Thermal insulation gypsum, and preparation method therefor and use thereof

By using a mixed formula of hydrophilic modified airgel and hydrophobic airgel in gypsum, the problem of reduced mechanical properties after compounding gypsum and airgel is solved, efficient heat insulation and strength improvement are achieved, and the mixing process is simplified. And reduce dust flying.

WO2024216431A1PCT designated stage expired Publication Date: 2024-10-24ZHONGKE RUNZI (CHONGQING) AEROGEL RES INST CO LTD

Patent Information

Application Number
PCT/CN2023/088651
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

After the existing gypsum is compounded with airgel, its mechanical properties are reduced and the mixture is uneven, making it difficult to improve the thermal insulation performance and strength at the same time.

Method used

A mixed formula of hydrophilic modified aerogel and hydrophobic aerogel is used to ensure the uniform dispersion and thickening of the aerogel in the gypsum by adjusting its mass ratio and particle size. It combines dispersants and auxiliary materials to improve the gypsum's properties. Liquidity and strength.

Benefits of technology

It realizes the efficient thermal insulation performance and mechanical strength improvement of gypsum, ensures the maintenance of thermal insulation performance and compressive strength, simplifies the mixing process, and reduces the problem of dust flying.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023088651_24102024_PF_FP_ABST
    Figure CN2023088651_24102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention are thermal insulation gypsum, and a preparation method therefor and a use thereof. The thermal insulation gypsum of the present invention comprises aerogels and gypsum; the aerogels are uniformly dispersed in the gypsum; and the aerogels include a hydrophilic modified aerogel and a hydrophobic aerogel. According to the present invention, after hydrophilic modified aerogel particles are added, mixing with a gypsum slurry is easier, and compared with untreated hydrophobic aerogel particles, hydrophilic aerogel particles have better thermal insulation performance.
Need to check novelty before this filing date? Find Prior Art

Description

Thermal insulation gypsum and its preparation method and application Technical Field

[0001] The invention belongs to the technical field of building thermal insulation and relates to thermal insulation gypsum and a preparation method and application thereof. Background Art

[0002] With the continuous development of the economy and construction technology, the demand for green, energy-saving, and environmentally friendly buildings continues to increase. Building insulation materials are a major research area for building energy conservation. Gypsum is a commonly used building insulation material with advantages such as simple processing and low cost. Optimizing the thermal insulation properties of gypsum meets the current demand for green and sustainable development.

[0003] Aerogel is a lightweight, solid material with a three-dimensional network structure and nanoscale pores. It boasts a large surface area, high porosity, low density, and extremely low thermal conductivity, enhancing the performance of traditional insulation materials.

[0004] However, when conventional aerogel is combined with gypsum, the hydrophobic nature of the aerogel degrades the mechanical properties of the gypsum, such as reduced compressive strength. Furthermore, the hydrophobic nature of the aerogel leads to uneven mixing, which also results in poor mechanical properties. There is an urgent need to develop an aerogel formulation that effectively incorporates aerogel into gypsum, hoping to produce a modified gypsum with both excellent thermal insulation and strength properties.

[0005] Summary of the Invention

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0007] A thermal insulation gypsum comprises aerogel and gypsum; the aerogel is uniformly dispersed in the gypsum; and the aerogel comprises hydrophilic modified aerogel and hydrophobic aerogel.

[0008] The inventors discovered that when hydrophilic modified aerogel is used alone as a modifying material, although the mixing uniformity of the aerogel and gypsum can be effectively improved, the introduction of the hydrophilic modified aerogel will cause a significant decrease in the strength of the gypsum. However, when a powder obtained by mixing hydrophobic aerogel and hydrophilic modified aerogel is used as an additive to the gypsum, it not only improves the dispersibility of the gypsum but also has a certain thickening effect, effectively maintaining or even increasing the strength of the gypsum. It is based on this discovery that the present invention is proposed.

