Electrochemical deintercalation-based lithium extraction method

By adjusting the concentration and sedimentation of magnesium ions in the electrochemical lithium extraction device, combined with an anion exchange membrane, the problem of magnesium ion interference during the electrochemical lithium extraction process is solved, and the extraction efficiency and economic benefits of lithium ions are improved.

WO2024216539A1PCT designated stage expired Publication Date: 2024-10-24GUANGDONG BRUNP RECYCLING TECH CO LTD +1

Patent Information

Application Number
PCT/CN2023/089238
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

During the electrochemical lithium extraction process, magnesium ions cause great interference to the extraction of lithium ions, resulting in a cation repulsion effect and affecting the lithium extraction efficiency.

Method used

By adjusting the Mg(OH)2 in the lithium solution to be extracted to a nearly saturated concentration in the electrochemical deintercalation and lithium extraction device, a local low supersaturation is formed to avoid the aggregation and sedimentation of magnesium ions, combined with an anion exchange membrane and a conductive current collector, to achieve Efficient extraction of lithium ions.

Benefits of technology

Effectively avoid or reduce the cation rejection effect, improve the extraction efficiency of lithium ions, reduce costs and improve economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023089238_24102024_PF_FP_ABST
    Figure CN2023089238_24102024_PF_FP_ABST
Patent Text Reader

Abstract

An electrochemical deintercalation-based lithium extraction method, relating to the technical field of electrochemical deintercalation-based lithium extraction. The method comprises: adding a solution waiting for lithium extraction containing Li+ and Mg2+ into a cathode chamber of an electrochemical deintercalation-based lithium extraction device, wherein Mg(OH)2 in said solution reaches a nearly saturated concentration, the electrochemical deintercalation-based lithium extraction device further comprises an anode chamber, an anion exchange membrane is arranged between the anode chamber and the cathode chamber, a cathode containing a lithium-deficient lithium ion sieve is provided in the cathode chamber, and an anode containing a lithium-intercalated lithium ion sieve is provided in the anode chamber; powering on and maintaining a voltage unchanged, so that the lithium-deficient lithium ion sieve adsorbs Li+; and powering off, exchanging the positions of the anode and the cathode, and powering on again and maintaining the voltage unchanged, so that the lithium-intercalated lithium ion sieve desorbs Li+ to obtain a lithium-rich solution.
Need to check novelty before this filing date? Find Prior Art

Description

A lithium extraction method by electrochemical deintercalation Technical Field

[0001] The present disclosure relates to the technical field of electrochemical deintercalation and lithium extraction, and in particular to a method for extracting lithium by electrochemical deintercalation. Background Art

[0002] Due to its unique properties, lithium metal has found widespread application in various fields, including new energy, aerospace, and the military industry. Lithium-ion batteries, currently the most widely used new energy battery, are widely used in mobile devices, electric vehicles, and energy storage. However, the uneven distribution of lithium mineral resources and the difficulty of mining them have limited the development of new energy batteries. Salt lake brines contain relatively abundant lithium resources, and therefore, extracting lithium from these brines has become a research hotspot.

[0003] Currently, the main processes used to extract lithium from salt lakes include precipitation, adsorption, solvent extraction, electrochemical deintercalation, and membrane separation. Among them, the use of manganese-based adsorbents to extract lithium from brine is a common method, but this method requires the use of acidic aqueous solutions for desorption, which consumes a lot of acid and base reagents and is a complicated process. The electrochemical deintercalation method has attracted the attention of researchers due to its advantages such as ease of operation, high efficiency, and environmental protection. However, in the process of electrochemical lithium extraction, coexisting cations, especially magnesium ions, can cause significant interference with the extraction of lithium. Therefore, how to avoid the cation rejection effect while ensuring the efficiency of lithium extraction has become a major difficulty in the process of electrochemical lithium extraction.

[0004] In view of this, the present disclosure is proposed.

[0005] Summary of the Invention

[0006] The purpose of the present disclosure is to provide a method for extracting lithium by electrochemical deintercalation, which can effectively avoid or reduce the cation repulsion effect that occurs during the lithium extraction process and improve the lithium extraction efficiency.

