Photosensitive polyimide precursor composition
By introducing multi-arm compounds with specific structures and free radical polymerization monomers into the photosensitive polyimide precursor composition, the problem of insufficient performance of traditional photosensitive polyimide materials during low-temperature curing is solved and high photolithography resolution is achieved. efficiency and excellent mechanical properties to meet high-density packaging requirements.
Patent Information
- Application Number
- PCT/CN2023/089831
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-19
- Filing Date
- 2023-04-21
- Publication Date
- 2024-10-24
AI Technical Summary
Traditional photosensitive polyimide materials have insufficient imidization due to low-temperature curing in high-density fan-out wafer-level packaging, poor mechanical properties, and poor chemical corrosion resistance, and the introduction of small molecule additives may cause photolithography Performance degradation and reliability issues.
A photosensitive polyimide precursor composition is used, including polyamic acid ester, a multi-arm structural compound containing an azole structure, a free radical polymerization monomer, a photoinitiator, a silane coupling agent and a polymerization inhibitor. The combination of structure and proportion, after low-temperature curing, obtains a polyimide cured film with excellent mechanical properties, good chemical resistance, and strong bonding force to the copper surface.
It achieves high lithography resolution, excellent mechanical properties, good chemical resistance and copper surface bonding at low temperatures, meets the application requirements of high-density fan-out wafer-level packaging, and avoids the introduction of small molecule additives. Disadvantages such as migration and venting issues.
Smart Images

Figure CN2023089831_24102024_PF_FP_ABST
Abstract
Description
A photosensitive polyimide precursor composition Technical Field
[0001] The present invention belongs to the technical field of semiconductor devices, specifically relates to the technical field of polyimides, and in particular relates to a photosensitive polyimide precursor composition. Background Art
[0002] Semiconductor devices are widely used in the manufacture of various electronic products, such as computers, mobile phones, digital cameras, and other electronic devices. With the development trend of semiconductor chip packaging towards high integration, miniaturization, and portability, the density requirements for package wiring are getting higher and higher. In order to have higher density wiring on the same package area, the line width and line spacing of the wiring need to be greatly reduced. In advanced semiconductor chip packaging (such as wafer-level packaging and fan-out packaging), the wiring layer is usually composed of a patterned polyimide dielectric layer and a metal filled and embedded therein. The accuracy and density of the patterning of the polyimide dielectric layer determine the density of the wiring layer.
[0003] Photosensitive polyimide (PSPI) materials possess the excellent heat resistance, chemical resistance, dielectric, and mechanical properties of polyimide (PI), and can also be used as photolithography materials. Therefore, they are widely used in surface passivation of integrated circuit chips and surface rewiring processes for wafer-level and panel-level packaging, making them a key material in wafer-level advanced packaging processes. Traditional PSPI materials require a curing temperature above 350°C to achieve the various excellent properties of polyimide materials. However, such high curing temperatures can easily lead to packaging compatibility issues such as wafer warpage and stress cracking in advanced packaging processes such as high-density fan-out wafer-level packaging. Therefore, PSPI needs to meet the requirements of lower curing temperatures. However, low-temperature curing PSPI materials often encounter problems such as insufficient imidization, resulting in poor mechanical properties and poor chemical corrosion resistance, which cannot meet the requirements of the packaging process, or poor adhesion with other materials in the packaging process, especially electroplated copper, resulting in poor device reliability.
[0004] In order to solve the above problems, people will introduce light / heat base generating agents in order to reduce the activation of imidization of polyimide precursor resin to achieve polyimide resin with excellent performance in all aspects under low temperature process, such as the technical solutions in patents CN112639616A, CN112513219A, CN112639615A, and CN111919172A. Or the molecular weight of the precursor resin is controlled so that the molecular chain obtains sufficiently high mobility during low temperature curing to increase the imidization rate, such as CN108475020A. Other solutions, such as the introduction of polymers containing carbamate and urea bond structures in CN112334833A, and the introduction of polymers containing sulfite structures in CN110741318A and CN113168093A, can obtain low temperature curing with a high imidization rate, good chemical resistance, and excellent copper surface adhesion. In addition, in order to improve the bonding strength between the redistribution layer and the copper surface, various small molecule copper surface additives are generally introduced, such as CN102375336B and CN112799281A.
[0005] By introducing light / heat base generators to promote the low-temperature imidization effect of PSPI or introducing copper surface additives to achieve excellent copper surface adhesion, the introduced additives are often small molecule free additives. When these additives are used in large quantities, they will have a significant adverse effect on the photolithography performance of PSPI. The residue of small molecule additives in the cured film is likely to cause outgassing problems in the later multi-layer structure process, or migration during long-term reliability testing, which will adversely affect reliability.
[0006] Summary of the Invention
[0007] In response to the above technical problems, the present invention provides a photosensitive polyimide precursor composition that can be cured at low temperature (below 260°C), and after curing, it has excellent mechanical properties, good chemical resistance, and excellent bonding strength with copper surfaces, thereby meeting the application requirements of advanced packaging processes such as high-density fan-out wafer-level packaging.
[0008] To achieve the above object, the technical solution adopted by the present invention is:
[0009] In one aspect, the present invention provides a photosensitive polyimide precursor composition comprising:
[0010] 100 parts by mass of polyamic acid ester as a photosensitive polyimide precursor;
[0011] 0.1-10 parts by mass of a multi-arm structure compound containing an azole structure;
[0012] 1-20 parts by mass of a free radical polymerization monomer;
[0013] 0.5-10 parts by mass of a photoinitiator;
[0014] 0.5-10 parts by mass of a silane coupling agent;
[0015] 0.01-5 parts by mass of a polymerization inhibitor;
[0016] 50-1500 parts by mass of an organic solvent;
[0017] The multi-arm structure compound containing an azole structure is a compound in which an azole structure Z1 is bonded to a multi-arm unit Z2;
[0018] The azole structure Z1 is selected from any one or more of the following structures:
[0019] The multi-arm unit Z2 is selected from any one or more of the following structures:
[0020] As a preferred embodiment, the polyamic acid ester has a structure as shown in formula (I):
[0021] In formula (I), X is a tetravalent organic group containing an aromatic group, Y is a divalent organic group containing an aromatic group, R1 and R2 are independently selected from monovalent organic groups having a structure as shown in formula (II), and n is 2 to 150;
[0022] In formula (II), R3, R4 and R5 are independently selected from hydrogen atom and alkyl group having 1 to 3 carbon atoms; m is 2 to 10.
[0023] In the technical solution of the present invention, the free radical polymerization monomer is preferably any one or more of (meth)acrylate compounds, and more preferably any one or more of difunctional (meth)acrylate compounds and trifunctional (meth)acrylate compounds; in the technical solution of the present invention, the (meth)acrylate compounds include acrylate compounds and / or methacrylate compounds;
[0024] Specifically, the free radical polymerization monomer is selected from tetraethylene glycol dimethacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylic acid, trimethylolpropane diacrylate, trimethylolpropane triacrylate, trimethylolpropane dimethacrylate, trimethylolpropane trimethacrylate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, 1,4-butanediol dimethacrylate, 1,6-hexanediol dimethacrylate, At least one or more of acrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, pentaerythritol trimethacrylate, pentaerythritol tetramethacrylate, styrene, divinylbenzene, 4-vinyltoluene, 4-vinylpyridine, N-vinylpyrrolidone, 2-hydroxyethyl methacrylate, 2-hydroxyethyl acrylate, 1,3-acryloyloxy-2-hydroxypropane, 1,3-methacryloyloxy-2-hydroxypropane, methylenebisacrylamide, N,N-dimethylacrylamide, and N-hydroxymethylacrylamide; preferably, tetraethylene glycol dimethacrylate.
