Water-resistant low-temperature co oxidation catalyst, and preparation method therefor and use thereof

By using SiO2-coated multi-metal oxide active components as a core-shell structure catalyst, combined with atomization-hydrolysis and hydrophobic modification technology, the problem of catalyst activity decline in humid environments is solved, and efficient CO oxidation and denitration effects are achieved. Suitable for pollution control in the steel industry.

WO2024217485A1PCT designated stage expired Publication Date: 2024-10-24INST OF COAL CHEM CHINESE ACAD OF SCI
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/088505
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-19
Filing Date
2024-04-18
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

The CO oxidation reaction activity of existing catalysts decreases in humid air, and trace gases in the flue gas affect the catalytic performance, resulting in reduced catalytic efficiency, making it difficult to effectively control CO pollution generated by the sintering process.

Method used

A core-shell structure catalyst using SiO2 coated multi-metal oxide active components is used to form a porous shell through the atomization-hydrolysis method. Combined with hydrophobic modification technology, the thickness of the silica shell is adjusted to form a catalyst with good water resistance.

Benefits of technology

The carbon monoxide conversion rate reaches 100% under water-containing conditions of 180°C, which improves catalytic activity and efficiency, overcomes the problem of activity decline of existing catalysts in humid environments, and is suitable for CO-SCR catalysts and denitration catalysts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024088505_24102024_PF_FP_ABST
    Figure CN2024088505_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of waste gas treatment. Provided are a water-resistant low-temperature CO oxidation catalyst, and a preparation method therefor and the use thereof. The water-resistant low-temperature CO oxidation catalyst provided in the present invention has a core-shell structure in which a multi-metal-oxide active component is coated with SiO2, wherein the active component comprises at least two of metal oxides of Cu, Co, Mn, Ce, Pt, Ag, Pd, Ir, etc. The preparation method for the water-resistant low-temperature CO oxidation catalyst comprises: first preparing a catalyst precursor having a core-shell structure in which an active component is coated with SiO2, and then subjecting the SiO2 shell of the precursor to hydrophobic modification, so as to obtain the catalyst. Further provided in the present invention is the use of the preparation method. The preparation method is applied to the preparation of a CO-SCR catalyst. The catalyst provided in the present invention has a controllable silicon dioxide shell thickness, good water resistance and high catalytic activity. The preparation method therefor involves a simple process, has controllable conditions, is low cost, is convenient for industrial promotion and utilization, and can be used for preparing a variety of catalysts.
Need to check novelty before this filing date? Find Prior Art

Description

A water-resistant low-temperature CO oxidation catalyst and its preparation method and application Technical Field

[0001] The present invention belongs to the technical field of waste gas treatment, and in particular relates to a water-resistant low-temperature CO oxidation catalyst and a preparation method and application thereof. Background Art

[0002] my country's steel production accounts for over 50% of the world's total. However, China's steel production is primarily characterized by a long process flow, multiple steps, high energy consumption, a wide range of pollutant types, and significant total emissions. Therefore, steel companies are a key industry for atmospheric pollution. The sintering process, in particular, generates significant amounts of CO, an atmospheric pollutant that harms human health and the natural environment. Due to its significant emissions, its control has become a key concern for the steel industry. Currently, various methods exist for removing CO from sintering flue gas, the most effective of which is catalytic oxidation. H₂O chemisorption on catalysts is stronger than CO₂ chemisorption, and the adsorption of CO₂ and H₂O has a synergistic effect, enhancing co-adsorption. Studies have shown that water molecules adsorb on oxygen vacancies, hindering the generation of active oxygen species and thus reducing the catalyst's CO oxidation activity in humid air. Under actual reaction conditions, the atmosphere often contains significant amounts of water vapor, which in most cases severely inhibits catalytic activity and reduces catalytic efficiency. Furthermore, the presence of other trace gases in the flue gas can also affect catalytic performance.

[0003] In view of the above problems, it is necessary to develop an efficient catalyst to solve the problem.

[0004] In view of this, the present invention is proposed.

[0005] Summary of the Invention

[0006] The object of the present invention is to provide a water-resistant low-temperature CO oxidation catalyst and its preparation method and application to solve the above problems.

