1 Pa·s or more and 5.0 Pa·s or less.
[0013] The present invention [5] includes the method for producing a cured composite resin product according to any one of the above [1] to [4], wherein the second resin composition further contains a third curable polyurethane resin, the third curable polyurethane resin contains a reaction product of a third polyisocyanate component, a third alcohol component, and a third active energy ray-curable group-containing component, and the third alcohol component is a polyhydric high-molecular-weight alcohol.
[0014] The present invention [6] includes the method for producing a cured composite resin product according to any one of the above [1] to [5], wherein the second resin composition contains a fourth curable polyurethane resin, the fourth curable polyurethane resin contains a reaction product of a fourth polyisocyanate component, a fourth alcohol component, and a fourth active energy ray-curable group-containing component, and the fourth alcohol component is a monohydric high-molecular-weight alcohol.
[0015] The present invention [7] includes the method for producing a cured composite resin product according to any one of the above [1] to [6], wherein the first resin composition does not contain a plasticizer.
[0016] The present invention [8] includes the method for producing a cured composite resin product according to any one of the above [1] to [7], wherein the ratio (M2 / M1) of the modulus of elasticity M2 (MPa) of the cured second resin product to the modulus of elasticity M1 (MPa) of the cured first resin product is 50 or more.
[0017] The present invention [9] includes the method for producing a cured composite resin product according to any one of the above [1] to [8], wherein the first step comprises a first discharging step of discharging the first resin composition from a dispenser and a first curing step of irradiating the discharged first resin composition with active energy rays to cure it, and the second step comprises a second discharging step of discharging the second resin composition from a dispenser and a second curing step of irradiating the discharged second resin composition with active energy rays to cure it.
[0018] The present invention
[10] includes the method for producing a cured composite resin product according to the above [9], wherein in the first step and / or the second step, the dispenser is an air pump dispenser and / or an aerojet dispenser.
[0019] The present invention
[11] includes the method for producing a cured composite resin product according to the above [9] or
[10] , in which first, either one of the first step or the second step is carried out, and then the other of the first step and the second step is carried out.
[0020] The present invention
[12] includes the method for producing a cured composite resin product according to the above [9] or
[10] , in which first, either one of the first discharging step or the second discharging step is carried out, then the other of the first discharging step and the second discharging step is carried out, and thereafter, the first curing step and the second curing step are carried out simultaneously.
[0021] The present invention
[13] includes the method for producing a cured composite resin product according to the above [9] or
[10] , in which the first discharging step and the second discharging step are first carried out simultaneously, and then the first curing step and the second curing step are carried out simultaneously.
[0022] The present invention
[14] is a curable resin composition used in the method for producing a cured composite resin product according to any one of the above [1] to
[13] , the curable resin composition comprising a first curable polyurethane resin, the first curable polyurethane resin comprising a reaction product of a first polyisocyanate component, a first alcohol component, and a first active energy ray-curable group-containing component, the first alcohol component being a monohydric high-molecular-weight alcohol.
[0023] The present invention
[15] includes the curable resin composition according to the above
[14] , further comprising a second curable polyurethane resin, the second curable polyurethane resin comprising a reaction product of a second polyisocyanate component, a second alcohol component, and a second active energy ray-curable group-containing component, and the second alcohol component is a polyhydric high-molecular-weight alcohol.
[0024] The present invention
[16] includes an ink containing a reaction product of a first polyisocyanate component, a first alcohol component, and a first active energy ray-curable group-containing component, wherein the first alcohol component is a monohydric high-molecular-weight alcohol.
[0025] The present invention
[17] includes an ink set having a first ink containing a reaction product of a first polyisocyanate component, a first alcohol component, and a first active energy ray-curable group-containing component, wherein the first alcohol component is a monohydric high-molecular-weight alcohol, and a second ink that is cured by active energy rays.
[0026] The present invention
[18] includes the ink set according to the above
[17] , wherein the first ink further contains a reaction product of a second polyisocyanate component, a second alcohol component, and a second active energy ray-curable group-containing component, and the second alcohol component is a polyhydric high-molecular-weight alcohol.
[0027] The present invention
[19] includes a cured product obtained by curing the ink set described in the above
[17] .
[0028] The present invention
[20] includes the cured product according to the above
[19] , wherein in the ink set, the ratio of the modulus of elasticity of the cured portion of the second ink to the modulus of elasticity of the cured portion of the first ink is 10 or more.
[0029] In the method for producing a cured composite resin product of the present invention, the cured composite resin product comprises a first cured resin product and a second cured resin product that are adjacent to each other, and the ratio (M2 / M1) of the modulus of elasticity M2 (MPa) of the second cured resin product to the modulus of elasticity M1 (MPa) of the first cured resin product is equal to or greater than a predetermined value. In other words, the cured composite resin product comprises a plurality of cured resin products that have different moduli of elasticity and are arranged adjacent to each other.
[0030] In the method for producing a cured composite resin product of the present invention, a first cured resin product is formed by curing a first cured resin composition. The first resin composition contains a first curable polyurethane resin. The first curable polyurethane resin contains a reaction product of a first polyisocyanate component, a first alcohol component, and a first active energy ray-curable group-containing component. The first alcohol component is a monohydric high-molecular-weight alcohol. Such a first curable polyurethane resin allows the elastic modulus M1 (MPa) of the cured first resin product to be adjusted without relying on a plasticizer.
[0031] Therefore, the method for producing a cured composite resin product of the present invention can produce a cured composite resin product that has excellent molding precision and is capable of suppressing changes in mechanical properties and surface tack.
[0032] The curable resin composition of the present invention is used in the method for producing the cured composite resin product, and therefore, the curable resin composition can produce a cured composite resin product that has excellent molding accuracy and is capable of suppressing changes in mechanical properties and surface tack.
[0033] Furthermore, the ink, ink set, and cured product of the present invention can achieve excellent molding precision and can suppress changes in mechanical properties and surface tack.
[0034] Figure 1A shows the first placement step. Figure 1B shows the first curing step. Figure 1C shows the second placement step. Figure 1D shows the second curing step. Figure 2A shows the first placement step. Figure 2B shows the second placement step. Figure 2C shows the first and second curing steps. Figure 3A shows the first and second placement steps. Figure 3B shows the first and second curing steps.
[0035] 1. Composite Resin Cured Product A composite resin cured product integrally comprises multiple resin cured products having different physical properties. More specifically, the composite resin cured product comprises at least a first resin cured product and a second resin cured product. The first resin cured product and the second resin cured product are resin cured products having different elastic moduli (described below). In the composite resin cured product, the first resin cured product and the second resin cured product are disposed adjacent to each other. More specifically, the first resin cured product and the second resin cured product are integrally molded so that the opposing surfaces of the first resin cured product and the second resin cured product are in contact with each other.
[0036] The first cured resin is a cured product of an active energy ray-curable resin composition (hereinafter referred to as the first resin composition). The second cured resin is a cured product of an active energy ray-curable resin composition (hereinafter referred to as the second resin composition) that is different from the first resin composition. The first resin composition and the second resin composition are described in detail below.
[0037] 1) First Resin Composition The first resin composition is a raw material component (molding material) of the first cured resin product. The first resin composition contains a resin component (hereinafter referred to as the first curable component) that can be cured by active energy rays. The first resin composition may also contain an additive (hereinafter referred to as the first additive) as needed. The first curable component and the first additive are each described in detail below.
[0038] (a) First Curable Component [First Curable Polyurethane Resin] The first curable component contains a first curable polyurethane resin. That is, the first resin composition (molding material) contains the first curable polyurethane resin as the first curable component.
[0039] The first curable polyurethane resin is a polyurethane resin that can be cured by active energy rays. The first curable polyurethane resin contains a reaction product of a first polyisocyanate component, a first alcohol component, and a first active energy ray-curable group-containing component. Preferably, the first curable polyurethane resin is a reaction product of the first polyisocyanate component, the first alcohol component, and the first active energy ray-curable group-containing component.
[0040] The first polyisocyanate component includes, for example, a polyisocyanate monomer and a polyisocyanate derivative.
[0041] Examples of polyisocyanate monomers include linear aliphatic polyisocyanate monomers, alicyclic polyisocyanate monomers, aromatic polyisocyanate monomers, and araliphatic polyisocyanate monomers. Examples of linear aliphatic polyisocyanate monomers include linear aliphatic diisocyanates. Examples of linear aliphatic diisocyanates include ethylene diisocyanate, trimethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate (PDI), and hexamethylene diisocyanate (HDI). Examples of alicyclic polyisocyanate monomers include alicyclic diisocyanates. Examples of alicyclic diisocyanates include cyclohexane diisocyanate, bis(isocyanatomethyl)cyclohexane (HDI), and bis(isocyanatomethyl)cyclohexane (HDI). 6 XDI), isophorone diisocyanate (IPDI), norbornene diisocyanate (NBDI), and methylenebis(cyclohexyl isocyanate) (H 12 Examples of aromatic polyisocyanate monomers include aromatic diisocyanates. Examples of aromatic diisocyanates include diphenylmethane diisocyanate (MDI), tolylene diisocyanate (TDI), toluidine diisocyanate (TODI), paraphenylene diisocyanate, and naphthalene diisocyanate (NDI). Examples of araliphatic polyisocyanate monomers include araliphatic diisocyanates. Examples of araliphatic diisocyanates include xylylene diisocyanate (XDI) and tetramethylxylylene diisocyanate (TMXDI). These can be used alone or in combination of two or more types.
[0042] Examples of polyisocyanate derivatives include modified products obtained by modifying the above-mentioned polyisocyanate monomers using known methods. More specifically, examples of polyisocyanate derivatives include polymers, isocyanurate modified products, allophanate modified products, polyol modified products, biuret modified products, urea modified products, oxadiazinetrione modified products, and carbodiimide modified products. Further, examples of polyisocyanate derivatives include polymethylene polyphenylene polyisocyanate. These can be used alone or in combination of two or more types.
[0043] These may be used alone or in combination of two or more. As the first polyisocyanate component, preferably, a polyisocyanate monomer is used, more preferably, an alicyclic polyisocyanate monomer is used, and further preferably, bis(isocyanatomethyl)cyclohexane (H 6 XDI).
[0044] The first alcohol component is a monohydric high molecular weight alcohol (high molecular weight monool). The monohydric high molecular weight alcohol has one hydroxyl group in the molecule and is an organic compound with a relatively high molecular weight. Note that the term "relatively high molecular weight" refers to a number average molecular weight of 400 or more (the same applies hereinafter).
[0045] Examples of monohydric high molecular weight alcohols include single-end-capped macrodiols. Examples of single-end-capped macrodiols include single-end-capped macrodiols containing a nonionic group. The nonionic group is, for example, a polyoxyethylene group having one end capped with an alkoxy group. Examples of single-end-capped macrodiols containing a nonionic group include single-end-capped polyoxyethylene glycols. Examples of single-end-capped polyoxyethylene glycols include alkoxyethylene glycols (monoalkoxypolyethylene glycols) having one end capped with an alkyl group. Examples of alkyl groups include alkyl groups having 1 to 20 carbon atoms, preferably alkyl groups having 1 to 10 carbon atoms, and more preferably alkyl groups having 1 to 4 carbon atoms. More specific examples of alkyl groups include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, s-butyl, and t-butyl, with methyl and ethyl being preferred. More specific examples of the one-end-capped polyoxyethylene glycol include methoxypolyoxyethylene glycol (MPEG) and ethoxypolyoxyethylene glycol, and preferably methoxypolyoxyethylene glycol.
[0046] The number average molecular weight of the primary alcohol component (monohydric high molecular weight alcohol) is, for example, 400 or more, preferably 500 or more, more preferably 1000 or more, and even more preferably 2000 or more. The number average molecular weight of the primary alcohol component (monohydric high molecular weight alcohol) is, for example, 20,000 or less, preferably 10,000 or less. The number average molecular weight can be calculated by a known method from the hydroxyl group equivalent weight and the average number of hydroxyl groups. The number average molecular weight can be measured as a polystyrene-equivalent molecular weight by gel permeation chromatography (the same applies below).
[0047] Examples of the first active energy ray-curable group-containing component include a hydroxyl group-containing unsaturated compound. The hydroxyl group-containing unsaturated compound is a compound having both one or more ethylenically unsaturated groups and one or more hydroxyl groups.
[0048] Examples of ethylenically unsaturated groups include (meth)acryloyl, vinylphenyl, propenyl ether, allyl ether, and vinyl ether groups. (Meth)acryloyl refers to acryloyl and / or methacryloyl. (Meth)acrylic refers to acrylic and / or methacrylic, and (meth)acrylate refers to acrylate and / or methacrylate.
