Polylactic acid modifier, polylactic acid resin composition, and method for producing molded article

The use of a block copolymer with polylactic acid and polyol structural units addresses the complexity of conventional polylactic acid modifier processes by improving flexibility and crystallinity with a single additive, enhancing production efficiency and molding capabilities.

WO2024214773A1PCT designated stage expired Publication Date: 2024-10-17DAICEL CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014661
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-14
Filing Date
2024-04-11
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Conventional polylactic acid modifiers require multiple additives to improve flexibility and crystallinity, complicating the manufacturing process and reducing production efficiency due to the need for separate equipment and solvent removal.

Method used

A block copolymer with a structure of polylactic acid/polyol/polylactic acid, containing structural units from L-type or D-type polylactic acid and a polyol, such as polycaprolactone, which acts as a single additive to enhance flexibility and crystallinity, allowing for easier mixing and processing without fluidity at room temperature.

Benefits of technology

The polylactic acid resin composition exhibits improved flexibility and crystallization rates, reducing crystallization time by 30% and enhancing production efficiency, with the block copolymer content between 0.5% to 50% by mass, suitable for various molding methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

The objective of the present invention is to provide a polylactic acid modifier that can improve flexibility and crystallinity with a single additive and that can produce a polylactic acid resin composition excellent in production efficiency. The polylactic acid modifier according to the present disclosure is characterized by comprising at least structural units derived from either L-type or D-type polylactic acid and structural units derived from a polyol, and being a triblock copolymer of polylactic acid / polyol / polylactic acid. Furthermore, the polylactic acid modifier preferably has an average particle size of 0.5 mm in diameter or more, and the polyol is preferably polycaprolactone.
Need to check novelty before this filing date? Find Prior Art

Description

Polylactic acid modifier, polylactic acid resin composition, and method for producing molded product

[0001] The present disclosure relates to a polylactic acid modifier, a polylactic acid resin composition, and a method for producing a molded article. This application claims priority from Japanese Patent Application No. 2023-066678, filed on April 14, 2023, the contents of which are incorporated herein by reference.

[0002] Polylactic acid is a resin material that is biodegradable and biomass-based, and demand for it as a material that can address environmental issues is growing. However, it has known problems, such as being hard and brittle, with poor impact resistance and flexibility, and poor crystallinity, which means it takes a long time to solidify or crystallize, and it has poor heat resistance.

[0003] It is known that various modifiers can be used to improve the physical properties of these polylactic acids. For example, it is known that a plasticizer or a nucleating agent can be added as an additive to improve flexibility and heat resistance (see, for example, Patent Document 1).

[0004] Another known modification method is to use a compound containing an optical isomer as an additive to form a stereocomplex (sc crystal) to improve crystallinity (see, for example, Patent Document 2).

[0005] JP 2014-118452 A International Publication No. 2011 / 030766

[0006] However, conventional additives have required the use of multiple additives in combination to improve flexibility and crystallinity. Furthermore, because the additives are typically in liquid or powder form, when used with polylactic acid, which is generally in pellet form, separate mixing equipment is required. This has led to the problem of complicated manufacturing processes.

[0007] Furthermore, in the compound disclosed in Patent Document 2, polylactic acid and additives need to be dissolved in a solution, which takes time for mixing and requires special equipment for dissolution, making the production process complicated. Furthermore, the need to remove the solvent also leads to problems such as a decrease in production efficiency.

[0008] Therefore, an object of the present disclosure is to provide a polylactic acid modifier that can improve flexibility and crystallinity with a single additive and that can produce a polylactic acid resin composition with excellent production efficiency.

[0009] That is, the present disclosure provides a polylactic acid modifier that is a block copolymer that contains at least a structural unit derived from either L-type or D-type polylactic acid and a structural unit derived from a polyol, and has a polylactic acid / polyol / polylactic acid structure.

[0010] The polylactic acid modifier preferably has an average particle size of 0.5 mmΦ or more.

[0011] The polylactic acid modifier preferably does not exhibit fluidity at room temperature.

[0012] The polylactic acid modifier preferably uses polycaprolactone as the polyol.

[0013] The present disclosure also provides a polylactic acid resin composition that is a mixture of L- or D-type polylactic acid and a block copolymer that is a polylactic acid modifier containing at least a polylactic acid of a type different from the polylactic acid and a polyol, wherein the block copolymer does not exhibit fluidity at room temperature and has an average particle size of 0.5 mmΦ or more, and the time required for crystallization when cooled from a molten state to 100 to 110°C and kept at that temperature can be reduced by 30% or more compared to the polylactic acid alone, and the flexibility at room temperature is improved by 5% or more.

[0014] The polylactic acid resin composition preferably has a block copolymer content of 0.5 to 50% by mass based on the total amount of the polylactic acid resin composition.

[0015] In the polylactic acid resin composition, the polyol is preferably polycaprolactone.

[0016] The present disclosure also provides a method for producing a molded article obtained by molding the polylactic acid resin composition using any one of molding methods selected from the group consisting of injection molding, extrusion molding, compression molding, transfer molding, lamination molding, cast molding, powder molding, calendar molding, foam molding, blow molding, vacuum / pressure molding, and melt spinning.

[0017] The polylactic acid modifier of the present disclosure can improve flexibility and crystallinity as a single additive, making it possible to prepare a polylactic acid resin composition with excellent production efficiency.

[0018] [Polylactic Acid Modifier] The polylactic acid modifier according to one embodiment of the present disclosure is a block copolymer containing at least a structural unit derived from either L-type or D-type polylactic acid and a structural unit derived from a polyol, and having a polylactic acid / polyol / polylactic acid structure (hereinafter, the block copolymer may be referred to as the "block copolymer of the present disclosure"). Only one type of block copolymer of the present disclosure may be used, or two or more types may be used.