[0009] According to an embodiment of the present invention, in the aerogel, the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 100:(0-100) and the content of the hydrophobic aerogel is not 0, preferably 100:(20-50), for example, 100:5, 100:10, 100:20, 100:30, 100:40, 100:60, 100:70, 100:80, 100:90. Studies have found that when the mass ratio of the hydrophobic aerogel to the hydrophilic modified aerogel is within the above range, the thermal insulation performance of the thermal insulation gypsum can be guaranteed while maintaining the mechanical strength of the thermal insulation gypsum.

[0010] According to an embodiment of the present invention, in the thermal insulation gypsum, the particle size of the aerogel is 1 nm-50 nm, preferably 20 nm-50 nm, for example, 1 nm, 10 nm, 20 nm, 30 nm, 40 nm or 50 nm.

[0011] According to an embodiment of the present invention, in the modified gypsum, the mass ratio of aerogel to gypsum is (0-30):100 and the content of the aerogel is not 0, for example, 5:100, 10:100, 15:100, 20:100, 25:100, or 30:100.

[0012] According to an embodiment of the present invention, the hydrophilically modified aerogel is a hydrophilically modified aerogel particle.

[0013] According to an embodiment of the present invention, the contact angle between the hydrophilic modified aerogel and water is less than 90°. Preferably, the surface of the hydrophilic modified aerogel contains hydrophilic groups, which are selected from groups known in the art, such as hydroxyl groups (-OH).

[0014] According to an embodiment of the present invention, the contact angle of the hydrophobic aerogel with water is greater than 90°. Preferably, the surface of the hydrophobic aerogel contains hydrophobic groups, which are selected from groups known in the art, such as alkoxy groups (-OR, R represents an alkyl group).

[0015] According to an embodiment of the present invention, the raw material of gypsum includes a gypsum matrix.

[0016] According to an embodiment of the present invention, the gypsum matrix is ​​selected from gypsum powder (eg, hemihydrate gypsum powder). Preferably, the purity of the gypsum powder is at least greater than 90 wt%, such as 98 wt%.

[0017] According to an embodiment of the present invention, the gypsum plaster powder has a relatively high fineness, for example, preferably 100 to 120 meshes.

[0018] According to an embodiment of the present invention, the gypsum raw material also includes a dispersant. Studies have found that the introduction of a dispersant can improve the fluidity of the product during molding and processing without affecting the performance of the product, and is non-toxic and reasonably priced.

[0019] According to an embodiment of the present invention, the dispersant is selected from at least one of polyoxyethylene dioleate, tetraethylene glycol monostearate, tetraethylene glycol monooleate, polyoxypropylene mannitol dioleate, polyoxyethylene sorbitol lanolin oleic acid derivatives, polyoxyethylene sorbitol lanolin derivatives, polyoxypropylene stearate, polyoxyethylene (5EO) lanolin ether, anhydrous sorbitan laurate, polyoxyethylene fatty acid, polyoxyethylene oxypropylene oleate, triethylhexyl phosphoric acid, sodium lauryl sulfate, methyl amyl alcohol, cellulose derivatives, polyacrylamide, gur gum, fatty acid polyethylene glycol esters, etc., preferably polyoxypropylene stearate and / or polyoxyethylene dioleate.

[0020] According to an embodiment of the present invention, the dispersant is present in an amount of 0.01-5 parts by mass, for example, 0.1 parts by mass, 0.5 parts by mass, 1 part by mass, 2 parts by mass, 3 parts by mass, or 4 parts by mass, per 100 parts by mass of the gypsum matrix.

[0021] According to an embodiment of the present invention, the raw materials of the gypsum may further include auxiliary materials.

[0022] According to an embodiment of the present invention, the auxiliary material is selected from at least one of an air entraining agent, glass microspheres, water, a reinforcing agent, a reinforcing fiber and a retarder.

[0023] According to an embodiment of the present invention, the air-entraining agent is present in an amount of 0.1 to 1 part by mass, for example, 0.1 part by mass or 0.5 part by mass, per 100 parts by mass of the gypsum matrix. The inventors have discovered that adding an air-entraining agent to the gypsum matrix and stirring it uniformly improves the fluidity and cohesiveness of the gypsum.

