Additive for supplementing lithium or sodium, preparation method therefor and use thereof
Lithium-supplementing or sodium-supplementing additives made from oxalic acid, salts and catalysts, through sanding and spray drying processes, solve the problem of capacity loss of lithium-ion and sodium-ion batteries during charging, achieving low-cost, high-capacity and stable Battery performance, suitable for mass production.
Patent Information
- Application Number
- PCT/CN2024/089183
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-21
- Filing Date
- 2024-04-22
- Publication Date
- 2024-10-24
AI Technical Summary
Existing lithium-ion and sodium-ion batteries will form an SEI film during the first week of charging, resulting in irreversible capacity loss of the cathode material, affecting battery capacity and cycle life. In addition, the stability and synthesis conditions of existing lithium replenishing agents are harsh, and the manufacturing cost is high. Failure to commercialize.
Lithium or sodium supplement additives made from oxalic acid, salt and catalyst are used to control particle size distribution and specific surface area through sand grinding and spray drying processes, reduce decomposition voltage, increase specific capacity, and make nanoscale additives.
A low-cost, residue-free, stable lithium or sodium supplement additive in the air is achieved, with low decomposition voltage, high specific capacity, and low catalyst usage, making it suitable for large-scale production and commercialization.
Smart Images

Figure CN2024089183_24102024_PF_FP_ABST
Abstract
Description
A lithium or sodium supplement additive and its preparation method and application
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to Chinese patent application number 2023104377951, filed with the Patent Office of China on April 21, 2023, entitled “A lithium or sodium supplement additive, its preparation method and application”, the entire contents of which are incorporated by reference into this application. Technical Field
[0003] The present disclosure belongs to the field of batteries and relates to a lithium or sodium supplement additive and a preparation method and application thereof. Background Art
[0004] When lithium-ion batteries and sodium-ion batteries are charged for the first week, a SEI film will form on the surface of the negative electrode, causing irreversible capacity loss of the positive electrode material, thereby affecting the capacity and cycle life of the battery. Therefore, the capacity and cycle performance of the battery can be improved by replenishing lithium or sodium at the positive or negative electrode. Compared with replenishing lithium and sodium at the negative electrode, replenishing lithium and sodium at the positive electrode is simpler and easier, and does not require additional production processes. It only requires adding lithium or sodium replenishers to the positive electrode slurry. Common positive electrode lithium replenishers include Li2O, Li2O2, Li2S, Li3N, Li2NiO2, Li2CuO2, Li2MnO3, Li2C2O4, Li5FeO4, etc. Common positive electrode sodium replenishers include Na2O, Na2O2, Na2S, Na3N, Na2NiO2, Na2CuO 2、 Na2C2O4, Na5FeO4, etc. Currently, the main commercialized positive electrode lithium supplements are Li2NiO2 and Li5FeO4, and positive electrode sodium supplements have not yet been commercialized. However, the stability of Li2NiO2 materials is poor and requires surface coating. The lithium supplement efficiency is low, and the product is LiNiO2, which has poor structural stability and serious gas production at high temperatures. Li5FeO4 releases a large amount of oxygen during the first delithiation process, oxidizing the electrolyte and causing gas production in the battery cell. LiOH is easily retained on the surface during the synthesis process, resulting in a homogenous gel jelly. In addition, the synthesis conditions of these two lithium supplements are harsh, and the moisture content in the synthesis process needs to be strictly controlled, resulting in high manufacturing costs. Therefore, it is imperative to develop a low-cost, residue-free, and air-stable lithium and sodium supplement.
[0005] Lithium oxalate and sodium oxalate are low-cost, air-stable, acidic lithium and sodium supplements that leave no residue after the first week of charging. However, their decomposition voltage is high (4.7V), which does not match the voltage of the current mainstream ternary positive electrode material and lithium iron phosphate, so they have not been commercialized. Patent CN 114300680 A dissolves unmodified lithium oxalate in water, then slowly dropwise adds a cobalt tetroxide quantum dot dispersion to the solution. After stirring, a carbon nanotube dispersion is slowly dropwise added to the solution to obtain a precursor solution. The precursor solution is then atomized by an ultrasonic atomizer to ultimately obtain modified lithium oxalate. The synthesis process is relatively complex. Patent CN114464909 disperses a prepared catalyst in a saturated aqueous solution of lithium oxalate, stirs, and slowly dropwise adds ethanol to the dispersion. The lithium oxalate is precipitated by recrystallization, and then centrifugally dried to obtain a composite lithium supplement material containing lithium oxalate and the catalyst. Patent CN110112475A separately prepares oxalic acid and sodium carbonate solutions, then slowly dropwise adds the oxalic acid solution to the sodium carbonate solution to form a uniform solution. The mixed solution is then dropwise added to ethanol to form a precipitate, which is then filtered and dried to obtain the final sodium oxalate product, Na2C2O4. However, the sodium oxalate particles synthesized by this method are relatively large, approximately 1 μm.