[0025] As a preferred embodiment, the preparation method of the polyamic acid ester comprises the following steps:
[0026] A tetracarboxylic dianhydride containing an X group, an alcohol having a free radical polymerizable unsaturated double bond and / or a saturated aliphatic alcohol having 1 to 4 carbon atoms are reacted to prepare a partially esterified tetracarboxylic acid; and then the tetracarboxylic acid is subjected to amide polycondensation with a diamine containing a Y group.
[0027] The tetracarboxylic dianhydride containing the X group is not particularly limited, and specific examples thereof include pyromellitic anhydride, diphenyl ether-3,3',4,4'-tetracarboxylic dianhydride, benzophenone-3,3',4,4'-tetracarboxylic dianhydride, biphenyl-3,3',4,4'-tetracarboxylic dianhydride, diphenylsulfone-3,3',4,4'-tetracarboxylic dianhydride, diphenylmethane-3,3',4,4'-tetracarboxylic dianhydride, 2,2-bis(3,4-phthalic anhydride)propane, 2,2-bis(3,4-phthalic anhydride)propane, and 2,2-bis(3,4-phthalic anhydride). -phthalic anhydride)-1,1,1,3,3,3-hexafluoropropane, etc., preferably pyromellitic anhydride, diphenyl ether-3,3',4,4'-tetracarboxylic dianhydride, benzophenone-3,3',4,4'-tetracarboxylic dianhydride, biphenyl-3,3',4,4'-tetracarboxylic dianhydride, more preferably pyromellitic anhydride, diphenyl ether-3,3',4,4'-tetracarboxylic dianhydride, biphenyl-3,3',4,4'-tetracarboxylic dianhydride, etc., the above can be used alone or in any combination.
[0028] The diamine containing the Y group is not particularly limited, and specific examples thereof include p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminobiphenyl, 3,4'-diaminobiphenyl, 3,3'-diaminobiphenyl, 4,4'-diaminobenzophenone, 3,4'-diaminobenzophenone, 3,3'-diaminobenzophenone, 4,4'-diaminodiphenylmethane, 3 ... '-Diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, 4,4-bis(4-aminophenoxy)biphenyl, 4,4-bis(3-aminophenoxy)biphenyl, bis[4-(4-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]ether, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 9,10-bis(4-aminophenyl)anthracene, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-aminophenyl)hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 1,4-bis(3-aminopropyldimethylsilyl)benzene, 3,3'-dimethyl-4,4'-diaminodiphenyl sulfone, 9,9-bis(4-aminophenyl)fluorene, etc., can be used alone or in any combination.
[0029] As a preferred embodiment, the photoinitiator is selected from any one or more of oxime ester compounds, benzophenone, N,N'-tetramethyl-4,4'-diaminobenzophenone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone, alkyl anthraquinone, benzoin alkyl ether, benzoin, alkyl benzoin and benzil dimethyl ketal, and is further preferably an oxime ester compound.
[0030] As a preferred embodiment, the organic solvent is selected from any one or more of esters, ethers, ketones, aromatic hydrocarbons, sulfoxides and amides;
[0031] Specifically, the solvent is selected from at least one of N,N-dimethylformamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N,N-dimethylacetamide, dimethyl sulfoxide, diethylene glycol dimethyl ether, cyclopentanone, γ-butyrolactone, α-acetyl-γ-butyrolactone, tetramethylurea, 1,3-dimethyl-2-imidazolidinone, N-cyclohexyl-2-pyrrolidone and an alcohol having an alcoholic hydroxyl group and no olefinic double bond in the molecule; the alcohol having an alcoholic hydroxyl group in the molecule The alcohol having a hydroxy group and not having an olefinic double bond is selected from any one or more of methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, tert-butanol, ethyl lactate, propylene glycol-1-methyl ether, propylene glycol-2-methyl ether, propylene glycol-1-ethyl ether, propylene glycol-2-ethyl ether, propylene glycol-1-(n-propyl) ether, propylene glycol-2-(n-propyl) ether, ethylene glycol methyl ether, ethylene glycol ethyl ether, ethylene glycol n-propyl ether, 2-hydroxyisobutyrate, ethylene glycol and propylene glycol.
[0032] In the technical solution of the present invention, the silane coupling agent is not particularly limited, and is preferably any one or more of the silane coupling agents containing a urea bond (-NH-CO-NH-);
[0033] Specifically, the silane coupling agent is selected from ureapropyl triethoxysilane, γ-aminopropyl dimethoxysilane, N-(β-aminoethyl)-γ-aminopropyl methyl dimethoxysilane, γ-glycidoxypropyl methyl dimethoxysilane, γ-mercaptopropyl methyl dimethoxysilane, 3-methacryloxypropyl dimethoxymethyl silane, 3-methacryloxypropyl trimethoxysilane, dimethoxymethyl-3-piperidinylpropyl silane, diethoxy-3-glycidoxypropyl methyl silane, N-(3-diethyl)- Any one or more of triethoxysilyl) propyl succinic anhydride, N-[3-(triethoxysilyl)propyl] phthalamic acid, benzophenone-3,3'-bis(N-[3-triethoxysilyl]propylamide)-4,4'-dicarboxylic acid, benzene-1,4-bis(N-[3-triethoxysilyl]propylamide)-2,5-dicarboxylic acid, 3-(triethoxysilyl)propyl succinic anhydride and N-phenylaminopropyltrimethoxysilane; preferably ureapropyltriethoxysilane.
[0034] In the technical solution of the present invention, the polymerization inhibitor is not particularly limited, and is preferably any one or more of the phenolic free radical polymerization inhibitors;
[0035] Specifically, the polymerization inhibitor is selected from any one or more of hydroquinone, N-nitrosodiphenylamine, p-tert-butylcatechol, phenothiazine, N-phenylnaphthylamine, ethylenediaminetetraacetic acid, 1,2-cyclohexanediaminetetraacetic acid, ethylene glycol ether diaminetetraacetic acid, 2,6-di-tert-butyl-p-methylphenol, 5-nitroso-8-hydroxyquinoline, 1-nitroso-2-naphthol, 2-nitroso-1-naphthol, 2-nitroso-5-(N-ethyl-N-sulfopropylamino)phenol, N-nitroso-N-phenylhydroxylamine ammonium salt and N-nitroso-N(1-naphthyl)hydroxylamine ammonium salt, preferably 2-nitroso-1-naphthol.
