Composite separator, and preparation method therefor and use thereof

By introducing a self-healing functional layer into the lithium-ion battery separator and using thermal cyclization polymerization to enhance the toughness and thermal stability of the base film layer, the problem of structural damage of the separator under high temperature conditions is solved, and the safety and electricity of the battery are improved. chemical properties.

WO2024216935A1PCT designated stage expired Publication Date: 2024-10-24CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/130534
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-17
Filing Date
2023-11-08
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Lithium-ion battery separators are prone to thermal shrinkage, deformation and closed pores under high temperature or cell thermal runaway conditions, leading to structural damage, which in turn triggers short-circuit current and thermal runaway, affecting the electrochemical performance of the battery.

Method used

A composite separator is used, including a base film layer and a self-healing functional layer. The self-healing functional layer contains a precursor material that can be thermally cyclized and polymerized. After self-healing, it forms a cross-linked polymer structure, provides thermal cyclization polymerization reaction, and strengthens the matrix. The toughness and thermal stability of the film layer prevent structural changes.

Benefits of technology

It effectively prevents the thermal shrinkage, deformation and closing of the separator under high temperature conditions, keeps the current and heat output within the normal range, avoids the increase in short-circuit current, improves the toughness and thermal stability of the composite separator, and enhances the safety performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023130534_24102024_PF_FP_ABST
    Figure CN2023130534_24102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed are a composite separator, and a preparation method therefor and the use thereof. The composite separator comprises at least one base film layer and a self-healing functional layer, which is arranged on the surface of the base film layer in a lamination fitting manner, wherein the self-healing functional layer contains a precursor material that can be subjected to heat cyclization polymerization, and / or the precursor material forms a crosslinked polymerization structure after the self-healing of the self-healing functional layer. When the interior of a secondary battery is overheated or thermal runaway occurs, the precursor material in the self-healing functional layer generates a thermal polymerization reaction to generate a high-temperature-resistant and high-mechanical-strength crosslinked polymer, and the crosslinked polymer has a supporting effect on the separator and can also inhibit irreversible deformations such as thermal closed pores and thermal shrinkage of a base film; in addition, a crosslinked polymer space structure also has a repairing effect on damage to a local pore structure of the base film.
Need to check novelty before this filing date? Find Prior Art

Description

Composite diaphragm and its preparation method and application

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on April 17, 2023, with application number 202310409267.5 and invention name “Composite diaphragm, preparation method and application thereof”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present application relates to the field of battery technology, and in particular to a composite diaphragm and a preparation method and application thereof. Background Art

[0003] The statements here only provide background information related to the present application and do not necessarily constitute prior art. Lithium-ion batteries have attracted much attention due to their high energy density, high volume density and reusability. With the continuous advancement and development of lithium-ion battery technology, they have been applied to many fields such as digital electronic products, energy storage, power, new energy vehicles, etc. One of the important factors that determine the performance and safety of lithium-ion batteries is the performance of its electrode materials, and another important factor is the battery separator. The separator is an extremely critical part of a lithium-ion battery. It is an electrically insulating film with a porous structure. Its function is to isolate the positive and negative electrodes of the battery and prevent electrons in the battery from passing freely, but at the same time allow ions to pass freely between the positive and negative electrodes. As a key component of lithium-ion battery cells, the performance of the separator determines the interface structure, internal resistance, etc. of the battery, and directly affects the battery's capacity, cycle and safety performance. A separator with excellent performance plays an important role in improving the overall performance of the battery.

[0004] Under high temperature or thermal runaway conditions, the battery separator will undergo irreversible structural changes such as thermal shrinkage, deformation, and closed pores, which will damage the separator structure. Severe thermal runaway may even cause the separator to rupture severely or shrink and melt, resulting in large short-circuit currents when the positive and negative electrodes come into contact, releasing a large amount of heat and directly affecting the electrochemical performance of the battery cell.

[0005] Application Contents

[0006] The purpose of the embodiments of the present application is to provide a composite diaphragm and its preparation method and application, including but not limited to solving the technical problem that the current diaphragm will undergo irreversible structural changes such as thermal shrinkage, deformation, and closed pores under high temperature or thermal runaway conditions of the battery cell, destroying the diaphragm structure, causing the positive and negative electrodes to contact and generate a large short-circuit current, releasing a large amount of heat, and affecting the electrochemical performance of the battery cell.

[0007] The technical solution adopted in the embodiment of this application is:

[0008] In a first aspect, a composite diaphragm is provided, comprising at least one base membrane layer and a self-healing functional layer laminated and arranged on the surface of the base membrane layer, wherein the self-healing functional layer contains a precursor material that can be thermally cyclopolymerized, and / or the precursor material forms a cross-linked polymer structure after the self-healing functional layer self-heals.

[0009] In a second aspect, a method for preparing a composite diaphragm is provided, comprising the following steps:

[0010] preparing a self-healing slurry, wherein the self-healing slurry comprises a precursor material capable of thermal cyclopolymerization;

[0011] At least one base film is obtained, and the self-healing slurry is used to form a self-healing functional layer on the surface of the base film to obtain a composite diaphragm; after the self-healing functional layer is self-healed, the precursor material forms a cross-linked polymer structure.

[0012] In a third aspect, the present application provides a secondary battery, comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the separator comprises the composite separator mentioned above or the composite separator prepared by the above method.

[0013] In a fourth aspect, the present application provides an electrical device, which includes the above-mentioned secondary battery.

[0014] The beneficial effect of the composite diaphragm provided in the embodiment of the present application is that after the composite diaphragm is applied to the battery cell, it plays the role of isolating the positive and negative electrodes, conducting lithium ions, and blocking electrons under normal working conditions of the battery cell. The precursor material that can be thermally cyclized and polymerized in the self-healing functional layer on the surface of the base film layer is electrochemically stable and does not affect the electrochemical performance of the battery cell. When the temperature inside the battery cell rises, the precursor material of the self-healing functional layer will undergo thermal cyclization polymerization under high temperature or thermal runaway conditions of the battery cell, thereby forming a cross-linked polymer structure in situ on the surface of the base film layer. That is, after the self-healing functional layer self-heals, the precursor material forms a cross-linked polymer structure. It plays an effective supporting role for the base film layer, and can effectively prevent and repair the base film layer from undergoing structural changes such as thermal shrinkage, deformation, and closed pores under high temperature or thermal runaway conditions. This allows the composite diaphragm to have a self-healing function and protect the diaphragm. By maintaining the pore structure of the diaphragm unchanged, the current and heat generation in the battery cell can be kept within a normal range, avoiding further contact between the positive and negative electrodes to form a short circuit due to damage and changes in the diaphragm, preventing the increase in short-circuit current, and preventing further deterioration of thermal runaway. In addition, the polymer layer formed after the thermal cyclopolymerization of the precursor material has the characteristics of thermal stability, insulation, low swelling rate, and high toughness, which is beneficial to improving the toughness, mechanical strength, and thermal stability of the composite diaphragm, and has a good thermal protection effect on the composite diaphragm and the battery cell system in which it is applied. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments or exemplary technical descriptions. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0016] FIG1 is a structural schematic diagram of a composite diaphragm according to an embodiment of the present application;

[0017] FIG2 is a second structural diagram of a composite diaphragm according to an embodiment of the present application;

[0018] FIG3 is a third structural diagram of a composite diaphragm according to an embodiment of the present application;

[0019] FIG4 is a fourth structural diagram of a composite diaphragm according to an embodiment of the present application;

[0020] FIG5 is a fifth structural diagram of a composite diaphragm according to an embodiment of the present application;

[0021] FIG6 is a sixth structural diagram of a composite diaphragm according to an embodiment of the present application;

[0022] FIG7 is a seventh structural diagram of a composite diaphragm according to an embodiment of the present application;

[0023] FIG8 is a schematic flow chart of a method for preparing a composite diaphragm according to an embodiment of the present application;

[0024] FIG9 is a schematic structural diagram of an embodiment of a battery cell according to the present application;

[0025] FIG10 is an exploded schematic diagram of the battery cell shown in FIG9 ;

[0026] FIG11 is a schematic structural diagram of an embodiment of a battery module according to the present application;

[0027] FIG12 is a schematic structural diagram of an embodiment of a battery pack according to the present application;

[0028] FIG13 is a schematic diagram of the exploded structure of the battery pack shown in FIG9 ;

[0029] FIG14 is a schematic diagram of an embodiment of an electric device including the secondary battery of an embodiment of the present application as a power source.

[0030] The accompanying drawings in the specific implementation manner are as follows:

[0031] 1. Basement membrane,

[0032] 2. Self-healing functional layer,

[0033] 3. Battery cell, 31. Housing, 32. Electrode assembly, 33. Cover plate;

[0034] 4. Battery module;

[0035] 5. Battery pack, 51. Box, 52. Lower box. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solutions and advantages of this application more clearly understood, the present application is further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit this application.

[0037] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned figure descriptions are intended to cover non-exclusive inclusions.

[0038] In the description of the embodiments of this application, the technical terms "first" and "second" are used only to distinguish different objects and should not be understood to indicate or imply relative importance or implicitly specify the quantity, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of this application, the meaning of "plurality" is more than two, unless otherwise clearly and specifically defined.