[0006] Summary of the Invention
[0007] The present disclosure provides a lithium or sodium supplement additive, which is mainly made of oxalic acid, salt and a catalyst;
[0008] Wherein, the salt includes: lithium salt or sodium salt;
[0009] The particle size distribution concentration of the lithium or sodium supplement additive satisfies the following formula:
[0010] 1≤(D90-D10) / D50≤100;
[0011] The specific surface area of the lithium-supplementing or sodium-supplementing additive is S, and S and D10, D50, and D90 of the lithium-supplementing or sodium-supplementing additive satisfy the following formula:
[0012] 1≤(S / ((D90-D10) / D50)≤100.
[0013] In some embodiments, the D50 of the oxalic acid, the salt, the catalyst, and the lithium or sodium supplementing additive are Da, Db, Dc, and Dd, respectively, and Da, Db, Dc, and Dd satisfy the following formula:
[0014] 0.5≤(Da+Db) / (Dc+Dd)≤200.
[0015] In some embodiments, the mass ratio of the oxalic acid, the salt, and the catalyst is 170-180:100-220:5-30.
[0016] In some embodiments, the particle size of the additive for lithium or sodium supplementation is 0.01 to 50 μm.
[0017] In some embodiments, the pH of the additive for lithium or sodium supplementation is < 7.
[0018] In some embodiments, the loose bulk density of the additive for lithium or sodium supplementation is 0.5 to 1.5 g / cm 3 .
[0019] In some embodiments, the catalyst includes at least one of: LiCoO2, LiNi x Co y Mn 1-x-y O2, LiFePO4, LiMn x Fe 1-x O4, LiMn2O4, LiNi 0.5 Mn 1.5 O4, lithium-rich manganese-based cathode, NiO, MnO2, Mn3O4, CoO, Co3O4, Fe3O4, MoO3, WO3, Nb2O5, Mo2C, TaC, SiC, TiN, MoN, WN, TiB2, WB, Ketjenblack, conductive carbon super-P, acetylene black, CNT, VGCF, polyaniline, polypyrrole, polythiophene or polypyridine; in the LiNi x Co y Mn 1-x-y O2, x + y = 1, 0 < x ≤ 1, 0 < y < 1; in the LiMn x Fe 1-x O4, 0 ≤ x ≤ 1.
[0020] In some embodiments, the lithium salt includes: Li2CO3 and / or LiOH.
[0021] In some embodiments, the sodium salt includes at least one of: NaOH, Na2CO3 or NaHCO3.
[0022] The present disclosure also provides a method for preparing the additive for lithium or sodium supplementation as described above, including the following steps:
[0023] Mix the mixed solution containing oxalic acid, salt and catalyst, and then perform sand grinding and spray drying.
[0024] In some embodiments, the time of sand grinding is 15 to 30 min.
[0025] In some embodiments, the material filling efficiency of sand grinding is 40% to 80%.
[0026] In some embodiments, the spray drying pressure is 0.2-1.0 MPa.
[0027] The present disclosure also provides a positive electrode material, comprising the lithium-supplementing or sodium-supplementing additive.
[0028] The present disclosure also provides a lithium ion or sodium ion battery, comprising the positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the following will briefly introduce the drawings required for use in the embodiments. It should be understood that the following drawings only represent the embodiments of the present disclosure by way of example, and the dimensional ratios in the drawings do not directly correspond to the actual ratios of the embodiments. At the same time, the following drawings only show certain embodiments of the present disclosure and therefore should not be regarded as limiting the scope.