[0049] The ethylenically unsaturated group is preferably a (meth)acryloyl group, more preferably an acryloyl group. When the ethylenically unsaturated group is a (meth)acryloyl group, the hydroxyl group-containing unsaturated compound may be, for example, a hydroxyl group-containing (meth)acrylate.
[0050] Examples of hydroxy group-containing (meth)acrylates include monohydroxyl mono(meth)acrylate, polyhydroxyl mono(meth)acrylate, monohydroxyl poly(meth)acrylate, and polyhydroxyl poly(meth)acrylate.
[0051] Monohydroxyl mono(meth)acrylate is a compound having one hydroxy group and one (meth)acryloyl group in one molecule. Examples of monohydroxyl mono(meth)acrylates include 2-hydroxyethyl(meth)acrylate (HE(M)A), 2-hydroxypropyl(meth)acrylate, 4-hydroxybutyl(meth)acrylate, 2-hydroxybutyl(meth)acrylate, 2-phenoxypropyl(meth)acrylate, 4-hydroxycyclohexyl(meth)acrylate, 3-chloro-2-hydroxypropyl(meth)acrylate, 2-hydroxy-3-phenyloxypropyl(meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxyethylphthalate, 2-hydroxyalkyl(meth)acryloylphosphate, pentanediol mono(meth)acrylate, neopentyl glycol mono(meth)acrylate, polyethylene glycol mono(meth)acrylate, and polypropylene glycol mono(meth)acrylate.
[0052] Polyhydroxyl mono(meth)acrylate is a compound having multiple hydroxy groups and one (meth)acryloyl group in one molecule. Examples of polyhydroxyl mono(meth)acrylate include trimethylolpropane mono(meth)acrylate, glycerin mono(meth)acrylate, and pentaerythritol mono(meth)acrylate.
[0053] Monohydroxyl poly(meth)acrylate is a compound having one hydroxy group and multiple (meth)acryloyl groups in one molecule. Examples of monohydroxyl poly(meth)acrylate include trimethylolpropane di(meth)acrylate, glycerin di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, and 2-hydroxy-3-(meth)acryloyloxypropyl(meth)acrylate.
[0054] Polyhydroxyl poly(meth)acrylate is a compound having multiple hydroxy groups and multiple (meth)acryloyl groups in one molecule. Examples of polyhydroxyl poly(meth)acrylate include pentaerythritol di(meth)acrylate, dipentaerythritol tri(meth)acrylate, and dipentaerythritol tetra(meth)acrylate.
[0055] These hydroxyl group-containing unsaturated compounds can be used alone or in combination of two or more. Preferred hydroxyl group-containing unsaturated compounds include hydroxyl group-containing (meth)acrylates, more preferably monohydroxyl mono(meth)acrylates, monohydroxyl poly(meth)acrylates, even more preferably monohydroxyl mono(meth)acrylates, still more preferably hydroxyalkyl (meth)acrylates, and particularly preferably 2-hydroxyethyl (meth)acrylate (HE(M)A).
[0056] The method for reacting the first polyisocyanate component, the first alcohol component, and the first active energy ray-curable group-containing component is not particularly limited. For example, the first polyisocyanate component, the first alcohol component, and the first active energy ray-curable group-containing component may be reacted all at once. Alternatively, the first polyisocyanate component, the first alcohol component, and the first active energy ray-curable group-containing component may be reacted sequentially. Preferably, the first polyisocyanate component and the first alcohol component are reacted first, and then the reaction product is reacted with the first active energy ray-curable group-containing component.
[0057] More specifically, in this method, a first polyisocyanate component and a first alcohol component are mixed in a predetermined ratio and subjected to a urethane reaction to produce a first alcohol-modified isocyanate (first isocyanate reaction step).
[0058] In the first isocyanate reaction step, the equivalent ratio of the isocyanate groups in the first polyisocyanate component to the hydroxyl groups in the first alcohol component (isocyanate groups / hydroxyl groups) is, for example, greater than 1, preferably 1.1 or more, more preferably 3 or more, even more preferably 6 or more, and preferably 20 or less, more preferably 15 or less, even more preferably 10 or less.
[0059] In the first isocyanate reaction step, a known reaction method is employed. Examples of the reaction method include bulk reaction and solution reaction. In the bulk reaction, for example, the above components are blended under a nitrogen atmosphere and reacted at a reaction temperature of 75 to 85°C for about 1 to 20 hours. In the solution reaction, for example, the above components are added to a known organic solvent under a nitrogen atmosphere and reacted at a reaction temperature of 20 to 80°C for about 1 to 20 hours. In addition, in the first isocyanate reaction step, a known urethane catalyst is added in an appropriate ratio as needed.
[0060] This results in a first alcohol-modified isocyanate being obtained as the reaction product of the first isocyanate reaction step. The first alcohol-modified isocyanate is purified by a known method, if necessary. Examples of the purification method include distillation and extraction, and preferably distillation. The distillation method is not particularly limited, but examples include batch distillation and continuous distillation, and preferably continuous distillation. Examples of continuous distillation methods include thin film distillation (Smith thin film distillation). The distillation conditions are set depending on the purpose and application.
[0061] The isocyanate group concentration of the primary alcohol-modified isocyanate is, relative to the total amount (solid content) of the primary alcohol-modified isocyanate, for example, 0.3% by mass or more, preferably 0.5% by mass or more, more preferably 1.0% by mass or more. The isocyanate group concentration of the primary alcohol-modified isocyanate is, relative to the total amount (solid content) of the primary alcohol-modified isocyanate, for example, 15% by mass or less, preferably 12% by mass or less, more preferably 10% by mass or less.
[0062] Next, in this method, the first alcohol-modified isocyanate is reacted with the first active energy ray-curable group-containing component in a predetermined ratio (first curable group addition step), thereby producing a first curable polyurethane resin.
[0063] More specifically, in the first curable group addition step, for example, the above-mentioned isocyanate group-terminated prepolymer and a first active energy ray-curable group-containing component (hydroxy group-containing unsaturated compound) are blended in a predetermined equivalent ratio under an inert gas atmosphere, and a urethane reaction is carried out.
[0064] The equivalent ratio (isocyanate group / hydroxy group) of the isocyanate group in the isocyanate group-terminated prepolymer to the hydroxy group in the first active energy ray-curable group-containing component (hydroxy group-containing unsaturated compound) is, for example, 0.7 or more, preferably 0.9 or more, and for example, 1.5 or less, preferably 1.2 or less.
[0065] The reaction conditions are not particularly limited and are appropriately set depending on the purpose and application. For example, the reaction temperature is, for example, 40°C or higher, preferably 50°C or higher, and more preferably 60°C or higher. The reaction temperature is, for example, 120°C or lower, preferably 100°C or lower, and more preferably 80°C or lower. The reaction time is, for example, 0.5 hours or higher, preferably 1.0 hour or higher. The reaction time is, for example, 24 hours or lower, preferably 10 hours or lower. In the first curable group addition step, a known urethane catalyst is added at an appropriate ratio, if necessary.
[0066] This results in a first curable polyurethane resin. The first curable polyurethane resin is obtained by a urethane reaction between the isocyanate groups of the first alcohol-modified isocyanate and the hydroxy groups of the first active energy ray-curable group-containing component (hydroxy group-containing unsaturated compound). In other words, the first curable polyurethane resin is a reaction product of the first alcohol-modified isocyanate and the first active energy ray-curable group-containing component. The first curable polyurethane resin is a polyurethane resin having unsaturated bonds derived from the first active energy ray-curable group-containing component (hydroxy group-containing unsaturated compound).
[0067] The composition (type) and number average molecular weight of the first curable polyurethane resin are not particularly limited and are appropriately selected so that the modulus of elasticity M1 (described below) of the cured first resin product is a desired value. Furthermore, the content of the first curable polyurethane resin in the cured first resin product is appropriately selected so that the modulus of elasticity M1 (described below) of the cured first resin product is a desired value.
[0068] For example, the content of the first curable polyurethane resin may be 100% by mass relative to the total amount of the first curable component. That is, the first curable component may consist of the first curable polyurethane resin. Furthermore, from the viewpoint of adjusting the elastic modulus M1 (described below) of the first resin cured product, the first curable component may contain the first curable polyurethane resin and another curable resin (described below).
[0069] The content of the first curable polyurethane resin is, for example, more than 0% by mass, preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 20% by mass or more, and particularly preferably 30% by mass or more, relative to the total amount of the first curable component. The content of the first curable polyurethane resin is, for example, 100% by mass or less, preferably 90% by mass or less, more preferably 70% by mass or less, even more preferably 50% by mass or less, and particularly preferably 40% by mass or less, relative to the total amount of the first curable component.
[0070] [Second Curable Polyurethane Resin] The first curable component may contain other curable resins as needed. In the first curable component, the other curable resins are curable resins other than the first curable polyurethane resin. Examples of the other curable resins include the second curable polyurethane resin.
[0071] The second curable polyurethane resin is a polyurethane resin having a different composition (type) from the first curable polyurethane resin. If the first curable component contains the second curable polyurethane resin, the mechanical properties of the cured first resin product can be more freely adjusted. Therefore, the first resin composition (molding material) preferably contains the second curable polyurethane resin as the first curable component.
[0072] The second curable polyurethane resin is a polyurethane resin that can be cured by active energy rays. The second curable polyurethane resin contains, for example, a reaction product of a second polyisocyanate component, a second alcohol component, and a second active energy ray-curable group-containing component. Preferably, the second curable polyurethane resin is a reaction product of a second polyisocyanate component, a second alcohol component, and a second active energy ray-curable group-containing component.
[0073] Examples of the second polyisocyanate component include the above-mentioned polyisocyanate monomer (the monomer described above as a raw material for the first curable polyurethane resin) and the above-mentioned polyisocyanate derivative (the derivative described above as a raw material for the first curable polyurethane resin). These can be used alone or in combination of two or more. As the second polyisocyanate component, preferably, a polyisocyanate monomer is used, more preferably, an alicyclic polyisocyanate monomer is used, and even more preferably, bis(isocyanatomethyl)cyclohexane (H 6 XDI), and isophorone diisocyanate (IPDI), and particularly preferred is bis(isocyanatomethyl)cyclohexane (H 6 XDI).
[0074] The second alcohol component is a polyhydric high-molecular-weight alcohol (high-molecular-weight polyol). A polyhydric high-molecular-weight alcohol has two or more hydroxyl groups in the molecule and is an organic compound with a relatively high molecular weight.
[0075] The polyhydric high molecular weight alcohol may be a known macropolyol. Examples of the macropolyol include polyether polyol, polyester polyol, polycarbonate polyol, polyurethane polyol, epoxy polyol, vegetable oil polyol, polyolefin polyol, acrylic polyol, and vinyl monomer-modified polyol. These may be used alone or in combination of two or more. The polyhydric high molecular weight alcohol is preferably polyether polyol.
[0076] Examples of polyether polyols include polyoxyalkylene (C2-3) polyols and polytetramethylene ether polyols, and preferably polyoxyalkylene (C2-3) polyols.
[0077] Polyoxyalkylene (C2-3) polyol is, for example, an addition polymer of alkylene oxide using a known low-molecular-weight polyol and / or a known low-molecular-weight polyamine as an initiator. Examples of alkylene oxides include alkylene oxides having 2 to 3 carbon atoms. More specific examples of alkylene oxides include ethylene oxide (IUPAC name: oxirane), propylene oxide (1,2-propylene oxide (IUPAC name: methyloxirane)), and triethylene oxide (1,3-propylene oxide). These alkylene oxides can be used alone or in combination of two or more. Preferred examples of alkylene oxides include ethylene oxide and propylene oxide.
[0078] More specific examples of polyoxyalkylene (C2-3) polyols include polyoxyethylene polyols, polyoxypropylene polyols, polyoxytriethylene polyols, and polyoxyethylene-polyoxypropylene polyols (random or block copolymers). The polyoxyalkylene (C2-3) polyols can be used alone or in combination of two or more.
[0079] As the polyoxyalkylene (C2-3) polyol, preferably, polyoxypropylene polyol is used, and more preferably, polyoxypropylene glycol is used.
[0080] The number average molecular weight of the second alcohol component (polyhydric high molecular weight alcohol) is, for example, 400 or more, preferably 500 or more, more preferably 1000 or more, and even more preferably 2000 or more. The number average molecular weight of the second alcohol component (polyhydric high molecular weight alcohol) is, for example, 20000 or less, preferably 10000 or less.
