Magnetically-coated carbon fiber material and preparation method therefor, and heat-conducting gasket and preparation method therefor
Through plasma treatment and magnetic coating technology, carbon fibers are endowed with magnetism and oriented in a magnetic field, which solves the problems of high cost and environmental pollution of oriented carbon fibers in traditional methods, and improves the thermal conductivity of thermal pads.
Patent Information
- Application Number
- PCT/CN2023/101913
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-20
- Filing Date
- 2023-06-21
- Publication Date
- 2024-10-24
AI Technical Summary
The traditional method uses a large amount of acid when imparting magnetism to carbon fiber, which affects environmental protection, and the magnetic coating effect is not good, resulting in high cost of directional arrangement of carbon fibers and affecting the thermal conductivity of the thermal pad.
The carbon fiber is treated with plasma to surface treat it under oxygen-containing conditions, introduce active groups, and then react with the magnetic solution to generate ferroferric oxide, which imparts magnetism to the carbon fiber and is oriented in the magnetic field to reduce the magnetic field strength requirements.
It improves the magnetic coating effect of carbon fiber, reduces the cost of directional arrangement of carbon fiber, improves the thermal conductivity of the thermal pad, and the process is safe, non-toxic and environmentally friendly.
Smart Images

Figure CN2023101913_24102024_PF_FP_ABST
Abstract
Description
A magnetic coated carbon fiber material and its preparation method, a thermal conductive gasket and its preparation method
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This disclosure claims priority to Chinese patent application No. 2023104393028 filed with the State Intellectual Property Office of China on April 20, 2023, entitled “A magnetic coated carbon fiber material and its preparation method, a thermal conductive gasket and its preparation method,” the entire contents of which are incorporated by reference into this disclosure. Technical Field
[0003] The present disclosure relates to the field of thermal interface materials, and in particular to a magnetic coated carbon fiber material and a preparation method thereof, a thermally conductive gasket and a preparation method thereof. Background Art
[0004] With the development of electronic information technology, chip operating frequencies are increasing, and the number of heat-generating devices is increasing. To maintain the normal and efficient operation of electronic equipment, the temperature of each heat-generating component must be effectively controlled to prevent burnout or high-temperature interruption of operation. In view of this, a variety of heat sinks or heat dissipation systems have been developed. In recent years, a series of high-thermal-conductivity metal and carbon materials, such as copper foil and graphite film, have been used to manufacture high-performance heat dissipation devices. With the continuous miniaturization and complexity of various electronic components, the shape of their heat dissipation surfaces has become irregular and has a certain degree of roughness. Traditional hard metal foil and graphite film have poor flexibility, resulting in poor adhesion between the heat dissipation surface and the heat dissipation material, resulting in a huge contact thermal resistance, making it difficult to achieve the expected heat dissipation performance of the heat dissipation material. Therefore, flexible and sticky polymer thermal interface materials reinforced with thermally conductive fillers have been further developed and applied. Among them, carbon fiber-filled thermal conductive materials have excellent electrical and thermal conductivity and have become one of the preferred materials for thermal interface materials.
[0005] Carbon fibers have significant anisotropy and possess excellent thermal and electrical conductivity along their length. Using orientation technology to align the carbon fibers according to a specific pattern can yield a material with excellent thermal conductivity in a single direction. Prior art methods for aligning carbon fibers often use magnetic field orientation. However, prior to magnetic field orientation, the fibers typically need to be imparted with magnetism. This method typically involves acid washing the fibers and then immersing them in a magnetic solution. This method uses large amounts of acid, which is environmentally unfriendly and also compromises the effectiveness of subsequent magnetic coating.
[0006] Summary of the Invention
[0007] In response to the above technical problems, the embodiments of the present disclosure provide a magnetic coated carbon fiber material and a preparation method thereof, a thermal conductive gasket and a preparation method thereof, aiming to reduce the cost of directional arrangement of carbon fibers in the thermal conductive gasket and improve production efficiency.
[0008] In a first aspect, the present disclosure provides a method for preparing a magnetic coated carbon fiber material, which may include:
[0009] Carbon fiber treatment: taking carbon fiber materials and performing plasma treatment under oxygen-containing conditions; and
[0010] Magnetic coating: The plasma-treated carbon fiber material is mixed with a magnetic solution containing ferric ions and ferrous ions, and then dried to obtain magnetically coated carbon fiber powder.
