Recycled polyester resin and film and methods for manufacturing same
By controlling the content of cyclic trimer and diethylene glycol in the recycling process, the challenges of chemical recycling are overcome, resulting in polyester films with enhanced heat resistance and mechanical properties, comparable to virgin products.
Patent Information
- Application Number
- PCT/KR2024/004247
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-11
- Filing Date
- 2024-04-02
- Publication Date
- 2024-10-17
AI Technical Summary
Chemical recycling methods for waste polyester resin struggle to control the content of oligomeric substances like cyclic trimer and diethylene glycol, leading to deterioration in the appearance, performance, and processability of the final product.
The process involves depolymerizing waste polyester to produce recycled bis(2-hydroxyethyl)terephthalate, adjusting its content through specific ranges using high-performance liquid chromatography and gas chromatography, and then using it in condensation polymerization to create a polyester resin with controlled cyclic trimer and diethylene glycol levels, followed by melt extrusion and stretching to produce a high-quality polyester film.
This approach improves the heat resistance, processability, and mechanical properties of the polyester film, ensuring it meets the quality standards equivalent to virgin products while being recycled.
Smart Images

Figure PCTKR2024004247-APPB-IMG-000001 
Figure PCTKR2024004247-APPB-IMG-000002 
Figure PCTKR2024004247-APPB-IMG-000003
Abstract
Description
Regenerated polyester resin and film, and method for producing the same
[0001] The present invention relates to a polyester resin and film regenerated from waste polyester, and a method for producing the same.
[0002]
[0003] Polyester boasts excellent mechanical strength, heat resistance, transparency, and gas barrier properties, making it widely used in beverage containers, packaging films, and audio and video films. Polyester is also widely produced worldwide as industrial materials, including medical fibers and tire cords. In particular, polyester sheets and boards, with their excellent transparency and mechanical strength, are widely used in cases, boxes, partitions, shelves, panels, packaging, building materials, and interior and exterior finishes.
[0004] Accordingly, plastic waste, such as polyester, is generated globally at an unmanageable rate each year. Recently, countries around the world are establishing regulations and measures for recycling waste plastic resources, including waste polyester. For example, there is a movement to require a certain percentage of recycled resin in packaging materials used in various fields. While physical and chemical methods are used to recycle waste polyester, physical recycling methods are not widely used due to their inability to guarantee purity.
[0005] Chemical recycling methods depolymerize waste polyester by breaking the ester bonds, utilizing reactions such as glycolysis, hydrolysis, methanolysis, and aminolysis. Among these, glycolysis involves adding a glycol, such as ethylene glycol or diethylene glycol, to waste polyester at high temperatures to decompose it, producing a reaction product that primarily includes bis(2-hydroxyethyl) terephthalate (BHET). After crystallization or purification, bis(2-hydroxyethyl) terephthalate can be used as a raw material for producing unsaturated polyester or ester polyol.
[0006] [Prior Art Literature]
[0007] (Patent Document 1) Korean Patent No. 1386683
[0008] (Patent Document 2) U.S. Patent No. 7211193
[0009]
[0010] Typically, the depolymerization reaction product of waste polyester resin contains a significant amount of oligomers such as dimers and trimers in addition to bis(2-hydroxyethyl) terephthalate (BHET), and inevitably contains by-products such as diethylene glycol (DEG) generated from high depolymerization temperatures. In particular, since a certain amount of oligomers always exists in equilibrium with the polymer during the manufacturing process, it is difficult to control and reduce their content, and these substances deteriorate the appearance, performance, and processability of the final product.
[0011] Accordingly, the inventors of the present invention have implemented a recycled polyester resin in which the content of cyclic trimer and diethylene glycol is adjusted to a specific range by controlling the recycled raw material and the condensation polymerization process, and have confirmed that the heat resistance, processability, and mechanical properties of the polyester film manufactured therefrom are improved.
[0012] Accordingly, the object of the present invention is to provide a polyester resin having such a composition, a polyester film containing the same having excellent properties, and a method for producing the same.
[0013]
[0014] The present invention provides a polyester resin comprising recycled bis(2-hydroxyethyl)terephthalate obtained by depolymerization of waste polyester, wherein the peak area fraction of a cyclic trimer measured by high-performance liquid chromatography (HPLC) is 3,000 ppm or less, and the content of diethylene glycol (DEG) measured by gas chromatography (GC) is 1.0 wt% or less.
[0015] The present invention also provides a polyester film comprising the polyester resin.
[0016] The present invention also provides a method for producing a polyester film, comprising the steps of: (1) depolymerizing waste polyester to produce recycled bis(2-hydroxyethyl) terephthalate; (2) mixing the recycled bis(2-hydroxyethyl) terephthalate with a solvent to obtain a recycled bis(2-hydroxyethyl) terephthalate solution; (3) producing a polyester resin by a polycondensation reaction using the recycled bis(2-hydroxyethyl) terephthalate solution; and (4) melt-extruding and stretching the polyester resin, wherein the polyester resin has a peak area fraction of a cyclic trimer of 3,000 ppm or less as measured by high-performance liquid chromatography (HPLC) and a content of diethylene glycol (DEG) of 1 wt% or less as measured by gas chromatography (GC).
[0017]
[0018] The polyester resin according to the present invention can improve the heat resistance, processability, and mechanical properties of a polyester film produced therefrom by controlling the content of cyclic trimer and diethylene glycol within a specific range. Furthermore, the polyester resin according to the present invention can also improve the hydrolysis resistance of the final product by controlling the concentration of carboxyl terminal groups within a specific range.
[0019] Accordingly, the film including the polyester resin of the present invention exhibits excellent properties in terms of strength, elongation, and elongation retention rate under high temperature and high humidity conditions.
[0020] Therefore, the polyester resin and film of the present invention can exhibit quality and performance equivalent to that of the original product even though they are products recycled through a chemical recycling method.
[0021]
[0022] The terms used to refer to each component in this specification are used to distinguish it from other components and are not intended to limit the implementation examples. Furthermore, the singular expressions used in this specification include the plural expressions unless the context clearly dictates otherwise.
[0023] In this specification, the terms "first," "second," etc. are used to describe various components, and the components should not be limited by the terms. The terms are used for the purpose of distinguishing one component from another.
[0024] The word "comprising" or "including" in this specification is intended to specify particular features, regions, steps, processes, elements and / or components, and does not exclude the presence or addition of other features, regions, steps, processes, elements and / or components, unless specifically stated to the contrary.
[0025] The molecular weight of the compound described in this specification or the molecular weight of the polymer, for example, the number average molecular weight or the weight average molecular weight, is a relative mass based on carbon-12, as is well known, and does not specify a unit, but may be understood as a molar mass (g / mol) of the same numerical value, if necessary.
[0026] In the numerical ranges that limit the size, physical properties, etc. of the components described in this specification, if a numerical range limited only to the upper limit and a numerical range limited only to the lower limit are separately exemplified, it should be understood that a numerical range in which these upper and lower limits are combined is also included in the exemplary range.
[0027] A polyester resin according to one embodiment comprises recycled bis(2-hydroxyethyl)terephthalate obtained by depolymerization of waste polyester, and has a peak area fraction of a cyclic trimer measured by high-performance liquid chromatography (HPLC) of 3,000 ppm or less, and a content of diethylene glycol (DEG) measured by gas chromatography (GC) of 1.0 wt% or less.
[0028] The present invention will be described in more detail below.
[0029]
[0030] Regenerated bis(2-hydroxyethyl)terephthalate
[0031] The polyester resin according to the present invention comprises bis(2-hydroxyethyl)terephthalate obtained by depolymerization of waste polyester.
[0032] Bis(2-hydroxyethyl)terephthalate is an ester of two ethylene glycols and one terephthalic acid, and is a compound formed as an intermediate in the process of producing polyesters such as polyethylene terephthalate (PET) through a polymerization reaction between ethylene glycol and terephthalic acid or an ester thereof.
[0033] Bis(2-hydroxyethyl)terephthalate (BHET), which is used as a polymerization raw material for the polyester resin according to the present invention, is obtained from waste polyester having ethylene glycol and terephthalic acid as repeating units, such as polyethylene terephthalate (PET) or glycol-modified polyethylene terephthalate (PETG), and can be obtained by a well-known depolymerization method such as glycolysis, hydrolysis, or methanolysis, for example.
[0034] Bis(2-hydroxyethyl) terephthalate (BHET) obtained by depolymerization of waste polyester is conveniently referred to herein as “recycled BHET” or as an abbreviation as r-BHET or rBHET, and it is necessary to understand it as distinct from a pure BHET compound.
[0035] The above-mentioned regenerated BHET may contain byproducts generated by reagents or solvents used in the various chemical steps during depolymerization from waste polyester, or by side reactions with these reagents. These impurities may remain in trace amounts even after multiple purifications. Therefore, regenerated BHET generally contains trace amounts of organic and inorganic impurities in addition to the main component, BHET. For this reason, regenerated BHET can be viewed as a composition comprising two or more components, or as a BHET composition, and can be used as a polymerization raw material for polyester resins.
[0036] Specifically, the above-mentioned regenerated BHET may contain, in addition to the main component BHET, a BHET analogue such as monohydroxyethyl terephthalic acid (MHET) as a heterogeneous organic component, a BHET dimer, a BHET trimer, by-products such as diethylene glycol ester, a metal ion as an inorganic component, and a trace amount of residual solvent components.
[0037] The present invention uses regenerated BHET in which the content of such heterogeneous organic components is controlled within a certain range. The content of each component of such regenerated BHET can be derived by measuring the fraction (%) of the corresponding peak area among the total peak area in a spectrum obtained using high-performance liquid chromatography (HPLC).
[0038] Specifically, the raw material of the present invention, recycled bis(2-hydroxyethyl)terephthalate (BHET), has a peak area fraction of BHET of 96% or more as measured by high-performance liquid chromatography (HPLC). More specifically, the peak area fraction of BHET as measured by HPLC may be 96.5% or more, 97% or more, 97.5% or more, or 98% or more.
[0039] Additionally, the above-mentioned regenerated bis(2-hydroxyethyl)terephthalate may have a peak area fraction of organic impurities measured by HPLC of less than 5% in total, and specifically less than 4%, less than 3%, less than 2%, less than 1%, or less than 0.7%.
[0040] In particular, the polyester resin according to the present invention includes regenerated bis(2-hydroxyethyl)terephthalate (BHET) in which the content of diethylene glycol ester (DEG ester) is adjusted to a certain level or less. For example, the regenerated bis(2-hydroxyethyl)terephthalate may have a peak area fraction of diethylene glycol ester compounds measured by HPLC of less than 2% in total. Specifically, the peak area fraction of diethylene glycol ester compounds may be less than 1.5%, less than 1%, less than 0.8%, or less than 0.7% in total.
[0041] As an example, the diethylene glycol ester compound may be a condensate between an aromatic dicarboxylic acid, such as terephthalic acid, and diethylene glycol. As another example, the diethylene glycol ester compound may be a condensate between an aromatic dicarboxylic acid, such as terephthalic acid, and another glycol, such as diethylene glycol, or ethylene glycol.
