Thermoplastic resin film and layered film

A thermoplastic resin film with a two-layer structure, featuring a methacrylic resin and a thermoplastic resin layer, addresses the challenge of maintaining surface irregularities during secondary molding, enabling controlled design and consistent appearance in matte resin films.

WO2024214738A1PCT designated stage expired Publication Date: 2024-10-17KURARAY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014528
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-12
Filing Date
2024-04-10
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Conventional methods for producing matte resin films struggle to freely design surface unevenness and maintain it after secondary molding, as the appearance and design are heavily dependent on the size and amount of fine particles, and secondary forming processes like vacuum forming can lead to shape reversion and deterioration of surface irregularities.

Method used

A thermoplastic resin film with a two-layer structure, comprising a methacrylic resin layer with a high glass transition temperature and a thermoplastic resin layer with a lower glass transition temperature, where the ratio of their thicknesses can vary from 1:1 to 1:10, allowing for controlled surface irregularities and maintaining them during secondary molding.

Benefits of technology

The film provides appropriate surface irregularities suitable for various applications and retains the uneven shape effectively after secondary molding, ensuring a consistent matte appearance and design.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014528_17102024_PF_FP_ABST
    Figure JP2024014528_17102024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure provides a thermoplastic resin film that can impart an appropriate surface relief for an application, and can satisfactorily maintain the surface relief shape after secondary molding. A thermoplastic resin film (1) according to the present disclosure has: a first resin layer (21) that comprises a methacrylic resin (composition) (MR); and a second resin layer (22) that comprises a thermoplastic resin (composition) (TR) having a lower glass transition temperature than the methacrylic resin (composition) (MR), wherein when Tg(1) (°C) is the glass transition temperature of the methacrylic resin (composition) (MR) and Tg(2) (°C) is the glass transition temperature of the thermoplastic resin (composition) (TR), Tg(1)≥130 and Tg(1)≥Tg(2)+20, the storage modulus (E') of the first resin layer at a temperature of Tg(2)+20 (°C) is 10 MPa or greater, and the ratio of the thickness of the first resin layer to the thickness of the second resin layer is 1 / 1 to 1 / 10.
Need to check novelty before this filing date? Find Prior Art

Description

Thermoplastic resin films and laminated films

[0001] The present disclosure relates to thermoplastic resin films and laminated films.

[0002] Matte resin films are sometimes used for applications such as interior and exterior parts of automobiles, exterior parts of household electrical appliances, exterior parts of furniture, and wall materials to impart design or decorative properties such as a sense of luxury and depth. Furthermore, depending on the application, printing may be applied to at least one film surface of the matte resin film. Conventional methods for producing matte resin films include a method of forming a film from a resin composition containing a transparent resin and fine particles (Patent Documents 1 to 4), and a method of imparting fine irregularities to the surface of a film using an embossing roll or the like having fine irregularities on the surface during or after film formation of a resin (composition) that does not contain fine particles (Patent Documents 5 and 6).

[0003] Japanese Patent Laid-Open No. 06-073199 Japanese Patent Laid-Open No. 10-237261 Japanese Patent Laid-Open No. 2002-361712 Japanese Patent Laid-Open No. 2009-143174 Japanese Patent Laid-Open No. 2009-202382 Japanese Patent Laid-Open No. 2009-196327

[0004] However, in the methods described in Patent Documents 1 to 4, the surface roughness level and the resulting appearance and design are determined by the size and amount of the fine particles added. Therefore, it is difficult to freely design the surface roughness level and the resulting appearance and design depending on the application, etc. When the matte resin film obtained by the methods described in Patent Documents 5 and 6 is subjected to secondary molding such as vacuum molding, it may return to its original shape due to heating during secondary molding, and the surface roughness level and the resulting appearance and design may be reduced after secondary molding.

[0005] The present disclosure has been made in consideration of the above circumstances, and aims to provide a thermoplastic resin film that can be given appropriate surface irregularities depending on the application, etc., and that can well retain the surface irregularity shape after secondary molding.

[0006] The present disclosure provides the following thermoplastic resin film and laminate film: [1] A thermoplastic resin film having a first resin layer made of a methacrylic resin (composition) (MR) and a second resin layer made of a thermoplastic resin (composition) (TR) having a glass transition temperature lower than that of the methacrylic resin (composition) (MR), wherein, when the glass transition temperature of the methacrylic resin (composition) (MR) is Tg(1) [°C] and the glass transition temperature of the thermoplastic resin (composition) (TR) is Tg(2) [°C], Tg(1) ≧ 130 and Tg(1) ≧ Tg(2) + 20, the storage modulus (E') of the first resin layer at a temperature of Tg(2) + 20 [°C] is 10 MPa or more, and the ratio of the thickness of the first resin layer to the thickness of the second resin layer is 1 / 1 to 1 / 10.

[0007] [2] The thermoplastic resin film according to [1], wherein the storage modulus (E') of the first resin layer of the methacrylic resin (composition) (MR) at a temperature of Tg(2) + 20 ° C. is 3000 MPa or less.

[0008] [3] The thermoplastic resin film of [1] or [2], wherein the methacrylic resin (composition) (MR) contains a methacrylic resin (M-RS) having, in the main chain, one or more ring structural units selected from the group consisting of an acid anhydride unit, an imide unit having a ring structure, and a lactone ring unit. [4] The thermoplastic resin film of [3], wherein the methacrylic resin (composition) (MR) contains a glutarimide resin (MG) containing a methyl methacrylate unit and a glutarimide unit. [5] The thermoplastic resin film of [4], wherein the glutarimide resin (MG) further contains an aromatic vinyl monomer unit. [6] The thermoplastic resin film of [5], wherein the aromatic vinyl monomer unit contains one or more styrene monomer units selected from the group consisting of a styrene unit and an α-methylstyrene unit.

[0009] [7] The thermoplastic resin film according to [6], wherein the glutarimide resin (MG) contains 5 to 73% by mass of methyl methacrylate units, 25 to 70% by mass of glutarimide units represented by the following formula (I), 1 to 48% by mass of α-methylstyrene units, 1 to 48% by mass of one or more units selected from the group consisting of styrene units and maleic anhydride units, and 0 to 20% by mass of unsubstituted or N-substituted maleimide units:

[0010] (In formula (I), two R 1 are each independently a hydrogen atom or a methyl group, and R 2 is a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, or an organic group having 6 to 15 carbon atoms and containing an aromatic ring.

[0011] [8] The thermoplastic resin film of any one of [1] to [7], wherein the methacrylic resin (composition) (MR) has a glass transition temperature of 140° C. or higher. [9] The thermoplastic resin film of any one of [1] to [8], wherein the thermoplastic resin (composition) (TR) is a methacrylic resin composition (T-MR) containing a methacrylic resin (TM) and a rubber-like polymer (R), or a polycarbonate resin composition (T-PC) containing a polycarbonate resin (PC).

[0012]

[10] The thermoplastic resin film according to any one of [1] to [9], wherein one surface of the first resin layer is exposed, and the exposed surface of the first resin layer has a concave-convex surface.

[11] The thermoplastic resin film according to any one of [1] to

[10] , which is a coextrusion molded film.

[0013]

[12] A laminated film having a thermoplastic resin film according to any one of [1] to

[11] and a printed layer formed on the surface of the second resin layer of the thermoplastic resin film opposite to the first resin layer.

[13] A laminated film having a thermoplastic resin film according to any one of [1] to

[11] and a hard coat layer formed on the surface of the first resin layer of the thermoplastic resin film opposite to the second resin layer.

[0014] According to the present disclosure, it is possible to provide a thermoplastic resin film that can be given appropriate surface irregularities depending on the application, etc., and that can well retain the surface irregularity shape after secondary molding.

[0015] Fig. 1 is a schematic cross-sectional view of a thermoplastic resin film according to an embodiment of the present invention. Fig. 2 is a schematic cross-sectional view of a laminate film with a printed layer according to an embodiment of the present invention. Fig. 3 is a schematic cross-sectional view of a laminate film with a hard coat layer according to an embodiment of the present invention. Fig. 4 is a schematic view of a manufacturing apparatus for a thermoplastic resin film according to an embodiment of the present invention.

[0016] Generally, terms such as "film" and "sheet" are used for thin film molded bodies depending on their thickness, but there is no clear distinction between them. In this specification, "film" includes "sheet." Unless otherwise specified, "units" contained in a polymer refer to repeating units contained in the polymer, and are monomer units derived from raw material monomers or derived units derived from one or more monomer units. In this specification, "resin (composition)" is a general term for resins and resin compositions containing one or more resins. In this specification, "(meth)acrylic" is a general term for acrylic and methacrylic, and the same applies to (meth)acrylonitrile, etc. In this specification, unless otherwise specified, "weight average molecular weight (Mw)" is the weight average molecular weight calculated as standard polymethyl methacrylate (PMMA) determined by gel permeation chromatography (GPC). Similarly, "number average molecular weight (Mn)" is the number average molecular weight of standard polymethyl methacrylate (PMMA) determined by GPC.

[0017] [Thermoplastic Resin Film] The thermoplastic resin film of the present disclosure is a laminated film having a first resin layer made of a methacrylic resin (composition) (MR) and a second resin layer made of a thermoplastic resin (composition) (TR) having a glass transition temperature lower than that of the methacrylic resin (composition) (MR). FIG. 1 is a schematic cross-sectional view of a thermoplastic resin film according to one embodiment of the present invention. The thermoplastic resin film 1 of this embodiment is a laminated film with a two-layer structure made of a first resin layer 21 made of a methacrylic resin (composition) (MR) and a second resin layer 22 made of a thermoplastic resin (composition) (TR) having a glass transition temperature lower than that of the methacrylic resin (composition) (MR). The configuration of the thermoplastic resin film can be modified as appropriate. The number of first resin layers may be single or multiple, and the number of second resin layers may be single or multiple. The thermoplastic resin film of the present disclosure can have one or more optional layers other than those described above, as necessary.

[0018] The thermoplastic resin film of the present disclosure may be a surface-textured thermoplastic resin film having at least one surface with irregularities. The surface-textured thermoplastic resin film has a matte appearance and can have design properties such as a luxurious feel and a sense of depth. From the viewpoint of maintaining the irregular shape during secondary molding, it is preferable that one surface of the first resin layer having a high glass transition temperature (Tg) is exposed, and that the exposed surface of this first resin layer is a textured surface.

[0019] The uneven pattern can be designed depending on the application, etc. The depth of the recesses may be uniform or non-uniform. There may be a plurality of recesses of different depths. For example, by forming a plurality of recesses of different depths, patterns such as wood grain and natural leather can be imparted. The unevenness level can be indicated by the maximum height (Rz) measured in accordance with JIS B0601-2001. From the viewpoint of design, the lower limit of the maximum height (Rz) is preferably 1 μm, more preferably 3 μm, and particularly preferably 5 μm. The upper limit of the maximum height (Rz) is preferably 50 μm, more preferably 20 μm, and particularly preferably 10 μm.

[0020] The thermoplastic resin film of the present disclosure may be a colored film or an uncolored film. Examples of coloring methods include a method of adding a pigment and / or a dye to the methacrylic resin (composition) (MR) and / or the thermoplastic resin (composition) (TR) before film formation, and a method of dyeing the thermoplastic resin film by immersing it in a dye dispersion.

[0021] In the thermoplastic resin film of the present disclosure, the glass transition temperature of the methacrylic resin (composition) (MR) is Tg(1) [°C], and the glass transition temperature of the thermoplastic resin (composition) (TR) is Tg(2) [°C]. Tg(1) is 130°C or higher (Tg(1)≧130). The lower limit of Tg(1) is preferably 135°C, more preferably 140°C, and particularly preferably 145°C. The upper limit of Tg(1) is not particularly limited, and is preferably 170°C, more preferably 160°C, and particularly preferably 155°C. When Tg(1) is equal to or higher than the above lower limit, the thermoplastic resin film with surface irregularities of the present disclosure, in which the first resin layer has an irregular surface, is prevented from excessive softening of the first resin layer during secondary molding, and the irregular surface shape can be well maintained after secondary molding.

[0022] Tg(1) is higher than Tg(2), and the difference between Tg(1) and Tg(2) (Tg(1)-Tg(2)) is 20°C or more (i.e., Tg(1)≧Tg(2)+20). The lower limit of Tg(1)-Tg(2) is preferably 25°C, more preferably 30°C. The upper limit of Tg(1)-Tg(2) is not particularly limited, and is, for example, 50°C.

[0023] The storage modulus (E') of the first resin layer at a temperature of Tg(2) + 20°C is 10 MPa or more. The lower limit is preferably 50 MPa, more preferably 100 MPa, even more preferably 150 MPa, even more preferably 200 MPa, even more preferably 250 MPa, even more preferably 300 MPa, even more preferably 350 MPa, even more preferably 400 MPa, particularly preferably 450 MPa, and most preferably 500 MPa. The upper limit is not particularly limited and is, for example, 3000 MPa or 2500 MPa.

[0024] Tg(2)+20°C is a suitable temperature for secondary molding. If Tg(1)≧Tg(2)+20 and the storage modulus (E') of the first resin layer at a temperature of Tg(2)+20°C is 10 MPa or more, the thermoplastic resin film with surface irregularities of the present disclosure, in which the first resin layer has an irregular surface, is prevented from excessive softening of the first resin layer during secondary molding, and the irregular surface shape can be well maintained after secondary molding. In this specification, the "glass transition temperature (Tg)" can be measured in accordance with JIS K7121 by the method described in the "Examples" section below.