[0019] The block copolymer of the present disclosure contains at least a structural unit derived from either L-type or D-type polylactic acid and a structural unit derived from a polyol, and is a block copolymer having a polylactic acid / polyol / polylactic acid structure, and forms sc crystals with the polylactic acid, thereby improving the crystallinity of the polylactic acid, and since it contains a polyol, it can also improve flexibility.

[0020] In the present disclosure, "crystalline" refers to the ease with which a polylactic acid resin composition crystallizes, and "good crystallinity" means that the composition crystallizes quickly.

[0021] The block copolymer of the present disclosure preferably further contains a structural portion derived from a polymerization initiator. As the polymerization initiator, known or conventional polymerization initiators can be used, such as low-molecular-weight diol compounds and low-molecular-weight diamines. The molecular weight of the polymerization initiator is preferably 500 or less.

[0022] Examples of the low molecular weight diol compound include ethylene glycol, propylene glycol, 1,4-butylene glycol, 2-methylpropanediol, neopentyl glycol, pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 3-methyl-1,5-pentanediol, 3,3-dimethylolheptane, neopentyl glycol, diethylene glycol, dipropylene glycol, cyclohexane-1,4-diol, cyclohexane-1,4-dimethanol, dimer acid diol, etc. Among these, diethylene glycol is particularly preferred.

[0023] The content of the polymerization initiator is preferably 0.2 to 2.0% by mass, more preferably 0.2 to 1.0% by mass, and even more preferably 0.2 to 0.5% by mass, relative to the total amount of the block copolymer of the present disclosure.

[0024] The polyol in the block copolymer of the present disclosure is preferably one having a thermal decomposition temperature of 200° C. or higher from the viewpoint of dissolving it together with polylactic acid, and specific examples thereof include polylactone polyols, polyester polyols, polyether polyols, polycarbonate polyols, polyolefin polyols, poly(meth)acrylic polyols, etc. Note that only one type of polyol may be used, or two or more types may be used.

[0025] Examples of the polylactone polyols include polybutyrolactone, polyvalerolactone, and polycaprolactone.

[0026] Examples of the polyester polyols include polyethylene adipate diol, polybutylene adipate diol, polyhexamethylene adipate diol, polyhexamethylene isophthalate diol, polyneopentyl adipate diol, polyethylene propylene adipate diol, polyethylene butylene adipate diol, polybutylene hexamethylene adipate diol, poly(polyoxytetramethylene) adipate diol, poly(3-methylpentylene adipate) diol, polyethylene azelate diol, polyethylene sebacate diol, polybutylene azelate diol, polybutylene sebacate diol, and polyneopentyl terephthalate diol.

[0027] Examples of the polyether polyols include polyalkylene glycols such as polyethylene glycol, polypropylene glycol, poly-1,2-butylene glycol, polytetramethylene glycol (poly-1,4-butanediol), poly-3-methyltetramethylene glycol, and polyneopentyl glycol.

[0028] Examples of the polycarbonate polyols include polyhexamethylene carbonate diol, polypentamethylene carbonate diol, polytetramethylene carbonate diol, and poly(tetramethylene / hexamethylene) carbonate diol (e.g., a diol obtained by condensing 1,4-butanediol and 1,6-hexanediol with a dialkyl carbonate while causing a dealcoholization reaction).

[0029] Examples of the poly(meth)acrylic polyols include homopolymers and copolymers of (meth)acrylic acid esters having a hydroxy group. Poly(meth)acrylic polyols can also be obtained by copolymerizing a compound having a polymerizable unsaturated bond in addition to a (meth)acrylic acid ester having a hydroxy group. In the present invention, "(meth)acrylic" means "methacrylic and / or acrylic."

[0030] Examples of the (meth)acrylic acid ester having a hydroxy group include those having one (meth)acryloyl group, such as those having a hydroxyalkyl group having 2 to 20 carbon atoms (for example, hydroxyalkyl (meth)acrylic acid esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate), and (meth)acrylic acid monoesters of trihydric alcohols (for example, glycerin (meth)acrylic acid monoester and trimethylolpropane (meth)acrylic acid monoester).

[0031] In particular, from the viewpoint of imparting flexibility to the polylactic acid resin composition, the polyol is preferably the polylactone polyol, and among these, polycaprolactone is particularly preferred because it does not contain any components harmful to the human body.

[0032] The number average molecular weight (Mn) of the polyol in the block copolymer of the present disclosure is preferably 1,300 to 22,000, more preferably 1,800 to 15,000, and even more preferably 3,000 to 10,000. A number average molecular weight (Mn) of 1,300 or more makes it easy to impart flexibility to the polylactic acid resin composition, and a number average molecular weight (Mn) of 22,000 or less makes it possible to suppress the formation of a continuous crystalline structure of the polyol, making it easier to maintain the flexibility of the material.

[0033] The polyol content in the block copolymer of the present disclosure is preferably 15 to 90% by mass, more preferably 20 to 85% by mass, and even more preferably 30 to 80% by mass, based on the total amount of the block copolymer of the present disclosure. When the polyol content is 15% by mass or more, the amount of polyol is sufficient, making it easy to impart flexibility to the polylactic acid resin composition. When the polyol content is 90% by mass or less, it makes it easy to improve crystallinity.

[0034] The polylactic acid in the block copolymer of the present disclosure is preferably a type different from that of the polylactic acid to be modified. That is, when the polylactic acid to be modified is L-type polylactic acid, the polylactic acid in the block copolymer of the present disclosure preferably contains D-type polylactic acid as a main component, and when the polylactic acid to be modified is D-type polylactic acid, the polylactic acid in the block copolymer of the present disclosure preferably contains L-type polylactic acid as a main component.

