Adhesive composition, cured body, laminate, optical article, lens, and spectacles
The polyurethaneurea resin-based adhesive composition with a specific structure addresses the limitation of rigid matrices in existing technologies by enabling structural changes of functional dyes, enhancing the functionality and adhesion in photochromic lenses.
Patent Information
- Application Number
- PCT/JP2024/014532
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-12
- Filing Date
- 2024-04-10
- Publication Date
- 2024-10-17
AI Technical Summary
Existing adhesive compositions for manufacturing photochromic lenses often limit the structural changes of functional dyes due to their rigid matrix structure, hindering their functionality.
A polyurethaneurea resin-based adhesive composition with a specific structure, including a urea bond and a urethane bond, is used, which provides a more flexible matrix allowing for structural changes of functional dyes, enhancing their functionality.
The adhesive composition enables excellent functionality and adhesion, improving the performance of photochromic lenses by allowing structural changes of functional dyes within a flexible matrix.
Smart Images

Figure JP2024014532_17102024_PF_FP_ABST
Abstract
Description
Adhesive composition, cured product, laminate, optical article, lens, and eyeglasses
[0001] The present invention relates to an adhesive composition, a cured product, a laminate, an optical article, a lens, and eyeglasses.
[0002] Plastic eyeglasses are eyeglasses that use plastic lenses. Plastic lenses are manufactured by, for example, subjecting semi-finished lenses, which are semi-finished products, to various processes. The convex front surface of the semi-finished lens is provided with a functional layer such as a hard coat layer or an anti-reflection film. The concave back surface of the semi-finished lens is also subjected to cutting and polishing.
[0003] In recent years, photochromic lenses, which change color depending on the amount of ultraviolet light, have been attracting attention. Photochromic lenses are obtained by adding a photochromic compound to a plastic lens. A photochromic compound is a compound that can reversibly generate two or more isomers with different light absorption spectra when exposed to light.
[0004] Conventional methods for manufacturing photochromic lenses include a kneading method in which a photochromic compound is dispersed in the matrix of a semi-finished lens, and a lamination method in which a layer containing a photochromic compound is formed on the surface of a semi-finished lens.
[0005] The binder sheet method is a method for producing a semi-finished lens by integrating a binder sheet, which is formed by sandwiching a resin layer containing a photochromic compound between two optical sheets, with a lens substrate. In this method, for example, a semi-finished lens is obtained by mounting the binder sheet in a mold and injection-molding a thermoplastic resin toward the binder sheet. The binder sheet method allows for the production of a semi-finished lens using a free-standing article containing a photochromic compound, which tends to improve production efficiency and facilitate mass production compared to the kneading method and lamination method.
[0006] JP 2016-169363 A International Publication No. 2013 / 099640 JP 2013-033131 A
[0007] An object of the present invention is to provide an adhesive composition capable of realizing an adhesive layer with excellent functionality, and a cured product thereof, a laminate, an optical article, a lens, and spectacles.
[0008] According to the present disclosure, there is provided an adhesive composition comprising a polyurethaneurea resin and an organic solvent, the polyurethaneurea resin having a urea bond, a urethane bond, and a structure represented by the following formula (I):
[0009]
[0010] In formula (I), R 1 and R 2 are each independently a linear alkylene group having 3 to 10 carbon atoms. 1 is 0 or 1 to 25. n and m are each independently 2 to 70.
[0011] According to the present disclosure, a cured product is provided. This cured product is a cured product of an adhesive composition according to an embodiment.
[0012] According to the present disclosure, there is provided a laminate. The laminate includes a resin layer and an optical substrate. The resin layer includes a cured product according to an embodiment.
[0013] According to the present disclosure, an optical article is provided, the optical article including a laminate according to an embodiment.
[0014] According to the present disclosure, a lens is provided, the lens including an optical article according to an embodiment.
[0015] According to the present disclosure, there is provided a pair of eyeglasses, the eyeglasses including lenses according to another embodiment.
[0016] According to the present invention, there are provided an adhesive composition capable of realizing an adhesive layer with excellent functionality, a cured product thereof, a laminate, an optical article, a lens, and spectacles.
[0017] 1 is a cross-sectional view schematically showing an example of a laminate according to an embodiment; 2 is a cross-sectional view schematically showing another example of a laminate according to an embodiment; 3 is a cross-sectional view schematically showing an example of a coating layer-containing laminate according to an embodiment; 4 is a cross-sectional view schematically showing an example of an optical article according to an embodiment; and 5 is a perspective view schematically showing an example of eyeglasses according to an embodiment.
[0018] According to an embodiment, there is provided an adhesive composition comprising a polyurethane urea resin and an organic solvent, the polyurethane urea resin having a urea bond, a urethane bond, and a structure represented by formula (I) above.
[0019] The adhesive composition can be used to achieve an adhesive layer with excellent functionality. The reasons for this are believed to be as follows: First, functional dyes include compounds capable of selectively absorbing visible light, as well as compounds that develop, lose, or change color in response to energy such as light, heat, an electric field, or pressure. Such functional dyes can exhibit specific functions by undergoing structural changes under specific conditions. Generally, the matrix of a cured plastic has a rigid structure. Therefore, functional dyes in a cured product are less likely to undergo structural changes than in a solution, and their functions may be limited. An adhesive composition according to an embodiment contains a polyurethane urea resin having a structure represented by the above formula (I). That is, this polyurethane urea resin has a structure containing a linear alkylene glycol having 3 to 10 carbon atoms as a repeating unit. In a cured product of an adhesive composition containing such a polyurethane urea resin, the alkylene glycol chain structure is believed to contribute to providing a matrix in which the functional dye can easily undergo structural changes.
[0020] That is, polyurethane urea resin is a polymer consisting of a urethane bond (-OC(=O)N(H)-) formed by a polyaddition reaction between an isocyanate group (-N=C=O) and a hydroxyl group (-OH), and a bond formed by a polyaddition reaction between an isocyanate group and an amino group (-NH 2) and a resin containing a plurality of urea bonds (—NH—C(═O)—NH—) formed by a polyaddition reaction with a diamine. Such resins are thought to have a structure in which polymer chains obtained by reacting a urethane prepolymer obtained by reacting a diisocyanate with a diol are intricately entangled. In urethane urea resins, intermolecular interactions are thought to occur between the polymer chains due to hydrogen bonding or the like. The structure represented by formula (I) has a lower proportion of heteroatoms, such as oxygen atoms, per unit mass than a polypropylene glycol chain structure, a chain consisting solely of a polycarbonate structure, or a polyester polycarbonate structure. Therefore, the structure represented by formula (I) is thought to have lower polarity than other structures and to be less susceptible to intermolecular interactions. In a cured product of a polyurethane urea resin having the structure represented by formula (I), the polymer chains exhibit low cohesion, resulting in a relatively large distance between the polymer chains and the formation of a more flexible matrix. Therefore, in this cured product, structural changes in the functional dye are less likely to be hindered, allowing the functional dye to exhibit excellent functionality. The adhesive composition according to the embodiment will be described in detail below.
[0021] [Adhesive Composition] The adhesive composition according to the embodiment contains a polyurethane urea resin and an organic solvent.
[0022] (Polyurethane urea resin) The polyurethane urea resin has a urea bond, a urethane bond, and a structure represented by the following formula (I). The structure represented by the following formula (I) is typically a structure derived from a diol. It can be confirmed that the urethane urea resin has the following structure by, for example, nuclear magnetic resonance spectroscopy (NMR) analysis.
[0023]
[0024] In formula (I), R 1 and R 2 are each independently a linear alkylene group having 3 to 10 carbon atoms. 1 and R 2are each independently preferably a linear alkylene group having 4 to 8 carbon atoms, more preferably a linear alkylene group having 4 to 6 carbon atoms. 1 and R 2 is particularly preferably a normal butylene group. 1 and R 2 are preferably of the same structure.
[0025] l is 0, or 1 or more and 25 or less. From the viewpoint of enhancing the functionality of the adhesive layer, l is preferably 0. That is, since a polyalkylene glycol structure has high flexibility, the functionality of the adhesive layer can be enhanced by using a urethane urea resin having such a structure. On the other hand, from the viewpoint of enhancing the adhesiveness of the adhesive layer, l is preferably 1 or more and 25 or less. That is, when a polyurethane urea resin having a polyether (poly)carbonate structure is used, the adhesiveness with resins such as optical substrates tends to be enhanced. When the resin has a polycarbonate structure, the adhesiveness tends to be particularly enhanced. l is preferably 1 or more and 7 or less, and more preferably 2 or more and 6 or less.
[0026] n and m are each independently 2 or more and 70 or less. When l is 0, m is 0. n and m are each a repeating unit R 1 O and R 2 It is preferable that n and m are 3 or more. 1 O or R 2 When the proportion of the molecular weight of O is high, the functionality of the adhesive layer tends to be enhanced. On the other hand, from the viewpoint of enhancing the heat resistance of the adhesive layer, n and m are preferably 16 or less, and more preferably 11 or less. 1 O or R 2 When the proportion of the molecular weight of O is low, the softening point of the polyurethane urea resin increases, and the heat resistance of the adhesive layer tends to be improved. n and m may be 7 or more and 10 or less, 9 or more and 15 or less, 20 or more and 40 or less, 25 or more and 35 or less, or 50 or more and 60 or less.
[0027] The softening point of the polyurethane urea resin is, for example, 40°C or higher and 200°C or lower. The softening point is preferably 50°C or higher, and more preferably 60°C or higher. A higher softening point tends to increase the heat resistance of the adhesive layer. The softening point can be measured, for example, by thermomechanical analysis (TMA). The urethane urea resin can have a structure represented by the following formula (II).
[0028]
[0029] In formula (II), X is a structure represented by formula (I). 3 and R 4 are each independently a substituted or unsubstituted linear or branched alkylene group, a substituted or unsubstituted cycloalkylene group, a substituted or unsubstituted dicycloalkylene group, a substituted or unsubstituted arylene group, a substituted or unsubstituted diarylene group, a norbornyl group, or a divalent group represented by the following formula (III): 5 -Y-R 5 - (III)
[0030] In formula (III), R 5 is a substituted or unsubstituted cycloalkylene group or a substituted or unsubstituted arylene group. Y is a substituted or unsubstituted linear or branched alkylene group or an oxygen atom.
[0031] R 3 R may be a structure derived from a diisocyanate. 3 is preferably a substituted or unsubstituted linear or branched alkylene group, a substituted or unsubstituted cycloalkylene group, a substituted or unsubstituted dicycloalkylene group, or a divalent group represented by formula (III), and more preferably a substituted or unsubstituted cycloalkylene group.
