Use of vinyl acetate copolymers as a low-profile additive

Vinyl acetate-isobornyl acrylate copolymers address the high water absorption and mechanical property limitations of polyvinyl acetate-based low-profile additives by reducing shrinkage and enhancing mechanical properties, making them suitable for outdoor applications with improved resistance and stability.

WO2024217658A1PCT designated stage expired Publication Date: 2024-10-24WACKER CHEMIE AG
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2023/059869
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Existing low-profile additives based on polyvinyl acetate reduce shrinkage and improve mechanical properties of composite components, but they have high water absorption capacity, which affects their resistance, especially in outdoor applications, and require enhancement in static mechanical properties like flexural modulus of elasticity.

Method used

The use of vinyl acetate-isobornyl acrylate copolymers as low-profile additives, with vinyl acetate comprising 20 to 97% and isobornyl acrylate 2 to 80% by weight, which are block-stable and accessible through a one-stage polymerization process, reducing shrinkage and water absorption while maintaining or improving mechanical properties.

Benefits of technology

The vinyl acetate-isobornyl acrylate copolymers effectively reduce shrinkage and water absorption, maintaining or improving the bending modulus of elasticity, and are block-stable without additional anti-blocking agents, suitable for use in composite components like those used in boat building.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IMGF000015_0001
    Figure IMGF000015_0001
  • Figure IMGF000015_0002
    Figure IMGF000015_0002
  • Figure IMGF000016_0001
    Figure IMGF000016_0001
Patent Text Reader

Abstract

The invention relates to the use of vinyl acetate-isobornyl acrylate copolymers as a low-profile additive (LPA), characterized in that the vinyl acetate-isobornyl acrylate copolymers are based on 2 to 98 wt.% vinyl acetate, 2 to 98 wt.% isobornyl acrylate (IBOA) and optionally one or more additional ethylenically unsaturated monomers, in each case relative to the total weight of the vinyl acetate-isobornyl acrylate copolymers.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Use of vinyl acetate copolymers as low-profile additives

[0002] The invention relates to the use of vinyl acetate copolymers as low-profile additives (LPAs), radically crosslinkable polymer compositions containing the aforementioned low-profile additives and the composite components obtainable therefrom.

[0003] For the production of composite components, radically crosslinkable polymer compositions based, for example, on unsaturated polyester resins (UP resins) are frequently used. Unsaturated polyester resins are generally polycondensates of dicarboxylic acid (anhydrides) with polyols. Another component of the radically crosslinkable polymer compositions is usually ethylenically unsaturated monomers, such as styrene or methacrylate monomers, in order to dissolve the crosslinkable polymer and convert the radically crosslinkable polymer composition into a flowable mass. To initiate the crosslinking of the polymer compositions, peroxides or hydroperoxides, for example, can be used as initiators.Furthermore, the radically crosslinkable polymer compositions may optionally contain fiber materials, such as glass fibers, carbon fibers, natural fibers, or corresponding fiber mats (fiber-reinforced plastic composites = FPR composites), which lead to a reinforcement of the composite components obtainable by curing the radically crosslinkable polymer compositions. Radically crosslinkable polymer compositions can also be used, for example, to manufacture filled solid surface or engineered stone products—composite materials made of unsaturated polyester resins or acrylate resins and mineral fillers, such as quartz or aluminum trihydrate (ATH).

[0004] One problem with processing radically crosslinkable polymer compositions into composite components, especially reinforced or filled components or materials, is their volume shrinkage during curing of the polymer composition. To reduce shrinkage during curing, shrinkage-reducing additives, so-called low-profile additives (LPAs), are added to the radically crosslinkable polymer compositions. Low-profile additives reduce shrinkage during curing, relieve residual stresses, minimize microcracking, and facilitate compliance with manufacturing tolerances.

[0005] Thermoplastics such as polystyrene, polymethyl methacrylate, saturated polyesters, or polyvinyl acetate are often used as low-profile additives. Low-profile additives based on polyvinyl acetate, optionally with carboxyl-functional comonomer units, are described, for example, in DE-OS 2163089, US 3,718,714 A, or US2009182090. Polyvinyl acetate LPAs result in significantly lower shrinkage values ​​in components compared to polystyrene and polymethyl methacrylate LPAs, and in significantly better mechanical properties of components compared to saturated polyester LPAs.

