Polyamide composite material, preparation method therefor and use thereof

Through the compounding technology of spherical boron nitride and needle-shaped boron nitride, combined with additives, polyamide composite materials are prepared, which solves the problems of low thermal conductivity and insufficient mechanical properties, achieves both thermal conductivity improvement and mechanical properties, and is suitable for Used in a variety of electronic appliances and new energy applications.

WO2024217454A1PCT designated stage expired Publication Date: 2024-10-24KINGFA SCI & TECH CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/088302
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-17
Filing Date
2024-04-17
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

When increasing the thermal conductivity of existing thermally conductive materials, the mechanical properties often decrease, and the possibility of practical application is lost. It is difficult to simultaneously increase the thermal conductivity and maintain the mechanical properties of the material.

Method used

A compound of spherical boron nitride and needle-shaped boron nitride thermally conductive fillers is used. The gaps in the spherical thermally conductive fillers are filled with needle-shaped thermally conductive fillers to enhance the thermal conductivity path of the material. It is extruded with additives such as antioxidants and lubricants. particles to prepare polyamide composite materials.

Benefits of technology

It significantly improves the thermal conductivity of the material while maintaining high mechanical properties. It is suitable for electronic appliances and new energy industries, reduces product use temperature, and improves safety performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2024088302-FTAPPB-I100001
    Figure PCTCN2024088302-FTAPPB-I100001
  • Figure PCTCN2024088302-FTAPPB-I100002
    Figure PCTCN2024088302-FTAPPB-I100002
  • Figure PCTCN2024088302-FTAPPB-I100003
    Figure PCTCN2024088302-FTAPPB-I100003
Patent Text Reader

Abstract

Disclosed in the present invention are a polyamide composite material, a preparation method therefor and the use thereof. The polyamide composite material comprises the following components in parts by weight: 35-80 parts of PA66 or PA6; 5-30 parts of spherical boron nitride; and 5-30 parts of needle-like boron nitride. The present invention can improve the heat conductivity of the polyamide composite material while ensuring good mechanical properties thereof.
Need to check novelty before this filing date? Find Prior Art

Description

A polyamide composite material and its preparation method and application Technical Field

[0001] The present invention relates to the technical field of engineering plastics, and in particular to a polyamide composite material and a preparation method and application thereof. Background Art

[0002] Nylon is one of the earliest synthetic fibers developed, used both as a fiber and an engineering plastic. Due to its excellent overall properties, including high strength, good rigidity, impact resistance, resistance to oils and chemicals, wear resistance, and self-lubrication, as well as its readily available and low-cost raw materials, nylon is widely used in industries such as industry, clothing, and engineering plastics. Glass fiber-reinforced and flame-retardant modified nylon materials offer even higher mechanical strength and flame retardancy, making them suitable for replacing some metals and other thermoplastic engineering plastics in electronic and electrical applications.

[0003] The thermal conductivity of currently available thermally conductive materials is difficult to improve. Even if this can be achieved, the overall mechanical properties will be severely degraded, rendering the material useless. Therefore, how to improve the thermal conductivity of a material while maintaining its mechanical properties is an urgent problem that needs to be solved.

[0004] Summary of the Invention

[0005] In order to overcome the above-mentioned defects of the prior art, the present invention proposes a polyamide composite material and its preparation method and application. The specific technical solution is as follows:

[0006] A polyamide composite material, comprising the following components in parts by weight:

[0007] PA66 or PA6 35-80 parts;

[0008] 5-30 parts of spherical boron nitride;

[0009] 5-30 parts of needle-shaped boron nitride.

[0010] PA66, molecular formula: (C 10 H 22 N2O2) n , melting point: 250-260℃, density: 1.14-1.47g / mL (25℃), relative viscosity 230-280.

[0011] PA6, molecular formula: [-NH(CH2)5CO-] n , melting point: 215-225℃, density: 1.13-1.15g / mL (25℃).

[0012] Furthermore, the spherical boron nitride has a sphericity of 0.8-1, preferably 0.85-1. Sphericity characterizes a parameter of particle morphology. The closer the particle's morphology is to a sphere, the closer its sphericity is to 1. Sphericity is the ratio of the surface area of ​​a sphere of equal volume to the surface area of ​​the object. The sphericity measurement standard is GB / T 37406-2019.

[0013] Furthermore, the aspect ratio of the needle-shaped boron nitride is 3-10, preferably 4-8. Spherical boron nitride thermal conductive filler is compounded with needle-shaped boron nitride thermal conductive filler, and the needle-shaped thermal conductive filler is used to fill the gaps in the spherical thermal conductive filler, thereby strengthening the thermal conductive path of the material and significantly improving the thermal conductivity of the material.