[0036] As a preferred embodiment, it further comprises 0.1-10 parts of a thermal base generating agent;
[0037] Preferably, the thermal base generator is a tert-butoxycarbonyl protected amine compound. In the technical solution of the present invention, the amine compound protected by the tert-butoxycarbonyl group is not particularly limited, and specific examples include ethanolamine, 3-amino-1-propanol, 1-amino-2-propanol, 2-amino-1-propanol, 4-amino-1-butanol, 2-amino-1-butanol, 1-amino-2-butanol, 3-amino-2,2-dimethyl-1-propanol, 4-amino- Amino-2-methyl-1-butanol, valinol, 3-amino-1,2-propanediol, 2-amino-1,3-propanediol, tyramine, norephedrine, 2-amino-1-phenyl-1,3-propanediol, 2-aminocyclohexanol, 4-aminocyclohexanol, 4-aminocyclohexaneethanol, 4-(2-aminoethyl)cyclohexanol, N-methylethanolamine, 3-(methylamino)-1-propanol, 3-(isopropylamino)propanol, N-cyclohexylethanolamine, α- [2-(Methylamino)ethyl]benzyl alcohol, diethanolamine, diisopropanolamine, 3-pyrrolidinol, 2-pyrrolidinemethanol, 4-hydroxypiperidine, 3-hydroxypiperidine, 4-hydroxy-4-phenylpiperidine, 4-(3-hydroxyphenyl)piperidine, 4-piperidinemethanol, 3-piperidinemethanol, 2-piperidinemethanol, 4-piperidineethanol, 2-piperidineethanol, 2-(4-piperidinyl)-2-propanol, 1,4-butanol bis(3-aminopropyl) ether, 1,2-bis(2- Any one or more of diaminoethyl)ethane, 2,2'-oxybisethylamine, 1,14-diamino-3,6,9,12-tetraoxatetradecane, 1-aza-15-crown-5-ether, diethylene glycol bis(3-aminopropyl) ether, 1,11-diamino-3,6,9-trioxaundecane and diethylene glycol bis(3-aminopropyl) ether; the tert-butoxycarbonyl-protected amine compound is further preferably N-tert-butoxycarbonyl-4-piperidinol.
[0038] In another aspect, the present invention provides a photosensitive polyimide composition obtained by thermal imidization of the photosensitive polyimide precursor composition. The thermal imidization temperature is preferably 150-400°C.
[0039] The above technical solution has the following advantages or beneficial effects:
[0040] The present invention introduces a multi-arm structure compound with a specific azole structure into a negative photosensitive polyamide ester composition. After low-temperature curing, a polyimide cured film with good lithography resolution, excellent mechanical properties, good chemical resistance, and excellent adhesion to the electroplated copper surface can be obtained, thereby meeting the application requirements of advanced packaging processes such as high-density fan-out wafer-level packaging.
[0041] Compared with the existing technical solution of introducing small molecule copper surface additives into polyamic acid ester compositions to enhance bonding strength, the present invention introduces a multi-arm structure compound with a specific azole structure, which increases the molecular weight of the additive, thereby helping to suppress the migration or outgassing problems that may be caused by small molecule residues. At the same time, due to the intramolecular pulling effect, the performance of the azole compound as a copper surface additive can be further enhanced, and better copper surface bonding strength can be obtained than that of small molecule copper surface additives. At the same time, the generation of copper surface gaps can be more effectively suppressed, thereby ensuring better reliability. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] FIG1 shows the chemical structures of CA-1 to CA-6 used in Production Example 2 of the present invention and the chemical structures of CA-7 to CA-10 used in Comparative Examples.
[0043] FIG2 is a table showing the components and contents, and the curing process of the polyamic acid ester compositions prepared in the examples and comparative examples of the present invention.
[0044] FIG3 is a table showing relevant performance test data of the polyamic acid ester compositions prepared in the examples and comparative examples of the present invention. DETAILED DESCRIPTION
[0045] The following embodiments are merely some of the embodiments of the present invention, rather than all of them. Therefore, the detailed description of the embodiments of the present invention provided below is not intended to limit the scope of the claimed invention, but rather merely represents selected embodiments of the present invention. All other embodiments derived by those skilled in the art based on the embodiments of the present invention without creative effort are intended to fall within the scope of protection of the present invention.
[0046] In the present invention, unless otherwise specified, all equipment and raw materials can be purchased from the market or are commonly used in the industry. The methods in the following embodiments, unless otherwise specified, are all conventional methods in the art.
[0047] The technical solution of the present invention is to design a photosensitive polyimide precursor composition, comprising:
[0048] (1) Polyamic acid ester as a precursor of photosensitive polyimide; (2) a multi-arm structure compound containing an azole structure; (3) a free radical polymerization monomer; and (4) a photoinitiator.
[0049] Component (1): Polyamic acid ester
[0050] In the technical solution of the present invention, polyamic acid ester is converted into polyimide by thermal imidization, and as the photosensitive polyimide precursor in the present invention, it has a structure as shown in formula (I):
[0051] (In formula (I), X is a tetravalent organic group containing an aromatic group, Y is a divalent organic group containing an aromatic group, R1 and R2 are each independently selected from a monovalent organic group having a structure as shown in formula (II), and n is 2 to 150);
[0052] (In formula (II), R3, R4 and R5 are independently selected from hydrogen atom and alkyl group having 1 to 3 carbon atoms; m is 2 to 10).
[0053] The tetracarboxylic dianhydride containing the X group is not particularly limited, and specific examples thereof include pyromellitic anhydride, diphenyl ether-3,3',4,4'-tetracarboxylic dianhydride, benzophenone-3,3',4,4'-tetracarboxylic dianhydride, biphenyl-3,3',4,4'-tetracarboxylic dianhydride, diphenylsulfone-3,3',4,4'-tetracarboxylic dianhydride, diphenylmethane-3,3',4,4'-tetracarboxylic dianhydride, 2,2-bis(3,4-phthalic anhydride)propane, 2,2-bis(3,4-phthalic anhydride)propane, and 2,2-bis(3,4-phthalic anhydride). -phthalic anhydride)-1,1,1,3,3,3-hexafluoropropane, etc., preferably pyromellitic anhydride, diphenyl ether-3,3',4,4'-tetracarboxylic dianhydride, benzophenone-3,3',4,4'-tetracarboxylic dianhydride, biphenyl-3,3',4,4'-tetracarboxylic dianhydride, more preferably pyromellitic anhydride, diphenyl ether-3,3',4,4'-tetracarboxylic dianhydride, biphenyl-3,3',4,4'-tetracarboxylic dianhydride, etc., the above can be used alone or in any combination.
[0054] The diamine containing the Y group is not particularly limited, and specific examples thereof include p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, -Diaminobenzidine, 3,4'-diaminobenzidine, 3,3'-diaminobenzidine, 4,4'-diaminobenzophenone, 3,4'-diaminobenzophenone, 3,3'-diaminobenzophenone, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene , bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, 4,4-bis(4-aminophenoxy)biphenyl, 4,4-bis(3-aminophenoxy)biphenyl, bis[4-(4-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]ether, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 9,10-bis(4-aminophenyl)anthracene, 2,2 -bis(4-aminophenyl)propane, 2,2-bis(4-aminophenyl)hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl)propane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 1,4-bis(3-aminopropyldimethylsilyl)benzene, 3,3'-dimethyl-4,4'-diaminodiphenyl sulfone, 9,9-bis(4-aminophenyl)fluorene, etc., which can be used alone or in any combination.