[0024] According to an embodiment of the present invention, the air entraining agent can be selected from air entraining agents known in the art, for example, rosin resin air entraining agents, alkylbenzene sulfonate air entraining agents, and fatty alcohol sulfonate air entraining agents.

[0025] Specifically, the air entraining agent can be selected from at least one of sodium lauryl sulfate, sodium rosinate, triterpenoid saponin, and sodium α-olefin sulfonate.

[0026] According to an embodiment of the present invention, in the raw material of the gypsum, the amount of the vitrified microspheres is 5 to 40 parts by weight per 100 parts by weight of the gypsum matrix, for example, 10 parts by weight, 20 parts by weight, 30 parts by weight, or 40 parts by weight.

[0027] According to an embodiment of the present invention, the glass microspheres can be selected from materials known in the art and are not specifically limited in the present invention.

[0028] According to an embodiment of the present invention, in the raw material of the gypsum, per 100 parts by mass of the gypsum matrix, water is 100-120 parts by mass, for example, 105 parts by mass, 110 parts by mass, 115 parts by mass, or 120 parts by mass.

[0029] According to an embodiment of the present invention, the reinforcing fibers are selected from inorganic fibers and organic fibers, such as polyester fibers, glass fibers, basalt fibers, etc. Preferably, the reinforcing fibers are short fibers, specifically fibers with a length of 3 mm to 60 mm, such as 10 mm, 20 mm, 30 mm, 40 mm, or 50 mm.

[0030] According to an embodiment of the present invention, the reinforcing fiber is present in an amount of 0.5-5 parts by mass, for example, 0.6 parts by mass, 0.7 parts by mass, 0.8 parts by mass, or 0.9 parts by mass, per 100 parts by mass of the gypsum matrix. In the present invention, the reinforcing fiber is used as a skeleton filler to increase the strength of the aerogel-modified gypsum.

[0031] According to an embodiment of the present invention, the retarder is selected from organic acids and their soluble salts, alkaline phosphates, and proteins. Exemplarily, the retarder is selected from citric acid, sodium citrate, tartaric acid, potassium tartrate, acrylic acid and sodium acrylate, sodium hexametaphosphate, sodium polyphosphate, borax, sodium borate, sodium tripolyphosphate, and sodium gluconate, with citric acid, tartaric acid, and sodium gluconate being preferred. In the present invention, the retarder can extend the mixing time, increase the paste-water ratio, and enhance the strength of the finished product.

[0032] According to an embodiment of the present invention, in the raw material of the gypsum, the retarder is 0.01-0.5 parts by mass per 100 parts by mass of the gypsum matrix, for example, 0.05 parts by mass, 0.1 parts by mass, 0.2 parts by mass, 0.3 parts by mass, or 0.4 parts by mass.

[0033] According to an embodiment of the present invention, the thermal conductivity of the thermal insulation gypsum is not higher than 0.25w / (mk), for example, 0.2w / (mk), 0.1w / (mk), 0.07w / (mk), or 0.05w / (mk).

[0034] According to an embodiment of the present invention, the compressive strength of the thermal insulation gypsum is 1 to 10 MPa, for example, 2 MPa, 3 MPa, 4 MPa, 5 MPa, 6 MPa, 7 MPa, 8 MPa, or 9 MPa.

[0035] The present invention further provides a method for preparing the modified gypsum, which comprises: mixing hydrophilic modified aerogel and hydrophobic aerogel, and then mixing the mixture with gypsum raw materials to obtain the aerogel-modified gypsum.

[0036] According to an embodiment of the present invention, the preparation method specifically comprises:

[0037] A: Aerogel is obtained by mixing hydrophilic modified aerogel and hydrophobic aerogel in proportion;

[0038] B: Mixing the aerogel obtained in step A with the raw materials of gypsum;

[0039] C: After stirring, the modified gypsum is obtained.

