Method for manufacturing aluminum alloy deoxidizing material

Through the method of making aluminum alloy deoxidized materials without heating, the problems of organic pollution and high energy consumption in aluminum recycling are solved, efficient production of aluminum alloy deoxidized materials is achieved, environmental pollution and costs are reduced, and aluminum utilization rate and material performance are improved. .

WO2024216528A1PCT designated stage expired Publication Date: 2024-10-24HF INVESTMENT CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/089113
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

The existing aluminum recycling model produces organic pollutants during the melting process, resulting in environmental pollution and high energy consumption. At the same time, the manufacturing of aluminum alloy deoxidized materials is high energy consumption and high cost, and it is difficult to effectively process aluminum waste containing organic matter with existing technology.

Method used

Using a non-heated aluminum alloy deoxidation material production method, the recycled aluminum material is compacted into aluminum strips and cut into aluminum particles. The high temperature of steelmaking is used to completely crack the organic matter, reduce the generation of dioxin, and improve the deoxidation effect by controlling the alloy composition.

Benefits of technology

It greatly reduces the generation of organic pollutants, saves energy, improves the ductility and toughness of aluminum alloy deoxidized materials, simplifies the recycling process, improves the utilization rate of aluminum materials, and reduces costs and environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023089113_24102024_PF_FP_ABST
    Figure CN2023089113_24102024_PF_FP_ABST
Patent Text Reader

Abstract

A method for manufacturing an aluminum alloy deoxidizing material, the method comprising the following steps: putting a plurality of recycled aluminum materials into a shaper and compacting same until the shaper is filled with the recycled aluminum materials; taking out the compacted and shaped recycled aluminum materials and then putting same into a mold; pouring an aluminum melt into the recycled aluminum materials to form a cast pack in a sealed manner; preheating the cast pack and then performing hot extrusion to form an aluminum bar; and cutting the aluminum bar into a plurality of aluminum particles to complete an aluminum alloy deoxidizing material.
Need to check novelty before this filing date? Find Prior Art

Description

Manufacturing method of aluminum alloy deoxidized material Technical Field

[0001] The present invention relates to a method for manufacturing a deoxidizing material, in particular to a method for manufacturing an aluminum alloy deoxidizing material. Background Art

[0002] The circular economy has become a prominent concept in modern society. Unlike the traditional linear economic model, which follows a progression from resource extraction to production, consumption, and ultimately disposal, this model, based on resource recovery and reuse, aims to minimize resource consumption and waste. The circular economy encourages the cyclical use of resources, maximizing their value through recycling, regeneration, and reuse, ultimately achieving a sustainable economic development model.

[0003] The metal and related manufacturing industries are significant resource consumers and environmental polluters, making the implementation of a circular economy crucial for this sector. Many relevant industries have long practiced metal recycling, as recycling can save significant amounts of raw materials and energy, reduce carbon emissions, and can be used to manufacture new products. However, the current aluminum recycling model requires smelting and tempering recycled aluminum, which consumes significant amounts of energy, requires numerous operations, and results in high operating costs. Oxidation caused by heating also results in significant yield losses and waste of aluminum, and the remelting of scrap aluminum produces toxic fumes and slag.

[0004] In addition, the recycled aluminum materials collected by the current aluminum recycling model, such as aluminum cans, aluminum foil packages, or aluminum scraps generated after machining and cutting, are all mixed with a certain degree of organic matter due to the use requirements and characteristics of the recycled aluminum materials before recycling. For example, the internal surface of aluminum cans contains a resin coating and the external printed coating, or the scrap aluminum scraps contain cutting fluid, etc. These organic substances attached to the recycled aluminum materials will produce organic pollutants such as dioxin during the remelting process of the recycled aluminum materials in the existing aluminum recycling process, causing serious environmental pollution and public hazards.