[0006] However, when using vinyl acetate polymers as low-profile additives, there is the challenge of reducing the water absorption capacity of the cured composite components. A higher water absorption capacity impairs the resistance of the composite components when in contact with water, which is particularly significant when used in boat building or generally outdoors. A higher water content can also lead to problems when painting the composite components. Furthermore, there is a need to improve the static mechanical properties, particularly the flexural modulus of elasticity, of composite components made with conventional polyvinyl acetate LPA.

[0007] Against this background, the task was to provide low-profile additives (LPAs) that counteract shrinkage during the curing of radically crosslinkable polymer compositions in a similar way to polyvinyl acetate, but lead to cured composite components with lower water absorption capacity and with the same or preferably higher flexural modulus of elasticity. Furthermore, the LPAs should preferably be block-stable and preferably accessible in a one-step polymerization process by copolymerization of ethylenically unsaturated monomers.

[0008] Surprisingly, the problem was solved with low-profile additives that contained isobornyl acrylate monomer units in addition to vinyl acetate monomer units.

[0009] The invention relates to the use of vinyl acetate-isobornyl acrylate copolymers as low-profile additive (LPA), characterized in that the vinyl acetate-isobornyl acrylate copolymers are based on 2 to 98 wt.% vinyl acetate, 2 to 98 wt.% isobornyl acrylate (IBOA) and optionally one or more further ethylenically unsaturated monomers, each based on the total weight of the vinyl acetate-isobornyl acrylate copolymers.

[0010] The vinyl acetate-isobornyl acrylate copolymers are based on vinyl acetate to an extent of preferably 20 to 97% by weight, particularly preferably 45 to 95% by weight and most preferably 65 to 90% by weight, based on the total weight of the vinyl acetate-isobornyl acrylate copolymers.

[0011] The vinyl acetate-isobornyl acrylate copolymers are based on preferably 2 to 80 wt.%, more preferably 4.9 to 50 wt.%, particularly preferably 8 to 35 wt.% and most preferably 9.5 to 30 wt.% of isobornyl acrylate, based on the total weight of the vinyl acetate-isobornyl acrylate copolymers.

[0012] The other ethylenically unsaturated monomers are generally different from vinyl acetate and isobornyl acrylate.

[0013] Further ethylenically unsaturated monomers can be, for example, one or more vinyl esters different from vinyl acetate. Examples of such vinyl esters are vinyl propionate, vinyl butyrate, isopropenyl acetate, vinyl 2-ethylhexanoate, vinyl laurate, vinyl pivalate and vinyl esters of alpha-branched monocarboxylic acids having 5 to 13 C atoms, for example VeoVa9R, VeoValOR or VeoVallR (trade names of Shell). The vinyl acetate-isobornyl acrylate copolymers are based preferably < 5 wt. %, more preferably < 3 wt. % and particularly preferably < 1 wt. % on vinyl esters different from vinyl acetate, based on the total weight of the vinyl acetate-isobornyl acrylate copolymers. Most preferred are vinyl acetate-isobornyl acrylate copolymers which do not contain any units of vinyl esters other than vinyl acetate.

[0014] Preferred further ethylenically unsaturated monomers are ethylenically unsaturated acids or their salts, especially carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, itaconic acid, and fumaric acid; maleic acid, monoesters of fumaric acid or maleic acid, or their salts, such as the ethyl and isopropyl esters; ethylenically unsaturated sulfonic acids or their salts, preferably vinylsulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid; ethylenically unsaturated phosphonic acids or their salts, preferably vinylphosphonic acid. Ethylenically unsaturated carboxylic acids or their salts are particularly preferred. Most preferred are acrylic acid, methacrylic acid, and crotonic acid. The vinyl acetate-isobornyl acrylate copolymers are based on ethylenically unsaturated acids or their salts to an extent of preferably 0 to 5% by weight, particularly preferably 0.1 to 3% by weight and most preferably 0.5 to 2% by weight, based on the total weight of the vinyl acetate-isobornyl acrylate copolymers.