[0025] The ratio (t1 / t2) of the thickness (t1) of the first resin layer to the thickness (t2) of the second resin layer is 1 / 1 to 1 / 10. t1 / t2 is preferably 1 / 1.5 to 1 / 8, more preferably 1 / 2 to 1 / 5. When t1 / t2 is within the above range, the thickness of the first resin layer having a high glass transition temperature (Tg) can be sufficiently ensured, and the thermoplastic resin film of the present disclosure can appropriately impart unevenness to the surface of the first resin layer depending on the application, etc. The thermoplastic resin film of the present disclosure also has good post-forming properties and shape retention after post-forming.

[0026] The total thickness of the thermoplastic resin film of the present disclosure is not particularly limited, and from the viewpoint of good appearance and productivity, it is preferably 0.03 to 0.5 mm. The lower limit is more preferably 0.04 mm, particularly preferably 0.05 mm. The upper limit is more preferably 0.4 mm, particularly preferably 0.3 mm. The thickness (t1) of the first resin layer is not particularly limited, and is preferably 3 to 250 μm. The lower limit is more preferably 4 μm, even more preferably 5 μm, particularly preferably 8 μm, and most preferably 10 μm. The upper limit is more preferably 200 μm, even more preferably 150 μm, even more preferably 100 μm, particularly preferably 75 μm, and most preferably 50 μm. If the thickness of the first resin layer is equal to or greater than the above lower limit, it is possible to impart an appropriate surface unevenness depending on the application, and the surface unevenness shape can be well maintained after secondary molding. If the thickness of the first resin layer is equal to or less than the above upper limit, it is possible to achieve good moldability. The thickness (t2) of the second resin layer is not particularly limited, and is preferably 15 to 450 μm. The lower limit is more preferably 20 μm, even more preferably 25 μm, particularly preferably 30 μm, and most preferably 35 μm. The upper limit is more preferably 360 μm, particularly preferably 270 μm, and most preferably 250 μm. If the thickness is within the above range, the second resin layer has good impact resistance and moldability.

[0027] When the thermoplastic resin film of the present disclosure is heated at a temperature of Tg(2) + 20°C, the retention of the maximum height (Rz) of the uneven surface after heating relative to the retention before heating (also referred to as the retention of surface unevenness) measured in accordance with JIS B0601-2001 can be 60 to 100%. The lower limit is preferably 70%, more preferably 80%, particularly preferably 90%, and most preferably 95%. The retention of surface unevenness can be measured by the method described in the Examples section below.

[0028] (First Resin Layer) The first resin layer is made of a methacrylic resin (composition) (MR) containing one or more methacrylic resins (M). The content of the methacrylic resins (M) in the methacrylic resin (composition) (MR) (the total amount when multiple types are used) is preferably 51% by mass or more, more preferably 65% ​​by mass or more, particularly preferably 80% by mass or more, and most preferably 90% by mass or more, and may even be 100% by mass.

[0029] The methacrylic resin (M) is a homopolymer or copolymer containing one or more methacrylic acid ester units and, if necessary, one or more other monomer units. In this specification, known methacrylic acid esters can be used, and specific examples thereof include alkyl methacrylates such as methyl methacrylate (MMA), ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, s-butyl methacrylate, t-butyl methacrylate, pentyl methacrylate, hexyl methacrylate, heptyl methacrylate, 2-ethylhexyl methacrylate, nonyl methacrylate, decyl methacrylate, and dodecyl methacrylate; 1-methylcyclopentyl methacrylate, cyclohexyl methacrylate, cycloheptyl methacrylate, cyclooctyl methacrylate, and tricyclo[5.2.1.0] methacrylate; 2,6 methacrylic acid cycloalkyl esters such as dec-8-yl methacrylate; methacrylic acid aryl esters such as phenyl methacrylate; and methacrylic acid aralkyl esters such as benzyl methacrylate. From the viewpoint of availability, MMA, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, and t-butyl methacrylate are preferred, and MMA is most preferred.

[0030] The content of methacrylic acid ester units in the methacrylic resin (M) (the total amount when multiple types are present) is preferably 90% by mass or more, more preferably 95% by mass or more, particularly preferably 98% by mass or more, and may be 100% by mass. The methacrylic resin (M) preferably contains methyl methacrylate (MMA) units, and the content of MMA units in the methacrylic resin (M) is preferably 80% by mass or more, more preferably 90% by mass or more, particularly preferably 95% by mass or more, and most preferably 98% by mass or more, and may be 100% by mass.

[0031] Examples of other monomers besides methacrylic acid esters include acrylic acid esters; unsaturated carboxylic acids such as (meth)acrylic acid, maleic anhydride, maleic acid, and itaconic acid; olefins such as ethylene, propylene, 1-butene, isobutylene, and 1-octene; conjugated dienes such as butadiene, isoprene, and myrcene; aromatic vinyl monomers such as styrene (St), α-methylstyrene, p-methylstyrene, and m-methylstyrene; (meth)acrylamide, (meth)acrylonitrile; vinyl acetate, vinylpyridine, vinyl ketone, vinyl chloride, vinylidene chloride, and vinylidene fluoride.

[0032] In this specification, known "acrylic esters" can be used, and specific examples include methyl acrylate (MA), ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, s-butyl acrylate, t-butyl acrylate, amyl acrylate, isoamyl acrylate, n-hexyl acrylate, 2-ethylhexyl acrylate, pentadecyl acrylate, dodecyl acrylate, phenyl acrylate, benzyl acrylate, phenoxyethyl acrylate, 2-hydroxyethyl acrylate, 2-ethoxyethyl acrylate, glycidyl acrylate, allyl acrylate, cyclohexyl acrylate, norbornenyl acrylate, and isobornyl acrylate.

[0033] The stereoregularity of the methacrylic resin (M) is not particularly limited. Methacrylic resins having stereoregularity such as isotactic, heterotactic, and syndiotactic may be used. As the methacrylic resin (M), a modified methacrylic resin obtained by modifying a general methacrylic resin (also called a non-modified methacrylic resin) that does not have a ring structure unit in the main chain by introducing a ring structure into the main chain may be used.

[0034] Methacrylic resins that do not have a ring structural unit in the main chain can be produced by (co)polymerizing a monomer (mixture) containing methyl methacrylate (MMA) and, if necessary, one or more other monomers, using a known method. Methods for producing methacrylic resins that have a ring structural unit in the main chain include a method in which a plurality of monomers, including methyl methacrylate (MMA), a monomer having a ring structure, and, if necessary, other monomers, are copolymerized using a known method; and a method in which a methacrylic resin that contains MMA units but does not have a ring structural unit is (co)polymerized using a known method, and then a ring structure is introduced into the main chain to form a ring structural unit. Examples of polymerization methods for methacrylic resins include radical polymerization methods such as suspension polymerization, (continuous) bulk polymerization, solution polymerization, and emulsion polymerization; and anionic polymerization.

[0035] The glass transition temperature Tg(1) of the methacrylic resin (composition) (MR) is 130°C or higher. Therefore, the glass transition temperature (Tg) of the methacrylic resin (M) contained in the methacrylic resin (composition) (MR) is preferably 130°C or higher, more preferably 135°C or higher, particularly preferably 140°C or higher, and most preferably 145°C or higher. The upper limit of the Tg of the methacrylic resin (M) is not particularly limited, and is preferably 170°C, more preferably 160°C, and particularly preferably 155°C.

[0036] Examples of the methacrylic resin (M) having a high Tg of 130°C or higher include a methacrylic resin (M-RS) having, in the main chain, one or more ring structure units selected from the group consisting of an acid anhydride unit, an imide unit having a ring structure, and a lactone ring unit; and a methacrylic resin (M-HS) having a syndiotacticity (rr) (also referred to as the rr ratio) expressed in triad notation of 56% or higher.

[0037] <Methacrylic Resin Having a Ring Structure Unit (M-RS)> The methacrylic resin (M-RS) is a methacrylic resin containing, in its main chain, a methyl methacrylate (MMA) unit and one or more ring structure units selected from the group consisting of an acid anhydride unit, an imide unit having a ring structure, and a lactone ring unit, and optionally containing one or more other units. Examples of the acid anhydride unit include a maleic anhydride unit and a glutaric anhydride unit. Examples of the imide unit having a ring structure include an unsubstituted or N-substituted glutarimide unit and an unsubstituted or N-substituted maleimide unit, with an unsubstituted or N-substituted glutarimide unit being preferred.

[0038] A preferred methacrylic resin (M-RS) is a glutarimide resin (MG) containing a methyl methacrylate (MMA) unit and a glutarimide (GI) unit. The glutarimide (GI) unit is a unit having an unsubstituted or N-substituted 2,6-dioxopiperidinediyl structure, and includes a unit represented by the following general formula (I) (also referred to as a glutarimide unit (I)):

[0039]

[0040] In formula (I), two R 1 are each independently a hydrogen atom or a methyl group, and two R 1 Preferably, both R are methyl groups. 2 represents a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, or an organic group having 6 to 15 carbon atoms and containing an aromatic ring, and is preferably a methyl group, an n-butyl group, a cyclohexyl group, or a benzyl group, more preferably a methyl group, an n-butyl group, or a benzyl group, and particularly preferably a methyl group.

[0041] Glutarimide resin (MG) has properties such as a high glass transition temperature (Tg), good impact resistance, good dimensional and shape stability against temperature, and high surface wetting tension. A first resin layer containing glutarimide resin (MG) can provide appropriate surface irregularities depending on the application, and can maintain the surface irregularities well after secondary molding. Depending on the application, a coating layer such as a hard coat layer may be formed on the first resin layer. Because the first resin layer containing glutarimide resin (MG) has a high glass transition temperature (Tg) and good dimensional stability against temperature, when a coating layer is formed thereon, even if it is exposed to high temperatures during drying and curing processes, the occurrence of poor appearance such as warping or curling is suppressed. Because the first resin layer containing glutarimide resin (MG) has high surface wetting tension, a coating layer can be formed thereon with good adhesion.

[0042] The glutarimide resin (MG) may contain one or more copolymerizable vinyl monomer units other than methyl methacrylate (MMA) units and glutarimide (GI) units, as necessary. From the viewpoint of heat resistance, thermal stability, etc., the vinyl monomer unit is preferably one or more selected from the group consisting of (meth)acrylic acid ester units other than methyl methacrylate (MMA) units, aromatic vinyl monomer units, and vinyl cyanide monomer units, and among these, aromatic vinyl monomer units are preferred.

[0043] Examples of (meth)acrylic acid esters other than MMA include methyl acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, s-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, benzyl (meth)acrylate, cyclohexyl (meth)acrylate, and phenyl (meth)acrylate. Among these, methyl acrylate, ethyl (meth)acrylate, and n-butyl (meth)acrylate are preferred, with methyl acrylate and ethyl (meth)acrylate being more preferred. The content of (meth)acrylic acid ester units other than MMA units in the glutarimide resin (MG) (the total amount when multiple types are present) is preferably 20% by mass or less, and more preferably 10% by mass or less, from the viewpoint of heat resistance and thermal stability.

[0044] Examples of aromatic vinyl monomers include styrene (St), α-methylstyrene (αMSt), o-, m-, or p-methylstyrene, 2,4-dimethylstyrene, 2,5-dimethylstyrene, 3,4-dimethylstyrene, 3,5-dimethylstyrene, o-, m-, or p-ethylstyrene, p-t-butylstyrene, 1-vinylnaphthalene, 2-vinylnaphthalene, 1,1-diphenylethylene, isopropenyltoluene, isopropenylethylbenzene, isopropenylpropylbenzene, isopropenylpropylbenzene, isopropenylbutylbenzene, isopropenylbenzylbenzene, isopropenylhexylbenzene, and isopropenyloctylbenzene. Among these, styrene (St), α-methylstyrene, and p-methylstyrene are preferred, with styrene (St) and α-methylstyrene being more preferred, and α-methylstyrene being particularly preferred from the viewpoints of productivity and heat resistance. The content of aromatic vinyl monomer units in the glutarimide resin (MG) (the total amount when multiple types are contained) is preferably 40% by mass or less, more preferably 30% by mass or less, and particularly preferably 25% by mass or less, from the viewpoints of heat resistance and thermal stability.

[0045] Examples of vinyl cyanide monomers include (meth)acrylonitrile and vinylidene cyanide. Among them, acrylonitrile is preferred from the viewpoints of availability and chemical resistance. The content of vinyl cyanide monomer units in the glutarimide resin (MG) (the total amount when multiple types are used) is preferably 20% by mass or less, more preferably 10% by mass or less, from the viewpoints of heat resistance and thermal stability.

[0046] The glutarimide resin (MG) may contain one or more vinyl-based monomer units other than those mentioned above. Examples of the vinyl-based monomer other than those mentioned above include amides such as (meth)acrylamide; various polyfunctional monomers; and the like. From the viewpoint of heat resistance and thermal stability, the content (total amount in the case of multiple types) of vinyl-based monomer units other than (meth)acrylic acid ester units, aromatic vinyl monomer units, and vinyl cyanide monomer units in the glutarimide resin (MG) is preferably 20% by mass or less, more preferably 10% by mass or less.

[0047] The weight average molecular weight (Mw) of the glutarimide resin (MG) is preferably 40,000 to 250,000. The lower limit is more preferably 50,000, particularly preferably 55,000, and most preferably 60,000. The upper limit is more preferably 200,000, particularly preferably 180,000. When Mw is equal to or greater than the lower limit, the impact resistance and other properties of the first resin layer are good. When Mw is equal to or less than the upper limit, the melt flowability and moldability of the glutarimide resin (MG) are good.