[0007] The present disclosure can be implemented as follows:

[0008] The present disclosure provides a method for extracting lithium by electrochemical deintercalation, comprising the following steps:

[0009] S1: Add the lithium solution to be extracted into the cathode chamber of the electrochemical deintercalation and extraction device. The lithium solution to be extracted contains Li + and Mg 2+ , and the Mg(OH)2 in the lithium solution to be extracted reaches a near saturated concentration;

[0010] The electrochemical deintercalation and lithium extraction device also includes an anode chamber, an anion exchange membrane is provided between the anode chamber and the cathode chamber; the cathode chamber has a cathode containing a lithium-deficient lithium ion sieve, and the anode chamber has an anode containing a lithium-intercalated lithium ion sieve;

[0011] S2: Turn on the power and keep the voltage constant, so that the lithium-poor lithium ion sieve undergoes a reduction reaction to adsorb Li in the lithium solution to be extracted + ;

[0012] S3: Stop the power supply, swap the positions of the anode and cathode, continue to power on and maintain the same voltage as in S2, so that the lithium-ion sieve in the lithium state undergoes oxidation reaction and desorbs Li + The lithium-poor state is then restored, and the desorbed lithium ions are used to form a lithium-rich solution in the anode chamber.

[0013] In an optional embodiment, the Mg in the lithium solution to be extracted is 2+ The concentration is 10mmol / L-100mmol / L, C Mg 2+ ×(C OH - ) 2 =1.60×10 -11 to 1.78×10 -11 .

[0014] In an optional embodiment, a recovery liquid is added into the anode chamber, and the recovery liquid is used to provide anions to form a lithium-rich solution together with the desorbed lithium ions.

[0015] In an optional embodiment, the recovery solution includes at least one of a sulfate salt solution and a chloride salt solution.

[0016] In an optional embodiment, the chloride salt solution includes at least one of a KCl solution and a NaCl solution; and / or the sulfate salt solution includes at least one of a K2SO4 solution and a Na2SO4 solution.

[0017] In an optional embodiment, the concentration of the cation in the recovered liquid is 0.2 mol / L-1 mol / L.

[0018] In an optional embodiment, in S3, when the lithium-poor lithium ion sieve changes from a lithium-poor state to a lithium-rich state, power is stopped and the positions of the anode and the cathode are swapped.

[0019] In an optional embodiment, the voltages in S2 and S3 are both 0.5V-1.0V, and in S3, when the current is as low as 0.2mA, power is stopped.

[0020] In an alternative embodiment, S2 and S3 are repeated 2-5 times in total.

[0021] In an optional embodiment, the lithium solution to be extracted is obtained by the following method

[0022] The pH value of the lithium-containing solution is adjusted by a regulator so that the Mg contained in the lithium-containing solution 2+Mg(OH)2 is formed and reaches a near saturated concentration, obtaining a lithium solution to be extracted.

[0023] In an optional embodiment, the lithium-containing liquid includes at least one of brine, seawater, waste battery leachate, lithium precipitation mother liquor and ore lithium extraction leachate.

[0024] In an alternative embodiment, the modifier is a - of soluble substances.

[0025] In an optional embodiment, the regulator includes at least one of sodium hydroxide, potassium hydroxide and ammonia water.

[0026] In an optional embodiment, while adding the regulator, the process also includes adding a flocculant to the lithium-containing solution.

[0027] In an optional embodiment, the flocculant includes at least one of starch, polyacrylamide, polyacrylic acid sodium salt and carboxymethyl cellulose sodium salt.

[0028] In an optional embodiment, the amount of flocculant added to the lithium-containing solution is 0.1 mg / L-5 mg / L.

[0029] In an optional embodiment, the lithium ion sieve includes at least one of lithium manganese phosphate, lithium titanate, lithium manganate, lithium iron phosphate and lithium manganese iron phosphate.

[0030] In an optional embodiment, the cathode is a first conductive current collector, which is loaded with a lithium-deficient lithium ion sieve; and / or the anode is a second conductive current collector, which is loaded with a lithium-intercalated lithium ion sieve.

[0031] In an optional embodiment, the first conductive current collector includes at least one of titanium mesh, graphite plate, carbon cloth, carbon paper, aluminum foil and copper foil; and / or the second conductive current collector includes at least one of titanium mesh, graphite plate, carbon cloth, carbon paper, aluminum foil and copper foil.

[0032] In an optional embodiment, the lithium-deficient lithium ion sieve is loaded on the surface of the first conductive current collector by coating; and / or the lithium-intercalated lithium ion sieve is loaded on the surface of the second conductive current collector by coating.

[0033] The present invention adjusts the Mg(OH)2 in the lithium solution to be extracted to a near saturated concentration before the electrochemical deintercalation treatment, so that the Mg near the electrode can be reduced during the electrochemical deintercalation treatment. 2+ Enrichment, forming a local low supersaturation (magnesium ions gather near the electrode to reach the local K sp >Magnesium hydroxide K sp), so that the small magnesium hydroxide crystals formed on the electrode due to cation enrichment tend to dissolve and fuse with the magnesium hydroxide crystals in the solution to form large-particle magnesium hydroxide crystals and settle, which can avoid or very small amounts of magnesium ions being adsorbed on the lithium-poor lithium ion sieve, thereby effectively avoiding the cation repulsion effect.

