Method for preparing flexible material by using fabric
Through ionic liquid alkaline aqueous solution activation and hot-pressure bonding, combined with the polymer penetration process, the problem of complex cellulose dissolution process and poor material flexibility has been solved, and efficient cellulose-based flexible material preparation and waste fabric degradability have been achieved. Production of packaging materials.
Patent Information
- Application Number
- PCT/CN2024/088184
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2024-04-17
- Publication Date
- 2024-10-24
AI Technical Summary
When existing technologies deal with waste textiles, the complete dissolution process of cellulose is complex, energy-intensive, and polluting. Moreover, the prepared cellulose materials have poor flexibility, making it difficult to achieve efficient reuse of waste fabrics and degradability of packaging materials.
The ionic liquid alkaline aqueous solution is used to activate and pretreat cellulose, combined with hot-pressure bonding and polymer penetration processes, to prepare a flexible material with partially dissolved cellulose as the connecting item and undissolved fiber as the skeleton.
It significantly improves the breaking stress and elongation at break of cellulose-based flexible materials, reduces processing time and energy consumption, and enables efficient waste fabric reuse and the production of degradable packaging materials.
Smart Images

Figure PCTCN2024088184-FTAPPB-I100001 
Figure PCTCN2024088184-FTAPPB-I100002 
Figure PCTCN2024088184-FTAPPB-I100003
Abstract
Description
Method for preparing flexible material using fabric
[0001] This invention claims priority to the Chinese invention patent application with application number 202310412795.6, entitled “A method for preparing flexible materials using fabrics”, filed with the State Intellectual Property Office of China on April 18, 2023. Technical Field
[0002] The invention belongs to the technical field of waste textile recycling, and particularly relates to a method for preparing a flexible degradable material by utilizing fabric. Background Art
[0003] With rising consumer spending and a faster pace of clothing renewal, a vast amount of textile waste is generated, of which cotton fabrics account for a significant proportion. Current methods for regenerating waste textiles or cellulose materials primarily involve completely dissolving the cellulose and then regenerating the dissolved material. Although cellulose is the primary component of waste textiles, complete dissolution and recycling is difficult. This is due to the fact that cellulose is a polyhydroxy substance, resulting in high crystallinity and difficulty in dissolving it completely. The traditional viscose process primarily involves alkali treatment, followed by esterification of the cellulose with carbon disulfide to produce cellulose xanthate, which is then dissolved in a dilute alkali solution to produce regenerated cellulose. This entire process is subject to significant energy consumption, heavy pollution, and complex procedures. The novel NMMO (N-methylmorpholine oxide) dissolution method is technically challenging, and NMMO is prone to explosion. Industrial production requires a recovery rate exceeding 95%. The ionic liquid method requires the use of a completely anhydrous pure ionic liquid to dissolve the cellulose, which has high viscosity and prohibitively high production costs. Secondly, since fabrics always come in a variety of colors, it becomes extremely difficult to decolorize these mixed waste fabrics, and they must go through multiple bleaching processes, further aggravating environmental pollution. Finally, there are always certain components of blended fibers in the fabric, which are extremely difficult to remove, which in turn creates certain difficulties in their dissolution. Therefore, the use of a cellulose full dissolution strategy to achieve the reuse of cellulose fabrics has always been difficult to industrialize. Existing cellulose full dissolution technology is mostly used for substances with a high cellulose content known in nature, such as pulp and cotton. The processed products are mainly regenerated fibers and regenerated cellulose films. In addition, the temperature required for complete dissolution is high and the time is long, which can easily cause the degree of polymerization of cellulose to decrease, resulting in low strength and toughness of the recycled material.
[0004] On the other hand, the rapid development of online shopping has led to an increase in the consumption of packaging materials and logistics waste. At present, the film materials used for express packaging are mainly polyethylene, polypropylene, cellulose, nylon and aluminum foil. Most of these plastics (such as polyethylene, polystyrene and polyvinyl chloride) take hundreds or even thousands of years to degrade due to their stable long polymer chains. Therefore, if a part of the waste fabric containing cellulose can be made into a flexible film material, it will not only solve the problem of recycling waste textiles, but also solve the problem of difficult degradation of packaging materials because the fabric contains a large amount of cellulose.