[0005] On the other hand, in the steel industry, deoxidizing materials are widely used during the steelmaking process to remove oxygen from molten steel, effectively improving its quality and properties, increasing its purity and uniformity, reducing defects, and enhancing its toughness and corrosion resistance. Aluminum alloys, in particular, are highly reactive with oxygen. However, aluminum alloys are expensive, and the energy consumption of existing technologies for producing aluminum alloy deoxidizers is also very high. Consequently, developing methods to reduce organic pollutants generated by recycled aluminum scrap and implement a circular economy has become a pressing goal in the relevant field.

[0006] Summary of the Invention

[0007] To address the environmental pollution caused by the generation of organic pollutants during the melting of scrap aluminum in existing aluminum recycling processes, the present invention provides a method for producing an aluminum alloy deoxidizer, comprising the following steps: placing a plurality of recycled aluminum materials into a predetermined shape and compacting them until the recycled aluminum materials fill the predetermined shape; placing the compacted recycled aluminum materials into a mold; pouring aluminum broth over the recycled aluminum materials and sealing them to form a ladle; forming the ladle into an aluminum bar by hot extrusion; and cutting the aluminum bar into a plurality of aluminum pellets to produce an aluminum alloy deoxidizer.

[0008] The shaped part is filled with recycled aluminum material from a single source, and the recycled aluminum material and the aluminum broth have the same alloy composition.

[0009] The recycled aluminum material is aluminum chips generated by aluminum alloy cutting.

[0010] The recycled aluminum material is shredded aluminum cans or aluminum foil packages.

[0011] The shaping piece is an aluminum alloy tube, and the recycled aluminum material and the shaping piece are composed of the same alloy, and the shaping piece filled with the recycled aluminum material is directly placed into the mold.

[0012] The ratio of the cross-sectional area of ​​the shaping piece to that of the aluminum strip is between 25:1 and 10:1.

[0013] The temperature of the hot extrusion is between 400°C and 550°C.

[0014] The extrusion speed of the hot extrusion is between 0.2 meters per minute and 2 meters per minute.

[0015] The porosity of the aluminum strip is less than one percent.

[0016] The step of cutting the aluminum strip into a plurality of aluminum particles is performed in an oxygen-free environment.

[0017] The step of placing the recycled aluminum material into the shaped part further comprises placing elements such as magnesium, manganese, silicon, zinc or copper into the shaped part.

[0018] It can be seen from the above description that the present invention has the following characteristics:

[0019] 1. The method for producing the aluminum alloy deoxidizer of the present invention does not require heating to melt the waste aluminum, which can significantly reduce the generation of organic pollutants such as dioxin and avoid the risk of organic pollutants escaping into the environment.

[0020] 2. The method for producing the aluminum alloy deoxidizer of the present invention does not require heating to melt the waste aluminum, which can save a lot of energy and does not produce toxic fumes and slag produced when the waste aluminum is melted.

[0021] 3. The method for producing the aluminum alloy deoxidizer of the present invention does not require heating to melt the waste aluminum, thereby avoiding yield loss caused by aluminum oxidation during the production process.

[0022] 4. The method for producing the aluminum alloy deoxidizer of the present invention further utilizes recycled aluminum as a deoxidizer for steelmaking, and simultaneously utilizes the high temperature of steelmaking to completely decompose organic matter attached to the recycled aluminum, thereby reducing the production of dioxin and also reducing the cost of the deoxidizer and raw material consumption in the steelmaking process.

[0023] 5. The method for producing the aluminum alloy deoxidizer of the present invention does not generate organic pollutants during the production process due to the organic matter contained in the recycled aluminum material. It can simplify or even eliminate the pre-treatment process of the recycled aluminum material, saving time, resources and costs, and is more environmentally friendly.

[0024] 6. The aluminum alloy deoxidizer formed by the manufacturing method of the aluminum alloy deoxidizer of the present invention has the characteristics of a high entropy alloy. Because the high entropy effect can promote the formation of solid solution phases of various elements, the phase change of the alloy with temperature is relatively simple, the crystal structure is stable and dense, and the formation of brittle metal compounds is suppressed, thereby greatly improving the ductility and toughness of the aluminum alloy deoxidizer.