[0035] When the polylactic acid in the block copolymer of the present disclosure is an L-type polylactic acid composed mainly of L-type lactic acid, the content of L-type lactic acid units is preferably 90% by mass or more, more preferably 99% by mass or more, and when the polylactic acid is a D-type polylactic acid composed mainly of D-type lactic acid, the content of D-type lactic acid units is also ...

[0036] Furthermore, the number average molecular weight (Mn) of the polylactic acid in the block copolymer of the present disclosure is preferably 4,000 to 15,000, more preferably 5,000 to 12,000, and even more preferably 6,000 to 10,000. A number average molecular weight (Mn) of 4,000 or more makes it easy to form sc crystals with the polylactic acid of the present disclosure and improve crystallinity, while a number average molecular weight of 15,000 or less can prevent the rapid growth of sc crystals or excessive expansion of sc crystal domains from forming non-uniform crystals and destabilizing physical properties.

[0037] The content of polylactic acid in the block copolymer of the present disclosure is preferably 10 to 85% by mass, more preferably 15 to 80% by mass, and even more preferably 20 to 75% by mass, based on the total amount of the block copolymer of the present disclosure. When the content of polylactic acid is 10% by mass or more, the amount of polylactic acid is sufficient, making it easy to impart crystallinity. When the content of polylactic acid is 85% by mass or less, it makes it easy to impart flexibility. Note that the above content of polylactic acid represents the total amount of polylactic acid added to both ends of the polyol.

[0038] The number-average molecular weight (Mn) of the block copolymer of the present disclosure is preferably 10,000 to 50,000, more preferably 12,000 to 45,000, and even more preferably 14,000 to 40,000. A number-average molecular weight of 10,000 or more of the block copolymer facilitates imparting flexibility and crystallinity. Furthermore, a number-average molecular weight of 50,000 or less can suppress variations in product quality caused by increased viscosity, which can lead to increased stirring blade load and uneven heat conduction in the reaction system.

[0039] The weight-average molecular weight (Mw) of the block copolymer of the present disclosure is preferably 10,000 to 100,000, more preferably 15,000 to 90,000, and even more preferably 20,000 to 80,000. A weight-average molecular weight of 10,000 or more of the block copolymer makes it easy to impart flexibility and crystallinity. Furthermore, a weight-average molecular weight of 100,000 or less can suppress variations in product quality caused by increased viscosity, which can lead to increased stirring blade load and uneven heat conduction in the reaction system.

[0040] The total amount of the polyol, the polylactic acid, and the polymerization initiator in the block copolymer of the present disclosure is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 100% by mass, based on the total amount of the block copolymer of the present disclosure.

[0041] The block copolymer of the present disclosure may also contain other components in addition to the polymerization initiator, polylactic acid, and polyol. Examples of such other components include antioxidants, fillers, flame retardants, pigments, antistatic agents, processing aids, and viscosity improvers. The content of such other compounds is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, even more preferably 1 part by mass or less, and particularly preferably 0 parts by mass, per 100 parts by mass of the total amount of the block copolymer of the present disclosure. The block copolymer of the present disclosure may also contain a solvent, but preferably does not contain a solvent in order to maintain the pellet shape.

[0042] The block copolymer of the present disclosure preferably does not exhibit fluidity at room temperature (25°C). In the present disclosure, "fluid" means a liquid or paste-like property that exhibits fluidity at room temperature, and is not solid. Since the block copolymer of the present disclosure does not exhibit fluidity at room temperature, it can be easily mixed with the polylactic acid of the present disclosure and has excellent handleability.

[0043] The block copolymer of the present disclosure preferably has an average particle size of 0.5 mmΦ or more, more preferably 1 mmΦ or more, and even more preferably 1.5 mmΦ or more. Having an average particle size of 0.5 mmΦ or more facilitates kneading with other resin compounds. The pellet shape of the block copolymer of the present disclosure is not particularly limited, and examples thereof include circular, spherical, and sliced ​​pellets. In the present disclosure, the average particle size was determined by shaking sieves with openings of 2.8 mm, 2.36 mm, 2.0 mm, 1.7 mm, and 1.4 mm and a tray stacked in that order for 30 seconds, selecting 10 pellets from the sieve with the largest remaining amount, measuring their sizes with a vernier caliper, and calculating the average value.

[0044] The block copolymer of the present disclosure can be synthesized by known or conventional methods. Specifically, for example, depending on the block copolymer to be obtained, polyol and polylactic acid can be melt-mixed or solution-mixed in a predetermined ratio, followed by solidification and solid-state polymerization. Alternatively, the block copolymer can be produced by first synthesizing a polyol, preferably by heating to 140 to 200°C, and then heating polylactic acid to its molecular terminals, preferably at 150 to 250°C, for sequential polymerization growth. Conversely, polylactic acid can also be produced by first synthesizing polylactic acid, then sequentially polymerizing and growing a polyol at its molecular terminals, followed by sequential polymerization growth of polylactic acid.

[0045] In particular, when the polyol is a polylactone polyol, it is preferable to produce the polylactone by ring-opening polymerization of lactone at the terminal of a polymerization initiator to obtain the polylactone, and then by sequentially polymerizing and growing polylactic acid at the molecular terminal of the polylactone.

[0046] [Polylactic Acid Resin Composition] A polylactic acid resin composition according to one embodiment of the present disclosure is a mixture of L- or D-polylactic acid and a block copolymer that is a polylactic acid modifier containing at least a polylactic acid of a type different from the polylactic acid and a polyol, wherein the block copolymer does not exhibit fluidity at room temperature, has an average particle size of 0.5 mmφ or more, and can reduce the time required for crystallization when cooled from a molten state to 100 to 110°C and maintained at that temperature by 30% or more compared to the polylactic acid alone, and has an improvement in flexibility at room temperature of 5% or more.