[0014] Furthermore, the mass content of the spherical boron nitride in the polyamide composite material is 5-32 wt%; the mass content of the needle-shaped boron nitride in the polyamide composite material is 5-32 wt%.

[0015] Furthermore, the weight ratio of the spherical boron nitride to the needle-shaped boron nitride is in the range of (0.3-2.5):1, preferably (0.5-2):1.

[0016] Furthermore, the polyamide composite material further comprises 0.2-0.3 parts by weight of an auxiliary agent, wherein the auxiliary agent is an antioxidant and / or a lubricant.

[0017] The antioxidant is one or more of antioxidant 1098, antioxidant 1010, antioxidant 1076, and antioxidant 168.

[0018] The lubricant may be a fatty acid lubricant, and the fatty acid lubricant is selected from one or more of fatty acids, fatty acid derivatives or fatty acid esters.

[0019] The present invention also provides a method for preparing the polyamide composite material, comprising the following steps:

[0020] S1: Weigh and pre-mix the components according to the ratio to obtain a premix;

[0021] S2: putting the premix of step S1 into an extruder, performing melt blending and extrusion granulation to obtain the polyamide composite material.

[0022] Furthermore, the extruder is a twin-screw extruder, the screw length-diameter ratio of the twin-screw extruder is (40-48):1, the barrel temperature of the twin-screw extruder is 200-275°C, and the screw speed of the twin-screw extruder is 250-500rpm.

[0023] The present invention also provides the use of the polyamide composite material in the preparation of electronic appliances, such as the preparation of circuit breaker housings, battery holders, etc.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The present invention uses a composite of spherical and needle-shaped boron nitride thermal conductive fillers to address the low thermal conductivity of existing materials while also exhibiting superior mechanical properties. This material can be applied not only in the mature low-voltage electrical appliance field but also in the emerging new energy industry, lowering the operating temperature of products and improving safety performance. The polyamide composite material of the present invention has a thermal conductivity of 0.72-2.34 W / m·K and a tensile strength of 78.3-85.2 MPa. DETAILED DESCRIPTION

[0026] The following is a clear and complete description of the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative efforts are within the scope of protection of the present invention.

[0027] <Preparation of Examples and Comparative Examples>

[0028] The raw materials used in the examples and comparative examples of the present invention are all commercially available, but are not limited to these materials:

[0029] PA66: brand PA66 EP-158, purchased from Zhejiang Huafeng Group;

[0030] PA6: brand PA6 HY-2500A, Jiangsu Haiyang Chemical Fiber Co., Ltd.

[0031] Spherical boron nitride A: sphericity 0.85, brand BNH-1, purchased from Shandong Jingyi New Materials Co., Ltd.

[0032] Spherical boron nitride B: sphericity 1, brand BNH-7, purchased from Shandong Jingyi New Materials Co., Ltd.

[0033] Spherical boron nitride C: sphericity 0.8, brand BHN-3, purchased from Shandong Jingyi New Materials Co., Ltd.

[0034] Needle-shaped boron nitride A: aspect ratio 4, brand PN15, purchased from Shandong Jingyi New Materials Co., Ltd.

[0035] Needle-shaped boron nitride B: aspect ratio 8, brand PN45, purchased from Shandong Jingyi New Materials Co., Ltd.

[0036] Needle-shaped boron nitride C: aspect ratio 3, brand PN03, purchased from Shandong Jingyi New Materials Co., Ltd.

[0037] Needle-shaped boron nitride D: aspect ratio 10, brand PN10, purchased from Shandong Jingyi New Materials Co., Ltd.

[0038] Spherical zinc oxide: brand XT-0806-6-1, purchased from Shanghai Xiangtian Nanomaterials Co., Ltd.

[0039] Needle-shaped zinc oxide: brand XT-0806-6-3, purchased from Shanghai Xiangtian Nanomaterials Co., Ltd.

[0040] Antioxidant: antioxidant 1098, commercially available, parallel experiments used the same commercial product;

[0041] Lubricant: Stearyl stearate, commercially available. Parallel experiments used the same commercial product.

[0042] The preparation methods of the embodiments of the present invention and the comparative examples are as follows:

[0043] S1: According to the ratios in Table 1 and Table 3, weigh and pre-mix the components to obtain a premix;

[0044] S2: The premix of step S1 is put into a twin-screw extruder for melt blending and extrusion granulation to obtain a polyamide composite material.

[0045] The screw length-diameter ratio of the twin-screw extruder is 40:1, the barrel temperature of the twin-screw extruder is 260° C., and the screw speed of the twin-screw extruder is 400 r / min.

[0046] <Test Standard>

[0047] The performance test standards of the embodiments and comparative examples of the present invention are as follows:

[0048] Tensile strength: Refer to standard ISO 527-2:2012, tensile speed is 10mm / min;

[0049] Thermal conductivity: The vertical thermal conductivity is tested according to the ASTM E1461-2013 laser method, with a test thickness of 1.0 mm.