[0081] The average number of functional groups of the second alcohol component (polyhydric high molecular weight alcohol) is, for example, 2.0 or more. The average number of functional groups of the second alcohol component (polyhydric high molecular weight alcohol) is, for example, 4.0 or less, preferably 3.0 or less, and more preferably 2.5 or less. The average number of functional groups of the second alcohol component is particularly preferably 2.0.
[0082] Examples of the second active energy ray-curable group-containing component include the above-mentioned hydroxy group-containing unsaturated compounds. Examples of the hydroxy group-containing unsaturated compound include preferably hydroxy group-containing (meth)acrylates, more preferably monohydroxyl mono(meth)acrylates, monohydroxyl poly(meth)acrylates, even more preferably monohydroxyl mono(meth)acrylates, still more preferably hydroxyalkyl (meth)acrylates, and particularly preferably 2-hydroxyethyl (meth)acrylate (HE(M)A).
[0083] The method for reacting the second polyisocyanate component, the second alcohol component, and the second active energy ray-curable group-containing component is not particularly limited. For example, the second polyisocyanate component, the second alcohol component, and the second active energy ray-curable group-containing component may be reacted all at once. Alternatively, the second polyisocyanate component, the second alcohol component, and the second active energy ray-curable group-containing component may be reacted sequentially. Preferably, the second polyisocyanate component and the second alcohol component are reacted first, and then the reaction product is reacted with the second active energy ray-curable group-containing component.
[0084] More specifically, in this method, a second polyisocyanate component and a second alcohol component are first mixed in a predetermined ratio and subjected to a urethane reaction, thereby producing a second isocyanate group-terminated prepolymer (second isocyanate reaction step).
[0085] In the second isocyanate reaction step, the equivalent ratio of the isocyanate groups in the second polyisocyanate component to the hydroxyl groups in the second alcohol component (isocyanate groups / hydroxyl groups) is, for example, greater than 1, preferably 1.1 or more, more preferably 3 or more, even more preferably 6 or more, and preferably 20 or less, more preferably 15 or less, even more preferably 10 or less.
[0086] In the second isocyanate reaction step, a known polymerization method is employed. Examples of the polymerization method include bulk polymerization and solution polymerization. In bulk polymerization, for example, the above components are blended under a nitrogen atmosphere and reacted at a reaction temperature of 75 to 85°C for about 1 to 20 hours. In solution polymerization, for example, the above components are added to a known organic solvent under a nitrogen atmosphere and reacted at a reaction temperature of 20 to 80°C for about 1 to 20 hours. In addition, in the second isocyanate reaction step, a known urethane catalyst is added in an appropriate ratio as needed.
[0087] This results in a second isocyanate group-terminated prepolymer being obtained as the reaction product of the second isocyanate reaction step. The second isocyanate group-terminated prepolymer is purified by a known method, if necessary. Examples of the purification method include distillation and extraction, and preferably distillation. The distillation method is not particularly limited, but examples include batch distillation and continuous distillation, and preferably continuous distillation. Examples of the continuous distillation method include thin film distillation (Smith thin film distillation). The distillation conditions are set according to the purpose and application.
[0088] The isocyanate group concentration of the second isocyanate group-terminated prepolymer is, for example, 0.3% by mass or more, preferably 0.5% by mass or more, and more preferably 1.0% by mass or more, based on the total amount (solid content) of the second isocyanate group-terminated prepolymer. The isocyanate group concentration of the second isocyanate group-terminated prepolymer is, for example, 15% by mass or less, preferably 12% by mass or less, and more preferably 10% by mass or less, based on the total amount (solid content) of the second isocyanate group-terminated prepolymer.
[0089] Next, in this method, the second isocyanate group-terminated prepolymer is reacted with a second active energy ray-curable group-containing component in a predetermined ratio (second curable group addition step), thereby producing a second curable polyurethane resin.
[0090] More specifically, in the second curable group addition step, for example, the above-mentioned isocyanate group-terminated prepolymer and a second active energy ray-curable group-containing component (hydroxy group-containing unsaturated compound) are blended in a predetermined equivalent ratio under an inert gas atmosphere, and a urethane reaction is carried out.
[0091] The equivalent ratio (isocyanate group / hydroxy group) of the isocyanate group in the isocyanate group-terminated prepolymer to the hydroxy group in the second active energy ray-curable group-containing component (hydroxy group-containing unsaturated compound) is, for example, 0.7 or more, preferably 0.9 or more, and for example, 1.5 or less, preferably 1.2 or less.
[0092] The reaction conditions are not particularly limited and are appropriately set depending on the purpose and application. For example, the reaction temperature is, for example, 40°C or higher, preferably 50°C or higher, and more preferably 60°C or higher. The reaction temperature is, for example, 120°C or lower, preferably 100°C or lower, and more preferably 80°C or lower. The reaction time is, for example, 0.5 hours or higher, preferably 1.0 hour or higher. The reaction time is, for example, 24 hours or lower, preferably 10 hours or lower. In the second curable group addition step, a known urethane catalyst is added at an appropriate ratio, if necessary.
[0093] This results in a second curable polyurethane resin. The second curable polyurethane resin is obtained by a urethane reaction between the isocyanate groups of the second isocyanate group-terminated prepolymer and the hydroxy groups of the second active energy ray-curable group-containing component (hydroxy group-containing unsaturated compound). In other words, the second curable polyurethane resin is a reaction product of the second isocyanate group-terminated prepolymer and the second active energy ray-curable group-containing component. The second curable polyurethane resin is a polyurethane resin having unsaturated bonds derived from the second active energy ray-curable group-containing component (hydroxy group-containing unsaturated compound).
[0094] The composition (type) and number average molecular weight of the second curable polyurethane resin are not particularly limited and are appropriately selected so that the modulus of elasticity M1 (described below) of the cured first resin product is a desired value. The content of the second curable polyurethane resin in the cured first resin product is appropriately selected so that the modulus of elasticity M1 (described below) of the cured first resin product is a desired value.
[0095] For example, the content of the second curable polyurethane resin may be, for example, 0% by mass relative to the total amount of the first curable component. That is, the first curable component does not need to contain the second curable polyurethane resin. From the viewpoint of adjusting the elastic modulus M1 (described below) of the first resin cured product, the first curable component preferably contains the first curable polyurethane resin and the second curable polyurethane resin.
[0096] The content of the second curable polyurethane resin relative to the total amount of the first curable component is, for example, 0% by mass or more, preferably 10% by mass or more, more preferably 30% by mass or more, even more preferably 50% by mass or more, and particularly preferably 60% by mass or more. The content of the second curable polyurethane resin relative to the total amount of the first curable component is, for example, less than 100% by mass, preferably 95% by mass or less, more preferably 90% by mass or less, even more preferably 80% by mass or less, and particularly preferably 70% by mass or less.
[0097] The content of the second curable polyurethane resin is, for example, 0 parts by mass or more, preferably 10 parts by mass or more, more preferably 50 parts by mass or more, and even more preferably 100 parts by mass or more, per 100 parts by mass of the first curable polyurethane resin. The content of the second curable polyurethane resin is, for example, 1000 parts by mass or less, preferably 800 parts by mass or less, more preferably 600 parts by mass or less, and even more preferably 400 parts by mass or less, per 100 parts by mass of the first curable polyurethane resin.
[0098] [Active Energy Ray Cation-Curable Resin] In the first curable component, the other curable resin is not limited to the second curable polyurethane resin. Examples of the other curable resin include an active energy ray cation-curable resin.
[0099] The active energy ray cationically curable resin is a cationically curable resin that can be cured by active energy rays. Examples of the active energy ray cationically curable resin include epoxy resins, oxetane resins, maleimide resins, and vinyl ether resins. These can be used alone or in combination of two or more. A preferred example of the active energy ray cationically curable resin is an epoxy resin.
[0100] The composition (type) and content of the active energy ray cationically curable resin are not particularly limited, and are appropriately selected so that the modulus of elasticity M1 (described below) of the first resin cured product becomes a desired value.
[0101] Preferably, the first curable component does not contain an active energy ray cationically curable resin. That is, preferably, the first resin composition (raw material component) does not contain an active energy ray cationically curable resin as the first curable component.
[0102] The content of the active energy ray cationically curable resin is, for example, 0% by mass or more relative to the total amount of the first curable component. The content of the active energy ray cationically curable resin is, for example, less than 100% by mass, preferably 95% by mass or less, more preferably 90% by mass or less, even more preferably 80% by mass or less, and particularly preferably 70% by mass or less relative to the total amount of the first curable component.
[0103] The content of the active energy ray cationically curable resin is, for example, 0 parts by mass or more relative to 100 parts by mass of the first curable polyurethane resin, and the content of the active energy ray cationically curable resin is, for example, 1,000 parts by mass or less, preferably 800 parts by mass or less, more preferably 600 parts by mass or less, and even more preferably 400 parts by mass or less relative to 100 parts by mass of the first curable polyurethane resin.
[0104] [Radical Reactive Diluent] The first curable component may further contain a radical reactive diluent. In other words, the first resin composition (molding material) may contain a radical reactive diluent as the first curable component.
[0105] The radical-reactive diluent is a compound that undergoes radical polymerization upon irradiation with active energy rays (described below), and is a diluent for diluting the first curable polyurethane resin (and the second curable polyurethane resin).
[0106] Examples of radical reactive diluents include reactive compounds having an aromatic hydrocarbon skeleton, reactive compounds having an alicyclic hydrocarbon skeleton, reactive compounds having a chain aliphatic hydrocarbon skeleton, reactive compounds having a chain ether skeleton, reactive compounds having an alicyclic ether skeleton, reactive compounds having an amide skeleton, reactive compounds having an oxyalkylene skeleton, compounds having both a (meth)acryloyl group and a vinyl group, poly(meth)acrylate, hydroxyl group-containing (meth)acrylate, and unsaturated carboxylic acid allyl ester. Examples of reactive compounds having an aromatic hydrocarbon skeleton include 3-phenoxybenzyl (meth)acrylate, styrene, vinyltoluene, divinylbenzene, and α-methylstyrene. Examples of reactive compounds having an alicyclic hydrocarbon skeleton include cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, 3,3,5-trimethylcyclohexyl (meth)acrylate, 4-tert-butylcyclohexyl (meth)acrylate, and dicyclopentanyl (meth)acrylate. Examples of reactive compounds having a chain aliphatic hydrocarbon skeleton include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and lauryl (meth)acrylate. Examples of reactive compounds having a chain ether skeleton include 2-ethylhexyl-diglycol (meth)acrylate. Examples of reactive compounds having an alicyclic ether skeleton include cyclic trimethylolpropane formal (meth)acrylate, (2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl acrylate, and 4-(meth)acryloylmorpholine. Examples of reactive compounds having an amide skeleton include N,N-diethyl (meth)acrylamide. Examples of reactive compounds having an oxyalkylene skeleton include 2-ethylhexyl-diglycol (meth)acrylate.Examples of compounds having both a (meth)acryloyl group and a vinyl group include methyl 2-(allyloxymethyl)acrylate, 2-vinyloxyethyl (meth)acrylate, 3-vinyloxypropyl (meth)acrylate, 1-methyl-2-vinyloxyethyl (meth)acrylate, 2-vinyloxypropyl (meth)acrylate, 4-vinyloxybutyl (meth)acrylate, 4-vinyloxycyclohexyl (meth)acrylate, 5-vinyloxypentyl (meth)acrylate, 6-vinyloxyhexyl (meth)acrylate, 4-vinyloxymethylcyclohexylmethyl (meth)acrylate, p-vinyloxymethylphenylmethyl (meth)acrylate, 2-(vinyloxyethoxy)ethyl (meth)acrylate, and 2-(vinyloxyethoxyethoxyethoxy)ethyl (meth)acrylate. Examples of polyol poly(meth)acrylates include ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate, pentanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, hexanediol di(meth)acrylate, nonanediol di(meth)acrylate, decanediol di(meth)acrylate, oligoethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, glycerin tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, and dipentaerythritol hexa(meth)acrylate. Examples of hydroxy group-containing (meth)acrylates include the above-mentioned monohydroxyl mono(meth)acrylates (e.g., 4-hydroxybutyl (meth)acrylate). Examples of unsaturated carboxylic acid allyl esters include allyl (meth)acrylate, diallyl maleate, diallyl fumarate, and diallyl itaconate. These can be used alone or in combination of two or more.
[0107] The type and content of the radical reactive diluent are not particularly limited and are appropriately selected so that the modulus of elasticity M1 (described below) of the first cured resin product becomes a desired value.