[0047] The polylactic acid resin composition contains the L- or D-polylactic acid, a polylactic acid of a different type from the polylactic acid, and a block copolymer containing at least a polyol, which allows the formation of SC crystals. This reduces the time required for crystallization by 30% or more compared to polylactic acid alone when the temperature is lowered from a molten state to 100-110°C and maintained at that temperature, thereby improving crystallinity. Furthermore, the block copolymer contains the polyol, which improves flexibility by 5% or more compared to polylactic acid alone. Furthermore, the block copolymer has no fluidity and an average particle size of 0.5 mm or more, allowing it to be easily mixed with the polylactic acid, resulting in excellent production efficiency.

[0048] The time required for crystallization when the polylactic acid resin composition is cooled from a molten state to 100 to 110°C and kept at that temperature (hereinafter sometimes referred to as the "half-crystallization time") is preferably within 100 seconds, more preferably within 80 seconds, and even more preferably within 70 seconds. Furthermore, compared to the half-crystallization time of polylactic acid alone (145 seconds), the half-crystallization time of the polylactic acid resin composition can be reduced by 30% or more, preferably by 40% or more, and even more preferably by 50% or more. By reducing the half-crystallization time of the polylactic acid resin composition by 30% or more compared to the half-crystallization time of polylactic acid alone, crystallization can be accelerated, improving production efficiency. In the present disclosure, the temperature at which the polylactic acid resin composition is cooled from a molten state to 100 to 110°C may be any temperature within the above range, as long as the temperatures being compared are the same.

[0049] In the present disclosure, the half-crystallization time is calculated as the time it takes for the peak area of ​​the exothermic peak of the polylactic acid resin composition to reach half when the polylactic acid resin composition is heated to 190°C by differential scanning calorimetry (DSC), held for 5 minutes to dissolve, rapidly cooled to 100-110°C, and held for 15 minutes.

[0050] The flexural modulus of the polylactic acid resin composition, measured by the method described in the Examples below, is preferably 3700 MPa or less, more preferably 3600 MPa or less, and even more preferably 3500 MPa or less. Furthermore, the reduction rate of the flexural modulus of the polylactic acid resin composition relative to the flexural modulus of the polylactic acid alone (flexibility improvement rate) is 5% or more, preferably 7% or more, and even more preferably 10% or more. By having the flexibility improvement rate of the polylactic acid resin composition relative to the polylactic acid alone of 5% or more, the polylactic acid resin composition can easily exhibit flexibility.

[0051] Furthermore, the difference between the mass ratio of the polylactic acid and the block copolymer in the polylactic acid resin composition measured by the method described in the Examples below and the designed mass ratio is preferably within ±20%, more preferably within ±10%. When the difference between the actual mass ratio and the designed mass ratio is within ±20%, mixing can be easily performed.

[0052] <Polylactic acid> The polylactic acid resin composition contains either L-type or D-type polylactic acid (hereinafter sometimes referred to as "polylactic acid of the present disclosure"). Furthermore, it is preferable to use the polylactic acid of the present disclosure in combination with the block copolymer of the present disclosure. The polylactic acid of the present disclosure is a polymer compound obtained by polymerizing a plurality of lactic acid units (CHCH(OH)COOH) via ester bonds.

[0053] Lactic acid, which is a structural unit of the polylactic acid of the present disclosure, is known to have two optical isomers: L-type and D-type. In the present disclosure, either L-type or D-type lactic acid can be used as a structural unit. Furthermore, in order to form sc crystals with the block copolymer described below, the polylactic acid of the present disclosure is preferably a polymer primarily composed of either L-type or D-type. In the case of an L-type polylactic acid primarily composed of L-type lactic acid, the content of L-type lactic acid units is preferably 90% by mass or more, more preferably 99% by mass or more, and is a homopolymer. Similarly, when the polylactic acid is a D-type polylactic acid primarily composed of D-type lactic acid, the content of D-type lactic acid units is preferably 90% by mass or more, more preferably 99% by mass or more, and is a homopolymer.

[0054] The polylactic acid of the present disclosure may also contain other components to the extent that their properties are not impaired. Examples of such other components include catalysts, end-capping agents, additives, etc. The content of such other components is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, and even more preferably 0 parts by mass, relative to the total amount of the polylactic acid.

[0055] The polylactic acid of the present disclosure can be produced by a known method for polymerizing polylactic acid, such as ring-opening polymerization of lactide, dehydration condensation of lactic acid, or a combination of these with solid-state polymerization, followed by melt-solidification.

[0056] The number average molecular weight (Mn) of the polylactic acid of the present disclosure is preferably 2,000 to 50,000,000, and more preferably 3,000 to 20,000,000. The weight average molecular weight (Mw) of the polylactic acid of the present disclosure is preferably 2,000 to 80,000,000, and more preferably 3,000 to 40,000,000.

[0057] The content of the polylactic acid of the present disclosure relative to the total amount of the polylactic acid resin composition is preferably 50 to 99.5% by mass, more preferably 60 to 99% by mass, and even more preferably 70 to 98% by mass. By having the content of the polylactic acid of the present disclosure be 50% by mass or more, it is possible to improve the crystallinity and flexibility while maintaining the physical properties of polylactic acid. Furthermore, by having the content be 99.5% by mass or less, it becomes easy to improve the flexibility and crystallinity of the polylactic acid resin composition.

[0058] The polylactic acid of the present disclosure preferably has an average particle size of 0.5 mmΦ or more, more preferably 1.0 mmΦ or more, and even more preferably 1.5 mmΦ or more. By having an average particle size of 0.5 mmΦ or more, the polylactic acid of the present disclosure can be easily kneaded.