[0034] In S2, the lithium-poor lithium ion sieve undergoes a reduction reaction by connecting the power supply, and the high-valent metal ions contained therein are converted into low-valent metal ions. At the same time, the Li + It is adsorbed on the lithium-poor lithium ion sieve. Since the Mg(OH)2 in the lithium solution to be extracted reaches a near saturated concentration, it can form large-particle magnesium hydroxide crystals and settle during the electrochemical deintercalation process, thereby making the Mg near the electrode 2+ Concentration reduction, avoid Mg 2+ Opposition + Produces a cation repelling effect.

[0035] In S3, the lithium-ion sieve in the lithium-embedded state undergoes an oxidation reaction by connecting the power supply, and the corresponding low-valent metal ions are converted into high-valent metal ions. At the same time, Li + It is deintercalated and precipitated into the recovery liquid. + The anions on the side of the lithium solution to be extracted are attracted and can pass through the anion exchange membrane and enter the recovery liquid, so Li + It can be enriched in the recovered liquid.

[0036] The electrochemical deintercalation lithium extraction method provided in the present disclosure is simple to operate, can effectively avoid or reduce the cation rejection effect that occurs during the lithium extraction process, improve lithium extraction efficiency, reduce costs, and is conducive to improving economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present disclosure and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other relevant drawings can be obtained based on these drawings without creative work.

[0038] FIG1 is a flow chart of the lithium extraction method of the present disclosure using electrochemical deintercalation. DETAILED DESCRIPTION

[0039] To make the purpose, technical solutions, and advantages of the embodiments of the present disclosure more clear, the technical solutions in the embodiments of the present disclosure are described clearly and completely below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer were followed. Reagents or instruments used where the manufacturer is not specified are conventional products that can be purchased commercially.

[0040] The following is a detailed description of the electrochemical deintercalation method for lithium extraction provided by the present disclosure.

[0041] The present disclosure provides a method for extracting lithium by electrochemical deintercalation, referring to FIG1 , comprising the following steps:

[0042] S1: Add the lithium solution to be extracted into the cathode chamber of the electrochemical deintercalation and extraction device. The lithium solution to be extracted contains Li + and Mg 2+ , and the Mg(OH)2 concentration in the lithium solution to be extracted reaches nearly saturated concentration.

[0043] Mg in the above lithium solution 2+ The concentration of Mg can be, for example, 10mmol / L-100mmol / L, such as 10mmol / L, 20mmol / L, 30mmol / L, 40mmol / L, 50mmol / L, 60mmol / L, 70mmol / L, 80mmol / L, 90mmol / L or 100mmol / L, or any other value within the range of 10mmol / L-100mmol / L. That is, the method provided by the present disclosure is superior to other Mg 2+ The concentration range is more suitable for Mg 2+ The concentration of cation-repelling agent is 10mmol / L-100mmol / L to show a more obvious effect of avoiding the cation exclusion effect.

[0044] In addition, in some other embodiments, the Mg in the lithium solution to be extracted is 2+ The concentration of Mg can also be less than 10mmol / L or greater than 100mmol / L, but the Mg content in the lithium solution to be extracted is 2+ The concentration of Mg in the lithium solution to be extracted is less than 10mmol / L, and the cation exclusion effect is not obvious. 2+ If the concentration is greater than 100mmol / L, it may increase the difficulty and cost of treatment.

[0045] In the present disclosure, the fact that Mg(OH)2 in the lithium solution to be extracted reaches a near saturated concentration can be understood as the fact that C Mg 2+ ×(C OH - ) 2 =1.60×10 -11to 1.78×10 -11 , where C OH - Corresponding to the pH value, it can be directly measured using a pH detection instrument.

[0046] It should be noted that by adjusting the Mg(OH)2 in the lithium solution to be extracted to a near saturated concentration before the electrochemical deintercalation treatment, the Mg near the electrode can be reduced during the electrochemical deintercalation treatment. 2+ Enrichment, forming a local low supersaturation (magnesium ions gather near the electrode to reach the local K sp >Magnesium hydroxide K sp ), so that the small magnesium hydroxide crystals formed on the electrode due to cation enrichment tend to dissolve and fuse with the magnesium hydroxide crystals in the solution to form large-particle magnesium hydroxide crystals and settle, which can avoid or very small amounts of magnesium ions being adsorbed on the lithium-poor lithium ion sieve, thereby effectively avoiding the cation repulsion effect.

[0047] In some embodiments, the lithium solution to be extracted can be obtained by the following method: using a regulator to adjust the pH value of the lithium-containing solution so that the Mg contained in the lithium-containing solution is 2+ Mg(OH)2 is formed and reaches a near saturated concentration, obtaining a lithium solution to be extracted.