[0039] References herein to "embodiments" mean that a particular feature, structure, or characteristic described in connection with the embodiments may be included in at least one embodiment of the present application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0040] The weights of the relevant components mentioned in the examples of this application may not only refer to the specific content of each component, but also represent the weight ratio between the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the examples of this application, it is within the scope disclosed in the examples of this application. Specifically, the mass in the examples of this application may be μg, mg, g, kg, etc., which are mass units known in the chemical industry.

[0041] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).

[0042] The term "air permeability" refers to the degree to which a membrane allows gas to pass through. This value is obtained by measuring the amount of air that can pass through a membrane per unit volume or cross-section per unit time and at a specific pressure. The unit is S / 100mL, representing the time required for 100ml of gas to pass through.

[0043] The term "porosity" refers to the percentage of the pore volume in the separator to the total volume of the material in its natural state.

[0044] The term "thermal shrinkage" refers to the volume change of the diaphragm due to its inherent thermal expansion rate, which is the main cause of shrinkage.

[0045] The term "thermal cyclopolymerization" refers to a polymerization reaction in which a non-conjugated diene compound forms a linear polymer having a cyclic structure repeating unit under heating conditions.

[0046] For the convenience of description, the following embodiments of the present application are described by taking a composite diaphragm and its preparation method and application as an example.

[0047] In a first aspect, an embodiment of the present application provides a composite diaphragm, which includes at least one base membrane layer and a self-healing functional layer laminated and arranged on the surface of the base membrane layer, the self-healing functional layer contains a precursor material that can be thermally cyclized and polymerized, and / or, after the self-healing functional layer self-heals, the precursor material forms a cross-linked polymer structure.

[0048] In the composite separators of the present application, the base membrane layer is a material layer used to separate the positive and negative electrodes in a battery, preventing direct contact between the electrodes and causing a short circuit. While electrons in the battery cannot freely pass through the base membrane layer, ions in the battery can freely pass through it, allowing ions to pass freely between the positive and negative electrodes.

[0049] In the composite diaphragm of the present embodiment, the base membrane layer has at least the following structure:

[0050] In the embodiment, the base film layer may be a single-layer structure, and the self-healing functional layer 2 is provided on one side surface of the base film 1 , as shown in FIG1 .

[0051] In the embodiment, self-healing functional layers 2 are provided on both sides of the base film 1 , as shown in FIG2 .

[0052] In an embodiment, the basement membrane layer may also have a double-layer structure, in which case the self-healing functional layer 2 may be disposed between two basement membranes 1 as an intermediate layer, as shown in FIG3 . The self-healing functional layer 2 may also be disposed on one outer surface of the outermost basement membrane 1, as shown in FIG4 . Alternatively, the self-healing functional layer 2 may be disposed on both outer surfaces of the outermost basement membrane 1, as shown in FIG5 . The self-healing functional layer 2 may also be disposed simultaneously between two basement membranes 1 and on the outer surface of the outermost basement membrane 1, as shown in FIG6 .

[0053] In an embodiment, the basement membrane layer may also be a multi-layer structure, in which case the self-healing functional layer 2 may be arranged between two adjacent basement membranes 1 and multiple self-healing functional layers 2 may be arranged in the basement membrane layer, or may be arranged simultaneously on one outer surface or both outer surfaces of the outermost basement membrane 1, as shown in FIG7 .

[0054] The structure and number of layers of the composite diaphragm in the embodiment of the present application can be flexibly designed according to actual application requirements to meet the requirements of different battery systems for diaphragm performance.

[0055] Thus, the composite diaphragm of the embodiment of the present application has at least the following beneficial effects:

[0056] First, the composite diaphragm includes at least one base film layer and a self-healing functional layer laminated and arranged on the surface of the base film layer. The self-healing functional layer contains a precursor material that can be thermally cyclopolymerized. The formation of the precursor material forms a self-healing functional layer on the surface of the base film layer, which can reduce the significant increase in the weight of the composite diaphragm caused by the functional layer, and avoid the excessive weight of the composite diaphragm due to the introduction of the functional layer, which affects the application of the diaphragm in the battery system. After the composite diaphragm is applied to the battery cell, it plays the role of isolating the positive and negative electrodes, conducting lithium ions, and blocking electrons under the normal working state of the battery cell. The precursor material that can be thermally cyclopolymerized in the self-healing functional layer on the surface of the base film layer is electrochemically stable and does not affect the electrochemical performance of the battery cell.

[0057] Secondly, when the temperature inside the battery cell rises, the precursor material of the self-healing functional layer will undergo thermal cyclopolymerization under high temperature or thermal runaway conditions, thereby forming a cross-linked polymer structure in situ on the surface of the base film layer. That is, after the self-healing functional layer heals, the precursor material forms a cross-linked polymer structure. It plays an effective supporting role for the base film layer, and can effectively prevent and repair the base film layer from undergoing structural changes such as thermal shrinkage, deformation, and closed pores under high temperature or thermal runaway conditions. It gives the composite diaphragm a self-healing function and forms a protective effect on the diaphragm. By maintaining the pore structure of the diaphragm unchanged, the current and heat generation in the battery cell can be kept within the normal range, avoiding further contact between the positive and negative electrodes to form a short circuit due to damage and changes in the diaphragm, preventing the increase of the short-circuit current, and preventing further deterioration of thermal runaway.

[0058] Third, the polymer layer formed after the thermal cyclopolymerization of the precursor material has the characteristics of thermal stability, insulation, low swelling rate, high toughness, etc., which is beneficial to improving the toughness, mechanical strength and thermal stability of the composite diaphragm, and has a good thermal protection effect on the composite diaphragm and the battery cell system in which it is used.

[0059] In some specific embodiments, the basement membrane layer comprises a double-layer basement membrane, and the self-healing functional layer is disposed on the outer surface of the basement membrane layer. In this case, when the basement membrane layer has a double-layer structure, the self-healing functional layer disposed on the outer surface of the basement membrane layer can further enhance the self-healing effect of the basement membrane layer, promptly repairing structural changes such as thermal shrinkage deformation and closed pores in the basement membrane, and improving the toughness, mechanical strength, and thermal stability of the composite diaphragm.

[0060] In some possible embodiments, the precursor material is heated at a temperature of 80 to 500°C to undergo a cyclopolymerization reaction. Under conditions of a temperature of 80 to 500°C, the precursor material in the self-healing functional layer can be heated to undergo a cyclopolymerization reaction to form a cross-linked polymer structure, and further form a cross-linked network structure. The cyclization temperature of different precursor materials will be different. In actual application, appropriate cyclization conditions are set according to the physicochemical properties of the precursor material. In addition, the ambient temperature of 80 to 500°C in the embodiment of the present application covers the baking process temperature of the composite diaphragm assembled into the battery cell, the temperature that can be reached by the normal operation of the battery, and the temperature conditions that can be reached when the battery is in a thermal runaway state. Therefore, after the composite diaphragm is applied to the battery cell, the precursor material in the self-healing functional layer can undergo a thermal cyclopolymerization reaction to form a cross-linked polymer structure under conditions such as the battery cell baking process, the battery operation heating stage, or the battery cell thermal runaway. A thermal protection layer is formed on the surface of the base film layer to improve the toughness, mechanical strength, heat resistance and other properties of the composite diaphragm.

[0061] Illustratively, the precursor material undergoes cyclopolymerization reaction when heated at a temperature of 80-100°C, 100-120°C, 120-150°C, 150-200°C, 200-250°C, 250-300°C, 300-350°C, 350-400°C, 400-450°C, 450-500°C, 100-400°C, 200-300°C, etc.

[0062] In some possible embodiments, the precursor material undergoes a cyclopolymerization reaction when heated in an environment of 120 to 250°C. In this case, the precursor material in the self-healing functional layer can undergo cyclopolymerization when heated in an environment of 120 to 250°C, thereby effectively ensuring that the precursor material can fully undergo cyclopolymerization to form a cross-linked polymer structure layer under the condition of thermal runaway of the battery. Exemplarily, the temperature at which the precursor material undergoes a cyclopolymerization reaction when heated can be 120 to 150°C, 150 to 180°C, 180 to 200°C, 200 to 220°C, 220 to 250°C, and the like.

[0063] In some possible embodiments, the precursor material includes at least one of an aromatic ether compound, an aromatic olefin compound, and an aromatic silane monomer. These precursor materials can undergo thermal cyclopolymerization reaction under high temperature or thermal runaway conditions of the battery cell to form a cross-linked polymer network structure, which plays a protective role on the base film. In addition, these precursor materials all contain aromatic structures. The aromatic rings in the cross-linked polymer layer formed after thermal cyclopolymerization can increase the mechanical properties and thermal stability of the polymer, so that the polymer layer containing aromatic rings has excellent mechanical strength and thermal stability and other properties. In addition, the precursor material also contains functional groups such as ether bonds and silane bonds, which can increase the flexibility of the cross-linked polymer after thermal cyclopolymerization, thereby improving the flexibility of the composite diaphragm. After application to the battery cell, it is beneficial for the composite diaphragm to cope with the volume expansion / deformation of the electrode during the charge and discharge process.