[0059] <Block Copolymer> The polylactic acid resin composition contains a block copolymer containing at least a polylactic acid different from the polylactic acid of the present disclosure and a polyol as a polylactic acid modifier. Only one type of the block copolymer may be used, or two or more types may be used.

[0060] Furthermore, the block copolymer preferably further contains a structural portion derived from a polymerization initiator, and depending on the structure of the polymerization initiator, a structure such as a diblock copolymer, a triblock copolymer, a star block copolymer, or a comb block copolymer can be formed.

[0061] As the polymerization initiator, known or commonly used polymerization initiators can be used, such as low-molecular-weight hydroxyl group-containing compounds and low-molecular-weight amines. The molecular weight of the polymerization initiator is preferably 500 or less.

[0062] Examples of the low molecular weight hydroxy group-containing compound include monool compounds such as ethanol, propanol, butanol, pentanol, and hexanol; diol compounds such as ethylene glycol, propylene glycol, 1,4-butylene glycol, 2-methylpropanediol, neopentyl glycol, pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 3-methyl-1,5-pentanediol, 3,3-dimethylolheptane, neopentyl glycol, diethylene glycol, dipropylene glycol, cyclohexane-1,4-diol, cyclohexane-1,4-dimethanol, and diol dimer acid; alkanetriols having 2 to 8 carbon atoms such as 1,2,4-butanetriol and 1,2,6-hexanetriol; and triol compounds such as 5- to 6-membered cycloalkanetriols such as 1,2,3-cyclohexanetriol; and low molecular weight hydroxy group-containing compounds having four or more hydroxy groups. Among these, diol compounds are preferred because they can be used to prepare triblock copolymers, and diethylene glycol is particularly preferred.

[0063] By using the monool compound as the polymerization initiator, a diblock copolymer containing the polyol and the polylactic acid on one side of the polymerization initiator can be prepared, by using the diol compound, a triblock copolymer containing the polyol and the polylactic acid on both ends of the polymerization initiator can be prepared, and by including a triol compound or a low-molecular-weight hydroxyl-containing compound having four or more hydroxyl groups, a star-shaped or comb-shaped block copolymer can be prepared. Among these, the block copolymer is preferably the block copolymer of the present disclosure.

[0064] The block copolymer does not exhibit fluidity at room temperature (25°C). In the present disclosure, "fluid" means a liquid or paste-like property that exhibits fluidity at room temperature, and is not solid. Because the block copolymer does not exhibit fluidity at room temperature, it can be easily mixed with the polylactic acid of the present disclosure and has excellent handleability.

[0065] The block copolymer has an average particle size of 0.5 mm or more, preferably 1 mm or more, and more preferably 1.5 mm or more. Having an average particle size of 0.5 mm or more facilitates blending with other resin compounds. The pellet shape of the block copolymer is not particularly limited, but may be circular, spherical, or sliced.

[0066] The content of the block copolymer in the polylactic acid resin composition is preferably 0.5 to 50% by mass, more preferably 1 to 40% by mass, and even more preferably 2 to 30% by mass. A block copolymer content of 0.5% or more facilitates improving the flexibility and crystallinity of the polylactic acid resin composition. A block copolymer content of 50% by mass or less improves the crystallinity and flexibility while maintaining the physical properties of polylactic acid.

[0067] The block copolymer can be prepared in the same manner as the block copolymer of the present disclosure described above.

[0068] The polylactic acid resin composition can be produced by mixing the polylactic acid of the present disclosure and the block copolymer by a known or conventional method. Specifically, the polylactic acid of the present disclosure and the block copolymer are fed through the main feeder of a twin-screw kneading extruder and kneaded and melted in the extruder. The polylactic acid resin composition can be easily mixed with polylactic acid in a pellet form, since the block copolymers do not exhibit fluidity at room temperature and can be fed in the form of pellets with an average particle size of 0.5 mm or more.

[0069] It is also preferable that the polylactic acid resin composition is produced without using a solvent, since the polylactic acid resin composition does not require steps for dissolution or solvent removal, and therefore, the production efficiency can be improved.

[0070] [Method for producing molded articles] Furthermore, molded articles can be produced by molding the polylactic acid resin composition produced by the above-mentioned method using a method such as injection molding, extrusion molding, compression molding, transfer molding, laminate molding, cast molding, powder molding, calendar molding, foam molding, blow molding, vacuum / pressure molding, or melt spinning.

[0071] It is known that when polylactic acid is used as a raw material, the crystallization of polylactic acid is slow during the molding process, which requires a long cooling process and reduces production efficiency, but the polylactic acid resin composition contains a block copolymer, which allows the formation of sc crystals and enables early crystallization, thereby improving production efficiency.In addition, the polyol structural unit provides excellent flexibility.

[0072] Each aspect disclosed in this specification can be combined with any other feature disclosed in this specification. Furthermore, each configuration and combination thereof in each embodiment is merely an example, and additions, omissions, and other modifications of configurations are possible as appropriate within the scope of the present disclosure. The present disclosure is not limited by the embodiments, but is limited only by the claims.

[0073] Hereinafter, one embodiment of the present disclosure will be described in more detail based on examples.

[0074] Production Example 1 (Synthesis of Block Copolymer) As raw materials, 246.77 g of ε-caprolactone (manufactured by Daicel Corporation) and 2.19 g of diethylene glycol (manufactured by Tokyo Chemical Industry Co., Ltd.) were charged into a separable flask and heated to 100°C, followed by the addition of 0.0314 g of stannous octoate (trade name "Stanoct", manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.). The temperature was then increased to 150°C, and the mixture was stirred and heated until the concentration of ε-caprolactone reached less than 1% by mass. After cooling to 60°C, 60.60 g of D-lactide (D-isomer purity: 96.4%) was added, and the mixture was heated to 170°C at normal pressure and stirred and heated until the concentration of D-lactide reached less than 4% by mass. Through the above steps, 306.1 g of a triblock copolymer of D-form polylactic acid (PDLA) / polycaprolactone (PCL) / D-form polylactic acid (PDLA) (weight average molecular weight (Mw): 31,000, number average molecular weight (Mn): 15,000; hereinafter, sometimes referred to as “block copolymer A”) was obtained.