[0048] For reference, the lithium-containing liquid may include at least one of brine, seawater, waste battery leachate, lithium precipitation mother liquor and ore lithium extraction leachate.

[0049] The pH value of the lithium-containing solution is adjusted by a regulator (in this process, the pH value can be measured by a pH measuring instrument, so that the corresponding C OH - ) so that its corresponding C OH - Able to meet C Mg 2+ ×(C OH - ) 2 =1.60×10 -11 to 1.78×10 -11 .

[0050] As a reference, the above-mentioned regulator is a regulator that can provide OH - The soluble substance may include at least one of sodium hydroxide, potassium hydroxide and ammonia water.

[0051] In some optional embodiments, when the regulator is added, a flocculant is also added to the lithium-containing solution to further promote the sedimentation of the magnesium hydroxide.

[0052] For reference, the flocculant may include at least one of starch, polyacrylamide, sodium polyacrylate, and sodium carboxymethyl cellulose. The amount of the flocculant added to the lithium-containing solution may be 0.1 mg / L to 5 mg / L, such as 0.1 mg / L, 0.5 mg / L, 1 mg / L, 1.5 mg / L, 2 mg / L, 2.5 mg / L, 3 mg / L, 3.5 mg / L, 4 mg / L, 4.5 mg / L, or 5 mg / L, or any other value within the range of 0.1 mg / L to 5 mg / L.

[0053] If the amount of flocculant added is less than 0.1 mg / L, the effect of promoting the sedimentation of magnesium hydroxide is not obvious; if the amount of flocculant added exceeds 5 mg / L, the cost is increased and the lithium extraction efficiency is not improved.

[0054] Herein, the electrochemical deintercalation and lithium extraction device is an electrolytic cell or electrolytic tank, which, in addition to the above-mentioned cathode chamber, also includes an anode chamber, and an anion exchange membrane is provided between the anode chamber and the cathode chamber (to allow only anions to be exchanged); the cathode chamber has a cathode containing a lithium-poor lithium ion sieve (as a negative electrode), and the anode chamber has an anode containing a lithium-intercalated lithium ion sieve (as a positive electrode).

[0055] Herein, the anion exchange membrane may illustratively include a benzyl anion exchange membrane, a polyester anion exchange membrane, a polypropylene anion exchange membrane, a fluorocarbon-based anion exchange membrane, or the like.

[0056] The lithium ion sieve may illustratively include at least one of lithium manganese phosphate, lithium titanate, lithium manganate, lithium iron phosphate, and lithium manganese iron phosphate.

[0057] The cathode is a first conductive current collector, which is loaded with a lithium-deficient lithium ion sieve; the anode is a second conductive current collector, which is loaded with a lithium-intercalated lithium ion sieve.

[0058] The first conductive current collector may include at least one of titanium mesh, graphite plate, carbon cloth, carbon paper, aluminum foil, and copper foil. Similarly, the second conductive current collector may also include at least one of titanium mesh, graphite plate, carbon cloth, carbon paper, aluminum foil, and copper foil.

[0059] In some embodiments, the lithium-deficient lithium ion sieve can be loaded onto the surface of the first conductive current collector by coating. Similarly, the lithium-intercalated lithium ion sieve can be loaded onto the surface of the second conductive current collector by coating.

[0060] In other embodiments, the lithium ion sieve may be combined with the electrode in any other feasible manner.

[0061] In this paper, a recovery liquid is also added to the anode chamber to provide anions (such as Cl - or SO42- ) to form a lithium-rich solution together with the desorbed lithium ions.

[0062] For reference, the recovery solution may include at least one of a sulfate salt solution and a chloride salt solution. The chloride salt solution may include at least one of a KCl solution and a NaCl solution. - The sulfate solution may include at least one of K2SO4 solution and Na2SO4 solution, SO4 2- It can form a lithium-rich solution containing Li2SO4 together with the desorbed lithium ions.

[0063] In some embodiments, the concentration of the cation in the recovered liquid can be 0.2mol / L-1mol / L, such as 0.2mol / L, 0.3mol / L, 0.4mol / L, 0.5mol / L, 0.8mol / L or 1mol / L, etc., or it can be any other value within the range of 0.2mol / L-1mol / L.

[0064] If the concentration of cations in the recovered solution is lower than 0.2 mol / L, it will be able to react with Li + Too few cathode electrons are combined, affecting the Li + extraction rate; if the concentration of cations in the recovered liquid is higher than 1 mol / L, it will easily increase the difficulty of subsequent impurity removal.

[0065] It should be noted that the structure and working principle of the electrochemical deintercalation and lithium extraction device not further described in detail in the present disclosure can refer to existing related technologies (such as CN107201452B, etc.), and will not be described in detail here.