[0042] According to one embodiment, the regenerated BHET may include 2-hydroxyethyl[2-(2-hydroxyethoxy)ethyl]terephthalate (CAS No. 65133-69-9) as the first diethylene glycol ester. According to another embodiment, the regenerated BHET may include bis[2-(2-hydroxyethoxy)ethyl]benzene-1,4-dicarboxylate (CAS No. 26850-76-0) as the second diethylene glycol ester. When polymerizing a polyester resin using the regenerated BHET in which the contents of the first diethylene glycol ester and the second diethylene glycol ester are reduced below a certain level, even though the resin is regenerated by a chemical recycling method, there is almost no deterioration in quality compared to the virgin resin.
[0043] In one embodiment, the recycled bis(2-hydroxyethyl)terephthalate (BHET) has a peak area fraction of 2-hydroxyethyl[2-(2-hydroxyethoxy)ethyl]terephthalate (first diethylene glycol ester) of 2.5% or less as measured by high performance liquid chromatography (HPLC). Specifically, the peak area fraction of 2-hydroxyethyl[2-(2-hydroxyethoxy)ethyl]terephthalate as measured by HPLC may be 2.0% or less, 1.5% or less, 1.0% or less, or 0.5% or less.
[0044] In another embodiment, the recycled bis(2-hydroxyethyl)terephthalate (BHET) has a peak area fraction of bis[2-(2-hydroxyethoxy)ethyl]benzene-1,4-dicarboxylate (second diethylene glycol ester) of 0.5% or less as measured by high performance liquid chromatography (HPLC). Specifically, the HPLC peak area fraction of bis[2-(2-hydroxyethoxy)ethyl]benzene-1,4-dicarboxylate as measured by HPLC may be 0.2% or less, and more specifically, 0.15% or less, 0.1% or less, or 0.05% or less.
[0045] Additionally, the above-mentioned regenerated bis(2-hydroxyethyl)terephthalate may have a peak area fraction of oligomers measured by high-performance liquid chromatography of 3% or less in total.
[0046] Specifically, the bis(2-hydroxyethyl)terephthalate produced by the method may have a peak area fraction of BHET dimer of less than 3%, less than 2%, less than 1%, or less than 0.7% as measured by HPLC. In addition, the bis(2-hydroxyethyl)terephthalate produced by the method may have a peak area fraction of BHET trimer of less than 1%, less than 0.5%, less than 0.3%, less than 0.1%, or 0% as measured by HPLC.
[0047] In addition, the above-mentioned recycled bis(2-hydroxyethyl)terephthalate may further include impurities having a structure similar to bis(2-hydroxyethyl)terephthalate, for example, may include at least one selected from the group consisting of monohydroxyethyl terephthalic acid (MHET), bis(2-hydroxypropyl)terephthalate, and monohydroxyethylethoxyterephthalic acid. Such impurities having a structure similar to bis(2-hydroxyethyl)terephthalate may have an HPLC peak fraction of less than 3%, less than 2%, less than 1%, or less than 0.5%.
[0048] Additionally, the total content of residual solvent (e.g., ethylene glycol) in the regenerated bis(2-hydroxyethyl) terephthalate may be less than 1 wt%, based on the weight ratio detected by gas chromatography analysis. Specifically, the total content of the oligomeric material may be less than 0.5 wt%, less than 0.3 wt%, less than 0.2 wt%, less than 0.1 wt%, or less than 0.9 wt%.
[0049] Additionally, the above-described regenerated bis(2-hydroxyethyl) terephthalate may have a yellowness index (YID) of 3.0 or less, as measured by a colorimeter in a 25 wt% solution state. Specifically, the yellowness index may be 2.5 or less, 2.0 or less, 1.5 or less, or 1.0 or less.
[0050] Additionally, the recycled bis(2-hydroxyethyl)terephthalate may have a total inorganic content of less than 5 ppm as measured by inductively coupled plasma atomic emission spectroscopy (ICP-AES). Specifically, the total inorganic content may be less than 3 ppm, less than 1 ppm, or substantially 0 ppm.
[0051]
[0052] polyester resin
[0053] In this way, the polyester resin of the present invention is a polyester resin that is regenerated through chemical recycling of waste polyester.
[0054] Specifically, since the polyester resin of the present invention is polymerized using recycled BHET, it includes repeating units derived from recycled BHET in the polymer chain.
[0055] The content of recycled BHET in the polyester resin of the present invention may be 1 wt% or more, 5 wt% or more, 10 wt% or more, 30 wt% or more, 50 wt% or more, 70 wt% or more, or 90 wt% or more. In addition, the content of the recycled BHET may be 100 wt% or less, 99 wt% or less, 80 wt% or less, 60 wt% or less, 40 wt% or less, or 20 wt% or less.
[0056] As an example, the recycled bis(2-hydroxyethyl)terephthalate may be included in an amount of 10 wt% to 99 wt% based on the weight of the polyester resin.
[0057] Meanwhile, since bis(2-hydroxyethyl)terephthalate has a structure in which two ethylene glycols and one terephthalic acid are combined, the polyester resin of the present invention may essentially include repeating units derived from ethylene glycol and terephthalic acid.
[0058] As such, the polyester resin of the present invention comprises a diacid component and a glycol component as its constituent monomers. In addition, the polyester resin of the present invention may further comprise additional diacid components and glycol components for polyester polymerization.
[0059] In the polyester resin of the present invention, the diacid component may be a dicarboxylic acid or a derivative thereof, and the glycol component may be a diol.
[0060] In particular, the dicarboxylic acid includes terephthalic acid, and the physical properties of the polyester resin, such as heat resistance, chemical resistance, and weather resistance, can be improved by the terephthalic acid. For example, the terephthalic acid can be included in an amount of 5 mol% to 100 mol% based on the total molar number of the dicarboxylic acid. In addition, the terephthalic acid component can also be formed from a terephthalic acid alkyl ester, for example, dimethylterephthalic acid.
[0061] In addition, the diol includes ethylene glycol, and the ethylene glycol can contribute to improving the transparency and impact strength of the polyester resin. For example, the ethylene glycol can be included in an amount of 5 mol% to 100 mol% based on the total number of moles of the diol.
[0062] According to one embodiment, the polyester resin of the present invention may be a copolymer resin comprising two or more dicarboxylic acid components and / or two or more diol components.
[0063] Specifically, the dicarboxylic acid component may further include an aromatic dicarboxylic acid component other than terephthalic acid, an aliphatic dicarboxylic acid component, or a mixture thereof. Such a dicarboxylic acid component other than terephthalic acid may be included in an amount of 1 wt% to 30 wt% based on the weight of the entire dicarboxylic acid component.
[0064] The above aromatic dicarboxylic acid component may be an aromatic dicarboxylic acid having 8 to 20 carbon atoms, preferably 8 to 14 carbon atoms, or a mixture thereof. Examples of the above aromatic dicarboxylic acid include, but are not limited to, isophthalic acid, naphthalenedicarboxylic acid such as 2,6-naphthalenedicarboxylic acid, diphenyl dicarboxylic acid, 4,4'-stilbenedicarboxylic acid, 2,5-furandicarboxylic acid, 2,5-thiophenedicarboxylic acid, and the like.
[0065] The aliphatic dicarboxylic acid component may be an aliphatic dicarboxylic acid component having 4 to 20 carbon atoms, preferably 4 to 12 carbon atoms, or a mixture thereof. Examples of the aliphatic dicarboxylic acid include, but are not limited to, linear, branched, or cyclic aliphatic dicarboxylic acid components such as cyclohexanedicarboxylic acid, such as 1,4-cyclohexanedicarboxylic acid and 1,3-cyclohexanedicarboxylic acid, phthalic acid, sebacic acid, succinic acid, isodecylsuccinic acid, maleic acid, fumaric acid, adipic acid, glutaric acid, and azelaic acid.
[0066] In addition, the above diol component may further include a comonomer other than ethylene glycol. The comonomer may include, for example, one or more selected from the group consisting of cyclohexanedimethanol, cyclohexanedimethanol derivatives, isosorbide, and diethylene glycol.
[0067] The above cyclohexanedimethanol (e.g., 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol) can contribute to improving the transparency and impact strength of the polyester resin being manufactured. For example, the cyclohexanedimethanol can be included in an amount of 5 mol% to 90 mol% based on the molar number of the total diol. The cyclohexanedimethanol derivative can be 4-(hydroxymethyl)cyclohexylmethyl 4-(hydroxymethyl)cyclohexanecarboxylate, or 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol. The cyclohexanedimethanol derivative can be included in an amount of 0.1 mol% to 25 mol% based on the molar number of the total diol.
[0068] The above isosorbide can improve the processability of the final polyester resin. The transparency and impact strength of the polyester resin are improved by the diol components of the cyclohexanedimethanol and ethylene glycol described above. However, for processability, shear flow characteristics must be improved and the crystallization rate must be delayed. However, it is difficult to achieve these effects with only cyclohexanedimethanol and ethylene glycol. Therefore, when isosorbide is included as a diol component, the processability of the resulting polyester resin can be improved by improving the shear flow characteristics and delaying the crystallization rate while maintaining transparency and impact strength. Preferably, the isosorbide residue may be included in an amount of 0.1 mol% to 50 mol% based on the total molar number of the diol.
[0069] As a specific example, the polyester resin comprises a diacid component and a glycol component, and the diacid component comprises at least one selected from the group consisting of terephthalic acid, isophthalic acid, dimethyl isophthalate, phthalic acid, dimethyl phthalate, phthalic anhydride, 2,6-naphthalenedicarboxylic acid, dimethyl 2,6-naphthalenedicarboxylate, diphenyl dicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, dimethyl 1,4-cyclohexanedicarboxylate, dimethyl 1,3-cyclohexanedicarboxylate, sebacic acid, succinic acid, isodecylsuccinic acid, maleic acid, maleic anhydride, fumaric acid, adipic acid, glutaric acid and azelaic acid, and the glycol component comprises Isosorbide, ethylene glycol, 1,2-propanediol, 1,3-propanediol, 2-methyl-1,3-propanediol, 2-methylene-1,3-propanediol, 2-ethyl-1,3-propanediol, 2-isopropyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 1,4-butanediol, 2,3-butanediol, 3-methyl-1,5-pentanediol, 3-methyl-2,4-pentanediol, 1,6-hexanediol, 1,2-cyclohexanediol, 1,4-cyclohexanediol, diethylene glycol, 4-(hydroxymethyl)cyclohexylmethyl 4-(hydroxymethyl)cyclohexanecarboxylate and It may include at least one selected from the group consisting of 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol.
[0070] The polyester resin according to the present invention can improve the heat resistance, processability, and mechanical properties of a polyester film manufactured therefrom by controlling the content of cyclic trimer and diethylene glycol within a specific range.
