Preparation method for collagen membrane
Through the combined use of double-layer bidirectional coating by a dispensing machine, water-absorbent materials and pressure frames, combined with heat pump drying and thermal cross-linking technology, the problems of uneven thickness, uneven surface and insufficient tensile strength of the collagen film were solved, and a Film with high mechanical strength and uniformity.
Patent Information
- Application Number
- PCT/CN2024/074337
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-19
- Filing Date
- 2024-01-26
- Publication Date
- 2024-10-24
AI Technical Summary
In the existing collagen membrane preparation methods, the membrane thickness is uneven, the surface is uneven, and the tensile strength is insufficient, which affects the quality and applicability of the product.
A dispensing machine is used for double-layer bidirectional coating, and water-absorbent materials are used at the bottom of the layer tray and a pressure frame is placed with a nylon mesh. Combined with heat pump drying and thermal cross-linking technology, the problems of uneven film thickness and uneven surface are improved and improved tensile strength.
The prepared collagen membrane has uniform thickness, flat surface and high tensile strength, and can be effectively used to separate soft tissue and hard tissue and accelerate tissue healing.
Smart Images

Figure CN2024074337_24102024_PF_FP_ABST
Abstract
Description
Preparation method of collagen membrane
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to Chinese patent application No. 2023104239699 filed on April 19, 2023. The entire contents of the above-mentioned Chinese patent application are incorporated into this application by reference. Technical Field
[0003] The present invention relates to the technical field of collagen processing, and in particular to a method for preparing a collagen film, more particularly to a collagen film suitable for periodontal regeneration and dura mater repair and a preparation method thereof. Background Art
[0004] Collagen is a natural fibrous protein found primarily in animal skin, tendons, and bones. It is also the most abundant functional protein in mammals, accounting for 25-30% of the total protein content. Collagen is widely used in the food industry, cosmetics, medical materials, and other fields.
[0005] Connective tissue in the body is mainly composed of collagen. Therefore, collagen is often used as a membrane to replace skin, blood vessels, ligaments and other connective tissues, and has a wide range of applications in the field of medical materials.
[0006] Currently, collagen membranes are typically prepared using an oven drying method, which involves pouring a collagen solution into a sterilized stainless steel tray and drying the tray in an oven. However, this method often results in uneven thickness, an uneven surface, and insufficient tensile strength, which impacts product quality.
[0007] Therefore, improving the uneven thickness and uneven surface of the collagen membrane and enhancing the tensile strength can make the collagen membrane more applicable.
[0008] Summary of the Invention
[0009] In view of the above-mentioned problems in the prior art, one of the objectives of the present invention is to provide a method for preparing a collagen membrane, which can improve the problems of uneven thickness and uneven surface of the collagen membrane and enhance the tensile strength of the collagen membrane.
[0010] After research, the inventors discovered that using a dispensing machine for double-layer, bidirectional coating can enhance the vertical and horizontal tensile strength of the collagen membrane. Furthermore, using a layering plate and pressing frame containing a water-absorbing material can improve the uneven thickness and surface smoothness of the membrane, thus resolving the shortcomings of traditional collagen membrane preparation. The collagen membrane prepared by this invention preserves the integrity of the collagen stranded helix, exhibits high tensile strength, uniform thickness, and a smooth surface, making it suitable for separating soft and hard tissues and accelerating tissue healing.
[0011] The present invention provides a method for preparing a collagen membrane, which comprises the following steps:
[0012] S4, applying the defoamed collagen raw material to the layer tray using a dispensing machine; and
[0013] S5, placing a pressing frame on the defoamed collagen raw material after step S4.
[0014] In some embodiments, the defoamed collagen raw material is obtained by diluting and defoaming a collagen raw material.
[0015] In some embodiments, the collagen raw material is at least one selected from the group consisting of collagen extracted from animal tissues and recombinant collagen.
[0016] In some embodiments, the collagen raw material may be in a solid state, a liquid state, or a combination of solid and liquid states.
[0017] In some embodiments, the method further includes S6: subjecting the defoamed collagen raw material to heat pump drying to obtain a dried collagen film.
[0018] In some embodiments, the method further includes S7: thermally cross-linking the dried collagen film to obtain a semi-finished collagen film.
[0019] In some embodiments, the method further includes S8: soaking the semi-finished collagen film in water to obtain a smooth collagen film.
[0020] In some embodiments, the method further includes S9: freeze-drying the collagen flat film to obtain a collagen film.