[0066] S2: Turn on the power and keep the voltage constant, so that the lithium-poor lithium ion sieve undergoes a reduction reaction to adsorb Li in the lithium solution to be extracted + .

[0067] In the above process, the voltage may be 0.5V-1.0V, such as being constant at 0.5V, 0.6V, 0.7V, 0.8V, 0.9V or 1.0V, or any other value within the range of 0.5V-1.0V.

[0068] When the voltage is less than 0.5V, the lithium extraction rate is too slow and the lithium extraction efficiency is low; if the voltage is greater than 1.0V, side reactions such as water electrolysis will occur.

[0069] In S2, by connecting a power source (such as a DC power source), the lithium-poor lithium ion sieve undergoes a reduction reaction, and the Fe 3+ or Mn 4+ High-valent metal ions such as Fe 2+ or Mn3+ At the same time, the Li + It is adsorbed on the lithium-poor lithium ion sieve. Since the Mg(OH)2 in the lithium solution to be extracted reaches a near saturated concentration, it can form large-particle magnesium hydroxide crystals and settle during the electrochemical deintercalation process, thereby making the Mg near the electrode 2+ Concentration reduction, avoid Mg 2+ Opposition + Produces a cation repelling effect.

[0070] S3: Stop the power supply, swap the positions of the anode and cathode, continue to power on and maintain the same voltage as in S2, so that the lithium-ion sieve in the lithium state undergoes oxidation reaction and desorbs Li + The lithium-poor state is then restored, and the desorbed lithium ions are used to form a lithium-rich solution in the anode chamber.

[0071] In S3, by connecting a power source (such as a DC power source), the lithium-ion sieve in the lithium-embedded state undergoes an oxidation reaction, and the corresponding Fe 2+ or Mn 3+ The low-valent metal ions are converted into Fe 3+ or Mn 4+ High valence metal ions, at the same time, Li + It is deintercalated and precipitated into the recovery liquid. + Cannot pass through the anion exchange membrane, and the anions on the side of the lithium solution to be extracted (such as Cl - etc.) are attracted to pass through the anion exchange membrane and enter the recovery liquid, so Li + It can be enriched in the recovery liquid in the form of LiCl, etc.

[0072] In some embodiments, once the lithium-deficient lithium ion sieve transitions from a lithium-deficient state to a lithium-rich state, the power supply can be stopped and the positions of the anode and cathode can be swapped. Based on the voltage and ion concentration of the lithium solution to be extracted, in some specific embodiments, the power supply can be stopped when the current drops to as low as 0.2 mA. Under these current conditions, the lithium-deficient lithium ion sieve described herein substantially transitions from a lithium-deficient state to a lithium-rich state.

[0073] In some embodiments, the entire electrochemical deintercalation and lithium extraction process can be repeated 2-5 times, such as 2, 3, 4, or 5 times. In addition, it is not excluded that the process can be repeated only once or more than 5 times. Repeating S2 and S3 2-5 times can achieve a higher lithium ion extraction efficiency.

[0074] The features and performance of the present disclosure are further described in detail below with reference to the embodiments.

[0075] Example 1

[0076] This embodiment provides a method for extracting lithium by electrochemical deintercalation, which includes the following steps:

[0077] S1: Determination of Mg in lithium-containing liquid (brine) 2+ The pH of the brine solution was adjusted to 9.27 using a regulator (ammonia water) to make the Mg(OH)2 concentration reach near saturation. Obtain the lithium solution to be extracted.

[0078] The electrochemical deintercalation and lithium extraction device (electrolyzer) used in this embodiment includes a cathode chamber and an anode chamber, and an anion exchange membrane (polypropylene anion exchange membrane) is provided between the anode chamber and the cathode chamber to separate the cathode chamber and the anode chamber; the cathode chamber has an aluminum foil as a cathode, and the aluminum foil is coated with a lithium-poor lithium ion sieve (lithium iron phosphate); the anode chamber has an aluminum foil as an anode, and the aluminum foil is coated with a lithium-intercalated lithium ion sieve (lithium iron phosphate).

[0079] The Mg(OH)2 solution to be extracted is added to the cathode chamber, and the recovery solution (sodium chloride aqueous solution, Na in the sodium chloride aqueous solution) is added to the anode chamber. + concentration is 1 mol / L).

[0080] S2: Direct current is applied and a constant voltage of 0.7V is maintained to extract lithium, causing the lithium-poor lithium ion sieve to undergo a reduction reaction and adsorb Li in the lithium solution to be extracted. + , when the current is as low as 0.2mA, the reaction stops.