[0108] Preferably, the first curable component does not contain a radical-reactive diluent, i.e., the first resin composition preferably does not contain a radical-reactive diluent.
[0109] The content of the radical reactive diluent relative to the total amount of the first curable component is, for example, 0% by mass or more, and for example, less than 100% by mass, preferably 95% by mass or less, more preferably 90% by mass or less, even more preferably 80% by mass or less, and particularly preferably 70% by mass or less, relative to the total amount of the first curable component.
[0110] The content of the radical reactive diluent relative to 100 parts by mass of the first curable polyurethane resin is, for example, 0 parts by mass or more, and the content of the radical reactive diluent relative to 100 parts by mass of the first curable polyurethane resin is, for example, 100 parts by mass or less, preferably 90 parts by mass or less, more preferably 70 parts by mass or less, and even more preferably 50 parts by mass or less.
[0111] (b) First Additive The first resin composition can optionally contain a first additive. The first resin composition preferably contains a first additive. Examples of the first additive include an active energy ray polymerization initiator, a plasticizer, a thixotropic agent, an antioxidant, an ultraviolet absorber, a fluorescent brightener, an internal mold release agent, a lubricant, a sensitizer, an antiblocking agent, a heat stabilizer, an active energy ray-resistant stabilizer, a light stabilizer, a catalyst, a pigment, a dye, a lubricant, a filler, and a hydrolysis inhibitor. The amount and timing of addition of these additives are appropriately determined depending on the purpose and application.
[0112] The first additive is preferably an active energy ray polymerization initiator. Examples of the active energy ray polymerization initiator include known active energy ray radical polymerization initiators (e.g., photoradical polymerization initiators) and known active energy ray cationic polymerization initiators (e.g., photocationic polymerization initiators). In addition, active energy ray polymerization initiators are commercially available. Examples of such commercially available products include TPO (trade name, manufactured by Tokyo Chemical Industry Co., Ltd.), Irgacure 819 (BAPO, trade name, manufactured by BASF), Irgacure 369 (Omnirad 369, trade name, manufactured by BASF), Irgacure OXE01 (trade name, manufactured by BASF), Irgacure OXE02 (trade name, manufactured by BASF), Irgacure OXE03 (trade name, manufactured by BASF), Irgacure OXE04 (trade name, manufactured by BASF), Omnirad 184 (trade name, manufactured by IGM resins B.V.), Darocur 1173 (trade name, manufactured by BASF), NCI-831 (trade name, manufactured by ADEKA), and BLUESIL PI2074 (Elkem These may be used alone or in combination of two or more types.
[0113] The active energy ray polymerization initiator is used in an amount of, for example, 0.1 parts by mass or more, preferably 0.5 parts by mass or more, per 100 parts by mass of the first curable component (total amount), and is used in an amount of, for example, 5.0 parts by mass or less, preferably 1.0 part by mass or less, per 100 parts by mass of the first curable component (total amount).
[0114] In addition, from the viewpoint of adjusting the mechanical properties of the cured first resin product, the first additive preferably contains a thixotropic agent. In addition, from the viewpoint of suppressing deterioration of the cured first resin product over time, the first additive preferably contains an antioxidant.
[0115] Furthermore, from the viewpoint of obtaining excellent molding precision and suppressing changes in mechanical properties and surface tackiness, the first additive preferably does not contain a plasticizer. That is, the first resin composition preferably does not contain a plasticizer.
[0116] In other words, when the first resin composition contains a plasticizer, the mechanical properties of the cured first resin product can be easily adjusted, but migration of the plasticizer may occur in the cured composite resin product. In contrast, since the first resin composition contains a first curable polyurethane resin, the elastic modulus M1 (MPa) of the cured first resin product can be adjusted without relying on a plasticizer. Therefore, the first resin composition preferably does not contain a plasticizer.
[0117] The viscosity of the first resin composition at 25°C is, for example, 0.1 Pa·s or more, preferably 0.3 Pa·s or more, more preferably 0.5 Pa·s or more. The viscosity of the first resin composition at 25°C is, for example, 5.0 Pa·s or less, preferably 3.0 Pa·s or less, more preferably 1.5 Pa·s or less.
[0118] The viscosity at 25°C is measured by the following method: an E-type viscometer (product name: TV25 Viscometer, manufactured by Toki Sangyo Co., Ltd.) is used. The rotor number is No. 1, the rotor angle is 1°34', and the rotor radius is 2.4 cm (the same applies below).
[0119] 2) Second Resin Composition The second resin composition is a raw material component (molding material) of the second resin cured product. The second resin composition contains a resin component that can be cured by active energy rays (hereinafter referred to as the second curable component). The second resin composition may also contain an additive (hereinafter referred to as the second additive) as needed. The second curable component and the second additive are each described in detail below.
[0120] (a) Second Curable Component [Third Curable Polyurethane Resin] The second curable component contains, for example, a third curable polyurethane resin. In other words, the second resin composition (molding material) contains, for example, a third curable polyurethane resin as the second curable component.
[0121] The third curable polyurethane resin is a polyurethane resin that can be cured by active energy rays. The third curable polyurethane resin contains, for example, a reaction product of a third polyisocyanate component, a third alcohol component, and a third active energy ray-curable group-containing component. Preferably, the third curable polyurethane resin is a reaction product of a third polyisocyanate component, a tertiary alcohol component, and a third active energy ray-curable group-containing component.
[0122] Examples of the third polyisocyanate component include the above-mentioned polyisocyanate monomers (monomers described above as the first polyisocyanate component) and the above-mentioned polyisocyanate derivatives (derivatives described above as the first polyisocyanate component). These can be used alone or in combination of two or more. As the third polyisocyanate component, preferably, a polyisocyanate monomer is used, more preferably, an alicyclic polyisocyanate monomer is used, and even more preferably, bis(isocyanatomethyl)cyclohexane (H 6 XDI), and isophorone diisocyanate (IPDI), and particularly preferred is bis(isocyanatomethyl)cyclohexane (H 6 XDI).
[0123] The third alcohol component is a polyhydric high molecular weight alcohol (high molecular weight polyol). Examples of the polyhydric high molecular weight alcohol include the above-mentioned polyhydric high molecular weight alcohols (the polyhydric high molecular weight alcohols described above as raw materials for the second curable polyurethane resin). These can be used alone or in combination of two or more. As the polyhydric high molecular weight alcohol, preferably, polyether polyol is used, more preferably, polyoxyalkylene (C2-3) polyol is used, even more preferably, polyoxypropylene polyol is used, and particularly preferably, polyoxypropylene glycol is used.
[0124] The number average molecular weight of the tertiary alcohol component (polyhydric high molecular weight alcohol) is, for example, 400 or more, preferably 500 or more, more preferably 1000 or more, and even more preferably 2000 or more. The number average molecular weight of the tertiary alcohol component (polyhydric high molecular weight alcohol) is, for example, 20000 or less, preferably 10000 or less.
[0125] The average number of functional groups of the tertiary alcohol component (polyhydric high molecular weight alcohol) is, for example, 2.0 or more. The average number of functional groups of the tertiary alcohol component (polyhydric high molecular weight alcohol) is, for example, 4.0 or less, preferably 3.0 or less, and more preferably 2.5 or less. The average number of functional groups of the tertiary alcohol component is particularly preferably 2.0.
[0126] Examples of the third active energy ray-curable group-containing component include the above-mentioned hydroxy group-containing unsaturated compounds (the hydroxy group-containing unsaturated compounds described above as raw materials for the second curable polyurethane resin). These can be used alone or in combination of two or more types.
[0127] A third curable polyurethane resin is produced by reacting a third polyisocyanate component, a third alcohol component, and a third active energy ray-curable group-containing component. The method for reacting the third polyisocyanate component, the third alcohol component, and the third active energy ray-curable group-containing component is not particularly limited. For example, the third curable polyurethane resin is produced by the same method as the method for producing the second curable polyurethane resin described above.
[0128] The composition (type) and number average molecular weight of the third curable polyurethane resin are not particularly limited and are appropriately selected so that the modulus of elasticity M2 (described below) of the cured second resin will be a desired value.
[0129] For example, the third curable polyurethane resin may be a resin having the same composition (type) as the second curable polyurethane resin, or may be a resin having a different composition (type) from the second curable polyurethane resin.
[0130] The content of the third curable polyurethane resin in the second cured resin is appropriately selected so that the modulus of elasticity M2 (described below) of the second cured resin becomes a desired value.
[0131] For example, the content of the third curable polyurethane resin may be 100% by mass relative to the total amount of the second curable component. That is, the second curable component may consist of the third curable polyurethane resin. Furthermore, from the viewpoint of adjusting the elastic modulus M2 (described below) of the cured second resin, the second curable component may contain the third curable polyurethane resin and another curable resin (described below).
[0132] The content of the third curable polyurethane resin is, for example, more than 0% by mass, preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 20% by mass or more, and particularly preferably 30% by mass or more, relative to the total amount of the second curable component. The content of the third curable polyurethane resin is, for example, 100% by mass or less, preferably 90% by mass or less, more preferably 70% by mass or less, even more preferably 50% by mass or less, and particularly preferably 40% by mass or less, relative to the total amount of the second curable component.
[0133] [Fourth Curable Polyurethane Resin] The second curable component may contain other curable resins as needed. In the second curable component, the other curable resins are curable resins other than the third curable polyurethane resin. Examples of the other curable resins include the fourth curable polyurethane resin.
[0134] The fourth curable polyurethane resin is a polyurethane resin having a different composition (type) from the third curable polyurethane resin. If the second curable component contains the fourth curable polyurethane resin, the mechanical properties of the cured second resin product can be more freely adjusted. Therefore, the second resin composition (molding material) preferably contains the fourth curable polyurethane resin as the second curable component.
[0135] The fourth curable polyurethane resin is a polyurethane resin that can be cured by active energy rays. The fourth curable polyurethane resin contains, for example, a reaction product of a fourth polyisocyanate component, a fourth alcohol component, and a fourth active energy ray-curable group-containing component. Preferably, the fourth curable polyurethane resin is composed of a reaction product of a fourth polyisocyanate component, a fourth alcohol component, and a fourth active energy ray-curable group-containing component.
[0136] Examples of the fourth polyisocyanate component include the above-mentioned polyisocyanate monomer (the monomer described above as the first polyisocyanate component) and the above-mentioned polyisocyanate derivative (the derivative described above as the first polyisocyanate component). These can be used alone or in combination of two or more. As the fourth polyisocyanate component, preferably, a polyisocyanate monomer is used, more preferably, an alicyclic polyisocyanate monomer is used, and even more preferably, bis(isocyanatomethyl)cyclohexane (H 6 XDI).
[0137] The fourth alcohol component is a monohydric high molecular weight alcohol (high molecular weight monool). Examples of the monohydric high molecular weight alcohol include the monohydric high molecular weight alcohols described above (the monohydric high molecular weight alcohols described above as raw materials for the first curable polyurethane resin). These can be used alone or in combination of two or more types.
[0138] The number average molecular weight of the quaternary alcohol component (monohydric high molecular weight alcohol) is, for example, 400 or more, preferably 500 or more, more preferably 1000 or more, and even more preferably 2000 or more. The number average molecular weight of the quaternary alcohol component (monohydric high molecular weight alcohol) is, for example, 20000 or less, preferably 10000 or less. The number average molecular weight can be calculated from the hydroxyl group equivalent and the average number of hydroxyl groups by a known method.
[0139] Examples of the fourth active energy ray-curable group-containing component include the above-mentioned hydroxy group-containing unsaturated compounds (the hydroxy group-containing unsaturated compounds described above as raw materials for the first curable polyurethane resin). These can be used alone or in combination of two or more types.
[0140] A fourth curable polyurethane resin is produced by reacting a fourth polyisocyanate component, a fourth alcohol component, and a fourth active energy ray-curable group-containing component. The method for reacting the fourth polyisocyanate component, the fourth alcohol component, and the fourth active energy ray-curable group-containing component is not particularly limited. For example, the fourth curable polyurethane resin is produced by the same method as the method for producing the first curable polyurethane resin described above.
[0141] The composition (type) and number average molecular weight of the fourth curable polyurethane resin are not particularly limited and are appropriately selected so that the modulus of elasticity M2 (described below) of the cured second resin will be a desired value.
[0142] For example, the fourth curable polyurethane resin may be a resin having the same composition (type) as the first curable polyurethane resin, or may be a resin having a different composition (type) from the first curable polyurethane resin.