[0021] In some embodiments, the collagen raw material is preferably at least one selected from the group consisting of collagen extracted from animal tissues and recombinant collagen.
[0022] In some embodiments, the collagen raw material may be in a solid state, a liquid state, or a combination of solid and liquid states.
[0023] In some embodiments, the solvent used to dilute the collagen raw material is preferably at least one selected from the group consisting of organic solvents and inorganic solvents.
[0024] Furthermore, as organic solvents, alcohols are preferred, such as C1-C5 alcohols. Among alcohols, isopropyl alcohol is particularly preferred. As inorganic solvents, water is particularly preferred.
[0025] In some embodiments, the ideal concentration of the diluted collagen raw material is 10 to 50 mg / g.
[0026] In some embodiments, the coating step is preferably performed using a dispenser for double-layer bidirectional coating. The inventors of this case speculate that the reasons for this are as follows.
[0027] Simply pouring collagen raw material into a layer tray and drying it will result in irregularly arranged collagen fibers, resulting in poor mechanical strength of the resulting collagen film. Using a dispensing machine for double-layer, bidirectional coating, as in the present invention, can align the collagen fibers in specific directions, thereby improving the mechanical strength of the collagen film.
[0028] In some embodiments, the so-called double-layer bidirectional coating refers to applying the first layer of coating with a dispensing machine in the left-right direction, and then applying the second layer of coating with a dispensing machine in the up-down direction, that is, perpendicular to the coating direction of the first layer.
[0029] In some embodiments, the bottom of the layer tray preferably contains a water-absorbing material. Furthermore, the water-absorbing material is preferably a porous inorganic material or an organic polymer material. The inventors of this application speculate that the reason for this is as follows.
[0030] If there is no absorbent material at the bottom of the layer tray during the drying process of the collagen raw material, the moisture will flow during the drying process, and the thickness of the formed collagen film will be relatively uneven.
[0031] If a water-absorbing material is placed at the bottom of the layer tray during the drying process of the collagen raw material, some of the water can be transferred to the water-absorbing material, which can effectively reduce the flow of water. Therefore, the collagen film formed in this way has a more uniform thickness.
[0032] In some embodiments, a mesh is preferably placed between the contact surface of the press frame and the collagen raw material. Furthermore, the mesh is preferably made of nylon. The inventors of this invention speculate that the reasons for this are as follows.
[0033] During the drying process, the press frame and mesh will apply weight to the collagen raw material, which can effectively reduce the excessive movement of collagen and moisture. The nylon mesh is breathable and will not affect the evaporation of water vapor during the drying process. Therefore, the thickness of the formed collagen film is more uniform.
[0034] In some embodiments, it is ideal to control the temperature of heat pump drying at 40-75°C.
[0035] In some embodiments, the ideal drying time for heat pump drying is 5 to 30 hours.
[0036] In some embodiments, it is ideal that the temperature of thermal crosslinking is controlled at 60-90°C.
[0037] In some embodiments, the crosslinking time of thermal crosslinking is ideally 8 to 20 hours. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] FIG1 is a flow chart showing a method according to an embodiment of the present invention.
[0039] FIG2 shows the appearance of the collagen membrane prepared in Example 1 of the present invention.
[0040] FIG3 shows the appearance of the collagen membrane prepared in Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0041] The following describes embodiments of the present invention.
[0042] Please refer to Figure 1, which is a flow chart of a method for preparing a collagen film according to an embodiment of the present invention. As shown in Figure 1, the method for preparing a collagen film of the present invention comprises the following steps: providing a collagen raw material (S1); diluting the collagen (S2); degassing the collagen raw material (S3); applying the collagen raw material to a layer tray using a dispensing machine (S4); placing a press frame on the collagen raw material (S5); drying the collagen raw material using a heat pump (S6); thermally crosslinking the collagen film (S7); soaking the collagen film (S8); and drying the collagen film (S9).
[0043] In step (S1), the collagen raw material provided can be collagen extracted from animal tissues, or recombinant collagen, such as collagen extracted from cow hide or tendon, or recombinant collagen produced using yeast as a genetic engineering vector.
[0044] In one embodiment, the collagen raw material is in a liquid state, but may also be in a solid state or a solid-liquid mixture. For example, it may be a collagen liquid dissolved in a solvent (liquid state), a freeze-dried sponge (solid state), or a fibrous collagen slurry (solid-liquid mixture).
[0045] In step (S2), the solvent used to dilute the collagen raw material includes but is not limited to organic solvents, inorganic solvents, and combinations thereof, such as isopropyl alcohol, water, and the like.