[0011] By adopting the above technical solution, carbon fibers can be plasma treated under oxygen-containing conditions, which can improve their surface hydrophilicity and make them easier to disperse in magnetic solutions. In addition, active groups such as -COOH and -OH can be introduced on the surface of the carbon fibers. In the subsequent magnetic coating process, these groups can react with iron ions and ferrous ions in the magnetic solution to generate ferroferric oxide. Ferroferric oxide is a unique iron oxide with magnetic properties. After attaching to the surface of the carbon fibers, the carbon fibers themselves also gain magnetism. This allows the materials to be oriented in a magnetic field when the magnetically coated carbon fiber materials are applied. If the magnetically coated carbon fiber materials are used to prepare thermally conductive gaskets, the carbon fibers can be oriented in the thickness direction, thereby aligning the axial direction of the carbon fibers with the thickness direction of the thermally conductive gaskets. This allows the thermally conductive gaskets to achieve good heat conduction in the thickness direction.
[0012] The plasma treatment of carbon fibers disclosed herein is simpler than conventional strong-acid oxidation, and the treatment process is safe, non-toxic, and environmentally friendly. Furthermore, plasma treatment allows the carbon fibers to react effectively with the magnetic solution, achieving magnetic coating. This allows the fibers to be easily oriented in a relatively low-intensity magnetic field, effectively reducing the cost of preparing the oriented carbon fibers. Furthermore, the improved orientation effect improves the thermal conductivity of the thermally conductive gasket.
[0013] In some embodiments, the plasma treatment conditions include a temperature of 20-30° C., a duration of 30-40 minutes, and a discharge power of 400-500 W. These treatment conditions can effectively treat the carbon fibers, to a certain extent avoiding affecting the properties of the carbon fibers themselves, thereby facilitating the production of a thermally conductive gasket with excellent thermal conductivity.
[0014] As an example, the temperature of the plasma treatment can be 20°C, 22°C, 24°C, 26°C, 28°C or 30°C; the time of the plasma treatment can be 30min, 32min, 34min, 36min, 38min or 30min; the discharge power of the plasma treatment can be 400W, 420W, 440W, 460W, 480W or 500W.
[0015] In some embodiments, the plasma treatment atmosphere may include nitrogen and oxygen, with the oxygen ratio being ≥50%. Oxygen ratio within this range is beneficial for surface treatment of carbon fibers under plasma conditions.
[0016] As an example, the proportion of oxygen may be 50%, 60%, 70%, 80%, 90% or 100%.
[0017] In some embodiments, the oxygen content can be 50% to 80%. When the oxygen content is within this range and combined with the above-mentioned plasma treatment conditions, the carbon fiber can be treated within a thickness of 100 nm on the surface, effectively reducing the impact on the carbon fiber performance.
[0018] In some embodiments, the configuration method of the magnetic solution may include: taking carbonate powder and dissolving it in an organic acid, and then adding ferric chloride solution to mix to obtain a magnetic solution. Carbonate powder dissolved in an organic acid can react to form a substance with a certain reducing property, which can convert part of the iron ions into ferrous ions, and obtain a magnetic solution in which iron ions and ferrous ions coexist. In the subsequent magnetic coating process, the active groups such as -COOH and -OH on the surface of the carbon fiber after activation treatment react with the iron ions and ferrous ions in the magnetic solution to generate magnetic ferrosoferric oxide and adhere to the surface of the carbon fiber, so that the carbon fiber itself has magnetism. So that when it is applied, the carbon fiber can be oriented and arranged in a magnetic field under the action of magnetic force.
[0019] In some embodiments, the carbonate salt may include at least one of sodium bicarbonate, sodium carbonate, calcium bicarbonate, and calcium carbonate.
[0020] In some embodiments, the organic acid may include at least one of ascorbic acid, citric acid, and acetic acid.
[0021] Sodium bicarbonate and ascorbic acid react to form sodium ascorbate with a certain reducing property; sodium carbonate and ascorbic acid react to form sodium ascorbate with a certain reducing property; calcium bicarbonate and ascorbic acid react to form calcium ascorbate with a certain reducing property; calcium carbonate and ascorbic acid react to form calcium ascorbate with a certain reducing property; sodium bicarbonate and citric acid react to form sodium citrate with a certain reducing property; sodium carbonate and citric acid react to form sodium citrate with a certain reducing property; calcium bicarbonate and citric acid react to form calcium citrate with a certain reducing property; calcium carbonate and citric acid react to form calcium citrate with a certain reducing property; sodium bicarbonate and acetic acid react to form sodium acetate with a certain reducing property; sodium carbonate and acetic acid react to form sodium acetate with a certain reducing property; calcium bicarbonate and acetic acid react to form calcium acetate with a certain reducing property; calcium carbonate and acetic acid react to form calcium acetate with a certain reducing property. These weakly reducing reactants can convert part of the ferric ions into ferrous ions, so as to obtain a mixture of ferric ions and ferrous ions, so as to form magnetic ferrosoferric oxide in the subsequent reaction.