[0005] Summary of the Invention
[0006] The present invention aims to utilize the cellulose present in fabrics containing cellulose fibers, first activate the cellulose using an ionic liquid alkaline aqueous solution, and then prepare a flexible material using a method of hot pressing bonding and polymer penetration modification, so as to solve the problems of the existing technology in treating waste fabrics, such as the complete dissolution of cellulose and the complex recycling process, and the poor flexibility of the prepared cellulose material.
[0007] In order to solve the above problems, the present invention discloses a method for preparing a flexible material using fabric, wherein the fabric is first pre-treated with an ionic liquid aqueous solution for activation, then subjected to heat-pressing bonding, and finally treated with a polymer infiltration process to obtain the flexible material.
[0008] The fabrics described in the present invention include woven fabrics, knitted fabrics, non-woven fabrics, braided fabrics and the like.
[0009] In one embodiment of the present invention, the ionic liquid aqueous solution is an alkaline ionic liquid aqueous solution obtained by adding deionized water to the ionic liquid and adjusting the pH value of the solution with an alkaline substance such as imidazole.
[0010] In one embodiment of the present invention, the fabric includes waste fabric, which refers to used or even discarded cellulose-containing fabrics by households, businesses, or individuals, including clothing, bed sheets, quilts, etc. The ionic liquid includes at least one of 1-allyl-3-methylimidazolium chloride, 1-butyl-3-methylimidazolium chloride, 1-ethyl-3-methylimidazolium chloride, 1-butyl-3-methylimidazolium acetate, and 1-ethyl-3-methylimidazolium diethyl phosphate.
[0011] In one embodiment of the present invention, the fabric is a pure or blended fabric with a cellulose fiber content of 30 to 100%, the pure fabric includes one of cotton fabric, linen fabric, viscose fabric, paper yarn fabric, and cuprammonia fabric, and the blended fabric is a fabric including at least two substances among cotton, linen, viscose, paper yarn, and cuprammonia.
[0012] In one embodiment of the present invention, the mass fraction of the ionic liquid in the ionic liquid aqueous solution system is 70-95%, the mass fraction of the alkaline substance in the ionic liquid aqueous solution is 1-5%, and the rest is deionized water, and the alkaline substance includes at least one of imidazole, sodium hydroxide, and choline.
[0013] The purpose of the present invention is to prepare a flexible material with partially dissolved cellulose as a connecting element and undissolved fibers as a skeleton. The present invention uses an ionic liquid aqueous solution to impregnate the fabric, and controls the degree of dissolution by evaporation of water. If there is too little water, the fibers in the fabric will dissolve too much, and the skeleton part of the product will be too little, affecting the mechanical properties and flexibility of the product; if there is too much water, the fibers in the fabric will dissolve too little, and the connecting elements in the product will be insufficient, making it difficult to produce a uniform film-like material. The addition of alkaline substances is to promote the swelling of the fibers in the fabric, so that the ionic liquid and cellulose mix more fully, and increase the uniformity of the product. The uniformity refers to the fact that the film material is a continuous material of the entire width, and there are no macroscopic pore defects on the width that affect the performance of the product. It is not limited to being the same everywhere in the film material.
[0014] In one embodiment of the present invention, the activation pretreatment includes an immersion step and a dissolution step. The immersion step is to immerse the fabric in an ionic liquid aqueous solution, and the dissolution step is to heat and activate the fabric after squeezing.
[0015] The temperature during the heating activation treatment is 45-200° C., preferably 90-200° C., more preferably 45-125° C., and the time is 5-120 min.
[0016] Optionally, there is a squeezing step between the impregnation step and the dissolution step, and the squeezing step is for removing excess ionic liquid aqueous solution in the impregnated fabric.