[0015] Further examples of further ethylenically unsaturated monomers are one or more monomers selected from the group comprising methacrylic acid esters or acrylic acid esters of carboxylic acids with unbranched or branched alcohols having 1 to 15 carbon atoms, which are different from isobornyl acrylate, vinyl aromatics, vinyl halides, dienes, and olefins. Such monomers are preferably copolymerized into the vinyl acetate-isobornyl acrylate copolymers at a concentration of <5% by weight, more preferably <3% by weight, and particularly preferably <1% by weight, based on the total weight of the vinyl acetate-isobornyl acrylate copolymers. Most preferably, no such monomers are copolymerized into the vinyl acetate-isobornyl acrylate copolymers. The vinyl acetate-isobornyl acrylate copolymers have a glass transition temperature Tg of preferably 30 to 100°C, particularly preferably 35 to 85°C, and most preferably 45 to 75°C. The monomer selection orThe weight fractions of the individual monomers are preferably selected to obtain the above-mentioned glass transition temperatures Tg of the vinyl acetate-isobornyl acrylate copolymers. The glass transition temperature Tg can be determined in a known manner by differential scanning calorimetry (DSC). The Tg can also be approximately predicted using the Fox equation. According to Fox TG, Bull. Am. Physics Soc. 1, 3, page 123 (1956), the following applies: 1 / Tg = x1 / Tgl + x2 / Tg2 + ... + xn / Tgn, where xn is the mass fraction (wt.% / 100) of monomer n, and Tgn is the glass transition temperature in Kelvin of the homopolymer of monomer n. Tg values ​​for homopolymers are listed in Polymer Handbook 2nd Edition, J. Wiley & Sons, New York (1975).

[0016] The vinyl acetate-isobornyl acrylate copolymers have molecular weights Mw of preferably 2,000 to 750,000 g / mol, particularly preferably 30,000 to 300,000 g / mol and most preferably 70,000 to 170,000 g / mol (determination method: SEC ("Size Exclusion Chromatography") using a polystyrene standard in THE at 60°C).

[0017] The vinyl acetate-isobornyl acrylate copolymers have a Höppler viscosity of preferably 1 to 100 mPas, particularly preferably 1.2 to 60 mPas, even more preferably 1.8 to 12 mPas and most preferably 2 to 10 mPas (Höppler method at 20°C, DIN 53015, in 10% solution in ethyl acetate).

[0018] The vinyl acetate-isobornyl acrylate copolymers are preferably not emulsifier stabilized and / or preferably not protective colloid stabilized.

[0019] The vinyl acetate-isobornyl acrylate copolymers are generally obtainable by polymerizing the ethylenically unsaturated monomers according to the invention in the presence of free-radical initiators, in particular by means of free-radical-initiated bulk, solution, or suspension polymerization processes. The solution polymerization process is particularly preferred. In the solution polymerization process, the solvent used is preferably an organic solvent or a mixture of organic solvents or a mixture of one or more organic solvents and water. Preferred solvents are alcohols, ketones, esters, ethers, aliphatic hydrocarbons, aromatic hydrocarbons, and water. Particularly preferred solvents are aliphatic alcohols having 1 to 6 carbon atoms, such as methanol, ethanol, n-propanol, or i-propanol; ketones such as acetone or methyl ethyl ketone; esters such as methyl acetate, ethyl acetate, propyl acetate, or butyl acetate; or water.Most preferred are methanol, i-propanol, methyl acetate, ethyl acetate and butyl acetate.

[0020] The temperature during polymerization is preferably from 20°C to 160°C, particularly preferably from 40°C to 140°C. Polymerization is generally carried out at atmospheric pressure, preferably under reflux.

[0021] Suitable free radical initiators are, for example, oil-soluble initiators such as t-butyl peroxy-2-ethylhexanoate, t-butyl peroxypivalate, t-butyl peroxyneodecanoate, dibenzoyl peroxide, t-amyl peroxypivalate, di-(2-ethylhexyl)peroxydicarbonate, 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane and di-(4-t-butylcyclohexyl)peroxydicarbonate. Azo initiators such as azobisisobutyronitrile are also suitable. The initiators are generally used in an amount of 0.005 to 3.0 wt. %, preferably 0.01 to 1.5 wt. %, in each case based on the total weight of the monomers for preparing the vinyl acetate-isobornyl acrylate copolymers.