[0032] R 4 R may be a structure derived from a diamine. 4is preferably a substituted or unsubstituted linear or branched alkylene group, a substituted or unsubstituted cycloalkylene group, a substituted or unsubstituted dicycloalkylene group, or a divalent group represented by formula (III), and more preferably a substituted or unsubstituted cycloalkylene group or a divalent group represented by formula (III). 3 and R 4 are preferably different in structure from each other.
[0033] R 3 or R 4 In the above formula, the number of carbon atoms in the alkylene group is, for example, 1 or more and 10 or less, and preferably 3 or more and 8 or less. The alkylene group is preferably an unsubstituted linear alkylene group.
[0034] In Y, the number of carbon atoms in the alkylene group is, for example, 1 or more and 5 or less, and preferably 1 or 2. The alkylene group is preferably an unsubstituted methylene group.
[0035] R 3 , R 4 , or R 5 In the formula (I), the number of carbon atoms in the cycloalkylene group is, for example, 4 or more and 20 or less, and preferably 6 or more and 15 or less. The cycloalkylene group is preferably an unsubstituted cyclohexyl group or a cyclohexyl group having an alkyl group as a substituent.
[0036] R 3 , R 4 , or R 5 In the above formula, the number of carbon atoms in the arylene group is, for example, 4 or more and 20 or less, and preferably 6 or more and 15 or less. The arylene group is preferably an unsubstituted phenylene group or an unsubstituted naphthylene group.
[0037] p is an integer of 1 or more and 9 or less. q is an integer of 3 or more and 56 or less. q is preferably an integer of 7 or more and 38 or less.
[0038] Both ends of the urethane urea resin represented by the above formula (II) may be an isocyanate group or a hydroxyl group, but may also be modified with a terminating group. The terminating group is preferably a substituted or unsubstituted alkyl group, a substituted or unsubstituted piperidino group, or a substituted or unsubstituted alkylenepiperidino group. The number of carbon atoms in the alkyl group is, for example, 1 or more and 10 or less, preferably 2 or more and 7 or less. The piperidino group is preferably a 2,2,6,6-tetramethylpiperidino group. With such a structure, light stability tends to be improved due to the effect of the hindered amine light stabilizer.
[0039] (Organic Solvent) In the adhesive composition, the polyurethane urea resin may be dissolved or dispersed in an organic solvent. The proportion of the polyurethane urea resin in the adhesive composition is, for example, 10% by mass or more and 60% by mass or less. This proportion is preferably 15% by mass or more and 50% by mass or less, and more preferably 20% by mass or more and 40% by mass or less.
[0040] The organic solvent used is one that can dissolve or disperse the polyurethane urea resin. The organic solvent includes, for example, at least one selected from the group consisting of N,N-dimethylformamide, N-methyl-2-pyrrolidone (NMP), tertiary butanol, diethyl ketone, tetrahydrofuran, cyclohexanone, cyclopentanone, methyl isobutyl ketone, and toluene. The organic solvent preferably includes at least one selected from the group consisting of N,N-dimethylformamide, tertiary butanol, diethyl ketone, tetrahydrofuran, and toluene.
[0041] In the adhesive composition, the organic solvent accounts for the remainder of the other substances contained in the adhesive composition. The proportion of the organic solvent is, for example, 40% by mass or more and 90% by mass or less. This proportion is preferably 50% by mass or more and 85% by mass or less, and more preferably 60% by mass or more and 80% by mass or less.
[0042] (Functional Dye) The adhesive composition may further contain a functional dye. The functional dye includes, for example, at least one selected from the group consisting of a photochromic compound, an ultraviolet absorber, a blue light absorber, a high-energy visible light absorber, an infrared absorber, a dye, and an electrochromic compound.
[0043] As the photochromic compound, for example, at least one selected from the group consisting of chromene compounds, fulgide compounds, and spirooxazine compounds is used. As the photochromic compound, a chromene compound is preferably used. Chromene compounds include compounds having a 1-benzopyran skeleton, spiropyran compounds having a spiropyran skeleton, and naphthopyran compounds having a naphthopyran skeleton. Naphthopyran compounds include indenonaphthopyran compounds having an indenonaphthopyran skeleton. Chromene compounds preferably include indenonaphthopyran compounds having an indeno[2,1-f]naphtho[1,2-b]pyran skeleton. Cured products containing chromene compounds having an indeno[2,1-f]naphtho[1,2-b]pyran skeleton tend to have excellent durability. The indenonaphthopyran compound preferably includes a compound represented by the following formula (IIIa):
[0044]
[0045] In formula (IIIa), R 11 , R 12 , R 13 , R 14 , R 15 , and R 16are each independently a hydrogen atom, a hydroxyl group, a methoxycarbonyl group, an ethoxycarbonyl group, an alkyl group, a cycloalkyl group, a haloalkyl group, an alkoxy group, an amino group, a substituted amino group, an optionally substituted heterocyclic group, a halogen atom, an alkylthio group, an optionally substituted arylthio group, a nitro group, a formyl group, a hydroxycarbonyl group, an alkylcarbonyl group, an alkoxycarbonyl group, an optionally substituted aralkyl group, an optionally substituted aralkoxy group, an optionally substituted aryloxy group, an optionally substituted aryl group, an optionally substituted heteroaryl group, a thiol group, an alkoxyalkylthio group, a haloalkylthio group, an optionally substituted cycloalkylthio group, or an oligomer group.
[0046] The number of carbon atoms in the alkyl group is preferably 1 to 10. Examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, a tert-butyl group, a pentyl group, and a hexyl group.
[0047] The haloalkyl group preferably has 1 to 10 carbon atoms. The haloalkyl group is preferably an alkyl group substituted with a fluorine atom, a chlorine atom, or a bromine atom. Suitable examples of the haloalkyl group include a trifluoromethyl group, a tetrafluoroethyl group, a chloromethyl group, a 2-chloroethyl group, and a bromomethyl group.
[0048] The number of ring carbon atoms in the cycloalkyl group is preferably 3 to 8. Examples of the cycloalkyl group include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, and a cyclohexyl group. The cycloalkyl group may have a substituent, but the number of ring carbon atoms (3 to 8 carbon atoms) does not include the number of carbon atoms in the substituent.
[0049] The number of carbon atoms in the alkoxy group is preferably 1 to 10, and more preferably 1 to 6. Suitable examples of the alkoxy group include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, a sec-butoxy group, and a tert-butoxy group.
[0050] The amino group is a primary amino group (-NH 2 ) The substituted amino group is a secondary or tertiary amino group in which one or two hydrogen atoms have been substituted. Examples of the substituent on the substituted amino group include an alkyl group having 1 to 6 carbon atoms, a haloalkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a cycloalkyl group having 3 to 7 carbon atoms, an aryl group having 6 to 14 carbon atoms, and a heteroaryl group having 4 to 14 carbon atoms. Examples of suitable amino groups include an amino group, a methylamino group, a dimethylamino group, an ethylamino group, a diethylamino group, a phenylamino group, and a diphenylamino group.
[0051] The heterocyclic group preferably has 3 to 10 ring members. The heterocyclic group may be an aliphatic heterocyclic group or an aromatic heterocyclic group. Specific examples of the aliphatic heterocyclic group include a morpholino group, a piperidino group, a pyrrolidinyl group, a piperazino group, and an N-methylpiperazino group. Specific examples of the aromatic heterocyclic group include an indolinyl group. The heterocyclic group may have a substituent. Preferred examples of the substituent include an alkyl group having 1 to 10 carbon atoms. Suitable examples of the substituted heterocyclic group include a 2,6-dimethylmorpholino group, a 2,6-dimethylpiperidino group, and a 2,2,6,6-tetramethylpiperidino group.
[0052] Examples of halogen atoms include fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms.
[0053] The number of carbon atoms in the alkylthio group is preferably 1 to 10. Examples of the alkylthio group include a methylthio group, an ethylthio group, an n-propylthio group, an isopropylthio group, an n-butylthio group, a sec-butylthio group, and a t-butylthio group.
[0054] The number of carbon atoms in the arylthio group is preferably 6 to 10. Examples of the arylthio group include a phenylthio group, a 1-naphthylthio group, and a 2-naphthylthio group.
[0055] The number of carbon atoms in the alkylcarbonyl group is preferably 2 to 10. Examples of the alkylcarbonyl group include an acetyl group and an ethylcarbonyl group.
[0056] The number of carbon atoms in the alkoxycarbonyl group is preferably 2 to 10. Examples of the alkoxycarbonyl group include a methoxycarbonyl group and an ethoxycarbonyl group.
[0057] The number of carbon atoms in the aralkyl group is preferably 7 to 11. Examples of the aralkyl group include a benzyl group, a phenylethyl group, a phenylpropyl group, a phenylbutyl group, and a naphthylmethyl group.
[0058] The number of carbon atoms in the aralkoxy group is preferably 7 to 11. Examples of the aralkoxy group include a benzyloxy group and a naphthylmethoxy group.
[0059] The number of carbon atoms in the aryl group is preferably 6 to 12. Examples of the aryl group include a phenyl group, a 1-naphthyl group, and a 2-naphthyl group.
[0060] The number of carbon atoms in the aryloxy group is preferably 6 to 12. Examples of the aryloxy group include a phenyloxy group and a naphthyloxy group.
[0061] The number of carbon atoms in the heteroaryl group is preferably 3 to 12. Examples of the heteroaryl group include a thienyl group, a furyl group, a pyrrolinyl group, a pyridyl group, a benzothienyl group, a benzofuranyl group, and a benzopyrrolinyl group.
[0062] The number of carbon atoms in the alkoxyalkylthio group is preferably 2 to 10. Examples of the alkoxyalkylthio group include a methoxymethylthio group, a methoxyethylthio group, a methoxy n-propylthio group, a methoxy n-butylthio group, an ethoxyethylthio group, and an n-propoxypropylthio group.
[0063] The number of carbon atoms in the haloalkylthio group is preferably 1 to 10. Examples of the haloalkylthio group include a trifluoromethylthio group, a tetrafluoroethylthio group, a chloromethylthio group, a 2-chloroethylthio group, and a bromomethylthio group.
[0064] The number of ring carbon atoms in the cycloalkylthio group is preferably 3 to 8. Examples of the cycloalkylthio group include a cyclopropylthio group, a cyclobutylthio group, a cyclopentylthio group, and a cyclohexylthio group. The cycloalkylthio group may have a substituent, but the number of ring carbon atoms (3 to 8 carbon atoms) does not include the number of carbon atoms in the substituent.
[0065] The oligomeric group comprises an oligomeric chain, a linking group, and a terminal group.
[0066] The oligomer chain may include at least one selected from the group consisting of a polyalkylene oxide chain, a polysiloxane chain, and a polyester chain. The oligomer chain is a divalent group.