[0007] In order to achieve the above objectives, the present invention adopts the following technical solutions:

[0008] A water-resistant low-temperature CO oxidation catalyst has a core-shell structure of SiO2-coated multi-metal oxide active components, wherein the active components include at least two metal oxides of Cu, Co, Mn, Ce, Pt, Ag, Pd, Ir, etc.

[0009] Optionally, the crystal form of the active component includes any one or more of spinel, perovskite and hydrotalcite-like crystal forms.

[0010] A method for preparing the water-resistant low-temperature CO oxidation catalyst comprises: first preparing a core-shell structure catalyst precursor in which SiO2 coats the active component, and then performing hydrophobic modification on the SiO2 shell of the precursor to obtain the catalyst.

[0011] Optionally, the preparation of the precursor includes: dissolving the active component and tetraethyl orthosilicate in ethanol, then adding an ammonia solution, stirring, washing, and then drying.

[0012] Optionally, the hydrophobic modification comprises: dispersing the precursor in n-hexane, adding chlorotrimethylsilane, ultrasonically treating, centrifuging, washing, and drying;

[0013] The ultrasonic treatment time is 1-5h;

[0014] The drying temperature is 60-100° C. and the drying time is 9-13 hours.

[0015] Optionally, the volume ratio of the precursor mass to the chlorotrimethylsilane is 1:0.5-2, where the mass is in g and the volume is in ml.

[0016] Optionally, the preparation of the precursor includes first coating by atomization and then hydrolyzing;

[0017] The atomization coating comprises: atomizing the ethyl silicate ethanol solution to form an atomization belt, and passing the active component gas flow into the atomization belt to achieve coating of the active component by ethyl silicate droplets;

[0018] The hydrolysis comprises: placing the atomized coated product in an alkaline solution for hydrolysis, and then sequentially performing centrifugation, filtration and dehydration.

[0019] The atomization-hydrolysis method is used to form a core-shell structure in which a porous silica shell layer covers the active components of multiple metal oxides. The active components of the catalyst will become condensation nuclei, and the liquid will condense into balls under the action of molecular tension, making the performance of the prepared catalyst better.

[0020] Optionally, the preparation of the precursor further satisfies one or more of the following conditions:

[0021] a. The mass fraction of the ethyl silicate ethanol solution is 10-55%; changing the concentration of ethyl orthosilicate can adjust the thickness of the SiO2 shell, so that the shell thickness is small, which is conducive to the catalytic oxidation process;

[0022] b. The alkaline solution comprises an aqueous ammonia solution and / or a sodium hydroxide solution;

[0023] c. The mass fraction of the ammonia solution is 5-15% and the temperature is 50-70°C;

[0024] d. The concentration of the sodium hydroxide solution is 0-0.01Mol / L and the temperature is 15-35 ℃;

[0025] e. The hydrolysis time is 3-5h;

[0026] f. The dehydration temperature is 40-60°C and the time is 8-14h.

[0027] The thickness of the porous silica shell has a significant impact on catalyst activity and hydrophobicity. A thicker silica shell prevents water from entering the catalyst core due to surface hydrophobic groups, but it also hinders the entry of reactive molecules. The present invention flexibly adjusts the thickness of the porous silica shell by adjusting reaction parameters, particularly by adjusting the concentration of ethyl silicate ethanol, thereby effectively adjusting the thickness of the porous shell to between 5 and 50 nm. The method is simple and feasible, with good control effects. The present invention also provides an application of the preparation method, which is applied to the preparation of a CO-SCR catalyst.

[0028] Optionally, the metal elements constituting the active component used in preparing the CO-SCR catalyst are Ir and Mn; the element usage ratio of Ir and Mn is 0.5-1.5:100.

[0029] Beneficial effects of the present invention:

[0030] The water-resistant low-temperature CO oxidation catalyst provided by the present invention has a silicon dioxide shell structure and a core of metal oxide active components. It has good water resistance and high catalytic activity. Experimental verification shows that the conversion rate of carbon monoxide can reach 100% under water conditions at 180°C.

[0031] The present invention first coats the active substance and then hydrophobically modifies the outer surface of the shell to form a core-shell structure catalyst. This achieves excellent water resistance while maintaining high catalytic activity, overcomes the problem of decreased CO oxidation reaction activity of existing catalysts in humid air, improves the catalyst's utilization efficiency, and enriches its application scenarios.