[0143] The content of the fourth curable polyurethane resin in the second cured resin is appropriately selected so that the modulus of elasticity M2 (described below) of the second cured resin becomes a desired value.
[0144] For example, the content of the fourth curable polyurethane resin may be, for example, 0% by mass relative to the total amount of the second curable component. That is, the second curable component does not need to contain the fourth curable polyurethane resin. From the viewpoint of adjusting the elastic modulus M2 (described below) of the second resin cured product, the second curable component preferably contains the third curable polyurethane resin and the fourth curable polyurethane resin.
[0145] The content of the fourth curable polyurethane resin relative to the total amount of the second curable component is, for example, 0% by mass or more, preferably 10% by mass or more, more preferably 30% by mass or more, even more preferably 50% by mass or more, and particularly preferably 60% by mass or more. The content of the fourth curable polyurethane resin relative to the total amount of the second curable component is, for example, less than 100% by mass, preferably 95% by mass or less, more preferably 90% by mass or less, even more preferably 80% by mass or less, and particularly preferably 70% by mass or less.
[0146] The content of the fourth curable polyurethane resin is, for example, 0 parts by mass or more, preferably 10 parts by mass or more, more preferably 50 parts by mass or more, and even more preferably 100 parts by mass or more, per 100 parts by mass of the third curable polyurethane resin. The content of the fourth curable polyurethane resin is, for example, 1,000 parts by mass or less, preferably 800 parts by mass or less, more preferably 600 parts by mass or less, and even more preferably 400 parts by mass or less, per 100 parts by mass of the third curable polyurethane resin.
[0147] [Active energy ray cationically curable resin] In the second curable component, the other curable resin is not limited to the fourth curable polyurethane resin. Examples of the other curable resin include the active energy ray cationically curable resin. A preferred example of the active energy ray cationically curable resin is an epoxy resin.
[0148] The composition (type) and content of the active energy ray cationically curable resin are not particularly limited, and are appropriately selected so that the modulus of elasticity M1 (described below) of the second resin cured product becomes a desired value.
[0149] Preferably, the second curable component does not contain an active energy ray cationically curable resin. That is, preferably, the second resin composition (raw material component) does not contain an active energy ray cationically curable resin as the second curable component.
[0150] The content of the active energy ray cationically curable resin is, for example, 0% by mass or more relative to the total amount of the second curable component. The content of the active energy ray cationically curable resin is, for example, less than 100% by mass, preferably 95% by mass or less, more preferably 90% by mass or less, even more preferably 80% by mass or less, and particularly preferably 70% by mass or less relative to the total amount of the second curable component.
[0151] The content of the active energy ray cationically curable resin is, for example, 0 parts by mass or more per 100 parts by mass of the third curable polyurethane resin, and the content of the active energy ray cationically curable resin is, for example, 1,000 parts by mass or less, preferably 800 parts by mass or less, more preferably 600 parts by mass or less, and even more preferably 400 parts by mass or less per 100 parts by mass of the third curable polyurethane resin.
[0152] [Radical Reactive Diluent] The second curable component may further contain the above-mentioned radical reactive diluent. In other words, the second resin composition (molding material) may contain the above-mentioned radical reactive diluent as the second curable component.
[0153] The type and content of the radical reactive diluent are not particularly limited and are appropriately selected so that the modulus of elasticity M2 (described below) of the second cured resin product becomes a desired value.
[0154] Preferably, the second curable component does not contain a radical-reactive diluent, i.e., preferably, the second resin composition does not contain a radical-reactive diluent.
[0155] The content of the radical reactive diluent relative to the total amount of the second curable component is, for example, 0% by mass or more, and for example, less than 100% by mass, preferably 95% by mass or less, more preferably 90% by mass or less, even more preferably 80% by mass or less, and particularly preferably 70% by mass or less, relative to the total amount of the second curable component.
[0156] The content of the radical reactive diluent relative to 100 parts by mass of the third curable polyurethane resin is, for example, 0 parts by mass or more, and the content of the radical reactive diluent relative to 100 parts by mass of the third curable polyurethane resin is, for example, 100 parts by mass or less, preferably 90 parts by mass or less, more preferably 70 parts by mass or less, and even more preferably 50 parts by mass or less.
[0157] (b) Second Additive The second resin composition can optionally contain a second additive. The second resin composition preferably contains a second additive. Examples of the second additive include an active energy ray polymerization initiator, a plasticizer, a thixotropic agent, an antioxidant, an ultraviolet absorber, a fluorescent brightener, an internal mold release agent, a lubricant, a sensitizer, an antiblocking agent, a heat stabilizer, an active energy ray-resistant stabilizer, a light stabilizer, a catalyst, a pigment, a dye, a lubricant, a filler, and a hydrolysis inhibitor. The amount and timing of addition of these additives are appropriately determined depending on the purpose and application.
[0158] The second additive is preferably an active energy ray polymerization initiator. Examples of the active energy ray polymerization initiator include the active energy ray polymerization initiators described above as the first additive.
[0159] The active energy ray polymerization initiator is used in an amount of, for example, 0.1 parts by mass or more, preferably 0.5 parts by mass or more, per 100 parts by mass of the second curable component (total amount), and is used in an amount of, for example, 5.0 parts by mass or less, preferably 1.0 part by mass or less, per 100 parts by mass of the second curable component (total amount).
[0160] In addition, from the viewpoint of adjusting the mechanical properties of the cured second resin product, the second additive preferably contains a thixotropic agent. In addition, from the viewpoint of suppressing deterioration of the cured second resin product over time, the second additive preferably contains an antioxidant.
[0161] Furthermore, from the viewpoint of obtaining excellent molding precision and suppressing changes in mechanical properties and surface tackiness, the second additive preferably does not contain a plasticizer. That is, the second resin composition preferably does not contain a plasticizer.
[0162] In other words, when the second resin composition contains a plasticizer, the mechanical properties of the cured second resin can be easily adjusted, but migration of the plasticizer may occur in the cured composite resin. In contrast, the second resin composition can contain a fourth curable polyurethane resin, so the elastic modulus M2 (MPa) of the cured second resin can be adjusted without relying on a plasticizer. Therefore, the first resin composition preferably does not contain a plasticizer.
[0163] The viscosity of the second resin composition at 25°C is, for example, 0.1 Pa·s or more, preferably 0.3 Pa·s or more, more preferably 0.5 Pa·s or more. The viscosity of the second resin composition at 25°C is, for example, 5.0 Pa·s or less, preferably 3.0 Pa·s or less, more preferably 1.5 Pa·s or less.
[0164] 2. Method for Producing a Cured Composite Resin The first resin composition and the second resin composition are used as molding materials in the following method for producing a cured composite resin. The method for producing a cured composite resin will be described in detail below.
[0165] The method for producing a cured composite resin comprises a first step and a second step. In the first step, a first resin composition is cured with active energy rays to form a cured first resin composition. In the second step, a second resin composition is cured with active energy rays to form a cured second resin composition. Each step is described in detail below.
[0166] 1) First Step The first step includes, for example, a first placement step of placing the first resin composition at an arbitrary position, and a first curing step of irradiating the first resin composition with active energy rays to cure it.
[0167] [First placement step] In the first placement step, the first resin composition is placed at an arbitrary position. The method for placing the first resin composition is not particularly limited, but examples thereof include 3D printing, bar coating, roll coating, and spraying. From the viewpoints of molding accuracy and production efficiency, 3D printing is preferred.
[0168] When a 3D printing method is employed, the first resin composition is disposed at a desired position by a 3D printer. A preferred example of the 3D printer is a dispenser-type 3D printer. The dispenser-type 3D printer includes, for example, a dispenser, a table, and an active energy ray irradiator. The dispenser is a device that dispenses molding materials (the first resin composition and the second resin composition). Examples of the dispenser include an air pump dispenser, an aerojet dispenser, an air pulse dispenser, a gear pump dispenser, and a mechanical dispenser, and preferably, an air pump dispenser and an aerojet dispenser. The table is a base for disposing the molding material at a desired position. The table is not particularly limited, and examples thereof include known platform tables. The active energy ray irradiator is a device that irradiates the molding material with active energy rays. Examples of active energy rays include ultraviolet rays and electron beams.
[0169] When a dispenser-type 3D printer is used, the first resin composition is discharged from the dispenser toward an arbitrary position on the table. That is, the first step preferably includes a step of discharging the first resin composition from the dispenser (first discharging step). The dispenser-type 3D printer can further improve molding accuracy and production efficiency.
[0170] In the first disposing step, the position and amount of the first resin composition are appropriately set depending on the purpose and application.
[0171] [First curing step] In the first curing step, the applied (discharged) first resin composition is irradiated with active energy rays to be cured. The curing conditions are appropriately set depending on the type and amount of the first resin composition. For example, the irradiation amount (integrated light amount) of the active energy rays is, for example, 10 × 10 -3 J / cm 2 More preferably, 15 x 10 -3 J / cm 2The irradiation amount (integrated light amount) of the active energy ray is, for example, 6 J / cm 2 Preferably, 4 J / cm or less 2 In addition, the output of the active energy ray is, for example, 1.0 mW / cm or less. 2 More than 10 mW / cm, preferably 10 mW / cm 2 More preferably, 100 mW / cm 2 In addition, the output of the active energy rays is, for example, 1000 mW / cm 2 The following is the result.
[0172] The curing with active energy rays may be a one-time curing or a divided curing. That is, the first resin composition may be cured by a single irradiation with active energy rays, or may be cured by two or more irradiations with active energy rays. This results in a cured product (cured first resin product) made of the first resin composition.
[0173] After irradiation with active energy rays, the cured first resin product may be aged, if necessary. The aging conditions are not particularly limited, but the temperature is, for example, 10 to 150°C, preferably 10 to 100°C. The humidity is, for example, 20 to 80% RH, preferably 30 to 70% RH. The aging time is, for example, 0.5 to 10 days, preferably 1 to 7 days.
[0174] The elastic modulus M1 of the first cured resin product is smaller than the elastic modulus M2 (described below) of the second cured resin product. More specifically, the elastic modulus M1 of the first cured resin product is, for example, 0.01 MPa or more, preferably 0.1 MPa or more. The elastic modulus M1 of the first cured resin product is, for example, 500 MPa or less, preferably 100 MPa or less.
[0175] The elastic modulus M1 is the tensile storage modulus (E') at 25° C. The tensile storage modulus (E') at 25° C. is measured in accordance with the examples described later.
[0176] 2) Second Step The second step includes, for example, a second placement step of placing the second resin composition at an arbitrary position, and a second curing step of irradiating the second resin composition with active energy rays to cure it.
[0177] [Second Placement Step] In the second placement step, the second resin composition is placed at an arbitrary position. Examples of the method for placing the second resin composition include the methods described above for placing the first resin composition, and preferably, 3D printing.
[0178] When a 3D printing method is employed, the second resin composition is disposed at any position by a 3D printer, similar to the first resin composition. As the 3D printer, a dispenser-type 3D printer is preferably used, and as the dispenser, an air pump-type dispenser or an aerojet-type dispenser is preferably used.
[0179] When a dispenser-type 3D printer is used, the second resin composition is discharged from the dispenser toward an arbitrary position on the table. That is, the second step preferably includes a step of discharging the second resin composition from the dispenser (second discharging step). The dispenser-type 3D printer can further improve molding accuracy and production efficiency.
[0180] In the second disposing step, the position and amount of the second resin composition are appropriately set depending on the purpose and application.
[0181] [Second curing step] In the second curing step, the applied (discharged) first resin composition is irradiated with active energy rays to be cured. The curing conditions are appropriately set depending on the type and amount of the second resin composition. For example, the irradiation amount (integrated light amount) of the active energy rays is, for example, 10 × 10 -3 J / cm 2 More preferably, 15 x 10 -3 J / cm 2 The irradiation amount (integrated light amount) of the active energy ray is, for example, 6 J / cm 2 Preferably, 4 J / cm or less 2In addition, the output of the active energy ray is, for example, 1.0 mW / cm or less. 2 More than 10 mW / cm, preferably 10 mW / cm 2 More preferably, 100 mW / cm 2 In addition, the output of the active energy rays is, for example, 1000 mW / cm 2 The following is the result.
[0182] The curing with active energy rays may be a one-time curing or a divided curing. That is, the second resin composition may be cured by a single irradiation with active energy rays, or may be cured by two or more irradiations with active energy rays. This results in a cured product (cured second resin product) made of the second resin composition.
[0183] After irradiation with active energy rays, the cured second resin product may be aged, if necessary. The aging conditions are not particularly limited, but the temperature conditions are, for example, 10 to 150°C, preferably 10 to 100°C. The humidity conditions are, for example, 20 to 80% RH, preferably 30 to 70% RH. The aging time is, for example, 0.5 to 10 days, preferably 1 to 7 days.