[0067] The polyalkylene oxide chain has a repeating unit of a linear or branched polyalkylene oxide having 1 to 10 carbon atoms. The number of repeating units is, for example, 3 to 1000. The repeating unit may be, for example, —CH 2 O-, -CH 2 CH 2 O-, -CH(CH 3 ) CH 2 O-, -CH 2 CH (CH 3 ) O—, —CH 2 CH 2 CH 2 O- or -CH 2 CH 2 C(CH 3 ) O-.
[0068] The polysiloxane chain may be, for example, dimethylsilyleneoxy (—Si(CH 3 ) 2 The repeating number of the repeating unit is, for example, 3 or more and 1,000 or less.
[0069] The polyester chain may be, for example, —OC(═O)CH 2 -, -OC(=O)CH 2 CH 2 CH 2 CH 2 C(=O)O- or -OC(=O)CH 2 CH 2 CH 2 CH 2 C(=O)OCH 2 CH 2 The number of repetitions of the repeating unit is, for example, 3 or more and 1,000 or less.
[0070] The linking group connects the photochromic compound to one end of the oligomer chain. Examples of the linking group include —O— and —O—CH 2 CH 2 —O—, —O—CH 2 CH 2 -OC(=O)CH 2 CH 2 C(═O)—O— or —O—CH 2 CH 2 -OC(=O)CH 2 CH 2 C(=O)-O-CH 2 The linking group may be a divalent group or a group with a valence of two or more.
[0071] The terminal group is bonded to the other end of the oligomer chain. The terminal group is, for example, a linear or branched alkyl group having from 1 to 10 carbon atoms, a linear or branched alkoxy group having from 1 to 10 carbon atoms, a linear or branched alkenyl group having from 2 to 30 carbon atoms, or an organic residue having from 1 to 10 carbon atoms and from 1 to 3 oxygen atoms. The terminal group is preferably a methyl group.
[0072] The oligomer group may include a first linking group, an oligomer chain, and a second linking group. The first linking group and the second linking group may have the same structure or different structures. The first linking group is linked to a first photochromic compound. The second linking group is linked to a second photochromic compound. The first photochromic compound and the second photochromic compound may have the same structure or different structures.
[0073] The above-mentioned cycloalkyl group, arylthio group, aralkyl group, aralkoxy group, aryloxy group, aryl group, heteroaryl group, and cycloalkylthio group may be unsubstituted or may have a substituent.
[0074] Substituents that may be substituted on the cycloalkyl group, arylthio group, aralkyl group, aralkoxy group, aryloxy group, aryl group, heteroaryl group, and cycloalkylthio group may be selected from the group consisting of a primary amino group, a secondary amino group, a tertiary amino group, an alkyl group having 1 to 10 carbon atoms, a haloalkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, a haloalkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, a hydroxyl group, a cycloalkyl group having 3 to 8 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkylaryl group having 1 to 20 carbon atoms, a heterocycloalkyl group having 1 to 8 carbon atoms and containing 1 to 5 heteroatoms, a heteroaryl group having 1 to 8 carbon atoms and containing 1 to 5 heteroatoms, an aryloxy group having 6 to 12 carbon atoms, an arylthio group having 6 to 12 carbon atoms, a cyano group, a nitro group, and a halogen atom. The number of substituents may be one or more.
[0075] Two adjacent R 13 , two adjacent R 14 , and R 15 and R 16may be bonded to each other to form an aliphatic ring having from 2 to 5 carbon atoms, an aliphatic heterocyclic ring having from 1 to 4 carbon atoms and containing from 1 to 3 heteroatoms, an aromatic ring having from 4 to 12 carbon atoms, or an aromatic heterocyclic ring having from 3 to 11 carbon atoms and containing from 1 to 6 heteroatoms. The aliphatic ring, the aliphatic heterocyclic ring, the aromatic ring, and the aromatic heterocyclic ring may be unsubstituted or may have at least one substituent selected from the above-mentioned group of substituents. 15 and R 16 may form a substituted or unsubstituted spiro ring with the carbon atom at position 13 as a spiro atom. This ring is preferably an aliphatic ring having 5 to 16 ring carbon atoms. The aliphatic ring more preferably has an alkyl group having 1 to 3 carbon atoms as a substituent.
[0076] In formula (IIIa), r and s each independently represent an integer of 0 to 4. r and s may be 1 or greater, or may be 2 or greater.
[0077] The ultraviolet absorber has an absorption wavelength in the ultraviolet (UV) region of 400 nm or less. The ultraviolet absorber may have a maximum absorption wavelength in the region of 330 nm or more and 380 nm or less, or may have a maximum absorption wavelength in the region of 250 nm or more and less than 330 nm. An organic compound can be used as the ultraviolet absorber. For example, at least one selected from the group consisting of benzophenone derivatives, ethylhexyl methoxycinnamate, benzotriazole derivatives, and triazine derivatives is used as the ultraviolet absorber. Preferably, the ultraviolet absorber includes at least one selected from the group consisting of benzophenone derivatives, ethylhexyl methoxycinnamate, and benzotriazole derivatives.
[0078] As the blue light absorber, a compound having an absorption peak in the wavelength region of more than 400 nm and not more than 450 nm in its absorption spectrum can be used. Such a compound is, for example, at least one selected from the group consisting of perylene compounds, porphyrin compounds, carotenoid compounds, and cyanine compounds. As the blue light absorber, a porphyrin compound is preferably used, and a tetraazaporphyrin compound is more preferably used.
[0079] The high-energy visible light absorber is a blue light absorber having an absorption peak in the wavelength region of 400 nm or more and 420 nm or less. As the high-energy visible light absorber, the same one as the blue light absorber can be used.
[0080] The dye preferably contains a compound having an absorption peak in the wavelength region of 540 nm to 650 nm in its absorption spectrum, and more preferably a compound having an absorption peak in the wavelength region of 550 nm to 600 nm. The inclusion of such a compound enhances the antiglare properties of the optical article. Examples of such compounds include nitro-based compounds, azo-based compounds, anthraquinone-based compounds, threne-based compounds, porphyrin-based compounds, and rare earth metal compounds. It is preferable to use at least one compound selected from the group consisting of tetraazaporphyrin compounds and neodymium compounds.
[0081] Examples of electrochemical compounds include organic compounds such as viologen, electrochemical polymers, and metal salt complexes having d atoms.
[0082] The proportion of the functional dye in the adhesive composition is, for example, 0.1% by mass or more and 10% by mass or less, and preferably 1% by mass or more and 5% by mass or less.
[0083] (Second Polyisocyanate) The adhesive composition may further contain a second polyisocyanate. A cured product of the adhesive composition containing the second polyisocyanate may have a crosslinked structure, such as an allophanate bond or a biuret bond, between polyurethane urea resins. A cured product having such a crosslinked structure tends to have an improved softening point and therefore higher heat resistance.
[0084] The second polyisocyanate contains two or more or three or more isocyanate groups. Preferably, the second polyisocyanate has two or three isocyanate groups.
[0085] The second polyisocyanate preferably contains at least one selected from the group consisting of an aliphatic isocyanate, an alicyclic isocyanate, and an aromatic isocyanate compound. The second polyisocyanate more preferably contains an alicyclic isocyanate, an isocyanate trimer (isocyanurate compound), and an isocyanate biuret compound. The second polyisocyanate may be used alone or in combination.
[0086] Examples of the aliphatic isocyanate include pentamethylene diisocyanate, hexamethylene diisocyanate, heptamethylene diisocyanate, octamethylene diisocyanate, 2,4,4-trimethylhexanemethylene diisocyanate, 1,2-bis(2-isocyanatoethylthio)ethane, and the like.
[0087] Examples of the alicyclic isocyanate include isophorone diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, 1,4-bis(isocyanatomethyl)cyclohexane, dicyclohexylmethane-4,4′-diisocyanate (hydrogenated diphenylmethane diisocyanate), norbornane diisocyanate, 2,5-bis(isocyanatomethyl)-bicyclo[2,2,1]-heptane, and 2,6-bis(isocyanatomethyl)-bicyclo[2,2,1]-heptane.
[0088] Examples of aromatic isocyanates include xylene diisocyanate (o-, m-, p-), toluene-2,4-diisocyanate, toluene-2,6-diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, 1,4-bis(isocyanatomethyl)cyclohexane, and 4,4'-diphenylmethane diisocyanate.
[0089] Examples of the second polyisocyanate include an isomer mixture of 4,4'-methylenebis(cyclohexylisocyanate), cyclobutane-1,3-diisocyanate, cyclohexane-1,3-diisocyanate, cyclohexane-1,4-diisocyanate, hexahydrotoluene-2,4-diisocyanate, hexahydrotoluene-2,6-diisocyanate, hexahydrophenylene-1,3-diisocyanate, and hexahydrophenylene-1,4-diisocyanate. In addition, nurate compounds, biuret compounds, adducts, and the like of polyisocyanate compounds can also be used without any restrictions, and examples thereof include a trimer of isophorone diisocyanate (isocyanurate compound), hexamethylene diisocyanate, a biuret compound of hexamethylene diisocyanate, an isocyanurate compound of hexamethylene diisocyanate, and an adduct compound of hexamethylene diisocyanate.
[0090] Also usable are blocked isocyanates in which the isocyanate groups of the second polyisocyanates shown above are blocked.
[0091] The proportion of the second polyisocyanate in the adhesive composition is, for example, 1% by mass or more and 20% by mass or less, and preferably 1% by mass or more and 10% by mass or less.
[0092] The ratio S2 / S1 of the mass S2 of the second polyisocyanate to the mass S1 of the polyurethane urea resin is, for example, 0.05 or more and 0.4 or less, preferably 0.05 or more and 0.3 or less.
[0093] (Additives) The adhesive composition may contain at least one additive selected from the group consisting of, for example, a polymerization catalyst, a polymerization initiator, an antistatic agent, an internal mold release agent, an antioxidant, a light stabilizer, a color inhibitor, a fluorescent dye, a dye, a pigment, a fragrance, a solvent, a leveling agent, and a resin modifier. The adhesive composition preferably contains at least one of an antioxidant and a leveling agent.
[0094] Examples of the antioxidant that can be used include 2,6-di-t-butyl-4-methyl-phenol, IRGANOX 245 (ethylene bis(oxyethylene)bis[3,5-tert-butyl-4-hydroxy-m-toluyl]propionate) manufactured by BASF Japan Ltd., IRGANOX 1076 (octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate) manufactured by BASF Japan Ltd., IRGANOX 1010 (pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] manufactured by BASF Japan Ltd., and IRGANOX 1035, 1075, 104, 3790, 5057, and 565 manufactured by BASF Japan Ltd.
[0095] As the leveling agent, a silicone surfactant, a fluorine-containing surfactant, etc. can be used. Specifically, L-7001, L-7002, L-7604, FZ-2123 manufactured by Dow Toray Co., Ltd., Megafac F-470, Megafac F-1405, Megafac F-479 manufactured by DIC Corporation, and FLORAD FC-430 manufactured by 3M Japan Ltd. can be used.