[0017] In one embodiment of the present invention, the temperature during hot pressing is 80-200° C., preferably 120-200° C., the pressure is 0.05-15 MPa, preferably 0.05-1.5 MPa, and the hot pressing time is 0.5-300 s, preferably 0.5-60 s.
[0018] The hot-pressing process is designed to bring the ionic liquid in the activated pretreated fabric to a dissolution temperature, allowing the fibers in the fabric to reach a predetermined solubility, resulting in a flexible material with partially dissolved cellulose as the connecting elements and undissolved fibers as the skeleton. Therefore, the hot-pressing temperature should be set within a range that allows the fibers to dissolve. The hot-pressing time should be neither too long nor too short. Too long a time will result in a film with too many connecting elements and a weak fiber skeleton, affecting the film's mechanical properties and flexibility. Too short a time will make it difficult to form a uniform film.
[0019] In one embodiment of the present invention, the polymer infiltration process includes infiltration treatment of the heat-pressed bonded fabric in a liquid containing a polymer, wherein the polymer includes at least one of polyethylene glycol, polyvinyl alcohol, a citrate polymer, and a sorbitol ester polymer, the concentration of the polymer in the polymer-containing liquid is 1-50%, and the infiltration treatment time is 0.1-24 hours.
[0020] The infiltration treatment is carried out in a liquid containing a polymer. The above-mentioned polymer can enter the interior of the cellulose, weaken the interaction between the cellulose molecular chains, and increase the mobility of the molecular chains, thereby increasing the plasticity and flexibility of the film material. Compared with infiltrating the fabric only with water or an aqueous solution of a solvent, the flexibility of the obtained film material can be significantly increased.
[0021] The invention also discloses a flexible material prepared by the method.
[0022] In one embodiment of the present invention, the flexible material comprises a cellulose-based film material.
[0023] One of the purposes of the present invention is to provide a use of the above-mentioned flexible material in the fields of textiles, medicine and food packaging, tapes, cables, insulating substrates, flexible electronic devices, etc.
[0024] Beneficial effects of the present invention:
[0025] (1) The present invention uses an alkaline ionic liquid aqueous solution to activate and dissolve cellulose, and then uses a hot pressing bonding-polymer penetration method to prepare a flexible material. The local activation and dissolution of the fiber surface produces a cellulose macromolecular ionic liquid solution similar to "glue", and then the remaining undissolved fibers are bonded together using a hot pressing process, thereby obtaining a flexible material with "partially dissolved cellulose as a connecting element and undissolved fibers as a skeleton". In order to achieve local dissolution rather than complete dissolution, the present invention uses an ionic liquid alkaline aqueous solution system to control the degree of dissolution by evaporation of water; in order to improve the toughness of the material, the present invention adopts a polymer penetration strategy, using alcohols or ester polymers that also have hydrogen bonding ability to penetrate into the cellulose molecular chains, thereby enhancing the flexibility of the material and finally preparing a degradable cellulose-based flexible material.
[0026] (2) The present invention does not require complete dissolution of cellulose, thus retaining the original strength of natural fibers and significantly improving the breaking stress of cellulose-based flexible materials, with the maximum breaking stress reaching over 60 MPa.
[0027] (3) The cellulose-based flexible material prepared by the method of the present invention has high elongation at break. After the polymer infiltration treatment, the toughness of the flexible material is greatly improved, and the maximum elongation at break can reach more than 50%.
[0028] (4) The method of the present invention can be used to recycle waste fabrics, which can significantly reduce processing time and achieve high efficiency and energy saving. The traditional cellulose film-making process requires complete dissolution before casting into a film. The dissolution temperature is high and the dissolution time often takes several hours. The present invention does not require complete dissolution of the cellulose. Only a few minutes of slight surface dissolution is required to obtain a cellulose ionic liquid solution, which can then be hot-pressed. This saves processing time and reduces energy consumption. DETAILED DESCRIPTION
[0029] To make the objectives, technical solutions, and advantages of the present invention more clear, the technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the embodiments described are part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.