[0025] 7. The method for manufacturing the aluminum alloy deoxidizer of the present invention does not require fixing the aluminum blocks with adhesives as in the prior art, which can save costs and avoid environmental pollution and resource waste caused by adhesives.

[0026] 8. The method for making the aluminum alloy deoxidizer of the present invention first forms the recycled aluminum into aluminum bars and then cuts them into multiple aluminum particles. This can reduce the surface area of ​​the aluminum alloy deoxidizer in contact with the atmosphere, thereby reducing the formation of aluminum oxide and improving the deoxidization effect of the deoxidizer.

[0027] 9. The present invention forms aluminum particles into shapes including concave and hollow shapes by cutting, thereby reducing the buoyancy of the aluminum alloy deoxidizer, making it easier for the aluminum particles to sink to the bottom of the steelmaking molten bath, and increasing the contact surface area, thereby significantly improving the deoxidation effect.

[0028] 10. The method for producing the aluminum alloy deoxidizer of the present invention can further add other elements before hot extrusion to adjust the redox capacity and specific gravity of the aluminum particles by adjusting the alloy composition, thereby improving the deoxidation effect of the deoxidizer.

[0029] 11. The method for making the aluminum alloy deoxidizer of the present invention can recycle aluminum waste that is difficult to process using conventional methods, such as aluminum chips generated by aluminum alloy cutting or used aluminum cans. This solves the problem that these aluminum chips have a large surface area to volume ratio, making them easily oxidized and often mixed with lubricants, cutting fluids, or beverage residues and coatings, making them difficult to remelt and recycle using conventional methods. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] FIG1 is a step diagram of an embodiment of the present invention.

[0031] Explanation of symbols:

[0032] S10-S50: Steps DETAILED DESCRIPTION

[0033] To more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing each embodiment. Obviously, the drawings described below are merely examples or embodiments of the present invention. Those skilled in the art can apply the present invention to other similar scenarios based on these drawings without inventive effort. Unless otherwise apparent from the context or otherwise noted, the same reference numerals in the figures represent the same structure or operation.

[0034] As used herein and in the claims, unless the context clearly indicates otherwise, the words "a," "an," "an," or "the" do not necessarily refer to one item but may also include multiple items. Generally speaking, the terms "comprises" and "include" only indicate the inclusion of the steps and elements specifically identified, and these steps and elements do not constitute an exclusive list. A method or apparatus may also include additional steps or elements.

[0035] Flowcharts are used in this disclosure to illustrate the operations performed by systems according to embodiments of the present invention. It should be understood that the preceding and following operations do not necessarily need to be performed in exact order. Instead, the steps may be processed in reverse order or simultaneously. Furthermore, other operations may be added to these processes, or one or more operations may be removed from these processes.

[0036] Please refer to FIG1 , which is a diagram of the steps of the present invention. The present invention mainly includes steps S10 to S50.

[0037] Step S10: Place a plurality of recycled aluminum materials into a forming part and compact them until the recycled aluminum materials fill the forming part. In this step S10, the collected recycled aluminum materials are concentrated and placed into the forming part and continuously compacted. When the recycled aluminum materials shrink due to compression, more recycled aluminum materials can be placed into the forming part until the recycled aluminum materials completely fill the forming part. Preferably, the forming part is a hollow tube, and the hollow tube can be a tube with openings at both ends or only one end. The cross-section of the hollow tube is circular. Preferably, the diameter of the cross-section circle of the hollow tube is 9 cm, and the length of the hollow tube is 60 cm.