[0048] The glutarimide resin (MG) is preferably a glutarimide resin (MGa) containing 5 to 73 mass% of methyl methacrylate (MMA) units, 25 to 70 mass% of glutarimide units represented by the above formula (I), 1 to 48 mass% of α-methylstyrene units, and 1 to 48 mass% of one or more units selected from the group consisting of styrene units and maleic anhydride units.

[0049] From the viewpoints of transparency and thermal decomposition resistance, the content of methyl methacrylate (MMA) units in the glutarimide resin (MGa) is 5 to 73 mass%. The lower limit is preferably 6 mass%, more preferably 10 mass%, particularly preferably 15 mass%, and most preferably 20 mass%. The upper limit is preferably 70 mass%, more preferably 60 mass%, and particularly preferably 50 mass%.

[0050] From the viewpoints of the heat resistance, thermal decomposition resistance, low water absorption, and moldability of the glutarimide resin, the content of the glutarimide unit (I) in the glutarimide resin (MGa) is 25 to 70 mass%. The lower limit is preferably 30 mass%, more preferably 35 mass%, particularly preferably 40 mass%, and most preferably 50 mass%. The upper limit is preferably 68 mass%, more preferably 65 mass%, and particularly preferably 60 mass%.

[0051] From the viewpoints of the heat resistance, rigidity, thermal decomposition resistance, productivity (polymerizability) of the glutarimide resin, and suppression of inhibition of the glutarimidation reaction in the production process of the glutarimide resin, the content of α-methylstyrene units in the glutarimide resin (MGa) is 1 to 48 mass%. The lower limit is preferably 3 mass%, more preferably 5 mass%, particularly preferably 7 mass%, and most preferably 10 mass%. The upper limit is preferably 40 mass%, more preferably 35 mass%, particularly preferably 30 mass%, and most preferably 20 mass%.

[0052] From the viewpoints of the heat resistance, thermal decomposition resistance, and melt fluidity of the glutarimide resin, and of suppressing inhibition of the glutarimidation reaction in the production process of the glutarimide resin, the content of styrene units and maleic anhydride units (total amount when multiple types are present) in the glutarimide resin (MGa) is 1 to 48 mass%. The lower limit is preferably 3 mass%, more preferably 5 mass%, and particularly preferably 7 mass%. The upper limit is preferably 40 mass%, more preferably 35 mass%, particularly preferably 30 mass%, and most preferably 20 mass%. From the viewpoint of productivity, it is preferable that the glutarimide resin (MGa) contains at least styrene units among the styrene units and maleic anhydride units.

[0053] From the viewpoint of suppressing inhibition of the glutarimidation reaction in the production process of the glutarimide resin, the total content of α-methylstyrene units and styrene units in the glutarimide resin (MGa) is preferably 2 to 40 mass%. The lower limit is more preferably 5 mass%, particularly preferably 10 mass%. The upper limit is more preferably 35 mass%, particularly preferably 30 mass%. Since the glutarimide resin has a good balance between heat resistance and low water absorption and the resulting film has good dimensional stability, the ratio of the content of α-methylstyrene units to 100 parts by mass of the total content of α-methylstyrene units and styrene units in the glutarimide resin (MGa) is preferably 30 to 95 parts by mass, more preferably 35 to 90 parts by mass, particularly preferably 40 to 85 parts by mass.

[0054] The glutarimide resin (MG) can be produced by known methods described in WO 2005 / 108438, JP 2010-254742 A, JP 2008-273140 A, and JP 2008-274187 A, etc.

[0055] A first production method includes an imide cyclization reaction step in which an imidization agent is added to a precursor resin having two adjacent methyl methacrylate (MMA) units and reacted with the precursor resin. Examples of the imidization agent include ammonia; aliphatic hydrocarbon group-containing amines such as methylamine (also referred to as monomethylamine), ethylamine, diethylamine, n-propylamine, isopropylamine, n-butylamine, isobutylamine, t-butylamine, and n-hexylamine; aromatic hydrocarbon group-containing amines such as aniline, toluidine, trichloroaniline, and n-methylbenzylamine; alicyclic hydrocarbon group-containing amines such as cyclohexylamine and n-methylcyclohexylamine; and urea compounds such as urea, 1,3-dimethylurea, 1,3-diethylurea, and 1,3-dipropylurea. Among these, methylamine is preferred.

[0056] In the imide cyclization reaction step, some of the methyl methacrylate (MMA) units may be hydrolyzed to form carboxy groups. In this case, it is preferable to return the carboxy groups to the original methyl methacrylate (MMA) units by an esterification reaction using a known esterifying agent. Examples of the esterifying agent include dimethyl carbonate and trimethyl acetate. In this reaction, a tertiary amine such as trimethylamine, triethylamine, or tributylamine may be used in combination as a catalyst.

[0057] In the second production method, a precursor resin having an acid anhydride unit (glutaric anhydride unit) represented by the following formula (IIa) is reacted with a compound represented by the general formula R 2 NH 2 and reacting the compound by adding an imidizing agent represented by the following formula:

[0058] (In the formula, R 1 , R 2 is as defined above.)

[0059] In the first and second production methods, the reaction between the precursor resin and the imidizing agent can be carried out in a continuous manner, in which the precursor resin is melted using an extruder or the like, and the imidizing agent is added to the melt to carry out the reaction, or in a batch manner, in which a precursor resin solution is prepared using a solvent that can dissolve the precursor resin but is non-reactive with the imidization reaction, and the imidizing agent is added to the melt to carry out the reaction.

[0060] A third production method includes a method including a step of intramolecular cyclization of a copolymer having a unit represented by the following formula (III): In this method, it is preferable to carry out the reaction under heating at an appropriate temperature in order to promote the intramolecular cyclization reaction.

[0061] (In the formula, R 1 , R 2 is as defined above. Me represents a methyl group.

[0062] The glutarimide resin (MGa) may further contain 0 to 20 mass % of unsubstituted or N-substituted maleimide units, which are units having an unsubstituted or N-substituted 2,5-pyrrolidinedione structure, such as units represented by the following formula (IV) (also referred to as maleimide units (IV)):

[0063]

[0064] In formula (IV), two R 11 are each independently a hydrogen atom or a methyl group, and two R 11 Preferably, both R are methyl groups. 12 represents a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, or an organic group having 6 to 15 carbon atoms and containing an aromatic ring, and is preferably a methyl group, an n-butyl group, a cyclohexyl group, or a benzyl group, more preferably a methyl group, an n-butyl group, or a benzyl group, and particularly preferably a methyl group.

[0065] Examples of methods for producing methacrylic resins containing maleimide units include a method of polymerizing a monomer mixture containing a monomer containing a maleimide unit, and a method of reacting maleic anhydride units in a polymerization reaction product of a monomer mixture containing maleic anhydride with an imidizing agent. For the latter method, see JP-B Nos. 61-026924, 7-042332, 9-100322, and 2001-329021.

[0066] The lactone ring unit that can be contained in the methacrylic resin (M-RS) is a unit containing a >CH-O-C(=O)- group in the ring structure. The unit containing a >CH-O-C(=O)- group in the ring structure preferably has 4 to 8, more preferably 5 to 6, and most preferably 6, ring constituent elements. Examples of units containing a >CH-O-C(=O)- group in the ring structure include lactone diyl units such as β-propiolactone diyl unit, γ-butyrolactone diyl unit, and δ-valerolactone diyl unit. Note that ">C" in the formula means that the carbon atom C has two bonds.

[0067] For example, the δ-valerolactonediyl unit includes a unit represented by the following formula (V) (also referred to as a lactone ring unit (V)).

[0068] In formula (V), R 21 , R 22 , and R 23 are each independently a hydrogen atom or an organic group having 1 to 20 carbon atoms, preferably a hydrogen atom or an organic group having 1 to 10 carbon atoms, more preferably a hydrogen atom or an organic group having 1 to 5 carbon atoms. Here, the organic group is not particularly limited as long as it has 1 to 20 carbon atoms, and examples thereof include a linear or branched alkyl group, a linear or branched aryl group, -OCOCH 3 The organic group may contain a heteroatom such as an oxygen atom. 22 is a methyl group, and R 21 and R 23 is a hydrogen atom.

[0069] The lactone ring unit can be obtained by intramolecular cyclization of a hydroxy group and an ester group, for example, by intramolecular cyclization of a 2-(hydroxyalkyl)acrylate unit and a methyl (meth)acrylate unit (see JP-A Nos. 2000-230016, 2001-151814, 2002-120326, 2002-254544, and 2005-146084).

[0070] The glutaric anhydride unit that can be contained in the methacrylic resin (M-RS) is a unit having a 2,6-dioxodihydropyrandiyl structure, and examples thereof include a unit represented by formula (VI) (also referred to as a glutaric anhydride unit (VI)).

[0071]

[0072] In formula (VI), two R 31 are each independently a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, and are preferably a methyl group.

[0073] The glutaric anhydride unit can be obtained by intramolecular cyclization of two adjacent (meth)acrylic acid units, or intramolecular cyclization of a (meth)acrylic acid unit and a methyl (meth)acrylate unit, etc. See JP-A-2007-197703 and JP-A-2010-96919, etc.

[0074] <Methacrylic Resin (M-HS)> The methacrylic resin (M-HS) is a methacrylic resin having a syndiotacticity (rr) (rr ratio) expressed in triad notation of 56% or more. The lower limit of the rr ratio is preferably 57%, more preferably 58%. From the viewpoints of moldability and surface hardness, the upper limit of the rr ratio is preferably 99%, more preferably 95%, particularly preferably 90%, and most preferably 85%. A methacrylic resin (composition) (MR) containing the methacrylic resin (M-HS) has a high glass transition temperature (Tg) and excellent heat resistance.

[0075] Here, the syndiotacticity (rr) of the triad notation is the proportion of two chains (diads) in a chain of three consecutive units (triads) that are both racemo (denoted as rr). Note that in the chains of units (diads) in the polymer molecule, those with the same configuration are called meso, and those with the opposite configuration are called racemo, and are denoted as m and r, respectively. The rr ratio of a methacrylic resin is determined in deuterated chloroform at 30°C, 1 A H-NMR spectrum is measured, and from the spectrum, the area (Y) of the region from 0.6 to 0.95 ppm and the area (Z) of the region from 0.6 to 1.35 ppm are measured when tetramethylsilane (TMS) is set to 0 ppm, and the chromaticity can be calculated using the formula: (Y / Z) × 100.

[0076] The weight average molecular weight (Mw) of the methacrylic resin (M-HS) is preferably 40,000 to 500,000. The lower limit is more preferably 50,000, even more preferably 55,000, particularly preferably 60,000, and most preferably 80,000. The upper limit is more preferably 300,000, particularly preferably 200,000. When Mw is equal to or greater than the lower limit, the impact resistance and other properties of the first resin layer are good. When Mw is equal to or less than the upper limit, the melt flowability and moldability of the methacrylic resin (M-HS) are good.

[0077] The melt flow rate (MFR) of the methacrylic resin (composition) (MR) is not particularly limited, but is preferably 1 to 30 g / 10 min. The lower limit of MFR is more preferably 1.5 g / 10 min, even more preferably 2 g / 10 min, particularly preferably 3 g / 10 min, and most preferably 5 g / 10 min. The upper limit of MFR is more preferably 25 g / 10 min, even more preferably 20 g / 10 min, particularly preferably 15 g / 10 min or less, and most preferably 10 g / 10 min. An MFR within the above range provides good stability in hot melt molding. Unless otherwise specified herein, the MFR of the methacrylic resin (composition) is a value measured in accordance with JIS K7210 using a melt indexer at a temperature of 230°C under a load of 3.8 kg.

[0078] The methacrylic resin (composition) (MR) may contain one or more polymers other than the methacrylic resin (M). Other polymers include polyolefin-based resins such as polyethylene, polypropylene, polybutene-1, poly-4-methylpentene-1, and polynorbornene; styrene-based resins such as polystyrene, high-impact polystyrene, methyl methacrylate-styrene copolymer (MS resin), styrene-maleic anhydride copolymer (SMA resin), styrene-maleic anhydride-methyl methacrylate copolymer (SMM resin), acrylonitrile-styrene copolymer (AS resin), acrylonitrile-butadiene-styrene (ABS) resin, acrylonitrile-ethylene-propylene-diene-styrene (AES) resin, acrylic-acrylonitrile-styrene (AAS) resin, acrylonitrile-chlorinated ethylene-styrene (ACS) resin, and methacrylic butadiene styrene (MBS) resin; polyester-based resins such as polyethylene terephthalate and polybutylene terephthalate; polyamide-based resins such as nylon 6, nylon 66, and polyamide elastomer; and polycarbonate-based resins. Resins; other thermoplastic resins such as polyphenylene sulfide, polyether ether ketone, polysulfone, polyphenylene oxide, polyimide, polyetherimide, polyvinyl chloride, polyvinylidene chloride, polyvinylidene fluoride, polyvinyl alcohol, ethylene-vinyl alcohol copolymer, polyacetal, ethylene-vinyl acetate copolymer, phenoxy resin, and ethylene-based ionomer; thermosetting resins such as phenolic resin, melamine resin, silicone resin, and epoxy resin; polyurethane and chlorinated polyurethane resin; modified polyphenylene ether; silicone-modified resin; acrylic rubber, silicone rubber; acrylic rubber, silicone rubber; acrylic thermoplastic elastomers such as diblock copolymers and triblock copolymers of methyl methacrylate polymer block-n-butyl acrylate polymer block; styrene thermoplastic elastomers such as SEPS, SEBS, and SIS; and olefin-based rubbers such as IR, EPR, and EPDM.The amount of other polymers (total amount when multiple types are used) in the methacrylic resin (composition) (MR) is preferably 10% by mass or less, more preferably 5% by mass or less, and most preferably 0% by mass.