[0030] The raw materials used in Examples 1-8 and Comparative Examples 1-2 of the present invention are spunlace non-woven fabrics made of cotton fibers, referred to as non-woven fabrics; the raw materials used in Example 9 are waste viscose fabrics with a gram weight of 200 g / m 2 The raw material used in Example 10 is paper yarn fabric, which is a blended fabric of 76% paper yarn and 24% polyester, with a gram weight of 20g / m 2 .
[0031] The ionic liquid used in Examples 1-8 and Comparative Examples 1-2 of the present invention is 1-butyl-3-methylimidazolium chloride; the ionic liquid used in Example 9 is 1-ethyl-3-methylimidazolium chloride.
[0032] For the liquid pick-up rate test, the weight of the fabric before and after immersion is weighed, recorded as W0 and W1, and the liquid pick-up rate is calculated according to the following formula: P = [(W1-W0) / W0] × 100%
[0033] The liquid carryover rate can be controlled by controlling the rolling mill time and pressure.
[0034] Tensile performance test: refer to GB / T13022-1991 "Test method for tensile properties of plastic films" for testing;
[0035] Biodegradation test method: Refer to JIS K6950-94 standard and use the natural biodegradation method to test. Weigh a certain weight of flexible film material, dry it to obtain a weight of M0, bury it below 10 cm in natural soil, take it out at regular intervals and weigh its residual weight M1. Calculate its degradation rate according to the following formula: Br (%) = [(M0-M1) / M0] × 100%
[0036] Example 1
[0037] A method for preparing a flexible material using waste fabrics comprises the following steps:
[0038] (1) Preparation of alkaline ionic liquid aqueous solution: 70 g of 1-butyl-3-methylimidazolium ionic liquid was added to 1 g of imidazole and 29 g of water, and stirred to form a uniform mixed solvent;
[0039] (2) Activation pretreatment: The cotton nonwoven fabric was placed in the alkaline aqueous solution of the ionic liquid and immersed at room temperature. After squeezing the liquid, the liquid carrying rate was ensured to be 100%. Then, the nonwoven fabric was placed in a 90°C oven and treated for 180 minutes to obtain an activation pretreated nonwoven fabric sample;
[0040] (3) Hot pressing bonding: The pretreated nonwoven fabric sample obtained in step (2) was placed on a hot pressing table, the hot pressing temperature was controlled at 120° C., and hot pressing was performed at a pressure of 1.5 MPa for 60 seconds to obtain a hot pressed film material.
[0041] (4) Infiltration treatment: The hot-pressed film material obtained in step (3) is placed in a 1% polyethylene glycol (Mn-20000) solution at room temperature for infiltration treatment for 24 hours. The prepared film material is taken out and dried to obtain a translucent flexible film material.
[0042] After testing, the tensile breaking stress of the obtained translucent flexible film material was 25.6 MPa, the elongation at break was 32.93%, and the 90-day biodegradation rate was 93.43%.
[0043] Example 2
[0044] The difference between Example 2 and Example 1 is that different polymers are used in the osmotic treatment process. In Example 1, the osmotic polymer selected is polyethylene glycol with a molecular weight of 20,000, while in Example 2, polyvinyl alcohol (PVA1788) and sorbitol ester are used as the osmotic treatment polymers.
[0045] Table 1 Effect of different polymer permeation on film mechanical properties
[0046] As shown in Table 1, the elongation at break of the regenerated film materials obtained by using the aqueous solution of the above polymer as a coagulation bath for infiltration treatment is significantly higher than 10%, and the mechanical properties are all obvious flexibility.
[0047] Example 3
[0048] The difference between Example 3 and Example 1 is that different polymers are used in the osmotic treatment process. In Example 1, the osmotic polymer selected is polyethylene glycol with a molecular weight of 20,000. In Example 3, the osmotic polymer selected is polyethylene glycol with a molecular weight of 600 and 4000, respectively.