[0022] In some embodiments, the ratio of carbonate, organic acid, and ferric chloride solution in the magnetic solution can be 1:20-22:28-32 (m / v / v); wherein the concentration of the organic acid can be 0.02-0.03 mol / L, and the concentration of the ferric chloride solution can be 0.1-0.5 mol / L. This allows the contents of ferric ions and ferrous ions in the resulting magnetic solution to be maintained within an appropriate range, allowing for more effective magnetic coating of the carbon fibers.
[0023] For example, the concentration of the organic acid may be 0.02 mol / L, 0.022 mol / L, 0.024 mol / L, 0.026 mol / L, 0.028 mol / L, or 0.03 mol / L; the concentration of the ferric chloride solution may be 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.4 mol / L, or 0.5 mol / L; and the ratio of the carbonate, the organic acid, and the ferric chloride solution may be 1:20:28 (m / v / v), 1:21:28 (m / v / v), 1:22: 28(m / v / v), 1:20:29(m / v / v), 1:21:29(m / v / v), 1:22:29(m / v / v), 1:20:30(m / v / v), 1:21:30(m / v / v), 1:22:30(m / v / v), 1:20:31(m / v / v), 1:21:31(m / v / v), 1:22:31(m / v / v), 1:20:32(m / v / v), 1:21:32(m / v / v) or 1:22:32(m / v / v).
[0024] In some embodiments, during the magnetic coating step, the mixing reaction conditions may include heating to 120-150°C for 4-6 hours, followed by filtration and washing until neutral. Reaction at this temperature and for this time allows for a relatively uniform magnetic ferrosoferric oxide to form on substantially all surfaces of the carbon fibers, facilitating subsequent applications.
[0025] Illustratively, the temperature of the mixing reaction may be 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, or 150°C; and the time of the mixing reaction may be 4 h, 4.5 h, 5 h, 5.5 h, or 6 h.
[0026] In some embodiments, the plasma treatment conditions include: a treatment time of 30 minutes, a temperature of 25° C., a process atmosphere of nitrogen and oxygen, with an oxygen ratio of 80%, and a discharge power of 500W.
[0027] In some embodiments, in the step of preparing the magnetic solution, 5 g of sodium bicarbonate powder is dissolved in 100 mL of 0.025 mol / L ascorbic acid, ultrasonically stirred for 15 minutes, and 150 mL of 0.1 mol / L ferric chloride solution is added, and ultrasonically stirred for 15 minutes to obtain a magnetic solution.
[0028] In a second aspect, embodiments of the present disclosure provide a magnetically coated carbon fiber material, produced by any of the methods provided in the first aspect. This magnetically coated carbon fiber material exhibits magnetic properties, with the ferrosoferric oxide bonding to the carbon fibers being relatively tight. Furthermore, this facilitates oriented alignment in a relatively low magnetic field during application.
[0029] On the third aspect, an embodiment of the present disclosure provides a method for preparing a thermally conductive gasket, which may include magnetic field orientation: magnetic coated carbon fiber powder and a thermal interface material base material may be mixed and filled into a mold, and then placed in a magnetic field for orientation. After the orientation is completed, the powder is baked and cured to obtain a thermally conductive gasket; wherein the direction of the magnetic field may be perpendicular to the thickness direction of the thermally conductive gasket, and the magnetic field lines pass through the mold.
[0030] By adopting the above technical solution, the magnetically coated carbon fibers are oriented under the action of magnetic force, and the carbon fibers in the manufactured thermal gasket are oriented along the thickness direction, so that the axial direction of the carbon fibers and the thickness direction of the thermal gasket can be consistent, and the thermal gasket can obtain good heat conduction effect in the thickness direction.
[0031] Among them, the magnetic coated carbon fiber material provided by the embodiments of the present disclosure can be used to prepare not only thermal conductive gaskets, but also other materials that require directional orientation of carbon fibers, such as wave absorbing gaskets.
[0032] In some embodiments, during the magnetic field orientation step, the magnetic field intensity may be no less than 0.6 T. In the present disclosure, since the aforementioned plasma treatment of the carbon fibers allows the active groups on the carbon fiber surface to react with the ferric ions and ferrous ions to generate magnetic ferrosoferric oxide, which is attached to the carbon fiber surface. The magnetic material has a good coating effect on the carbon fiber surface. Therefore, the magnetic field intensity can be set to a minimum of 0.6 T to achieve a good directional orientation effect.