[0022] The polymerization rate can be controlled, for example, by the temperature, the initiators, by using initiator accelerators or by the initiator concentration. The adjustment of the molecular weight and the degree of polymerization is known to the person skilled in the art. This can be achieved, for example, by adding regulators, by the ratio of solvent to monomers, by varying the initiator concentration, by varying the metered dose of monomers and by varying the polymerization temperature. Regulators or chain transfer agents are, for example, alcohols such as methanol, ethanol and isopropanol, aldehydes or ketones such as acetaldehyde, propionaldehyde, butyraldehyde, acetone or methyl ethyl ketone, and also mercapto-containing compounds such as dodecyl mercaptan, mercaptopropionic acid or mercapto-containing silicones.

[0023] The polymerization can be carried out by initially introducing all or individual components of the reaction mixture, or by partially introducing and subsequently metering all or individual components of the reaction mixture, or by the metering method without introducing any components.

[0024] Volatile residual monomers or other volatile components can be removed, for example, by distillation or stripping processes, preferably under reduced pressure.

[0025] The invention further relates to radically crosslinkable polymer compositions comprising a) at least one crosslinkable, unsaturated polyester resin (UP resin) or vinyl ester resin (VE resin), b) at least one monomer with an ethylenically unsaturated group (reactive monomers), c) at least one initiator, in particular peroxides or hydroperoxides, d) optionally one or more accelerators, such as cobalt- or amine-based accelerators, e) optionally fiber materials, f) optionally fillers, in particular mineral fillers and g) optionally additives, characterized in that one or more vinyl acetate-isobornyl acrylate copolymers according to the invention are additionally present.

[0026] The vinyl acetate-isobornyl acrylate copolymers act as LPA in the radically crosslinkable polymer compositions.

[0027] The radically crosslinkable polymer compositions contain the vinyl acetate-isobornyl acrylate copolymers preferably in an amount of 2 to 35% by weight and particularly preferably in an amount of 4 to 20% by weight, based on the total weight of resin a) and monomer b) and vinyl acetate-isobornyl acrylate copolymer.

[0028] In general, the vinyl acetate-isobornyl acrylate copolymers are used in the form of a 10 to 70 wt.% solution, preferably 30 to 55 wt.% solution, in ethylenically unsaturated monomers, preferably styrene or methacrylates, such as methyl methacrylate (MMA), 1,3-butanediol dimethacrylate (1,3-BDMA), and 1,4-butanediol dimethacrylate (1,4-BDDMA). The vinyl acetate-isobornyl acrylate copolymers are particularly preferably used in a 35 to 55 wt.% solution in styrene, 1,4-BDDMA, or 1,3-BDDMA.

[0029] To improve the mechanical strength after curing, 1 to 20 wt.%, based on vinyl acetate-isobornyl acrylate copolymer, of multifunctional acrylates or methacrylates, such as trimethylolpropane trimethacrylate (TMPTMA), may optionally be added to the solutions.

[0030] The components a) to g) and their amounts used in the radically crosslinkable polymer compositions can in principle be selected by the person skilled in the art in accordance with the requirements of the respective application in a conventional manner.

[0031] Unsaturated polyester resins (UP resins) suitable as resin a) are generally available by polycondensation of unsaturated and saturated dicarboxylic acids or dicarboxylic anhydrides with polyols. Vinyl ester resins (VE resins) suitable as resin a) are obtainable, for example, by esterification of epoxy resins with acrylic or methacrylic acid. Suitable UP resins and VE resins are also commercially available.

[0032] The radically crosslinkable polymer compositions also contain monomers b) with ethylenically unsaturated groups, generally styrene or methacrylate monomers such as methyl methacrylate (MMA) or 1,3- and 1,4-butanediol dimethacrylate (1,3-BDDMA / 1,4-BDDMA). The addition of these monomers to the radically crosslinkable polymer compositions can serve, for example, to dissolve the crosslinkable resin a) or to convert the radically crosslinkable polymer composition into a flowable mass.