[0038] The recycled aluminum material can be various recycled aluminum scraps. For example, the recycled aluminum material can be aluminum chips generated during the cutting process of an aluminum alloy block, or recycled aluminum cans and aluminum foil scraps that have been pre-treated and shredded. Preferably, the recycled aluminum materials placed and filled in the hollow tube are all recycled aluminum materials from a single source. The so-called single source means that the recycled aluminum materials are all aluminum alloy scraps of the same alloy or the same Aluminum Association alloy number. In one embodiment, the recycled aluminum material placed and filled in the forming part comes from aluminum alloy aluminum chips generated by the same cutting process performed by the same machine tool. In another embodiment, recycled aluminum alloy cans with the Aluminum Association alloy number 3004 are shredded and placed in the forming part for compaction and filling.

[0039] The recycled aluminum material may undergo a series of pre-treatments before being placed into the molded part for compaction and filling. In one embodiment, the recycled aluminum material undergoes preliminary cleaning and air separation to remove larger impurities, followed by magnetic separation to remove ferromagnetic metals. However, these pre-treatments are not absolutely necessary; appropriate pre-treatment techniques can be selected based on the source of the recycled aluminum material. For example, in one embodiment, the recycled aluminum material is aluminum shavings generated during the cutting process of an aluminum alloy block. Pre-cleaning the recycled aluminum material to remove the cutting fluid is sufficient before the recycled aluminum material is placed into the molded part for filling and compaction.

[0040] Therefore, the recycled aluminum material contains a variety of residual organic compounds. In one embodiment, the recycled aluminum material is aluminum chips generated during the cutting process of an aluminum alloy block. The various organic compounds remaining in the recycled aluminum material are mostly cutting fluid, which may contain ingredients such as mineral oil, emulsifiers, water, rust-proof additives, and defoamers. In another embodiment, the recycled aluminum material is recycled aluminum cans and aluminum foil bag scraps. The various organic compounds remaining in the recycled aluminum material may be paper components contained in the aluminum foil bag, such as cellulose, hemicellulose, or lignin, or the printed layer on the aluminum can body that has not been completely removed, and the coating layer on the inner layer of the aluminum can. The components of this coating layer may be various lipids such as waxes, various resins such as epoxy resins, or various polyesters such as acrylic copolymers or polycarbonates. These organic compounds are difficult to completely remove during the pre-treatment process without consuming a huge amount of time, energy, and resources. However, in this step S10, the recycled aluminum material does not need to undergo a tedious pre-treatment process before it can be placed into the molded part for compaction and filling.

[0041] To achieve even better results in the aluminum alloy deoxidizer formed by the present invention, elements such as magnesium, manganese, silicon, zinc, or copper can be added to the aluminum package during the step of placing the recycled aluminum into the cladding material for filling and compacting, thereby further enhancing the overall deoxidization effect and regulating the specific gravity of the aluminum alloy deoxidizer formed by the present invention. Preferably, different proportions of elements can be added to the recycled aluminum to achieve a specific ratio, such that the aluminum package contains 0.1 to 2 weight percent silicon, 0 to 2 weight percent copper, 0.1 to 30 weight percent magnesium, 0.1 to 10 weight percent manganese, and 0 to 10 weight percent zinc.

[0042] Step S20: Place the compacted recycled aluminum into a mold. In this step S20, when the recycled aluminum has been compacted and fills the forming part, the compacted recycled aluminum is removed from the forming part and placed into the mold. This step S20 allows the recycled aluminum to be removed from the forming part and placed into the mold. Because the recycled aluminum has been compacted, it maintains its shape within the coating material when removed and will not scatter or deform. Preferably, the coating material is the hollow tube, and the compacted recycled aluminum is cylindrical after removal. Place the compacted recycled aluminum into the mold. The mold is a long, hollow cylinder with a length and cross-section greater than that of the hollow tube. A fixed ring is placed at the bottom of the mold at the center of a long axis. The fixed ring is equal to or slightly larger than the cross-section of the compacted recycled aluminum, allowing the fixed ring to secure the compacted recycled aluminum in the center of the long axis of the mold without shifting. The mold may also include one or more clamping devices to securely hold the compacted recycled aluminum material within the mold. In a preferred embodiment, the mold opening has a diameter of 12.7 cm and is 60 cm long. A retaining ring with a diameter of 10 cm and a depth of 1 cm is located at the bottom of the mold, while an aluminum sheet and a screw are located at the top of the mold for tightening. In another preferred embodiment, the mold secures the compacted recycled aluminum material with an aluminum alloy tube.