[0033] As an example, the magnetic field strength may be 0.6T, 0.7T, 0.8T, 0.9T, 1.0T, 1.1T or 1.2T.
[0034] In some embodiments, the magnetic field strength may be 0.6 to 1 T. This relatively weak magnetic field strength can achieve directional orientation while also helping to reduce energy consumption.
[0035] In some embodiments, during the magnetic field step, mechanical vibration is simultaneously performed in the magnetic field.
[0036] By adopting the above technical solution, mechanical vibration can reduce the viscosity effect of liquid rubber on carbon fibers, reduce the difficulty of orienting carbon fibers, and assist in promoting the directional arrangement of carbon fibers.
[0037] In some embodiments, the magnetic coated carbon fibers may account for 8-12% of the thermal interface material base material by mass, which can improve the thermal conductivity of the thermally conductive gasket and facilitate obtaining a gasket structure.
[0038] In some embodiments, the thermal interface material base comprises the following raw materials in parts by weight: 50-60 parts of polysiloxane; 50-60 parts of thermal conductive filler; 0.1-1 part of coupling agent; 0.01-0.1 part of inhibitor; 1-5 parts of vulcanizing agent; and 1-5 parts of catalyst.
[0039] By employing this technical solution, magnetically coated carbon fibers are mixed with a liquid adhesive-like thermal interface material base. The magnetic coating material is randomly distributed within the thermal interface material base. A magnetic field is used to orient the magnetically coated carbon fibers, and then heat-curing is performed to form a stable thermally conductive gasket. Adding thermally conductive fillers to the polysiloxane system further enhances the thermal conductivity of the thermally conductive gasket. The thermally conductive gasket made from this thermal interface material base retains a certain degree of stickiness after curing.
[0040] In some embodiments, the thermally conductive filler may include one or more combinations of aluminum nitride, aluminum oxide, silicon nitride, boron nitride, zinc oxide, and magnesium oxide.
[0041] In some embodiments, the polysiloxane may be vinyl liquid silicone rubber, and the viscosity of the polysiloxane may be 300 to 500 mPa·s.
[0042] In some embodiments, the coupling agent may be a silane coupling agent.
[0043] In some embodiments, the catalyst may be a platinum catalyst.
[0044] In some embodiments, the inhibitor can be ethynylcyclohexanol.
[0045] In some embodiments, the vulcanizing agent may be a hydrogen-containing accelerator.
[0046] In some embodiments, the carbon fibers may be pitch-based chopped carbon fibers, and the length of the carbon fibers may be 150 to 200 μm, and the diameter may be 5 to 10 μm.
[0047] In a fourth aspect, the present disclosure provides a thermally conductive gasket that can be manufactured by any method provided in the third aspect.
[0048] In summary, the present disclosure includes at least one of the following beneficial technical effects:
[0049] 1. In the technical solution disclosed in the present invention, the carbon fibers that are not magnetic are endowed with magnetism through plasma treatment of the carbon fibers and magnetic coating, so that the carbon fibers can be easily oriented by the magnetic force in a magnetic field of relatively low intensity, thereby making a thermally conductive gasket with directional arrangement of carbon fibers, thereby effectively improving the thermal conductivity of the thermally conductive gasket, and at the same time reducing the cost of orienting the carbon fibers and improving production efficiency.
[0050] 2. In the technical solution disclosed herein, the carbon fibers treated with plasma are made magnetic by reacting with a magnetic solution. The magnetic coating treatment process is simple, efficient, and low-cost.
[0051] 3. In the technical solution disclosed in the present invention, the carbon fiber is surface treated by plasma treatment, which improves the hydrophilicity of the carbon fiber surface and introduces active groups such as -COOH and -OH on the carbon fiber surface by ionizing air. Compared with the strong acid oxidation treatment of carbon fiber in the existing technology, the process is more efficient and safe and non-toxic, and will not affect the environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] In order to more clearly illustrate the embodiments of the present disclosure or the technical solutions in the prior art, the following briefly introduces the drawings required for describing the embodiments or the prior art.