[0049] Table 2 Effect of PEG molecular weight on film mechanical properties
[0050] As shown in Table 2, the elongation at break of the regenerated film materials obtained by infiltration treatment using polyethylene glycol solutions of different molecular weights as the coagulation bath was significantly higher than 10%, and the mechanical properties of all films were significantly flexible. Among them, PEG20000 had the best overall mechanical properties.
[0051] Example 4
[0052] The difference between Example 4 and Example 1 is that the process parameters during hot pressing welding are different. In Example 1, hot pressing is performed at 120°C and 1.5 MPa for 60 seconds. The hot pressing process parameters used in Example 4 and the various properties of the prepared film are shown in Table 3.
[0053] Table 3 Effect of hot pressing process parameters on film properties
[0054] As shown in Table 3, the recycled film materials obtained by the above hot pressing process parameters all have good fracture stress and elongation at break, and their mechanical properties all show good flexibility.
[0055] Example 5
[0056] The difference between Example 5 and Example 1 is that the temperature during activation pretreatment is different. In Example 1, the oven temperature in the activation pretreatment step is 90 degrees. The activation pretreatment temperature used in Example 5 and the various properties of the prepared film are shown in Table 4.
[0057] Table 4 Effect of activation pretreatment temperature on film properties
[0058] As can be seen from Table 4, the regenerated film materials obtained at the above activation pretreatment temperatures all have good breaking stress and breaking elongation, and their mechanical properties all show good flexibility.
[0059] Example 6
[0060] The difference between Example 6 and Example 1 is that the concentration of the ionic liquid used is different. The concentration of the ionic liquid aqueous solution in Example 1 is 70%. The concentration of the ionic liquid used in Example 6 and the various properties of the prepared film are shown in Table 5.
[0061] Table 5 Effect of ionic liquid concentration on film properties
[0062] It can be seen from Table 5 that compared with pure ionic liquid, the regenerated film material prepared by activation pretreatment of the aqueous solution of the particle liquid has better mechanical properties and flexibility.
[0063] Example 7
[0064] The difference between Example 7 and Example 1 is that the alkali content of the ionic liquid solution used is different. The alkali content in Example 1 is 1%. The alkali content of the ionic liquid solution used in Example 7 and the various properties of the prepared film are shown in Table 6.
[0065] Table 6 Effect of alkali content on film properties
[0066] As shown in Table 6, the elongation at break of the regenerated film materials obtained by activation pretreatment with the ionic liquid aqueous solution having the above-mentioned alkali content is significantly higher than 10%, and the mechanical properties are all obvious flexibility.
[0067] Example 8
[0068] The difference between Example 8 and Example 1 is that the types of bases used in the ionic liquid solution are different. The base added in Example 1 is imidazole. The different bases used in Example 8 and the various properties of the prepared films are shown in Table 7.
[0069] Table 7 Effect of alkali type on film properties
[0070] As shown in Table 7, the elongation at break of the regenerated film materials obtained by activation pretreatment with the ionic liquid aqueous solution prepared by the above-mentioned types of alkali is significantly higher than 10%, and the mechanical properties are all obvious flexibility.
[0071] Comparative Example 1
[0072] The difference between Comparative Example 1 and Example 1 is that the non-woven fabric after heat pressing is not subjected to polymer penetration treatment. The various properties of the prepared film are shown in Table 8.
[0073] Table 8 Effect of polymer permeation treatment on film properties
[0074] It can be seen from Table 8 that the elongation at break of the recycled film material treated with polymer infiltration is significantly increased, and the flexibility of the material is significantly increased.
[0075] Comparative Example 2
[0076] The difference between Comparative Example 2 and Example 1 is that the order of polymer treatment is different. In Comparative Example 2, PEG of the same concentration is directly added to the fabric before hot pressing, and no polymer penetration treatment is performed after hot pressing; in Example 1, the fabric is subjected to penetration treatment after hot pressing. The various properties of the prepared film are shown in Table 9.