[0043] Furthermore, step S20 can also involve directly placing the shaped member filled with the recycled aluminum material into the mold, without removing the recycled aluminum material from the shaped member. In a preferred embodiment, the shaped member is a hollow tube made of an aluminum alloy. This allows the recycled aluminum material to be compacted within the hollow tube without being removed. Instead, the hollow tube is placed into the mold along with the aluminum alloy hollow tube, with the hollow tube serving as the clamping device. More preferably, the aluminum alloy hollow tube and the recycled aluminum material have the same alloy composition, i.e., the hollow tube and the recycled aluminum material have the same alloy or the same Aluminum Association alloy number.

[0044] Step S30: The recycled aluminum is poured into an aluminum broth and sealed to form a ladle. In step S30, the recycled aluminum placed in the mold is poured into an aluminum broth, which completely encapsulates the recycled aluminum. After cooling and solidification, a ladle is formed. The aluminum broth is molten aluminum alloy. Preferably, the aluminum broth and the recycled aluminum have the same alloy composition, that is, the aluminum broth and the recycled aluminum have the same alloy or the same Aluminum Association alloy number. In one embodiment, the recycled aluminum formed by compacting and filling recycled aluminum cans with Aluminum Association alloy number 3004 into the hollow tube is poured with the aluminum broth with Aluminum Association alloy number 3004 in this step, so that the aluminum alloy of the ladle maintains the same homogeneous aluminum alloy properties. Preferably, the aluminum sheet used for compaction also has the same alloy composition as the recycled aluminum. The aluminum broth completely encapsulates the recycled aluminum, thereby encapsulating the plurality of organic compounds within the ladle.

[0045] Step S40: After preheating the ladle, form an aluminum bar by hot extrusion. In this step S40, the ladle is taken out of the mold and preheated as an aluminum billet, which is formed by hot extrusion to form an aluminum bar. The cross-sectional shape of the aluminum bar can be designed according to the needs of an extrusion die through which the ladle passes, and the hot extrusion can be direct extrusion or indirect extrusion. The indirect extrusion can produce a hollow structure inside the aluminum bar. Preferably, the temperature of the hot extrusion is between 400°C and 550°C, and the extrusion speed of the hot extrusion is between 0.2 meters per minute and 2 meters per minute; the so-called extrusion speed is the speed at which the aluminum bar is formed by hot extrusion. Preferably, the cross-sectional area ratio of the hollow tube to the aluminum bar is between 25:1 and 10:1; the cross-sectional area ratio of the hollow tube to the aluminum bar is the extrusion ratio, that is, the preferred extrusion ratio of this step S40 is between 10 and 25, and the porosity of the resulting aluminum bar is less than 1%.

[0046] Step S50: Cut the aluminum bar into multiple aluminum granules to complete an aluminum alloy deoxidizing material. In this step S50, the aluminum bar formed by hot extrusion is cut into multiple aluminum granules, and the production of the aluminum alloy deoxidizing material is completed. The aluminum granules can be cut into round or polygonal shapes. Preferably, the aluminum granules may also include concave surfaces and hollows, so that the surface area of ​​the aluminum granules is increased, thereby exerting a better deoxidizing effect, while also reducing buoyancy, so that the aluminum granules are easy to sink to the bottom of the steelmaking molten soup, thereby increasing the deoxidizing effect. In one embodiment, the aluminum bar formed by indirect hot extrusion in step S40 includes a hollow along the axial direction in the aluminum bar, so that when the aluminum bar is cut into multiple aluminum granules, the aluminum granules are formed with through holes.