[0079] The methacrylic resin (composition) (MR) may contain one or more types of fine particles (P), also known as matting agents or light diffusing agents. The fine particles (P) may be inorganic or organic. Examples of the fine particles (P) include inorganic particles such as calcium carbonate, magnesium carbonate, barium sulfate, titanium oxide, magnesium oxide, zinc oxide, zirconium oxide, aluminum oxide, aluminum hydroxide, silica (silicon dioxide), calcined calcium silicate, calcined kaolin, hydrated calcium silicate, aluminum silicate, magnesium silicate, calcium phosphate, glass, talc, clay, mica, carbon black, and white carbon; and resin particles such as crosslinked styrene-based resin particles, high-molecular-weight styrene-based resin particles, and crosslinked siloxane-based resin particles. The fine particles (P) may be particles obtained by surface-treating the above-mentioned exemplary particles with a fatty acid or the like. The content of the fine particles (P) in the methacrylic resin (composition) (MR) (the total amount when multiple types are used) is preferably 3% by mass or less, more preferably 1.5% by mass or less.

[0080] The methacrylic resin (composition) (MR) may contain one or more additives other than those described above, as needed, such as antioxidants, heat deterioration inhibitors, ultraviolet absorbers, plasticizers, light stabilizers, lubricants, mold release agents, polymer processing aids, antistatic agents, flame retardants, dyes, pigments, organic dyes, impact resistance modifiers, and fluorescent materials.

[0081] The timing of adding the additives is optional, such as during or after polymerization of the methacrylic resin (M), during preparation of the methacrylic resin (composition) (MR), etc. The content of the additives in the methacrylic resin (composition) (MR) (the total amount when multiple types of additives are used) is preferably 7% by mass or less, more preferably 5% by mass or less, and particularly preferably 4% by mass or less, from the viewpoint of suppressing defective appearance.

[0082] The method for preparing the methacrylic resin (composition) (MR) is not particularly limited. One type of methacrylic resin (M) (preferably, glutarimide resin (MG) and methacrylic resin (M-HS)) produced by a known method or commercially available can be used as the methacrylic resin (composition) (MR) as is. Multiple materials including a methacrylic resin (M) (preferably, glutarimide resin (MG) and methacrylic resin (M-HS)) produced by a known method or commercially available can be mixed and / or kneaded to form the methacrylic resin (composition) (MR). The blending procedure for multiple materials can be designed as appropriate. Mixing or kneading can be performed using a mixing or kneading device such as a kneader-ruder, extruder, mixing roll, or Banbury mixer. Among these, a twin-screw extruder is preferred.

[0083] The first resin layer containing the methacrylic resin (M) can have good surface hardness. The surface hardness can be measured using pencil hardness as an index. The pencil hardness of the surface of the first resin layer is preferably B or higher, more preferably HB or higher, particularly preferably F or higher, and most preferably H or higher. The pencil hardness can be measured by the method described in the Examples section below.

[0084] (Second Resin Layer) The second resin layer is made of a thermoplastic resin (composition) (TR) having a glass transition temperature lower than that of the methacrylic resin (composition) (MR). The thermoplastic resin (composition) (TR) contains one or more thermoplastic resins (T). Known thermoplastic resins can be used as the thermoplastic resin (T). The thermoplastic resin (T) may be a general-purpose resin or a so-called engineering plastic. The thermoplastic resin (T) may be a non-rubber polymer (NR) or a rubber polymer (R).

[0085] Non-rubber polymers (NR) include methacrylic resins (TM); polycarbonate resins (PC); polyolefin resins such as polyethylene, polypropylene, polybutene-1, poly-4-methylpentene-1, and polynorbornene; polystyrene, high-impact polystyrene, methyl methacrylate-styrene copolymers (MS resins), styrene-maleic anhydride copolymers (SMA resins), styrene-maleic anhydride-methyl methacrylate copolymers (SMM resins), acrylonitrile-styrene copolymers (AS resins), acrylonitrile-butadiene-styrene (ABS) resins, acrylonitrile-ethylene-propylene-diene-styrene (AES) resins, acrylic-acrylonitrile- Examples of suitable thermoplastic resins include styrene-based resins such as styrene (AAS) resin, acrylonitrile-chlorinated ethylene-styrene (ACS) resin, and methacrylic butadiene styrene (MBS) resin; polyester-based resins such as polyethylene terephthalate and polybutylene terephthalate; polyamide-based resins such as nylon 6 and nylon 66; and other thermoplastic resins such as polyphenylene sulfide, polyether ether ketone, polysulfone, polyphenylene oxide, polyimide, polyetherimide, polyvinyl chloride, polyvinylidene chloride, polyvinylidene fluoride, polyvinyl alcohol, ethylene-vinyl alcohol copolymer, polyacetal, ethylene-vinyl acetate copolymer, and phenoxy-based resin.

[0086] Examples of the rubbery polymer (R) include styrene-based thermoplastic elastomers such as SEPS, SEBS, and SIS; olefin-based rubbers such as IR, EPR, and EPDM; acrylic-based thermoplastic elastomers; vinyl chloride-based thermoplastic elastomers; urethane-based thermoplastic elastomers; ester-based thermoplastic elastomers; amide-based thermoplastic elastomers; ionomer-based resins; styrene-butadiene block copolymers; ethylene-propylene rubber; butadiene-based resins; acrylic rubbers; silicone rubbers; and acrylic multilayer structure polymers.

[0087] From the viewpoints of transparency and moldability, the thermoplastic resin (T) preferably contains one or more thermoplastic resins selected from the group consisting of methacrylic resins (TM), polycarbonate resins (PC), polycyclic olefin resins, and styrene resins, and more preferably contains a methacrylic resin (TM) or a polycarbonate resin (PC).

[0088] The glass transition temperature (Tg(2)) of the thermoplastic resin (composition) (TR) is preferably 145°C or lower, more preferably 140°C or lower, even more preferably 130°C or lower, even more preferably 125°C or lower, even more preferably 120°C or lower, particularly preferably 115°C or lower, and most preferably 110°C or lower. When Tg(2) is equal to or lower than the upper limit, it is easy to design a combination of the methacrylic resin (composition) (MR) and the thermoplastic resin (composition) (TR) that satisfies Tg(1) ≥ 130 and Tg(1) ≥ Tg(2) + 20, and the thermoplastic resin film of the present disclosure can be appropriately post-molded at a relatively low temperature. As a result, the thermoplastic resin film with surface irregularities of the present disclosure, in which the first resin layer has a textured surface, is prevented from excessive softening of the first resin layer during post-molding, and the surface irregularities can be well maintained after post-molding.

[0089] From the viewpoint of impact resistance and the like, the thermoplastic resin (composition) (TR) is preferably a methacrylic resin composition (T-MR) containing a methacrylic resin (TM) and a rubber-like polymer (R); a polycarbonate resin composition (T-PC) containing a polycarbonate resin; or the like.

[0090] <Methacrylic Resin Composition (T-MR)> The methacrylic resin composition (T-MR) contains one or more methacrylic resins (TM) and one or more rubbery polymers (R). The methacrylic resin composition (T-MR) containing the rubbery polymer (R) is excellent in impact resistance, surface hardness, etc. From the viewpoint of impact resistance, surface hardness, etc., the methacrylic resin composition (T-MR) preferably contains 1 to 99 parts by mass of the methacrylic resin (TM) and 99 to 1 part by mass of the rubbery polymer (R), and more preferably contains 10 to 90 parts by mass of the methacrylic resin (TM) and 90 to 10 parts by mass of the rubbery polymer (R).

[0091] The preferred embodiments, specific examples, and production methods of the methacrylic resin (TM) are the same as those of the methacrylic resin (M). Commercially available methacrylic resins (TM) may be used.

[0092] As the rubbery polymer (R), from the viewpoints of transparency, impact resistance, and dispersibility, crosslinked rubber particles such as multilayered polymer particles (RP); block copolymers (BL), etc. are preferred. The multilayered polymer particles (RP) have at least one rubber component layer (I) (also simply referred to as layer (I)) inside and at least one thermoplastic resin component layer (II) (also simply referred to as layer (II)) on the outermost surface. This particle has a core-shell structure consisting of an interior containing one or more rubber component layers and an exterior consisting of one or more thermoplastic resin component layers. In the multilayered polymer particles (RP), the core is considered to be a "layer." The number of layers in the multilayered polymer particles (RP) is preferably 2 to 4. Examples of the layer structure include, from the center, a two-layer structure of layer (I)-layer (II); a three-layer structure of layer (I)-layer (I)-layer (II), layer (I)-layer (II)-layer (II), or layer (II)-layer (I)-layer (II); and a four-layer structure such as layer (I)-layer (II)-layer (I)-layer (II). Among these, from the viewpoint of handleability, a two-layer structure of layer (I)-layer (II); and a three-layer structure of layer (I)-layer (I)-layer (II) or layer (II)-layer (I)-layer (II) are preferred.

[0093] The mass ratio (layer (I) / layer (II)) of the total amount of the rubber component layers (I) to the total amount of the thermoplastic resin component layers (II) is 30 / 70 to 90 / 10. If the proportion of the layers (I) is less than the above range, the flexibility of the thermoplastic resin composition (TR) may be insufficient. If the proportion of the layers (I) exceeds the above range, it may be difficult to form a particle structure, and the melt fluidity of the multilayered polymer particles (RP) may decrease, making it difficult to melt-knead with other components and to mold the thermoplastic resin composition (TR). The mass ratio (layer (I) / layer (II)) is preferably 50 / 50 to 90 / 10, more preferably 60 / 40 to 80 / 20.

[0094] Layer (I) is composed of a copolymer containing 50 to 99.99% by mass of acrylic acid ester monomer units, 49.99 to 0% by mass of other monofunctional monomer units, and 0.15 to 10% by mass of polyfunctional monomer units. This copolymer preferably contains other monomer units. The content of the acrylic acid ester monomer units is preferably 55 to 99.9% by mass, the content of the other monofunctional monomer units is preferably 44.9 to 0% by mass, and the content of the polyfunctional monomer units is preferably 0.16 to 2% by mass.

[0095] If the amount of acrylic acid ester monomer units is less than the above lower limit, the rubber elasticity of the multilayered polymer particles (RP) may decrease, and the weather resistance of the thermoplastic resin composition (TR) may decrease. If the amount exceeds the above upper limit, the layer structure of the multilayered polymer particles (RP) may not be formed in a complete form, and the melt fluidity of the multilayered polymer particles (RP) may decrease, making it difficult to melt-knead with other components and mold the thermoplastic resin composition (TR). If the amount of polyfunctional monomer units exceeds the above upper limit, the rubber elasticity of the multilayered polymer particles (RP) may decrease, and the flexibility of the thermoplastic resin composition (TR) may be insufficient. If the amount of acrylic acid ester monomer units is less than the above lower limit, the layer (I) may not be formed as a particle structure.

[0096] The raw material monomers for layer (I) are described below. One or more known acrylic acid esters can be used. The polyfunctional monomer is a monomer having two or more carbon-carbon double bonds in the molecule. Examples of polyfunctional monomers include esters of unsaturated monocarboxylic acids such as (meth)acrylic acid and cinnamic acid with unsaturated alcohols such as (meth)allyl alcohol; diesters of unsaturated monocarboxylic acids with glycols such as ethylene glycol, butanediol, and hexanediol; and esters of dicarboxylic acids such as phthalic acid, terephthalic acid, isophthalic acid, and maleic acid with unsaturated alcohols. Specific examples include allyl acrylate, methallyl acrylate, allyl methacrylate (ALMA), methallyl methacrylate, (meth)allyl cinnamate, diallyl maleate, diallyl phthalate, diallyl terephthalate, diallyl isophthalate, divinylbenzene, ethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, and hexanediol di(meth)acrylate. These may be used alone or in combination. Of these, allyl methacrylate (ALMA) is preferred.

[0097] Other monofunctional monomers include methacrylic acid esters, aromatic vinyl monomers, and vinyl cyanide monomers. One or more of these can be used. For specific examples, see the descriptions of the methacrylic resin (M) and the glutarimide resin (MG).

[0098] Layer (II) is composed of a copolymer consisting of 40 to 100% by mass of methacrylic acid ester units and 60 to 0% by mass of other monomer units. This copolymer preferably contains other monomer units. The content of the methacrylic acid ester units is preferably 60 to 99% by mass, more preferably 80 to 99% by mass, and the content of the other monomer units is preferably 40 to 1% by mass, more preferably 20 to 1% by mass. If the content of the methacrylic acid ester units is less than the above lower limit, the compatibility of the multilayered polymer particles (RP) with other components may decrease, and the dispersibility of the multilayered polymer particles (RP) during melt-kneading and molding may be insufficient.

[0099] The raw material monomers for layer (II) are described below. As the methacrylic acid ester, one or more known methacrylic acid esters can be used, with methyl methacrylate (MMA) being preferred. Other monomers include acrylic acid esters; aromatic vinyl monomers; vinyl cyanide-based monomers; maleimide-based monomers such as maleimide, N-methylmaleimide, N-ethylmaleimide, N-propylmaleimide, N-isopropylmaleimide, N-cyclohexylmaleimide, N-phenylmaleimide, N-(p-bromophenyl)maleimide, and N-(chlorophenyl)maleimide; and the polyfunctional monomers exemplified for layer (I). One or more of these can be used. For specific examples of acrylic acid esters, aromatic vinyl monomers, and vinyl cyanide-based monomers, see the descriptions of the methacrylic resin (M) and glutarimide resin (MG). Among these, alkyl acrylates such as methyl acrylate (MA), ethyl acrylate, and n-butyl acrylate (BA) are preferred.