[0064] In some possible embodiments, the aryl ether compound includes at least one of: a diarylmethane sulfide compound, an aryl disulfide compound, and a fluorinated aryl vinyl ether compound. The general structural formula of these aryl ether compounds can be expressed as Ar—O—Ar' or Ar—O—R, wherein Ar and Ar' are aromatic groups, R is an alkyl group, and - represents a connecting chemical bond. These aryl ether precursor materials can undergo thermal cyclopolymerization reactions under high temperature or thermal runaway conditions of the battery cell. The cross-linked polymer network structure formed contains aromatic ring groups, which can increase the mechanical properties and thermal stability of the polymer. On the other hand, the ether bond can increase the flexibility of the polymer molecular chain, thereby ensuring the flexibility of the polymer after being composited with the base film, and ensuring the toughness of the composite diaphragm. In addition, it also contains elements such as fluorine, which can improve the solvent resistance and oil resistance of the polymer, thereby reducing the swelling rate of the composite diaphragm and improving its liquid absorption effect.

[0065] In some possible embodiments, the aromatic olefin compound includes at least one of: fluorinated vinyl aromatic ether, γ-hydroxyalkyl enol ether, and bromobenzene derivatives. Among them, bromobenzene derivatives include but are not limited to a series of bromobenzene derivatives generated by the reaction of o-lithium bromobenzene with an electrophilic reagent acetophenone. These aromatic olefin compound precursor materials undergo thermal cyclopolymerization under high temperature or battery core thermal runaway conditions to form a cross-linked spatial network structure. The presence of aromatic ring groups can increase the mechanical properties and thermal stability of the polymer. It is beneficial to enhance the supporting effect of the self-healing functional layer on the base membrane, and can prevent and repair the irreversible structural changes such as thermal shrinkage, deformation, and closed pores in the base membrane layer under high temperature or battery core thermal runaway conditions, forming a protective effect on the base membrane layer. By maintaining the pore structure of the diaphragm unchanged, the current and heat generation in the battery cell can be kept within the normal range, avoiding further contact between the positive and negative electrodes to form a short circuit due to damage and changes in the diaphragm, preventing the increase of the short-circuit current, effectively preventing short circuits and deterioration in the battery cell, and having a good thermal protection effect on the battery cell.

[0066] In some possible embodiments, the aryl silane monomer includes at least one of [4-trifluorovinyl aryl ether] methyldiethoxysilane, 1,2,3,3,4,4-hexafluoro-1,2-bis[4-(dimethylsilyl)aryl ether] cyclobutane, and 1,1,3,3-tetramethyl-1,3-bis[4-trifluorovinyl aryl ether] disiloxane. These aryl silane monomer precursors undergo thermal cyclopolymerization at high temperatures or under thermal runaway conditions to form a macromonomer with a cross-linked fluorinated polyarylsiloxane network structure. This organosilane macromonomer has excellent thermal and insulating properties, high mechanical strength and plasticity, good compatibility with the base film, and protects the base film layer, effectively improving the mechanical properties and heat resistance of the composite diaphragm.

[0067] In some possible embodiments, the self-healing functional layer further includes at least one of a binder and a dispersant. In this case, the binder has excellent adhesive properties, and through adhesion and cohesion, the thermally cyclizable precursor material in the self-healing functional layer is bonded to the surface of the base film layer to form a stable film layer. The dispersant helps ensure the uniform distribution of the thermally cyclizable precursor material in the self-healing functional layer, improves the uniformity and flatness of the film layer, and ensures that under subsequent high temperature or battery thermal runaway conditions, the precursor material can form a uniform cross-linked network structure film layer on the surface of the base film layer, thereby improving the thermal stability, mechanical properties, toughness, and other properties of the base film layer.

[0068] In some possible embodiments, in the self-healing functional layer, the mass ratio of the precursor material, the binder and the dispersant is (70-99.9): (0.1-25): (0.1-5). Under this ratio, the content of the precursor material ensures that the polymer with a cross-linked network structure formed after thermal cyclopolymerization can fully cover the surface layer of the base film, effectively improving the mechanical properties, thermal stability, toughness and other properties of the base film layer, and ensuring the self-healing effect of the base film layer. It effectively inhibits and repairs irreversible structural changes such as thermal shrinkage, deformation, and closed pores of the base film. The ratio of the binder and the dispersant fully ensures the uniformity of the film layer of the self-healing functional layer and the firmness of the bonding between the self-healing functional layer and the base film layer. It avoids problems such as unstable bonding between the self-healing functional layer and the base film layer, resulting in separation of the film layer, weakening of the thermal protection effect, increase in the impedance of the battery cell, and increase in the thickness of the composite diaphragm, thereby reducing the influence of the composite diaphragm on the dynamic performance of the battery cell. Exemplarily, in the self-healing functional layer, the mass ratio of the precursor material, the binder and the dispersant can be (70-99.9): (0.1-20): (0.1-5), (80-99.9): (5-20): (2-4), (70-80): (10-20): (3-5), (75-90): (5-15): (1-3), (80-95): (5-20): (1-2), (85-95): (6-15): (2-4), etc.

[0069] In some possible embodiments, the binder includes at least one of shellac, butyl rubber, carboxymethyl cellulose, polyurethane, polystyrene, polyacrylate, ethylene-vinyl acetate copolymer, vinyl acetate resin, acrylic resin, and chlorinated rubber. These binders all have high adhesive properties, enabling the self-healing functional layer comprising a thermally cyclopolymerizable precursor material to be stably and firmly bonded to the surface of the base film layer. Furthermore, these binders can coexist with the thermally cyclopolymerizable precursor polymer, are insoluble in the electrolyte, have an electrochemical window that covers the operating voltage window of the battery cell, and are applied to the composite separator. After the composite separator is applied to the battery cell, no chemical or electrochemical side reactions occur.

[0070] In some possible embodiments, the dispersant includes at least one of: ethylene glycol type, polyol type, oleyl amino oleate, polycaprolactone polyol-polyethyleneimine block copolymer type dispersant, acrylate polymer dispersant, polyurethane or polyester polymer dispersant. These dispersants can all improve the dispersion uniformity of the precursor material that can be thermally cyclopolymerized in the self-healing functional layer, thereby improving the film uniformity, flatness and other properties of the self-healing functional layer. In addition, these dispersants can coexist with the polymer of the precursor material that can be thermally cyclopolymerized, are insoluble in the electrolyte, and the electrochemical window covers the operating voltage window of the battery cell. When applied to the composite diaphragm, there are no chemical side reactions and electrochemical side reactions after the composite diaphragm is applied to the battery cell.

[0071] In some possible embodiments, the thickness of the self-healing functional layer is 0.01 to 20 μm. Under this thickness condition, the self-healing functional layer not only ensures the improvement of the self-healing effect of the base film layer, but also can effectively reduce and repair the irreversible structural changes such as thermal shrinkage deformation and closed pores of the base film, and can improve the toughness, mechanical strength, thermal properties and other properties of the composite diaphragm, and improve the dynamics of the composite diaphragm after being applied to the battery cell. At the same time, it avoids the problems of the self-healing functional layer being too thin to repair and heal the base film layer, and the functional layer being too thick affecting the mechanical toughness of the composite diaphragm, increasing the battery cell impedance, and reducing the battery cell capacity. Exemplarily, the thickness of the self-healing functional layer can be 0.01 to 0.1 μm, 0.1 to 1 μm, 1 to 2 μm, 2 to 5 μm, 5 to 8 μm, 8 to 10 μm, 10 to 13 μm, 13 to 15 μm, 15 to 18 μm, 18 to 20 μm, etc.

[0072] In some possible embodiments, the thickness of the self-healing functional layer is 1 to 10 μm. Under this thickness condition, the self-healing functional layer is more conducive to taking into account the self-healing effect of the base film layer, and improving the toughness, mechanical strength, and thermal performance of the composite separator, and reducing the spatial occupancy of the composite separator on the internal electrode of the battery cell, thereby reducing the proportion of inactive substances in the battery cell and improving the energy density of the battery cell. Exemplary thicknesses of the self-healing functional layer can be 1 to 2 μm, 2 to 3 μm, 3 to 4 μm, 4 to 5 μm, 5 to 6 μm, 6 to 7 μm, 7 to 8 μm, 8 to 9 μm, 9 to 10 μm, etc.

[0073] In some possible embodiments, the thickness of the base film layer is 0.1 to 100 μm. The thickness range of the base film layer includes the requirements for the thickness of the diaphragm in the current conventional battery system, so that the composite diaphragm can meet the requirements of different battery systems for the thickness of the diaphragm and has a wide range of applications. In practical applications, the appropriate thickness of the base film layer can be selected according to the specific application requirements. For example, the thickness of the base film layer can be 0.1 to 1 μm, 1 to 10 μm, 10 to 20 μm, 20 to 30 μm, 30 to 40 μm, 40 to 50 μm, 50 to 60 μm, 60 to 70 μm, 70 to 80 μm, 80 to 90 μm, 90 to 100 μm, etc.