[0184] The elastic modulus M2 of the cured second resin product is greater than the elastic modulus M1 of the cured first resin product. More specifically, the elastic modulus M2 of the cured second resin product is, for example, 0.1 MPa or more, or preferably 1 MPa or more. The elastic modulus M2 of the cured second resin product is, for example, 5000 MPa or less, preferably 2000 MPa or less, or more preferably 1000 MPa or less.
[0185] The elastic modulus M2 is the tensile storage modulus (E') at 25° C. The tensile storage modulus (E') at 25° C. is measured in accordance with the examples described later.
[0186] The first cured resin and the second cured resin have different moduli of elasticity.
[0187] The ratio (M2 / M1) of the elastic modulus M2 (MPa) of the cured second resin product to the elastic modulus M1 (MPa) of the cured first resin product is 10 or more, preferably 15 or more, more preferably 50 or more, and even more preferably 100 or more. In addition, the ratio (M2 / M1) of the elastic modulus M2 (MPa) of the cured second resin product to the elastic modulus M1 (MPa) of the cured first resin product is, for example, 100,000 or less.
[0188] The difference between the modulus of elasticity M2 of the cured second resin product and the modulus of elasticity M1 of the cured first resin product is, for example, 0.1 MPa or more, or preferably 1 MPa or more, and the difference between the modulus of elasticity M2 of the cured second resin product and the modulus of elasticity M1 of the cured first resin product is, for example, 5000 MPa or less, or preferably 1000 MPa or less.
[0189] If the first resin cured product and the second resin cured product have different elastic moduli, various molded products can be designed with a relatively high degree of freedom in various industrial fields described below.
[0190] 3) Curing Method and Curing Order In producing a composite resin cured product, for example, the first and second steps are carried out simultaneously or sequentially. That is, the first resin cured product and the second resin cured product are produced simultaneously or sequentially. The order in which the first and second steps are carried out is not particularly limited.
[0191] For example, as shown in Fig. 1, first, one of the first step and the second step is performed, and then the other of the first step and the second step is performed. Preferably, first, the first step is performed, and then the second step is performed.
[0192] More specifically, in this method, first, as shown in FIG. 1A, a first disposing step (preferably a first discharging step) is carried out. That is, a first resin composition (reference numeral 10 in FIG. 1A) is placed at a desired position in a desired amount. Next, as shown in FIG. 1B, in this method, a first curing step is carried out. That is, the first resin composition is irradiated with active energy rays to cure the first resin composition. As a result, the first step is carried out before the second step, and a first cured resin product (reference numeral 11 in FIG. 1A) is obtained.
[0193] Next, in this method, as shown in FIG. 1C , a second disposing step (preferably a second discharging step) is carried out. That is, a second resin composition (reference numeral 20 in FIG. 1C ) is placed adjacent to the first cured resin. Next, in this method, as shown in FIG. 1D , a second curing step is carried out. That is, the second resin composition is irradiated with active energy rays to cure the second resin composition. In this way, the second step is carried out after the first step, and a second cured resin (reference numeral 21 in FIG. 1D ) is obtained.
[0194] By the above method, a composite resin cured product (reference numeral 1 in FIG. 1D) comprising the first resin cured product and the second resin cured product is obtained.
[0195] Furthermore, if necessary, the first and second steps can be repeated to arrange multiple first and second resin cured products in parallel. The first and second resin cured products can also be stacked in the thickness direction (the vertical direction of the paper). Alternatively, the second step can be performed first, followed by the first step. In such a case, a composite resin cured product comprising a first resin cured product and a second resin cured product can also be obtained.
[0196] As another method, for example, as shown in FIG. 2, the placement (discharge) of the first resin composition and the placement (discharge) of the second resin composition can be carried out sequentially, and the curing of the first resin composition and the curing of the second resin composition can be carried out simultaneously.
[0197] For example, in this method, first, one of the first disposing step and the second disposing step is performed. Next, one of the first disposing step (preferably the first discharging step) and the second disposing step (preferably the second discharging step) is performed in turn. After that, the first curing step and the second curing step are performed simultaneously.
[0198] More specifically, in this method, a first disposing step (preferably a first discharging step) is first carried out as shown in Fig. 2A. That is, a first resin composition (10 in Fig. 2A) is disposed (discharged) at a desired position in a desired amount.
[0199] Next, in this method, a second disposing step (preferably a second discharging step) is performed as shown in Fig. 2B. That is, a second resin composition (reference numeral 20 in Fig. 2B) is disposed (discharged) adjacent to the first resin composition.
[0200] Next, in this method, as shown in Fig. 2C , the first curing step and the second curing step are carried out simultaneously. That is, the first resin composition and the second resin composition are simultaneously irradiated with active energy rays. This cures the first resin composition and the second resin composition, resulting in a first cured resin (reference numeral 11 in Fig. 2C ) and a second cured resin (reference numeral 21 in Fig. 2C ).
[0201] By the above method, a composite resin cured product (reference numeral 1 in FIG. 2C) including the first resin cured product and the second resin cured product is obtained.
[0202] Furthermore, if necessary, the first disposing step (preferably the first discharging step), the second disposing step (preferably the second discharging step), the first curing step, and the second curing step can be repeated to arrange a plurality of first cured resin products and a plurality of second cured resin products in parallel. The first cured resin products and the second cured resin products can also be stacked in the thickness direction (the vertical direction of the paper). Alternatively, the second disposing step (preferably the second discharging step) may be performed first, followed by the first disposing step (preferably the first discharging step). In such a case, a composite resin cured product comprising a first cured resin product and a second cured resin product can also be obtained.
[0203] Alternatively, for example, the disposition (discharge) of the first resin composition and the disposition (discharge) of the second resin composition may be performed simultaneously, and the curing of the first resin composition and the curing of the second resin composition may be performed simultaneously.
[0204] More specifically, in this method, first, as shown in Fig. 3A, a first disposing step (preferably a first discharging step) and a second disposing step (preferably a second discharging step) are simultaneously performed. That is, a first resin composition (reference numeral 10 in Fig. 3A) is disposed (discharged) at a desired position in a desired amount, and simultaneously, a second resin composition (reference numeral 20 in Fig. 3A) is disposed (discharged) adjacent to the first resin composition.
[0205] Next, in this method, the first curing step and the second curing step are carried out simultaneously. That is, the first resin composition and the second resin composition are simultaneously irradiated with active energy rays, and the first resin composition and the second resin composition are cured. This results in a first cured resin (reference numeral 11 in FIG. 3B ) and a second cured resin (reference numeral 21 in FIG. 3B ). As a result, a composite resin cured product is obtained.
[0206] Furthermore, if necessary, the first disposing step (preferably the first dispensing step), the second disposing step (preferably the second dispensing step), the first curing step, and the second curing step can be repeated to arrange a plurality of first cured resin products and a plurality of second cured resin products in parallel. The first cured resin products and the second cured resin products can also be stacked in the thickness direction (the vertical direction of the paper). Alternatively, the second disposing step (preferably the second dispensing step) may be performed first, followed by the first disposing step (preferably the first dispensing step). In such a case, a composite resin cured product comprising a first cured resin product and a second cured resin product can also be obtained.
[0207] 3. Effects In the method for producing a composite resin-cured product described above, the composite resin-cured product comprises a first resin-cured product and a second resin-cured product that are adjacent to each other. The ratio (M2 / M1) of the modulus of elasticity M2 (MPa) of the second resin-cured product to the modulus of elasticity M1 (MPa) of the first resin-cured product is equal to or greater than a predetermined value. In other words, the composite resin-cured product comprises a plurality of resin-cured products that have different moduli of elasticity and are adjacent to each other.
[0208] In the method for producing a cured composite resin, a first cured resin is formed by curing a first cured resin composition. The first resin composition contains a first curable polyurethane resin. The first curable polyurethane resin contains a reaction product of a first polyisocyanate component, a first alcohol component, and a first active energy ray-curable group-containing component. The first alcohol component is a monohydric high-molecular-weight alcohol. This first curable polyurethane resin allows the elastic modulus M1 (MPa) of the cured first resin to be adjusted without relying on a plasticizer.
[0209] Therefore, the above-described method for producing a cured composite resin product can produce a cured composite resin product that has excellent molding precision and is capable of suppressing changes in mechanical properties and surface tack.
[0210] Furthermore, the cured composite resin may be coated with a coating material (coating layer) as needed. The coating material is not particularly limited, and known coating materials can be used. The coating material (coating layer) is formed by applying a known coating composition to the cured composite resin and drying it. Even in this case, the cured composite resin contains a first curable polyurethane resin, and the elastic modulus M1 (MPa) of the cured first resin is adjusted independently of the plasticizer. Therefore, migration of the plasticizer to the coating material can be suppressed, and changes in surface tackiness can be suppressed.
[0211] The present invention also includes a curable resin composition used in the method for producing the composite resin cured product. Examples of the curable resin composition include the first resin composition and the second resin composition, and preferably the first resin composition.
[0212] The curable resin composition is used in the method for producing a cured composite resin product, and therefore, the curable resin composition can produce a cured composite resin product that has excellent molding accuracy and is capable of suppressing changes in mechanical properties and surface tack.
[0213] Therefore, the above-mentioned method for producing a cured composite resin product and the curable resin composition can be suitably used in various industrial fields.
[0214] The cured composite resin product is used, for example, in the field of three-dimensional shaping. That is, the cured composite resin product is preferably a molded article obtained by three-dimensional shaping.
[0215] More specifically, the first resin composition is used as an ink in three-dimensional shaping.
[0216] In other words, the ink contains the first curable polyurethane resin. That is, the ink contains a reaction product of a first polyisocyanate component, the first alcohol component, and the first active energy ray-curable group-containing component. Note that, as described above, the first alcohol component is a monohydric high-molecular-weight alcohol.
[0217] The ink may also contain the second curable polyurethane resin described above. That is, the ink may contain a reaction product of a second polyisocyanate component, a second alcohol component, and a second active energy ray-curable group-containing component. The second alcohol component is, as described above, a polyhydric high-molecular-weight alcohol.
[0218] Such an ink (first ink) is used in combination with another actinic energy ray curable ink (second ink).
[0219] That is, an ink set including the above ink (first ink) and a second ink that is cured by actinic energy rays is used in three-dimensional solid modeling.
[0220] More specifically, the ink set is cured to form a cured product by the same method as the method for producing the cured composite resin product described above. That is, the first ink and the second ink are arranged adjacent to each other by the method described above, and then the first ink and the second ink are cured by the method described above. As a result, a cured product is obtained that has a portion where the first ink is cured and a portion where the second ink is cured.
[0221] The portion where the first ink is cured is the first resin cured product. The elastic modulus of the portion where the first ink is cured is, for example, the same as the elastic modulus M1 (MPa).
[0222] The portion where the second ink is cured is the second resin cured product. The elastic modulus of the portion where the second ink is cured is, for example, the same as the elastic modulus M2 (MPa).
[0223] The ratio of the modulus of elasticity of the portion where the second ink is cured to the modulus of elasticity of the portion where the first ink is cured is the same as the ratio of the moduli of elasticity (M2 / M1) described above.
[0224] The ink, ink set, and cured product described above can achieve excellent molding precision and can suppress changes in mechanical properties and surface tack.
[0225] Next, the present invention will be described based on examples and comparative examples, but the present invention is not limited to the following examples. Note that "parts" and "%" are by mass unless otherwise specified. Furthermore, specific numerical values such as blending ratios (content ratios), physical property values, and parameters used in the following description can be substituted with the upper limit values (numeric values defined as "equal to or less than") or lower limit values (numeric values defined as "equal to or more than" or "exceeding") of the corresponding blending ratios (content ratios), physical property values, and parameters described in the above "Description of the Invention."
[0226] 1. Curable Polyurethane Resin Preparation Example 1 In a nitrogen atmosphere, a glass separable flask was charged with methoxypolyoxyethylene glycol having a number average molecular weight of 10,000 (ML10000, one-end-capped polyoxyethylene glycol (MPEG)) and 1,3-bis(isocyanatomethyl)cyclohexane (1,3-H 6 The amounts of 1,3-bis(isocyanatomethyl)cyclohexane and 1,3-bis(isocyanatomethyl)cyclohexane were adjusted so that the equivalent ratio (NCO / OH) of the isocyanate groups of the methoxypolyoxyethylene glycol (single-end-capped polyoxyethylene glycol) was 8.0.