[0077] Table 9 Effect of polymer addition order on film properties
[0078] As shown in Table 9, the mechanical properties and flexibility of the prepared film can be significantly improved by performing infiltration treatment on the fabric after hot pressing, compared with adding polymer before hot pressing.
[0079] Example 9
[0080] The difference between Example 9 and Example 1 is that different raw materials are used. The raw material used in Example 1 is cotton fiber non-woven fabric, and the raw material used in Example 9 is viscose fabric. After testing, the tensile breaking stress of the obtained flexible film material is 33.4 MPa, and the elongation at break is 34.27%.
[0081] Example 10
[0082] The difference between Example 10 and Example 1 is that different raw materials are used. The raw material used in Example 1 is cotton non-woven fabric, and the raw material used in Example 10 is paper yarn fabric. After testing, the tensile breaking stress of the obtained flexible film material is 28 MPa, and the elongation at break is 18%.
Claims
1. A method for preparing a flexible material using fabric, characterized in that: The method comprises the following steps: firstly using an ionic liquid aqueous solution to perform activation pretreatment on the fabric, then performing heat-pressing bonding on the fabric, and finally using a polymer infiltration process to perform treatment to obtain a flexible material.
2. The method according to claim 1, characterized in that The ionic liquid aqueous solution is an alkaline ionic liquid aqueous solution obtained by adding deionized water to the ionic liquid and adjusting the pH value of the solution with an alkaline substance.
3. The method according to claim 1 or 2, characterized in that The ionic liquid includes at least one of 1-allyl-3-methylimidazolium chloride, 1-butyl-3-methylimidazolium chloride, 1-ethyl-3-methylimidazolium chloride, 1-butyl-3-methylimidazolium acetate, and 1-ethyl-3-methylimidazolium diethyl phosphate.
4. The method according to claim 1 or 2, characterized in that The fabric is a pure or blended fabric with a cellulose fiber content of 30 to 100%. The pure fabric includes any one of cotton fabric, linen fabric, viscose fabric, paper yarn fabric, and cuprammonia fabric. The blended fabric includes a fabric containing at least two substances among cotton, linen, viscose, paper yarn, and cuprammonia.
5. The method according to claim 1 or 2, characterized in that The mass fraction of the ionic liquid in the ionic liquid aqueous solution system is 70-95%, the mass fraction of the alkaline substance is 1-5%, and the rest is deionized water. The alkaline substance includes at least one of imidazole, sodium hydroxide, and choline.
6. The method according to claim 1 or 2, characterized in that The activation pretreatment includes an immersion step and a dissolution step. The immersion step is to immerse the fabric in an ionic liquid aqueous solution. The dissolution step is to heat and activate the fabric after squeezing. The temperature of the heat activation treatment is 90-200° C. and the time is 5-120 minutes.
7. The method according to claim 1 or 2, characterized in that The temperature during the hot pressing bonding is 100-200° C., the pressure is 0.05-1.5 MPa, and the hot pressing time is 0.5-60 seconds.
8. The method according to claim 1 or 2, characterized in that: The polymer infiltration treatment process is to perform infiltration treatment on the heat-pressed bonded fabric in a liquid containing a polymer, wherein the polymer includes at least one of polyethylene glycol, polyvinyl alcohol, a citrate polymer, and a sorbitol ester polymer. The concentration of the polymer in the liquid containing the polymer is 1-50%, and the infiltration treatment time is 0.1-24 hours.
9. The flexible material prepared according to the method according to any one of claims 1 to 8.
10. Use of the flexible material according to claim 9 in the fields of textiles, medicine and food packaging, adhesive tapes, cables, insulating substrates, and flexible electronic devices.
Citation Information
Patent Citations
Method for recovering waste textile by aid of ionic liquid
CN106146877A
Process for the treatment of materials containing fibers
EP3339508A1
CN202310412795A
Cited By
Low-temperature one-bath dyeing process for cotton-polyester blended fabric
CN120231242A