[0074] In some possible embodiments, the thickness of the base film layer is 5 to 20 μm. Under this condition, the thickness of the base film layer can effectively ensure the migration and transmission efficiency of ions in the positive and negative electrodes in the battery cell, and is conducive to the lightweight design of the battery cell and improves the energy density of the battery cell. For example, the thickness of the base film layer can be 5 to 7 μm, 7 to 10 μm, 10 to 12 μm, 12 to 15 μm, 15 to 18 μm, 18 to 20 μm, etc.

[0075] In some possible implementations, the base film layer includes at least one material selected from polypropylene (PP), polyethylene (PE), glass fiber, polyvinylidene fluoride, polyimide film, glass fiber film, cellulose film, and polyvinylidene fluoride-hexafluoropropylene film (PVDF+HFP). The materials of these base film layers all have good electrical insulation properties and maintain chemical stability over a wide temperature and voltage range. They are also advantageous in producing a base film layer that is thin in thickness, highly uniform, and has an appropriate porosity and pore size, which can quickly wet the electrolyte, while isolating electrons and maintaining the free flow of ions, to meet the requirements of high energy, high power, and cycle performance of the battery. Furthermore, they also have a certain mechanical strength and processing strength to meet the needs of the battery during assembly and use.

[0076] In some possible embodiments, in the composite diaphragm, the mass ratio of the self-healing functional layer to the base film layer is (0.1-1):1. In the case of this mass ratio, it can fully ensure that the self-healing functional layer reduces and repairs the irreversible structural changes of the base film such as thermal shrinkage deformation and closed pores, ensures its self-healing effect on the base film layer, and improves the toughness, mechanical strength, thermal properties and other characteristics of the base film layer; it can also improve the dynamics of the composite diaphragm after being applied to the battery cell, and improve the energy density of the battery cell. Exemplarily, the mass ratio of the self-healing functional layer to the base film layer can be (0.1-0.3):1, (0.3-0.5):1, (0.5-0.8):1, (0.8-1.0):1, etc.

[0077] In some possible embodiments, the thermal shrinkage of the composite diaphragm is reduced by 15 to 55% relative to the base film layer. The composite diaphragm of the embodiment of the present application includes a self-healing functional layer. Under high temperature or battery thermal runaway conditions, the precursor material in the functional layer can undergo a thermal cyclopolymerization reaction, generating an in-situ cross-linked network structure on the surface of the base film layer, which has a self-healing effect on the structural changes of the base film layer and improves the thermal stability of the base film layer. As a result, the composite diaphragm has excellent thermal properties and can significantly reduce the thermal shrinkage of the composite diaphragm. Compared with a base film layer without a self-healing functional layer, the thermal shrinkage of the composite diaphragm comprising the base film layer and the self-healing functional layer can be reduced by 15 to 55%. For example, relative to the base film layer, the thermal shrinkage of the composite diaphragm can be reduced by 15 to 20%, 20 to 25%, 25 to 30%, 30 to 35%, 35 to 40%, 40 to 45%, 45 to 50%, etc.

[0078] In some possible embodiments, the porosity of the composite membrane is 30-70%. For example, the porosity of the composite membrane can be 30-40%, 40-50%, 50-60%, 60-70%, etc.

[0079] In some possible embodiments, the composite membrane has an air permeability of 100-250 s / 100 mL. For example, the air permeability may be 100-120 s / 100 mL, 120-150 s / 100 mL, 150-180 s / 100 mL, 180-200 s / 100 mL, 200-230 s / 100 mL, 230-250 s / 100 mL, etc.

[0080] The precursor materials that can be thermally cyclized and polymerized in the self-healing functional layer set in the composite membrane of the embodiment of the present application exist separately before thermal cyclization, and the precursor materials that can be thermally cyclized and polymerized after thermal cyclization are thermally cyclized to form a cross-linked network structure, which will not affect the parameters such as the porosity and permeability of the composite membrane, and will not affect the dynamic characteristics of the membrane.

[0081] The composite diaphragm of the above embodiment of the present application can be prepared by the following embodiment method.

[0082] As shown in FIG8 , in a second aspect, an embodiment of the present application provides a method for preparing a composite diaphragm, comprising the following steps:

[0083] S10. Preparing a self-healing slurry, wherein the self-healing slurry comprises a precursor material that can be thermally cyclopolymerized;

[0084] S20. Obtain at least one base film, and form a self-healing functional layer on the surface of the base film with a self-healing slurry to obtain a composite diaphragm; after the self-healing functional layer self-heals, the precursor material forms a cross-linked polymer structure.

[0085] The preparation method of the composite diaphragm provided in the embodiment of the present application, after preparing a self-healing slurry containing a precursor material that can be thermally cyclopolymerized, the self-healing slurry is made into a self-healing functional layer on the surface of the base film to obtain a composite diaphragm. The preparation process is simple, the conditions are mild, and it is suitable for industrial large-scale production and application. In the prepared composite diaphragm, the self-healing functional layer has an excellent self-healing effect on the base film layer. Under high temperature or battery core thermal runaway conditions, the precursor material will undergo thermal cyclopolymerization, and a cross-linked polymer structure will be formed in situ on the surface of the base film layer, which plays an effective supporting role on the base film layer, preventing and repairing the base film layer from undergoing thermal shrinkage, deformation, closed pores and other structural changes under high temperature or battery core thermal runaway conditions. By maintaining the pore structure of the diaphragm unchanged, the current and heat generation in the battery cell can be kept within the normal range, avoiding further contact between the positive and negative electrodes to form a short circuit due to damage and changes in the diaphragm, preventing the increase of the short-circuit current, and preventing further deterioration of thermal runaway. The toughness, mechanical strength and thermal stability of the composite diaphragm are improved, and the composite diaphragm and the battery cell system used therein have a good thermal protection effect.

[0086] In the above step S10, a self-healing slurry containing a thermally cyclopolymerizable precursor material is prepared. The thermally cyclopolymerizable precursor material in the slurry will undergo thermal cyclopolymerization under high temperature or thermal runaway conditions of the battery cell, and form an in situ cross-linked polymer structure on the surface of the base film layer, thereby making the composite diaphragm have a self-healing function.

[0087] In some possible embodiments, the step of preparing a self-healing slurry includes: preparing a precursor material, and then mixing it with a binder, a dispersant, and a solvent to form a self-healing slurry. In this case, the binder has excellent bonding properties, and the precursor material that can be thermally cyclized and polymerized in the self-healing functional layer is bonded to the surface of the base film layer through adhesion and cohesion to form a stable film layer. The dispersant is beneficial to ensure that the precursor material that can be thermally cyclized and polymerized in the self-healing functional layer is evenly distributed, thereby improving the uniformity and flatness of the film layer. The solvent allows the components to be fully dispersed and dissolved to form a stable slurry system, which is convenient for the subsequent preparation of the self-healing functional film layer.

[0088] In some possible embodiments, the mass ratio of the precursor material, binder, and dispersant in the self-healing slurry is (70-99.9): (0.1-25): (0.1-5). Under this ratio, the content of the precursor material ensures that the cross-linked network structure formed by the thermal cyclopolymerization can fully cover the surface layer of the base film, effectively improving the mechanical properties, thermal stability, toughness, and other characteristics of the base film layer, and ensuring the self-healing effect of the base film layer.

[0089] In some possible embodiments, the solid content of the self-healing slurry is 30-80%. For example, the solid content of the self-healing slurry can be 30-40%, 40-50%, 50-60%, 60-70%, 70-80%, 80-90%, etc. At this solid content, the precursor material, binder, dispersant and other components are uniformly and stably dissolved and dispersed, and the self-healing slurry is conducive to forming a self-healing functional layer on the surface of the base film.

[0090] In some possible embodiments, the precursor material includes at least one of an aromatic ether compound, an aromatic olefin compound, and an aromatic silane monomer. These precursor materials can undergo thermal cyclopolymerization reaction under high temperature or thermal runaway conditions of the battery cell to form a cross-linked polymer network structure, which plays a protective role on the base film. In addition, these precursor materials all contain aromatic structures. The aromatic rings in the cross-linked polymer layer formed after thermal cyclopolymerization can increase the mechanical properties and thermal stability of the polymer, so that the polymer layer containing aromatic rings has excellent mechanical strength and thermal stability and other properties. In addition, the precursor material also contains functional groups such as ether bonds and silane bonds, which can increase the flexibility of the cross-linked polymer after thermal cyclopolymerization, thereby improving the flexibility of the composite diaphragm. After application to the battery cell, it is beneficial for the composite diaphragm to cope with the volume expansion / deformation of the electrode during the charge and discharge process.

[0091] In some possible embodiments, the aryl ether compound includes at least one of a diarylmethane sulfide compound, an aryl disulfide compound, and a fluorinated aryl vinyl ether compound. These aryl ether compound precursor materials can undergo thermal cyclopolymerization under high temperature or thermal runaway conditions of the battery cell. The cross-linked polymer network structure formed contains aromatic ring groups, which can increase the mechanical properties and thermal stability of the polymer. On the other hand, the ether bond can increase the flexibility of the polymer molecular chain, thereby ensuring the flexibility of the polymer after being composited with the base film and ensuring the toughness of the composite diaphragm. In addition, it also contains elements such as fluorine, which can improve the solvent resistance and oil resistance of the polymer, thereby reducing the swelling rate of the composite diaphragm and improving its liquid absorption effect.