[0046] Water is ideal because it allows for a uniform dispersion of the collagen. Isopropyl alcohol is also ideal because it also allows for a uniform dispersion of the collagen and has antibacterial properties.
[0047] The ideal concentration of the diluted collagen raw material, i.e., the collagen raw material per 1g of solvent, is 10-50 mg / g. 15-45 mg / g is more ideal, 20-40 mg / g is even more ideal, and 25-30 mg / g is particularly ideal. Because collagen has viscosity in a solvent, a concentration of 50 mg / g or higher will result in excessive viscosity and poor handling. Concentrations below 10 mg / g are too low, resulting in insufficient mechanical strength for the membrane.
[0048] In step (S3), conventional methods can be used for degassing, including but not limited to centrifugation, vacuuming, or a combination thereof. Among them, degassing with a centrifugal vacuum degasser is more ideal, as the obtained raw material is uniform and free of bubbles.
[0049] In step (S4), if the conventional method of pouring the raw materials into a layering pan for coating is used, a multi-layer structure cannot be achieved, and the tensile strength of the collagen film is poor. In contrast, if the coating is applied by a dispensing machine, multi-layer and multi-directional coating can be achieved, and the tensile strength of the collagen film is higher.
[0050] Furthermore, the present invention uses a glue dispensing machine manufactured by Pinxu Automation Equipment Co., Ltd. The collagen raw material is poured into a material tank, the glue gun is positioned at the origin, and the coating path is input into the controller to start the operation process.
[0051] Among them, if double-layer bidirectional coating is used, the tensile strength is more ideal because the collagen fibers are arranged vertically and have a double-layer structure.
[0052] In step (S4), a layer plate containing a water-absorbing material is used for coating, wherein the water-absorbing material is preferably a diatomaceous earth plate. The diatomaceous earth plate has a large number of small holes, which can achieve rapid water absorption.
[0053] In step (S5), after coating, a press frame is placed over the collagen material. Preferably, a nylon mesh is stretched over the press frame. The nylon mesh can fix the shape of the collagen material during drying, reduce deformation after drying, and improve the uneven film thickness and surface unevenness.
[0054] Furthermore, the pressing frame of the present invention is made of stainless steel and has the same size as the layer plate. It is placed on the top after the collagen raw material is coated.
[0055] In step (S6), the temperature of heat pump drying is ideally controlled at 40-75°C. 45-70°C is more ideal, 50-65°C is even more ideal, and 55-60°C is particularly ideal. If the temperature is too low, the drying efficiency is poor; on the other hand, if the temperature is too high, there is a concern that the collagen will denature. The drying time is ideally 5-30 hours. 7-27 hours is more ideal, 10-25 hours is even more ideal, and 15-20°C is particularly ideal. If the time is too short, the collagen raw material cannot be completely dried; on the other hand, if the time is too long, it will only increase the burden on time costs.
[0056] In step (S7), the temperature of thermal cross-linking is ideally controlled at 60 to 90°C. 63 to 87°C is more ideal, 66 to 84°C is even more ideal, and 73 to 77°C is particularly ideal. If the temperature is too low, the thermal cross-linking effect is not good; on the other hand, if the temperature is too high, there may be concerns about denaturation of the original protein. The cross-linking time is ideally 8 to 20 hours. 10 to 18 hours is more ideal, and 13 to 15 hours is even more ideal. If the cross-linking time is too short, cross-linking will not be possible, and the excellent effects of the present invention cannot be obtained; however, if the cross-linking time is too long, it will only increase the burden on time costs.
[0057] Furthermore, the thermal cross-linking of the present invention is performed by placing the collagen raw material in a heat pump drying oven, adjusting the heat pump drying oven to a target temperature and a target time, and then allowing the raw material to stand.
[0058] In step (S8), water for injection is used as the solvent for this coating step. The coating step (S8) of the present invention refers to immersing the collagen membrane in water. This step can reduce wrinkles on the surface of the collagen membrane and increase the smoothness of the collagen membrane.
[0059] In step (S9), the drying method can be heat pump drying, vacuum drying or freeze drying. Among them, freeze drying can retain the shape of the collagen film while drying, and the process is carried out at a relatively low temperature, so it is more ideal.
[0060] The present invention is described in detail below with reference to the following examples. However, these examples are merely illustrative and do not limit the present invention to these examples.
[0061] [Example 1]
[0062] A collagen drying film-forming method, the specific steps of which are as follows:
[0063] 1) Water and fibrous collagen were uniformly mixed to a concentration of 24 mg / g.