[0053] FIG1 is a picture of carbon fibers after plasma treatment and after mixing with a magnetic solution in Example 1 of the present disclosure;
[0054] FIG2 is a picture of the carbon fibers after acid treatment and after mixing with the magnetic solution in Comparative Example 3 of the present disclosure;
[0055] FIG3 is a microscopic photograph of a cross section of the thermally conductive gasket prepared in Example 1 of the present disclosure;
[0056] FIG4 is a microscopic photograph of a cross section of the thermally conductive gasket prepared in Comparative Example 3 of the present disclosure. DETAILED DESCRIPTION
[0057] The present disclosure is further described in detail below with reference to the accompanying drawings and specific examples. It should be noted that, unless otherwise specified in the following examples, all procedures were carried out under conventional conditions or conditions recommended by the manufacturer; and all raw materials used in the following examples were commercially available unless otherwise specified.
[0058] Example 1
[0059] A thermally conductive pad can be prepared by the following method:
[0060] S1. Plasma treatment: Take virgin carbon fiber (asphalt-based chopped carbon fiber, the average length can be 180 μm, the average diameter can be 6 μm) and place it in a drum plasma surface treatment instrument for surface treatment. The treatment time can be 30 minutes, the temperature can be 25°C, the process atmosphere can be nitrogen and oxygen, the oxygen ratio can be 80%, and the discharge power can be 500W.
[0061] S2. Prepare a magnetic solution: dissolve 5 g of sodium bicarbonate powder in 100 mL of 0.025 mol / L ascorbic acid, stir ultrasonically for 15 min, add 150 mL of 0.1 mol / L ferric chloride solution, and stir ultrasonically for 15 min to obtain a magnetic solution.
[0062] S3, magnetic coating: take the plasma-treated carbon fiber in step S1, disperse it in 150 mL of deionized water and stir it evenly, then mix it with the magnetic solution, place it in a hydrothermal reactor and heat it to 150°C for 5 hours, filter it, wash it with deionized water until it is neutral, transfer it to a 70°C drying furnace and dry it for 4 hours to obtain magnetic coated carbon fiber.
[0063] S4. Magnetic field orientation: Take 10g of magnetic coated carbon fiber, 50g of aluminum oxide, 50g of vinyl silicone rubber (viscosity: 300mPa·s), and 0.8g of vinyl silane coupling agent and put them into a vacuum mixer and stir for 5 minutes. After taking them out, add 0.08g of ethynyl cyclohexanol, 2.7g of vulcanizing agent, and 2g of platinum catalyst and continue stirring for 5 minutes. Pour the mixture into a mold and place it together with the mold in a 0.6T magnetic field for orientation for 1 hour. The magnetic field lines are along the thickness direction of the thermal gasket and pass through the mold. After the orientation is completed, transfer the mold to an oven and bake at 100°C for 5 hours to obtain a thermal gasket.
[0064] Comparative Example 1
[0065] The difference between this comparative example and Example 1 is that the carbon fiber does not need to be subjected to magnetic coating treatment, and the rest is consistent with Example 1.
[0066] Comparative Example 2
[0067] The difference between this comparative example and Example 1 is that the carbon fibers can be directly magnetically coated without undergoing plasma treatment, and the rest are consistent with Example 1.
[0068] Comparative Example 3
[0069] This comparative example differs from Example 1 in that the carbon fibers are surface-treated by strong acid oxidation. Specifically, the carbon fibers are immersed in 70% concentrated sulfuric acid, heated to 60°C for 2 hours, filtered, rinsed with deionized water until neutral, and dried at 100°C to obtain surface-treated carbon fibers. All other steps remain the same as in Example 1.
[0070] Comparative Example 4
[0071] The difference between this comparative example and Example 1 is that the carbon fibers may be magnetically coated without being oriented in a magnetic field, and the rest are the same as in Example 1.
[0072] Performance testing
[0073] The thermally conductive pads prepared in the examples and comparative examples were subjected to performance testing, specifically including:
[0074] Hardness: tested according to ASTM D 2240 standard;
[0075] Rebound performance: Rebound rate is tested according to ASTM D 412 standard;
[0076] Tensile strength: tested according to ASTM D 412 standard;
[0077] Density: tested according to ASTM D 792 standard;
[0078] Thermal conductivity: tested according to ASTM D 5470 standard.
[0079] The performance test results of Example 1 and Comparative Examples 1 to 4 are shown in Table 1 below.
[0080] Table 1: Performance test results of Example 1 and Comparative Examples 1 to 4.
[0081] It can be seen from the data in Table 1 that in the technical solution disclosed herein, the carbon fibers are magnetically coated and then oriented in the thickness direction of the thermally conductive gasket by means of magnetic field orientation, thereby effectively exerting the excellent heat conduction effect of the carbon fibers in the axial direction, and the resulting thermally conductive gasket has good thermal conductivity.