[0030] FIG1 is a SEM image (1000 times) of the lithium or sodium supplement additive provided in Example 1 of the present disclosure;
[0031] FIG2 is a SEM image (20,000 times) of the lithium or sodium supplement additive provided in Example 1 of the present disclosure;
[0032] Figure 3 is a graph showing the results of a lithium-ion battery charging test;
[0033] Figure 4 shows the results of the sodium ion battery charging test. DETAILED DESCRIPTION
[0034] Advantages of the embodiments in the summary of the invention will be explained in the embodiment section of the following specification, and some of them are obvious from the specification, or can be obtained through some embodiments of the disclosed embodiments.
[0035] The technical solution of the present disclosure will be further described below with reference to the accompanying drawings and through some implementation methods.
[0036] In order to make the purpose, technical solutions and advantages of the present disclosure more clear, the present disclosure is further described in detail below with reference to the accompanying drawings and examples. It should be understood that the embodiments described herein are only used to explain the present disclosure and are not intended to limit the present disclosure. In addition, the technical features involved in the various embodiments of the present disclosure described below can be combined with each other as long as they do not conflict with each other. Without departing from the principles of the embodiments of the present disclosure, several improvements and modifications can be made, and these improvements and modifications are also considered to be within the scope of protection of the embodiments of the present disclosure.
[0037] The present disclosure provides a lithium or sodium supplement additive, which is mainly made of oxalic acid, salt and a catalyst;
[0038] Wherein, salts include: lithium salts or sodium salts;
[0039] The particle size distribution concentration of the lithium or sodium supplement additive satisfies the following formula:
[0040] 1≤(D90-D10) / D50≤100;
[0041] The specific surface area of the lithium or sodium supplementing additive is S, and S and D10, D50 and D90 of the lithium or sodium supplementing additive satisfy the following formula:
[0042] 1≤(S / ((D90-D10) / D50)≤100.
[0043] The lithium or sodium supplement additive disclosed herein is prepared by strictly selecting raw materials and rigorously designing the particle size distribution, specific surface area, and particle size of the additive, so that the additive has a low decomposition voltage, a high specific capacity, a small particle size, and a small amount of catalyst.
[0044] The particle size distribution concentration of the additive satisfies the following formula: 1≤(D90-D10) / D50≤100. If the concentration is too high, the material D90 is too large and there are too many large particles, resulting in less contact with the catalyst and low material capacity. If the concentration is too low, the material particles are too small and side reactions will occur with the electrolyte, resulting in a decrease in battery capacity and cycle performance.
[0045] The catalyst particle size is small and the specific surface area is too large, which easily leads to gelation during the positive electrode homogenization process. The additive particle size is too small, which is not conducive to the uniform mixing of the additive and the positive electrode material. The specific surface area S of the additive, S and the D10, D50 and D90 of the additive satisfy the following formula: 1≤(S / ((D90-D10) / D50)≤100. If the parameter is too large, it means that the specific surface area is too large and the particle size distribution concentration is small, which is not conducive to the mixing and homogenization of the additive and the positive electrode material. If the parameter is too small, it means that the specific surface area is too small, the particle size distribution concentration is large, and the material particle size is too large, resulting in low capacity utilization.
[0046] In some embodiments, the D50 of oxalic acid, salt, catalyst, and lithium or sodium supplement additive are Da, Db, Dc, and Dd, respectively, and Da, Db, Dc, and Dd satisfy the following formula:
[0047] 0.5≤(Da+Db) / (Dc+Dd)≤200.
[0048] The D50 values for oxalic acid, lithium salt, catalyst, and additive are Da, Db, Dc, and Dd, respectively. These values satisfy the following equation: 0.5≤(Da+Db) / (Dc+Dd)≤200. This equation must be satisfied between the raw materials and the finished product. A low value for this parameter indicates that the oxalic acid and lithium salt used are relatively small in particle size, while the catalyst and synthesized additives are relatively large. This, on the one hand, hinders uniform mixing during sand milling. On the other hand, large catalyst particle size results in poor catalytic effect, while large additive particle size results in longer paths for lithium ion insertion and extraction, resulting in poor material rate performance and inability to fully utilize the capacity. A high value for this parameter indicates that the oxalic acid and lithium salt used are relatively large in particle size, while the catalyst and additives are relatively small in particle size, hindering uniform mixing during sand milling.