[0033] The addition of initiators c) to the radically crosslinkable polymer compositions generally serves to initiate crosslinking of the unsaturated polyester or vinyl ester resin. Common peroxides or hydroperoxides can be used in conventional amounts, for example, cumene hydroperoxide, dibenzoyl peroxide, or methyl ethyl ketone peroxide.

[0034] The radically crosslinkable polymer compositions optionally also contain accelerators d). Accelerators d) can serve to accelerate the decomposition of the initiator. Suitable accelerators and their use amounts are generally known to the person skilled in the art and are commercially available, for example, such as cobalt salts, in particular cobalt octoate, cobalt neodecanoate, or cobalt naphthenate. Preferred radically crosslinkable polymer compositions do not contain accelerators d).

[0035] The radically crosslinkable polymer compositions may optionally contain fiber materials e ) or fillers f ) or additives such as processing aids, in particular thickeners.

[0036] Suitable fiber materials e) include, for example, glass fibers, carbon fibers, natural fibers, or corresponding fiber mats (fiber-reinforced plastic composites = FPR composites). Such fiber materials can be used to reinforce the composite components obtained by curing the radically crosslinkable polymer compositions.

[0037] A further subject of the invention are composite components obtainable by curing the radically crosslinkable polymer compositions according to the invention.

[0038] The free-radically crosslinkable polymer compositions are preferably cured at temperatures of > 0 ° C, particularly preferably from 40 ° C to 180 ° C and most preferably from 70 to 130 ° C. Curing is preferably carried out in the presence of one or more initiators by free-radically initiated polymerization. If appropriate, the free-radically crosslinkable polymer compositions are pressed during curing at the respective temperature using pressures of > 1 mbar, particularly preferably from 1 to 200,000 mbar and most preferably from 1,000 to 200,000 mbar.

[0039] The composite components can be obtained from the radically crosslinkable polymer compositions using all common manufacturing processes, preferably by means of sheet molding compound technology (SMC), bulk molding compound technology (BMC), resin transfer molding (RTM), pultrusion, continuous lamination, or resin injection molding (RIM). The radically crosslinkable polymer compositions according to the invention can be processed into composite components using conventional processes.

[0040] When used as LPAs in radically crosslinkable polymer compositions, the vinyl acetate-isobornyl acrylate copolymers of the invention exhibit a surprisingly strong shrinkage-reducing effect during their curing, similar to polyvinyl acetate, and lead to cured composite components with lower water absorption capacity and the same or even greater flexural modulus of elasticity. Furthermore, the LPAs of the invention are also surprisingly block-stable, even without the addition of antiblocking agents such as carbonates, talc, gypsum, silica, kaolins, or silicates. Advantageously, the LPAs of the invention can also be granulated and provided in the form of block-stable granules.

[0041] The following examples serve to further illustrate the invention without limiting it in any way.

[0042] Production of vinyl acetate-isobornyl acrylate copolymers:

[0043] Example 1: VAc-IBOA copolymer with 15% IBOA and 1% crotonic acid (LPA1): 41 g of vinyl acetate and 24 g of isopropanol were initially charged in a 2 liter glass reactor fitted with an anchor stirrer, reflux condenser and metering devices. The initial charge was then heated to reflux at 150 rpm under a protective gas atmosphere. Once reflux was reached, 0.14 g of tert-butyl peroxypivalate (TBPPI75AL; 75% solution in aliphatics) was added all at once. 15 minutes after the start of the reaction, the initiator mixture comprising 2.3 g of tert-butyl peroxypivalate (TBPPI75AL; 75% solution in aliphatics), 0.90 g of tert. Butylperoxy-2-ethylhexanoate (TBPEH, pure) in 10.8 ml of isopropanol was added over a period of 5 hours. 30 minutes after the start of the reaction, the monomer mixture consisting of 130 g of isobornyl acrylate, 8.6 g of crotonic acid, and 684 g of vinyl acetate was added over a period of 4 hours.After cooling the reaction mixture, the resulting copolymer was dried in vacuum to constant weight.