[0071] The content of the cyclic trimer in the polyester resin according to the present invention can be measured using liquid chromatography or the like. Specifically, the content of the cyclic trimer can be derived by measuring the fraction (ppm) of the cyclic trimer peak area among the total peak area in a spectrum obtained using high-performance liquid chromatography (HPLC).
[0072] For example, the polyester resin according to the present invention may have a peak area fraction of cyclic trimers measured by high-performance liquid chromatography (HPLC) of 9,000 ppm or less, 7,000 ppm or less, or 5,000 ppm or less.
[0073] According to one embodiment, the polyester resin according to the present invention has a peak area fraction of cyclic trimer as measured by high-performance liquid chromatography (HPLC) of 3,000 ppm or less. Within this range, the processability of the polyester resin and films produced therefrom can be further improved, and heat resistance and mechanical properties can also be excellent.
[0074] For example, the peak area fraction of the cyclic trimer measured by the HPLC may be 3,000 ppm or less, 2,900 ppm or less, 2,800 ppm or less, 2,700 ppm or less, or 2,600 ppm or less. Meanwhile, the lower limit of the peak area fraction of the cyclic trimer is not particularly limited, but may be, for example, 0 ppm or more, 1 ppm or more, 10 ppm or more, 100 ppm or more, or 1,000 ppm or more.
[0075] The above cyclic trimers can be generated during the process of manufacturing polyester resin through a chemical regeneration process from waste polyester, and cause a decrease in the quality of the final product.
[0076] The above cyclic trimer may be a cyclic trimer composed of any one of the repeating units constituting the polyester resin.
[0077] For example, the repeating unit of the cyclic trimer may include an aliphatic alkylene group and an aromatic dicarboxylate group.
[0078] As a specific example, the cyclic trimer may be, for example, an ethylene terephthalate cyclic trimer.
[0079] As a more specific example, the cyclic trimer may include an ethylene terephthalate cyclic trimer.
[0080] These cyclic trimers are easily extracted or precipitated onto the surface during the manufacturing process of polyester resin or film, causing problems in the process or lowering the appearance or performance of the final product. However, if the content is controlled to the level described above, these problems can be resolved.
[0081] In addition, the polyester resin of the present invention may have a concentration of diethylene glycol measured by gas chromatography of, for example, 2.5 wt% or less, 1.5 wt% or less, 1.2 wt% or less, 1.0 wt% or less, 0.9 wt% or less, or 0.8 wt% or less.
[0082] According to one embodiment, the polyester resin has a diethylene glycol (DEG) content of 1.0 wt% or less, as measured by gas chromatography (GC). Within this content range, the melting point of the polyester resin, as well as the heat resistance, mechanical properties, and processability of a film manufactured therefrom, can be improved.
[0083] Meanwhile, the lower limit of the content of the diethylene glycol (DEG) is not particularly limited, but may be, for example, 0 wt% or more, 0.01 wt% or more, 0.1 wt% or more, or 0.3 wt% or more.
[0084] The polyester resin according to the present invention has a carboxyl terminal group (-COOH) concentration controlled within a specific range, so that the hydrolysis resistance of the polyester resin and a film manufactured therefrom can be improved and the heat resistance and mechanical properties can also be excellent.
[0085] For example, the polyester resin may have a carboxyl terminal group concentration (E) calculated by Equation (1) below of 40 eq / ton or less, 30 eq / ton or less, or 20 eq / ton or less when dissolved in benzyl alcohol at 180°C and titrated using a 0.1 N sodium hydroxide-benzyl alcohol solution.
[0086] As a specific example, the polyester resin may have a carboxyl terminal group concentration (E) calculated by Equation (1) below of 20 eq / ton or less when dissolved in benzyl alcohol at 180°C and titrated using a 0.1 N sodium hydroxide-benzyl alcohol solution.
[0087] (1)
[0088] Here, S is the volume (L) of 0.1 N sodium hydroxide-benzyl alcohol solution consumed in the polyester resin titration, B is the volume (L) of 0.1 N sodium hydroxide-benzyl alcohol solution consumed in the blank titration, N is the concentration of the sodium hydroxide-benzyl alcohol solution, which is 0.1 N, W is the weight (kg) of the polyester resin used in the titration, and f is a factor of the 0.1 N sodium hydroxide-benzyl alcohol solution, which is 0.95 to 0.99.
[0089] Specifically, the carboxyl terminal group concentration may be 20 eq / ton or less, 19 eq / ton or less, 18 eq / ton or less, 16 eq / ton or less, or 15 eq / ton or less. Meanwhile, the lower limit of the carboxyl terminal group concentration is not particularly limited, but may be, for example, 0 eq / ton or more, 1 eq / ton or more, 3 eq / ton or more, 5 eq / ton or more, or 10 eq / ton or more.
[0090] In addition, the melting point (Tm) of the polyester resin of the present invention measured by a differential scanning calorimeter (DSC) may be, for example, 240°C or higher, 245°C or higher, 250°C or higher, or 255°C or higher, and may also be 270°C or lower, 265°C or lower, or 260°C or lower. As a specific example, the melting point of the polyester resin measured by a differential scanning calorimeter (DSC) may be 255°C or higher. The melting point may be measured by a method including, for example, a step of placing the polyester resin in a differential scanning calorimeter (DSC) and heating it from room temperature to 280°C at a constant rate.
[0091] The polyester resin according to the present invention may have an intrinsic viscosity (IV) of 0.5 dl / g or more, 0.6 dl / g or more, or 0.7 dl / g or more at 35°C, and may also have an IV of 1.2 dl / g or less, 1.1 dl / g or less, 1.0 dl / g or less, or 0.9 dl / g or less. For example, the polyester resin may have an intrinsic viscosity of 0.6 dl / g to 1.2 dl / g at 35°C. The intrinsic viscosity can be calculated, for example, by obtaining a specific viscosity using an Ubbelohde viscosity tube or the like after dissolving the polyester resin in a solvent such as orthochlorophenol.
[0092]
[0093] polyester film
[0094] The present invention provides a polyester film comprising the polyester resin described above.
[0095] That is, the polyester film of the present invention is obtained from a polyester resin containing recycled bis(2-hydroxyethyl)terephthalate obtained by depolymerization of waste polyester, having a peak area fraction of cyclic trimer measured by high-performance liquid chromatography (HPLC) of 3,000 ppm or less, and having a content of diethylene glycol (DEG) measured by gas chromatography (GC) of 1.0 wt% or less.
[0096] The polyester film of the present invention is manufactured from the polyester resin described above, and therefore has excellent processability, mechanical strength, hydrolysis resistance, and heat resistance.
[0097] As an example, in the process of melt extrusion to manufacture a film from the polyester resin, the pressure applied to the 10 ㎛ filter is 100 kg / cm 2 Below 90 kg / cm 2 Below 80 kg / cm 2 Below 70 kg / cm 2 Less than or equal to 60 kg / cm 2 It may be as follows. In addition, in the process of stretching the polyester film, the number of times the film breaks may occur on average less than 1 time per 24 hours, and specifically may be 0 times.
[0098] The tensile strength of the longitudinal direction (MD) of the above polyester film is, for example, 10 kgf / mm 2 Above, 13 kgf / mm 2 Above, 14 kgf / mm 2 Above, 15 kgf / mm 2 Above, 17 kgf / mm 2 or more than 19 kgf / mm 2 It can be ideal. Also, the tensile strength in the longitudinal direction (MD) is, for example, 40 kgf / mm. 2 Below 30 kgf / mm 2 Below 25 kgf / mm 2 Less than or equal to 20 kgf / mm 2 It could be as follows:
[0099] The tensile strength of the above polyester film in the transverse direction (MD) is, for example, 20 kgf / mm 2 Above, 22 kgf / mm 2 Above, 23 kgf / mm 2 Above, 24 kgf / mm 2 or more than 25 kgf / mm 2 It can be ideal. In addition, the tensile strength in the transverse direction (MD) is, for example, 80 kgf / mm 2 Below 70 kgf / mm 2 Less than or equal to 60 kgf / mm 2 It could be as follows:
[0100] The above polyester film may have an elongation in the machine direction (MD) of, for example, 100% or more, 115% or more, 120% or more, 125% or more, 130% or more, or 135% or more. In addition, the above polyester film may have an elongation in the machine direction (MD) of, for example, 180% or less, 170% or less, 160% or less, or 150% or less.
[0101] The polyester film may have an elongation in the transverse direction (MD) of, for example, 60% or more, 70% or more, 75% or more, or 80% or more. In addition, the polyester film may have an elongation in the transverse direction (MD) of, for example, 120% or less, 110% or less, or 100% or less.
[0102] The above tensile strength and elongation can be measured, for example, by cutting the sample to a width of 1.5 cm and mounting it on clips spaced at 5 cm intervals in the length direction, and then measuring it at a tensile speed of 200 mm / min at 25°C according to ASTM D882.
[0103] As a specific example, the polyester film is cut into 1.5 cm widths and mounted on clips spaced 5 cm apart in the longitudinal direction. When measured at 25°C under a tensile speed condition of 200 mm / min according to ASTM D882, the tensile strength in the longitudinal direction (MD) is 15 kgf / mm. 2And, the longitudinal (MD) elongation can be 125% or more.
[0104] In addition, the polyester film may have an elongation retention rate (R) calculated from the following equation (2) of 30% or more, 35% or more, 40% or more, 45% or more, or 50% or more.
[0105] As a specific example, the polyester film may have an elongation retention rate (R) calculated from the following equation (2) of 40% or more.
[0106] (2)
[0107] Here, S0 is the initial elongation (%) of the polyester film sample, and S1 is the elongation (%) measured after leaving it for 96 hours under the conditions of 121℃, 100% RH, and 2 atm. The elongation is measured at a tensile speed of 200 mm / min according to ASTM D882 at 25℃ after cutting the polyester film into 1.5 cm widths and mounting it on clips spaced 5 cm apart in the length direction.
[0108] Meanwhile, the upper limit of the above-mentioned elasticity retention rate (R) is not particularly limited, but may be, for example, 100% or less, 80% or less, 70% or less, or 60% or less.
[0109] According to one embodiment, a method for producing a polyester film of the present invention comprises the steps of: (1) depolymerizing waste polyester to produce recycled bis(2-hydroxyethyl)terephthalate; (2) mixing the recycled bis(2-hydroxyethyl)terephthalate with a solvent to obtain a recycled bis(2-hydroxyethyl)terephthalate solution; (3) producing a polyester resin by a polycondensation reaction using the recycled bis(2-hydroxyethyl)terephthalate solution; and (4) melt-extruding and stretching the polyester resin, wherein the polyester resin has a peak area fraction of a cyclic trimer of 3,000 ppm or less as measured by high-performance liquid chromatography (HPLC) and a content of diethylene glycol (DEG) of 1 wt% or less as measured by gas chromatography (GC).
[0110] The polycondensation reaction of the above step (3) may include, for example, at least one of (3a) a polycondensation reaction under a pressure of 200 mmHg to 600 mmHg (first polycondensation reaction) and (3b) a polycondensation reaction under a pressure of less than 200 mmHg (second polycondensation reaction).