[0055] The alcohol having a radically polymerizable unsaturated double bond is not particularly limited, and specific examples thereof include 2-acryloyloxyethanol, 1-acryloyloxy-3-propanol, 2-acrylamidoethanol, hydroxymethyl vinyl ketone, 2-hydroxyethyl vinyl ketone, 2-hydroxy-3-methoxypropyl acrylate, 2-hydroxy-3-butoxypropyl acrylate, 2-hydroxy-3-phenoxypropyl acrylate, 2-hydroxy-3-butoxypropyl acrylate, 2-hydroxy-3-tert-butoxypropyl acrylate, 2-hydroxy-3-cyclohexyloxy Propyl acrylate, 2-methacryloyloxyethanol, 1-methacryloyloxy-3-propanol, 2-methacrylamidoethanol, 2-hydroxy-3-methoxypropyl methacrylate, 2-hydroxy-3-butoxypropyl methacrylate, 2-hydroxy-3-phenoxypropyl methacrylate, 2-hydroxy-3-butoxypropyl methacrylate, 2-hydroxy-3-tert-butoxypropyl methacrylate, 2-hydroxy-3-cyclohexyloxypropyl methacrylate, etc., can be used alone or in any combination.
[0056] The saturated aliphatic alcohols having 1 to 4 carbon atoms are not particularly limited, and specific examples thereof include methanol, ethanol, n-propanol, isopropanol, n-butanol, and tert-butanol. These alcohols may be used alone or in any combination.
[0057] Preparation of polyamic acid ester
[0058] In the technical solution of the present invention, the following method can be used to prepare the polyamic acid ester having the structure shown above:
[0059] A tetracarboxylic dianhydride containing an X group, an alcohol having a free radical polymerizable unsaturated double bond and / or a saturated aliphatic alcohol having 1 to 4 carbon atoms are reacted to prepare a partially esterified tetracarboxylic acid; and then the tetracarboxylic acid is subjected to amide polycondensation with a diamine containing a Y group.
[0060] The tetracarboxylic dianhydride and the alcohol are reacted in a suitable reaction solvent preferably in the presence of a basic catalyst such as pyridine at 20 to 50° C. for 4 to 10 hours with stirring to obtain a partially esterified tetracarboxylic acid.
[0061] The solvent used in the above reaction is preferably one that completely dissolves the reaction raw materials and / or products, and more preferably one that completely dissolves the photosensitive polyimide precursor. Specific examples of such solvents include N-methyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, tetramethylurea, ketones, esters, lactones, ethers, halogenated hydrocarbons, and hydrocarbons. These solvents may be used alone or in any combination.
[0062] The solution containing partially esterified tetracarboxylic acid obtained in the above reaction is preferably added with a dehydrating condensation agent under ice-cold conditions to obtain a polyanhydride, and then the above-mentioned diamine containing a Y group or its solution is added to obtain the target polyamic acid ester through amide polycondensation.
[0063] The dehydration condensation agent is not particularly limited, and specific examples thereof include dicyclohexylcarbodiimide, 1-ethoxycarbonyl-2-ethoxy-1,2-dihydroquinoline, 1,1-carbonyldioxy-di-1,2,3-benzotriazole, and N,N'-disuccinimidyl carbonate. These can be used alone or in any combination.
[0064] Component (2): Multi-arm structure compound containing azole structure
[0065] In the technical solution of the present invention, a multi-arm structure compound containing an azole structure is added to the photosensitive polyimide precursor composition, which increases the molecular weight of the azole copper surface additive, thereby suppressing the migration or exhaust problems that may be caused by small molecule residues. At the same time, due to the pulling effect within the molecule, the performance of the azole compound as a copper surface additive can be further enhanced, and better copper surface bonding strength can be obtained than that of small molecule copper surface additives. At the same time, the generation of copper surface gaps can be more effectively suppressed, thereby ensuring more excellent reliability. Z1 A compound bonded to the multi-arm unit Z2, wherein:
[0066] The azole structure Z1 is selected from any one or more of the following structures:
[0067] The multi-arm unit Z2 is selected from any one or more of the following structures:
[0068] In the technical solution of the present invention, the addition amount of the multi-arm structure compound containing an azole structure is 0.1-10 parts by mass based on 100 parts of polyamic acid ester from the perspective of improving the copper surface bonding strength. If the addition amount is less than 0.1 parts by mass, the effect of enhancing the copper surface bonding strength is limited. If the addition amount is greater than 10 parts, the mechanical properties of the cured film will be reduced and the photolithography performance will be damaged.
[0069] Component (3): Free radical polymerization monomer
[0070] The present invention further compounded a free radical polymerization monomer containing an unsaturated bond into the photosensitive polyimide precursor composition, which can undergo a free radical polymerization reaction with the free radical polymerizable substituent on the side chain of the polyamic acid ester.
[0071] As the above-mentioned free radical polymerization monomer, it is preferably any one or more of the (meth)acrylate compounds that can undergo free radical polymerization reaction under the action of a photoinitiator. In the technical solution of the present invention, the (meth)acrylate compounds include acrylate compounds and / or methacrylate compounds: including but not limited to mono(meth)acrylate or di(meth)acrylate of ethylene glycol or polyethylene glycol headed by diethylene glycol dimethacrylate and tetraethylene glycol dimethacrylate; mono(meth)acrylate or di(meth)acrylate of propylene glycol or polypropylene glycol; mono(meth)acrylate, di(meth)acrylate or tri(meth)acrylate of glycerol; cyclohexane di(meth)acrylate; diacrylate and dimethacrylate of 1,4-butanediol, di(meth)acrylate of 1,6-hexanediol; neopentyl Di(meth)acrylates of glycols; mono(meth)acrylates or di(meth)acrylates of bisphenol A; phenyl trimethacrylate; isobornyl(meth)acrylate; acrylamide and its derivatives; methacrylamide and its derivatives; trimethylolpropane tri(meth)acrylate; di(meth)acrylate or tri(meth)acrylate of glycerol; di(meth)acrylate, tri(meth)acrylate, or tetra(meth)acrylate of pentaerythritol; and compounds such as ethylene oxide or propylene oxide adducts of these compounds, and further preferably any one or more of difunctional (meth)acrylate compounds and trifunctional (meth)acrylate compounds.
[0072] Specific examples of the above-mentioned radical polymerization monomers include tetraethylene glycol dimethacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, trimethylolpropane diacrylate, trimethylolpropane triacrylate, trimethylolpropane dimethacrylate, trimethylolpropane trimethacrylate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, 1,4-butanediol dimethacrylate, and 1,6-hexanediol dimethacrylate. , pentaerythritol triacrylate, pentaerythritol tetraacrylate, pentaerythritol trimethacrylate, pentaerythritol tetramethacrylate, styrene, divinylbenzene, 4-vinyltoluene, 4-vinylpyridine, N-vinylpyrrolidone, 2-hydroxyethyl methacrylate, 2-hydroxyethyl acrylate, 1,3-acryloyloxy-2-hydroxypropane, 1,3-methacryloyloxy-2-hydroxypropane, methylenebisacrylamide, N,N-dimethylacrylamide, N-hydroxymethylacrylamide, etc., the above can be used alone or in any combination, preferably triethylene glycol dimethacrylate.