[0082] It can be seen from the data in Example 1 and Comparative Example 3 that after the carbon fiber surface is plasma-treated and the carbon fiber is strong acid-treated, the carbon fiber obtained by plasma treatment is finally made into a thermal conductive gasket, and its rebound rate, tensile strength, density and thermal conductivity coefficient are all increased, indicating that after the plasma-treated carbon fiber is used to prepare a directional and oriented thermal conductive gasket, its performance is improved. At the same time, the cost of plasma treatment can be lower, the efficiency is higher, and the pollution to the environment is less.
[0083] Figure 1 shows a picture of carbon fibers after plasma treatment and a magnetic solution in Example 1 of the present disclosure; Figure 2 shows a picture of carbon fibers after acid treatment and a magnetic solution in Comparative Example 3 of the present disclosure. Comparison of Figures 1 and 2 shows that when the plasma-treated carbon fibers are mixed with the magnetic material, the carbon fibers essentially do not agglomerate and can be evenly dispersed in the magnetic solution, which facilitates the formation of a uniform distribution of magnetic material on the carbon fibers' surfaces and facilitates subsequent directional orientation via a magnetic field.
[0084] Figure 3 is a microscopic photograph of a cross-section of the thermally conductive gasket produced in Example 1 of the present disclosure; Figure 4 is a microscopic photograph of a cross-section of the thermally conductive gasket produced in Comparative Example 3 of the present disclosure. Figures 3 and 4 show that the plasma-treated carbon fibers mixed with the magnetic material and then magnetically coated result in a thermally conductive gasket with improved orientation, which helps improve the thermal conductivity of the thermally conductive gasket.
[0085] Example 2
[0086] The difference between this embodiment and embodiment 1 is that the amount of ascorbic acid added can be 150 mL, the amount of ferric chloride solution added can be 100 mL, and the rest are consistent with embodiment 1.
[0087] Example 3
[0088] The difference between this embodiment and embodiment 1 is that the amount of ascorbic acid added can be 50 mL, the amount of ferric chloride solution added can be 200 mL, and the rest are consistent with embodiment 1.
[0089] Example 4
[0090] The difference between this embodiment and embodiment 1 is that the concentration of ascorbic acid can be 0.01 mol / L, the concentration of ferric chloride solution can be 0.8 mol / L, and the rest are consistent with embodiment 1.
[0091] Example 5
[0092] The difference between this embodiment and embodiment 1 is that the concentration of ascorbic acid can be 0.05 mol / L, the concentration of ferric chloride solution can be 0.1 mol / L, and the rest are consistent with embodiment 1.
[0093] Example 6
[0094] The difference between this embodiment and embodiment 1 is that the magnetic field strength can be 1 T, and the rest are consistent with embodiment 1.
[0095] Example 7
[0096] The difference between this embodiment and embodiment 1 is that the magnetic field strength can be 0.5 T, and the rest are consistent with embodiment 1.
[0097] Example 8
[0098] The difference between this embodiment and embodiment 7 is that mechanical vibration is also applied during the magnetic field orientation process, specifically:
[0099] S1. Carbon fiber cleaning: Take the original carbon fiber and put it into the roller plasma surface treatment instrument for surface treatment; the plasma treatment time can be 20 minutes, the temperature can be 25°C, the process atmosphere can be nitrogen, and the discharge power can be 400W;
[0100] S2, prepare magnetic solution: take 5g sodium bicarbonate powder and dissolve it in 100mL ascorbic acid with a concentration of 0.025mol / L, ultrasonically stir for 15min, add 150mL 0.1mol / L ferric chloride solution, ultrasonically stir for 15min to obtain magnetic solution;
[0101] S3, magnetic coating: take 10g of plasma-cleaned carbon fiber and evenly disperse it in 150mL of deionized water, then mix it evenly with the magnetic solution, place it in a hydrothermal reactor, heat it at 150℃ for 5h, filter it, wash it to the center with deionized water, and place it in a drying oven at 70℃ for 24h to obtain magnetic coated carbon fiber;
[0102] S4. Magnetic field orientation: Take 10g of magnetic coated carbon fiber, 50g of alumina, 50g of polysiloxane, and 0.8g of silane coupling agent and put them into a vacuum mixer and stir for 5 minutes. After taking them out, add 0.08g of ethynyl cyclohexanol, 2.7g of vulcanizing agent, and 2g of platinum catalyst and continue stirring for 5 minutes. Pour the mixture into a mold and place it together with the mold in a 0.6T magnetic field for orientation for 1 hour. The magnetic field lines are along the thickness direction of the thermal gasket and pass through the mold. The magnetic field orientation also applies mechanical vibration to the mold. After the orientation is completed, the mold is transferred to an oven and baked at 100°C for 5 hours to obtain a thermal gasket.