[0111] As a specific example, the polycondensation reaction of step (3) may include a step of (3a) subjecting the regenerated bis(2-hydroxyethyl)terephthalate solution to a first polycondensation reaction under a pressure of 200 mmHg to 600 mmHg to produce an oligomer. In addition, the polycondensation reaction may further include, after step (3a), a step of (3b) subjecting the oligomer to a second polycondensation reaction under a pressure of less than 200 mmHg to produce a polyester resin.
[0112] A method for producing a polyester resin according to one specific example comprises the steps of: (1) depolymerizing waste polyester to produce recycled bis(2-hydroxyethyl)terephthalate; (2) mixing the recycled bis(2-hydroxyethyl)terephthalate with a solvent to obtain a recycled bis(2-hydroxyethyl)terephthalate solution; (3a) subjecting the recycled bis(2-hydroxyethyl)terephthalate solution to a first polycondensation reaction under a pressure of 200 mmHg to 600 mmHg to produce an oligomer; And (3b) a step of producing a polyester resin by subjecting the oligomer to a second polycondensation reaction under a pressure of less than 200 mmHg, wherein the polyester resin has a peak area fraction of a cyclic trimer measured by high-performance liquid chromatography (HPLC) of 3,000 ppm or less, and a content of diethylene glycol (DEG) measured by gas chromatography (GC) of 1 wt% or less.
[0113] In the manufacturing process of polyester resin, a certain amount of oligomers such as cyclic trimers always exist in equilibrium concentration with the polymer, so it is difficult to control and reduce their content. However, a method for manufacturing a recycled polyester resin according to a preferred embodiment uses recycled bis(2-hydroxyethyl) terephthalate as a main monomer (e.g., 100% monomer), does not perform a transesterification reaction, and performs the polycondensation reaction by dividing it into the first low vacuum and the second high vacuum, thereby reducing the cyclic trimer content to a significantly lower level than before.
[0114] Hereinafter, the method for manufacturing a polyester resin and film according to the present invention will be described in detail step by step.
[0115]
[0116] Preparation of waste polyester
[0117] The waste polyester used as a raw material in the present invention can be obtained from a product made of polyester material discarded after use.
[0118] For example, the above-mentioned waste polyester can be obtained from various products such as beverage bottles, fabrics, films, cases, boxes, partitions, shelves, protective panels, packaging, building materials, and interior and exterior materials made of polyester materials that are discarded after use by consumers.
[0119] The above waste polyester material may be pretreated before being fed into the depolymerization step.
[0120] First, other plastics, metals, and other foreign substances mixed in the polyester material waste are removed and washed, and then sorted according to detailed characteristics such as color as needed.
[0121] The selected waste polyester material is fed into a shredder and crushed into small flakes. The resulting waste polyester flakes can be screened to a desired particle size using a mesh. The mesh size may be, for example, 4 mm or less, 3 mm or less, or 2 mm or less.
[0122] The selected flakes are washed and dried by hot air or the like, and can then be put into the depolymerization step.
[0123] Meanwhile, the waste polyester used in the glycolysis reaction may have a controlled particle size. For example, the waste polyester may be pulverized into flake form through a pretreatment process as described above.
[0124] Specifically, the particle size of the waste polyester may be 4 mm or less, 3 mm or less, 2 mm or less, or 1 mm or less. Within the particle size range, a glycolysis reaction under relatively low temperature conditions is possible, for example, the temperature condition of the first glycolysis reaction may be adjusted to 195°C or less, 190°C or less, 185°C or less, or 180°C, and the temperature condition of the subsequent second glycolysis reaction may be adjusted to 160°C or less, or 150°C or less. In addition, a glycolysis reaction over a relatively short period of time is possible within the particle size range, for example, the progress time of the first and second glycolysis reactions may be set to 3 hours or less, 2 hours or less, or 1 hour or less from the time when the appropriate temperature is reached.
[0125] In addition, the waste polyester may have a fine structure, such as a fiber. For example, the waste polyester may be a waste fiber or a fibrous material, such as a waste banner. As a specific example, the waste polyester may have a fine particle or fibrous form with a particle diameter of 4 mm or less. The fiber may include at least one of a monofilament yarn and a multifilament yarn. The diameter of the monofilament yarn may be, for example, 0.05 denier to 100 denier, and may correspond to approximately 0.001 mm to 0.1 mm. Specifically, the diameter of the monofilament yarn may be 0.05 denier to 7 denier, or 7 denier to 100 denier. The diameter of the multifilament yarn may be, for example, 1 denier to 10,000 denier, and may correspond to approximately 0.01 mm to 1 mm. Specifically, the diameter of the multifilament yarn may be 0.01 denier to 0.2 denier, or 0.2 denier to 1 denier.
[0126] In this way, when depolymerization is performed by adjusting the particle size or diameter of waste polyester to a certain range or less, solvation can be promoted even under relatively low temperature and short reaction time conditions.
[0127] In particular, according to the present invention, a two-step glycolysis reaction (i.e., a first glycolysis reaction and a second glycolysis reaction) is performed, and if solvation is promoted in the first glycolysis reaction, an ester exchange reaction of waste polyester can be performed under lower temperature and shorter reaction time conditions in the second glycolysis reaction, so that the concentration of diethylene glycol (DEG) naturally generated at a general glycolysis reaction temperature can be significantly reduced, and the content of diethylene glycol ester compound (DEG ester) in the final bis(2-hydroxyethyl) terephthalate can also be significantly reduced.
[0128] The diethylene glycol ester compound present in bis(2-hydroxyethyl) terephthalate acts as a factor that breaks the regularity of the final polymer during the polymerization process of polyester and polyester copolymer, thereby acting as a key factor that reduces the heat resistance properties of the final polymer, such as the melting point (Tm) and glass transition temperature (Tg).
[0129] However, the polyester resin and product manufactured using the bis(2-hydroxyethyl)terephthalate obtained according to the depolymerization process of the present invention can be polymerized into a polymer without unnecessary structural defects, as in the case of using the initial non-renewable raw material.
[0130]
[0131] Preparation of recycled bis(2-hydroxyethyl)terephthalate
[0132] First, waste polyester is depolymerized to produce recycled bis(2-hydroxyethyl)terephthalate.
[0133] According to one embodiment, the recycled bis(2-hydroxyethyl)terephthalate can be produced by the steps of (1a) depolymerizing waste polyester by a first glycolysis reaction at a temperature of 180°C to 200°C to obtain a first reactant; (1b) depolymerizing the first reactant by a second glycolysis reaction at a temperature of 150°C to 170°C to obtain a second reactant; (1c) ion-exchanging the second reactant through an ion exchange resin to obtain a third reactant; (1d) removing unreacted glycol from the third reactant by distillation at a temperature of 150°C or lower to obtain a fourth reactant; and (1e) obtaining crude bis(2-hydroxyethyl)terephthalate by distillation from the fourth reactant.
[0134] According to the above embodiment, by applying a multi-stage depolymerization reaction at low temperature after going through a crushing pretreatment process of waste polyester, the content of glycol dimer (diethylene glycol) generated during the depolymerization reaction can be significantly reduced, thereby increasing the purity of the bis(2-hydroxyethyl) terephthalate finally obtained and minimizing side reaction structures in future repolymerization into polyester.
[0135] According to one embodiment, the depolymerization includes a step of depolymerizing waste polyester through a first glycolysis reaction at a high temperature (180 to 200°C) to obtain a first reactant; and a step of depolymerizing the first reactant through a second glycolysis reaction at a low temperature (150 to 170°C) to obtain a second reactant.
[0136] The above glycolysis reaction, as is well known, refers to a chemical reaction in which a polymer chain or the like is decomposed by glycol. The glycol may include, for example, one or more selected from the group consisting of ethylene glycol, propylene glycol, and diethylene glycol.
[0137] A catalyst may be used in the above glycolysis reaction. The catalyst may be a metal catalyst, such as a metal salt catalyst or a metallic organic catalyst. Specifically, the catalyst may be a metal acetate, carbonate, oxide, hydroxide, etc., and the metal may be an alkali metal, alkaline earth metal, transition metal, etc.
[0138] As a specific example, the catalyst may include a metal acetate, an anhydride or a hydrate thereof, and more specifically, may be at least one selected from the group consisting of zinc acetate, sodium acetate, cobalt acetate and manganese acetate, or may be in the form of a hydrate or anhydride thereof.
[0139] The total weight of the glycol added may be 1 to 7 times, 2 to 5 times, or 3 to 4 times the weight of the waste polyester resin, and may also be 7 to 5 times, or 4 to 4 times the weight of the waste polyester resin. For example, the weight of the glycol added may be 1 to 7 times the weight of the waste polyester resin, specifically 2 to 5 times, and more specifically 3 to 4 times.
[0140] In addition, the input weight of the catalyst may be 0.01 part by weight or more, 0.1 part by weight or more, 0.2 part by weight or more, or 0.3 part by weight or more, and may also be 5 parts by weight or less, 1 part by weight or less, 0.7 part by weight or less, 0.5 part by weight or less, or 0.4 part by weight or less, relative to 100 parts by weight of the waste polyester resin. For example, the input weight of the catalyst may be 0.1 part by weight to 1 part by weight, and specifically, 0.2 part by weight to 0.7 part by weight. More specifically, the catalyst may be used in an amount of 0.2 part by weight to 0.4 part by weight relative to 100 parts by weight of the waste polyester.
[0141] The temperature during the first glycolysis reaction may be 170°C or higher, 180°C or higher, 190°C or higher, and may also be 205°C or lower, 200°C or lower, 195°C or lower, or 190°C or lower. For example, the temperature during the first glycolysis reaction may be 180°C to 200°C, specifically 180°C to 195°C, and more specifically 180°C to 190°C.
[0142] In addition, the temperature during the second glycolysis reaction may be 140°C or higher, 150°C or higher, 160°C or higher, and may also be 170°C or lower, 160°C or lower. For example, the temperature during the second glycolysis reaction may be 150°C to 170°C, specifically 150°C to 160°C, and more specifically 150°C to 155°C.
[0143] The time required for the first and second glycolysis reactions may be 1 hour or more or 2 hours or more from the time the appropriate temperature is reached, and may also be 4 hours or less or 3 hours or less. For example, the time required for the first and second glycolysis reactions may be 1 hour to 4 hours, specifically 1 hour to 3 hours, and more specifically 1 hour to 2 hours from the time the appropriate temperature is reached.
[0144] As a specific example, the first glycolysis reaction may be performed at a temperature of 180°C to 190°C for 1 to 3 hours. Additionally, the second glycolysis reaction may be performed at a temperature of 150°C to 160°C for 1 to 3 hours.
[0145] As an example, the first glycolysis reaction may be performed under a zinc acetate anhydride catalyst. As a specific example, the first glycolysis reaction may be performed under a zinc acetate anhydride catalyst at a temperature of 180°C to 200°C for 1 to 3 hours. The zinc acetate anhydride may be used in an amount of 0.2 to 0.4 parts by weight based on 100 parts by weight of the waste polyester. In addition, the second glycolysis reaction may be performed at a temperature of 140°C to 160°C for 1 to 3 hours after additional addition of ethylene glycol without additional addition of a catalyst.