[0075] Block copolymer A was placed in a melting cylinder (500 ml) of a simple extrusion device and melted by heating with a heating jacket at 170°C to 190°C for 10 minutes. The pressure cylinder was operated, and the resin was passed through a (circular) die with a hole diameter of 2.5 mmΦ and pelletized with a small pelletizer, yielding pellets of the block copolymer of Production Example 1 with an average particle diameter of 2.3 mmΦ.

[0076] Production Example 2 531 g of block copolymer pellets for Production Example 2 were obtained under the same conditions as in Production Example 1, except that 108.56 g of ε-caprolactone (manufactured by Daicel Corporation) and 488.5 g of D-lactide (D-isomer purity: 96.4%) were used as raw materials. The block copolymer of Production Example 2 was a PDLA / PCL / PDLA triblock copolymer (weight average molecular weight (Mw): 34,000, number average molecular weight (Mn): 20,000; hereinafter, sometimes referred to as "block copolymer B").

[0077] Production Example 3 583 g of block copolymer pellets for Production Example 3 were obtained under the same conditions as in Production Example 1, except that 238.91 g of ε-caprolactone (manufactured by Daicel Corporation) and 358.4 g of D-lactide (D-isomer purity: 96.4%) were used as raw materials. The block copolymer of Production Example 3 was a PDLA / PCL / PDLA triblock copolymer (weight average molecular weight (Mw): 44,000, number average molecular weight (Mn): 30,000; hereinafter, sometimes referred to as "block copolymer C").

[0078] Production Example 4 814 g of block copolymer pellets for Production Example 4 were obtained under the same conditions as in Production Example 1, except that 413.68 g of ε-caprolactone (manufactured by Daicel Corporation) and 413.7 g of D-lactide (D-isomer purity: 96.4%) were used as raw materials. The block copolymer of Production Example 4 was a PDLA / PCL / PDLA triblock copolymer (weight average molecular weight (Mw): 73,000, number average molecular weight (Mn): 39,000; hereinafter, sometimes referred to as "block copolymer D").

[0079] Example 1: Pellets of block copolymer A and L-type polylactic acid (PLLA) pellets (L-isomer purity 99% or more, average particle size 2.5 mm) from Production Example 1 were each dried in a constant temperature dryer at 80°C for at least 3 hours. After drying, they were allowed to cool in a desiccator, and a mixture of 3% by mass of block copolymer A and 97% by mass of PLLA was weighed out and placed in a shaker for blending. The cylinder temperature of a small resin kneading device (trade name: Labo Plastomill 4M150, manufactured by Toyo Seiki Seisakusho, Ltd.) was set to 190°C, and 30 g of the weighed pellets were placed in the kneading chamber while rotating the cylinder at 10 rpm. The lid was then closed, the cylinder rotation speed was increased to 50 rpm, and kneading was performed for 5 minutes. The cylinder was stopped, and the uniformly kneaded molten resin was removed, placed in a metal tray, and cooled in a desiccator to prepare the polylactic acid resin composition of Example 1.

[0080] Example 2 A polylactic acid resin composition of Example 2 was prepared in the same manner as in Example 1, except that the blending amounts shown in Table 1 were used.

[0081] Examples 3 and 4 Polylactic acid resin compositions of Examples 3 and 4 were prepared in the same manner as in Example 1, except that the block copolymer B prepared in Production Example 2 was used in the amounts shown in Table 1.

[0082] Examples 5 and 6 Polylactic acid resin compositions of Examples 5 and 6 were prepared in the same manner as in Example 1, except that the block copolymer C prepared in Production Example 3 was used in the amounts shown in Table 1.

[0083] Examples 7 and 8 Polylactic acid resin compositions of Examples 7 and 8 were prepared in the same manner as in Example 1, except that the block copolymer D prepared in Production Example 4 was used in the amounts shown in Table 1.

[0084] Comparative Example 1 A polylactic acid resin composition of Comparative Example 1 was prepared in the same manner as in Example 1, except that L-type polylactic acid alone was used.

[0085] Comparative Example 2: Powdered crystallinity improver B (aromatic sulfonate, average particle size 35 μm) and L-form polylactic acid (PLLA) pellets (L-form purity 99% or higher, average particle size 2.5 mm) were dried in a constant-temperature dryer at 80°C for at least 3 hours. The cylinder temperature of a small resin kneading device (trade name "Labo Plastomill 4M150," manufactured by Toyo Seiki Seisaku-sho, Ltd.) was set to 190°C. While rotating the cylinder at 10 rpm, 29.1 g of weighed PLLA pellets were placed in the kneading chamber, followed by 0.9 g of crystallinity improver B. The lid was then closed, and the cylinder rotation speed was increased to 50 rpm for 5 minutes of kneading. The cylinder was then stopped, and the uniformly kneaded molten resin was removed, placed in a metal tray, and cooled in a desiccator to produce the polylactic acid resin composition of Comparative Example 2.

[0086] Comparative Example 3 A polylactic acid resin composition of Comparative Example 3 was prepared in the same manner as in Comparative Example 2, except that a powdery physical property improver A (acrylic compound, average particle size 100 μm) was used.