[0081] S3: Switch the cathode and anode, continue to energize and maintain the same voltage as in S2, so that the lithium-ion sieve in the lithium state undergoes oxidation reaction and desorbs Li + The battery then returns to a lithium-poor state, and the desorbed lithium ions accumulate in the anode chamber.

[0082] S4: Repeat the above steps S2 and S3 three times to obtain a lithium-rich solution.

[0083] The lithium ion concentration in the final lithium-rich solution was measured and the result was 13.52 mmol / L.

[0084] Example 2

[0085] The only difference between this embodiment and embodiment 1 is that 0.5 mg / L of flocculant (polyacrylamide) is added to the brine at the same time as ammonia water.

[0086] The concentration of lithium ions in the lithium-rich liquid finally obtained in this example is 13.68 mmol / L.

[0087] Example 3

[0088] The only difference between this embodiment and embodiment 1 is that the Mg content in the lithium-containing liquid (brine) is 2+ The concentration is 10mmol / L, and Mg(OH)2 reaches a near saturation concentration by adding ammonia water Obtain the lithium solution to be extracted.

[0089] The concentration of lithium ions in the lithium-rich liquid finally obtained in this example is 13.47 mmol / L.

[0090] Example 4

[0091] The only difference between this embodiment and embodiment 1 is that the Mg content in the lithium-containing liquid (brine) is 2+ The concentration is 100mmol / L, and Mg(OH)2 reaches a near saturation concentration by adding ammonia water Obtain the lithium solution to be extracted.

[0092] The concentration of lithium ions in the lithium-rich liquid finally obtained in this example is 13.51 mmol / L.

[0093] Example 5

[0094] The only difference between this embodiment and embodiment 1 is that the regulator is NaOH solution.

[0095] The concentration of lithium ions in the lithium-rich liquid finally obtained in this example is 13.52 mmol / L.

[0096] Example 6

[0097] The only difference between this embodiment and embodiment 1 is that the regulator is a KOH solution.

[0098] The concentration of lithium ions in the lithium-rich liquid finally obtained in this example is 13.51 mmol / L.

[0099] Example 7

[0100] The only difference between this embodiment and embodiment 1 is that the lithium ion sieves loaded on the cathode and the anode are both lithium manganese phosphate.

[0101] The concentration of lithium ions in the lithium-rich liquid finally obtained in this example is 13.36 mmol / L.

[0102] Example 8

[0103] The only difference between this embodiment and embodiment 1 is that the lithium ion sieves loaded on the cathode and the anode are both lithium titanate.

[0104] The concentration of lithium ions in the lithium-rich liquid finally obtained in this example is 13.17 mmol / L.

[0105] Example 9

[0106] The only difference between this embodiment and embodiment 1 is that the lithium ion sieves loaded on the cathode and the anode are both lithium manganese oxide.

[0107] The concentration of lithium ions in the lithium-rich liquid finally obtained in this example is 13.28 mmol / L.

[0108] Example 10

[0109] The only difference between this embodiment and embodiment 1 is that the lithium ion sieves loaded on the cathode and the anode are both lithium manganese iron phosphate.

[0110] The concentration of lithium ions in the lithium-rich liquid finally obtained in this example is 13.27 mmol / L.

[0111] Example 11

[0112] The only difference between this embodiment and embodiment 1 is that the first conductive current collector and the second conductive current collector are both titanium meshes. The concentration of lithium ions in the lithium-rich solution finally obtained in this embodiment is 13.46 mmol / L.

[0113] Example 12

[0114] The only difference between this embodiment and embodiment 1 is that both the first conductive current collector and the second conductive current collector are graphite plates.

[0115] The concentration of lithium ions in the lithium-rich liquid finally obtained in this example is 13.42 mmol / L.

[0116] Example 13

[0117] The only difference between this embodiment and embodiment 1 is that both the first conductive current collector and the second conductive current collector are carbon cloth.

[0118] The concentration of lithium ions in the lithium-rich liquid finally obtained in this example is 13.38 mmol / L.

[0119] Example 14

[0120] The only difference between this embodiment and embodiment 1 is that the recovery liquid is a KCl aqueous solution, and the K + The concentration is 0.2mol / L.

[0121] The concentration of lithium ions in the lithium-rich liquid finally obtained in this example is 13.41 mmol / L.

[0122] Example 15

[0123] The only difference between this embodiment and embodiment 1 is that the recovered liquid is a Na2SO4 aqueous solution, and the Na + The concentration is 0.5mol / L.

[0124] The concentration of lithium ions in the lithium-rich liquid finally obtained in this example is 13.42 mmol / L.

[0125] Example 16

[0126] The only difference between this embodiment and embodiment 1 is that the recovery liquid is a K2SO4 aqueous solution.