[0032] The preparation method provided by the present invention can not only prepare a water-resistant low-temperature CO oxidation catalyst with excellent performance, but also prepare a denitration catalyst by selecting active components and dosages, and has a wide range of uses. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the specific embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0034] FIG1 is a schematic diagram of the device and process for preparing a precursor used in Example 1;

[0035] FIG2 is a TEM image of the water-resistant low-temperature CO oxidation catalyst prepared in Example 1;

[0036] FIG3 is a TEM image of the water-resistant low-temperature CO oxidation catalyst prepared in Example 5;

[0037] Figure numerals: 1-high pressure pump; 2-atomizing nozzle; 3-atomizing chamber; 4-air flow pump; 5-collector. DETAILED DESCRIPTION

[0038] To make the objectives, technical solutions, and advantages of the embodiments of the present invention more clear, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts shall fall within the scope of protection of the present invention.

[0039] Comparative Example 1

[0040] The core-shell CO oxidation catalyst was prepared in a common manner, and the specific steps are as follows:

[0041] S1: Preparation of active ingredients:

[0042] 2.416 g of Cu(NO3)2·3H2O, 1.458 g of Co(NO3)2·6H2O, and 2.632 g of Mn(NO3)2(aq) (50 wt%) were weighed and placed in a beaker. Deionized water was added and stirred at 25°C for 15 min until uniformly mixed. Ammonium bicarbonate solution was then added and stirred for 60 min until complete precipitation. The mixture was then allowed to stand for 6 h, washed with distilled water, centrifuged, and dried in an oven at 80°C overnight. The resulting product was then placed in a tube furnace and heated to 500°C at 3°C / min in an air atmosphere and calcined for 3 h to obtain the active component.

[0043] S2: Precursor preparation: The active component obtained in S1 was dispersed in ethanol by ultrasound, tetraethyl orthosilicate (TEOS) was added, and the mixture was stirred at 450 rpm for 4 hours. Ammonia (25-28%, AR) and water were then added. The mixture was stirred at 450 rpm for another 4 hours, washed with ethanol, and dried at 100°C for 11 hours to obtain A@SiO2. A@SiO2 was preheated in a vacuum oven at 150°C for 11 hours and then cooled to 30°C in the vacuum oven.

[0044] S3: Hydrophobic modification:

[0045] The precursor obtained from S2 was dispersed in n-hexane, and chlorotrimethylsilane was added at a rate of 1 ml of chlorotrimethylsilane per gram of precursor. The mixture was then ultrasonically treated at 25°C for 3 hours and centrifuged. The product was washed with n-hexane and dried in a vacuum oven at 80°C for 11 hours to obtain a core-shell CO oxidation catalyst obtained by the conventional method. The silica shell thickness was 120 nm.

[0046] Performance testing:

[0047] The obtained catalyst was loaded into a fixed bed reactor. The experimental conditions were: 4000ppmCO, 200ppmNO, 16%O2, 10%H2O, N2 as carrier gas, reaction temperatures of 130℃, 180℃, 210℃ and 250℃, respectively, reaction pressure of atmospheric pressure, and evaluation space velocity of 60000gscm. -3 .

[0048] Example 1

[0049] According to the method provided by the present invention, a water-resistant low-temperature CO oxidation catalyst is prepared, and the specific steps are as follows:

[0050] S1: Preparation of active ingredients:

[0051] 2.416 g of Cu(NO3)2·3H2O and 3.579 g of Mn(NO3)2(aq) (50 wt%) were weighed and placed in a beaker. Deionized water was added and stirred at 25°C for 15 min until uniformly mixed. Ammonium bicarbonate solution was then added and stirred for 60 min until complete precipitation. The mixture was then allowed to stand for 6 h, washed with distilled water, centrifuged, and dried in an oven at 80°C overnight. The resulting product was then placed in a tube furnace and heated to 500°C at 3°C / min in an air atmosphere and calcined for 3 h to obtain the active component.

[0052] S2: Preparation of precursors:

[0053] Using the device shown in FIG1 , a 20% ethyl silicate ethanol solution is passed through a high-pressure pump 1 for pressurization, and then passes through an atomizing nozzle 2 into an atomizing chamber 3 to form an atomized zone.