[0049] In some embodiments, the mass ratio of oxalic acid, salt and catalyst is 170-180:100-220:5-30 (e.g., 170:220:5, 172:200:10, 174:180:14, 176:160:20, 178:140:25 or 180:100:30).
[0050] In some embodiments, the particle size of the lithium or sodium supplement additive is 0.01 to 50 μm (e.g., 0.01 μm, 0.05 μm, 0.1 μm, 0.5 μm, 1 μm, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, or 50 μm).
[0051] In some embodiments, the pH of the lithium or sodium supplement is <7.
[0052] In some embodiments, the bulk density of the lithium or sodium supplement additive is 0.5 to 1.5 g / cm 3 (e.g. 0.5 g / cm 3 , 0.7g / cm 3 , 0.9g / cm 3 , 1.1g / cm 3 , 1.3g / cm 3 or 1.5g / cm 3 ).
[0053] In some embodiments, the catalyst includes: LiCoO2, LiNi x Co y Mn 1-x-y O2, LiFePO4, LiMn x Fe 1-x O4, LiMn2O4, LiNi 0.5 Mn 1.5At least one of O4, lithium-rich manganese-based positive electrode, NiO, MnO2, Mn3O4, CoO, Co3O4, Fe3O4, MoO3, WO3, Nb2O5, Mo2C, TaC, SiC, TiN, MoN, WN, TiB2, WB, Ketjen black, conductive carbon super-P, acetylene black, CNT, VGCF, polyaniline, polypyrrole, polythiophene or polypyridine; LiNi x Co y Mn 1-x-y In O2, x+y=1,0 <x≤1,0<y<1;LiMn x Fe 1-x In O4, 0≤x≤1.
[0054] In some embodiments, the lithium salt includes: Li2CO3 and / or LiOH.
[0055] In some embodiments, the sodium salt comprises at least one of NaOH, Na2CO3, or NaHCO3.
[0056] The present disclosure also relates to a method for preparing a lithium or sodium supplement additive, comprising the following steps:
[0057] The mixed solution containing oxalic acid, salt and catalyst is mixed and then sand-milled and spray-dried.
[0058] The disclosed method for preparing a lithium- or sodium-supplementing additive is simple and easy, and has important practical significance for accelerating the commercialization of lithium oxalate and sodium oxalate. Oxalic acid, a lithium salt (sodium salt), and a catalyst are sand-milled and spray-dried to obtain a lithium- or sodium-supplementing additive with excellent performance. The additives synthesized by this method are all nano-sized and are very uniformly mixed with the catalyst, resulting in extremely low manufacturing costs and ease of large-scale production and commercialization.
[0059] In some embodiments, the sanding time is 15 to 30 minutes (eg, 15 minutes, 20 minutes, 25 minutes, or 30 minutes).
[0060] In some embodiments, the material filling efficiency of the sand mill is 40% to 80% (eg, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, or 80%).
[0061] In some embodiments, the spray drying pressure is 0.2 to 1.0 MPa (eg, 0.2 MPa, 0.4 MPa, 0.6 MPa, 0.8 MPa, or 1.0 MPa).
[0062] In some embodiments, the spray drying is followed by drying.
[0063] In some embodiments, the drying temperature is 95-150°C (e.g., 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, or 150°C).
[0064] In some embodiments, the drying time is 5 to 15 hours (e.g., 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, or 15 hours).
[0065] The present disclosure also relates to a positive electrode material, including a lithium-supplementing or sodium-supplementing additive.
[0066] The present disclosure also relates to a lithium-ion or sodium-ion battery, including a positive electrode material.
[0067] Example
[0068] The following are typical but non-limiting embodiments of the present disclosure:
[0069] Example 1
[0070] The preparation method of the lithium supplement additive provided in this embodiment comprises the following steps:
[0071] 1. Dissolve 173 g of oxalic acid dihydrate (H2C2O4·2H2O), 115 g of lithium hydroxide monohydrate (LiOH·H2O), 7.8 g of Co3O4, and 7.8 g of KB (Ketjen Black) in 400 g of water and stir continuously for 4 h.
[0072] 2. After the reaction is complete, add the solution to the sand mill for sand grinding for 23 minutes, and the material filling efficiency is 60%;
[0073] 3. Add the sand-milled material into the spray dryer for spraying at a pressure of 0.2 MPa;
[0074] 4. Dry the sprayed material in an oven at 100°C for 10 hours to obtain the final product.