[0087] Comparative Example 4 A polylactic acid resin composition of Comparative Example 4 was prepared in the same manner as in Comparative Example 2, except that a liquid property improver B (aliphatic ester surfactant) was used.

[0088] Comparative Example 5: D-type polylactic acid (PDLA, granular crystallinity improver A, average particle size 2.5 mmΦ), the powdered physical property improver A, and L-type polylactic acid (PLLA) pellets (L-isomer purity 99% or higher) were dried in a constant temperature dryer at 80°C for 3 hours or more. The cylinder temperature of a small resin kneading device (trade name: Labo Plastomill 4M150, manufactured by Toyo Seiki Seisakusho) was set to 190°C, and while rotating the cylinder at 10 rpm, 29.1 g of weighed PLLA pellets were placed in the kneading chamber, followed by 0.3 g of the granular crystallinity improver A and 0.6 g of the powdered physical property improver A. The lid was then closed, the cylinder rotation speed was increased to 50 rpm, and the mixture was kneaded for 5 minutes. The cylinder was stopped, and the uniformly kneaded molten resin was removed, placed in a metal tray, and cooled in a desiccator to prepare a polylactic acid resin composition of Comparative Example 5.

[0089] Comparative Example 6 A polylactic acid resin composition of Comparative Example 6 was prepared in the same manner as in Comparative Example 5, except that the liquid property improver B was used instead of the powdery property improver A.

[0090] Comparative Example 7 A polylactic acid resin composition of Comparative Example 7 was prepared in the same manner as in Comparative Example 5, except that the powdery crystallinity improving agent B was used instead of the granular crystallinity improving agent A.

[0091] Comparative Example 8 A polylactic acid resin composition of Comparative Example 8 was prepared in the same manner as in Comparative Example 7, except that the liquid property improver B was used instead of the powdery property improver A.

[0092] [Evaluation] The polylactic acid resin compositions prepared in the Examples and Comparative Examples were evaluated as follows, and the results are shown in Table 1. In Table 1, " / " indicates that measurement was not possible, and "-" indicates that measurement was not performed.

[0093] (1) Half-Crystalization Time and Crystallization Time Reduction Rate The polylactic acid resin compositions prepared in the Examples and Comparative Examples were dried at 80°C for 3 hours, and 5 mg of each sample was measured using a DSC under the following conditions. The half-crystallization time was calculated by integrating the time from the start of the exothermic peak formed due to the crystallization of PLLA, the main component of the polylactic acid resin composition, until the peak area reached half. The results are shown below. Measurement device: DSC Q2000 (manufactured by TA Instruments). Measurement conditions: Heat from room temperature to 190°C (heating rate: 86°C / min) and hold for 5 minutes. Then, cool to 100°C (cooling rate: 83°C / min) and hold for 15 minutes.

[0094] The reduction rate of the half-crystallization time compared to the single-unit poly-L lactic acid of Comparative Example 1 was calculated as the reduction rate of the crystallization time.

[0095] (2) Flexural Modulus and Flexibility Improvement Rate The polylactic acid resin compositions prepared in the Examples and Comparative Examples were sheared to particle sizes of 1 to 3 mm and dried in a constant temperature dryer at 80° C. for 3 hours. A mold having multiple frames measuring 1 x 10 x 55 mm was placed on a metal plate, 1 g of the polylactic acid resin composition was placed in each frame, and a metal plate was placed on top of it. The mold was then set in a hot press (trade name "Mini Test Press 10", manufactured by Toyo Seiki Co., Ltd.) previously set at 190°C. The metal plate and mold were placed between the hot press and preheated for 3 minutes without applying pressure, after which the pressing pressure was increased to 10 MPa and maintained for 5 minutes. The metal plate and mold were then transferred to a water-circulating cooling press and cooled for 5 minutes. The test piece was then removed from the mold, and the 1 x 10 x 55 mm test piece was placed in a constant temperature dryer and subjected to a crystallization treatment at 100°C for 20 minutes. The test piece prepared by the above method was subjected to Tensilon bending modulus measurement under the following conditions. Apparatus: RTC-1350A manufactured by Orentec Co., Ltd. Measurement conditions: Test type: 3-point bending test Distance between the lower two supports: 32 mm Testing machine body rigidity: 0 mm / kgf Load full scale: 5 N Test speed: 1 mm / min Control method: Constant moving speed control Measurement temperature: Room temperature

[0096] The reduction rate of the flexural modulus relative to the L-type polylactic acid alone in Comparative Example 1 was calculated as the flexibility improvement rate.

[0097] (3) Handling and manufacturing stability For the polylactic acid resin compositions prepared in the Examples and Comparative Examples, the additives were pre-dyed red and the PLLA pellets were pre-dyed blue with a dye. When two additives were used, the crystallinity improver was pre-dyed red and the physical property improver was pre-dyed blue. The additives were mixed in the same manner except for the coloring and heating, and samples were taken from five random locations in a 10 ml bottle. The pellets removed from the 10 ml bottle were visually separated by color with tweezers, and the mass of each color pellet was measured. The difference between the measured mass ratio of each color pellet and the designed mass ratio was evaluated as follows. When powdery additives were used, the additives were sieved and separated by color for measurement. 〇: The difference between the measured mass ratio and the design mass ratio is 10% or less. △+: The difference between the measured mass ratio and the design mass ratio is between 10% and 20%. △: The difference between the measured mass ratio and the design mass ratio is between 20% and 30%. △-: The difference between the measured mass ratio and the design mass ratio is between 30% and 40%. ×: The difference between the measured mass ratio and the design mass ratio is over 40%, or mixing in an actual machine is difficult.