[0100] The average particle size of the multilayered polymer particles (RP) is preferably 30 to 300 nm. The lower limit is more preferably 50 nm, particularly preferably 80 nm, and most preferably 100 nm. The upper limit is more preferably 250 nm. If the average particle size exceeds the above upper limit, the flexibility and melt flowability of the thermoplastic resin composition (TR) may be insufficient. If the average particle size is equal to or less than the above lower limit, the multilayered polymer particles (RP) are easily produced. In this specification, unless otherwise specified, "average particle size" refers to the volume average particle size (median size). The average particle size of the multilayered polymer particles (RP) in the latex can be measured by dynamic light scattering using a laser diffraction / scattering particle size distribution measuring device or the like. The average particle size of the multilayered polymer particles (RP) in the film can be measured by observation with a transmission electron microscope or the like.

[0101] From the viewpoints of physical properties and ease of production, the multilayered polymer particles (RP) are preferably multilayered polymer particles (BX) having a three-layer structure consisting of, from the center, a rubber component layer (Ia) which is the first rubber component layer (I), a rubber component layer (Ib) which is the second rubber component layer (I), and a thermoplastic resin component layer (II). From the viewpoint of achieving both flexibility and other mechanical properties (tensile properties, etc.) of the thermoplastic resin composition (TR), the mass ratio of the rubber component layer (Ia) to the rubber component layer (Ib) ((Ia) / (Ib)) is preferably 5 / 95 to 95 / 5, more preferably 20 / 80 to 80 / 20.

[0102] The method for producing multilayered polymer particles (RP) includes a polymerization reaction step (S1) for forming a rubber component layer (I) and a polymerization reaction step (S2) for forming a thermoplastic resin component layer (II). In the polymerization reaction step (S1), a monomer mixture (i) corresponding to the copolymer composition of the rubber component layer (I) is copolymerized by a known method. Similarly, in the polymerization reaction step (S2), a monomer mixture (ii) corresponding to the copolymer composition of the thermoplastic resin component layer (II) is copolymerized by a known method. In the polymerization reaction step (S2), a molecular weight modifier can be used in an amount of 0.4 to 10% by mass, more preferably 0.4 to 5% by mass, and particularly preferably 0.6 to 2% by mass, relative to the monomer mixture (ii). When the amount of molecular weight modifier used is equal to or greater than the above-mentioned lower limit, the number average molecular weight (Mn) of the thermoplastic resin component constituting the outermost layer is stably 30,000 or less, thereby stably achieving both flexibility and moldability of the thermoplastic resin composition (TR). Even if the amount of molecular weight modifier used exceeds the upper limit, no further effect of improving flexibility can be obtained, and the amount of molecular weight modifier remaining, which is essentially unnecessary, will simply increase.

[0103] Examples of molecular weight regulators include mercaptans such as n-octyl mercaptan (n-OM), t-octyl mercaptan, n-dodecyl mercaptan, t-dodecyl mercaptan, and mercaptoethanol; terpene mixtures consisting of terpinolene, dipentene, t-terpinene, and small amounts of other cyclic terpenes; and halogenated hydrocarbons such as chloroform and carbon tetrachloride. One or more of these may be used. Among these, alkyl mercaptans such as n-octyl mercaptan (n-OM) are preferred.

[0104] The polymerization method for producing multilayered polymer particles (RP) is not particularly limited, and examples include emulsion polymerization, suspension emulsion polymerization, solution polymerization, and combinations thereof. Preferred polymerization conditions for producing multilayered polymer particles (RP) using emulsion polymerization are described below as an example. The polymerization temperature is generally 0 to 100°C. Examples of emulsifiers include alkali metal salts of fatty acids such as sodium oleate, sodium laurate, and sodium stearate; sulfate ester salts of fatty alcohols such as sodium lauryl sulfate; rosinates such as potassium rosinate; and alkylarylsulfonic acids such as dodecylbenzenesulfonic acid. One or more of these may be used. Radical polymerization initiators are generally used as polymerization initiators. Examples of radical polymerization initiators that can be used alone include peroxides such as persulfates, azobisisobutyronitrile, and benzoyl peroxide. Redox initiators combining organic hydroperoxides such as cumene hydroperoxide, diisopropylbenzene hydroperoxide, and paramenthane hydroperoxide with a reducing agent such as a transition metal salt can also be used. The average particle size of the multilayered polymer particles (RP) can be controlled within a preferred range by adjusting polymerization conditions such as the amount of emulsifier added. After polymerization is complete, the multilayered polymer particles (RP) can be separated and obtained from the reaction system by known methods such as acid precipitation, salting out, spray drying, and freeze-coagulation.

[0105] The block copolymer (BL) is preferably a copolymer containing one or more methacrylic acid ester polymer blocks (b1) and one or more acrylic acid ester polymer blocks (b2).

[0106] The methacrylic acid ester polymer block (b1) is a polymer block mainly containing methacrylic acid ester units and optionally containing other monomer units. From the viewpoint of surface hardness and the like, the content of the methacrylic acid ester units in the methacrylic acid ester polymer block (b1) is preferably 80% by mass or more, more preferably 90% by mass or more, particularly preferably 95% by mass or more, and most preferably 98% by mass or more.

[0107] As the methacrylic acid ester, one or more known methacrylic acid esters can be used. From the viewpoints of transparency and heat resistance, methacrylic acid alkyl esters such as MMA, ethyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, t-butyl methacrylate, cyclohexyl methacrylate, and isobornyl methacrylate are preferred, and MMA is more preferred.

[0108] The content of other monomer units than the methacrylate ester units optionally contained in the methacrylate ester polymer block (b1) is preferably 20% by mass or less, more preferably 10% by mass or less, particularly preferably 5% by mass or less, and most preferably 2% by mass or less, from the viewpoint of surface hardness and the like.

[0109] Examples of other monomers besides methacrylic acid esters include acrylic acid esters, unsaturated carboxylic acids, aromatic vinyl monomers, olefins, conjugated dienes, (meth)acrylonitrile, (meth)acrylamide, vinyl acetate, vinylpyridine, vinyl ketone, vinyl chloride, vinylidene chloride, and vinylidene fluoride, and these may be used alone or in combination.

[0110] The weight average molecular weight (Mw) of the methacrylic acid ester polymer block (b1) is not particularly limited and is preferably 5.00 to 150,000, more preferably 8,000 to 120,000, and particularly preferably 12,000 to 100,000. When the block copolymer (BL) contains a plurality of methacrylic acid ester polymer blocks (b1), the monomer compositions and molecular weights of these blocks may be the same or different.

[0111] The acrylic ester polymer block (b2) is a polymer block mainly containing acrylic ester units and, if necessary, containing other monomer units. The proportion of the acrylic ester units in the acrylic ester polymer block (b2) is preferably 45% by mass or more, more preferably 50% by mass or more, particularly preferably 60% by mass or more, and most preferably 90% by mass or more.

[0112] One or more known acrylic esters can be used as the acrylic ester. From the viewpoint of transparency and the like, it is preferable for the acrylic ester to contain an alkyl acrylate unit and an aromatic (meth)acrylate unit. Examples of alkyl acrylate esters include methyl acrylate, ethyl acrylate, isopropyl acrylate, n-butyl acrylate, 2-ethylhexyl acrylate, and dodecyl acrylate. Of these, n-butyl acrylate and 2-ethylhexyl acrylate are preferred. The aromatic (meth)acrylate ester is an ester of an aromatic acrylic ester or an aromatic methacrylic ester with a compound containing an aromatic ring. Examples include phenyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, and styryl (meth)acrylate. Of these, from the viewpoint of transparency, phenyl methacrylate, benzyl methacrylate, phenoxyethyl methacrylate, and benzyl acrylate are preferred.

[0113] From the viewpoint of transparency, the content of the acrylic acid alkyl ester unit in the acrylic acid ester polymer block (b2) is preferably 50 to 90 mass %, more preferably 60 to 80 mass %, and the content of the (meth)acrylic acid aromatic ester unit is preferably 50 to 10 mass %, more preferably 40 to 20 mass %.

[0114] The content of monomer units other than acrylate esters, which may be optionally contained in the acrylate ester polymer block (b2), is preferably 55% by mass or less, more preferably 50% by mass or less, particularly preferably 40% by mass or less, and most preferably 10% by mass or less.

[0115] Examples of the monomer other than the acrylic acid ester include methacrylic acid ester, unsaturated carboxylic acid, aromatic vinyl monomer, olefin, conjugated diene, (meth)acrylonitrile, (meth)acrylamide, vinyl acetate, vinylpyridine, vinyl ketone, vinyl chloride, vinylidene chloride, and vinylidene fluoride, and these can be used alone or in combination.

[0116] The weight average molecular weight (Mw) of the acrylic acid ester polymer block (b2) is not particularly limited and is preferably 5,000 to 120,000, more preferably 15,000 to 110,000, and particularly preferably 30,000 to 100,000. When the block copolymer (BL) contains a plurality of acrylic acid ester polymer blocks (b2), the monomer compositions and molecular weights of these blocks may be the same or different.

[0117] The melt flow rate (MFR) of the methacrylic resin composition (T-MR) is not particularly limited, but is preferably 1 to 30 g / 10 min. The lower limit of MFR is more preferably 1.5 g / 10 min, even more preferably 2 g / 10 min, particularly preferably 3 g / 10 min, and most preferably 5 g / 10 min. The upper limit of MFR is more preferably 25 g / 10 min, even more preferably 20 g / 10 min, particularly preferably 15 g / 10 min or less, and most preferably 10 g / 10 min. When the MFR is within the above range, the stability of hot melt molding is good.

[0118] <Polycarbonate-based resin composition (T-PC)> The polycarbonate-based resin composition (T-PC) contains a polycarbonate-based resin (PC). The polycarbonate-based resin (PC) is preferably obtained by copolymerizing one or more dihydric phenols with one or more carbonate precursors. Examples of production methods include an interfacial polymerization method in which an aqueous solution of a dihydric phenol is reacted with an organic solvent solution of a carbonate precursor at an interface, and a transesterification method in which a dihydric phenol is reacted with a carbonate precursor under high-temperature, reduced-pressure, and solvent-free conditions.

[0119] Examples of dihydric phenols include 2,2-bis(4-hydroxyphenyl)propane (commonly known as bisphenol A), 1,1-bis(4-hydroxyphenyl)ethane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 2,2-bis(3-methyl-4-hydroxyphenyl)propane, 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, bis(4-hydroxyphenyl)sulfide, and bis(4-hydroxyphenyl)sulfone, with bisphenol A being preferred. Examples of carbonate precursors include carbonyl halides such as phosgene; carbonate esters such as diphenyl carbonate; and haloformates such as dihaloformates of dihydric phenols.

[0120] The Mw of the polycarbonate-based resin (PC) is preferably 10,000 to 100,000, more preferably 20,000 to 70,000. When the Mw is 10,000 or more, the second resin layer has excellent impact resistance and heat resistance, and when the Mw is 100,000 or less, the second resin layer has excellent moldability. Commercially available polycarbonate-based resins (PC) may be used.

[0121] The glass transition temperature of a typical polycarbonate-based resin (PC) is about 150°C. Examples of embodiments that can achieve a lower Tg than when a polycarbonate-based resin (PC) is used alone, for example, a Tg of 145°C or less, include a first embodiment in which the second resin layer contains an alloy or copolymer of a polycarbonate-based resin (PC) and an aromatic polyester, and a second embodiment in which the second resin layer contains a polycarbonate-based resin (PC) and a plasticizer. In the second embodiment, the second resin layer preferably contains 85 to 99 parts by mass of the polycarbonate-based resin (PC) and 15 to 1 part by mass of the plasticizer.

[0122] Examples of aromatic polyesters include polycondensates of aromatic dicarboxylic acid components and diol components. Representative aromatic dicarboxylic acid components include terephthalic acid, isophthalic acid, and naphthalenedicarboxylic acid. Other dicarboxylic acid components include oxalic acid, malonic acid, succinic acid, adipic acid, azelaic acid, sebacic acid, neopentylic acid, isophthalic acid, naphthalenedicarboxylic acid, diphenyl ether dicarboxylic acid, and p-oxybenzoic acid. These may be used alone or in combination. Representative diol components include ethylene glycol, diethylene glycol, triethylene glycol, and cyclohexanedimethanol. Other diol components include propylene glycol, trimethylene glycol, tetramethylene glycol, hexamethylene glycol, diethylene glycol, neopentyl glycol, polyalkylene glycol, 1,4-cyclohexanedimethanol, glycerin, pentaerythritol, trimethylol, and methoxypolyalkylene glycol. These may be used alone or in combination.

[0123] A typical example of an aromatic polyester is polyethylene terephthalate (PET), which is a polycondensate of terephthalic acid and ethylene glycol. Copolymerized polyesters using terephthalic acid and ethylene glycol with other dicarboxylic acid components and / or other diol components are also preferred. Another typical example of an aromatic polyester is polybutylene terephthalate (PBT), which is a polycondensate of terephthalic acid or dimethyl terephthalate with 1,4-butanediol. Copolymerized polyesters using terephthalic acid and 1,4-butanediol with other dicarboxylic acid components and / or other diol components are also preferred. Among these, copolymerized polyesters (PCTG) in which cyclohexanedimethanol (1,4-CHDM) is used in combination with a portion of the ethylene glycol in PET, preferably 55 to 75 mol%, more preferably 50 to 75 mol%, and copolymerized polyesters (PCTG) in which isophthalic acid is used in combination with a portion of the terephthalic acid in PBT, preferably 10 to 30 mol%, and combinations thereof are preferred. These copolymer polyesters can be melt-blended with polycarbonate resins to form polymer alloys, which are completely compatible with each other, and this polymer alloying effectively lowers the glass transition temperature.