[0064] 2) Degassing was performed using a centrifugal degassing machine at a speed of 2000 rpm and a vacuum degree of -90 kPa for 5 minutes.
[0065] 3) Use a dispensing machine to apply the defoamed collagen raw material to the layer tray. There is a diatom mud board at the bottom of the layer tray as a water-absorbing material. A total of 2 layers are applied in perpendicular directions.
[0066] 4) The pressing frame is placed on the defoamed collagen raw material, and a nylon mesh is stretched on the contact surface between the pressing frame and the defoamed collagen raw material.
[0067] 5) Drying the collagen by heat pump drying at a temperature of 45° C. for 20 hours. After this step, the collagen raw material has become a film.
[0068] 6) The dried collagen film is then subjected to thermal crosslinking in the manner described above, wherein the temperature is controlled at 70° C. for 16 hours to obtain a semi-finished collagen film.
[0069] 7) Soak the semi-finished collagen membrane in water for injection and cover it with water to make the membrane surface smooth.
[0070] 8) The collagen flat film after being covered with water is placed in a freeze dryer for freeze drying to obtain a collagen film.
[0071] [Example 2]
[0072] A collagen drying film-forming method, the specific steps of which are as follows:
[0073] 1) Mix water and fibrous collagen evenly to a concentration of 35 mg / g.
[0074] 2) Degassing was performed using a centrifugal degassing machine at a speed of 2000 rpm and a vacuum degree of -90 kPa for 5 minutes.
[0075] 3) Use a dispensing machine to apply the defoamed collagen raw material to the layer tray. There is a gypsum board at the bottom of the layer tray as a water-absorbing material. A total of 2 layers are applied in perpendicular directions.
[0076] 4) Place the pressing frame on the collagen raw material, and a nylon mesh is stretched on the contact surface between the pressing frame and the defoamed collagen raw material.
[0077] 5) Drying the collagen by heat pump at a temperature of 60° C. for 12 hours. After this step, the collagen raw material has become a film.
[0078] 6) The dried collagen film is then subjected to thermal crosslinking in the manner described above, wherein the temperature is controlled at 80° C. for 12 hours to obtain a semi-finished collagen film.
[0079] 7) Soak the collagen membrane in water for injection and cover it with water to make the membrane surface smooth.
[0080] 8) The collagen flat film after being covered with water is placed in a freeze dryer for freeze drying to obtain a collagen film.
[0081] [Comparative Example 1]
[0082] A collagen membrane was prepared in the same manner as in Example 1, except that the collagen raw material was directly poured into the layer tray instead of using a dispenser.
[0083] [Comparative Example 2]
[0084] The collagen membrane was prepared in the same manner as in Example 1 except that the layer tray did not use a water-absorbing material as the bottom tray and no press frame was placed on top of the collagen raw material.
[0085] [Comparative Example 3]
[0086] A collagen film was prepared in the same manner as in Example 1 except that the temperature during heat pump drying was 80°C.
[0087] [Comparative Example 4]
[0088] A collagen membrane was prepared in the same manner as in Example 1, except that the dispensing machine was used for single-layer unidirectional coating.
[0089] The average thickness, thickness standard deviation, stranded helical structure, and tensile strength of the collagen membranes obtained in Example 1, Example 2, and Comparative Examples 1 to 4 were evaluated by the following methods. The results are shown in Table 1 below.
[0090] <Average Thickness>
[0091] The average thickness was determined by measuring the thickness of the collagen membrane at 20 points using a thickness gauge and calculating the average value.
[0092] <Thickness standard deviation>
[0093] The thickness standard deviation was determined by measuring the thickness of the collagen membrane at 20 points using a thickness gauge and then calculating the standard deviation.
[0094] <Participating Helix Structure>
[0095] The helical structure is determined by electrophoresis to separate proteins and the α1 and α2 bands are used to determine whether the helical structure is intact.
[0096] <Tensile Strength>
[0097] Tensile strength was tested using a microcomputer-controlled electronic universal testing machine from Shanghai Xieqiang Instrument Manufacturing Co., Ltd. Collagen membranes were cut into 5x15mm pieces and secured to a tensile fixture along their long sides. The test was performed at a fixture movement rate of 1mm / min. The tensile strength was calculated by dividing the maximum load by the sample's cross-sectional area.
[0098] Table 1
[0099] In order to more clearly understand the difference in flatness between the films of Example 1 and Comparative Example 2, their appearance results are also shown in FIG. 2 and FIG. 3 .