[0047] Preferably, step S50 can be performed in an oxygen-free environment, such as cutting the aluminum bar into multiple aluminum particles and packaging them in a nitrogen environment, so that aluminum oxide will not form on the surface of the aluminum particles, thereby increasing the deoxidation capacity and efficiency of the aluminum alloy deoxidizer.

[0048] <Application of aluminum alloy deoxidizing materials>

[0049] The aluminum alloy deoxidizer produced by the method of the present invention can be used in steelmaking blast furnaces as a deoxidizer for molten steel. Since the temperature of a steelmaking blast furnace is well above 900°C, the recycled aluminum material contains various residual organic compounds. These organic compounds can be completely decomposed at this temperature, thus preventing the formation of toxic organic pollutants such as dioxin and effectively assisting in the deoxidation of molten steel.

[0050] It can be seen from the above description that the present invention achieves the following effects:

[0051] 1. The method for producing the aluminum alloy deoxidizer of the present invention can significantly reduce the generation of organic pollutants such as dioxin because it does not require heating to melt the waste aluminum.

[0052] 2. The method for producing the aluminum alloy deoxidizer of the present invention does not require heating to melt the waste aluminum, which can save a lot of energy and does not produce toxic fumes and slag produced when the waste aluminum is melted.

[0053] 3. The aluminum alloy deoxidizer production method of the present invention eliminates the need to heat the scrap aluminum to melt, thus avoiding yield losses caused by aluminum oxidation during the process. While existing scrap aluminum recycling methods generate high amounts of new scrap, ultimately recovering no more than 52% of the metal, the present invention achieves a recycling rate of approximately 96%, significantly increasing the amount of recyclable aluminum.

[0054] 4. The method for producing the aluminum alloy deoxidizer of the present invention further utilizes recycled aluminum as a deoxidizer for steelmaking, and simultaneously utilizes the high temperature of steelmaking to completely decompose organic matter attached to the recycled aluminum, thereby reducing the production of dioxin and also reducing the cost of the deoxidizer and raw material consumption in the steelmaking process.

[0055] 5. The method for producing the aluminum alloy deoxidizer of the present invention does not generate organic pollutants during the production process due to the organic matter contained in the recycled aluminum material. It can simplify or even eliminate the pre-treatment process of the recycled aluminum material, saving time, resources and costs, and is more environmentally friendly.

[0056] 6. The aluminum alloy deoxidizer formed by the manufacturing method of the aluminum alloy deoxidizer of the present invention has the characteristics of a high entropy alloy. Because the high entropy effect can promote the formation of solid solution phases of various elements, the phase change of the alloy with temperature is relatively simple, the crystal structure is stable and dense, and the formation of brittle metal compounds is suppressed, thereby greatly improving the ductility and toughness of the aluminum alloy deoxidizer.

[0057] 7. The method for manufacturing the aluminum alloy deoxidizer of the present invention does not require fixing the aluminum blocks with adhesives as in the prior art, which can save costs and avoid environmental pollution and resource waste caused by adhesives.

[0058] 8. The method for making the aluminum alloy deoxidizer of the present invention first forms the recycled aluminum into aluminum bars and then cuts them into multiple aluminum particles. This can reduce the surface area of ​​the aluminum alloy deoxidizer in contact with the atmosphere, thereby reducing the formation of aluminum oxide and improving the deoxidization effect of the deoxidizer.

[0059] 9. The present invention forms aluminum particles into shapes including concave and hollow shapes by cutting, thereby reducing the buoyancy of the aluminum alloy deoxidizer, making it easier for the aluminum particles to sink to the bottom of the steelmaking molten bath, and increasing the contact surface area, thereby significantly improving the deoxidation effect.

[0060] 10. The method for producing the aluminum alloy deoxidizer of the present invention can further add other elements before hot extrusion to adjust the redox capacity and specific gravity of the aluminum particles by adjusting the alloy composition, thereby improving the deoxidation effect of the deoxidizer.