[0096] As the light stabilizer, it is preferable to use a hindered amine compound having a 2,2,6,6-tetramethyl-4-piperidyl skeleton, and commercially available products can be used. For example, bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, bis(1-octyloxy-2,2,6,6-tetramethyl-4-piperidyl)sebacate, 1-{2-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionyloxy]ethyl}-4-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionyloxy]-2,2,6,6-tetramethylpiperidine, 4-benzoyloxy-2,2,6,6-tetramethylpiperidine, methyl(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate ... lysyl) sebacate, 1,2,2,6,6-pentamethyl-4-piperidinyl methacrylate, 2-{[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl}-2-butylpropanedioate (1,2,2,6,6-pentamethyl-4-piperidinyl), poly{[6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperidyl)imino]hexamethylene[(2,2,6,6-tetramethyl-4-piperidyl)imino]}, and 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate. Examples of product names include the ADK STAB (registered trademark) LA series (LA-52, LA-57, LA-63P, LA-68, LA-72, LA-77Y, LA-81, LA-82, etc.) manufactured by ADEKA Corporation, the TINUVIN (registered trademark) series (TINUVIN123, TINUVIN171, TINUVIN249, TINUVIN292, TINUVIN765, TINUVIN622SF, etc.) manufactured by BASF Japan Ltd., and the Chimassorb (registered trademark) series (Chimassorb2020FDL, Chimassorb944FDL).
[0097] (Method for Producing Adhesive Composition) The adhesive composition according to the embodiment is obtained by mixing a polyurethane urea resin with an organic solvent. The polyurethane urea resin may be a third reaction product of a second reaction product having two isocyanate groups and a monoamine. The second reaction product may be a reaction product of a first reaction product having two isocyanate groups and a first diamine. The first reaction product may be a reaction product of a first diol containing a compound represented by the following formula (Ia) and a first polyisocyanate. In other words, the polyurethane urea resin is obtained by reacting a first diol with a first polyisocyanate to obtain a first prepolymer, reacting this first prepolymer with a first diamine to obtain a second prepolymer, and then reacting this second prepolymer with a monoamine. The method for producing the polyurethane urea resin is described in detail below.
[0098] First, a first polyisocyanate is contacted with a first diol to obtain a first reaction product. The first reaction product is a urethane prepolymer having two isocyanate groups, i.e., a first prepolymer. The first diol includes a compound represented by the following formula (Ia):
[0099]
[0100] In formula (Ia), R 1 , R 2 , l, m and n have the same meanings as in formula (I).
[0101] The number average molecular weight of the first diol, determined by the hydroxyl value, is, for example, 500 to 4000. The number average molecular weight is preferably 800 to 3000, and more preferably 1000 to 2000.
[0102] The first diol may be a polyether glycol, a polyether (poly)carbonate diol, or a mixture thereof. The polyether glycol may be, for example, at least one compound selected from the group consisting of polytetramethylene ether glycol (PTMG), polypentamethylene ether glycol, polyhexylene ether glycol, polyheptamethylene ether glycol, polyoctamethylene ether glycol, polynonamethylene ether glycol, and polydecane methylene ether glycol. The polyether (poly)carbonate diol may be a reaction product obtained by polymerizing the above-mentioned polyether glycol with a carbonate compound in the presence of a catalyst.
[0103] The first diol may contain a polyol compound other than the compound represented by formula (Ia). The polyol compound may contain at least one selected from the group consisting of polyether polyol, polyester polyol, polycarbonate polyol, and polycaprolactone polyol.
[0104] Examples of polycarbonate polyols that can be used include the "Duranol (registered trademark)" series manufactured by Asahi Kasei Chemicals Corporation, the "Kuraray Polyol (registered trademark)" series manufactured by Kuraray Co., Ltd., the "Placcel (registered trademark)" series manufactured by Daicel Corporation, the "Nippolan (registered trademark)" series manufactured by Tosoh Corporation, and the "ETERNACOLL (registered trademark)" series manufactured by UBE Inc.
[0105] Polycaprolactone polyol can be obtained, for example, by ring-opening polymerization of ε-caprolactone. Examples of polycaprolactone polyol that can be used include the "Placcel (registered trademark)" series manufactured by Daicel Corporation.
[0106] Examples of polyether polyols include the "EXCENOL (registered trademark)" series and "EMULSTAR (registered trademark)" series manufactured by AGC Inc., and the "ADEKA POLYETHER" series manufactured by ADEKA Corporation.
[0107] Examples of polyester polyols that can be used include the "Polylite (registered trademark)" series manufactured by DIC Corporation, the "Nippolan (registered trademark)" series manufactured by Tosoh Corporation, and the "Maximol (registered trademark)" series manufactured by Kawasaki Chemical Industries, Ltd.
[0108] The first polyisocyanate may be the same compound as the second polyisocyanate described above. The first polyisocyanate is preferably an alicyclic polyisocyanate, and more preferably contains at least one selected from the group consisting of isophorone diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, 1,4-bis(isocyanatomethyl)cyclohexane, dicyclohexylmethane-4,4'-diisocyanate (hydrogenated diphenylmethane diisocyanate), norbornane diisocyanate, 2,5-bis(isocyanatomethyl)-bicyclo[2,2,1]-heptane, and 2,6-bis(isocyanatomethyl)-bicyclo[2,2,1]-heptane.
[0109] The ratio M2 / M1 of the molar amount M2 of the first diol to the molar amount M1 of the first polyisocyanate compound is preferably adjusted to 0.30 or more and 0.90 or less. When the ratio M2 / M2 is within the above range, a sufficient amount of urethane bonds is formed in the first prepolymer. From the viewpoint of improving the functionality of the adhesive layer, the ratio M2 / M1 is preferably 0.40 or more, and more preferably 0.50 or more. From the viewpoint of improving the adhesiveness of the adhesive layer, the ratio M2 / M1 is preferably 0.85 or less, more preferably 0.80 or less, and even more preferably 0.70 or less.
[0110] The ratio S4 / S3 of the mass S4 of the first diol to the mass S3 of the first polyisocyanate is preferably 0.1 or more and 20 or less. When the ratio S4 / S3 is within the above range, a second prepolymer having a sufficient amount of isocyanate groups per unit mass is obtained. The ratio S4 / S3 is preferably 1 or more and 7 or less, and more preferably 2 or more and 5 or less.
[0111] The number average molecular weight of the first prepolymer is preferably 500 or more and 10,000 or less, and more preferably 1,000 or more and 5,000 or less. The number average molecular weight of the first prepolymer can be measured by the same method as that for the second prepolymer. The number average molecular weight of the first prepolymer can be measured, for example, by gel permeation chromatography (GPC).
[0112] The first reaction product is then contacted with a first diamine to obtain a second reaction product, which is a urethane urea prepolymer having two isocyanate groups, i.e., a second prepolymer.
[0113] The contact of the first reaction product with the first diamine may be carried out in two stages. That is, the first reaction product may be contacted with a portion of the first diamine to obtain a second' reaction product, and then the second' reaction product may be contacted with the remainder of the first diamine to obtain a second reaction product. The proportion of the portion of the first diamine relative to the total amount of the first diamine is, for example, 10% by mass or more and 50% by mass or less, and preferably 20% by mass or more and 40% by mass or less.
[0114] The number-average molecular weight of the second prepolymer is preferably 5,000 or more, more preferably 10,000 or more, and even more preferably 13,000 or more. Using a second prepolymer with a high number-average molecular weight tends to increase the adhesiveness of the cured product. That is, second prepolymers with a high number-average molecular weight are more likely to entangle with each other, which is thought to increase cohesive strength and therefore adhesive strength. The number-average molecular weight of the second prepolymer is preferably 50,000 or less, more preferably 40,000 or less, and even more preferably 30,000 or less. A second prepolymer with an excessively high number-average molecular weight contains a small amount of iso(thio)cyanate groups per unit mass, which can reduce adhesive strength. The number-average molecular weight of the second prepolymer can be measured by gel permeation chromatography (GPC).
[0115] The molar mass of the first diamine is preferably 50 to 500. When a diamine having a molar mass within this range is used, a second prepolymer having a desired number average molecular weight tends to be obtained. The molar mass of the diamine is more preferably 50 to 300.
[0116] Examples of primary diamines include isophoronediamine, ethylenediamine, 1,2-diaminopropane, 1,3-diaminopropane, 1,2-diaminobutane, 1,3-diaminobutane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, piperazine, N,N-bis-(2-aminoethyl)piperazine, bis-(4-aminocyclohexyl)methane, bis-(4-amino-3-butylcyclohexyl)methane, 1,2-, 1,3-, and 1,4- Examples of the alkyl esters include diaminocyclohexane, norbornanediamine, hydrazine, dihydrazine adipate, phenylenediamine, 4,4'-diphenylmethanediamine, N,N'-diethylethylenediamine, N,N'-dimethylethylenediamine, N,N'-dipropylethylenediamine, N,N'-dibutylethylenediamine, N-methylethylenediamine, N-ethylethylenediamine, bis(hexamethylene)triamine, and 1,2,5-pentanetriamine.
[0117] The first diamine preferably includes at least one selected from the group consisting of isophoronediamine, ethylenediamine, bis-(4-aminocyclohexyl)methane, and 1,6-diaminohexane.
[0118] The ratio M3 / M1 of the molar amount M3 of the first diamine to the molar amount M1 of the first polyisocyanate is preferably adjusted to 0.1 or more and 0.9 or less. When the ratio M3 / M1 is within the above range, a sufficient amount of the second prepolymer is produced. From the viewpoint of improving the adhesiveness of the adhesive layer, the ratio M3 / M1 is preferably 0.20 or more, and more preferably 0.3 or more. From the viewpoint of improving the functionality of the adhesive layer, the ratio M3 / M1 is preferably 0.50 or less, and more preferably 0.49 or less.
[0119] The ratio M3 / M2 of the molar amount M3 of the primary diamine to the molar amount M2 of the primary diol is preferably adjusted to 0.01 or more and 0.9 or less. From the viewpoint of improving the adhesiveness of the adhesive layer, this ratio M3 / M2 is preferably 0.10 or more, more preferably 0.30 or more, and even more preferably 0.50 or more.
[0120] The ratio S5 / S6 of the mass S5 of the first diamine to the mass S6 of the first prepolymer is preferably 0.01 or more and 0.5 or less. When the ratio S5 / S6 is within the above range, a second prepolymer having a sufficient amount of isocyanate groups per unit mass is obtained. The ratio S5 / S6 is more preferably 0.04 or more and 0.3 or less.
[0121] The second reaction product is then contacted with a monoamine to obtain a third reaction product, which is a non-reactive urethane urea polymer that does not have an active group such as an isocyanate group, i.e., the first polymer.