[0054] The active component obtained from S1 is dispersed and input into the atomization chamber 3 through the air flow pump 4. At this time, after the ethyl silicate droplets in the atomization chamber 3 cover the active component, the ethyl silicate droplets gradually grow with the active component as the core, and fall into the collector 5 under the action of gravity for hydrolysis. The collector 5 is filled with a 10% ammonia solution at 60°C. The ethyl silicate is hydrolyzed in the ammonia solution to form a porous silica shell. After hydrolysis for 4 hours, the product is centrifuged and collected and placed in a vacuum oven at 50°C for 12 hours to obtain a precursor;

[0055] S3: Hydrophobic modification:

[0056] The precursor obtained from S2 was dispersed in n-hexane, and chlorotrimethylsilane was added at a rate of 1 ml of chlorotrimethylsilane per gram of precursor. The product was then ultrasonically treated at 25°C for 3 hours and centrifuged. The product was washed with n-hexane and dried in a vacuum oven at 80°C for 11 hours to obtain a water-resistant low-temperature CO oxidation catalyst with a silica shell thickness of 9 nm.

[0057] The TEM image of the water-resistant low-temperature CO oxidation catalyst prepared in Example 1 is shown in FIG2 . As shown in FIG2 , the method provided by the present invention can be used to effectively synthesize core-shell catalysts.

[0058] The performance test conditions are the same as those of Comparative Example 1.

[0059] Example 2

[0060] The difference from Example 1 is that the constituent metal elements and dosage of the active components in S1 are 2.416gCu(NO3)2·3H2O, 2.037gCo(NO3)2·6H2O, and 1.302gCe(NO3)3·6H2O, and the calcination temperature is 550°C; the concentration of the ethyl silicate ethanol solution in S2 is 10%.

[0061] Example 3

[0062] The difference from Example 1 is that the constituent metal elements and amounts of the active components in S1 are 3.81 g Ce(NO3)3·6H2O, 1.569 g Mn(NO3)2(aq) (50 wt%), and 0.0482 g Pt(NO3)2; the concentration of the ethyl silicate ethanol solution used in step S2 is 35%.

[0063] The silica shell thickness of the water-resistant low-temperature CO oxidation catalyst obtained in this example is 11 nm.

[0064] Example 4

[0065] The difference from Example 1 is that the constituent metal elements and amounts of the active components in S1 are 3.81gCe(NO3)3·6H2O, 2.416gCu(NO3)2·3H2O, and 0.0482gPt(NO3)2; the concentration of the ethyl silicate ethanol solution used in step S2 is 55%.

[0066] Example 5

[0067] The difference from Example 1 is that the constituent metal elements and amounts of the active components in S1 are 3.579 g Mn(NO3)2(aq) (50 wt%), 2.9103 g Co(NO3)2·6H2O, and 0.1152 g Pd(NO3)2(aq) (15 wt%); the concentration of the ethyl silicate ethanol solution used in step S2 is 10%.

[0068] The silica shell thickness of the water-resistant low-temperature CO oxidation catalyst obtained in this example is 6 nm, and its TEM image is shown in FIG3 .

[0069] Table 1 Test results of catalyst performance obtained in Examples 1-5 and Comparative Example 1

[0070] As shown in Figures 2 and 3, the water-resistant low-temperature CO oxidation catalyst prepared by the method provided by the present invention has a clear core-shell structure with adjustable shell thickness. While being hydrophobic, it is also conducive to the entry of CO into the interior of the catalyst for oxidation reaction, thereby improving the CO oxidation efficiency.

[0071] The catalyst preparation method provided in the embodiment of the present invention has the same active components and modification method as those in comparative example 1. Only the core-shell preparation method is different, resulting in different core-shell thicknesses. From the performance results, it can be seen that the thinner core-shell layer provided by the present invention is conducive to the entry of reaction molecules such as CO and O2 and the progress of the catalytic reaction. The conversion rate of 95% can be reduced from 250°C in the traditional preparation method to below 180°C.

[0072] Example 6

[0073] The difference from Example 1 is that the metal elements and amounts of the active components in S1 are 3.579g Mn(NO3)2(aq) (50wt%), 0.1152g C 12 H 18 Ir3O 13 .C2H3O2.3(H2O), the concentration of the ethyl silicate ethanol solution used in step S2 is 15%.