[0124] The plasticizer is not particularly limited, and examples thereof include phosphate ester compounds such as trimethyl phosphate, triethyl phosphate, tributyl phosphate, tris(2-ethylhexyl)phosphate, triphenyl phosphate, tricresyl phosphate, trixylenyl phosphate, cresyl diphenyl phosphate, and 2-ethylhexyl diphenyl phosphate; phosphite compounds corresponding to these phosphate ester compounds; phthalate ester compounds such as dimethyl phthalate, diethyl phthalate, dibutyl phthalate, bis(2-ethylhexyl phthalate), diisodecyl phthalate, butyl benzyl phthalate, diisononyl phthalate, and ethyl phthalyl ethyl glycolate; and trimellitate esters such as tris(2-ethylhexyl) trimellitate. ester compounds; aliphatic dibasic acid ester compounds such as dimethyl adipate, dibutyl adipate, diisobutyl adipate, bis(2-ethylhexyl) adipate, diisononyl adipate, diisodecyl adipate, diisodecyl adipate, bis(butyldiglycol) adipate, bis(2-ethylhexyl) azelate, dimethyl sebacate, dibutyl sebacate, bis(2-ethylhexyl) sebacate, and diethyl succinate; polyester compounds containing an aliphatic dibasic acid unit contained in these aliphatic dibasic acid ester compounds; ricinoleic acid ester compounds such as methyl acetyl ricinoleate; acetate ester compounds such as triacetin and octyl acetate; and sulfonamide compounds such as N-butylbenzenesulfonamide. Among these, phosphate ester compounds, particularly cresyl diphenyl phosphate (CDP) and tricresyl phosphate (TCP), are preferred because they have good compatibility with polycarbonate resins (PC) and the transparency of the resin after compatibility is good.

[0125] From the viewpoint of hot melt molding stability, the melt flow rate (MFR) of the polycarbonate resin composition (T-PC) is not particularly limited, but is preferably 1 to 30 g / 10 min. The lower limit of MFR is more preferably 1.5 g / 10 min, even more preferably 2 g / 10 min, particularly preferably 3 g / 10 min, and most preferably 5 g / 10 min. The upper limit of MFR is more preferably 25 g / 10 min, even more preferably 20 g / 10 min, particularly preferably 15 g / 10 min or less, and most preferably 10 g / 10 min. An MFR within the above range ensures good hot melt molding stability. Unless otherwise specified, the MFR of a polycarbonate resin (composition) in this specification is a value measured using a melt indexer at a temperature of 300°C and under a load of 1.2 kg.

[0126] The thermoplastic resin (composition) (TR) may contain various additives as necessary, and examples and amounts of additives are the same as those for the methacrylic resin (composition) (MR).

[0127] (Other Layers) The thermoplastic resin film of the present disclosure may optionally have one or more other layers in addition to the first resin layer made of a methacrylic resin (composition) (MR) and the second resin layer made of a thermoplastic resin (composition) (TR). The thermoplastic resin film of the present disclosure may also include a layer that does not contain a thermoplastic resin. In such a case, the thermoplastic resin film of the present disclosure is also simply referred to as a laminate film. Examples of other layers include a resin layer containing a thermoplastic resin, a thermosetting resin, an energy ray curable resin, or a combination thereof; an inorganic layer; an organic-inorganic composite layer containing a resin and an inorganic material; etc. The other resin layer may be a surface layer or an inner layer.

[0128] [Method for Producing Thermoplastic Resin Film] The thermoplastic resin film of the present disclosure can be produced by known multilayer molding methods such as coextrusion (also referred to as multilayer extrusion), multilayer blow molding, and multilayer injection molding. A monolayer film consisting of one of the first and second resin layers may be prepared, and the other resin layer may be laminated onto this monolayer film. Examples of laminating the other resin layer include insert molding; a method in which a solution containing the material of the other resin layer is applied to a monolayer film consisting of one resin layer and then dried or cured; a method in which a monolayer film consisting of the other resin layer is bonded to a monolayer film consisting of one resin layer via an adhesive layer; and a multilayer press molding method in which a monolayer film consisting of one resin layer and a monolayer film consisting of the other resin layer are thermocompression bonded together. The same manufacturing method as described above can also be applied when the thermoplastic resin film of the present disclosure includes resin layers other than the first and second resin layers.

[0129] From the viewpoint of productivity, a coextrusion molding method is preferred, and a T-die method using an extruder equipped with a T-die is preferred. FIG. 4 shows a schematic diagram of an extrusion molding apparatus of one embodiment. The constituent resins (compositions) of each layer are melt-kneaded using each extruder, and are coextruded in the form of a film from a T-die 11 having a wide discharge port in the form of a desired laminate structure. Examples of extruders include single-screw extruders, twin-screw extruders, multi-screw extruders, and combinations thereof. Examples of lamination methods include a feedblock method in which lamination is performed before flowing into the T-die, and a multi-manifold method in which lamination is performed inside the T-die. The multi-manifold method is preferred from the viewpoint of improving the interfacial smoothness between layers.

[0130] To remove foreign matter, each molten resin is preferably melt-filtered using a filter before extrusion. By using melt-filtered molten resins to produce a film with fewer defects caused by foreign matter and gels, the filter material is appropriately selected based on the operating temperature, viscosity, filtration accuracy, etc. Examples include nonwoven fabrics made of glass fiber, etc.; sheets made of phenolic resin-impregnated cellulose; sintered metal fiber nonwoven sheets; sintered metal powder sheets; wire mesh; and combinations thereof. Among these, from the viewpoint of heat resistance and durability, a filter made of multiple laminated sintered metal fiber nonwoven sheets is preferred. The filtration accuracy of the filter is not particularly limited, but is preferably 30 μm or less, more preferably 15 μm or less, and particularly preferably 5 μm or less.

[0131] The molten thermoplastic resin laminate coextruded from the T-die 11 is pressed and cooled using multiple cooling rolls 12-14. Examples of cooling rolls include rigid metal rolls and elastic metal rolls. Rigid metal rolls are inelastic rolls made of metal such as stainless steel, and include drilled rolls and spiral rolls. The surface of the rigid metal roll may be a mirror finish or may have a pattern or irregularities. Elastic metal rolls are rolls with an elastic outer cylinder made of a thin metal film on their outer periphery. The elastic metal roll, for example, comprises a metal shaft roll made of stainless steel or the like, a thin metal film (elastic outer cylinder) made of stainless steel or the like covering the outer surface of the shaft roll, and a fluid sealed between the shaft roll and the thin metal film (elastic outer cylinder), and can exhibit elasticity in the presence of the fluid. Examples of fluids include water and oil. The thickness of the thin metal film of the elastic metal roll is not particularly limited, but is preferably approximately 2 to 8 mm. The thin metal film preferably has flexibility and bendability, and preferably has a seamless structure without welded joints. Such a metal elastic roll equipped with a metal thin film is highly durable, and if the metal thin film is mirror-finished, it can be handled in the same way as a normal mirror-finished roll. If a pattern, irregularities, etc., are imparted to the metal thin film, the roll can be used to transfer the shape, making it easy to use. By using a roll with an irregular surface (also called an embossing roll or a grain roll) as one or more cooling rolls, a thermoplastic resin film having irregularities on at least one surface can be produced. The thermoplastic resin film 16 obtained after cooling is taken up by a pair of take-up rolls 15. The above extrusion, cooling, and take-up processes are carried out continuously. The configuration of the manufacturing apparatus can be appropriately modified within the scope of the present invention. In this specification, a material in a heated and molten state is mainly referred to as a "thermoplastic resin laminate," and a solidified material is referred to as a "thermoplastic resin laminate film," but there is no clear boundary between the two.

[0132] [Method of imparting unevenness] Examples of methods for forming an uneven surface structure include an embossing roll method, in which a roll having an uneven surface (embossing roll or embossing roll) is used as one or more cooling rolls in a co-extrusion molding method, a calendar roll method, and a profile extrusion method. Among these, the embossing roll method is preferred because it can easily form a relatively large amount of unevenness. Other examples include a method in which a thermoplastic resin film having a smooth surface is molded, and then the surface is embossed using a roll having an uneven surface (embossing roll or embossing roll); a method in which a thermoplastic resin film is formed on a release paper having an uneven surface, and the like.

[0133] The embossing temperature is preferably 100 to 200°C, more preferably 110 to 190°C, and particularly preferably 120 to 180°C. If the embossing temperature is below the lower limit, the embossing temperature is too low relative to the glass transition temperature (Tg(1)) of the first resin layer, and the uneven shape may not be transferred well. If the embossing temperature exceeds the upper limit, the thermoplastic resin film may soften, making the embossing process unstable. In the thermoplastic resin film of the present disclosure, the first resin layer has a high glass transition temperature (Tg) and can have a sufficient thickness, and appropriate unevenness can be imparted to the surface of the first resin layer depending on the application, etc.

[0134] As described above, according to the present disclosure, it is possible to provide a thermoplastic resin film that can be imparted with appropriate surface irregularities depending on the application, etc., and that can well retain the surface irregularity shape after secondary molding.

[0135] [Laminate Film] The laminate film of the present disclosure includes the thermoplastic resin film of the present disclosure and one or more functional layers, such as a print layer, a hard coat layer (also called a scratch-resistant layer), an antistatic layer, an antifouling layer, a friction-reducing layer, an antiglare layer, an antireflection layer, an adhesive layer, an impact strength-imparting layer, and an anchor layer.

[0136] The printed layer-equipped laminate film of the present disclosure comprises the thermoplastic resin film of the present disclosure described above and a printed layer formed on the surface of the second resin layer of the thermoplastic resin film opposite the first resin layer. The printed layer can include characters, pictures, figures, patterns, colors, and combinations thereof. Figure 2 is a schematic cross-sectional view of a printed layer-equipped laminate film of one embodiment according to the present invention. In the figure, reference numeral 2 denotes the printed layer-equipped laminate film, and reference numeral 31 denotes the printed layer. The same reference numerals are used for the same components as in Figure 1, and descriptions thereof will be omitted.

[0137] The laminate film with a hard coat layer of the present disclosure has the thermoplastic resin film of the present disclosure described above and a hard coat layer formed on the surface of the first resin layer of this thermoplastic resin film opposite to the second resin layer. Figure 3 is a schematic cross-sectional view of a laminate film with a hard coat layer of one embodiment of the present invention. In the figure, reference numeral 3 denotes the laminate film with a hard coat layer, and reference numeral 41 denotes the hard coat layer. The same reference numerals are used for the same components as in Figure 1, and their explanations are omitted.

[0138] Materials for the hard coat layer include inorganic, organic, organic-inorganic, and silicone materials, and from the viewpoint of productivity, organic and organic-inorganic materials are preferred. The thickness of the hard coat layer is not particularly limited, and is preferably 0.5 to 30 μm, more preferably 1 to 20 μm, and particularly preferably 1.5 to 15 μm.

[0139] The inorganic hard coat layer may be, for example, SiO 2 , Al 2 O 3 , TiO 2 , and ZrO 2The hard coat layer can be formed by depositing an inorganic material such as a metal oxide by vapor-phase deposition, such as vacuum deposition or sputtering. The organic hard coat layer can be formed by applying a curable composition containing one or more curable compounds and curing it by heating or ionizing radiation. Examples of the curable compound include monomers, oligomers, prepolymers, and curable resins. Examples of curable compounds that cure upon heating include thermosetting resins such as polyester resins, epoxy resins, polyurethane resins, aminoalkyd resins, melamine resins, guanamine resins, urea resins, and thermosetting acrylic resins. Examples of curable compounds that cure upon ionizing radiation include oligomers and prepolymers having radically polymerizable unsaturated groups in the molecule. Specific examples include oligomers and prepolymers such as epoxy (meth)acrylates, urethane (meth)acrylates, polyether-based urethane (meth)acrylates, caprolactone-based urethane (meth)acrylates, polyester (meth)acrylates, and polyether (meth)acrylates. Ionizing radiation is electromagnetic waves and charged particle beams that have an energy quantum capable of polymerizing or crosslinking molecules, and specific examples include electromagnetic waves such as ultraviolet (UV) rays, electron beams (EB), X-rays, and gamma rays; and charged particle beams such as alpha rays, beta rays, and ion beams.

[0140] The organic-inorganic hard coat layer can be formed, for example, by applying an ultraviolet-curable hard coat coating material containing inorganic ultrafine particles such as silica ultrafine particles having photopolymerizable functional groups introduced on the surface and a curable organic component, and then polymerizing the curable organic component with the photopolymerizable functional groups of the inorganic ultrafine particles by ultraviolet irradiation. This method results in a network-like crosslinked film in which the inorganic ultrafine particles are dispersed in the organic matrix while being chemically bonded to the organic matrix.

[0141] The silicone-based hard coat layer can be formed, for example, by polycondensing partial hydrolysates of carbon functional alkoxysilane, alkyltrialkoxysilane, tetraalkoxysilane, etc., or materials obtained by blending these with colloidal silica.

[0142] Examples of methods for applying the curable composition include dip coating, various roll coating methods such as gravure roll coating, flow coating, rod coating, blade coating, spray coating, die coating, and bar coating.

[0143] [Laminate] The thermoplastic resin film of the present disclosure can be subjected to secondary forming such as pressure forming, vacuum forming, and three-dimensional surface decoration forming (Three Dimension Overlay Method: TOM forming). A laminate can be obtained by laminating the thermoplastic resin film of the present disclosure on a substrate of any shape. When the first resin layer has a surface irregularity, it is preferable to use the first resin layer as the outermost layer, as this provides a good matte appearance. The thermoplastic resin film with a surface irregularity of the present disclosure is prevented from excessive softening of the first resin layer during secondary forming, and can well retain the surface irregularity shape after secondary forming.