[0073] In the technical solution of the present invention, the amount of free radical polymerization monomer added is 1-20 parts by mass based on 100 parts of polyamic acid ester from the perspective of improving photolithographic resolution. If the amount is too low, it is not conducive to obtaining high photolithographic resolution, and if it is too high, it will reduce the chemical corrosion resistance of the cured film.
[0074] Component (4): Photoinitiator
[0075] The photoinitiator applicable to the present invention is not particularly limited, and specific examples include oxime ester compounds, benzophenone, N,N'-tetramethyl-4,4'-diaminobenzophenone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone, alkyl anthraquinone, benzoin alkyl ether, benzoin, alkyl benzoin and benzyl dimethyl ketal. The above can be used alone or in any combination, and oxime ester compounds are more preferred.
[0076] In the technical solution of the present invention, the amount of photoinitiator added is 0.1-10 parts by mass based on 100 parts of polyamic acid ester, considering the improvement of lithography resolution and the widening of lithography window. Too low a number will greatly reduce the residual film rate after development, while too high a number will easily lead to overexposure of lithography and thus make the lithography window significantly smaller.
[0077] Other components:
[0078] The photosensitive polyimide precursor composition of the present invention may further include components other than the above components.
[0079] The photosensitive polyimide precursor composition of the present invention can be prepared by dissolving the above-mentioned components and any optional ingredients added as needed in a solvent to form a liquid resin composition. Therefore, other components include a solvent. Other components include resins other than the above-mentioned components, silane coupling agents, polymerization inhibitors, and thermal base generators.
[0080] Component (5): organic solvent
[0081] In the technical solution of the present invention, the applicable solvent is not particularly limited, and can be specifically selected from any one or more of esters, ethers, ketones, aromatic hydrocarbons, sulfoxides and amides.
[0082] Based on the solubility of the polyimide precursor, polar solvents such as N,N-dimethylformamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N,N-dimethylacetamide, dimethyl sulfoxide, diethylene glycol dimethyl ether, cyclopentanone, γ-butyrolactone, α-acetyl-γ-butyrolactone, tetramethyl urea, 1,3-dimethyl-2-imidazolidinone and N-cyclohexyl-2-pyrrolidone are preferred. The above solvents can be used alone or in any combination.
[0083] Considering the stability of the photosensitive polyimide precursor composition, alcohols having an alcoholic hydroxyl group and no olefinic double bond in the molecule are preferred; specifically, alkyl alcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, and tert-butanol; lactic acid esters such as ethyl lactate; propylene glycol mono-1-methyl ether, propylene glycol-2-methyl ether, propylene glycol-1-ethyl ether, propylene glycol-2-ethyl ether, propylene glycol-1-(n-propyl) ether, propylene glycol-2-(n-propyl) ether, and the like. Alkyl ethers; monoalcohols such as ethylene glycol methyl ether, ethylene glycol ethyl ether, and ethylene glycol n-propyl ether; 2-hydroxyisobutyrates; any one or more of diols such as ethylene glycol and propylene glycol, preferably any one or more of lactates, propylene glycol monoalkyl ethers, 2-hydroxyisobutyrates, and ethanol, more preferably ethyl lactate, propylene glycol-1-methyl ether, propylene glycol-1-ethyl ether, and propylene glycol-1-(n-propyl) ether, etc., which can be used alone or in any combination.
[0084] In the technical solution of the present invention, the amount of the solvent used above can be determined according to the viscosity of the photosensitive polyimide precursor composition and the coating thickness requirement, for example, 50-1500 parts by mass based on 100 parts of polyamic acid ester.
[0085] Component (6): Silane coupling agent
[0086] In the technical solution of the present invention, adding a silane coupling agent to the photosensitive polyimide precursor composition can increase the bonding strength between the photosensitive polyimide precursor composition and the substrate.
[0087] The silane coupling agent used in the present invention is not particularly limited, and specific examples thereof include ureapropyltriethoxysilane, γ-aminopropyldimethoxysilane, N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, 3-methacryloxypropyldimethoxymethylsilane, 3-methacryloxypropyltrimethoxysilane, dimethoxymethyl-3-piperidinylpropylsilane, diethoxy-3-glycidoxypropylmethylsilane, N-(3-dimethoxypropyl)-1,2-dimethoxy ... Ethoxymethylsilylpropyl) succinimide, N-[3-(triethoxysilyl)propyl]phthalamic acid, benzophenone-3,3'-bis(N-[3-triethoxysilyl]propylamide)-4,4'-dicarboxylic acid, benzene-1,4-bis(N-[3-triethoxysilyl]propylamide)-2,5-dicarboxylic acid, 3-(triethoxysilyl)propylsuccinic anhydride and N-phenylaminopropyltrimethoxysilane, etc., which can be used alone or in any combination, are preferably ureapropyltriethoxysilane.
[0088] Preferably, the silane coupling agent is selected from any one or more silane coupling agents containing a urea bond (-NH-CO-NH-).
[0089] In the technical solution of the present invention, the amount of silane coupling agent added is 0.5-10 parts by mass based on 100 parts of polyamic acid ester in order to improve the adhesion of the silicon surface and the coating uniformity. If the amount is too low, the adhesion performance of the silicon surface will be poor, and if it is too high, the coating uniformity will be significantly damaged.
[0090] Component (7): Polymerization inhibitor
[0091] In the technical solution of the present invention, a polymerization inhibitor may be optionally added to increase the viscosity and stability of the photosensitive polyimide precursor composition during storage, especially when the composition contains a solvent. The polymerization inhibitor is not particularly limited, but is preferably any one or more phenolic free radical polymerization inhibitors. Specific examples of polymerization inhibitors suitable for the present invention include hydroquinone, N-nitrosodiphenylamine, p-tert-butylcatechol, phenothiazine, N-phenylnaphthylamine, ethylenediaminetetraacetic acid, 1,2-cyclohexanediaminetetraacetic acid, glycol ether diaminetetraacetic acid, 2,6-di-tert-butyl-p-methylphenol, 5-nitroso-8-hydroxyquinoline, 1-nitroso-2-naphthol, 2-nitroso-1-naphthol, 2-nitroso-5-(N-ethyl-N-sulfopropylamino)phenol, N-nitroso-N-phenylhydroxylamine ammonium salt, and N-nitroso-N(1-naphthyl)hydroxylamine ammonium salt. These can be used alone or in any combination, and 2-nitroso-1-naphthol is preferred.
[0092] In the technical solution of the present invention, the amount of polymerization inhibitor added is 0.005-12 parts by mass based on 100 parts of polyamic acid ester from the perspective of improving the storage stability of the glue. Too low an amount will destroy the storage stability of the glue, while too high an amount will destroy the photolithographic performance of the glue.
[0093] Component (8): thermal alkali generator
[0094] In the technical solution of the present invention, the photosensitive polyimide precursor composition may further include a thermal base generator, which can generate a base by heating and promote the imidization of the photosensitive polyimide precursor composition.