[0092] In some possible embodiments, the preparation of an aryl olefin compound includes the steps of: reacting a halogenated aryl non-conjugated olefin compound with an organolithium reagent to undergo a lithium-halogen exchange reaction to obtain an aryl olefin lithium; and reacting the aryl olefin lithium with an electrophilic reagent to undergo an electrophilic addition reaction to obtain an aryl olefin compound. In this case, a halogenated aryl non-conjugated diene compound is reacted with an organolithium reagent to undergo a lithium-halogen exchange reaction to obtain an organolithium radical cation and a halogenated olefin anion, respectively. The lithium ion and the halogen ion are eliminated to form two carbon radical intermediates, which ultimately undergo disproportionation and recombine to obtain a new aryl olefin lithium reagent. The selectivity of the lithium-halogen exchange reaction is controlled by the stability of the formed carbon anion. Because the carbon anion of the organolithium reagent is stable, it is highly active and lithium can replace the position of the halogen element. The aryl olefin lithium generated after the lithium-halogen exchange reaction has nucleophilic reagent characteristics and has strong electron donating ability. It can spontaneously react with electrophilic reagents (with strong electron accepting ability) to undergo atom transfer, free radical recombination, and unsaturated bond addition-fragmentation. Therefore, an electrophilic reagent is used to attack the unsaturated bond of the aromatic olefin lithium to cause an electrophilic addition reaction, the molecular weight of the monomer increases, and the molecular chain becomes longer, that is, a thermal polymerization precursor material of an aromatic olefin compound macromonomer with stable room temperature performance is obtained.

[0093] In some possible embodiments, the molar mass ratio of the halogenated aryl non-conjugated olefin compound, the organolithium reagent, and the electrophilic reagent is (0.4-0.8):(0.1-0.4):(0.1-0.2). Under this ratio, the lithium-halogen exchange reaction between the halogenated aryl non-conjugated olefin compound and the organolithium reagent, as well as the electrophilic addition reaction between the aromatic olefin lithium and the electrophilic reagent, are fully ensured.

[0094] In some possible embodiments, the halogenated aryl non-conjugated olefin compound includes at least one of bromo-trifluorovinyloxybenzene, trifluorovinyl aryl ether, and perfluorocyclobutyl aryl ether. These are all compounds containing non-conjugated dienes and are capable of undergoing a lithium-halide displacement reaction with an organolithium reagent. Because the organolithium reagent's carbon anion is stable, it is highly active. Lithium can replace the halogen element, eliminating the lithium ion and the halogen ion to form two carbon free radical intermediates, which ultimately undergo disproportionation and recombine to obtain a new aryl olefin lithium reagent.

[0095] In some possible embodiments, the organolithium reagent includes at least one of butyllithium, lithium hexamethyldisilazide, phenyllithium, n-hexyllithium, lithium diisopropylamide, and n-butyllithium. The carbon anions of these organolithium reagents are stable and highly reactive, and lithium can replace the halogen element in halogenated aromatic non-conjugated olefin compounds. This results in a strong nucleophilic reaction for the resulting lithiated compound, facilitating subsequent thermal cyclopolymerization.

[0096] In some possible embodiments, the electrophilic reagent includes at least one of a hydrogen halide, a halogenated hydrocarbon, an acyl halide, a carbonyl compound, expanded hydrogen, diisobutylaluminum hydride, diisopropylphosphoric acid fluoride, isopropyl methylphosphoric acid fluoride, and iodoacetic acid. These electrophiles have strong electron-accepting abilities, and the aromatic olefin lithium generated after the lithium-halide exchange has nucleophilic properties and strong electron-donating ability. Therefore, it can spontaneously react with these electrophiles, causing atom transfer, free radical recombination, and unsaturated bond addition-breakage, resulting in molecular chain lengthening, thereby obtaining an aromatic olefin macromonomer thermal polymerization precursor material.

[0097] In some possible embodiments, the reaction temperature for preparing aromatic olefin compounds may be 75-450° C., and in the actual preparation process, appropriate reaction temperature conditions may be set according to the physicochemical properties of the raw material components.

[0098] In some possible embodiments, the preparation of the aryl silane monomer includes the steps of: condensing a silicate compound with a halogenated olefin ether compound in the presence of a catalyst to produce the aryl silane monomer. In this case, the condensation reaction of the silicate compound and the halogenated olefin ether compound in the presence of a catalyst forms a functionalized aryl silane monomer. This monomer, upon heating, can form a cross-linked polyaryl siloxane network structure, imparting self-healing properties to the composite membrane and improving the toughness, mechanical strength, thermal stability, and other properties of the composite membrane.

[0099] In some possible embodiments, the mass ratio of the total mass of the silicate compound and the halogenated olefin ether compound to the catalyst is 1:(0.01-0.5). When this amount of catalyst is used, the reaction free energy can be effectively reduced, fully ensuring the condensation reaction between the silicate compound and the halogenated olefin ether compound. For example, the mass ratio of the total mass of the silicate compound and the halogenated olefin ether compound to the catalyst can be 1:(0.01-0.05), 1:(0.05-0.1), 1:(0.1-0.2), 1:(0.2-0.3), 1:(0.3-0.4), 1:(0.4-0.5), etc.

[0100] In some possible embodiments, the molar ratio of the silicate compound to the halogenated olefin ether compound can be (1-1.2): (1-1.2), and illustratively, it can be 1:1, 1:1.1, 1:1.2, 1.2:1, 1.1:1, etc., to ensure complete reaction of the reactants, and can also be any other ratio that can promote the efficiency of the condensation reaction.

[0101] In some possible implementations, the silicate compound includes at least one of tetraethoxysilane, vinyltrimethoxysilane, triethoxysilane, methyl ether dimethyl silane, and triisopropylsilane.

[0102] In some possible embodiments, the halogenated olefin ether compound includes at least one of trifluorovinyl aryl ether, distyryl ether, brominated distyryl ether, perfluoromethyl isopropyl ether, perfluoroisobutyl vinyl ether, and hexafluoroisopropenyl methyl ether.

[0103] In some possible embodiments, the catalyst is selected from metallocene catalysts, specifically, the catalyst includes at least one of organic boron compound (B(C6F5)3) and alkylaluminoxane (MAO).

[0104] The silicate compounds and halogenated olefin ether compounds used in the above-mentioned embodiments of this application, under the action of metallocene catalysts, effectively reduce the free energy of the reaction, and both undergo condensation reactions to obtain novel functionalized arylsilane monomers, namely organosiloxane macromonomers. These monomers exhibit high-temperature thermal polymerization properties, a large mass-average molecular weight exceeding 10,000, a high degree of polymerization, high mechanical strength and plasticity, excellent heat resistance, and good compatibility with the base film.

[0105] In some possible embodiments, the binder includes at least one of shellac, butyl rubber, carboxymethyl cellulose, polyurethane, polystyrene, polyacrylate, ethylene-vinyl acetate copolymer, vinyl acetate resin, acrylic resin, and chlorinated rubber. These binders all have high adhesive properties, enabling the self-healing functional layer comprising a thermally cyclopolymerizable precursor material to be stably and firmly bonded to the surface of the base film layer. Furthermore, these binders can coexist with the thermally cyclopolymerizable precursor polymer, are insoluble in the electrolyte, have an electrochemical window that covers the operating voltage window of the battery cell, and are applied to the composite separator. After the composite separator is applied to the battery cell, no chemical or electrochemical side reactions occur.

[0106] In some possible embodiments, the dispersant includes at least one of: ethylene glycol type, polyol type, oleyl amino oleate, polycaprolactone polyol-polyethyleneimine block copolymer type dispersant, acrylate polymer dispersant, polyurethane or polyester polymer dispersant. These dispersants can all improve the dispersion uniformity of the precursor material that can be thermally cyclopolymerized in the self-healing functional layer, thereby improving the film uniformity, flatness and other properties of the self-healing functional layer. In addition, these dispersants can coexist with the polymer of the precursor material that can be thermally cyclopolymerized, are insoluble in the electrolyte, and the electrochemical window covers the operating voltage window of the battery cell. When applied to the composite diaphragm, there are no chemical side reactions and electrochemical side reactions after the composite diaphragm is applied to the battery cell.

[0107] In some possible embodiments, the solvent includes at least one of water, methanol, ethanol, NMP, acetone, tetrachloroethylene, dichloroethane, trichloroethane, anisole, propanol, butyl acetate, and tetrahydrofuran. These solvents not only have a high solubility effect on components such as precursor materials, dispersants, and binders, but are also small molecules with stable chemical properties, which helps to improve the stability of the self-healing slurry.