[0127] The concentration of lithium ions in the lithium-rich liquid finally obtained in this example is 13.39 mmol / L.

[0128] Example 17

[0129] The only difference between this embodiment and embodiment 2 is that the flocculant is starch.

[0130] The concentration of lithium ions in the lithium-rich liquid finally obtained in this example is 13.63 mmol / L.

[0131] Example 18

[0132] The only difference between this embodiment and embodiment 2 is that the flocculant is sodium polyacrylate.

[0133] The concentration of lithium ions in the lithium-rich liquid finally obtained in this example is 13.61 mmol / L.

[0134] Example 19

[0135] The only difference between this embodiment and embodiment 2 is that the flocculant is sodium carboxymethyl cellulose.

[0136] The concentration of lithium ions in the lithium-rich liquid finally obtained in this example is 13.64 mmol / L.

[0137] Example 20

[0138] The only difference between this embodiment and embodiment 2 is that the amount of flocculant added to the lithium-containing liquid is 0.1 mg / L.

[0139] The concentration of lithium ions in the lithium-rich solution finally obtained in this example is 13.54 mmol / L.

[0140] Example 21

[0141] The only difference between this embodiment and embodiment 2 is that the amount of flocculant added to the lithium-containing liquid is 5 mg / L.

[0142] The concentration of lithium ions in the lithium-rich solution finally obtained in this example is 13.59 mmol / L.

[0143] Example 22

[0144] The only difference between this embodiment and embodiment 2 is that the voltage is kept constant at 0.5V.

[0145] The concentration of lithium ions in the lithium-rich solution finally obtained in this example is 13.38 mmol / L.

[0146] Example 23

[0147] The only difference between this embodiment and embodiment 2 is that the voltage is kept constant at 1.0V.

[0148] The concentration of lithium ions in the lithium-rich solution finally obtained in this example is 13.56 mmol / L.

[0149] Comparative Example 1

[0150] The difference between this comparative example and Example 1 is that the pH value of the lithium-containing solution was not adjusted before the electrochemical deintercalation treatment, and the lithium-containing solution (Mg(OH)2 did not reach a near-saturated concentration) was directly used as the lithium solution to be extracted for electrochemical deintercalation treatment.

[0151] The concentration of lithium ions in the lithium-rich liquid finally obtained in this comparative example is 10.49 mmol / L.

[0152] Comparative Example 2

[0153] The difference between this comparative example and Example 2 is that during the preparation of the lithium solution to be extracted, no regulator was added to the lithium-containing solution, but only a flocculant was added.

[0154] The concentration of lithium ions in the lithium-rich liquid finally obtained in this comparative example is 9.11 mmol / L.

[0155] Comparative Example 3

[0156] The difference between this comparative example and Example 2 is that the amount of flocculant added to the lithium-containing liquid is 0.05 mg / L.

[0157] The concentration of lithium ions in the lithium-rich liquid finally obtained in this comparative example is 11.38 mmol / L.

[0158] In summary, the electrochemical deintercalation lithium extraction method provided by the present disclosure is simple to operate, can effectively avoid or reduce the cation rejection effect that occurs during the lithium extraction process, improve lithium extraction efficiency, reduce costs, and is conducive to improving economic benefits.

[0159] The above are merely preferred embodiments of the present disclosure and are not intended to limit the present disclosure. Those skilled in the art will readily appreciate that various modifications and variations of the present disclosure are possible. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present disclosure shall be included within the scope of protection of the present disclosure. Industrial Applicability

[0160] The electrochemical deintercalation lithium extraction method provided in the present disclosure is simple to operate, can effectively avoid or reduce the cation rejection effect that occurs during the lithium extraction process, improve lithium extraction efficiency, reduce costs, and is conducive to improving economic benefits.

Claims

1. A lithium extraction method by electrochemical deintercalation, characterized in that: The following steps are involved: S1: Add the lithium solution to be extracted into the cathode chamber of the electrochemical lithium extraction device, and the lithium solution to be extracted contains Li + and Mg 2+ , and the Mg(OH)2 in the lithium solution to be extracted reaches a near saturation concentration; The electrochemical deintercalation and lithium extraction device also includes an anode chamber, an anion exchange membrane is provided between the anode chamber and the cathode chamber; the cathode chamber has a cathode containing a lithium-deficient lithium ion sieve, and the anode chamber has an anode containing a lithium-intercalated lithium ion sieve; S2: Turn on the power and keep the voltage constant, so that the lithium-poor lithium ion sieve undergoes a reduction reaction to adsorb Li in the lithium solution to be extracted + ; S3: Stop the power supply, swap the positions of the anode and the cathode, continue to supply power and maintain the same voltage as in S2, so that the lithium-ion sieve in the lithium-embedded state undergoes oxidation reaction to desorb Li + The battery is then restored to a lithium-poor state, and the desorbed lithium ions are used to form a lithium-rich solution in the anode chamber.