[0146] The second reactant obtained through the above depolymerization can then be cooled and used in the next step.
[0147] The cooling temperature may be, for example, 150°C or less, 140°C or less, 130°C or less, 120°C or less, 110°C or less, 100°C or less, and may also be 50°C or more, 60°C or more, 70°C or more, 80°C or more, or 90°C or more.
[0148] As an example, the cooling may be performed through a reduced pressure flash process. Specifically, the temperature of the second reactant may be lowered by applying a vacuum through the reduced pressure flash process to evaporate the ethylene glycol.
[0149] For example, the second reactant may additionally undergo a pressure-reducing flash cooling step to a temperature of 120°C or lower prior to the subsequent step. More specifically, the temperature of the second reactant may be lowered to 110°C or lower, or 100°C or lower, by the pressure-reducing flash process.
[0150] The pressure conditions of the above-described reduced pressure flash process may be, for example, 200 Torr or less, 100 Torr or less, or 50 Torr or less, and specifically, 10 Torr to 200 Torr, 10 Torr to 100 Torr, or 10 Torr to 50 Torr.
[0151] Thereafter, insoluble foreign substances can be removed from the cooled second reactant through filtration. As a specific example, a step of cooling the second reactant to 120°C or lower and filtering it using a filter aid may be additionally included prior to the ion exchange in step (1c). As a result, fine particles and insoluble organic substances present in the second reactant can be filtered out through solid-liquid separation.
[0152] The filter aid may be a known component such as diatomaceous earth, perlite, asbestos powder, etc., and for example, 0.1 to 2.0 parts by weight of the filter aid may be added relative to 100 parts by weight of the second reactant.
[0153] Since bis(2-hydroxyethyl) terephthalate (BHET) or oligomers obtained through a depolymerization reaction exist in a solid form at room temperature, it is difficult to separate foreign substances at room temperature. Therefore, it is recommended to separate them under temperature conditions of 90°C to 150°C, more specifically, 110°C to 150°C. In addition, if the above temperature range is maintained, the fluidity is good, making it easy to remove insoluble foreign substances.
[0154] Removal of insoluble foreign substances through solid-liquid separation can be accomplished using various methods and devices. For example, equipment such as pressure filters, centrifuges, filter presses, and belt presses can be used. However, the method is not limited to these as long as it can separate foreign substances.
[0155] The second reactant, which has been previously depolymerized, cooled and filtered, is ion-exchanged through an ion exchange resin to obtain a third reactant.
[0156] By performing the above ion exchange, ionic impurities, specifically catalysts and metal foreign substances, present in the second reactant can be removed.
[0157] As is well known, an ion-exchange resin refers to a resin or polymer that acts as a medium for ion exchange. The ion-exchange resin may include a cation exchange resin, an anion exchange resin, an amphoteric ion exchange resin, a chelating resin, etc.
[0158] The cation exchange resin may include a strongly acidic cation exchange resin having a sulfonic acid group (-SO3H) and a weakly acidic cation exchange resin having a carboxyl group (-COOH), and the anion exchange resin may include a strongly basic anion exchange resin in the form of a quaternary ammonium salt and a weakly basic anion exchange resin having a primary to tertiary amino group.
[0159] As a specific example, the ion exchange resin may include at least one selected from the group consisting of a strongly acidic cation exchange resin, a weakly acidic cation exchange resin, and a chelating resin.
[0160] According to one embodiment, the ion exchange is performed by introducing an ion exchange resin into the first reactant.
[0161] The weight of the ion exchange resin added may be 1 to 20 times, 3 to 15 times, 10 to 15 times, or 8 to 10 times the weight of the catalyst added in the depolymerization reaction, and may also be 10 to 15 times, 10 to 15 times, or 10 to 15 times the weight of the catalyst added in the depolymerization reaction. For example, the weight of the ion exchange resin added may be 1 to 20 times, specifically 3 to 15 times, and more specifically 5 to 8 times the weight of the catalyst added in the depolymerization reaction.
[0162] In addition, the weight of the ion exchange resin may be 1 part by weight or more, 3 parts by weight or more, or 5 parts by weight or more, and may also be 50 parts by weight or less, 20 parts by weight or less, 15 parts by weight or less, 10 parts by weight or less, or 7 parts by weight or less, relative to 100 parts by weight of the waste polyester introduced in the previous depolymerization reaction.
[0163] As a specific example, the ion exchange resin may be used in an amount of 1 to 20 parts by weight based on 100 parts by weight of the waste polyester.
[0164] According to another embodiment, the ion exchange is performed using a column comprising an ion exchange resin.
[0165] Specifically, the column may be filled with particles of an ion exchange resin, and ion exchange may be performed as the second reactant passes through the column.
[0166] The particle size of the ion exchange resin particles may be, for example, 0.3 mm to 1.5 mm, and more specifically, 0.6 mm to 0.9 mm.
[0167] The temperature during the above ion exchange may be, for example, 140°C or less, 130°C or less, 120°C or less, 110°C or less, 100°C or less, and may also be 50°C or more, 60°C or more, 70°C or more, 80°C or more, or 90°C or more.
[0168] The unreacted glycol is removed from the third reactant through distillation to obtain the fourth reactant.
[0169] Since unreacted glycol still remains in the depolymerized product filtered through the previous step, it is necessary to remove it from the reactant before the subsequent step.
[0170] Additionally, for an economical depolymerization process, it is necessary to perform a process for recovering unreacted glycols. That is, among the glycols previously introduced into the depolymerization process, such as ethylene glycol, propylene glycol, and diethylene glycol, it is possible to recover the remaining glycols that are not involved in the glycolysis reaction and reuse them in the glycolysis reaction.
[0171] Distillation to remove the unreacted glycol can be performed, for example, by vacuum distillation, and a glass distillation apparatus or a rotary evaporator can be used for this purpose.
[0172] The reduced pressure distillation for removing the unreacted glycol can be performed at a temperature of 150°C or lower, thereby further reducing the generation of diethylene glycol and impurities derived therefrom, thereby improving the purity of BHET. For example, the reduced pressure distillation for removing the unreacted glycol can be performed at 150°C or lower, 130°C or lower, or 120°C or lower, and can also be performed at 80°C or higher, 90°C or higher, 100°C or higher, or 110°C or higher. Specifically, the temperature during the distillation for removing the unreacted glycol can be 80°C to 190°C, or 90°C to 150°C. As a more specific example, the distillation for removing the unreacted glycol can be performed at a temperature of 100°C to 130°C.
[0173] The pressure during the reduced pressure distillation for removing the unreacted glycol may be, for example, 0.1 Torr to 200 Torr, and more specifically, 0.5 Torr to 30 Torr.
[0174] Crude bis(2-hydroxyethyl)terephthalate is obtained through distillation from the fourth reactant from which the unreacted glycol has been removed.
[0175] Various methods can be used for the above distillation, but a distillation method that increases the surface area in contact with the heat source by making the mixture to be separated into a thin film can be used.
[0176] For example, the distillation may be performed by thin film evaporation, falling film evaporation, or short path evaporation, and for this purpose, a thin film distiller, a falling film distiller, and a short path distiller may be used, respectively.
[0177] As a specific example, the distillation for obtaining the above bis(2-hydroxyethyl)terephthalate can be performed by thin-film distillation. Specifically, a mixture introduced into the evaporator of the thin-film distiller forms a thin film on the inner wall of the thin-film distiller by a wiper rotor, and distillation is then performed under appropriate temperature conditions by heating. In addition, a condenser may be provided inside the thin-film distiller for recovering the evaporated substance.
[0178] The above-described thin-film distillation can be performed using short-path evaporation. This short-path thin-film distillation method, with its short residence time and the ability to perform reduced-pressure distillation using high vacuum, minimizes heat-induced changes in reactants while allowing the separation of high-boiling-point or high-molecular-weight substances that are difficult to separate using other distillation methods. Furthermore, lowering the pressure within the thin-film distillation chamber lowers the vapor pressure of the substance, allowing evaporation to occur at a temperature lower than its original boiling point.
[0179] As a specific example, the fourth reactant is introduced into a short-path thin-film distiller, and a wiper that forms a thin film rotates at 300 rpm or more, so that vaporized substances and non-vaporized substances can be separated and obtained.
[0180] The internal film temperature of the upper film distillation device during the above film distillation may be, for example, 100°C or higher, 110°C or higher, 120°C or higher, or 125°C or higher, and may also be 250°C or lower, 200°C or lower, 150°C or lower, or 135°C or lower, and specifically, may be 150°C to 250°C, 190°C to 250°C, or 180°C to 220°C.
[0181] In addition, the internal pressure of the upper thin film distillation device during the thin film distillation may be, for example, 0.005 Torr to 5.0 Torr, specifically 0.05 Torr to 5.0 Torr, 0.05 Torr to 1.5 Torr, or 0.05 Torr to 1 Torr. More specifically, the distillation for obtaining the crude bis(2-hydroxyethyl)terephthalate may be performed by thin film distillation under a pressure of 0.05 Torr to 0.4 Torr.
[0182] The above-mentioned bis(2-hydroxyethyl)terephthalate can then be provided as high-purity, high-quality bis(2-hydroxyethyl)terephthalate through an adsorption-crystallization process.
[0183] For example, the above adsorption-crystallization can be performed by adding an adsorbent, filtration, and crystallization using water as a solvent.
[0184] Although various solvents can be used for the above adsorption-crystallization, a solvent that can dissolve bis(2-hydroxyethyl)terephthalate well is preferably used. As a specific example, to obtain the final reactant, water is added as a solvent to crude bis(2-hydroxyethyl)terephthalate, heated to dissolve, an adsorbent is added, filtering is performed, and cooling-crystallization is performed from the obtained solution, and finally filtering is performed to obtain high-purity bis(2-hydroxyethyl)terephthalate.
[0185] The water to be added may be added in an amount of 100 to 500 parts by weight, specifically 200 to 400 parts by weight, and more specifically 300 to 350 parts by weight, based on 100 parts by weight of crude bis(2-hydroxyethyl)terephthalate.
[0186] Additionally, the melting temperature may be 50°C to 95°C, specifically 60°C to 85°C, and more specifically 70°C to 75°C.
[0187] The above-mentioned adsorbent can serve to adsorb and remove other foreign substances, and can be added in an amount of 0.1 to 3 parts by weight relative to 100 parts by weight of the above-mentioned bis(2-hydroxyethyl)terephthalate. The type and form of the adsorbent are not particularly limited, and for example, activated carbon can be used.
[0188] The bis(2-hydroxyethyl) terephthalate, i.e., regenerated BHET, finally obtained through the above steps has high purity, and the content of organic impurities, especially diethylene glycol and by-products derived therefrom (such as DEG ester) or other oligomers and inorganic substances, is below a certain level, and has excellent color quality.