[0074] Performance test: The obtained catalyst was loaded into a fixed bed reactor. The experimental conditions were: 4000ppmCO, 200ppmNO, 5%O2, 10%H2O, carrier gas was N2, and the evaluation space velocity was 30000gscm -3 The reaction pressure is normal pressure. The reaction temperatures are 130℃, 180℃, 210℃ and 250℃, and the denitrification rates are 22.2%, 24.6%, 41.8% and 66.4% respectively.

[0075] It can be seen from Example 6 that a CO-SCR catalyst with excellent denitration performance can be prepared using the preparation method provided by the present invention.

[0076] Please note that the technical features of the above embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. The above embodiments only express several implementation methods of the present application. The description is relatively specific and detailed, but it cannot be understood as a limitation on the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of this application, several variations and improvements can be made, which all fall within the scope of protection of this application. Therefore, the scope of protection of the patent in this application shall be based on the attached claims.

Claims

1. A water-resistant low-temperature CO oxidation catalyst, characterized in that: The catalyst has a core-shell structure of SiO2-coated multi-metal oxide active components, and the active components include at least two of the metal oxides of Cu, Co, Mn, Ce, Pt, Ag, Pd, and Ir.

2. The catalyst according to claim 1, characterized in that The crystal form of the active component includes any one or more of spinel, perovskite and hydrotalcite-like crystal forms.

3. A method for preparing a water-resistant low-temperature CO oxidation catalyst according to any one of claims 1 to 2, characterized in that: include: Firstly, a core-shell structure catalyst precursor in which the active component is coated with SiO2 is prepared, and then the SiO2 shell layer of the precursor is hydrophobically modified to obtain the catalyst.

4. The preparation method according to claim 3, characterized in that: The preparation of the precursor comprises: dissolving the active component and tetraethyl orthosilicate in ethanol, then adding an ammonia solution, stirring, washing and then drying.

5. The preparation method according to claim 3, characterized in that: The hydrophobic modification comprises: dispersing the precursor in n-hexane, adding chlorotrimethylsilane, ultrasonically treating, centrifuging, washing and drying; The ultrasonic treatment time is 1-5h; The drying temperature is 60-100° C. and the drying time is 9-13 hours.

6. The preparation method according to claim 5, characterized in that: The volume ratio of the precursor mass to the chlorotrimethylsilane is 1:0.5-2, wherein the mass is in g and the volume is in ml.

7. The preparation method according to claim 3, characterized in that: The preparation of the precursor includes first coating by atomization and then hydrolyzing; The atomization coating comprises: atomizing the ethyl silicate ethanol solution to form an atomization belt, and passing the active component gas flow into the atomization belt to achieve coating of the active component by ethyl silicate droplets; The hydrolysis comprises: placing the atomized coated product in an alkaline solution for hydrolysis, and then sequentially centrifuging, filtering and dehydrating.

8. The preparation method according to claim 7, characterized in that: The preparation of the precursor also satisfies one or more of the following conditions: a. The mass fraction of the ethyl silicate ethanol solution is 10-55%; b. The alkaline solution comprises an aqueous ammonia solution and / or a sodium hydroxide solution; c. The mass fraction of the ammonia solution is 5-15% and the temperature is 50-70°C; d. The concentration of the sodium hydroxide solution is 0-0.01Mol / L and the temperature is 15-35°C; e. The hydrolysis time is 3-5h; f. The dehydration temperature is 40-60°C and the time is 8-14h.

9. An application of the preparation method according to any one of claims 3 to 8, characterized in that: The method is applied to the preparation of a CO-SCR catalyst.

10. The use according to claim 9, characterized in that: The metal elements constituting the active components used in preparing the CO-SCR catalyst are Ir and Mn; The element dosage ratio of Ir and Mn is 0.5-1.5:100.

Citation Information

Patent Citations

  • High-stability Co3O4-based catalyst, preparation method thereof and application to CO oxidation reaction

    CN104437497A

  • Methane combustion catalyst, and preparation method and application thereof

    CN106492824A

  • Core-shell catalyst, preparation method thereof and method for treating industrial tail gas

    CN112337504A

  • Core-shell type composite catalyst as well as preparation method and application thereof

    CN114054077A

  • Water-resistant low-temperature CO oxidation catalyst as well as preparation method and application thereof

    CN116586075A