[0122] The monoamine is preferably a primary amine. The monoamine preferably includes an alkylamine or an amine having a 2,2,6,6-pentamethyl-4-piperidyl moiety represented by the following formula (3). The number of carbon atoms in the alkylamine is, for example, 1 or more and 10 or less, preferably 2 or more and 7 or less. As the alkylamine, it is preferable to use normal butylamine. From the viewpoint of improving adhesion, it is preferable to use an alkylamine.
[0123] Amines having a 2,2,6,6-pentamethyl-4-piperidyl moiety can function as hindered amines, thereby increasing light stability.
[0124]
[0125] In formula (3), R 21 is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. 22 is an alkylene group having 1 to 3 carbon atoms; a is 0 or 1.
[0126] Monoamines are R 21is a methyl group and a is 0, ie, 1,2,2,6,6-pentamethyl-4-aminopiperidine.
[0127] The ratio M4 / M1 of the molar amount M4 of the monoamine to the molar amount M1 of the first polyisocyanate is, for example, 0.01 or more and 0.5 or less, preferably 0.02 or more and 0.2 or less.
[0128] The ratio S7 / S8 of the mass S7 of the monoamine to the mass S8 of the second prepolymer is preferably 0.001 or more and 0.100 or less. When the ratio S7 / S8 is within the above range, a first prepolymer having a sufficient amount of isocyanate groups per unit mass is obtained. The ratio S7 / S8 is more preferably 0.002 or more and 0.030 or less.
[0129] The first to third reaction products described above are preferably produced under an inert gas atmosphere such as nitrogen. These productions may also be carried out in the presence of a reaction solvent. The first reaction product may be produced without a solvent, and the resulting first reaction product may be dissolved in a reaction solvent. A first diamine may then be added to this solution to obtain a solution containing the second reaction product. A monoamine may then be added to this solution to obtain a solution containing the third reaction product, i.e., an adhesive composition. The reaction solvent may be the same as the organic solvent described above. The reaction solvent may also serve as the organic solvent for the adhesive composition. The adhesive composition may also be obtained by removing the reaction solvent by drying the solution containing the third reaction product, and then dissolving or dispersing the third reaction product in an organic solvent. An optional component such as a functional dye may further be added to the adhesive composition obtained by the above method.
[0130] [Laminate] As described above, the laminate according to the embodiment can be used as a binder sheet. In particular, the laminate according to the embodiment can be used as a functional sheet in which a functional dye such as a photochromic compound is blended in the resin layer.
[0131] The laminate includes an optical substrate and a resin layer containing a cured product of the adhesive composition according to the embodiment. The resin layer is laminated on at least one main surface of the optical substrate. The laminate may also include first and second optical substrates and a resin layer positioned between them to bond them together.
[0132] The thickness of the laminate according to the embodiment is preferably 100 μm or more, more preferably 120 μm or more, and even more preferably 150 μm or more. A thicker laminate tends to have higher shape stability. There is no particular upper limit to the thickness of the laminate, but in one example, it is 1000 μm or less, and in another example, it is 500 μm or less, and more preferably 400 μm or less. This makes it possible to improve the handleability even when manufacturing eyeglass lenses with a thin center thickness.
[0133] Fig. 1 is a cross-sectional view schematically showing an example of a laminate according to an embodiment. The laminate 1 shown in Fig. 1 comprises a first optical substrate 2, a second optical substrate 3, and a resin layer 4 interposed therebetween. The first optical substrate 2 comprises a first main surface 2a and a second main surface 2b. The first main surface 2a constitutes one of the outermost surfaces of the laminate 1. The second main surface 2b is in contact with the resin layer 4. The second optical substrate 3 comprises a first main surface 3a and a second main surface 3b. The first main surface 3a constitutes the other outermost surface of the laminate 1. The second main surface 3b is in contact with the resin layer 4.
[0134] (First and second optical substrates) The first and second optical substrates may be optical films or sheets having visible light transmittance. The first and second optical substrates may be colorless transparent films, semi-transparent films, or colored transparent films.
[0135] The thickness of the first and second optical substrates is, for example, 10 μm to 100 μm, preferably 20 μm to 80 μm. The thickness of the second optical substrate may be the same as or different from the thickness of the first optical substrate. The thickness of the first and second optical substrates may be, for example, 50 μm to 1000 μm, or 200 μm to 500 μm.
[0136] The first and second optical substrates may contain at least one resin selected from the group consisting of polycarbonate resin, cellulose resin, acrylic resin, methacrylic resin, polyurethane resin, polyurethane urea resin, polyamide resin, polyester resin, polyimide resin, epoxy resin, polyolefin resin, and polyvinyl alcohol resin.
[0137] Examples of polycarbonate resins that can be used include aromatic polycarbonate resins primarily composed of aromatic phenols having a typical bisphenol A skeleton, and polymer alloys of aromatic polycarbonate resins with other resins. Examples of such other resins include synthetic resins such as polyester resins, polysiloxanes, polyamides, polystyrenes, polyolefins, acrylics, amorphous polyolefins, ABS, and AS. The weight-average molecular weight of the polycarbonate resin used in the optical sheet or optical film is preferably 10,000 to 200,000, and more preferably 15,000 to 80,000.
[0138] Examples of cellulose resins include diacetyl cellulose, tripropyl cellulose, and dipropyl cellulose.
[0139] Examples of polyamide resins that can be used include polyamide resins obtained by polycondensation of ω-aminocarboxylic acids such as ε-caprolactam, 10-aminodecanoic acid lactam, and ω-laurin lactam, polyamide resins obtained by co-condensation of diamines and dicarboxylic acids, and copolymers thereof. Among polyamides obtained by co-condensation, alicyclic polyamide resins or semi-aromatic polyamide resins are preferred.
[0140] Examples of polyester resins include polycondensates of dicarboxylic acids such as terephthalic acid and isophthalic acid with diols such as ethylene glycol, butylene glycol and 1,4-cyclohexanedimethanol.
[0141] As the (meth)acrylic resin, for example, a homopolymer such as methyl methacrylate or a resin made of a copolymer of a plurality of (meth)acrylic monomers can be used.
[0142] As the polyurethane resin and polyurethane urea resin, known resins obtained by reacting a diisocyanate compound such as isophorone diisocyanate with a polyol compound such as polycarbonate polyol, polyester polyol, etc. can be used. Furthermore, polyurethane resins or polyurethane urea resins obtained by reacting a chain extender such as a low molecular weight diol, triol, diamine, or triamine can be preferably used.
[0143] The polyimide resin may be a polymer of an aromatic tetracarboxylic acid and an aromatic diamine. Examples of the aromatic tetracarboxylic acid include pyromellitic acid, 3,3',4,4'-biphenyltetracarboxylic acid, 2,3',3,4'-biphenyltetracarboxylic acid, 3,3',4,4'-benzophenonetetracarboxylic acid, 2,3,6,7-naphthalenetetracarboxylic acid, 2,2-bis(3,4-dicarboxyphenyl)propane, pyridine-2,3,5,6-tetracarboxylic acid, or an aromatic tetracarboxylic acid derived from an acid anhydride or acid dianhydride thereof, or an ester compound or halide of the acid.
[0144] As the epoxy resin, for example, resins obtained by condensation reaction of bisphenol A, bisphenol F, etc. with epichlorohydrin, other polyfunctional epoxy resins, biphenyl type epoxy resins, etc. can be suitably used.
[0145] Suitable polyolefin resins include, for example, polypropylene, polyethylene, ethylene-propylene copolymer, ethylene-α-olefin copolymer, and propylene-α-olefin copolymer.
[0146] The first and second optical substrates are preferably made of polycarbonate resin. The use of polycarbonate resin allows for the production of a laminate with excellent adhesion and appearance. Furthermore, when an adhesive composition containing a urethane urea resin having a polyether polycarbonate structure is used, adhesion to an adhesive layer containing a cured product of the urethane urea resin tends to be enhanced.
[0147] (Resin Layer) The resin layer is located between the first optical substrate and the second optical substrate. The resin layer may be in contact with the second main surface of the first optical substrate and the second main surface of the second optical substrate. That is, the resin layer can function as an adhesive layer for bonding the first optical substrate and the second optical substrate.
[0148] The resin layer includes a cured product of the adhesive composition according to the embodiment. This cured product is considered to include a structure represented by formula (I). The resin layer may include a functional dye such as a photochromic compound.
[0149] The thickness of the resin layer is, for example, 0.1 μm or more and 100 μm or less. The thickness of the resin layer may be thinner or thicker than the thickness of the first and second base materials.
[0150] (Manufacturing Method) A manufacturing method of a laminate according to an embodiment includes, for example, applying the adhesive composition described above onto a support to obtain a coating film, peeling the coating film from the support and laminating it on the second main surface of a first optical substrate, laminating a second optical substrate on the coating film so that the second main surface is in contact with the coating film to obtain a first structure, and heating the first structure to cure the coating film. Note that the coating film may also be provided directly by applying the adhesive composition onto the first optical substrate and drying it.
[0151] The method for manufacturing the laminate will be described in detail below. First, first and second optical substrates are prepared. Commercially available resin films or sheets can be used as the first and second optical substrates. An unstretched sheet may be used, or a sheet that has been subjected to a stretching treatment and a dyeing treatment may be used. A commercially available resin film or sheet that has been saponified may be used, or the resin film or sheet may be subjected to a saponification treatment. Furthermore, the first and second optical substrates may be subjected to a surface treatment such as an etching treatment or a corona treatment.
[0152] Next, the adhesive composition is applied to a support to form a coating film. This coating film is dried, for example, at a temperature of 70°C or higher and 150°C or lower for 1 minute to 1 hour to obtain a coating film. The coating film peeled from the support is laminated on the second main surface of the first optical substrate. The second main surface of the second optical substrate is laminated so as to contact the coating film. This results in a first structure in which the first optical substrate, coating film, and second optical substrate are laminated in this order.
[0153] Next, the first structure is heated to cure the coating film. This results in a laminate in which the first optical substrate and the second optical substrate are bonded together by the resin layer. The heat treatment of the first structure is performed, for example, at a temperature of 40°C to 160°C for 1 minute to 10 hours.
[0154] The obtained laminate may be subjected to a degassing treatment. During the degassing treatment, the laminate is left to stand, for example, under a vacuum of 500 Pa at a temperature of 40° C. to 80° C. for 5 hours to 20 hours. The structure after the degassing treatment may further be subjected to a heat treatment.
[0155] <Laminate Variation 1> The laminate may further include first and second adhesive layers. The first adhesive layer is located between the resin layer and the first optical substrate to bond them together. The second adhesive layer is located between the resin layer and the second optical substrate to bond them together.