[0189]
[0190] Preparation of a regenerated bis(2-hydroxyethyl)terephthalate solution
[0191] A solution of recycled bis(2-hydroxyethyl)terephthalate is prepared by mixing the previously manufactured recycled bis(2-hydroxyethyl)terephthalate with a solvent.
[0192] Examples of solvents used for preparing the above-described regenerated BHET solution include water, ethylene glycol, methanol, ethanol, and the like. As a specific example, the solvent may include at least one of water and ethylene glycol. As a more specific example, the solvent may simultaneously include water and ethylene glycol, in which case the weight ratio of water to ethylene glycol may be 1:5 or 1:2.
[0193] The temperature (dissolution temperature) at which the above-mentioned BHET is mixed with a solvent may be, for example, 60°C or higher, 65°C or higher, 70°C or higher, or 75°C or higher, and may also be 197°C or lower, 180°C or lower, 165°C or lower, 140°C or lower, 120°C or lower, 100°C or lower, 90°C or lower, or 80°C or lower.
[0194] According to one embodiment, the temperature when the regenerated BHET is mixed with water may be 60°C to 100°C. According to another embodiment, the temperature when the regenerated BHET is mixed with ethylene glycol may be 60°C to 197°C. According to yet another embodiment, the temperature when the regenerated BHET is mixed with a mixed solvent of water and ethylene glycol may be 60°C to 197°C. It is more advantageous in that the regenerated BHET is sufficiently dissolved within the above preferred temperature range, while preventing the problem of the purity being lowered due to the generation of diethylene glycol ester due to thermal decomposition at high temperatures.
[0195] The concentration of the above-mentioned regenerated BHET solution may be, for example, 25 wt% or more, 35 wt% or more, 50 wt% or more, 65 wt% or more, or 75 wt% or more, and may also be 99 wt% or less, 95 wt% or less, 90 wt% or less, 85 wt% or less, or 80 wt% or less. As a specific example, the concentration of the above-mentioned regenerated BHET solution may be 25 wt% to 99 wt%, and more specifically, 50 wt% to 95 wt%. When it is within the above-mentioned preferred range, it may be more advantageous in inducing a uniform polymerization reaction while improving the reaction efficiency. The concentration of the above-mentioned regenerated BHET solution may be calculated as a percentage of the weight of the regenerated BHET relative to the total weight of the solution (i.e., the total combined weight of the regenerated BHET and the solvent).
[0196]
[0197] Manufacturing of polyester resin
[0198] Polyester resin is polymerized using the previously prepared recycled bis(2-hydroxyethyl)terephthalate solution.
[0199] In the present invention, the polymerization of the polyester resin includes a step of producing a low molecular weight oligomer by performing a polycondensation reaction (first polycondensation reaction) under low vacuum; and a step of producing a polyester resin by performing a polycondensation reaction (second polycondensation reaction) on the oligomer under high vacuum.
[0200] The above first polycondensation reaction and the above second polycondensation reaction can be carried out by applying reduced pressure conditions to remove the solvent contained in the regenerated bis(2-hydroxyethyl) terephthalate solution and the by-products of the polycondensation reaction (glycol, etc.) by discharging them to the outside of the system.
[0201] The pressure during the first polycondensation reaction may be, for example, 700 mmHg or less, 600 mmHg or less, 500 mmHg or less, 400 mmHg or less, 350 mmHg or less, 300 mmHg or less, or 250 mmHg or less, and may also be 160 mmHg or more, 180 mmHg or more, 200 mmHg or more, 220 mmHg or more, or 240 mmHg or more. According to one embodiment, the pressure during the first polycondensation reaction is 200 mmHg to 600 mmHg, and when it is within the preferred range, it may be more advantageous to sufficiently remove by-products of the low-vacuum polycondensation reaction while maintaining the degree of vacuum during the polycondensation reaction.
[0202] In addition, the temperature during the first polycondensation reaction may be, for example, 100°C or higher, 130°C or higher, 160°C or higher, 180°C or higher, or 200°C or higher, and may also be 300°C or lower, 280°C or lower, 250°C or lower, or 230°C or lower. As a specific example, the first polycondensation reaction may be performed at a temperature of 180°C to 250°C and a pressure of 200 mmHg to 400 mmHg.
[0203] In addition, the first polycondensation reaction may be performed until the number average molecular weight of the low molecular weight oligomer reaches an appropriate level. The time required for the first polycondensation reaction is not particularly limited, but may be, for example, 30 minutes or more, 1 hour or more, 2 hours or more, or 3 hours or more, and may also be 15 hours or less, 10 hours or less, 5 hours or less, or 4 hours or less, and specifically, may be 1 hour to 5 hours.
[0204] The pressure during the second polycondensation reaction may be, for example, less than 200 mmHg, less than 150 mmHg, less than 100 mmHg, less than 50 mmHg, less than 10 mmHg, or less than 1 mmHg, and may also be 0.001 mmHg or more, 0.01 mmHg or more, 0.1 mmHg or more, or 0.5 mmHg or more. According to one embodiment, the pressure during the second polycondensation reaction is less than 200 mmHg, and when it is within the preferred range, it may be more advantageous to sufficiently remove by-products of the polycondensation reaction while maintaining the degree of vacuum during the polycondensation reaction.
[0205] In addition, the temperature during the second polycondensation reaction may be, for example, 230°C or higher, 240°C or higher, 250°C or higher, or 260°C or higher, and may also be 300°C or lower, 290°C or lower, 280°C or lower, or 270°C or lower. As a specific example, the second polycondensation reaction may be performed at a temperature of 250°C to 300°C and a pressure of 0.01 mmHg to 150 mmHg. Within the above preferred range, the vacuum degree during the polycondensation reaction is maintained while sufficiently removing byproducts of the polycondensation reaction, which may be more advantageous in suppressing yellowing of the final resin.
[0206] In addition, the second polycondensation reaction may be performed until the number average molecular weight of the polyester resin reaches an appropriate level. The time required for the second polycondensation reaction is not particularly limited, but may be, for example, 30 minutes or more, 1 hour or more, 2 hours or more, or 5 hours or more, and may also be 60 hours or less, 48 hours or less, 24 hours or less, or 15 hours or less, and specifically, may be 1 hour to 24 hours.
[0207] The method for producing a polyester resin of the present invention may additionally include a process commonly employed in this field in addition to the process described above.
[0208] As an example, the method for producing the polyester resin may additionally include a process of forming pellets by molding the polyester resin after the polycondensation reaction.
[0209] As another example, the method for producing the polyester resin may further include a step of solid-state polymerizing the polyester resin after the condensation polymerization reaction. The temperature during the solid-state polymerization may be, for example, 180°C or higher, 190°C or higher, 200°C or higher, or 205°C or higher, and may also be 260°C or lower, 240°C or lower, 220°C or lower, or 215°C or lower. As a specific example, the solid-state polymerization may be performed at a temperature of 200°C to 220°C. In addition, the pressure during the solid-state polymerization may be, for example, 10.0 torr or lower, 5.0 torr or lower, 2.0 torr or lower, or 1.0 torr or lower, and may be 0.01 torr or higher, 0.1 torr or higher, 0.2 torr or higher, or 0.5 torr or higher, and specifically, may be 0.2 torr to 2.0 torr. Additionally, the above solid-state polymerization can be performed in an atmosphere of an inert gas such as nitrogen.
[0210] The polyester resin according to the present invention can be manufactured as a copolymerized polyester resin by further adding an additional diacid component in addition to the regenerated bis(2-hydroxyethyl)terephthalate. The additional diacid component may be a dicarboxylic acid or a derivative thereof, and the dicarboxylic acid may include at least one selected from terephthalic acid and isophthalic acid. For example, the dicarboxylic acid or a derivative thereof may be additionally added during the first polycondensation reaction.
[0211] In addition, the polycondensation reaction may be carried out in the presence of a polycondensation catalyst, and the polycondensation catalyst may be selected from the group consisting of a titanium-based compound, a germanium-based compound, an antimony-based compound, and an aluminum-based compound. The amount of the polycondensation catalyst used is preferably 0.1 ppm to 500 ppm based on the amount of metal elements relative to the weight of the final polyester resin, but since the amount used affects the color of the final polyester resin, the amount used may vary depending on the desired color and the stabilizer and coloring agent used.
[0212] In addition to the above-mentioned polycondensation catalyst, stabilizers, coloring agents, crystallizers, antioxidants, branching agents, etc. may be further used, and the timing of adding these additives is not particularly limited and may be added at any time during the manufacturing stage of the polyester resin.
[0213] As the above stabilizer, phosphorus compounds such as phosphoric acid, trimethyl phosphate, triethyl phosphate, and triethylphosphonoacetate can be generally used, and the amount added can be 10 to 200 ppm based on the amount of phosphorus element relative to the weight of the polyester resin. In addition, as a coloring agent added to improve the color of the polyester resin, typical coloring agents such as cobalt acetate and cobalt propionate can be exemplified, and the amount added can be 10 to 200 ppm based on the amount of cobalt element relative to the weight of the polyester resin. If necessary, anthraquinone compounds, perinone compounds, azo compounds, methine compounds, etc. can be used as an organic compound coloring agent, and commercially available products include toners such as Polysynthren Blue RLS from Clarient or Solvaperm Red BB from Clarient. The amount of the organic compound coloring agent added can be adjusted to 0 to 50 ppm based on the weight of the polyester resin. Examples of the crystallizer include a crystal nucleating agent, an ultraviolet absorber, a polyolefin resin, a polyamide resin, and the like. Examples of the antioxidant include a hindered phenol antioxidant, a phosphite antioxidant, a thioether antioxidant, or a mixture thereof. Examples of the branching agent include a typical branching agent having three or more functional groups, such as trimellitic anhydride, trimethylol propane, trimellitic acid, or a mixture thereof.
[0214]
[0215] Manufacturing of polyester films
[0216] Thereafter, the polyester resin is melt-extruded and stretched to manufacture a polyester film. In one embodiment, the polyester film can be manufactured by biaxially stretching the polyester resin. Specifically, the polyester film can be manufactured through a step of melt-extruding the polyester resin to manufacture an unstretched polyester film including a resin layer formed from the polyester resin; and a step of biaxially stretching the unstretched polyester film at a temperature higher than the glass transition temperature of the polyester resin.
[0217] In the step of manufacturing the above-mentioned unstretched polyester film, the polyester resin may be melt-extruded to minimize thermal decomposition of the polymer. Specifically, the step of manufacturing the above-mentioned unstretched polyester film may be performed at a temperature of 265°C to 300°C. If the melt-extrusion temperature is lower than 265°C, the polymer may not melt, and if it exceeds 300°C, the thermal decomposition of the polymer may increase, causing the film to be damaged or broken during stretching molding, making it difficult to realize the desired physical properties. The above-mentioned unstretched polyester film may be cooled to an appropriate temperature. Thereafter, the unstretched polyester film may be stretched at a temperature higher than the glass transition temperature of the polyester resin.