[0100] <Comparison with Commercially Available Products>
[0101] The tensile strength of Example 1 and the commercial product was measured in the above-mentioned manner, and the results are shown in Table 2.
[0102] Among them, commercial product 1 is a product of Matricel under the trade name Remaix, commercial product 2 is a product of Geistlich Biomaterials under the trade name Bio-Gide, and commercial product 3 is a product of Datum Dental Biotech under the trade name Ossix Plus.
[0103] Table 2
[0104] From the results in Table 1, it can be found that the collagen membrane prepared by meeting the process conditions of the present invention has a lower thickness standard deviation than that of Comparative Example 2 which does not meet the process conditions of the present invention, that is, it has better membrane flatness.
[0105] The results in Table 1 also show that the collagen membrane prepared using the process conditions of the present invention exhibits a more complete collagen stranded helical structure than the collagen membrane prepared in Comparative Example 3, which does not meet the process conditions of the present invention. The results in Tables 1 and 2 also show that the collagen membrane prepared using the process conditions of the present invention exhibits superior physical strength compared to both Comparative Example 1, which does not meet the process conditions of the present invention, and conventional commercially available products.
[0106] In summary, the collagen membrane prepared according to the present invention has the following advantages:
[0107] (1) Collagen is a heat-sensitive substance. If the drying temperature is too high, its helical structure will be destroyed, and its original efficacy will be lost. In the present invention, the drying temperature is controlled within a specific range, which can avoid the destruction of the helical structure in the collagen and preserve the integrity of the collagen.
[0108] (2) The collagen membrane prepared according to the present invention has a relatively uniform thickness and reduced surface unevenness and wrinkles due to the effects of the pressing frame and the water-absorbing material.
[0109] (3) The tensile strength of the collagen membrane prepared according to the present invention is effectively improved by the action of the dispensing machine.
[0110]
Explanation of symbols
[0111] S1~S9:Steps
Claims
1. A method for preparing a collagen film, comprising the following steps: S4, applying the defoamed collagen raw material to the layer plate by a dispensing machine; S5, placing a pressing frame on the defoamed collagen raw material after step S4.
2. The preparation method according to claim 1, in, The defoamed collagen raw material is obtained by diluting and defoaming the collagen raw material; Optionally, the collagen raw material is at least one selected from the group consisting of collagen extracted from animal tissues and recombinant collagen; Optionally, the collagen raw material may be in a solid state, a liquid state, or a combination of the solid state and the liquid state.
3. The preparation method according to claim 1 or 2, in, The method further comprises: performing heat pump drying on the defoamed collagen raw material to obtain a dried collagen film; Optionally, the method further comprises S7: thermally cross-linking the dried collagen film to obtain a semi-finished collagen film; Optionally, the method further comprises S8: soaking the semi-finished collagen film in water to obtain a smooth collagen film; and Optionally, the method further comprises S9: freeze-drying the collagen flat film to obtain a collagen film.
4. The preparation method according to claim 2, in, The solvent used in the dilution step is at least one selected from the group consisting of organic solvents and inorganic solvents; and / or the concentration of the diluted collagen raw material is 10 to 50 mg / g.
5. The preparation method according to claim 4, in, The organic solvent is a C1-C5 alcohol solvent; the inorganic solvent is water.
6. The preparation method according to claim 4, in, The organic solvent is isopropanol.
7. The preparation method according to claim 1 or 2, in, The coating step is implemented by using a dispensing machine to perform double-layer bidirectional coating; and / or The bottom of the layer tray contains a water-absorbing material; and / or A net is stretched on the contact surface between the pressing frame and the defoamed collagen raw material.
8. The preparation method according to claim 7, in, The water-absorbing material is at least one of a group consisting of porous inorganic materials and organic polymer materials.
9. The preparation method according to claim 7, in, The net is made of nylon material.
10. The preparation method according to any one of claims 3 to 9, in, The heat pump drying temperature is 40 to 75° C., and / or the drying time is 5 to 30 hours; and / or The thermal cross-linking temperature is 60 to 90° C., and / or the cross-linking time is 8 to 20 hours.
Citation Information
Patent Citations
Industrial collagen film production method
CN103435825A
Preparation method of pigskin collagen with certain molecular weight range
CN112608380A
Cell expression recombinant human collagen as well as preparation and application thereof
CN115611977A
Preparation method of collagen membrane
CN116396515A
Automatic pet toilet