[0075] The additive obtained in Example 1 was observed using a scanning electron microscope. Figure 1 is a low-magnification electron microscope image. In Figure 1, Pa1 is equal to 17.65 μm, Pa2 is equal to 12.81 μm, Pa3 is equal to 12.58 μm, Pa4 is equal to 8.293 μm, Pa5 is equal to 5.362 μm, and Pa6 is equal to 10.44 μm. Figure 2 is a high-magnification electron microscope image. In Figure 2, Pa1 is equal to 695.3 nm, Pa2 is equal to 756 nm, Pa3 is equal to 195.0 nm, Pa4 is equal to 443.4 nm, Pa5 is equal to 1.263 μm, and Pa6 is equal to 273.8 nm. As can be seen from Figures 1 and 2, the additive has a spherical morphology and a primary particle size of approximately 400 nm, indicating that it is a nanomaterial.
[0076] Example 2
[0077] The preparation method of the lithium supplement additive provided in this embodiment comprises the following steps:
[0078] 1. Dissolve 170 g of oxalic acid dihydrate (H2C2O4·2H2O), 110 g of lithium hydroxide monohydrate (LiOH·H2O), 5 g of Co3O4, and 5 g of KB (Ketjen Black) in 400 g of water and stir continuously for 4 h.
[0079] 2. After the reaction is complete, add the solution to the sand mill for sand grinding for 15 minutes, and the material filling efficiency is 40%;
[0080] 3. Add the sand-milled material into the spray dryer for spraying at a pressure of 0.2 MPa;
[0081] 4. Dry the sprayed material in an oven at 100°C for 10 hours to obtain the final product.
[0082] Example 3
[0083] The preparation method of the lithium supplement additive provided in this embodiment comprises the following steps:
[0084] 1. Dissolve 180 g of oxalic acid dihydrate (H2C2O4·2H2O), 120 g of lithium hydroxide monohydrate (LiOH·H2O), 10 g of Co3O4, and 10 g of KB (Ketjen Black) in 400 g of water and stir continuously for 4 h.
[0085] 2. After the reaction is complete, add the solution to the sand mill for sand grinding for 30 minutes, and the material filling efficiency is 80%;
[0086] 3. Add the sand-milled material into the spray dryer for spraying at a pressure of 0.2 MPa;
[0087] 4. Dry the sprayed material in an oven at 100°C for 10 hours to obtain the final product.
[0088] Example 4
[0089] The preparation method of the lithium supplement additive provided in this embodiment comprises the following steps:
[0090] 1. Dissolve 176 g of oxalic acid dihydrate (H2C2O4·2H2O), 118 g of lithium hydroxide monohydrate (LiOH·H2O), 8.5 g of Co3O4, and 8.5 g of KB (Ketjen Black) in 400 g of water and stir continuously for 4 h.
[0091] 2. After the reaction is complete, add the solution to the sand mill for sand grinding for 26 minutes, and the material filling efficiency is 75%;
[0092] 3. Add the sand-milled material into the spray dryer for spraying at a pressure of 0.2 MPa;
[0093] 4. Dry the sprayed material in an oven at 100°C for 10 hours to obtain the final product.
[0094] Example 5
[0095] The preparation method of the lithium supplement additive provided in this embodiment comprises the following steps:
[0096] 1. Dissolve 173 g of oxalic acid dihydrate (H2C2O4·2H2O), 115 g of lithium hydroxide monohydrate (LiOH·H2O), 7.8 g of polyaniline, and 7.8 g of LiCoO2 in 400 g of water and stir continuously for 4 h.
[0097] Steps 2 to 4 are the same as in Example 1.
[0098] Example 6
[0099] The preparation method of the lithium supplement additive provided in this embodiment comprises the following steps:
[0100] 1. Dissolve 173 g of oxalic acid dihydrate (H2C2O4·2H2O), 115 g of lithium hydroxide monohydrate (LiOH·H2O), 7.8 g of WN, and 7.8 g of Fe3O4 in 400 g of water and stir continuously for 4 h.
[0101] Steps 2 to 4 are the same as in Example 1.