[0227] Next, the mixture of methoxypolyoxyethylene glycol and 1,3-bis(isocyanatomethyl)cyclohexane was heated to 80°C. Next, a urethanization catalyst (tin(II) ethylhexanoate) was added to the mixture. The amount added was adjusted so that the urethanization catalyst was 10 ppm relative to the mixture. Thereafter, the mixture was reacted at 80°C for 4 hours. This resulted in a crude product containing primary alcohol-modified isocyanate and unreacted 1,3-bis(isocyanatomethyl)cyclohexane. Next, the crude product was subjected to thin-film distillation (160-170°C, 70-100 Pa) to purify the primary alcohol-modified isocyanate.
[0228] Next, the primary alcohol-modified isocyanate and 2-hydroxyethyl acrylate (HEA) were added to the separable flask. The amounts added were adjusted so that the equivalent ratio (NCO / OH) of the isocyanate groups of the primary alcohol-modified isocyanate to the hydroxyl groups of the 2-hydroxyethyl acrylate was 1.0.
[0229] Next, the mixture of primary alcohol-modified isocyanate and 2-hydroxyethyl acrylate was heated to 70°C. Next, a urethane-forming catalyst (tin(II) ethylhexanoate) was added to the mixture. The amount added was adjusted so that the urethane-forming catalyst was 200 ppm relative to the mixture. The mixture was then reacted at 70°C for 4 hours. This resulted in MPEG-modified polyurethane (meth)acrylate 1 (MPEG-UA1). Preparative Example 2: Instead of methoxypolyoxyethylene glycol (ML10000) having a number-average molecular weight of 10,000, methoxypolyoxyethylene glycol (ML3000, one-end-capped polyoxyethylene glycol) having a number-average molecular weight of 3,000 was used. Except for this, MPEG-modified polyurethane (meth)acrylate 2 (MPEG-UA2) was obtained in the same manner as in Preparative Example 1.
[0230] Preparation Example 3 In a nitrogen atmosphere, polyoxypropylene glycol (PPG10000) having a number average molecular weight of 10,000 and 1,3-bis(isocyanatomethyl)cyclohexane (1,3-H 6The amounts of 1,3-bis(isocyanatomethyl)cyclohexane and 1,3-bis(isocyanatomethyl)cyclohexane were adjusted so that the equivalent ratio (NCO / OH) of the isocyanate groups of the methoxypolyoxyethylene glycol (single-end-capped polyoxyethylene glycol) was 8.0.
[0231] Next, the mixture of polyoxypropylene glycol and 1,3-bis(isocyanatomethyl)cyclohexane was heated to 80°C. Next, a urethanization catalyst (tin(II) ethylhexanoate) was added to the mixture. The amount added was adjusted so that the urethanization catalyst was 10 ppm relative to the mixture. Thereafter, the mixture was reacted at 80°C for 4 hours. This resulted in a crude product containing a second isocyanate group-terminated prepolymer and unreacted 1,3-bis(isocyanatomethyl)cyclohexane. Next, the crude product was subjected to thin-film distillation (160 to 170°C, 70 to 100 Pa) to purify the second isocyanate group-terminated prepolymer.
[0232] Next, the second isocyanate group-terminated prepolymer and 2-hydroxyethyl acrylate (HEA) were charged into the separable flask, with the amounts adjusted so that the equivalent ratio (NCO / OH) of the isocyanate groups of the second isocyanate group-terminated prepolymer to the hydroxyl groups of the 2-hydroxyethyl acrylate was 1.0.
[0233] Next, the mixture of the second isocyanate group-terminated prepolymer and 2-hydroxyethyl acrylate was heated to 70°C. Next, a urethane-forming catalyst (tin(II) ethylhexanoate) was added to the mixture. The amount added was adjusted so that the urethane-forming catalyst was 200 ppm relative to the mixture. Thereafter, the mixture was reacted at 70°C for 4 hours. This yielded polyurethane (meth)acrylate 1 (UA1).
[0234] Preparative Example 4 Polyurethane (meth)acrylate 2 (UA2) was obtained in the same manner as in Synthesis Example 3, except that isophorone diisocyanate (IPDI) was used instead of 1,3-bis(isocyanatomethyl)cyclohexane.
[0235] 2. Other Curable Resins Preparation Example 5 (EP) EPICLON HP-4032D (1,6-bis(2,3-epoxypropan-1-yloxy)naphthalene, manufactured by DIC) was prepared as an epoxy resin (EP).
[0236] 3. Composite Resin Cured Product Example 1 1) First Resin Composition The first curable polyurethane resin was the MPEG-modified polyurethane (meth)acrylate 1 (MPEG-UA1) of Preparative Example 1. The second curable polyurethane resin was the polyurethane (meth)acrylate 1 (UA1) of Preparative Example 3.
[0237] Then, 30 parts by mass of curable polyurethane resin 1 (MEPG-UA1), 70 parts by mass of second curable polyurethane resin 1 (UA1), 0.5 parts by mass (phr) of a photopolymerization initiator (TPO, diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, manufactured by Tokyo Chemical Industry Co., Ltd.), 3 parts by mass (phr) of a thixotropic agent (trade name Reolosil HM-30S, dry silica, manufactured by Tokuyama), and 0.1 parts by mass (phr) of an antioxidant (trade name Irganox 245, manufactured by BASF) were mixed and mixed with a grinding mixer to obtain a first resin composition.
[0238] The viscosity of the first resin composition was measured by the following method. That is, an E-type viscometer (product name: TV25 Viscometer, manufactured by Toki Sangyo Co., Ltd.) was used. The rotor number was No. 1, the rotor angle was 1°34′, and the rotor radius was 2.4 cm (the same applies below).
[0239] The viscosity of the first resin composition was in the range of 0.1 Pa·s or more and 5.0 Pa·s or less.
[0240] 2) Second Resin Composition The third curable polyurethane resin was polyurethane (meth)acrylate 1 (UA1) of Preparative Example 3. The fourth curable polyurethane resin was not used.
[0241] Then, 100 parts by mass of the third curable polyurethane resin 1 (UA1), 0.5 parts by mass (phr) of a photopolymerization initiator (TPO, diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, manufactured by Tokyo Chemical Industry Co., Ltd.), 3 parts by mass (phr) of a thixotropic agent (product name Reolosil HM-30S, dry silica, manufactured by Tokuyama), and 0.1 parts by mass (phr) of an antioxidant (product name Irganox 245, manufactured by BASF) were mixed and mixed with a grinding mixer to obtain a second resin composition.
[0242] The viscosity of the second resin composition was measured in the same manner as the viscosity of the first resin composition.
[0243] The viscosity of the second resin composition was in the range of 0.1 Pa·s or more and 5.0 Pa·s or less.
[0244] 3) Cured Composite Resin Product A dispenser-type 3D printer was created by attaching multiple heads and a spot light source (Lightning LC8, manufactured by Hamamatsu Photonics) to a commercially available dispenser machine (SHOTMASTER 500ΩX, manufactured by Musashi Engineering Co., Ltd.).
[0245] Then, using a dispenser-type 3D printer, the first resin composition and the second resin composition were sequentially discharged from the dispenser, thereby causing the first resin composition and the second resin composition to be adjacent to each other.
[0246] The first resin composition and the second resin composition were then irradiated with active energy rays from a spot light source to simultaneously cure the first resin composition and the second resin composition, producing a composite cured resin. More specifically, the first resin composition was cured to obtain a cured first resin. The second resin composition was cured to obtain a cured second resin. The cured first resin and the cured second resin were arranged adjacent to each other so as to be in contact with each other.
[0247] The above-mentioned operation was repeated to laminate the first cured resin and then the second cured resin.
[0248] The output of the active energy rays was 500 mW / cm 2 The cumulative light intensity was 1.5 J / cm 2The output and integrated light amount were measured using an illuminance meter (Ushio Inc. UIT-250 (measurement wavelength 405 nm)).
[0249] The shape and size of the first cured resin product and the shape and size of the second cured resin product were appropriately set according to the evaluations described below.
[0250] Examples 2 to 9 and Comparative Examples 1 to 8 A first resin composition, a second resin composition, and a cured composite resin were produced in the same manner as in Example 1, except for the formulations shown in Tables 1 and 2. The viscosity of each first resin composition was in the range of 0.1 Pa s to 5.0 Pa s. The viscosity of each second resin composition was in the range of 0.1 Pa s to 5.0 Pa s.
[0251] 4. Evaluation 1) Tensile storage modulus of each cured resin product A first cured resin product (10 mm x 5 mm x 2 mm) and a second cured resin product (10 mm x 5 mm x 2 mm) were separately produced using the method described above.
[0252] The cured first resin and the cured second resin were each punched in the thickness direction to prepare samples for measuring dynamic viscoelasticity. The dynamic viscoelasticity spectrum of the cured first resin was measured using a dynamic viscoelasticity measuring device (manufactured by IT Measurement & Control Co., Ltd., model: DVA-220) to determine the tensile storage modulus (M 1 The dynamic viscoelasticity spectrum of the cured second resin was measured using a dynamic viscoelasticity measuring device (manufactured by IT Measurement & Control Co., Ltd., model: DVA-220), and the tensile storage modulus (M 2 The measurement conditions are as follows:
[0253] Measurement temperature -100 to 250°C, heating rate 5°C / min, tension mode, gauge length 20mm, static / dynamic stress ratio 1.8, measurement frequency 10Hz
[0254] The elastic modulus M of the first cured resin 1 (MPa) 2 (MPa) ratio (elastic modulus ratio: M 2 / M 1 ) was calculated. 2 / M 1) was evaluated according to the following criteria.
[0255] ◎: Elastic modulus ratio (M 2 / M 1 ) ≧1000 ◯: Elastic modulus ratio (M 2 / M 1 ) 999-100 △: Elastic modulus ratio (M 2 / M 1 ) 99-10 ×: Elastic modulus ratio (M 2 / M 1 ) ≦9
[0256] 2) Tensile storage modulus of composite resin cured product A composite resin cured product including a first resin cured product (50 mm x 50 mm x 2 mm) and a second resin cured product (50 mm x 50 mm x 2 mm) was produced by the method described above.
[0257] The cured first resin was disposed below the cured second resin, and the cured second resin was disposed above the cured first resin so as to be in contact with (adjacent to) the cured first resin.
[0258] The cured composite resin was punched in the thickness direction to prepare a sample for measuring dynamic viscoelasticity. The dynamic viscoelasticity spectrum of the cured composite resin was measured using a dynamic viscoelasticity measuring device (manufactured by IT Measurement & Control Co., Ltd., model: DVA-220), and the tensile storage modulus was calculated. The measurement conditions are as follows:
[0259] Measurement temperature -100 to 250°C, heating rate 5°C / min, tension mode, gauge length 20mm, static / dynamic stress ratio 1.8, measurement frequency 10Hz
[0260] 3) Change in tensile storage modulus of cured composite resin (change in physical properties) The cured composite resins whose tensile storage modulus had been measured were stored in a constant temperature and humidity chamber (25°C, 50% humidity) for one week. The tensile storage modulus of the cured composite resins after storage was measured under the same conditions.
[0261] The percentage change in the tensile storage modulus of the cured composite resin was calculated from the tensile storage modulus of the cured composite resin before storage and the tensile storage modulus of the cured composite resin after storage using the following formula: Percent change in tensile storage modulus (%) = (tensile storage modulus after storage - tensile storage modulus before storage) / tensile storage modulus before storage
[0262] The rate of change in tensile storage modulus was evaluated according to the following criteria: ∘: The rate of change in tensile storage modulus was 2% or less; Δ: The rate of change in tensile storage modulus was more than 2% and less than 10%; ×: The rate of change in tensile storage modulus was more than 10%.
[0263] 4) Volume Change of the First Resin Cured Product (Molding Precision) A composite resin cured product including a first resin cured product (10 mm x 2 mm x 2 mm) and a second resin cured product (10 mm x 2 mm x 2 mm) was produced using the method described above. The first resin cured product and the second resin cured product were arranged adjacent to each other in the horizontal direction.
[0264] Next, the volumes of the first and second resin cured products contained in the composite resin cured product were measured using a digital caliper (manufactured by Mitutoyo, CD-20APX). The measurement method is described in detail below.
[0265] Specifically, the length, width, and height of the cured composite resin product placed on a flat plate were measured. The length, width, and height of the cured first resin product contained in the cured composite resin product were also measured. Furthermore, the length, width, and height of the cured second resin product contained in the cured composite resin product were also measured. The measurement temperature was 25°C, and the measurement humidity (relative humidity) was 50% RH. The volumes (length x width x height) of the cured first resin product and the cured second resin product contained in the cured composite resin product were then calculated.