[0095] The thermal base generating agent applicable to the present invention is not particularly limited, and is preferably an amine compound protected by a tert-butoxycarbonyl group;
[0096] The amine compound protected by the tert-butoxycarbonyl group is not particularly limited, and specific examples thereof include ethanolamine, 3-amino-1-propanol, 1-amino-2-propanol, 2-amino-1-propanol, 4-amino-1-butanol, 2-amino-1-butanol, 1-amino-2-butanol, 3-amino-2,2-dimethyl-1-propanol, 4-amino-2-methyl-1-butanol, valinol, 3-amino-1,2-propanediol, 2-Amino-1,3-propanediol, tyramine, nomethylephedrine, 2-amino-1-phenyl-1,3-propanediol, 2-aminocyclohexanol, 4-aminocyclohexanol, 4-aminocyclohexaneethanol, 4-(2-aminoethyl)cyclohexanol, N-methylethanolamine, 3-(methylamino)-1-propanol, 3-(isopropylamino)propanol, N-cyclohexylethanolamine, α-[2-(methylamino)ethyl]benzyl alcohol, diethanolamine, diisopropanolamine, 3-Pyrrolidone, 2-pyrrolidonemethanol, 4-hydroxypiperidine, 3-hydroxypiperidine, 4-hydroxy-4-phenylpiperidine, 4-(3-hydroxyphenyl)piperidine, 4-piperidinol, 3-piperidinolmethanol, 2-piperidinolmethanol, 4-piperidinolethanol, 2-piperidinolethanol, 2-(4-piperidinyl)-2-propanol, 1,4-butanol bis(3-aminopropyl) ether, 1,2-bis(2-aminoethoxy)ethane, 2,2'-bis(2-aminoethoxy)ethane Ethylamine, 1,14-diamino-3,6,9,12-tetraoxatetradecane, 1-aza-15-crown-5-ether, diethylene glycol bis(3-aminopropyl) ether, 1,11-diamino-3,6,9-trioxaundecane, diethylene glycol bis(3-aminopropyl) ether, etc.; and compounds in which the amino groups of amino acids and their derivatives are protected by tert-butoxycarbonyl, etc., can be used alone or in any combination.
[0097] The thermal base generator in the present invention is more preferably N-tert-butyloxycarbonyl-4-piperidinol.
[0098] In the technical solution of the present invention, the amount of the thermal alkali generator added is 0.1-10 parts by mass based on 100 parts of polyamic acid ester from the perspective of improving the degree of thermal imidization of the polyimide precursor resin. If the amount is too low, it will not be conducive to improving the degree of thermal imidization of the polyimide precursor resin, and if the amount is too high, the storage stability of the glue will be significantly shortened.
[0099] Production Example 1:
[0100] Polyamic acid ester A
[0101] Disperse 103g of 4,4'-oxydiphthalic anhydride (ODPA) in γ-butyrolactone (GBL) solvent. Add 87g of hydroxyethyl methacrylate (HEMA) to the reaction system all at once, then add 3g of pyridine dropwise. React at room temperature for 16 hours. Dissolve 137g of dicyclohexylcarbodiimide (DCC) in GBL, slowly add dropwise to the reaction system, and stir for 2 hours. Dissolve 67g of 4,4'-diaminodiphenyl ether (ODA) in GBL under a nitrogen atmosphere and slowly add dropwise to the reaction system. Stir for 9 hours after addition (if stirring becomes difficult during the reaction, add appropriate solvent to dilute the reaction system). Add 2g of ethanol and react for 2 hours to terminate the reaction.
[0102] The quenched reaction liquid was filtered, and the filtrate was immediately added to methanol to precipitate a block solid, which was refrigerated for 12 hours and then dissolved and added dropwise to water, and filtered and dried to obtain the corresponding polyamic acid ester A.
[0103] The molecular weight of the polymer was obtained by using an ultra-high performance polymer chromatography (APC) instrument: M w It is 24000 and PDI is 1.85.
[0104] Polyamic acid ester B
[0105] Polyamic acid ester B was obtained in the same manner as in the polyamic acid ester A production example except that 82.4 g of ODPA and 14.5 g of pyromellitic dianhydride (PMDA) were used in place of 103 g of ODPA.
[0106] The molecular weight of the polymer was obtained by APC test: M w It is 23500 and PDI is 1.91.
[0107] Polyamic acid ester C
[0108] Polyamic acid ester C was obtained by replacing 103 g of the ODPA component in the polyamic acid ester A production example with 62 g of ODPA and 29 g of PMDA, with the remainder being the same.
[0109] The molecular weight of the polymer was obtained by APC test: M w It is 24200 and PDI is 1.89.
[0110] Polyamic acid ester D
[0111] Polyamic acid ester D was obtained by substituting 41.3 g of ODPA and 43.6 g of PMDA for 103 g of the ODPA component in the polyamic acid ester A production example and performing the other procedures in the same manner.
[0112] The molecular weight of the polymer was obtained by APC test: M w It is 23800 and PDI is 1.95.
[0113] Polyamic acid ester E
[0114] Polyamic acid ester E was obtained by replacing 103 g of the ODPA component in the polyamic acid ester A production example with 72.7 g of PMDA and remaining the same.
[0115] The molecular weight of the polymer was obtained by APC test: M w It is 24500 and PDI is 1.85.
[0116] Polyamic acid ester F
[0117] Polyamic acid ester F was obtained by replacing 67 g of the ODA component in the polyamic acid ester production example A with 36 g of p-phenylenediamine (PPDA) and making the same modifications as above.
[0118] The molecular weight of the polymer was obtained by APC test: M w It is 23000 and PDI is 1.88.
[0119] Production Example 2:
[0120] Multi-arm compound CA-1
[0121] 39.7 g of 1,2,3-benzotriazole was dispersed in N-methylpyrrolidone (NMP) solvent, and then 40.7 g of 4,4,4-triphenylmethane triisocyanate was dissolved in NMP and slowly added dropwise to the reaction system in a room temperature water bath. After the addition was complete, the temperature was slowly raised to 50°C and reacted in a water bath for 12 hours to obtain an NMP solution of CA-1 (mass concentration 30%). The solution was stored at low temperature for later use. The product purity was 95.7% as determined by high performance liquid chromatography (HPLC).
[0122] Multi-arm compound CA-2
[0123] 26.4 g of 1,2,3-benzotriazole and 24.7 g of isophorone diisocyanate were used to replace 39.7 g of 1,2,3-benzotriazole and 40.7 g of 4,4,4-triphenylmethane triisocyanate in the preparation example of the multi-arm compound CA-1, respectively. The rest of the ingredients remained the same. The product purity was 98.5% as determined by HPLC.
[0124] Multi-arm compound CA-3
[0125] 26.4 g of 1,2,3-benzotriazole and 18.7 g of hexamethylene diisocyanate were used to replace 39.7 g of 1,2,3-benzotriazole and 40.7 g of 4,4,4-triphenylmethane triisocyanate in the preparation example of multi-arm compound CA-1, respectively. The rest of the ingredients were the same as those in the preparation example. The product purity was 98.7% as determined by HPLC.