[0040] According to an embodiment of the present invention, in step A, the preparation method of the hydrophilic modified aerogel is as follows: taking a hydrophobic aerogel, treating it at a high temperature of 200 to 350° C. for 1 to 10 minutes to obtain a hydrophilic modified aerogel; or,

[0041] The hydrophilic modified aerogel is obtained by impregnation with a hydrophilic agent.

[0042] According to an embodiment of the present invention, the hydrophilic agent is selected from surfactants, low surface tension solvents or silicones.

[0043] Preferably, the surfactant is selected from one or more of anionic surfactants, cationic surfactants, amphoteric surfactants, and nonionic surfactants. Furthermore, the anionic surfactant is selected from one or more of fatty alcohol phosphates, fatty alcohol polyoxyethylene ether phosphates, alkyl sulfates, fatty alcohol polyoxyethylene ether sulfates, glycerol fatty acid ester sulfates, sulfated ricinoleates, cycloalkyl sulfates, fatty amide alkyl sulfates, alkylbenzene sulfonates, alkyl sulfonates, fatty acid methyl ester ethoxylate sulfonates, fatty acid methyl ester sulfonates, and fatty alcohol polyoxyethylene ether carboxylates. Furthermore, the cationic surfactant is selected from aliphatic ammonium salts. Furthermore, the amphoteric surfactant is selected from one or more of alkyl amino acids, carboxylic acid betaines, sulfobetaines, phosphate betaines, and alkyl hydroxyamine oxides. Furthermore, the nonionic surfactant is selected from one or more of aliphatic polyesters, alkylphenol polyoxyethylene ethers, high-carbon fatty alcohol polyoxyethylene ethers, fatty acid polyoxyethylene esters, fatty acid methyl ester ethoxylates, ethylene oxide adducts of polypropylene glycol, sorbitan esters, sucrose fatty acid esters, and alkyl ester amides.

[0044] Preferably, the low surface tension solvent is selected from one or more mixtures of acetone, n-hexane, n-pentane, n-heptane, ethanol, isopropanol, tert-butanol, propylene glycol, and glycerol.

[0045] Preferably, the organosilicon is selected from silane coupling agent ethyl orthosilicate, vinyl silane, aminosilane, methacryloxysilane, isobutyl triethoxysilane, propyl trimethoxysilane, triethoxysilane, and specifically KH-550 and KH-560.

[0046] According to an embodiment of the present invention, in step B, the raw material of the gypsum has the meaning as described above.

[0047] According to an embodiment of the present invention, in step C, the stirring is carried out at 5-20°C, preferably 8-10°C.

[0048] According to an embodiment of the present invention, step C further includes hardening and / or drying after stirring. Preferably, the hardening conditions are: a temperature of 40°C, a humidity not exceeding 70%, and a hardening time of 48-72 hours. Preferably, the drying can be performed using methods known in the art and is not specifically limited in the present invention.

[0049] The present invention further provides an application of the modified gypsum, which is used in the fields of heat insulation, sound insulation, fire prevention, thermal insulation, etc., preferably used in the heat insulation, sound insulation, fire prevention, and thermal insulation of buildings.

[0050] For example, the modified gypsum is applied to concrete walls, building ceilings, masonry walls, and the bottom layer of gypsum boards.

[0051] 1. After adding hydrophilic modified aerogel particles, the present invention is easier to mix with gypsum slurry. Compared with untreated hydrophobic aerogel particles, the hydrophilic aerogel particles have better thermal insulation performance.

[0052] 2. In order to solve the problem that adding hydrophilic aerogel particles to gypsum will reduce the strength of gypsum, this application also introduces hydrophobic aerogel. Under the premise of maintaining thermal insulation performance, the strength is not reduced. That is, the mixed aerogel has better thermal insulation performance and the strength of gypsum is not reduced much, especially the compressive strength. After adding hydrophobic powder as an additive, the dispersibility of the gypsum slurry can be improved.

[0053] 3. After the hydrophilic modified aerogel particles are added to the present invention, the dust flying problem during the mixing process of aerogel powder and gypsum is effectively solved.