[0103] The rest are consistent with Example 1.
[0104] The performance test results of Examples 2 to 8 are shown in Table 2 below.
[0105] Table 2: Performance test results of Examples 2 to 8
[0106] It can be seen from the data in Table 2 that by adjusting the addition amount and parameters of each raw material for preparing the magnetic solution, the thermal conductivity and strength of the obtained thermally conductive pad can be further optimized. Examples 2 to 5 make adjustments to the addition amount and specifications of ascorbic acid and ferric chloride solution. It can be seen that when the range defined in the technical solution of the present disclosure is exceeded, the thermal conductivity of the thermally conductive pad decreases significantly. This may be because outside the range defined in the present disclosure, the amount of ferrous ions generated by the redox reaction of sodium ascorbate and iron ions changes, resulting in a decrease in the amount of ferroferric oxide replaced on the surface of the carbon fiber during the subsequent magnetic coating process, affecting the magnetic properties of the carbon fiber after magnetic coating, resulting in the directional arrangement of the carbon fiber during the magnetic field orientation process being affected, thereby affecting the thermal conductivity of the thermally conductive pad.
[0107] The intensity of the magnetic field was adjusted in Examples 6 and 7. It can be seen that when the magnetic field intensity is lower than 0.6 T, the thermal conductivity of the thermal gasket is significantly weakened. This may be because the insufficient magnetic field intensity causes the orientation quantity or orientation degree of the carbon fibers to change, thereby affecting the thermal conductivity of the thermal gasket.
[0108] Based on Example 7, Example 8 additionally applies mechanical vibration during the magnetic field orientation process. It can be seen that on the basis of reducing the magnetic field intensity, the additional addition of mechanical vibration can improve the thermal conductivity of the thermal conductive gasket to a certain extent. This may be because the auxiliary carbon fiber gets rid of the viscosity of the rubber on the carbon fiber during the mechanical vibration, making the orientation of the carbon fiber more easily change under the action of the magnetic field.
[0109] The above are all preferred embodiments of the present disclosure, and are not intended to limit the protection scope of the present disclosure. Therefore, any equivalent changes made based on the structure, shape, and principle of the present disclosure should be included in the protection scope of the present disclosure. Industrial Applicability
[0110] The embodiments of the present disclosure provide a magnetic coated carbon fiber material and a preparation method thereof, a thermal conductive gasket and a preparation method thereof, and through plasma treatment of carbon fiber and magnetic coating and other treatments, the carbon fiber that does not have magnetism is given magnetism, so that the carbon fiber can be easily affected by the magnetic force in a magnetic field of lower intensity and change its orientation, thereby making a thermal conductive gasket with directional arrangement of carbon fibers, effectively improving the thermal conductivity of the thermal conductive gasket, while reducing the cost of orienting the carbon fibers and improving production efficiency. The carbon fibers that have been treated with plasma react with a magnetic solution to make the carbon fibers magnetic, and the process of magnetic coating treatment is simple, efficient, and low-cost. In addition, the carbon fibers are surface-treated by plasma treatment, and while improving the hydrophilicity of the carbon fiber surface, active groups such as -COOH and -OH are introduced on the carbon fiber surface by ionized air. Compared with the strong acid oxidation treatment of carbon fibers in the prior art, the process is more efficient and safe and non-toxic, and will not affect the environment.
[0111] Furthermore, it is understood that the magnetic coated carbon fiber material and its preparation method, as well as the thermally conductive gasket and its preparation method provided by the embodiments of the present disclosure are reproducible and can be used in a variety of industrial applications. For example, the magnetic coated carbon fiber material and its preparation method, as well as the thermally conductive gasket and its preparation method provided by the embodiments of the present disclosure can be used in the technical field involving thermal interface materials.
Claims
1. A method for preparing a magnetic coated carbon fiber material, comprising: Carbon fiber treatment: The carbon fiber material is subjected to plasma treatment under oxygen-containing conditions; as well as Magnetic coating: The carbon fiber material treated with plasma is mixed with the magnetic solution containing ferric ions and ferrous ions, and then dried to obtain magnetically coated carbon fiber powder.
2. The method for preparing a magnetic coated carbon fiber material according to claim 1, wherein: The plasma treatment conditions include: temperature of 20-30°C, time of 30-40min, and discharge power of 400-500W; Optionally, the atmosphere of the plasma treatment includes nitrogen and oxygen, and the proportion of oxygen is ≥50%; Optionally, the oxygen ratio is 50% to 80%.