[0108] In the above step S20, after obtaining at least one base film, the method of forming a self-healing functional layer on the surface of the base film with the self-healing slurry includes but is not limited to forming a slurry wet film on the surface of the base film by coating, spraying, etc., and then drying the self-healing slurry to volatilize the solvent and solidify the film layer, thereby forming a tightly bonded and stable self-healing functional layer on the surface of the base film to obtain a composite diaphragm. After the composite diaphragm is applied to the battery cell, it plays the role of isolating the positive and negative electrodes, conducting lithium ions, and blocking electrons. The electrochemical stability of the precursor material that can be thermally cyclized and polymerized in the self-healing functional layer on the surface of the base film layer does not affect the electrochemical performance of the battery cell. When the battery cell is overheated or thermally runaway, the thermally cyclizable precursor material in the self-healing functional layer undergoes a thermal polymerization reaction to form a cross-linked polymer structure, which effectively supports the base membrane layer and effectively prevents and repairs the base membrane layer from undergoing structural changes such as thermal shrinkage, deformation, and closed pores under high temperature or thermal runaway conditions. The composite diaphragm has a self-healing function and forms a protective effect on the diaphragm. By maintaining the pore structure of the diaphragm unchanged, the current and heat generation in the battery cell can be kept within a normal range, avoiding further contact between the positive and negative electrodes to form a short circuit due to damage and changes in the diaphragm, preventing the increase of the short-circuit current, and preventing further deterioration of thermal runaway.

[0109] In a third aspect, an embodiment of the present application provides a secondary battery, which includes a positive electrode, a negative electrode, a separator and an electrolyte, wherein the separator includes the above-mentioned composite separator or the composite separator prepared by the above-mentioned method.

[0110] In the secondary battery of the embodiment of the present application, since the diaphragm includes the above-mentioned composite diaphragm, the surface of the base film layer of the composite diaphragm is provided with a self-healing functional layer. Under normal operating conditions of the secondary battery, the composite diaphragm plays the role of isolating the positive and negative electrodes, conducting lithium ions, and blocking electrons. When the secondary battery is overheated or thermally runaway, the precursor material that can be thermally cyclized and polymerized in the self-healing functional layer undergoes a thermal polymerization reaction to generate a high-temperature resistant, high-mechanical-strength cross-linked polymer, which not only supports the diaphragm, but also suppresses irreversible deformations such as thermal closure and thermal shrinkage of the base film. The spatial structure of the cross-linked polymer can also repair the damage to the local pore structure of the base film. Therefore, it can effectively prevent the further deterioration of the thermal runaway of the secondary battery, play a good thermal protection role for the secondary battery system, and significantly improve the safety performance and electrochemical performance of the secondary battery.

[0111] This application does not specifically limit the positive electrode, negative electrode, electrolyte, etc. in the secondary battery of the embodiment, and is applicable to any battery system.

[0112] In some possible implementations, the negative electrode materials in the secondary battery include but are not limited to carbon materials such as graphite, soft carbon (such as coke), hard carbon, or nitrides, tin-based oxides, tin-based oxides, tin alloys, and silicon-based negative electrode materials.

[0113] In some possible implementations, the preparation of the negative electrode sheet includes the following steps: mixing the negative electrode material with a conductive agent such as conductive carbon black, a binder such as carboxymethyl cellulose and styrene-butadiene rubber, and a solvent such as water in a mass ratio of (80-99):(1-5):(2-10):100 to form a positive electrode mixed slurry, vacuum degassing, discharging, coating on a coating machine, and obtaining a negative electrode sheet after rolling, slitting, and die-cutting.

[0114] In some possible implementations, the positive electrode materials in secondary batteries include metal oxides, such as lithium cobalt oxide, lithium nickel oxide, nickel-cobalt-manganese ternary materials, lithium nickel-cobalt-aluminum oxide, lithium-rich manganese-based materials, lithium manganate, lithium nickel-manganese oxide, ferroferric oxide, lithium vanadate, etc.; polyanion salts such as phosphates, silicates, sulfates, borates, and titanates, such as lithium iron phosphate, lithium manganese phosphate, lithium iron manganese phosphate, lithium vanadium phosphate, lithium vanadium phosphate, lithium cobalt phosphate, lithium nickel phosphate, lithium iron silicate, lithium iron fluorosulfate, lithium iron borate, and lithium iron titanate; and fluorides, sulfides, and selenides, such as iron trifluoride, cobalt trifluoride, nickel trifluoride (NiF3), titanium disulfide, iron disulfide, molybdenum disulfide, and niobium triselenide.

[0115] In some possible implementations, the preparation of the positive electrode sheet includes the following steps: mixing the positive electrode material with a conductive agent such as conductive carbon black, a binder such as polyvinylidene fluoride, and a solvent such as N-methylpyrrolidone in a mass ratio of (80-99):(1-5):(2-10):100 to form a positive electrode mixed slurry, vacuum degassing, discharging, coating on a coating machine, and obtaining a positive electrode sheet after rolling, slitting, and die-cutting.

[0116] In some possible implementations, the electrolyte in the secondary battery includes at least one soluble metal salt.

[0117] In some possible implementations, the secondary battery includes at least one of a battery cell, a battery module, and a battery pack.

[0118] In some possible implementations, battery cell types include lithium-ion batteries, as well as new types of batteries such as sodium-ion batteries, lithium-air batteries, and lithium metal batteries.

[0119] In some possible implementations, the present invention has no particular restrictions on the shape of the battery cell, which can be cylindrical, square, or any other shape. FIG9 shows a battery cell 3 with a square structure as an example.

[0120] In some embodiments, as shown in Figure 10, the outer packaging of the battery cell 3 may include a shell 31 and a cover plate 33. The shell 31 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 31 has an opening connected to the receiving cavity, and the cover plate 33 is used to cover the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 32 through a winding process and / or a lamination process. The electrode assembly 32 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 32. The number of electrode assemblies 32 contained in the battery cell 3 can be one or more, which can be adjusted according to actual needs. Among them, the composite diaphragm of the above embodiment is arranged between the positive electrode sheet and the negative electrode sheet.

[0121] In some possible implementations, the battery cells according to the present application may be assembled into a battery module. The battery module may contain multiple battery cells, and the specific number may be adjusted according to the application and capacity of the battery module.

[0122] In one possible embodiment, as shown in FIG11 , a schematic diagram of an exemplary battery module 4 is shown. In the battery module 4, multiple battery cells 3 may be arranged sequentially along the length of the battery module 4. Of course, the arrangement may also be arranged in any other manner. Furthermore, the multiple battery cells 3 may be secured using fasteners.

[0123] In a possible embodiment, the battery module 4 may further include a housing having a receiving space, and the plurality of battery cells 3 are received in the receiving space.

[0124] In a possible implementation, the above-mentioned battery cells and / or battery modules may also be assembled into a battery pack, and the number of battery cells or battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.

[0125] In one possible embodiment, as shown in Figures 12 and 13 , a schematic diagram of an exemplary battery pack 5 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box includes an upper box body 51 and a lower box body 52. ​​The upper box body 51 covers the lower box body 52 and forms an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 may be arranged in any manner within the battery box.

[0126] In a fourth aspect, an embodiment of the present application provides an electrical device, which includes the above-mentioned secondary battery.

[0127] The electrical equipment of the embodiment of the present application includes the secondary battery with high safety performance and excellent electrochemical performance, thereby improving the power safety and stability of the electrical equipment.

[0128] In a possible implementation, the electrical equipment may select the above-mentioned battery cells, battery modules or battery packs according to its usage requirements.

[0129] In one possible embodiment, the electrical device may be, but is not limited to, a mobile device, such as a mobile phone, a laptop computer, etc., or an electric vehicle, such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc., or an electric train, a ship, a satellite, an energy storage system, etc.

[0130] In one possible embodiment, the electric device may be a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, etc. In order to meet the high power and high energy density requirements of such electric devices, the above-mentioned battery pack or battery module may be used.

[0131] In some specific embodiments, a schematic diagram of an exemplary electric device is shown in FIG11 . The electric device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the electric device, a battery pack or battery module may be used.

[0132] In other possible implementations, the electrical device may also be a tape recorder, a radio, an electronic learning machine, a mobile phone, a tablet computer, a laptop computer, etc. Such electrical devices are generally required to be lightweight and thin, and the battery cells in the above embodiments may be used as power sources.

[0133] Example

[0134] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.

[0135] Example 1

[0136] The present invention provides a composite membrane, the preparation of which includes the following steps:

[0137] 1. Take a sample of tetraethoxysilane and trifluorovinyl aryl ether in a molar ratio of 1:1, place it in a clean container, maintain a constant temperature of 80°C, add a catalyst (B(C6F3)3), maintain a stirring speed of 100r / min, and react for 2h to prepare an organosiloxane macromonomer of trifluorovinyl aryl ether.

[0138] 2. The organic siloxane macromonomer of trifluorovinyl aryl ether is evenly mixed with polyacrylate and ethylene glycol in a mass ratio of 9:0.6:0.4, 45% by volume of N-methylpyrrolidone solvent (NMP) is added, and stirred at 600 r / min for 30 minutes to prepare a self-healing slurry.

[0139] 3. The self-healing slurry is coated on the surface of a single-layer 7 μm PE base film with a thickness of 3 μm to obtain a composite diaphragm with self-healing function.

[0140] Example 2

[0141] This embodiment provides a composite diaphragm, the preparation of which includes the following steps:

[0142] 1. Trifluorovinyl aryl ether, styrene-butadiene rubber and polyacrylamide were uniformly mixed in a mass ratio of 8.5:1:0.5, 40% by volume of NMP solvent was added, and the mixture was stirred at a speed of 500 r / min for 3 h to prepare a self-healing slurry.