[0054] 4. Hydrophilic modified aerogel particles are easier to mix with gypsum. Compared with the traditional mixing process, the stirring time is shortened and the mixing process is simplified. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] FIG1 is a schematic diagram of a preparation process of an aerogel thermal insulation gypsum according to the present invention.

[0056] FIG2 is a schematic diagram of the preparation process of another aerogel thermal insulation gypsum of the present invention. DETAILED DESCRIPTION

[0057] The technical solutions of the present invention will be described in further detail below with reference to specific embodiments. It should be understood that the following embodiments are merely illustrative and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are encompassed within the scope of protection that the present invention is intended to protect.

[0058] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.

[0059] The reagents used in the following examples are as follows:

[0060] Plaster of Paris powder: Commercially available plaster of Paris powder (calcium sulfate hemihydrate) can be used, and the content (purity) of CaSO4·0.5H2O is greater than 90%, preferably above 98%.

[0061] The reinforcing fibers include at least one of glass fibers, polypropylene fibers, and polyester fibers. The reinforcing fibers can improve the anti-cracking performance of the thermal insulation gypsum and increase the tensile strength.

[0062] Vitrified microbeads: particle size is 100μm~300μm.

[0063] Hydrophobic aerogel: Zhongke Runzi Technology Co., Ltd., brand RZF500 or RZF1000.

[0064] Dispersant: polyoxyethylene oleate, Polyshun Chemical.

[0065] Preparation Example 1

[0066] Preparation of hydrophilic modified aerogel:

[0067] The hydrophobic aerogel (produced by Zhongke Runzi Technology Co., Ltd., brand RZF500 or RZF1000) is treated at a high temperature of 200-350° C. for 1-10 minutes to obtain a hydrophilic modified aerogel.

[0068] Preparation Example 2

[0069] Preparation of hydrophilic modified aerogel:

[0070] The hydrophobic aerogel (Zhongke Runzi Technology Co., Ltd., brand RZF500 or RZF1000) is impregnated with ethanol and dried to obtain a hydrophilic modified aerogel. Drying can be natural drying or heat drying. The heat drying conditions are: high temperature 90-110°C for 1-10 minutes.

[0071] The performance of the hydrophilic modified aerogel prepared in Preparation Example 2 is basically equivalent to that in Preparation Example 1. Both hydrophilic modification methods can achieve the hydrophilic modification effect.

[0072] Example 1

[0073] The preparation method of the hybrid aerogel thermal insulation gypsum is as follows (the following parts are all by mass):

[0074] 1) Pretreatment: sieve commercially available gypsum powder through a 100-150 mesh sieve to obtain gypsum powder with a particle size of 100-120 mesh;

[0075] 2) Mixing dry powder raw materials: 100 parts of the gypsum powder prepared in step 1) and auxiliary materials are uniformly mixed to obtain a dry powder mixture, wherein the auxiliary materials include: 0.2 parts of citric acid as a retarder, 1 part of a dispersant, 0.2 parts of sodium lauryl sulfate as an air entraining agent, 10 parts of glass microspheres, and 1 part of reinforcing fiber glass fiber;

[0076] 3) Adding aerogel: Add 5 parts of mixed aerogel (which may be powder or aerogel premix paste) to the dry powder mixture of step 2) and mix evenly to obtain a mixture; wherein the mixed aerogel comprises the hydrophilic modified aerogel of Preparation Example 1 and commercially available hydrophobic aerogel in a mass ratio of 1:1, with the hydrophilic modified aerogel accounting for 2.5 parts;

[0077] 4) Stirring: Add 100-120 parts of water to the mixture of step 3) at a temperature of 5-20° C. (preferably 8-10° C., which can reduce the dissolution rate of hemihydrate gypsum in water, prolong the dissolution time of gypsum in water and the crystal nucleation time, i.e., slow down the reaction rate of gypsum and water) to obtain a slurry;

[0078] 5) Hardening: Pour the slurry from step 4) into a mold, harden, and dry to obtain aerogel-modified gypsum. Hardening conditions are: temperature 40°C, humidity not exceeding 70%, and hardening time 48-72 hours.