[0156] Fig. 2 is a cross-sectional view schematically showing another example of a laminate. The laminate 1a shown in Fig. 2 has the same structure as the laminate 1 shown in Fig. 1, except that it includes a first adhesive layer FA between the resin layer 4 and the first optical substrate 2, and a second adhesive layer SA between the resin layer 4 and the second optical substrate 3.
[0157] The thickness of the first and second adhesive layers is, for example, 1 μm or more. When the thickness of the first and second adhesive layers is large, the adhesion between the first and second optical substrates and the resin layer tends to be improved. The thickness of the first and second adhesive layers is preferably 3 μm or more, and more preferably 5 μm or more. On the other hand, when the thickness of the first and second adhesive layers is excessively large, the appearance of the laminate tends to be deteriorated. The thickness of the first and second adhesive layers is preferably 50 μm or less, more preferably 30 μm or less, and even more preferably 20 μm or less.
[0158] At least one of the first and second adhesive layers preferably contains a cured product of the adhesive composition according to the embodiment. The components and their contents of this adhesive composition are preferably different from those of the adhesive composition used to form the resin layer. The first and second adhesive layers may contain a cured product of an adhesive composition containing a urethane urea resin that does not contain the structure represented by formula (I). However, from the viewpoint of photochromic properties, it is preferable that the adhesive composition at least partially contains the structure represented by formula (1). Furthermore, the urethane urea resin that does not contain the structure represented by formula (1) can be obtained by a manufacturing method similar to that of the adhesive composition according to the embodiment described above, except that, for example, a polycarbonate diol is used as the first diol. The first and second adhesive layers may contain at least one resin selected from the group consisting of an epoxy resin, an oxetane resin, an acrylic resin, and a methacrylic resin.
[0159] The first and second adhesive layers can be formed, for example, by applying an adhesive composition onto the surface of at least one of the first and second optical substrates and curing it.
[0160] <Laminate Variation 2> The laminate according to the embodiment may include a release substrate instead of the optical substrate. The laminate according to the embodiment may be a laminate of a first optical substrate, a resin layer, and a release substrate. This laminate can be used as a seal or sticker, and the adhesive composition according to the embodiment can be used as a seal glue.
[0161] The release substrate is not particularly limited as long as it has releasability. Paper or plastic may be used as the release substrate. The release substrate may have a surface coated with a release agent.
[0162] When used as a seal, it is preferable to peel off the release substrate from the laminate, attach the resin layer, which is the adhesive, to an object to be adhered, and then heat the laminate. Heating can make the adhesion stronger. The heating temperature is, for example, 50°C or higher and 150°C or lower. The object to be adhered can be plastic, metal, stone, wood, etc., but is not particularly limited. The object to be adhered is preferably plastic.
[0163] <Support> The laminate according to the embodiment may further include a support. The support may be located between the resin layer and the first or second adhesive layer, or between the first or second adhesive layer and the first or second optical substrate. The support can further enhance the shape stability of the laminate. The support may be colorless and transparent, white and transparent, or colored and transparent.
[0164] The support preferably contains at least one resin selected from the group consisting of polyethylene terephthalate, triacetyl cellulose, polyamide, polycarbonate sheet, cellulose acetate butyrate, and (meth)acrylic.
[0165] The thickness of the support is preferably 50 μm or more. A thicker support tends to increase the strength of the laminate. There is no particular upper limit to the thickness of the support, but in one example, it is 1000 μm or less, and in another example, it is 500 μm or less.
[0166] (Manufacturing method) A manufacturing method of a modified example of the laminate according to the embodiment includes, for example, applying a second adhesive composition to at least one main surface of a first optical substrate and a second optical substrate and drying the composition to form a first coating film and a second coating film, applying the first adhesive composition described above to a support to form a third coating film, peeling the third coating film from the support and laminating it on the first coating film of the first optical substrate, laminating the second optical substrate so that the second coating film is laminated on the third coating film on the first coating film to form a first structure, and heating the first structure to cure the first coating film, the second coating film, and the third coating film. Note that an adhesive composition may be applied to the first coating film and dried to directly form a third coating film.
[0167] A method for producing a modified laminate is described in detail below. First, the second adhesive composition is applied to the second main surfaces of the first optical substrate and the second optical substrate using, for example, a bar coater to form a coating film. This coating film is dried, for example, at a temperature of 70°C or higher and 150°C or lower for 1 minute to 1 hour. This results in a first optical substrate having a first coating film formed on one main surface and a second optical substrate having a second coating film formed on one main surface.
[0168] Next, the first adhesive composition is applied to a support to form a coating film. This coating film is dried, for example, at a temperature of 70°C or higher and 150°C or lower for 1 minute to 1 hour. This results in a third coating film. The third coating film peeled from the support is laminated on the first coating film on the first optical substrate. This results in a structure in which the first optical substrate, the first coating film, and the third coating film are laminated in this order.
[0169] Next, the second coating film on the second optical substrate is laminated so as to be in contact with the third coating film, thereby obtaining a first structure in which the first optical substrate, the first coating film, the third coating film, the second coating film, and the second optical substrate are laminated in this order.
[0170] Next, the first structure is heated to cure the first to third coating films. This results in a laminate in which the first optical substrate and the second optical substrate are bonded via the first adhesive layer, the resin layer, and the second adhesive layer. The heat treatment of the first structure is performed, for example, at a temperature of 40°C to 160°C for 1 minute to 240 hours.
[0171] The obtained laminate may be subjected to a degassing treatment. During the degassing treatment, the laminate is left to stand, for example, under a vacuum of 500 Pa at a temperature of 40° C. to 80° C. for 5 hours to 20 hours. The structure after the degassing treatment may further be subjected to a heat treatment.
[0172] At least one of the first adhesive composition and the second adhesive composition is the adhesive composition according to the embodiment. It is preferable to use the adhesive composition according to the embodiment as the first adhesive composition, and it is more preferable that both the first and second adhesive compositions are the adhesive composition according to the embodiment.
[0173] When adhesive compositions according to the embodiment are used as the first and second adhesive compositions, their compositions preferably differ from each other. Specifically, the first adhesive composition preferably contains a functional dye and a second polyisocyanate, and the second adhesive composition preferably does not contain a functional dye and a second polyisocyanate. Furthermore, the polyurethane urea resin of the first adhesive composition and the polyurethane urea resin of the second adhesive composition preferably have different compositions. That is, the ratio M2 / M1 of the molar amount M2 of the first diol to the molar amount M1 of the first polyisocyanate compound in the production of the polyurethane urea resin contained in the first adhesive composition is preferably higher than the ratio M2 / M1 in the production of the polyurethane urea resin contained in the second adhesive composition. Furthermore, the ratio M3 / M1 of the molar amount M3 of the first diamine to the molar amount M1 of the first polyisocyanate compound in the production of the polyurethane urea resin contained in the first adhesive composition is preferably lower than the ratio M3 / M1 in the production of the polyurethane urea resin contained in the second adhesive composition. By using polyurethane urea resins having different ratios M2 / M1 and M3 / M1 in this way, a laminate having excellent adhesiveness and functionality can be realized.
[0174] [Coating layer-containing laminate] The laminate according to the embodiment may include a coating layer. The coating layer covers at least a portion of the first optical substrate and the second optical substrate. The coating layer includes at least one resin selected from the group consisting of epoxy resin, oxetane resin, acrylic resin, methacrylic resin, and urethane resin. The coating layer-containing laminate has excellent processing stability due to the inclusion of the coating layer. In addition, it has excellent adhesion to the optical element substrate described below.
[0175] 3 is a cross-sectional view schematically showing an example of a coating layer-containing laminate according to an embodiment. The coating layer-containing laminate 7 shown in FIG. 3 includes the laminate 1 shown in FIG. 1, a first coating layer 5 that entirely covers the first main surface 2a of the first optical substrate 2, and a second coating layer 6 that entirely covers the first main surface 3a of the second optical substrate 3. The first coating layer 5 may cover a portion of the first main surface 2a, and the second coating layer 6 may cover a portion of the first main surface 3a. One of the first coating layer 5 and the second coating layer 6 may be omitted. Note that the laminate 1 may be replaced with the laminate 1a shown in FIG. 2.
[0176] <Coating layer> The coating layer covers at least a portion of the surface of at least one of the first and second optical substrates. The coating layer preferably covers the surfaces of both the first and second optical substrates. The coating layer preferably covers the entire surfaces of the first and second optical substrates. When the area covered by the coating layer on the surfaces of the first and second optical substrates is large, adhesion to the optical element substrate and shape stability of the laminate tend to be improved.
[0177] The thickness of the coating layer is, for example, 5 μm or more. When the coating layer is thick, the adhesion to the optical element substrate and the shape stability of the laminate tend to be improved. The thickness of the coating layer is preferably 10 μm or more, more preferably 20 μm or more, and even more preferably 25 μm or more. On the other hand, when the coating layer is excessively thick, the appearance of the laminate tends to be deteriorated. The thickness of the coating layer is preferably 100 μm or less, more preferably 75 μm or less, and even more preferably 50 μm or less.
[0178] The coating layer contains at least one resin selected from the group consisting of epoxy resin, oxetane resin, acrylic resin, methacrylic resin, and urethane resin. The coating layer preferably contains an epoxy resin. Coating layers containing epoxy resin tend to have excellent appearance and higher adhesion to the optical element substrate. The type of resin contained in the coating layer can be confirmed by gas chromatography or Fourier transform infrared spectroscopy (FT-IR) analysis.
[0179] The surface of the coating layer preferably has at least one functional group selected from the group consisting of an epoxy group, an acryloyl group, a methacryloyl group, and a vinyl group. Having a coating layer with these functional groups on its surface tends to improve adhesion to the optical element substrate. More preferably, the coating layer contains at least one functional group selected from the group consisting of an acryloyl group, a methacryloyl group, and a vinyl group, and an epoxy group. Such a coating layer can further enhance adhesion.
[0180] The presence of functional groups on the surface of the coating layer can be confirmed, for example, by Fourier transform infrared spectroscopy (FT-IR) analysis. That is, when an acryloyl group, a methacryloyl group, or a vinyl group is present on the surface, the functional groups are detected at 1600 cm in the IR spectrum. -1 1680cm or more -1 Below, and 790 cm -1 More than 1000cm -1 Peaks can be detected within the following ranges:
[0181] The coating layer can be formed, for example, by applying a coating layer-forming composition to the surface of at least one of the first and second optical substrates and curing the composition. The coating layer-forming composition contains, for example, at least one resin selected from the group consisting of epoxy resins, oxetane resins, acrylic resins, methacrylic resins, and urethane resins, and an organic solvent.
[0182] [Optical Article] The optical article according to the embodiment includes the laminate according to the embodiment. The optical article may include the laminate according to the embodiment and an optical element substrate that covers at least a portion of the first optical substrate and the second optical substrate.