[0218] The stretching process of the above-mentioned unstretched polyester film is performed at a temperature of 80°C to 200°C, so that the above-mentioned unstretched polyester film can be stretched at a high magnification. Specifically, for biaxial stretching, the above-mentioned unstretched polyester film can be stretched 2 to 6 times, specifically 2 to 5 times, in the longitudinal direction, and 2 to 6 times, specifically 2 to 5 times, in the transverse direction.
[0219] After the biaxial stretching of the above-mentioned unstretched polyester film, a heat-setting step may be additionally included to provide dimensional stability to the obtained biaxially stretched polyester film. The heat-setting step may be performed at a temperature of 160°C to 240°C for 1 second to 60 seconds.
[0220]
[0221] The present invention is described in more detail through the following examples. However, the following examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention.
[0222]
[0223] Example 1
[0224] Step 1) Preparation of regenerated bis(2-hydroxyethyl)terephthalate
[0225] 2000 g of waste polyester resin pulverized to a particle size of 4 mm or less, 4000 g of ethylene glycol, and 7.0 g of zinc acetate anhydride were charged into a first reactor made of stainless steel (SUS), and the internal temperature of the reactor was raised to 180°C to conduct depolymerization (first glycolysis reaction) for 2 hours. The obtained reactant (first reactant) was transferred to a second reactor and cooled to 150°C, and then 2000 g of ethylene glycol was additionally charged, and depolymerization (second glycolysis reaction) was conducted for 2 hours while maintaining the reactor temperature at 150°C.
[0226] The obtained reactant (second reactant) was cooled to 120°C through a reduced pressure flash, 16 g of filter aid was added, and pressure filtration was performed to perform solid-liquid separation. The separated liquid reactant was passed through a column filled with ion exchange resin (BC107(H) from Bonlite) to remove ionic impurities, thereby obtaining a mixture (third reactant) containing bis(2-hydroxyethyl) terephthalate and ethylene glycol.
[0227] The above mixture (third reactant) was transferred to a 10 L distillation apparatus, and distillation under reduced pressure at 130°C was performed to recover unreacted ethylene glycol. The reactant (fourth reactant) from which ethylene glycol was removed was subjected to thin-film distillation at 220°C and 0.08 Torr using a thin-film distiller (VKL70-4S, VTA Corporation) to remove oligomers higher than dimers, obtaining 1040 g of the product.
[0228] Afterwards, 1040 g of the above product and 3120 g of distilled water were placed in a 20 L glass reactor for adsorption-crystallization, dissolved at a temperature of 70°C, 5.2 g of activated carbon was added, stirred for 30 minutes, and filtered. The filtrate was cooled to room temperature to crystallize, filtered, and dried in a vacuum oven. As a result, 1980 g of the final product containing regenerated bis(2-hydroxyethyl)terephthalate was obtained.
[0229] Step 2) Preparation of regenerated bis(2-hydroxyethyl)terephthalate solution
[0230] An r-BHET solution (concentration 71.4 wt%) was prepared by uniformly mixing 1,980 g of regenerated bis(2-hydroxyethyl) terephthalate (r-BHET), 312 g of water, and 483 g of ethylene glycol (EG) at 70°C.
[0231] Step 3) Low-vacuum polycondensation reaction
[0232] Into a 7 L reactor capable of vacuum reaction, 2775 g of the prepared regenerated bis(2-hydroxyethyl)terephthalate (r-BHET) solution, 0.8 g of antimony oxide as a catalyst, 0.6 g of triethyl phosphate as a stabilizer, and 0.4 g of cobalt acetate as a coloring agent were charged. The temperature of the reactor was increased to 190°C over 2 hours, and after reaching 190°C, the pressure of the reactor was decreased from atmospheric pressure to 200 Torr (absolute pressure: 200 mmHg) over 30 minutes, and a low-vacuum polycondensation reaction was performed for 1 hour while maintaining the pressure of the reactor at 200 Torr (absolute pressure: 200 mmHg).
[0233] Step 4) High vacuum polycondensation reaction
[0234] The pressure of the reactor was lowered from 200 Torr (absolute pressure: 200 mmHg) to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes, and at the same time, the temperature of the reactor was raised to 280°C over 1 hour. The high-vacuum polycondensation reaction was performed while maintaining the pressure of the reactor below 1 Torr (absolute pressure: 1 mmHg). In the initial stage of the high-vacuum polycondensation reaction, the stirring speed was set to be fast, but as the high-vacuum polycondensation reaction progresses, the stirring force may be weakened due to the increase in the viscosity of the reactants, or the stirring speed may be appropriately adjusted when the temperature of the reactants rises above the set temperature. The high-vacuum polycondensation reaction was performed until the intrinsic viscosity (IV) of the mixture (melt) in the reactor became 0.64 dl / g. When the intrinsic viscosity of the mixture inside the reactor reached the desired level, the mixture was discharged outside the reactor to form strands, which were solidified with a cooling liquid and then granulated to an average weight of about 12 to 14 mg to obtain a polyester resin.
[0235]
[0236] Example 2
[0237] A polyester resin was prepared by repeating the same procedure as in Example 1, except that in Step 2, 1980 g of recycled bis(2-hydroxyethyl) terephthalate (r-BHET) and 312 g of water were uniformly mixed at 70°C to prepare an r-BHET solution (concentration 86.4 wt%).
[0238]
[0239] Example 3
[0240] A polyester resin was prepared by repeating the same procedure as Example 1, except that the low vacuum polycondensation reaction of Step 3 was not performed and the high vacuum polycondensation reaction of Step 4 was performed.
[0241]
[0242] Example 4
[0243] A polyester resin was manufactured by repeating the same procedure as Example 1, except that the first glycolysis reaction in Step 1 was performed at 180°C for 1 hour.
[0244]
[0245] Example 5
[0246] A polyester resin was manufactured by repeating the same procedure as Example 1, except that 2000 g of waste fiber was used as the waste polyester raw material in Step 1.
[0247]
[0248] Example 6
[0249] A polyether resin was prepared by repeating the same procedure as Example 1, except that 2000 g of waste banner film was used as the waste polyester raw material in Step 1.
[0250]
[0251] Example 7
[0252] A polyester resin was prepared by repeating the same procedure as Example 1, except that adsorption-crystallization was not performed after thin film distillation in Step 1.
[0253]
[0254] Comparative Example 1
[0255] 2,000 g of waste polyester resin, 8,000 g of ethylene glycol, and 7.0 g of zinc acetate anhydride were placed in a stainless steel (SUS) reactor, and the internal temperature of the reactor was raised to 196°C to perform depolymerization (glycolysis) for 4 hours. The obtained reactant was cooled to 30°C, and then crystallization of bis(2-hydroxyethyl) terephthalate was performed for 2 hours. The resulting slurry of bis(2-hydroxyethyl) terephthalate / ethylene glycol was subjected to solid-liquid separation in a centrifuge. The bis(2-hydroxyethyl) terephthalate obtained through centrifugation was washed twice with sufficient distilled water, and the residual solvent was removed in an oven to obtain approximately 2,020 g of the final product containing bis(2-hydroxyethyl) terephthalate.
[0256] A polyester resin was prepared using the bis(2-hydroxyethyl)terephthalate obtained above using the same procedure as in Example 1.
[0257]
[0258] Comparative Example 2
[0259] A polyester resin was manufactured by repeating the same procedure as Comparative Example 1, except that depolymerization (glycolysis reaction) in Step 1 was performed at 210°C.
[0260]
[0261] Comparative Example 3
[0262] A polyester resin was manufactured by repeating the same procedure as in Comparative Example 1, except that depolymerization (glycolysis reaction) was performed at 196°C in Step 1 and adsorption-crystallization was not performed.
[0263]
[0264] Comparative Example 4
[0265] In a batch reactor with a capacity of 5 kg, terephthalic acid (2,161.9 g), ethylene glycol (1,050 g), antimony trioxide (0.8 g) as a catalyst, triethyl phosphate (0.6 g) as a stabilizer, and cobalt acetate (0.4 g) as a coloring agent were charged. After the above raw materials were charged, nitrogen was injected into the reactor so that the pressure of the reactor was 2.0 kgf / cm2 higher than the atmospheric pressure. 2 The reactor was pressurized to a high degree. Then, the temperature of the reactor was raised to 250°C, and the mixture inside the reactor was observed with the naked eye, and the esterification reaction was carried out while maintaining the reactor temperature at 250°C until the mixture became transparent. When the esterification reaction was completed, the nitrogen inside the pressurized reactor was discharged to the outside to lower the pressure inside the reactor to atmospheric pressure, and the mixture inside the reactor was transferred to a 7 L reactor capable of vacuum reaction.
[0266] Then, the pressure of the reactor was lowered from atmospheric pressure to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes, and at the same time, the temperature of the reactor was raised to 280°C. While maintaining the temperature of the reactor at 280°C, the polycondensation reaction was conducted at a pressure of 0.5 to 1.0 Torr for 2 hours. The reaction was conducted until the intrinsic viscosity (IV) of the mixture (melt) inside the reactor became 0.64 dl / g, and when the intrinsic viscosity reached the desired level, the mixture was discharged outside the reactor to be stranded, which was solidified with a cooling liquid and granulated to an average weight of about 12 to 14 mg.
[0267]
[0268] Test Example 1: Evaluation of Regenerated Bis(2-Hydroxyethyl)Terephthalate
[0269]
[0270] 1A. r-BHET component analysis - HPLC
[0271] The components of recycled bis(2-hydroxyethyl)terephthalate were analyzed by high-performance liquid chromatography (HPLC).
[0272] - Approximately 0.01 g of the sample was diluted in approximately 20 mL of methanol and measured using HPLC.
[0273] - Model: Waters e2695
[0274] - Column: C18 (4.6 x 250 mm), 5 ㎛
[0275] - UV Detector: 242 nm
[0276] - Injection volume: 10 μL
[0277] - Eluent (Gradient) A: H2O+H3PO4, B: Acetonitrile
[0278] - Measurement components: Bis(2-hydroxyethyl)terephthalate (BHET), mono(2-hydroxyethyl)terephthalic acid (MHET), 2-hydroxyethyl[2-(2-hydroxyethoxy)ethyl]terephthalate (DEG ester 1), bis[2-(2-hydroxyethoxy)ethyl]benzene-1,4-dicarboxylate (DEG ester 2), dimer, trimer, others
[0279]
[0280] 1B. Residual solvent - GC
[0281] The residual ethylene glycol (EG) content in the recycled bis(2-hydroxyethyl)terephthalate was measured by gas chromatography (GC).
[0282] - 0.1 g of the sample was dissolved in 10 mL CHCl3, filtered through a 0.45 μm filter, and measured by GC.