[0079] The test shows that the compressive strength of the thermal insulation gypsum of this embodiment is 6.69 MPa and the thermal conductivity is 0.170 W / (m·K), which are recorded in Table 1.

[0080] Example 1-1

[0081] The preparation method of the thermal insulation gypsum of this embodiment is basically the same as that of Example 1, except that in step 3), the mixed aerogel is 5 parts, of which the hydrophilic modified aerogel is added in an amount of 3.33 parts, that is, the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 2:1.

[0082] The test shows that the compressive strength of the thermal insulation gypsum of this embodiment is 6.73 MPa and the thermal conductivity is 0.167 W / (m·K), which are recorded in Table 1.

[0083] Example 2

[0084] The preparation method of the thermal insulation gypsum of this embodiment is basically the same as that of Example 1, except that in step 3), the mixed aerogel is 10 parts, of which the hydrophilic modified aerogel is added in an amount of 5 parts, and the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 1:1.

[0085] The test shows that the compressive strength of the thermal insulation gypsum of this embodiment is 5.63 MPa and the thermal conductivity is 0.118 W / (m·K), which are recorded in Table 1.

[0086] Example 2-1

[0087] The preparation method of the thermal insulation gypsum of this embodiment is basically the same as that of Example 2, except that in step 3), the mixed aerogel is 10 parts, of which the hydrophilic modified aerogel is added in an amount of 6.67 parts, and the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 2:1.

[0088] The test shows that the compressive strength of the thermal insulation gypsum of this embodiment is 5.43 MPa and the thermal conductivity is 0.116 W / (m·K), which are recorded in Table 1.

[0089] Example 3

[0090] The preparation method of the thermal insulation gypsum of this embodiment is basically the same as that of Example 1, except that in step 3), the mixed aerogel is 20 parts, of which the hydrophilic modified aerogel is added in an amount of 10 parts, and the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 1:1.

[0091] The test shows that the compressive strength of the thermal insulation gypsum of this embodiment is 2.51 MPa and the thermal conductivity is 0.097 W / (m·K), which are recorded in Table 1.

[0092] Example 3-1

[0093] The preparation method of the thermal insulation gypsum of this embodiment is basically the same as that of Example 3, except that in step 3), the mixed aerogel is 20 parts, of which the hydrophilic modified aerogel is added in an amount of 13.33 parts, and the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 2:1.

[0094] The test shows that the compressive strength of the thermal insulation gypsum of this embodiment is 2.23 MPa and the thermal conductivity is 0.087 W / (m·K), which are recorded in Table 1.

[0095] Example 4

[0096] The preparation method of the thermal insulation gypsum of this embodiment is basically the same as that of Example 1, except that in step 3), the mixed aerogel is 15 parts, of which the hydrophilic modified aerogel is added in an amount of 7.5 parts, and the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 1:1.

[0097] The test shows that the compressive strength of the thermal insulation gypsum of this embodiment is 3.76 MPa and the thermal conductivity is 0.104 W / (m·K), which are recorded in Table 1.

[0098] Example 4-1

[0099] The preparation method of the thermal insulation gypsum of this embodiment is basically the same as that of Example 4, except that in step 3), the mixed aerogel is 15 parts, of which the hydrophilic modified aerogel is added in an amount of 10 parts, and the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 2:1.

[0100] The test shows that the compressive strength of the thermal insulation gypsum of this embodiment is 3.31 MPa and the thermal conductivity is 0.095 W / (m·K), which are recorded in Table 1.

[0101] Example 5

[0102] The preparation method of the thermal insulation gypsum of this embodiment is basically the same as that of Example 1, except that in step 3), the mixed aerogel is 25 parts, of which the hydrophilic modified aerogel is added in an amount of 12.5 parts, and the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 1:1.

[0103] The test shows that the compressive strength of the thermal insulation gypsum of this embodiment is 1.75 MPa and the thermal conductivity is 0.090 W / (m·K), which are recorded in Table 1.