[0183] Examples of optical articles include binder sheets, lenses, eyeglasses, window materials for houses and automobiles, liquid crystal displays, sun visors, watches, etc. Lenses include semi-finished lenses and finished lenses.
[0184] FIG. 4 is a cross-sectional view schematically illustrating an example of an optical article according to an embodiment. The optical article 10 illustrated in FIG. 4 includes a first optical element substrate 11 and the laminate 1 illustrated in FIG. 1. The optical article 10 has a concave-convex lens shape. The laminate 1 has a curved surface that conforms to the shape of the lens. The first optical element substrate 11 is located on the concave side. The first optical element substrate 11 covers the entire surface of a second optical substrate (not shown) of the laminate 1. The side surfaces of the laminate 1 are not covered by the first optical element substrate 11. The side surfaces of the laminate 1 may be covered by the first optical element substrate 11. The laminate 1 and the first optical element substrate 11 may be integrated by, for example, thermal welding.
[0185] In the optical article according to the embodiment, the laminate 1 shown in Fig. 1 may be replaced by a laminate 1a shown in Fig. 2 or a coated layer-containing laminate 7 shown in Fig. 3. The first optical element substrate 11 may cover the entire surface of the first coating layer 5 of the coated layer-containing laminate 7.
[0186] Fig. 5 is a perspective view schematically illustrating an example of eyeglasses according to an embodiment. The eyeglasses 100 shown in Fig. 5 include a lens 101 and a frame 102 that supports the lens 101. The lens 101 includes an optical article 10 according to an embodiment.
[0187] (Optical element substrate) The optical element substrate may contain a resin. The resin may contain at least one selected from the group consisting of polyester resin, polyamide resin, allyl resin, (meth)acrylic resin, polyurethane resin, polyurethane urea resin, polythiourethane resin, polythiourethane urea resin, polythioepoxy resin, and polycarbonate resin. The optical element substrate preferably contains a polycarbonate resin.
[0188] (Method for manufacturing optical article) An optical article according to an embodiment is manufactured, for example, by the following method. First, a laminate is shaped. Specifically, the laminate is placed in a mold of a curved surface processing device. The mold has, for example, a lens shape such as a hemisphere. A hole is provided in the bottom surface of the mold. A pressure adjusting device such as a vacuum pump is connected to the hole via a pipe. The pressure adjusting device is activated to reduce the pressure in the space between the mold and the laminate. At this time, the ambient temperature may be set to 70°C or higher and 160°C or lower to facilitate deformation of the laminate. After a certain period of time has elapsed, the operation of the pressure adjusting device is stopped, and the deformed laminate is removed from the mold. The removed laminate is cooled, for example, at a temperature of 0°C or higher and 40°C or lower. In this way, a curved surface processed laminate is obtained.
[0189] Next, the deformed laminate is placed inside an injection molding mold. Liquid thermoplastic resin is poured onto the rear surface (concave surface) of the placed laminate. The interior of the mold is cooled to solidify the thermoplastic resin. In this way, an optical article is obtained in which the laminate and the thermoplastic resin that will become the optical element substrate are integrated.
[0190] Alternatively, a curable composition of a thermosetting resin is poured into a mold in which the laminate is placed, and the mold is filled with the curable composition. The mold after filling with the curable composition is heat-treated to cure the curable composition. During the heat treatment, for example, the temperature is gradually increased from room temperature to the curing temperature, and after reaching the curing temperature, it is maintained for a certain period of time. The curing temperature is, for example, 60°C or higher and 100°C or lower. The temperature increase rate is, for example, 1°C / hour or higher and 10°C / hour or lower. The maintenance time at the curing temperature is, for example, 1 hour or higher and 30 hours or lower. After completion of the heat treatment, the cured body is removed from the mold. The removed cured body is further heated within a range of 60°C or higher and 150°C or lower for 1 hour or higher and 10 hours or lower. In this way, an optical article in which the surface of the second optical substrate of the laminate is coated with the optical element substrate is obtained.
[0191] The present invention will be described in more detail by the following examples, which are merely illustrative of the present invention and are not intended to limit the scope and spirit of the present invention.
[0192] The abbreviations of the compounds used as the components in the examples and comparative examples are summarized below. Photochromic compound PC1: a compound represented by the following formula
[0193]
[0194] Primary diols PL1: PEPCD NT2006 manufactured by Mitsubishi Chemical Corporation (a polyether polycarbonate diol made of polytetramethylene oxide having a number average molecular weight of 650, a number average molecular weight of 2000) PL2: PEPCD NT1002 manufactured by Mitsubishi Chemical Corporation (a polyether polycarbonate diol made of polytetramethylene oxide having a number average molecular weight of 250, a number average molecular weight of 1000) PL3: PEPCD NT2002 manufactured by Mitsubishi Chemical Corporation (a polyether polycarbonate diol made of polytetramethylene oxide having a number average molecular weight of 250, a number average molecular weight of 2000) PL4: Polytetramethylene Oxide 1000 manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. (a polyether polyol, a number average molecular weight of 1000) PL5: Polytetramethylene oxide 2000 (polyether polyol, number average molecular weight 2000) manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. PL6: PTMG4000 (polytetramethylene ether glycol, number average molecular weight 4000) manufactured by Mitsubishi Chemical Corporation PL7: Duranol (polycarbonate diol made from 1,5-pentanediol and hexanediol, number average molecular weight 1000) manufactured by Asahi Kasei Chemicals Corporation PL8: Duranol (polycarbonate diol made from 1,5-pentanediol and hexanediol, number average molecular weight 2000) manufactured by Asahi Kasei Chemicals Corporation The properties of the first diol are summarized in Table 1 below.
[0195]
[0196] First and second polyisocyanates NCO1: isophorone diisocyanate NCO2: dicyclohexylmethane-4,4-diisocyanate NCO3: Duranate TPA-100 (polyisocyanate having an isocyanurate structure) manufactured by Asahi Kasei Chemicals Corporation NCO4: Duranate 24A-100 (polyisocyanate having a biuret structure) manufactured by Asahi Kasei Chemicals Corporation NCO5: Duranate AE700-100 (polyisocyanate having an adduct structure) manufactured by Asahi Kasei Chemicals Corporation NCO6: Duranate E402-100 (polyisocyanate having an adduct structure) manufactured by Asahi Kasei Chemicals Corporation NCO7: Duranate SBB-70P (polyblock isocyanate having a biuret structure) manufactured by Asahi Kasei Chemicals Corporation NCO8: TRIXENE BI7992 (polyblock isocyanate having a biuret structure) manufactured by GSI Creos Co., Ltd.
[0197] Primary diamine H1: bis-(4-aminocyclohexyl)methane H2: isophoronediamine
[0198] Monoamine HA1: 1,2,2,6,6-pentamethyl-4-aminopiperidine HA2: n-butylamine
[0199] Organic solvent D1: Diethyl ketone / tertiary butanol mixed solvent (volume ratio 8 / 2) D2: Propylene glycol monomethyl ether D3: Diethyl ketone
[0200] Other components L1: Ethylene bis(oxyethylene) bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate] L2: FZ2162 manufactured by Dow Chemical Company
[0201] (Synthesis of Polyurethane Urea Resin Solutions US1 to US16) 269.9 g of polyether polycarbonate diol (PL1) having a number average molecular weight of 2000 and 50 g of isophorone diisocyanate (NCO1) were charged into a three-neck flask equipped with a stirring blade, a condenser, a thermometer, and a nitrogen gas inlet tube, and the mixture was reacted at 130°C for 8 hours under a nitrogen atmosphere to synthesize a urethane prepolymer. The end point of the reaction was confirmed by back titration of the isocyanate group. After completion of the reaction, the reaction solution was cooled to approximately 30°C and dissolved in 630 g of a diethyl ketone / tertiary butanol = 8 / 2 mixed solvent ((organic solvent) component: D1). After cooling the reaction solution to 0°C, 4.97 g of bis-(4-aminocyclohexyl)methane (H1), a chain extender, was added dropwise. After stirring for 1 hour, the reaction solution was heated to 25°C. Thereafter, an additional 10.43 g of H1 was added dropwise, and the mixture was stirred for 1 hour. Subsequently, 4.1 g of 1,2,2,6,6-pentamethyl-4-aminopiperidine (HA1) was added dropwise, and the mixture was allowed to react for 1 hour, yielding a diethyl ketone / tertiary butanol solution of urethane urea resin US1. When the infrared absorption spectrum of the resulting polyurethane urea resin was measured, no absorption due to isocyanate groups at the molecular terminals was observed, confirming that no isocyanate groups remained at the molecular terminals. Furthermore, the softening point measured by TMA was 95°C.
[0202] As shown in Table 2, polyurethane urea resin solutions US2 to US16 were obtained in the same manner as polyurethane urea resin solution US1, except that the blending components were changed.
[0203]
[0204] In Table 2, the "molar ratio" indicates the molar ratio of first diol / first isocyanate / first diamine / monoamine.
[0205] Example 1 Preparation of Photochromic Adhesive Composition AC1 50 g of the urethane urea resin solution US1, 1.27 g of the photochromic compound (PC1), 2.8 g of dicyclohexylmethane-4,4-diisocyanate as a crosslinking agent, 0.2 g of ethylene bis(oxyethylene) bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate] as an antioxidant, and 0.016 g of FZ2162 as a surfactant were added, and the mixture was stirred and mixed at room temperature to obtain a mixture for constituting a photochromic adhesive composition.
[0206] Examples 2 to 13, 27 to 35, Comparative Examples 1 to 3 As shown in Table 3, adhesive compositions AC2 to AC16 were obtained in the same manner as in Example 1, except that the formulation was changed.
[0207]
[0208] Example 14 (Preparation of Photochromic Laminate) Polyurethane urea resin solution US14 was used as adhesive composition AC16 to form an adhesive layer. Adhesive composition AC16 was applied to one main surface of a 300 μm-thick polycarbonate sheet, and the coating was dried at 110° C. for 10 minutes to obtain a polycarbonate sheet having an adhesive layer with a thickness of 10 μm. Two such polycarbonate sheets were obtained.
[0209] The adhesive composition AC1 was applied to a PET (polyethylene terephthalate) film (Teijin DuPont Films Co., Ltd. Purex film with a silicone coating), and the coating was dried at 80 ° C. for 5 minutes to obtain a dry film with a thickness of about 30 μm. This dry film was peeled off from the PET film, and the dry film was placed between polycarbonate sheets having adhesive layers so as to contact each adhesive layer. This laminate was left standing at 40 ° C. under vacuum for 20 hours, then heat-treated at 100 ° C. for 1 hour, then humidified at 60 ° C. and 80% RH for 22 hours, and finally left standing at 80 ° C. under vacuum for 6 hours to obtain a photochromic laminate LB1 in which the first optical substrate, the first adhesive layer, the resin layer, the second adhesive layer, and the second optical substrate were laminated in this order.