[0126] Multi-arm compound CA-4
[0127] 15.6 g of 1H-tetrazole and 18.7 g of hexamethylene diisocyanate were used to replace 39.7 g of 1,2,3-benzotriazole and 40.7 g of 4,4,4-triphenylmethane triisocyanate in the preparation example of multi-arm compound CA-1, respectively. The rest of the ingredients were the same as those in the preparation example. The product purity was 97.5% as determined by HPLC.
[0128] Multi-arm compound CA-5
[0129] 26.7 g of 7H-purine and 18.7 g of hexamethylene diisocyanate were used to replace 39.7 g of 1,2,3-benzotriazole and 40.7 g of 4,4,4-triphenylmethane triisocyanate in the preparation example of multi-arm compound CA-1, respectively. The rest of the ingredients were the same as those in the preparation example. The product purity was 96.5% as determined by HPLC.
[0130] Multi-arm compound CA-6
[0131] 26.7 g of 1H-imidazo[4,5-b]pyrazine and 18.7 g of hexamethylene diisocyanate were used to replace 39.7 g of 1,2,3-benzotriazole and 40.7 g of 4,4,4-triphenylmethane triisocyanate in the preparation example of multi-arm compound CA-1, respectively. The rest of the ingredients were the same as those in the preparation example. The product purity was 95.8% as determined by HPLC.
[0132] The structural formulas of the multi-arm compounds CA-1 to CA-6 in this production example are shown in FIG1 .
[0133] Example 1
[0134] Under a constant temperature and humidity environment (24° C., 50% RH), 20 g of polyamic acid ester A, 34 g of NMP solvent, 2.0 g of free radical polymerization monomer triethylene glycol dimethacrylate (PC-1), 0.5 g of the above-synthesized CA-3 NMP solution, 0.8 g of photoinitiator BASF IRGACURE OXE-01, 0.4 g of silane coupling reagent ureapropyl triethoxysilane, and 0.04 g of polymerization inhibitor 2-nitroso-1-naphthol were added to a 100 mL brown plastic bottle in sequence. After being shaken and dissolved on a shaker for 24 hours, an appropriate amount of NMP was further added to adjust the viscosity of the resulting solution to approximately 30 poise to prepare a negative photosensitive resin composition.
[0135] Example 2
[0136] 20 g of polyamic acid ester A in Example 1 was replaced by 20 g of polyamic acid ester B, and the remaining components and operation procedures remained the same as in Example 1.
[0137] Example 3
[0138] 20 g of polyamic acid ester A in Example 1 was replaced by 20 g of polyamic acid ester C, and the remaining components and operation procedures were consistent with those in Example 1.
[0139] Example 4
[0140] 20 g of polyamic acid ester A in Example 1 was replaced by 20 g of polyamic acid ester D, and the remaining components and operation procedures were consistent with Example 1.
[0141] Example 5
[0142] 20 g of polyamic acid ester A in Example 1 was replaced by 20 g of polyamic acid ester E, and the remaining components and operation procedures were consistent with those in Example 1.
[0143] Example 6
[0144] 20 g of polyamic acid ester A in Example 1 was replaced with 10 g of polyamic acid ester E and 10 g of polyamic acid ester F, and the remaining components and operation procedures were consistent with those in Example 1.
[0145] Example 7
[0146] The 0.5 g NMP solution of CA-3 in Example 6 was replaced with a 0.5 g NMP solution of CA-1. The remaining components and operating procedures remained the same as those in Example 6.
[0147] Example 8
[0148] The 0.5 g CA-3 NMP solution in Example 6 was replaced with a 0.5 g CA-2 NMP solution, and the remaining components and operating procedures were consistent with Example 6.
[0149] Example 9
[0150] The 0.5 g NMP solution of CA-3 in Example 6 was replaced with a 0.5 g NMP solution of CA-4. The remaining components and operating procedures were consistent with those of Example 6.
[0151] Example 10
[0152] The 0.5 g NMP solution of CA-3 in Example 6 was replaced with a 0.5 g NMP solution of CA-5. The remaining components and operating procedures remained the same as in Example 6.
[0153] Example 11
[0154] The 0.5 g NMP solution of CA-3 in Example 6 was replaced with a 0.5 g NMP solution of CA-6. The remaining components and operating procedures remained the same as those in Example 6.
[0155] Example 12
[0156] The 0.5 g CA-3 NMP solution in Example 6 was replaced with a 0.2 g CA-3 NMP solution, and the remaining components and operating procedures were consistent with Example 6.
[0157] Example 13
[0158] The 0.5 g NMP solution of the self-synthesized CA-3 in Example 6 was replaced with 1.0 g NMP solution of the self-synthesized CA-3. The remaining components and operation procedures were consistent with those in Example 6.
[0159] Example 14
[0160] On the basis of the preparation process of Example 6, 0.4 g of a thermal base generator, N-tert-butyloxycarbonyl-4-piperidiniummethanol, was added, and the remaining components and operation procedures remained the same as those of Example 6.
[0161] Comparative Example 1
[0162] The 0.5 g NMP solution of CA-3 in Example 6 was replaced with 0.1 g CA-7 (chemical formula shown in FIG1 ). The remaining components and operation procedures were consistent with those in Example 6.
[0163] Comparative Example 2
[0164] The 0.5 g NMP solution of CA-3 in Example 6 was replaced with 0.1 g CA-8 (chemical formula shown in FIG1 ). The remaining components and operation procedures were consistent with those in Example 6.
[0165] Comparative Example 3
[0166] The 0.5 g NMP solution of CA-3 in Example 6 was replaced with 0.1 g CA-9 (chemical formula shown in FIG1 ). The remaining components and operation procedures were consistent with those in Example 6.
[0167] Comparative Example 4
[0168] The 0.5 g NMP solution of CA-3 in Example 6 was replaced with 0.1 g CA-10 (chemical formula shown in FIG1 ). The remaining components and operation procedures were the same as those in Example 6.
[0169] Effect embodiment:
[0170] 1. Weight average molecular weight test:
[0171] The weight average molecular weight of the polyamic acid ester in the above manufacturing example was obtained by ultra-high performance polymer chromatography analysis instrument (ACQUITY APC). The relevant test conditions are as follows: the chromatographic column model is ACQUITY APC XT45 1.7 μm / ACQUITY APC XT200 2.5 μm / ACQUITYAPC XT450 2.5 μm, the column oven and detector temperatures are both 40 ° C, the mobile phase is tetrahydrofuran (THF), and the flow rate is 0.5 mL / min.
[0172] 2. Preparation and evaluation methods of photolithographic patterns:
[0173] The photosensitive polyamic acid ester composition prepared in the above example was spin-coated on an 8-inch silicon wafer using a spin coater (WS-650Mz-8NPPB, MYCRO) and pre-baked on a hot plate at 100°C for 240 seconds to form a coating film of about 10 μm in thickness. The coating film was irradiated with 400 mJ / cm2 using an i-line stepper (Shanghai Microelectronics) using a mask with a test pattern. 2 energy. Next, the coating film was spray-developed using cyclopentanone as a developer using a developer (MST-EF1-DV, Shenzhen Kaierdi) and rinsed with propylene glycol methyl ether acetate to obtain a photoresist pattern. A heat treatment was performed for 2 hours in a nitrogen atmosphere at the curing temperature listed in Table 1 using a temperature-programmed curing oven (HCM-500D, Shanghai Siwang Electronics) to obtain a cured photoresist pattern of approximately 10 μm thick formed from the composition.