3. The method for preparing a magnetic coated carbon fiber material according to claim 1 or 2, further comprising the step of preparing a magnetic solution, wherein the step of preparing a magnetic solution comprises: Dissolving carbonate powder in organic acid, then adding ferric chloride solution and mixing, to obtain the magnetic solution; Optionally, the carbonate includes at least one of sodium bicarbonate, sodium carbonate, calcium bicarbonate and calcium carbonate; Optionally, the organic acid includes at least one of ascorbic acid, citric acid and acetic acid.
4. The method for preparing a magnetic coated carbon fiber material according to claim 3, wherein: In the magnetic solution, the ratio of the carbonate, the organic acid and the ferric chloride solution is 1:20-22:28-32 (m / v / v); wherein the concentration of the organic acid is 0.02-0.03 mol / L; the concentration of the ferric chloride solution is 0.1-0.5 mol / L; optionally, in the magnetic coating step, the conditions of the mixed reaction include: heating to 120-150°C for 4-6 hours; and then also including: filtering and washing to neutrality.
5. The method for preparing a magnetic coated carbon fiber material according to any one of claims 2 to 4, wherein: The plasma treatment conditions include: treatment time of 30 minutes, temperature of 25° C., process atmosphere of nitrogen and oxygen, oxygen accounting for 80%, and discharge power of 500W.
6. The method for preparing a magnetic coated carbon fiber material according to claim 3 or 4, wherein: In the step of preparing the magnetic solution, 5 g of sodium bicarbonate powder is dissolved in 100 mL of ascorbic acid with a concentration of 0.025 mol / L, ultrasonically stirred for 15 min, 150 mL of ferric chloride solution with a concentration of 0.1 mol / L is added, and ultrasonically stirred for 15 min to obtain a magnetic solution.
7. The method for preparing a magnetic coated carbon fiber material according to any one of claims 1 to 6, wherein: The carbon fiber material is asphalt-based chopped carbon fiber with a length of 150 to 200 μm and a diameter of 5 to 10 μm.
8. A magnetic coated carbon fiber material, wherein: The magnetic coated carbon fiber material is prepared by the method according to any one of claims 1 to 7.
9. A method for preparing a thermally conductive gasket, comprising: Magnetic field orientation: The magnetic coated carbon fiber material according to claim 8 is mixed with a thermal interface material base material and filled into a mold, and then placed in a magnetic field for orientation. After the orientation is completed, it is baked and cured to obtain a thermally conductive gasket; wherein the direction of the magnetic field is perpendicular to the thickness direction of the thermally conductive gasket, and the magnetic field lines pass through the mold.
10. A method for preparing a thermally conductive gasket according to claim 9, wherein: In the magnetic field orientation step, the magnetic field intensity is not less than 0.6T.
11. A method for preparing a thermally conductive gasket according to claim 9 or 10, wherein: The mass percentage of the magnetic coated carbon fiber to the thermal interface material base material is 8-12%.
12. A method for preparing a thermally conductive gasket according to claim 11, wherein: The thermal interface material base comprises the following raw materials in parts by weight: 50-60 parts of polysiloxane; 50-60 parts of thermal conductive filler; 0.1-1 part of coupling agent; 0.01-0.1 part of inhibitor; 1-5 parts of vulcanizing agent; and 1-5 parts of catalyst.
13. A thermally conductive pad, wherein: The thermally conductive gasket is made by the method according to any one of claims 9 to 12.
Citation Information
Patent Citations
High-temperature-resistance carbon fiber magnetic wave-absorbing composite material and preparation method thereof
CN110241611A
Method for loading hydroxyl iron oxide nanoparticle composite structural colors on carbon fiber woven fabrics and carbon fiber woven fabrics obtained according to method
CN110656488A
Composite carbon fiber with high electromagnetic wave absorption performance and preparation method thereof
CN115450044A
Coiled carbon fiber having ferromagnetism, method for producing the same, coiled carbon fiber composite having ferromagnetism and electric wave absorber
JP2001146644A
Coiled carbon fiber composite having ferromagnetism, method for producing the same and electric wave absorber
JP2001146645A
Cited By
Carbon fiber-carbon nanotube thermal interface material and preparation method thereof
CN119613962A
Magnetic carbon fiber modified PEEK material, gear prepared from magnetic carbon fiber modified PEEK material and method
CN120988452A
Wear-resistant sintered magnetic conductive coating
CN121628506A