[0102] Example 7
[0103] The preparation method of the sodium supplement additive provided in this embodiment comprises the following steps:
[0104] 1. Dissolve 173 g of oxalic acid dihydrate (H2C2O4·2H2O), 110 g of NaOH, 7.8 g of Co3O4, and 7.8 g of Ketjen Black in 400 g of water and stir continuously for 4 h.
[0105] Steps 2 to 4 are the same as in Example 1.
[0106] Comparative Example 1
[0107] The only difference from Example 1 is that Step 2 and Step 3 are omitted.
[0108] Comparative Example 2
[0109] The only difference from Example 7 is that Step 2 and Step 3 are omitted.
[0110] Experimental Example 1
[0111] The particle size distribution, specific surface area and pH of the obtained additive were tested using a laser particle size analyzer and a pH meter. The results are shown in Tables 1 and 2. The D50 of the additive in the embodiment is between 5.25 and 8.38 μm, and the pH is between 6.54 and 6.85. The material is acidic, so it will not affect the homogenization of the positive electrode material. The specific surface area is 37 to 57 m 2 The additives in the comparative example were not subjected to grinding and spraying, and the particle size of the material did not meet the conditions defined in the present disclosure, and the specific surface area was small.
[0112] Table 1
[0113] Table 2
[0114] Experimental Example 2
[0115] The additives obtained in Examples 1-6, Comparative Examples 1, and 3 were mixed with a conductive agent, SP (carbon black), and a binder, PVDF (polyvinylidene fluoride), at a mass ratio of 8:1:1 to form a positive electrode slurry. This slurry was then coated onto aluminum foil to form a positive electrode sheet. Lithium metal was used as the negative electrode sheet, a Celgard 2400 microporous polypropylene membrane was used as the separator, and LiPF6 (lithium hexafluorophosphate) / EC (ethylene carbonate)-DMC (dimethyl carbonate) was used as the electrolyte to assemble lithium-ion batteries. The assembled lithium-ion batteries were charged and tested, and the results are shown in Figure 3.
[0116] The additives obtained in Example 7 and Comparative Example 2 were mixed with a conductive agent, SP (carbon black), and a binder, PVDF (polyvinylidene fluoride), at a mass ratio of 8:1:1 to form a positive electrode slurry. This was then coated on aluminum foil to form a positive electrode sheet. Sodium metal was used as the negative electrode sheet, a Celgard 2400 microporous polypropylene membrane was used as the separator, and NaPF6 (sodium hexafluorophosphate) / EC (ethylene carbonate)-DMC (dimethyl carbonate) was used as the electrolyte to assemble a sodium ion battery. The assembled sodium ion batteries were charged and tested, and the results are shown in Figure 4.
[0117] The lithium oxalate prepared in Example 1 has a low decomposition voltage of 4.2-4.3V and a specific capacity of 520 mAh / g. The lithium oxalate prepared in Comparative Example 1 has a high decomposition voltage of 4.3-4.5V and a specific capacity of 438 mAh / g. The superior performance of Example 1 is due to the nanoscale material and the thorough and uniform mixing of the lithium oxalate and catalyst, which helps the catalyst lower the decomposition voltage of the lithium oxalate and increase the capacity.
[0118] The sodium oxalate prepared in Example 7 had a low decomposition voltage of 4.2-4.3V and a specific capacity of 400 mAh / g. The sodium oxalate prepared in Comparative Example 2 had a high decomposition voltage of 4.4-4.7V and a specific capacity of 249 mAh / g. The superior performance of Example 2 is due to the nanoscale nature of the material and the thorough and uniform mixing of the sodium oxalate and catalyst, which facilitated the catalyst in lowering the decomposition voltage of the sodium oxalate and increasing the capacity. Industrial Applicability
[0119] In summary, the present disclosure provides a lithium- or sodium-supplementing additive, its preparation method, and its application. This lithium- or sodium-supplementing additive exhibits a low decomposition voltage, high specific capacity, small particle size, and requires minimal catalyst. The preparation method is simple and easy to operate, resulting in an excellent lithium- or sodium-supplementing additive. The additive synthesized by this method is nanoscale and mixes very uniformly with the catalyst, resulting in extremely low manufacturing costs and amenability to large-scale production.