[0098] (4) Injection molding demolding time and demolding time reduction rate The polylactic acid resin composition of Example 4 was dried in a constant temperature dryer at 80°C for 3 hours, and test specimens were produced using an injection molding machine under the following conditions. The pellets were melted once on the extruder side of the injection molding machine, injected into a mold, and held at a constant pressure after injection. The injection molding demolding time was defined as the shortest time from the time when the holding pressure was released to the time when the test specimen had sufficiently crystallized and solidified so that it could be removed from the mold without deformation. Injection molding machine: Electric injection molding machine (product name "J110AD-180H, manufactured by The Japan Steel Works, Ltd.") Screw diameter: Φ35 mm Mold shape: JIS K 7139 (ISO 20753) Type A1 dumbbell test specimen shape Cylinder temperature: 40 to 200°C (average temperature: 190°C) Mold temperature: 100 to 105°C (set temperature: 100°C)

[0099] Further, the reduction rate (mold release time reduction rate) of the injection molding demolding time of the L-type polylactic acid alone in Comparative Example 1 was calculated.

[0100]

[0101] It was confirmed that the polylactic acid resin compositions using the polylactic acid modifiers of the Examples had improved flexibility and crystallinity compared to conventional additives. Furthermore, the polylactic acid resin compositions of the Examples could be easily mixed without special kneading equipment, and the crystallization time was shortened, demonstrating excellent production efficiency. On the other hand, when polylactic acid alone was used, semi-crystallization took a long time and the flexural modulus was poor (Comparative Example 1). Furthermore, when a powdered crystallinity improver was used alone, flexibility could not be improved, and kneading was difficult, resulting in poor handleability (Comparative Example 2). The use of powdered or liquid physical property improvers also improved flexibility and crystallinity, but poor handleability (Comparative Examples 3 and 4). Furthermore, when the above crystallinity improver and physical property improver were used in combination, flexibility and crystallinity were improved, but handleability was poor (Comparative Examples 5 to 8).

[0102] Variations of the present disclosure are described below. [Appendix 1] A polylactic acid modifier that is a block copolymer containing at least structural units derived from either L-type or D-type polylactic acid and structural units derived from a polyol, and has a polylactic acid / polyol / polylactic acid structure. [Appendix 2] The polylactic acid modifier according to Appendices 1 and 2, which has an average particle size of 0.5 mmΦ or more. [Appendix 3] The polylactic acid modifier according to Appendices 1 or 2, which does not exhibit fluidity at room temperature. [Appendix 4] The polylactic acid modifier according to any one of Appendices 1 to 3, wherein the polyol is polycaprolactone. [Appendix 5] A polylactic acid resin composition comprising a mixture of L- or D-type polylactic acid and a block copolymer that is a polylactic acid modifier containing at least a polylactic acid of a type different from the polylactic acid and a polyol, wherein the block copolymer does not exhibit fluidity at room temperature and has an average particle size of 0.5 mmΦ or more, and which can reduce the time required for crystallization when cooled from a molten state to 100 to 110°C and maintained at that temperature by 30% or more compared to the polylactic acid alone, and which has an improvement in flexibility at room temperature of 5% or more. [Appendix 6] The polylactic acid resin composition according to Appendices 5 and 6, wherein the content of the block copolymer in the total amount of the polylactic acid resin composition is 0.5 to 50% by mass. [Appendix 7] The polylactic acid resin composition according to Appendices 5 and 6, wherein the polyol is polycaprolactone. [Appendix 8] A method for producing a molded product obtained by molding the polylactic acid resin composition according to any one of Appendices 5 to 7 using any one molding method selected from the group consisting of injection molding, extrusion molding, compression molding, transfer molding, lamination molding, cast molding, powder molding, calendar molding, foam molding, blow molding, vacuum / pressure molding, and melt spinning.

Claims

1. A polylactic acid modifier which is a block copolymer containing at least a structural unit derived from either L-type or D-type polylactic acid and a structural unit derived from a polyol and has a structure of polylactic acid / polyol / polylactic acid.

2. The polylactic acid modifier according to claim 1, having an average particle size of 0.5 mmΦ or more.

3. The polylactic acid modifier according to claim 1 or 2, which does not exhibit fluidity at room temperature.

4. The polylactic acid modifier according to claim 1 or 2, wherein the polyol is polycaprolactone.

5. A polylactic acid resin composition comprising a mixture of L-type or D-type polylactic acid and a block copolymer which is a polylactic acid modifier containing at least a polylactic acid of a type different from that of the polylactic acid and a polyol, the block copolymer exhibiting no fluidity at room temperature and having an average particle size of 0.5 mmΦ or more, the time required for crystallization when cooled from a molten state to 100-110°C and kept at that temperature can be reduced by 30% or more compared to the polylactic acid alone, and the flexibility improvement rate at room temperature is 5% or more.

6. The polylactic acid resin composition according to claim 5, wherein the content of said block copolymer in the total amount of said polylactic acid resin composition is 0.5 to 50 mass %.

7. A polylactic acid resin composition according to claim 5 or 6, wherein the polyol is polycaprolactone.

8. A method for producing a molded product obtained by molding the polylactic acid resin composition according to claim 5 or 6 using any one of the molding methods selected from the group consisting of injection molding, extrusion molding, compression molding, transfer molding, lamination molding, cast molding, powder molding, calendar molding, foam molding, blow molding, vacuum / pressure molding, and melt spinning.

Citation Information

Patent Citations

  • Polylactic acid resin composition and its resin molded article

    JP2014118452A

  • Aluminum alloy brazing sheet and method for manufacturing the same

    JP2023066678A

  • Method for producing stereo complex crystals of polylactic acid, polylactic acid, and molded body, synthetic fiber, porous body and ion conductor comprising same

    WO2011030766A1

  • Lactic acid based polymer composition

    JP2002167497A

  • Polylactic acid composition

    JP2004250697A