[0061] 11. The method for making the aluminum alloy deoxidizer of the present invention can recycle aluminum waste that is difficult to process using conventional methods, such as aluminum chips generated by aluminum alloy cutting or used aluminum cans. This solves the problem that these aluminum chips have a large surface area to volume ratio, making them easily oxidized and often mixed with lubricants, cutting fluids, or beverage residues and coatings, making them difficult to remelt and recycle using conventional methods.

[0062] It should be noted that, based on the explanations and elaborations of the above description, those skilled in the art may also make changes and modifications to the above embodiments. Therefore, the present disclosure is not limited to the specific embodiments disclosed and described above, and equivalent modifications and variations of the present disclosure are also within the scope of protection of the claims of the present disclosure. Furthermore, although certain specific terms are used in this description, these terms are for convenience only and do not constitute any limitation on the invention.

Claims

1. A method for producing an aluminum alloy deoxidizing material, It is characterized in that It contains the following steps: Putting a plurality of recycled aluminum materials into a certain shaped part and compacting the recycled aluminum materials until the shaped part is filled with the recycled aluminum materials; placing the compacted recycled aluminum material into a mold; The recycled aluminum material is poured into an aluminum soup and sealed to form a casting ladle; forming the casting bag into an aluminum bar by hot extrusion; as well as The aluminum strip is cut into a plurality of aluminum grains to complete an aluminum alloy deoxidized material.

2. The method for producing the aluminum alloy deoxidizing material according to claim 1, It is characterized in that The shaped part is filled with recycled aluminum material from a single source, and the recycled aluminum material and the aluminum soup have the same alloy composition.

3. The method for producing the aluminum alloy deoxidizing material according to claim 2, It is characterized in that The recycled aluminum material is aluminum chips generated by cutting aluminum alloy.

4. The method for producing the aluminum alloy deoxidizing material according to claim 2, It is characterized in that The recycled aluminum material is shredded aluminum cans or aluminum foil packages.

5. The method for producing the aluminum alloy deoxidizing material according to claim 2, It is characterized in that The shaping piece is an aluminum alloy tube, and the recycled aluminum material and the shaping piece are composed of the same alloy, and the shaping piece filled with the recycled aluminum material is directly placed in the mold.

6. The method for producing the aluminum alloy deoxidizing material according to any one of claims 1 to 5, It is characterized in that The cross-sectional area ratio of the shaping piece to the aluminum strip is between 25:1 and 10:

1.

7. The method for producing the aluminum alloy deoxidizing material according to claim 1 or 2, It is characterized in that The temperature of the hot extrusion is between 400°C and 550°C.

8. The method for producing the aluminum alloy deoxidizing material according to claim 1 or 2, It is characterized in that The extrusion speed of the hot extrusion is between 0.2 meters per minute and 2 meters per minute.

9. The method for producing the aluminum alloy deoxidizing material according to claim 1, It is characterized in that The aluminum strip has a porosity of less than one percent.

10. The method for producing the aluminum alloy deoxidizing material according to claim 1, It is characterized in that The step of cutting the aluminum strip into a plurality of aluminum particles is performed in an oxygen-free environment.

11. The method for producing the aluminum alloy deoxidizing material according to claim 1, It is characterized in that The step of placing the recycled aluminum material into the shaped part further comprises placing specified elements into the shaped part, wherein the specified elements include but are not limited to one or more of magnesium, manganese, silicon, zinc and copper.

Citation Information

Patent Citations

  • Method for processing steelmaking aluminum deoxidizing agent using aluminum waste

    CN108977622A

  • Aluminum alloy recovery process

    CN111926186A

  • Briquettes for deoxidizing steel

    GB2482885A

  • Manufacture of aluminum deoxidizer

    JP1995090346A

  • Aluminum pressure molding and deoxidizing agent for iron and steel or raw material for remolten aluminum