[0104] Example 5-1

[0105] The preparation method of the thermal insulation gypsum of this embodiment is basically the same as that of Example 5, except that in step 3), the mixed aerogel is 25 parts, of which the hydrophilic modified aerogel is added in an amount of 16.7 parts, and the mass ratio of the hydrophilic modified aerogel to the hydrophobic aerogel is 2:1.

[0106] The test shows that the compressive strength of the thermal insulation gypsum of this embodiment is 1.55 MPa and the thermal conductivity is 0.082 W / (m·K), which are recorded in Table 1.

[0107] Comparative Example 1

[0108] This embodiment is basically the same as embodiment 2, except that in step 3), only hydrophilic modified aerogel is used, and the addition amount thereof is 10 parts.

[0109] The test shows that the compressive strength of the thermal insulation gypsum of this comparative example is 5.23 MPa and the thermal conductivity is 0.111 W / (m·K), which are recorded in Table 1.

[0110] Comparative Example 2

[0111] This embodiment is basically the same as embodiment 2, except that only hydrophobic aerogel is used in step 3), and the amount of hydrophobic aerogel added is 10 parts.

[0112] The test shows that the compressive strength of the thermal insulation gypsum of this comparative example is 6.16 MPa and the thermal conductivity is 0.130 W / (m·K), which are recorded in Table 1.

[0113] Table 1

[0114] The above describes exemplary embodiments of the present invention. However, the scope of protection of this application is not limited to the above embodiments. Any modifications, equivalent substitutions, improvements, etc. made by those skilled in the art within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A thermal insulation gypsum, comprising aerogel and gypsum; characterized in that: The aerogel is uniformly dispersed in the gypsum; the aerogel includes hydrophilic modified aerogel and hydrophobic aerogel.

2. The thermal insulation gypsum according to claim 1, characterized in that: In the aerogel, the mass ratio of the hydrophilic aerogel to the hydrophobic aerogel is 100:(0-100) and the content of the hydrophobically modified aerogel is not zero.

3. The thermal insulation gypsum according to claim 1, characterized in that: In the modified gypsum, the mass ratio of aerogel to gypsum is (0-30):100 and the content of aerogel is not 0.

4. The thermal insulation gypsum according to claim 1, characterized in that: The hydrophilic modified aerogel is a hydrophilic modified aerogel particle.

5. The thermal insulation gypsum according to claim 1, characterized in that: The raw material of the gypsum includes a gypsum matrix.

6. The thermal insulation gypsum according to claim 5, characterized in that: The raw materials of the gypsum also include a dispersant.

7. The thermal insulation gypsum according to claim 5, characterized in that: The raw materials of the gypsum further include auxiliary materials; the auxiliary materials are selected from at least one of air entraining agent, vitrified microspheres, water, reinforcing agent, reinforcing fiber and retarder.

8. The thermal insulation gypsum according to any one of claims 1 to 7, characterized in that: The thermal conductivity of the thermal insulation gypsum is not higher than 0.2w / (mk); And / or, the compressive strength of the thermal insulation gypsum is 1 to 10 MPa.

9. The method for preparing the modified gypsum according to any one of claims 1 to 8, characterized in that: The preparation method comprises: mixing hydrophilic modified aerogel and hydrophobic aerogel, and then mixing with raw materials of gypsum to obtain the aerogel modified gypsum.

10. Use of the modified gypsum according to any one of claims 1 to 8 in the fields of heat insulation, sound insulation, fire protection or thermal insulation.

Citation Information

Patent Citations

  • Aerogel compositions and methods of making and using them

    CN105753388A

  • Aerogel-containing gypsum material and preparation method thereof

    CN106747189A

  • Super-thermal-insulation aerogel foamed concrete and preparation method thereof

    CN107265963A

  • Super-thermal-insulation aerogel foamed concrete and preparation method thereof

    CN107265964A

  • Aerogel composite material and preparation method thereof

    CN109987963A

Cited By

  • Surface hydrophobically modified gypsum-aerogel composite thermal insulation material as well as preparation method and application thereof

    CN119462053A

  • A surface-hydrophobically modified gypsum-aerogel composite thermal insulation material, its preparation method and application