[0210] <Examples 15 to 26, 36 to 44, Comparative Examples 4 and 5> As shown in Tables 4 and 5, laminates LB2 to LB15 were obtained in the same manner as in Example 14, except that the type of adhesive composition was changed.
[0211] Example 45 A laminate LB25 was obtained in the same manner as in Example 14, except that a polycarbonate sheet having a thickness of 100 μm was used and that the type of adhesive composition was changed as shown in Table 5.
[0212] Example 46 A laminate LB25 was obtained in the same manner as in Example 14, except that a polycarbonate sheet having a thickness of 200 μm was used and that the type of adhesive composition was changed as shown in Table 5.
[0213] Example 47 Preparation of Photochromic Adhesive Composition AC25 50 g of the urethane urea resin solution US4, 1.27 g of the photochromic compound (PC1), 0.2 g of ethylene bis(oxyethylene) bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate] as an antioxidant, and 0.016 g of FZ2162 as a surfactant were added, and the mixture was stirred and mixed at room temperature to obtain Photochromic Adhesive Composition AC25.
[0214] Comparative Example 6 As shown in Table 6, an adhesive composition AC26 was obtained in the same manner as in Example 47, except that US9 was used in the urethane urea resin solution.
[0215] Example 48: A 60 μm thick saponified TAC (triacetyl cellulose) film was prepared as the first optical substrate. The adhesive composition AC25 was applied to this TAC film, and the coating was dried at 80 ° C for 5 minutes to obtain a dry film with a thickness of approximately 30 μm. This dry film was placed in contact with a diethylene glycol bis-allyl carbonate resin coating substrate with a thickness of approximately 2 mm. This laminate was heat-treated at 90 ° C for 1 hour to obtain a photochromic laminate LB28 in which the first optical substrate, the resin layer, and the coating substrate were laminated in this order.
[0216] Comparative Example 7 As shown in Table 7, a photochromic laminate LB29 was obtained in the same manner as in Example 48, except that the type of adhesive composition was changed.
[0217] <Evaluation> The photochromic properties and peel strength of the laminates obtained in the examples and comparative examples were measured. The results are shown in Tables 4 to 7.
[0218] Photochromic Properties The obtained laminate was used as a sample, and was irradiated with a xenon lamp L-2480 (300 W) SHL-100 manufactured by Hamamatsu Photonics K.K. at 23°C through an Aeromass filter (manufactured by Corning Inc.) at a beam intensity of 365 nm = 2.4 mW / cm on the surface of the laminate. 2 , 245nm=24μW / cm 2 The laminate was then irradiated with light at 1000 kJ / cm 3 for 300 seconds to develop color, and the photochromic properties of the laminate were measured.
[0219] 1) Maximum absorption wavelength (λmax): The maximum absorption wavelength after color development measured using a spectrophotometer (Instant Multichannel PhotoDirector MCPD1000) manufactured by Otsuka Electronics Co., Ltd. The maximum absorption wavelength is related to the color tone during color development. 2) Color density [ε(120) - ε(0)]: The difference between the absorbance ε(120) at the maximum absorption wavelength after 300 seconds of irradiation and the absorbance ε(0) at the maximum absorption wavelength before irradiation. The higher this value, the better the photochromic properties. 3) Fading rate [t1 / 2 (sec)]: The time required for the absorbance of the sample at the maximum wavelength to decrease to half of [ε(120) - ε(0)] after 300 seconds of irradiation and then the light irradiation is stopped. The shorter this time, the better the photochromic properties.
[0220] Peel Strength The obtained photochromic laminate was cut into a test piece having an adhesive portion of 25 × 100 mm, which was attached to a testing machine (Autograph AGS-500NX, manufactured by Shimadzu Corporation) equipped with a thermostatic bath, and left to stand for 10 minutes under conditions of 70°C, after which a tensile test was carried out at a crosshead speed of 100 mm / min to measure the peel strength.
[0221]
[0222]
[0223]
[0224]
[0225] As is clear from the above examples, laminates using photochromic compositions containing polyurethane urea resins having a structure represented by formula (I), such as polytetramethylene groups, have excellent photochromic properties. The use of polyurethanes with high softening points derived from polyether polycarbonate diols increases peel strength. Furthermore, the use of polyurethane urea resins having a structure represented by formula (I) in the adhesive layer also exhibits even better photochromic properties. Furthermore, the incorporation of triisocyanate into the adhesive composition improves peel strength without reducing the fading rate.
[0226] On the other hand, when polycarbonate diol is used as in Comparative Example 1, sufficient photochromic properties are not obtained. Also, by increasing the molecular weight of the polyol as in Comparative Example 2, the photochromic properties are improved, but the photochromic properties are not sufficient compared to the polyurethane urea resin having the structure represented by formula (I). As shown in Table 7, the seal-like laminate of Example 48 exhibited excellent photochromic properties. Furthermore, in the laminate of Example 48, the adhesion between the resin layer and the substrate was high and it was not easily peeled off by hand. On the other hand, the seal-like laminate of Comparative Example 7 did not obtain high adhesion.
[0227] Preferred aspects of the present invention are described below: [1] An adhesive composition comprising a polyurethane urea resin having a urea bond, a urethane bond, and a structure represented by the following formula (I), and an organic solvent.
[0228]
[0229] In the formula (I), R 1 and R 2 are each independently a linear alkylene group having 3 to 10 carbon atoms; l is 0 or 1 to 25; and n and m are each independently 2 to 70.
[0230] [2] The adhesive composition according to [1], wherein in formula (I), l is 1 or more and 25 or less.
[0231] [3] The adhesive composition according to [1] or [2], further comprising a functional dye.
[0232] [4] The adhesive composition according to any one of [1] to [3], further comprising a photochromic compound.
[0233] [5] The adhesive composition according to any one of [1] to [4], wherein the polyurethane urea resin contains a third reaction product of a second reaction product having two isocyanate groups and a monoamine, the second reaction product containing a reaction product of a first reaction product having two isocyanate groups and a first diamine, and the first reaction product containing a reaction product of a first diol containing a compound represented by the following formula (Ia) and a first polyisocyanate:
[0234]
[0235] In the formula (Ia), R 1 , R 2 , l, m and n have the same meanings as in formula (I).
[0236] [6] The adhesive composition according to [5], wherein the ratio M3 / M2 of the molar amount M3 of the primary amine to the molar amount M2 of the primary diol is 0.1 or more and 0.9 or less.
[0237] [7] The adhesive composition according to [5] or [6], wherein the number average molecular weight of the first diol determined by the hydroxyl value is 500 or more and 4,000 or less.
[0238] [8] The adhesive composition according to any one of [1] to [7], wherein the softening point of the polyurethane urea resin as determined by thermomechanical analysis (TMA) is 40°C or higher and 200°C or lower.
[0239] [9] The adhesive composition according to any one of [1] to [8], further comprising a second polyisocyanate compound.
[0240]
[10] A cured product of the adhesive composition according to any one of [1] to [9].
[0241]
[11] A laminate comprising a resin layer containing the cured product according to
[10] and an optical substrate.
[0242]
[12] A laminate comprising: a first optical substrate and a second optical substrate; a resin layer containing the cured product according to
[10] ; a first adhesive layer that bonds the first optical substrate and the resin layer; and a second adhesive layer that bonds the second optical substrate and the resin layer.
[0243]
[13] The laminate according to
[12] , wherein at least one of the first adhesive layer and the second adhesive layer contains the cured product according to
[10] .
[0244]
[14] The laminate according to
[11] , wherein the optical substrate contains at least one resin selected from the group consisting of a polycarbonate resin, a cellulose resin, and a polyvinyl alcohol resin.
[0245]
[15] An optical article comprising the laminate according to
[11] .
[0246]
[16] A lens comprising the optical article according to
[15] .
[0247]
[17] Eyeglasses including the lens according to
[16] .
Claims
1. An adhesive composition comprising a polyurethane urea resin having a urea bond, a urethane bond, and a structure represented by the following formula (I), and an organic solvent. In the formula (I), R 1 and R 2 each independently represents a linear alkylene group having 3 to 10 carbon atoms; l is 0 or 1 to 25; and each independently represents 2 to 70.
2. The adhesive composition according to claim 1, wherein in formula (I), l is 1 or more and 25 or less.
3. The adhesive composition of claim 1, further comprising a functional dye.
4. The adhesive composition of claim 1, further comprising a photochromic compound.
5. The adhesive composition according to claim 1, wherein the polyurethane urea resin comprises a third reaction product of a second reaction product having two isocyanate groups and a monoamine, the second reaction product comprising a reaction product of a first reaction product having two isocyanate groups and a first diamine, and the first reaction product comprising a reaction product of a first diol comprising a compound represented by the following formula (Ia) and a first polyisocyanate: In the formula (Ia), R 1 , R 2 , l, m and n are as defined above in formula (I).
6. The adhesive composition according to claim 5, wherein the ratio M3 / M2 of the molar amount M3 of the first diamine to the molar amount M2 of the first diol is 0.1 or more and 0.9 or less.
7. The adhesive composition according to claim 5, wherein the number average molecular weight of the first diol based on the hydroxyl value is 500 or more and 4,000 or less.
8. The adhesive composition according to claim 1, wherein the softening point of the polyurethane urea resin as determined by thermomechanical analysis (TMA) is 40°C or higher and 200°C or lower.
9. The adhesive composition of claim 1, further comprising a second polyisocyanate compound.
10. A cured product of the adhesive composition according to claim 1.
11. A laminate comprising a resin layer containing the cured product according to claim 10 and an optical substrate.
12. A laminate comprising a first optical substrate and a second optical substrate; a resin layer containing the cured product according to claim 10; a first adhesive layer bonding the first optical substrate and the resin layer; and a second adhesive layer bonding the second optical substrate and the resin layer.
13. The laminate according to claim 12, wherein at least one of the first adhesive layer and the second adhesive layer comprises the cured product according to claim 10.
14. The laminate according to claim 11, wherein the optical substrate comprises at least one resin selected from the group consisting of polycarbonate resins, cellulose resins, and polyvinyl alcohol resins.
15. An optical article comprising the laminate of claim 11.
16. A lens comprising the optical article of claim 15.
17. Eyeglasses comprising the lens of claim 16.
Citation Information
Patent Citations
Photochromic laminate and production method of the same
JP2013033131A
Photochromic composition, laminate comprising the composition, and article using the laminate
JP2016169363A
Thermoplastic polyurethane produced by using polytetramethylene carbonate diol and production of polytetramethylene carbonate diol
JP1994206965A
Adhesive comprising polyurethane composition
JP2000044918A
Photochromic composition
JP2012052091A