[0144] [Applications] The thermoplastic resin film and laminate film of the present disclosure can be used in any application, and are preferably used in various applications requiring design, and are suitable for applications requiring a matte appearance. The thermoplastic resin film and laminate film of the present disclosure can be preferably used as a decorative film and a film for building materials. Suitable applications include, for example, interior parts such as furniture, wallpaper, pendant lights, and mirrors; and architectural parts such as doors, sashes, domes, safety window glass, partitions, staircase wainscoting, balcony wainscoting, and roofs of leisure buildings. Other uses include, for example, sign parts or marking films such as advertising towers, stand signs, side signs, transom signs, and rooftop signs; display parts such as showcases, partitions, and store displays; lighting parts such as fluorescent light covers, mood lighting covers, lampshades, illuminated ceilings, illuminated walls, and chandeliers; transportation parts such as aircraft windshields, pilot visors, motorcycle windshields, motorboat windshields, bus shades, automobile side visors, rear visors, head wings, headlight covers, automobile interior parts, and automobile exterior parts such as bumpers; electronic device parts such as mobile phones and personal computers; television protection solar cell parts such as back films for solar cells and front films for flexible solar cells; audiovisual nameplates, stereo covers; vending machines; medical equipment parts such as incubators and X-ray parts; equipment parts such as clock panels, machine covers, instrument covers, laboratory equipment, dial faces, and observation windows; traffic-related parts such as road signs, information boards, convex mirrors, and soundproof walls; bathroom parts such as bathtubs, sanitary parts; greenhouses, large aquariums, box aquariums; stationery such as rulers and desk mats; game parts, toys, musical instruments; decorative and protective films to be provided on the surface of face protection masks used during welding, etc.

[0145] Examples and comparative examples according to the present invention will be described. [Evaluation Items and Evaluation Methods] The evaluation items and evaluation methods are as follows. (Weight-average molecular weight (Mw)) The weight-average molecular weight (Mw) was determined by gel permeation chromatography (GPC). A GPC device "HLC-8320" manufactured by Tosoh Corporation was used as the measurement device. A series connection of a "TSKguardcolumn Super HZ-H," a "TSKgel HZM-M," and a "TSKgel Super HZ4000" manufactured by Tosoh Corporation was used as the separation column. A differential refractive index detector (RI detector) was used as the detector. A sample solution was prepared by dissolving 4 mg of the resin to be measured in 5 ml of tetrahydrofuran. The column oven temperature was set to 40°C. Tetrahydrofuran was used as the eluent, and the eluent flow rate was set to 0.35 ml / min. 20 μl of the sample solution was injected into the device, and a chromatogram was measured. Ten standard polymethyl methacrylate (PMMA) samples with molecular weights ranging from 400 to 5,000,000 were analyzed by GPC, and a calibration curve was created showing the relationship between retention time and molecular weight. Based on this calibration curve, the Mw of the resin to be measured was calculated from the chromatogram in terms of standard PMMA.

[0146] (Glass Transition Temperature (Tg)) The resin (composition) to be measured was vacuum dried at 100°C for 12 hours or more. The glass transition temperature (Tg) of this resin (composition) to be measured was measured using a differential scanning calorimeter (Shimadzu Corporation, "DSC-50") in accordance with JIS K7121. 10 mg of the resin (composition) to be measured was placed in an aluminum pan and set in the apparatus. After nitrogen substitution for 30 minutes or more, the sample was heated from room temperature (20-25°C) to 250°C at a rate of 20°C / min in a 10 ml / min nitrogen stream, held for 5 minutes, and cooled to room temperature (primary scan). The sample was then heated to 200°C at a rate of 10°C / min (secondary scan), and the DSC curve was measured. The midpoint glass transition temperature determined from the DSC curve obtained in the secondary scan was taken as the glass transition temperature (Tg).

[0147] (Syndiotacticity (rr) (rr ratio) in triad notation) A methacrylic resin was dissolved in deuterated chloroform to prepare a sample solution. The obtained sample solution was analyzed using a nuclear magnetic resonance spectrometer ("ULTRA SHIELD 400 PLUS" manufactured by Bruker) at room temperature with 64 accumulations. 1 The H-NMR spectrum was measured. From the spectrum, the area (A0) of the region from 0.6 to 0.95 ppm and the area (AY) of the region from 0.6 to 1.35 ppm, when TMS was set to 0 ppm, were measured, and then the syndiotacticity (rr) expressed in triad form was calculated using the formula: (A0 / AY)×100.

[0148] (Storage Modulus (E')) In the Examples and Comparative Examples in which a laminated thermoplastic resin film was produced, a single-layer thermoplastic resin film having the same composition and thickness as the first resin layer was extrusion-molded. In each Example, a strip-shaped test piece measuring 20 mm in length and 5 mm in width was cut from the single-layer thermoplastic resin film consisting of only the first resin layer. Dynamic viscoelasticity measurement was performed using a dynamic viscoelasticity measurement device ("Rheogel-E4000" manufactured by UBM) by applying sinusoidal vibration with a set frequency and amplitude to the test piece under elevated temperature. The measurement conditions were as follows: measurement frequency: 1 Hz, measurement mode: temperature dependent, measurement temperature: 30 to 250°C, and temperature increase condition: 3°C / min. The storage modulus (E') at the glass transition temperature (Tg(2)) + 20°C of the material constituting the second resin layer was determined. When the second resin layer was not present, the storage modulus (E') at the glass transition temperature (Tg(1)) + 20°C of the constituent material of the first resin layer was determined.

[0149] (Retention of Surface Unevenness) The maximum height (Rz) of the thermoplastic resin film with uneven surface was measured before and after heating, as measured in accordance with JIS B0601-2001. Heating was performed as follows. A thermoplastic resin film with a laminated structure in which unevenness was imparted to the surface of the first resin layer was placed in an oven set to a temperature of 20°C above the glass transition temperature (Tg(2)) of the constituent material of the second resin layer, and heated for 10 minutes until the uneven surface reached the set heating temperature. A thermoplastic resin film with a single-layer structure in which unevenness was imparted to one surface was placed in an oven set to a temperature of 20°C above the glass transition temperature (Tg(1)) of the constituent material of the first resin layer, and heated until the uneven surface reached the set heating temperature. The maximum height (Rz) of the uneven surface before and after heating was measured using a surface roughness meter (Mitutoyo Corporation, "Surftest SJ-210"). The retention rate of surface irregularities after heating (retention rate of maximum height (Rz)) relative to before heating was calculated using the following formula, and evaluated according to the following criteria: [Retention rate of surface irregularities (%)] = ([Rz after heating] / [Rz before heating]) x 100 Good (◯): Rz retention rate was 60% or more, Poor (×): Rz retention rate was less than 60%.

[0150] (Surface Hardness) A 10 cm x 10 cm test piece was cut out from the thermoplastic resin film before the surface roughness was imparted, and the pencil hardness of the surface of the first resin layer was measured in accordance with JIS K5600-5-4. The evaluation was based on the following criteria: Good (◯): Pencil hardness of B or higher, Poor (×): Pencil hardness of 2B or lower.

[0151] [Materials] The materials used are as follows. <Methacrylic resins (M)> (MG-1): glutarimide resin obtained in Production Example PE11 described below (Mw = 85,000, MMA unit amount / GI unit amount / αMSt unit amount / St unit amount = 23% by mass / 53% by mass / 16% by mass / 8% by mass, Tg = 143°C), (MG-2): glutarimide resin, "PLEXIMID TT50" manufactured by Polypla-Evonik (Mw = 76,000, MMA unit amount / N-methylglutarimide unit amount = 30% by mass / 70% by mass, Tg = 150°C), (M-3): polymethyl methacrylate (PMMA), "PARAPET SP" manufactured by Kuraray Co., Ltd. (Mw = 70,000, MMA unit amount = 100% by mass, rr ratio = 75%, Tg = 131°C), (M-4): A copolymer of methyl methacrylate (MMA) and methyl acrylate (MA), "Parapet HR" manufactured by Kuraray Co., Ltd. (Mw = 90,000, MMA unit amount / MA unit amount = 99.3% by mass / 0.7% by mass, rr ratio = 52%, Tg = 117°C).

[0152] <Multilayered Polymer Particles (RP-1) and (RP-2)> A first rubber component layer (Ia) (first layer), a second rubber component layer (Ib) (second layer), and a thermoplastic resin component layer (II) (third layer), each composed of a copolymer having the following composition, were successively formed by a known method to produce three-layered acrylic multilayered polymer particles (RP-1) and (RP-2). First rubber component layer (Ia) (first layer): methyl methacrylate (MMA) units / methyl acrylate (MA) units / allyl methacrylate (ALMA) units (mass ratio) = 94 / 6 / 0.2, Second rubber component layer (Ib) (second layer): n-butyl acrylate (BA) units / styrene units / allyl methacrylate (ALMA) units (mass ratio) = 82 / 18 / 2, Thermoplastic resin component layer (II) (third layer): methyl methacrylate (MMA) units / methyl acrylate (MA) units (mass ratio) = 95 / 5. At the end of formation of the second layer and the third layer, the volume average particle size was measured by dynamic light scattering using a laser diffraction / scattering particle size distribution analyzer. The multilayer structure polymer particles (RP-1) had a first layer / second layer / third layer (mass ratio) of 10 / 50 / 40, a weight average molecular weight (Mw) of the outermost layer of 63,000, a volume average particle diameter of the two layers (first and second layers) of 0.09 μm, and a volume average particle diameter of the three layers (first to third layers) of 0.11 μm. The multilayer structure polymer particles (RP-2) had a first layer / second layer / third layer (mass ratio) of 35 / 45 / 20, a weight average molecular weight (Mw) of the outermost layer of 62,000, a volume average particle diameter of the two layers (first and second layers) of 0.21 μm, and a volume average particle diameter of the three layers (first to third layers) of 0.23 μm. The particle structure and physical properties of the resulting multilayer structure polymer particles are shown in Table 1.

[0153]

[0154] <Block Copolymer (BL)> (BL-1): A triblock copolymer consisting of [methyl methacrylate (MMA) polymer block]-[n-butyl acrylate (BA) polymer block]-[methyl methacrylate (MMA) polymer block], having a weight average molecular weight (Mw) of 70,000 and a ratio (mass ratio) of the total amount of MMA polymer blocks to the amount of BA polymer blocks (mass ratio) of 50 / 50.

[0155] <Polycarbonate Resin (PC)> (PC-1): Polycarbonate resin, "SD Polyca 300 Series" manufactured by Sumika Polycarbonate Co., Ltd. (Mw=50,000, Tg=150°C).

[0156] <Aromatic Polyester> (PCT) Commercially available polycyclohexanedimethylene terephthalate.

[0157] [Production Example PE11] (Production of Glutarimide Resin (MG-1)) (Precursor Resin Production Process) 68.0 parts by mass of purified methyl methacrylate (MMA), 28.0 parts by mass of α-methylstyrene (αMSt), 7.0 parts by mass of styrene (St), 0.05 parts by mass of 2,2'-azobis(2-methylpropionitrile) (AIBN), and 0.01 parts by mass of n-octyl mercaptan (n-OM) were charged into an autoclave equipped with a stirrer and uniformly dissolved to obtain a polymerization raw material. Nitrogen gas was blown into this polymerization raw material to adjust the dissolved oxygen concentration to 3 ppm. Next, a continuous flow tank-type reactor equipped with a brine cooling condenser was prepared, and the interior thereof was purged with nitrogen gas. The polymerization raw materials were continuously fed into the reactor at a constant flow rate so that the average residence time was 3 hours. Bulk polymerization was carried out at a polymerization temperature of 140°C, and a liquid containing precursor resin (Pre-1) (methacrylic resin) was continuously discharged from the reactor. The pressure inside the reactor was adjusted using a pressure control valve connected to a brine cooling condenser. The polymerization conversion rate was 35%. The liquid discharged from the reactor was then heated to 210°C and fed to a twin-screw extruder adjusted to 230°C. Volatiles, primarily consisting of unreacted monomers, were separated and removed. The resin was extruded into strands and cut using a pelletizer to obtain pellets of precursor resin (Pre-1) (MMA / αMSt / St copolymer). The composition and physical properties of the resulting precursor resin were as follows: Mw = 85,000, MMA unit amount / αMSt unit amount / St unit amount = 76 mass % / 16 mass % / 8 mass %, Tg = 124°C.

[0158] (Glutarimide Cyclization Step) A twin-screw extruder ("TEX30α-77AW-3V" manufactured by Nippon Steel Corporation) having a transport section, a melt-kneading section, a devolatilizing section, and a discharge section, with the screw rotation speed set to 150 rpm and the temperature set to 210 to 270°C, was prepared. A precursor resin (Pre-1) was supplied to the transport section of this twin-screw extruder at a flow rate of 15 kg / hr, and monomethylamine was injected as an imidizing agent from the additive supply port of the twin-screw extruder in an amount such that the glutarimide (GI) unit content was the value described below. In the melt-kneading section including the kneading block, the precursor resin (Pre-1) and monomethylamine were reacted. From the resulting molten resin, by-products and excess monomethylamine were volatilized in the devolatilizing section and discharged through multiple vents. The molten resin was extruded in the form of a strand from a die provided at the end of the discharge section of the twin-screw extruder, cooled in a water bath, and cut with a pelletizer to obtain a pellet-shaped glutarimide resin (MG-1). The composition and physical properties of the obtained glutarimide resin were as follows: Mw = 85,000, MMA unit amount / GI unit amount / αMSt unit amount / St unit amount = 23% by mass / 53% by mass / 16% by mass / 8% by mass, and Tg = 143°C.