[0283] - Model: Agilent 7890B
[0284] - Column: DB-624 (30 mx 0.25 mm x 1.4 ㎛)
[0285] - Oven Temp.: 60℃(2 min)-10℃ / min-200℃(0 min)-20℃ / min-260℃(5 min)
[0286] - Injector Temp.: 250℃
[0287] - Detector Temp.: 250℃
[0288] - Flow: 1.5 mL / min (N2), Split ratio: 1 / 50
[0289]
[0290] 1C. Melting point / glass transition temperature / crystallization temperature - DSC
[0291] Using a differential scanning calorimeter (DSC, Q20 model, TA instrument), the sample was filled into an aluminum pan, heated to 280℃ at 10℃ / min, maintained at 280℃ for 5 minutes, then cooled to 30℃ at -300℃ / min, and then heated again to 280℃ at 10℃ / min. The glass transition temperature (Tg) and melting temperature (Tm) were obtained from the heat flow obtained when the temperature was increased again to 280℃. Then, the temperature at the peak of the exothermic curve when the temperature was maintained at 280℃ for 5 minutes and then cooled to 30℃ at -10℃ / min was defined as the cooling crystallization temperature (Tmc).
[0292]
[0293] 1D. Inorganic substances - ICP-AES
[0294] Approximately 0.3 g of the sample was pretreated with ultrasound, diluted with ultrapure water, and analyzed for inorganic components using inductively coupled plasma atomic emission spectrometry (ICP-AES, 5100, Agilent) (detection limit 5 ppm).
[0295]
[0296] Test Example 2: Evaluation of polyester resin
[0297]
[0298] 2A. Melting point (Tm) - DSC
[0299] The melting point of the polyester resin was measured using DSC in the same manner as 1C above.
[0300]
[0301] 2B. Intrinsic viscosity (IV)
[0302] After obtaining a solution by dissolving polyester resin in orthochlorophenol (OCP) at a concentration of 1.2 g / dL at 150°C, the intrinsic viscosity was measured using an Ubbelohde viscosity tube. Specifically, the temperature of the viscosity tube was maintained at 35°C, and the time taken for the solvent to pass through a specific internal section of the viscosity tube (efflux time) and the time taken for the solution to pass through were measured to obtain the specific viscosity, which was then used to calculate the intrinsic viscosity.
[0303]
[0304] 2C. DEG content - GC
[0305] Polyester resin was pulverized in a grinder, 2 g of the resin was aminolyzed with hydrazine hydrate, and then the diethylene glycol (DEG) content (wt%) was measured by gas chromatography (GC).
[0306]
[0307] 2D. Carboxyl end group concentration
[0308] The resin sample and benzyl alcohol, a solvent, were placed in a glass container of a certain size, heated and dissolved at 180℃. A small amount of phenol red as an indicator was added to the dissolved sample solution, and the color change of the solution was observed while adding small amounts of diluted sodium hydroxide solution. The amount of sample added, the concentration of the sodium hydroxide solution, and the amount added were substituted into the following equation to calculate the -COOH terminal group concentration (E) (unit: eq / ton).
[0309] [Mathematical Formula 1]
[0310]
[0311] Here, S is the volume (L) of 0.1 N sodium hydroxide-benzyl alcohol solution consumed in the polyester resin titration, B is the volume (L) of 0.1 N sodium hydroxide-benzyl alcohol solution consumed in the blank titration, N is the concentration of the sodium hydroxide-benzyl alcohol solution, which is 0.1 N, W is the weight (kg) of the polyester resin used in the titration, and f is a factor of the 0.1 N sodium hydroxide-benzyl alcohol solution, which is 0.95 to 0.99, and specifically, 0.97.
[0312]
[0313] 2E. Cyclic trimer - HPLC
[0314] A polyester resin was pulverized with a grinder to obtain a sample, and 0.1 g of the sample was dissolved in 1 mL of 1,1,1,3,3,3-hexafluoro-2-propanol / chloroform = 2 / 3 (v / v). 3 mL of methanol was additionally added, vortexed to re-precipitate, and treated with a 0.2 μm filter. The content of the cyclic trimer was measured by high-performance liquid chromatography (HPLC).
[0315]
[0316] Test Example 3: Evaluation of polyester film
[0317]
[0318] 3A. Manufacturing of polyester film
[0319] Each polyester resin manufactured in the examples and comparative examples was dried at 150°C for 6 hours under a nitrogen atmosphere to control the moisture content to 50 ppm or less.
[0320] A dried polyester resin was melt-extruded into a sheet shape through a die at 280°C, and then rapidly solidified to produce an unstretched film. Thereafter, the unstretched film was first stretched 3.6 times in the machine direction (MD) at 100°C, and then secondarily stretched 3.6 times in the transverse direction (TD) at 120°C. To impart dimensional stability to the stretched film, heat-setting was performed at 230°C for 10 seconds, producing a polyester film having a thickness of 50 μm.
[0321]
[0322] 3B. Tensile strength and elongation
[0323] Using a universal testing machine (UTM 5566A, Instron), samples cut to a length of 5 cm or more and a width of 1.5 cm in each of the longitudinal (MD) and transverse (TD) directions of the film sample were mounted on clips spaced at 5 cm intervals in the longitudinal direction, and then stretched at a rate of 200 mm / min according to ASTM D882 at 25°C until fracture occurred, to obtain stress-strain curves.
[0324] The strength at the point where the film sample breaks was taken as the tensile strength, and the length it stretches was taken as the elongation.
[0325]
[0326] 3C. Elongation Retention Rate (%) - MD, PCT conditions
[0327] The manufactured film was left for 96 hours under the conditions of a high temperature and humidity test (Pressure Cooker Test) at 121°C, 100% relative humidity, and 2 atm, and then the elongation was measured in the longitudinal direction (MD). The elongation measurement method was the same as described above in 3B. Based on the measured values, the elongation retention rate (R) value was calculated according to the following mathematical equation 2.
[0328] [Equation 2]
[0329]
[0330] Here, S0 is the initial elongation (%) of the polyester film sample, and S1 is the elongation (%) measured after leaving the film sample for 96 hours under the conditions of 121°C, 100% RH, and 2 atm.
[0331]
[0332] 3D. Processability Evaluation
[0333] In the process of melt-extruding the polyester resin, a 10 μm filter was used, and the filter pressure generated in the process of removing foreign substances and unmelted resin in a gel state was measured, and in the process of stretching the polyester film, the number of times the film broke over 24 hours was measured, and the processability was evaluated based on the following criteria.
[0334] - ○ (very good): filter pressure 80 kg / cm 2 Below and 0 occurrences of breakage
[0335] - △ (Good): Filter pressure 80~150 kg / cm 2 and 1 occurrence of fracture
[0336] - × (bad): filter pressure 150 kg / cm 2 Below and more than 2 occurrences of breakage
[0337]
[0338] The results of the above test examples are summarized in the table below.
[0339]
[0340]
[0341]
[0342] As shown in the table above, the polyester resins regenerated in Examples 1 to 7 had a cyclic trimer content of 3,000 ppm or less, a diethylene glycol (DEG) content and a carboxyl terminal group concentration controlled to a specific level or less, a high melting point, and excellent processability, strength, elongation, and elongation retention under high temperature and high humidity conditions when manufactured into a film.
[0343] On the other hand, the polyester resins regenerated in Comparative Examples 1 and 3 had concentrations of cyclic trimer, diethylene glycol, and carboxyl terminal groups exceeding the desired ranges, had low melting points, and had poor processability, strength, elongation, and elongation retention under high temperature and humidity conditions when manufactured into films. In addition, Comparative Example 4 is a virgin polyester resin and film thereof that did not undergo a regeneration process, and it was confirmed that Examples 1 to 7 exhibited properties equivalent to or better than these.
Claims
1. Contains regenerated bis(2-hydroxyethyl)terephthalate obtained by depolymerization of waste polyester, The peak area fraction of the cyclic trimer measured by high-performance liquid chromatography (HPLC) is 3,000 ppm or less, A polyester resin having a diethylene glycol (DEG) content of 1.0 wt% or less as measured by gas chromatography (GC).
2. In paragraph 1, The above polyester resin is a polyester resin having a melting point (Tm) of 255°C or higher as measured by differential scanning calorimetry (DSC).
3. In paragraph 1, The above polyester resin is a polyester resin having an intrinsic viscosity of 0.6 dl / g to 1.2 dl / g at 35°C.
4. In paragraph 1, The above-mentioned regenerated bis(2-hydroxyethyl)terephthalate is A polyester resin having a peak area fraction of oligomers of 3% or less as measured by high-performance liquid chromatography.
5. A polyester film comprising a polyester resin according to any one of claims 1 to 4.
6. In paragraph 5, The above polyester film When cut to 1.5 cm in width and mounted on clips spaced 5 cm apart in the longitudinal direction, the tensile strength in the longitudinal direction (MD) is 15 kgf / mm when measured at 25℃ under a tensile speed of 200 mm / min according to ASTM D882. 2 A polyester film having an elongation in the longitudinal direction (MD) of 125% or more.
7. In paragraph 5, The above polyester film is a polyester film having a longitudinal (MD) elongation retention rate (R) of 40% or more, as calculated by the following equation (2): (2) Here S0 is the initial elongation (%) of the polyester film sample, S1 is the elongation (%) measured after leaving it for 96 hours under the conditions of 121℃, 100% RH, and 2 atm. The above elongation is measured at a tensile speed of 200 mm / min according to ASTM D882 at 25°C after cutting the polyester film into 1.5 cm widths and mounting it on clips spaced 5 cm apart in the longitudinal direction. 8.(1) A step of manufacturing recycled bis(2-hydroxyethyl)terephthalate by depolymerizing waste polyester; (2) A step of mixing the above-mentioned regenerated bis(2-hydroxyethyl) terephthalate with a solvent to obtain a regenerated bis(2-hydroxyethyl) terephthalate solution; (3) A step of producing a polyester resin by a polycondensation reaction using the above-mentioned regenerated bis(2-hydroxyethyl)terephthalate solution; and (4) including a step of melting and extruding and stretching the polyester resin; A method for manufacturing a polyester film, wherein the polyester resin has a peak area fraction of a cyclic trimer measured by high-performance liquid chromatography (HPLC) of 3,000 ppm or less and a content of diethylene glycol (DEG) measured by gas chromatography (GC) of 1 wt% or less.
9. In paragraph 8, The polycondensation reaction of the above step (3) (3a) A method for producing a polyester film, comprising a step of producing an oligomer by subjecting the above-mentioned regenerated bis(2-hydroxyethyl)terephthalate solution to a first polycondensation reaction under a pressure of 200 mmHg to 600 mmHg.
10. In paragraph 9, The condensation polymerization reaction of the above step (3) is performed after the above step (3a). (3b) A method for producing a polyester film, further comprising a step of producing a polyester resin by subjecting the above oligomer to a second polycondensation reaction under a pressure of less than 200 mmHg.
Citation Information
Patent Citations
Crystallizing method and apparatus thereof for chemical recycling waste polyester
KR101386683B1
Processes for the purification of bis(2-hydroxyethyl)terephthalate
US7211193B2
METHOD FOR PRODUCING BIS-beta-HYDROXYETHYL TEREPHTHALATE
JP2003055300A
BIS-β-HYDROXYETHYL TEREPHTHALATE
KR1020030019630A
Polyester resin, molded object thereof, and processes for producing these