[0050] Table 1. Examples 1-12 formulations (parts by weight)

[0051] Table 2. Performance test results of Examples 1-12

[0052] Table 3. Comparative Examples 1-6 Formula (Unit: parts by weight)

[0053] Table 4. Performance test results of comparative examples 1-6

[0054] Compared with Example 1, Comparative Examples 1 and 2 do not add needle-shaped boron nitride in Comparative Example 1, and do not add spherical boron nitride in Comparative Example 2. Both Comparative Examples 1 and 2 do not adopt the method of compounding needle-shaped boron nitride and spherical boron nitride. The thermal conductivity of Comparative Examples 1 and 2 is reduced, and the tensile strength is not as good as that of Example 1.

[0055] Compared with Example 1, in Comparative Examples 3 and 4, the addition of too much or too little spherical boron nitride will reduce the thermal conductivity of the material, and the tensile strength is not as good as that of Example 1.

[0056] Compared with Example 1, Comparative Examples 5 and 6 have excessive needle-shaped boron nitride added in Comparative Example 5 and too little needle-shaped boron nitride added in Comparative Example 6. The thermal conductivity of Comparative Examples 5 and 6 is lower than that of Example 1, and the tensile strength is not as good as that of Example 1.

[0057] Compared with Example 1, Comparative Example 7 does not add spherical boron nitride, but adds spherical zinc oxide. The thermal conductivity of Comparative Example 7 is lower than that of Example 1, and the tensile strength is not as good as that of Example 1.

[0058] Compared with Example 1, Comparative Example 8 does not add needle-shaped boron nitride, but adds needle-shaped zinc oxide. The thermal conductivity of Comparative Example 8 is lower than that of Example 1, and the tensile strength is not as good as that of Example 1.

[0059] Compared with Example 1, Comparative Example 9 does not add needle-shaped boron nitride and spherical boron nitride, but adds needle-shaped zinc oxide and spherical zinc oxide. The thermal conductivity of Comparative Example 9 is much lower than that of Example 1, and the tensile strength is far lower than that of Example 1.

[0060] The present invention uses a composite of spherical and needle-shaped boron nitride thermal conductive fillers to address the low thermal conductivity of existing materials while also exhibiting superior mechanical properties. This material can be applied not only in the mature low-voltage electrical appliance field but also in the emerging new energy industry, lowering the operating temperature of products and improving safety performance. The polyamide composite material of the present invention has a thermal conductivity of 0.72-2.34 W / m·K and a tensile strength of 78.3-85.2 MPa.

[0061] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A polyamide composite material, characterized in that: By weight, it includes the following components: PA66 or PA6 35-80 parts; 5-30 parts of spherical boron nitride; 5-30 parts of needle-shaped boron nitride.

2. The polyamide composite material according to claim 1, characterized in that: The sphericity of the spherical boron nitride is 0.8-1, preferably 0.85-1.

3. The polyamide composite material according to claim 1, characterized in that: The aspect ratio of the needle-shaped boron nitride is 3-10, preferably 4-8.

4. The polyamide composite material according to claim 1, characterized in that: The weight ratio of the spherical boron nitride to the needle-shaped boron nitride is (0.3-2.5):1, preferably (0.5-2):

1.

5. The polyamide composite material according to claim 1, characterized in that: The polyamide composite material further comprises 0.2-0.3 parts by weight of an auxiliary agent.

6. The polyamide composite material according to claim 1, characterized in that: The auxiliary agent is an antioxidant and / or a lubricant.

7. A method for preparing a polyamide composite material according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1: According to the ratio, weigh and pre-mix the components to obtain a premix; S2: putting the premix of step S1 into an extruder, performing melt blending and extrusion granulation to obtain the polyamide composite material.

8. The method for preparing the polyamide composite material according to claim 7, characterized in that: The extruder is a twin-screw extruder, the screw length-diameter ratio of the twin-screw extruder is (40-48):1, the barrel temperature of the twin-screw extruder is 200-275°C, and the screw speed of the twin-screw extruder is 250-500rpm.

9. Use of the polyamide composite material according to any one of claims 1 to 6 in the preparation of electronic appliances.

Citation Information

Patent Citations

  • Super flexible high-molecular heat conduction material and preparation method thereof

    CN102352110A

  • Special heat-conducting and insulating material for LED (light-emitting diode) lamp holder and preparation method thereof

    CN103044904A

  • High-toughness and high-thermal-conductivity polymer material and preparation method thereof

    CN104559145A

  • Polyamide resin composition and molded article comprising same

    CN106661324A

  • Impact-resistant scratch-resistant thermal-conduction nylon composite material and preparation method thereof

    CN106977908A