[0266] The cured composite resin was then stored in a constant temperature and humidity chamber (25°C, 50% humidity) for one week. After storage, the volumes (length x width x height) of the cured first resin and the cured second resin contained in the cured composite resin were measured using the same method as above.
[0267] The volume change rate of the cured first resin product was calculated from the volume of the cured first resin product before storage and the volume of the cured first resin product after storage using the following formula: Volume change rate (%) = (volume after storage - volume before storage) / volume before storage
[0268] The volume change rate was evaluated according to the following criteria: ◯: The volume change rate was 2% or less; Δ: The volume change rate was more than 2% and less than 10%; ×: The volume change rate was more than 10%.
[0269] 5) Change in surface tackiness of the first cured resin of the composite resin cured product Using the method described above, a composite resin cured product was produced comprising a first cured resin (10 mm x 2 mm x 2 mm) and a second cured resin (10 mm x 2 mm x 2 mm). The first cured resin and the second cured resin were arranged adjacent to each other in the horizontal direction.
[0270] Next, the surface tackiness of the first resin cured product side of the composite resin cured product was evaluated by touching with a finger.
[0271] The cured composite resin products for which surface tackiness had been evaluated were stored in a constant temperature and humidity chamber (25°C, 50% humidity) for one week. After storage, the surface tackiness of the cured first resin side of the cured composite resin products was measured using the same method as above.
[0272] Then, the change in tackiness was confirmed based on the presence or absence of tackiness before and after storage. The change in tackiness was evaluated according to the following criteria: ◯: No change in tackiness before and after storage. ×: Change in tackiness before and after storage.
[0273]
[0274]
[0275] Details of the abbreviations in the table are as follows: 1,3-H 6XDI: 1,3-bis(isocyanatomethyl)cyclohexane, manufactured by Mitsui Chemicals; IPDI: isophorone diisocyanate, trade name VESTANAT IPDI, manufactured by Evonik; MPEG-UA1: MPEG-modified polyurethane (meth)acrylate 1 of Preparative Example 1; MPEG-UA2: MPEG-modified polyurethane (meth)acrylate 2 of Preparative Example 2; UA1: Polyurethane (meth)acrylate 1 of Preparative Example 3; UA2: Polyurethane (meth)acrylate 2 of Preparative Example 4; EP: trade name EPICLON HP-4032D, epoxy resin, 1,6-bis(2,3-epoxypropan-1-yloxy)naphthalene, manufactured by DIC; FX-AO-MA: radical-reactive diluent, 2-(allyloxymethyl)methyl acrylate, a compound having both a (meth)acryloyl group and a vinyl group, manufactured by Nippon Shokubai 4-HBA: radical reactive diluent, 4-hydroxybutyl acrylate, manufactured by Osaka Organic Chemical Industry Co., Ltd. Phthalate ester: DINCH, plasticizer, diisononylcyclohexanedicarboxylate, manufactured by BASF Benzoate ester: Benzoflex 9-98, plasticizer, dipropylene glycol dibenzoate, manufactured by CBC Corporation Olefin: Linearene 168, plasticizer, 1-hexadecene / 1-octadecene, manufactured by Idemitsu Kosan Co., Ltd. TPO: photopolymerization initiator, diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, manufactured by Tokyo Chemical Industry Co., Ltd. Omnirad 184: photopolymerization initiator, 1-hydroxycyclohexyl phenyl ketone, manufactured by IGM resins B.V. BLUESIL PI2074: Photopolymerization initiator, 4-isopropyl-4'-methyldiphenyliodonium tetrakis(pentafluorophenyl)borate, manufactured by Elkem Silicones Rheolosil HM-30S: Thixotropic agent, dry silica, manufactured by Tokuyama AEROSIL RY200S: Thixotropic agent, dry silica, manufactured by Nippon Aerosil Irganox 245: Antioxidant, manufactured by BASF
[0276] Example 10 A polyurethane resin solution as a coating composition was prepared in the following manner.
[0277] That is, in a nitrogen atmosphere, in a reactor equipped with a stirring blade, a thermometer, and a water-cooled condenser, 41.5 parts by mass of polycarbonate diol having a number average molecular weight of 1000 (trade name: ETERNACOLL UH-100, manufactured by UBE), 81.4 parts by mass of polycarbonate diol having a number average molecular weight of 2000 (trade name: ETERNACOLL UH-200, manufactured by UBE), and 31.9 parts by mass of 1,4-bisisocyanatomethylcyclohexane (trade name: FORTIMO, manufactured by Mitsui Chemicals) were mixed and stirred, and reacted at 80°C for 1 hour.
[0278] Next, 0.002 parts by mass of dibutyltin dilaurate (catalyst, manufactured by Wako Pure Chemical Industries, Ltd.) was added to the reactor, and the contents of the reactor were reacted at 80° C. until the isocyanate group content of the contents of the reactor no longer changed, thereby obtaining an isocyanate group-terminated polyurethane prepolymer (hereinafter referred to as prepolymer).
[0279] Next, dehydrated N,N'-dimethylacetamide (organic synthesis grade, manufactured by Wako Pure Chemical Industries, Ltd., abbreviated as DMAC) was added to the prepolymer so that the solid content concentration of the prepolymer became 22% by mass, thereby obtaining a prepolymer solution.
[0280] On the other hand, an amine solution was prepared by mixing 13.5 parts by mass of isophoronediamine, 0.48 parts by mass of diethylamine, and 88 parts by mass of DMAC.
[0281] Next, the amine solution was added dropwise to the prepolymer solution. The rate of addition of the amine solution was adjusted so that the temperature did not exceed 20°C. After the addition of the amine solution was completed, the mixture of the amine solution and the prepolymer solution was reacted at room temperature for 2 hours, and then heated to 50°C and reacted for 1 hour. Then, 0.5 parts by mass of Irganox 245 (a stabilizer, manufactured by Ciba Japan) and 0.4 parts by mass of Tinuvin 234 (a stabilizer, manufactured by Ciba Japan) were added to the reaction product and mixed. Furthermore, DMAC was added to the reaction product to adjust the solids concentration to 20% by mass. This resulted in a polyurethane resin solution as a coating composition.
[0282] Next, the above coating composition (polyurethane resin solution) was applied to the cured composite resin of Example 1 using a paint brush. The cured composite resin with the coating composition applied was then heated in an oven at 80°C for 2 hours. This dried the coating composition, forming a coating material on the surface of the cured composite resin. In other words, a cured composite resin with a coating material was obtained.
[0283] Thereafter, the change in tackiness of the coating material on the surface of the coated cured composite resin product was evaluated using the method described above. As a result, there was no change in the tackiness of the surface of the coating material before and after storage.
[0284] The above invention is provided as an exemplary embodiment of the present invention, but it is merely an example and should not be interpreted as being limiting. Modifications of the present invention that are obvious to those skilled in the art are intended to be included in the scope of the following claims.
[0285] The method for producing a cured composite resin product and the curable resin composition of the present invention are suitable for use in the field of three-dimensional modeling.
[0286] 1 Composite resin cured product 10 First resin composition 11 First resin cured product 20 Second resin composition 21 Second resin cured product
Claims
1. A method for producing a composite resin cured product comprising a first resin cured product and a second resin cured product adjacent to each other, comprising: a first step of curing a first resin composition with active energy rays to form the first resin cured product; and a second step of curing a second resin composition with active energy rays to form the second resin cured product, wherein a ratio (M2 / M1) of an elastic modulus M2 (MPa) of the second resin cured product to an elastic modulus M1 (MPa) of the first resin cured product is 10 or more, the first resin composition contains a first curable polyurethane resin, the first curable polyurethane resin contains a reaction product of a first polyisocyanate component, a first alcohol component, and a first active energy ray-curable group-containing component, and the first alcohol component is a monohydric high molecular weight alcohol.
2. A method for producing a cured composite resin product as described in claim 1, wherein the first resin composition further contains a second curable polyurethane resin, the second curable polyurethane resin containing a reaction product of a second polyisocyanate component, a second alcohol component, and a second active energy ray curable group-containing component, and the second alcohol component is a polyhydric high molecular weight alcohol.
3. A method for producing a composite resin cured product as described in claim 2, wherein the content of the second curable polyurethane resin is 10 mass% or more and 95 mass% or less relative to the total amount of the first curable component.
4. A method for producing a cured composite resin product as described in claim 1, wherein the viscosity of the first resin composition at 25°C is 0.1 Pa·s or more and 5.0 Pa·s or less.
5. A method for producing a cured composite resin product as described in claim 1, wherein the second resin composition further contains a third curable polyurethane resin, the third curable polyurethane resin containing a reaction product of a third polyisocyanate component, a third alcohol component, and a third active energy ray curable group-containing component, and the third alcohol component is a polyhydric high molecular weight alcohol.
6. A method for producing a cured composite resin product as described in claim 1, wherein the second resin composition contains a fourth curable polyurethane resin, the fourth curable polyurethane resin contains a reaction product of a fourth polyisocyanate component, a fourth alcohol component, and a fourth active energy ray curable group-containing component, and the fourth alcohol component is a monohydric high molecular weight alcohol.
7. The method for producing a cured composite resin product according to claim 1, wherein the first resin composition does not contain a plasticizer.
8. A method for producing a composite resin cured product as described in claim 1, wherein the ratio (M2 / M1) of the elastic modulus M2 (MPa) of the second resin cured product to the elastic modulus M1 (MPa) of the first resin cured product is 50 or more.
9. A method for producing a composite resin cured product as described in claim 1, wherein the first step comprises: a first discharging step of discharging the first resin composition from a dispenser; and a first curing step of irradiating the discharged first resin composition with active energy rays to cure it; and the second step comprises: a second discharging step of discharging the second resin composition from a dispenser; and a second curing step of irradiating the discharged second resin composition with active energy rays to cure it.
10. The method for producing a composite resin cured product according to claim 9, wherein in the first step and / or the second step, the dispenser is an air pump type dispenser and / or an aerojet type dispenser.
11. A method for producing a composite resin cured product as described in claim 9, wherein first, one of the first step and the second step is carried out, and then the other of the first step and the second step is carried out.
12. A method for producing a composite resin cured product as described in claim 9, wherein first, one of the first discharging process and the second discharging process is carried out, then the other of the first discharging process and the second discharging process is carried out, and thereafter, the first curing process and the second curing process are carried out simultaneously.
13. A method for producing a composite resin cured product as described in claim 9, wherein first, the first discharging step and the second discharging step are carried out simultaneously, and then, the first curing step and the second curing step are carried out simultaneously.
14. A curable resin composition for use in the method for producing a composite resin cured product described in claim 1, comprising a first curable polyurethane resin, the first curable polyurethane resin comprising a reaction product of a first polyisocyanate component, a first alcohol component, and a first active energy ray curable group-containing component, the first alcohol component being a monohydric high molecular weight alcohol.
15. The curable resin composition according to claim 14, further comprising a second curable polyurethane resin, the second curable polyurethane resin comprising a reaction product of a second polyisocyanate component, a second alcohol component, and a second active energy ray curable group-containing component, the second alcohol component being a polyhydric high molecular weight alcohol.
16. An ink comprising a reaction product of a first polyisocyanate component, a first alcohol component, and a first active energy ray curable group-containing component, the first alcohol component being a monohydric high molecular weight alcohol.
17. An ink set comprising: a first ink containing a reaction product of a first polyisocyanate component, a first alcohol component, and a first active energy ray-curable group-containing component, the first alcohol component being a monohydric high molecular weight alcohol; and a second ink that is cured by active energy rays.
18. The ink set according to claim 17, wherein the first ink further contains a reaction product of a second polyisocyanate component, a second alcohol component, and a second active energy ray curable group-containing component, and the second alcohol component is a polyhydric high molecular weight alcohol.
19. A cured product obtained by curing the ink set according to claim 17.
20. The cured product according to claim 19, wherein in the ink set, a ratio of the elastic modulus of a cured portion of the second ink to the elastic modulus of a cured portion of the first ink is 10 or greater.
Citation Information
Patent Citations
Model material for forming optically shaped article, support material for supporting shape during optical shaping of optically shaped article, and method for manufacturing optically shaped article in inkjet optically shaping method
JP2012111226A
Isocyanate composition and polyurethane composition
JP2020007450A
Curable resin composition, curable resin composition for 3D printer and resin cured product
JP2023131636A
Water-soluble waxy support material for three-dimensional printing applications
JP2023511529A