2. The lithium extraction method according to claim 1, characterized in that: The Mg in the lithium solution to be extracted 2+ The concentration is 10mmol / L-100mmol / L, C Mg 2+ ×(C OH - ) 2 =1.60×10 -11 to 1.78×10 -11 .

3. The lithium extraction method according to claim 1 or 2, characterized in that: A recovery liquid is added into the anode chamber, and the recovery liquid is used to provide anions to form a lithium-rich solution together with the desorbed lithium ions.

4. The lithium extraction method according to claim 3, characterized in that: The recovery solution includes at least one of a sulfate salt solution and a chloride salt solution.

5. The lithium extraction method according to claim 4, characterized in that: The chloride salt solution includes at least one of a KCl solution and a NaCl solution; and / or, the sulfate salt solution includes at least one of a K2SO4 solution and a Na2SO4 solution.

6. The lithium extraction method according to claim 4 or 5, characterized in that: The concentration of the cation in the recovery liquid is 0.2 mol / L-1 mol / L.

7. The lithium extraction method according to any one of claims 1 to 6, characterized in that: In S3, when the lithium-deficient lithium ion sieve changes from a lithium-deficient state to a lithium-rich state, power is stopped and the positions of the anode and the cathode are swapped.

8. The lithium extraction method according to claim 7, characterized in that: The voltages in S2 and S3 are both 0.5V-1.0V. In S3, when the current drops to 0.2mA, power is stopped.

9. The lithium extraction method according to any one of claims 1 to 8, characterized in that: Repeat S2 and S3 as a whole 2-5 times.

10. The lithium extraction method according to any one of claims 1 to 9, characterized in that: The lithium solution to be extracted is obtained by the following method: The pH value of the lithium-containing solution is adjusted by a regulator so that the Mg contained in the lithium-containing solution 2+ Mg(OH)2 is formed and reaches a near saturated concentration, obtaining a lithium solution to be extracted.

11. The lithium extraction method according to claim 10, characterized in that: The lithium-containing liquid comprises at least one of brine, seawater, waste battery leaching solution, lithium precipitation mother liquor and ore lithium extraction leaching solution.

12. The lithium extraction method according to claim 10, characterized in that: The regulator can provide OH - of soluble substances.

13. The lithium extraction method according to claim 12, characterized in that: The regulator includes at least one of sodium hydroxide, potassium hydroxide and ammonia water.

14. The lithium extraction method according to any one of claims 10 to 13, characterized in that: The method also includes adding a flocculant into the lithium-containing liquid while adding the regulator.

15. The lithium extraction method according to claim 14, characterized in that: The flocculant includes at least one of starch, polyacrylamide, polyacrylic acid sodium salt and carboxymethyl cellulose sodium salt.

16. The lithium extraction method according to claim 14 or 15, characterized in that: The amount of the flocculant added to the lithium-containing liquid is 0.1 mg / L-5 mg / L.

17. The lithium extraction method according to any one of claims 1 to 16, characterized in that: The lithium ion sieve includes at least one of lithium manganese phosphate, lithium titanate, lithium manganate, lithium iron phosphate and lithium iron manganese phosphate.

18. The lithium extraction method according to any one of claims 1 to 17, characterized in that: The cathode is a first conductive current collector, which is loaded with a lithium-deficient lithium ion sieve; and / or the anode is a second conductive current collector, which is loaded with a lithium-embedded lithium ion sieve.

19. The lithium extraction method according to claim 18, characterized in that: The first conductive current collector includes at least one of titanium mesh, graphite plate, carbon cloth, carbon paper, aluminum foil and copper foil; and / or the second conductive current collector includes at least one of titanium mesh, graphite plate, carbon cloth, carbon paper, aluminum foil and copper foil.

20. The lithium extraction method according to claim 19, characterized in that: The lithium-deficient lithium ion sieve is loaded on the surface of the first conductive current collector by coating; and / or the lithium-intercalated lithium ion sieve is loaded on the surface of the second conductive current collector by coating.

Citation Information

Patent Citations

  • Method and device for separating magnesium and lithium and enriching lithium from salt lake brine

    CN102382984A

  • Electrochemical de-intercalation and lithium extraction method and electrochemical de-intercalation and lithium extraction system

    CN115772609A

  • Process for extraction and production of lithium salt products from brine

    US20200283921A1

  • Method for lithium processing

    US20210207240A1

  • System and process for enriching lithium from seawater

    WO2022157624A1

Cited By

  • Electroactive membrane protection assembly and lithium extraction device

    CN122828570A