[0143] 2. The self-healing slurry is coated on the surface of the 9μm PP base film with a thickness controlled at 5μm to obtain a composite diaphragm with self-healing function.

[0144] Example 3

[0145] This embodiment provides a composite diaphragm, the preparation of which includes the following steps:

[0146] 1. Completely react p-bromo-trifluoroethyleneoxybenzene with butyl lithium in a molar ratio of 1:1 to obtain an organic lithium compound, and then react the organic lithium compound with an electrophilic reagent iodoacetic acid in a molar ratio of 1:1.05 to ensure that the organic lithium compound reacts completely to obtain a fluorinated vinyl aryl ether.

[0147] 2. The fluorinated vinyl aryl ether, polyvinylidene fluoride (PVDF), and stearic acid monoglyceride were uniformly mixed in a mass ratio of 8.8:0.8:0.4, 45% by volume of NMP solvent was added, and the mixture was stirred at 600 r / min for 30 minutes to prepare a self-healing slurry.

[0148] 3. Spray the self-healing slurry onto the surface of a 20 μm PP / PE composite base film with a thickness of 8 μm. The PP / PE film thickness ratio is 1:1, thereby obtaining a composite diaphragm with self-healing function.

[0149] The air permeability, porosity, thermal shrinkage and other properties of the above-mentioned embodiments and the base film layers used in each embodiment after heat treatment under a high temperature condition were tested respectively.

[0150] 1. Air permeability test method: With the composite diaphragm fixed, apply a certain air pressure to one side of the composite diaphragm. Due to the micropores in the diaphragm, the air pressure will gradually decrease until it equals atmospheric pressure. The time it takes for the pressure to drop from the initial pressure to the final pressure is compared, which is the air permeability of the diaphragm.

[0151] 2. Porosity test method:

[0152] ①. Stack the composite diaphragm into 6 layers, flatten them, press them tightly, and remove the air from the composite diaphragm. Cut the stacked composite diaphragm according to the cutting board, measure the cut sample, and obtain the sample area S.

[0153] ②Measure the thickness of the sample 10 or 20 times and calculate the average value as B.

[0154] ③. Use an electronic balance to measure the weight of the composite diaphragm 3 times and obtain the average value M.

[0155] ④. Calculate by the formula: Porosity p = [(density of composite diaphragm raw material*S*BM) / (density of diaphragm raw material*S*B)]*100%.

[0156] 3. Thermal shrinkage test method:

[0157] ①. Stack the composite diaphragm into 3 layers, flatten them, expel the air between the membranes, take out the cutting plate (300*100), cut out the composite diaphragm membrane samples, and measure the length A1 and width B1 of the cut samples.

[0158] ② Set the oven temperature to 90°C and hold for 1 hour. Place the sample in the oven and hold for 2 hours. Use a stopwatch or the oven's built-in timer to time the sample.

[0159] ③. After 2 hours, take out the composite diaphragm, cool it for 10 minutes, and then measure the length A2 and width B2 of the sample.

[0160] ④. The longitudinal thermal shrinkage of the composite diaphragm (MD) = (A1-A2) / A1*100%; the transverse thermal shrinkage of the diaphragm (TD) = (B1-B2) / B1*100%.

[0161] The test results are shown in Tables 1 to 3 below:

[0162] Table 1 shows the performance test of the composite membrane of Example 1 and the comparative base membrane layer.

[0163] It can be seen from the test results in Table 1 above that tetraethoxysilane (TEOS) and an organosilane containing a trifluorovinyl aryl ether (TFVE) unit in Example 1 of the present application undergo a condensation reaction under the catalytic action of B(C6F5)3, and a new type of TFVE-functionalized trifluorovinyl aryl ether organosiloxane macromonomer is efficiently prepared. After it is made into a self-healing functional layer on the surface of the base film layer, the composite membrane can form a polyarylsiloxane cross-linked network structure bridged by hexafluorocyclobutyl aryl ether (PFCB) under heating conditions. This material has excellent thermal and insulating properties, significantly reduces the thermal shrinkage of the composite membrane, reduces the transverse tensile strength to 15%, and reduces the longitudinal tensile strength to 30%. And the air permeability of the composite membrane is improved. At the same time, under the premise of ensuring the air permeability and thermal shrinkage properties of the membrane, the porosity of the composite membrane is more conducive to avoiding contact between the positive and negative electrodes, reducing leakage current, and thus improving battery safety performance.

[0164] Table 2 shows the performance test of the composite membrane of Example 2 and the comparative base membrane layer.

[0165] As can be seen from the test results in Table 2 above, the trifluorovinyl aryl ether compound in the self-healing functional layer of Example 2 of the present application has the solvent resistance and oil resistance characteristics common to fluoropolymers. The aromatic ring-containing polymer has excellent mechanical strength, thermal stability, and flexibility, significantly improving the heat resistance of the composite membrane and reducing the thermal shrinkage of the composite membrane. The transverse tensile strength is reduced to 18%, and the longitudinal tensile strength is reduced to 28%. The air permeability of the composite membrane is also improved. At the same time, while ensuring the air permeability and thermal shrinkage performance of the membrane, the porosity of the composite membrane is more conducive to avoiding contact between the positive and negative electrodes, reducing leakage current, and thus improving battery safety.

[0166] Table 3 shows the performance test of the composite membrane of Example 3 and the comparative base membrane layer.

[0167] As can be seen from the test results in Table 3 above, Example 3 of the present application shows that bromo-trifluoroethyleneoxybenzene reacts with butyllithium to form a lithium-halogen substitution reaction to obtain a new aromatic olefin lithium. The electrophilic reagent iodoacetic acid attacks the unsaturated bonds of the aromatic olefin lithium, causing an electrophilic addition reaction. The molecular weight of the monomer increases and the molecular chain lengthens, thereby obtaining a fluorinated vinyl aryl ether thermally polymerizable precursor material with stable room temperature performance. After being formed into a self-healing functional layer on the surface of the base film layer, the composite membrane is further polymerized under heating conditions to form a cross-linked spatial network structure. This provides structural support for the base membrane, preventing thermal shrinkage and changes in the pore structure of the base membrane, improving the heat resistance of the composite membrane, and reducing the thermal shrinkage of the composite membrane. The transverse tensile strength is reduced to 20%, and the longitudinal tensile strength is reduced to 30%. The air permeability of the composite membrane is also improved. At the same time, while ensuring the membrane's air permeability and thermal shrinkage, the porosity of the composite membrane is more conducive to avoiding contact between the positive and negative electrodes, reducing leakage current, and thus improving battery safety.

[0168] In addition, assembling the composite separator of each embodiment and the corresponding pure base film layer into the battery cell includes the following steps:

[0169] 1. Positive electrode sheet: Add NMP (N-methylpyrrolidone) solvent to the positive electrode material NCM811, binder PVDF and conductive agent Super-p in a mass ratio of 95:3:2 according to the solid content of 60%, stir for 3 hours with a double planetary mixer, vacuum degassing for 30 minutes, discharge the material, coat it on a coater, and obtain the positive electrode sheet after roller pressing, slitting and die cutting.

[0170] 2. Negative electrode sheet: Graphite, styrene-butadiene rubber SBR / carboxymethyl cellulose CMC and carbon black in a mass ratio of 96:2:2 are added with water at a solid content of 40%, stirred in a double planetary mixer for 3 hours, vacuum degassed for 30 minutes, discharged, coated on a coater, and rolled, slitting and die-cut to obtain the negative electrode sheet.

[0171] 3. Electrolyte: Ethylene carbonate EC / ethyl methyl carbonate EMC volume ratio 3:7 + 1M lithium hexafluorophosphate.

[0172] 4. Cell Assembly: The composite separator prepared in Example and the corresponding pure base film layer were wound with the positive and negative electrode sheets according to conventional processes to produce a core. The core was assembled into a shell, welded and sealed, baked, and then injected with electrolyte, impregnated, formed, and divided into different volumes to obtain a cell. The cell had a designed capacity of 60 Ah, and the electrolyte injection rate was 2.5 g / Ah.

[0173] The temperature change, leakage current, voltage drop and other parameters of the battery cells using the composite diaphragms of various embodiments after thermal runaway were tested respectively.

[0174] 1. Temperature change test method: The temperature sensor is located on the outside of the battery cell. When the battery cell has thermal runaway, the temperature change of the battery cell shell is monitored in real time, and the temperature of the large surface of the battery cell is used to represent the temperature change inside the battery cell.

[0175] 2. Leakage current test method: Connect the battery cell as a current source into a shunt circuit. When the battery cell is short-circuited, the large current change causes the voltmeter in the current circuit to change its reading. The current size can be calculated according to Ohm's law.

[0176] 3. Voltage drop test method: monitor the open circuit voltage V1 before thermal runaway, the open circuit voltage V2 after thermal runaway, and the thermal runaway voltage drop δV = V1-V2.