Claims
1. An additive for lithium supplementation or sodium supplementation, characterized in that: Made mainly from oxalic acid, salts and catalysts; Wherein, the salt includes: lithium salt or sodium salt; The particle size distribution concentration of the lithium or sodium supplement additive satisfies the following formula: 1≤(D90-D10) / D50≤100; The specific surface area of the lithium or sodium supplementing additive is S, and S and D10, D50 and D90 of the lithium or sodium supplementing additive satisfy the following formula: 1≤(S / ((D90-D10) / D50)≤100.
2. The lithium or sodium supplement additive according to claim 1, characterized in that: The D50 of the oxalic acid, the salt, the catalyst and the lithium or sodium supplement additive are Da, Db, Dc and Dd respectively, and Da, Db, Dc and Dd satisfy the following formula: 0.5≤(Da+Db) / (Dc+Dd)≤200.
3. The lithium or sodium supplement additive according to claim 1, characterized in that: The mass ratio of the oxalic acid, the salt and the catalyst is 170-180:100-220:5-30.
4. The lithium or sodium supplement additive according to claim 1, characterized in that: The particle size of the lithium or sodium supplement additive is 0.01 to 50 μm.
5. The lithium or sodium supplement additive according to claim 1, characterized in that: The pH of the lithium or sodium supplementing additive is less than 7.
6. The lithium or sodium supplement additive according to claim 1, characterized in that: The bulk density of the lithium or sodium supplement additive is 0.5 to 1.5 g / cm 3 .
7. The lithium or sodium supplement additive according to claim 1, characterized in that: The catalyst includes: LiCoO2, LiNi x Co y Mn 1-x-y O2, LiFePO4, LiMn x Fe 1-x O4, LiMn2O4, LiNi 0.5 Mn 1.5 O4, a lithium-rich manganese-based cathode, NiO, MnO2, Mn3O4, CoO, Co3O4, Fe3O4, MoO3, WO3, Nb2O5, Mo2C, TaC, SiC, TiN, MoN, WN, TiB2, WB, Ketjen black, conductive carbon super-P, acetylene black, CNT, VGCF, polyaniline, polypyrrole, polythiophene or polypyridine; in the LiNi x Co y Mn 1-x-y O2, x + y = 1, 0 < x ≤ 1, 0 < y < 1; in the LiMn x Fe 1-x O4, 0 ≤ x ≤ 1.
8. The lithium or sodium supplement additive according to claim 1, characterized in that: The lithium salt includes: Li2CO3 and / or LiOH.
9. The lithium or sodium supplement additive according to claim 1, characterized in that: The sodium salt includes at least one of NaOH, Na2CO3 or NaHCO3.
10. The method for preparing the lithium or sodium supplement additive according to any one of claims 1 to 9, characterized in that: The following steps are involved: The mixed solution containing oxalic acid, salt and catalyst is mixed and then sand-milled and spray-dried.
11. The method for preparing the lithium or sodium supplement additive according to claim 10, characterized in that: The sand grinding time is 15 to 30 minutes.
12. The method for preparing the lithium or sodium supplement additive according to claim 10, characterized in that: The material filling efficiency of the sand mill is 40% to 80%.
13. The method for preparing the lithium or sodium supplement additive according to claim 10, characterized in that: The spray drying pressure is 0.2-1.0 MPa.
14. A positive electrode material, characterized in that: The lithium or sodium supplementing additive comprises the additive according to any one of claims 1 to 9.
15. A lithium ion or sodium ion battery, characterized in that: Comprising the positive electrode material according to claim 14.
Citation Information
Patent Citations
Sodium ion battery positive electrode containing sodium supplementation additive and preparation method and application thereof
CN110112475A
Modified lithium oxalate as well as preparation method and application thereof
CN114300680A
Nanocrystallized composite positive electrode lithium supplementing slurry and positive electrode
CN114464909A
Lithium supplementing slurry, positive plate and lithium ion battery
CN113394371A
Positive electrode additive, preparation method thereof, positive plate and lithium ion battery
CN114497553A
Cited By
Positive lithium supplement agent, positive pole piece, secondary battery and electric device
CN119650648A
Nitrogen-doped transition metal carbide catalyst for decomposing positive electrode material sodium supplement and preparation method and application of nitrogen-doped transition metal carbide catalyst
CN119764453A
Method for promoting oxidation of sodium oxalate through coating of conductive polymer, composite sodium supplementing agent and application of composite sodium supplementing agent
CN119786608A