[0174] The cured photolithography pattern obtained above was sliced and analyzed using a focused ion beam electron microscope (FIB, Helios G4, Thermo Fisher) to evaluate its photolithography accuracy and cross-sectional morphology profile, and then the photolithography performance of the negative photosensitive resin composition was evaluated: a photolithography line accuracy of less than 10 μm was rated as "excellent", a photolithography line accuracy of 10-20 μm was rated as "good", a photolithography line accuracy of 20-50 μm was rated as "acceptable", and a photolithography line accuracy greater than 50 μm was rated as "poor".
[0175] 3. Mechanical and thermal properties test of cured film:
[0176] The cured exposure film prepared by the above method using a mask with a specific pattern and a curing method was soaked in a 1% hydrofluoric acid aqueous solution for 10 minutes and then peeled off from the silicon wafer to obtain a 5mm×10cm film strip. After drying the moisture in an oven at 150°C, the film strip was subjected to a mechanical tensile test using a universal stretching machine (Shenzhen Sansi Zongheng Technology). The mechanical properties were evaluated based on their elongation at break: an elongation at break greater than 50% was rated as "excellent", an elongation at break between 40%-50% was rated as "good", an elongation at break between 20%-40% was rated as "acceptable", and an elongation at break less than 20% was rated as "poor".
[0177] The film specimens prepared above were tested using a dynamic mechanical analyzer (DMA, TA Instruments) to obtain the modulus-temperature curve and the glass transition temperature, thereby evaluating the thermal properties.
[0178] 4. Chemical resistance test of cured film:
[0179] The cured exposed film prepared by the above method using a mask with a specific pattern and a curing method was soaked in a 1% hydrofluoric acid aqueous solution for 10 minutes and then peeled off from the silicon wafer to obtain a complete cured film. After drying the film in an oven at 150°C, the film was placed in a 2.38% tetramethylammonium hydroxide solution in dimethyl sulfoxide and soaked at 50°C for 60 minutes. The film was then rinsed with deionized water and dried in an oven at 150°C. The chemical resistance of the cured film was evaluated based on its weight loss before and after the chemical resistance treatment: a weight loss of less than 5% was rated as "excellent", a weight loss between 5% and 15% was rated as "good", a weight loss between 15% and 25% was rated as "acceptable", and a weight loss greater than 25% was rated as "poor".
[0180] 5. Test of the bonding strength of the cured film on the copper surface:
[0181] Using a mask with a specific pattern and the above-mentioned method 3, a cured exposure film was prepared on a copper substrate and placed in a high-temperature and high-humidity accelerated aging test chamber (EHS-222MD, ESPEC). The test conditions were 130°C and 85% RH for 264 hours. After the test, the adhesion of the cured film on the copper surface was evaluated using the 100-grid method: if the grid did not fall off 100%, it was rated as "excellent", if the grid shedding rate was within 5%, it was rated as "good", if the grid shedding rate was within 5%-15%, it was rated as "acceptable", and if the grid shedding rate was greater than 15%, it was rated as "poor".
[0182] The components and contents of the polyamic acid ester compositions prepared in the above-mentioned examples and comparative examples, as well as the curing process, are shown in Table 1 in Figure 2 , and the relevant performance test data are shown in Table 2 in Figure 3 . As can be seen from Tables 1 and 2, compared to the comparative examples in which a small molecule azole compound was added, the examples in which the multi-arm compound containing an azole structure synthesized according to the present invention was added exhibited overall superior chemical corrosion resistance and copper surface adhesion.
[0183] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A photosensitive polyimide precursor composition, It is characterized in that include: 100 parts by mass of polyamic acid ester as a photosensitive polyimide precursor; 0.1-10 parts by weight of a multi-arm structure compound containing an azole structure; 1-20 parts by weight of a free radical polymerization monomer; 0.5-10 parts by mass of a photoinitiator; 0.5-10 parts by mass of a silane coupling agent; 0.01-5 parts by mass of a polymerization inhibitor; 50-1500 parts by mass of an organic solvent; The multi-arm structure compound containing an azole structure is an azole structure Z 1 With multi-arm unit Z 2 bonded compounds; The azole structure Z 1 Select from any one or more of the following structures: The multi-arm unit Z 2 Select from any one or more of the following structures:
2. The photosensitive polyimide precursor composition according to claim 1, It is characterized in that The polyamic acid ester has a structure as shown in formula (I): In formula (I), X is a tetravalent organic group containing an aromatic group, Y is a divalent organic group containing an aromatic group, and R 1 and R 2 Each of them is independently selected from a monovalent organic group having a structure as shown in formula (II), and n is 2 to 150; In formula (II), R 3 , R 4 and R 5 Each of them is independently selected from a hydrogen atom and an alkyl group having 1 to 3 carbon atoms; and m is 2 to 10.
3. The photosensitive polyimide precursor composition according to claim 1, It is characterized in that The free radical polymerization monomer is selected from any one or more of (meth)acrylate compounds.
4. The photosensitive polyimide precursor composition according to claim 1, It is characterized in that The free radical polymerization monomer is any one or more of a difunctional (meth)acrylate compound and a trifunctional (meth)acrylate compound.
5. The photosensitive polyimide precursor composition according to claim 1, It is characterized in that The photoinitiator is selected from any one or more of oxime ester compounds, benzophenone, N,N'-tetramethyl-4,4'-diaminobenzophenone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone, alkyl anthraquinone, benzoin alkyl ether, benzoin, alkyl benzoin and benzil dimethyl ketal.
6. The photosensitive polyimide precursor composition according to claim 5, It is characterized in that The photoinitiator is an oxime ester compound.
7. The photosensitive polyimide precursor composition according to claim 1, It is characterized in that The solvent is selected from any one or more of esters, ethers, ketones, aromatic hydrocarbons, sulfoxides and amides.
8. The photosensitive polyimide precursor composition according to claim 1, It is characterized in that The silane coupling agent is selected from any one or more silane coupling agents containing a urea bond (-NH-CO-NH-).
9. The photosensitive polyimide precursor composition according to claim 1, It is characterized in that The polymerization inhibitor is selected from any one or more of phenolic free radical polymerization inhibitors.
10. The photosensitive polyimide precursor composition according to claim 1, It is characterized in that Also included is 0.1-10 parts of a thermal alkali generator.
11. The photosensitive polyimide precursor composition according to claim 10, It is characterized in that The thermal base generator is an amine compound protected by tert-butoxycarbonyl.
12. A photosensitive polyimide composition, It is characterized in that The photosensitive polyimide precursor composition is obtained by thermal imidization of any one of claims 1 to 11.
13. The photosensitive polyimide composition according to claim 12, It is characterized in that The temperature of the thermal imidization is 150-400°C.
Citation Information
Patent Citations
Composite thermoplastic elastomer and preparation method thereof
CN107488334A
Adhesive composition and connection structure
JP2015151536A
Negative type photosensitive resin composition, method for producing polyimide, and method for producing cured relief pattern
JP2020173431A
Ethylenically unsaturated blocked aromatic diisocyanates and polymers thereof
US4101491A