[0177] The test results are shown in Table 4 below:

[0178] Table 4

[0179] It can be seen from the above test structure that after the composite membrane prepared in the embodiment of the present application is applied to the battery cell, under the condition of thermal runaway of the battery, the thermally cyclizable precursor material in the self-healing membrane is polymerized to form a cross-linked spatial network structure. The polymer network structure has excellent thermal and insulating properties, significantly improves the heat resistance of the composite membrane, reduces the temperature of the composite membrane, prevents thermal shrinkage of the base membrane and changes in the pore structure, significantly reduces leakage current and voltage drop, effectively prevents the deterioration of internal short circuit, and has a good thermal protection effect on the battery cell.

[0180] The above are merely optional embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application should be included within the scope of the claims of the present application.

Claims

1. A composite diaphragm, It is characterized in that The composite diaphragm includes at least one base film layer and a self-healing functional layer laminated and bonded to the surface of the base film layer. The self-healing functional layer contains a precursor material that can be thermally cyclopolymerized, and / or the precursor material forms a cross-linked polymer structure after the self-healing functional layer self-heals.

2. The composite diaphragm according to claim 1, It is characterized in that The precursor material undergoes a cyclopolymerization reaction when heated at a temperature of 80 to 500°C.

3. The composite diaphragm according to claim 1 or 2, It is characterized in that The precursor material undergoes a cyclopolymerization reaction when heated at a temperature of 120 to 250°C.

4. The composite diaphragm according to any one of claims 1 to 3, It is characterized in that The precursor material includes at least one of aryl ether compounds, aryl olefin compounds, and aryl silane monomers.

5. The composite diaphragm according to claim 4, It is characterized in that The aryl ether compound includes at least one of a diarylmethane sulfide compound, an aryl disulfide compound, and a fluorine-containing aryl vinyl ether compound; and / or, the aromatic olefin compound comprises at least one of: fluorinated vinyl aromatic ethers, γ-hydroxyalkyl enol ethers, and bromobenzene derivatives; And / or, the aromatic silane monomer includes at least one of [4-trifluorovinyl aryl ether]methyldiethoxysilane, 1,2,3,3,4,4-hexafluoro-1,2-bis[4-(dimethylsilyl)aryl ether]cyclobutane, and 1,1,3,3-tetramethyl-1,3-bis[4-trifluorovinyl aryl ether]disiloxane.

6. The composite diaphragm according to any one of claims 1 to 5, It is characterized in that The self-healing functional layer further includes at least one of a binder and a dispersant.

7. The composite diaphragm according to claim 6, It is characterized in that In the self-healing functional layer, the mass ratio of the precursor material, the binder and the dispersant is (70-99.9): (0.1-25): (0.1-5); And / or, the binder comprises: at least one of shellac, butyl rubber, carboxymethyl cellulose, polyurethane, polystyrene, polyacrylate, ethylene-vinyl acetate copolymer, vinyl acetate resin, acrylic resin, and chlorinated rubber; And / or, the dispersant includes: at least one of ethylene glycol type, polyol type, oleyl amino oleate, polycaprolactone polyol-polyethyleneimine block copolymer type dispersant, acrylate polymer dispersant, polyurethane or polyester polymer dispersant.

8. The composite diaphragm according to any one of claims 1 to 7, It is characterized in that The thickness of the self-healing functional layer is 0.01 to 20 μm; And / or, the base film layer has a thickness of 0.1 to 100 μm.

9. The composite diaphragm according to claim 8, It is characterized in that The thickness of the self-healing functional layer is 1 to 10 μm; And / or, the base film layer has a thickness of 5 to 20 μm.

10. The composite diaphragm according to any one of claims 1 to 9, It is characterized in that In the composite diaphragm, the mass ratio of the self-healing functional layer to the base film layer is (0.1-1):1; and / or, the thermal shrinkage of the composite diaphragm is reduced by 15 to 55% relative to the base film layer; and / or, the porosity of the composite membrane is 30-70%; And / or, the air permeability of the composite membrane is 100 to 250 s / 100 mL.

11. The composite diaphragm according to any one of claims 1 to 10, It is characterized in that The base film layer is a multi-layer structure, and the self-healing functional layer is arranged between two adjacent base films and / or arranged on the outer surface of the outermost base film.

12. The composite diaphragm according to claim 11, It is characterized in that The base film layer includes a double-layer base film, and the self-healing functional layer is arranged on the outer surface of the base film layer.

13. A method for preparing a composite diaphragm, It is characterized in that The following steps are involved: Preparing a self-healing slurry, wherein the self-healing slurry contains a precursor material capable of thermal cyclopolymerization; At least one base film is obtained, and the self-healing slurry is used to form a self-healing functional layer on the surface of the base film to obtain a composite diaphragm; after the self-healing functional layer is self-healed, the precursor material forms a cross-linked polymer structure.

14. The method for preparing the composite diaphragm according to claim 13, It is characterized in that The step of preparing the self-healing slurry comprises: preparing the precursor material, and then mixing it with a binder, a dispersant and a solvent to form the self-healing slurry.

15. The method for preparing the composite diaphragm according to claim 14, It is characterized in that In the self-healing slurry, the mass ratio of the precursor material, the binder and the dispersant is (70-99.9): (0.1-25): (0.1-5); And / or, the precursor material includes at least one of aryl ether compounds, aryl olefin compounds, and aryl silane monomers; And / or, the binder comprises: at least one of shellac, butyl rubber, carboxymethyl cellulose, polyurethane, polystyrene, polyacrylate, ethylene-vinyl acetate copolymer, vinyl acetate resin, acrylic resin, and chlorinated rubber; And / or, the dispersant includes: at least one of ethylene glycol type, polyol type, oleyl amino oleate, polycaprolactone polyol-polyethyleneimine block copolymer type dispersant, acrylate polymer type dispersant, polyurethane or polyester polymer dispersant; And / or, the solvent includes at least one of water, methanol, ethanol, NMP, acetone, tetrachloroethylene, dichloroethane, trichloroethane, anisole, propanol, butyl acetate, and tetrahydrofuran.

16. The method for preparing the composite diaphragm according to claim 15, It is characterized in that The aryl ether compound includes at least one of a diarylmethane sulfide compound, an aryl disulfide compound, and a fluorine-containing aryl vinyl ether compound; And / or, the preparation of the aromatic olefin compound comprises the steps of: reacting a halogenated aromatic non-conjugated olefin compound with an An organic lithium reagent is subjected to a lithium-halogen replacement reaction to obtain an aryl olefin lithium; the aryl olefin lithium is subjected to an electrophilic addition reaction with an electrophilic reagent to obtain the aryl olefin compound; And / or, the preparation of the aromatic silane monomer comprises the steps of: subjecting a silicate compound and a halogenated olefin ether compound to a condensation reaction under the action of a catalyst to obtain the aromatic silane monomer.

17. The method for preparing the composite diaphragm according to claim 16, It is characterized in that The molar mass ratio of the halogenated aromatic non-conjugated olefin compound, the organic lithium reagent and the electrophilic reagent is (0.4-0.8): (0.1-0.4): (0.1-0.2); and / or, the mass ratio of the total mass of the silicate compound and the halogenated olefin ether compound to the mass ratio of the catalyst is 1:(0.01-0.5); And / or, the halogenated aromatic non-conjugated olefin compound comprises at least one of bromo-trifluorovinyloxybenzene, trifluorovinyl aromatic ether, and perfluorocyclobutyl aromatic ether; And / or, the organic lithium reagent includes at least one of butyl lithium, lithium hexamethyldisilazide, phenyl lithium, n-hexyl lithium, lithium diisopropylamide, and n-butyl lithium; And / or, the electrophilic reagent includes at least one of: hydrogen halide, halogenated hydrocarbon, acyl halide, carbonyl compound, expanded hydrogen, diisobutylaluminum hydride, diisopropyl fluorophosphate, methyl isopropyl fluorophosphate, and iodoacetic acid; And / or, the silicate compound includes at least one of tetraethoxysilane, vinyltrimethoxysilane, triethoxysilane, methyl ether dimethyl silane and triisopropyl silane; And / or, the halogenated olefin ether compound includes at least one of trifluorovinyl aryl ether, distyryl ether, brominated distyryl ether, perfluoromethyl isopropyl ether, perfluoroisobutyl vinyl ether, and hexafluoroisopropenyl methyl ether; And / or, the catalyst includes at least one of an organic boron compound and an alkylaluminoxane.

18. A secondary battery, It is characterized in that The secondary battery comprises a positive electrode, a negative electrode, a separator and an electrolyte, wherein the separator comprises the composite separator as claimed in any one of claims 1 to 12 or the composite separator prepared by the method as claimed in any one of claims 13 to 17.

19. The secondary battery according to claim 18, It is characterized in that The secondary battery includes at least one of a battery cell, a battery module, and a battery pack.

20. An electrical device, It is characterized in that The electrical equipment comprises the secondary battery as claimed in any one of claims 18 to 19.

Citation Information

Patent Citations

  • Composite diaphragm as well as preparation method and application thereof

    CN118825555A

  • Cathode modified high security lithium ion battery

    CN105244551A

  • Diaphragm, preparation method thereof, and lithium ion battery using diaphragm

    CN109148789A

  • A preparation method and application of a thermally responsive diaphragm

    CN109167003A

  • Composite diaphragm with thermal runaway prevention function and lithium ion battery

    CN112490586A