[0159] [Preparation of methacrylic resin (composition) (MR) or (MRC)] As resin (composition) (MR-1), 100 parts by mass of pellets of glutarimide resin (MG-1) were prepared. As resin (composition) (MR-2), 100 parts by mass of pellets of glutarimide resin (MG-2) were prepared. As resin (composition) (MR-3), 100 parts by mass of pellets of methacrylic resin (M-3) were prepared. As comparative resin (composition) (MRC-4), 100 parts by mass of pellets of methacrylic resin (M-4) were prepared. The compositions and glass transition temperatures (Tg) of the resins (compositions) are shown in Table 2.

[0160] [Production Example PE21] 55 parts by mass of pellets of methacrylic resin (M-4), 34 parts by mass of pellets of multilayer structure polymer particles (RP-1), 7 parts by mass of pellets of multilayer structure polymer particles (RP-2), and 4 parts by mass of pellets of block copolymer (BL-1) were melt-kneaded using a twin-screw extruder and pelletized using a pelletizer to obtain a thermoplastic resin composition (methacrylic resin composition) (TR-1). The obtained thermoplastic resin composition had a Tg of 105°C. The blending composition and glass transition temperature (Tg) are shown in Table 2.

[0161] [Production Example PE22] 61 parts by mass of polycarbonate resin (PC-1) and 39 parts by mass of polycyclohexanedimethylene terephthalate (PCT) were mixed to obtain a thermoplastic resin composition (polycarbonate resin composition) (TR-2). The obtained thermoplastic resin composition had a Tg of 120°C. The blend composition and glass transition temperature (Tg) are shown in Table 2.

[0162] [Preparation of Thermoplastic Resin (Composition) (TR)] 100 parts by mass of pellets of polycarbonate resin (PC-1) were prepared as resin (composition) (TR-3). The composition and glass transition temperature (Tg) are shown in Table 2.

[0163]

[0164] [Examples E1 to E4, Comparative Examples EC1 to EC3] The resins (compositions) (MR), (MRC), or (TR) shown in Table 3 were prepared as the resins (compositions) for the first resin layer. The resins (compositions) (TR) shown in Table 3 were prepared as the resins (compositions) for the second resin layer. The resins (compositions) for the first resin layer and the resins (compositions) for the second resin layer were each placed in the hoppers of separate 25 mmφ vented single-screw extruders ("VGM25-28EX" manufactured by G.M. ENGINEER JNG) and melt-kneaded. These resins (compositions) were introduced into a junction block and co-extruded at an extrusion temperature of 250°C using a multi-manifold die. The thickness of each layer was adjusted by adjusting the discharge rate of each resin (composition). Next, the molten co-extruded resin (composition) was sandwiched between adjacent first and second cooling rolls, wrapped around the second cooling roll, sandwiched between the second and third cooling rolls, and cooled by being wrapped around the third cooling roll. After cooling, the resulting film was taken up by a pair of take-up rolls. In this manner, a two-layer thermoplastic resin film was produced. The exposed surface of the first resin layer of the resulting thermoplastic resin film was embossed using an embossing roll (grain roll) at a resin temperature of 180°C. In this manner, a thermoplastic resin film with a textured surface was obtained, in which the exposed surface of the first resin layer was a textured surface. The main manufacturing conditions and evaluation results are shown in Table 3. The temperature conditions for the storage modulus (E') of the first resin layer and the heating temperature conditions for evaluating the surface texture retention were the glass transition temperature (Tg(2)) of the constituent material of the second resin layer + 20°C. In each example in Table 3, conditions not listed in the table were common conditions.

[0165] Comparative Example EC4: The resin (composition) (TR) shown in Table 3 was prepared as the resin (composition) for the first resin layer. This resin (composition) was placed in the hopper of a 25 mmφ vented single-screw extruder, melt-kneaded, extruded at an extrusion temperature of 250°C, cooled using first to third cooling rolls, and the film obtained after cooling was taken up by a pair of take-up rolls. In this manner, a single-layer thermoplastic resin film was produced. One surface of the obtained thermoplastic resin film was embossed using an embossing roll (shiboron) at a resin temperature of 180°C. In this manner, a thermoplastic resin film with a textured surface, one surface of which was textured, was obtained. The main production conditions and evaluation results are shown in Table 3. The temperature conditions for the storage modulus (E') of the first resin layer and the heating temperature conditions for evaluating the surface texture retention rate were the glass transition temperature (Tg(1)) of the constituent material of the first resin layer + 20°C.

[0166]

[0167] [Summary of Results] In Examples E1 to E4, a laminated thermoplastic resin film was produced, comprising a first resin layer made of a methacrylic resin (composition) (MR) and a second resin layer made of a thermoplastic resin (composition) (TR) having a glass transition temperature lower than that of the methacrylic resin (composition) (MR). In these examples, when the glass transition temperature of the methacrylic resin (composition) (MR) is Tg(1) [°C] and the glass transition temperature of the thermoplastic resin (composition) (TR) is Tg(2) [°C], Tg(1) ≧ 130 and Tg(1) ≧ Tg(2) + 20, and the storage modulus (E') of the first resin layer at a temperature of Tg(2) + 20 [°C] was 10 MPa or more. In addition, the ratio of the thickness of the first resin layer to the thickness of the second resin layer was 1 / 1 to 1 / 10. In all of the thermoplastic resin films obtained in these examples, the surface hardness of the first resin layer was high and favorable. In all of the thermoplastic resin films obtained in these examples, unevenness could be imparted well to the exposed surface of the first resin layer, and the retention of the surface unevenness after heating at Tg(2)+20°C was high and good. Tg(2)+20°C is a suitable temperature for secondary molding. In all of the thermoplastic resin films obtained in these examples, the retention of the surface unevenness when secondary molded after imparting unevenness was high and good.

[0168] [Comparative Examples EC1 and EC2] In Comparative Examples EC1 and EC2, a laminated thermoplastic resin film was produced, consisting of a first resin layer made of a methacrylic resin (composition) (MR) and a second resin layer made of a thermoplastic resin (composition) (TR). In Comparative Example EC1, Tg(1) was 130°C or higher, but Tg(2) was higher than Tg(1). Therefore, the storage modulus (E') of the first resin layer at a temperature of Tg(2) + 20°C was less than 10 MPa. The obtained thermoplastic resin film was able to impart irregularities to the exposed surface of the first resin layer, but the retention of the surface irregularities after heating at Tg(2) + 20°C was low and poor. Because the storage modulus (E') of the first resin layer at a temperature of Tg(2) + 20°C was low, the first resin layer softened and reverted to its original shape when heated at Tg(2) + 20°C. The obtained thermoplastic resin film was poor in that it had a low retention rate of the surface irregularities when subjected to secondary molding after being provided with irregularities.

[0169] In Comparative Example EC2, Tg (2) was lower than Tg (1), but Tg (1) was less than 130 ° C., the difference between Tg (1) and Tg (2) was less than 20 ° C., and the storage modulus (E ') of the first resin layer at a temperature of Tg (2) + 20 [° C.] was less than 10 MPa. The obtained thermoplastic resin film was able to impart irregularities to the exposed surface of the first resin layer, but the retention of the surface irregularities after heating at Tg (2) + 20 [° C.] was low and poor. Because the storage modulus (E ') of the first resin layer at a temperature of Tg (2) + 20 [° C.] was low, the first resin layer softened when heated at Tg (2) + 20 [° C.], and reshaping occurred. The obtained thermoplastic resin film had a low retention of surface irregularities when subjected to secondary molding after imparting irregularities, and was poor.

[0170] [Comparative Example EC3] In Comparative Example EC3, a laminated thermoplastic resin film was produced, consisting of a first resin layer containing a polycarbonate resin but not a methacrylic resin, and a second resin layer containing a polycarbonate resin but not a methacrylic resin. In this comparative example, Tg(1) was 130°C or higher, Tg(2) was lower than Tg(1), the difference between Tg(1) and Tg(2) was 20°C or higher, and the storage modulus (E') of the first resin layer at a temperature of Tg(2) + 20°C was 10 MPa or higher. The obtained thermoplastic resin film was able to impart irregularities to the exposed surface of the first resin layer, and the retention of the surface irregularities after heating at Tg(2) + 20°C was high and favorable. However, the obtained thermoplastic resin film had a first resin layer that did not contain a methacrylic resin, and the surface hardness of the first resin layer was poor.

[0171] [Comparative Example EC4] In Comparative Example EC4, a single-layer thermoplastic resin film consisting only of a first resin layer made of a methacrylic resin (composition) (MR) was obtained. The Tg (1) was less than 130°C, and the storage modulus (E') of the first resin layer at a temperature of Tg (1) + 20°C was less than 10 MPa. The obtained thermoplastic resin film was able to impart irregularities to the exposed surface of the first resin layer, but the retention of the surface irregularities after heating at Tg (1) + 20°C was low and unsatisfactory. Because the storage modulus (E') of the first resin layer at a temperature of Tg (1) + 20°C was low, the first resin layer softened and reverted to its original shape when heated at Tg (1) + 20°C. The obtained thermoplastic resin film was poor in terms of the retention of the surface irregularities when subjected to secondary molding after imparting irregularities.

[0172] The present invention is not limited to the above-described embodiments and examples, and appropriate design changes are possible without departing from the spirit of the present invention.

[0173] This application claims priority based on Japanese Patent Application No. 2023-064606, filed April 12, 2023, the disclosure of which is incorporated herein by reference in its entirety.

[0174] REFERENCE SIGNS LIST 1, 16 Thermoplastic resin film 2, 3 Laminated film 21 First resin layer 22 Second resin layer 31 Printed layer 41 Hard coat layer

Claims

1. A thermoplastic resin film having a first resin layer made of a methacrylic resin (composition) (MR) and a second resin layer made of a thermoplastic resin (composition) (TR) having a glass transition temperature lower than that of the methacrylic resin (composition) (MR), wherein, when the glass transition temperature of the methacrylic resin (composition) (MR) is Tg(1) [°C] and the glass transition temperature of the thermoplastic resin (composition) (TR) is Tg(2) [°C], Tg(1)≧130 and Tg(1)≧Tg(2)+20, the storage modulus (E') of the first resin layer at a temperature of Tg(2)+20 [°C] is 10 MPa or more, and the ratio of the thickness of the first resin layer to the thickness of the second resin layer is 1 / 1 to 1 / 10.

2. The thermoplastic resin film described in claim 1, wherein the storage modulus (E') of the first resin layer of the methacrylic resin (composition) (MR) at a temperature of Tg(2) + 20°C is 3000 MPa or less.

3. The thermoplastic resin film according to claim 1, wherein the methacrylic resin (composition) (MR) contains a methacrylic resin (M-RS) having, in the main chain, one or more ring structure units selected from the group consisting of an acid anhydride unit, an imide unit having a ring structure, and a lactone ring unit.

4. The thermoplastic resin film according to claim 3, wherein the methacrylic resin (composition) (MR) contains a glutarimide resin (MG) containing methyl methacrylate units and glutarimide units.

5. The thermoplastic resin film according to claim 4, wherein the glutarimide resin (MG) further contains an aromatic vinyl monomer unit.

6. The thermoplastic resin film according to claim 5, wherein the aromatic vinyl monomer units include one or more styrene-based monomer units selected from the group consisting of styrene units and α-methylstyrene units.

7. The thermoplastic resin film according to claim 6, wherein the glutarimide resin (MG) contains 5 to 73 mass% methyl methacrylate units, 25 to 70 mass% glutarimide units represented by the following formula (I), 1 to 48 mass% α-methylstyrene units, 1 to 48 mass% of one or more units selected from the group consisting of styrene units and maleic anhydride units, and 0 to 20 mass% unsubstituted or N-substituted maleimide units. (In formula (I), two R 1 are each independently a hydrogen atom or a methyl group; R 2 is a hydrogen atom, an alkyl group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, or an organic group having 6 to 15 carbon atoms and containing an aromatic ring.

8. The thermoplastic resin film according to claim 1, wherein the glass transition temperature of the methacrylic resin (composition) (MR) is 140° C. or higher.

9. The thermoplastic resin film according to claim 1, wherein the thermoplastic resin (composition) (TR) is a methacrylic resin composition (T-MR) containing a methacrylic resin (TM) and a rubber-like polymer (R), or a polycarbonate resin composition (T-PC) containing a polycarbonate resin (PC).

10. The thermoplastic resin film according to claim 1, wherein one surface of the first resin layer is exposed, and the exposed surface of the first resin layer is an uneven surface.

11. The thermoplastic resin film of claim 1 which is a coextruded film.

12. A laminated film comprising the thermoplastic resin film according to any one of claims 1 to 11 and a printed layer formed on the surface of the second resin layer of the thermoplastic resin film opposite to the first resin layer.

13. A laminated film comprising the thermoplastic resin film according to any one of claims 1 to 11 and a hard coat layer formed on the surface of the first resin layer of the thermoplastic resin film opposite to the second resin layer.

Citation Information

Patent Citations

  • Resin laminate for forming while providing protective film, protective film-provided molding and molding

    JP2014237302A

  • Methacrylic resin composition, optical film, and optical component

    JP2018002994A

  • Liquid crystal display protection plate, liquid crystal display protection plate having curved surface and method for manufacturing the same

    JP2022025963A

  • Multilayer film and decorative molded body of fiber-reinforced resin

    WO2019065912A1

  • Resin composition and molded object

    WO2023219103A1