[0044] Properties of the VAc-IBOA copolymer LPA1 : Höppler viscosity: 6.2 mPas (determined according to DIN 53015 (10% in ethyl acetate at 20°C) ); number average molecular weight M n : 35,300 g / mol, weight-average molecular weight M w: 132,300 g / mol (determined by size exclusion chromatography in THE at 60°C against a narrowly distributed polystyrene standard); glass transition temperature Tg: 49.3°C (determined by differential scanning calorimetry (DSC)). Example 2: VAc-IBOA copolymer with 30% IBOA and 1% crotonic acid (LPA2): 40 g of vinyl acetate and 21 g of isopropanol were placed in a 2-liter glass reactor equipped with an anchor stirrer, reflux condenser, and metering devices. The mixture was then heated to reflux at a stirrer speed of 150 rpm under a protective gas atmosphere. Once reflux was reached, 0.14 g of tert-butyl peroxypivalate (TBPPI75AL; 75% solution in aliphatics) was added all at once. 15 minutes after the start of the reaction, the initiator mixture consisting of 2.3 g of tert-butyl peroxypivalate (TBPPI75AL; 75% solution in aliphatics) and 0.90 g of tert-butyl peroxy-2-ethylhexanoate (TBPEH, pure) in 10.8 ml of isopropanol was added over a period of 5 hours.30 minutes after the start of the reaction, the monomer mixture consisting of 254 g of isobornyl acrylate, 8.5 g of crotonic acid, and 544 g of vinyl acetate was added over a period of 4 hours. After cooling the reaction mixture, the resulting copolymer was dried under vacuum to constant weight.

[0045] Properties of the VAc-IBOA copolymer LPA2 : Höppler viscosity: 5.2 mPas (determined according to DIN 53015 (10% in ethyl acetate at 20°C) ); number average molecular weight M n : 40,100 g / mol, weight-average molecular weight M w : 127,400 g / mol (determined by size exclusion chromatography in THE at 60°C against a narrowly distributed polystyrene standard); glass transition temperature Tg: 57.8°C (determined by differential scanning calorimetry (DSC)).

[0046] Example 3: VAc-IBOA copolymer with 50% IBOA and 1% crotonic acid (LPA3): 39 g of vinyl acetate and 18 g of isopropanol were initially charged in a 2 liter glass reactor equipped with an anchor stirrer, reflux condenser, and metering devices. The initial charge was then heated to reflux at 150 rpm under a protective gas atmosphere. Once reflux was reached, 0.13 g of tert-butyl peroxypivalate (TBPPI75AL; 75% solution in aliphatics) was added all at once. 15 minutes after the start of the reaction, the initiator mixture consisting of 2.2 g of tert-butyl peroxypivalate (TBPPI75AL; 75% solution in aliphatics), 0.90 g of tert. Butylperoxy-2-ethylhexanoate (TBPEH, pure) in 10.5 ml of isopropanol was added over a period of 5 hours. 30 minutes after the start of the reaction, the monomer mixture consisting of 412 g of isobornyl acrylate, 8.2 g of crotonic acid, and 364 g of vinyl acetate was added over a period of 4 hours.After cooling the reaction mixture, the resulting copolymer was dried in vacuum to constant weight.

[0047] Properties of the VAc-IBOA copolymer LPA3 : Höppler viscosity: 4.0 mPas (determined according to DIN 53015 (10% in ethyl acetate at 20°C) ); number average molecular weight M n : 42,100 g / mol, weight-average molecular weight M w : 136,500 g / mol (determined by size exclusion chromatography in THE at 60°C against a narrow-distribution polystyrene standard); glass transition temperature Tg: 67.2°C (determined by differential scanning calorimetry (DSC)).

[0048] Testing of vinyl acetate-isobornyl acrylate copolymers as shrinkage-reducing additives (LPA):

[0049] 1) UP resin compositions and curing at 90°C:

[0050] A mixture was prepared from the raw materials listed in Table 1 and briefly degassed. The density D vof the degassed mixture was determined, then 15 g of the mixture was poured into a mold, cured at 90°C for 2 hours, and then post-cured for 24 hours at room temperature. Finally, the density D H of the cured molded body. The shrinkage was determined by comparing the density D v the mixture before curing with density D H of the molded body after curing with the formula shrinkage (%) = (D H -D V ) / D v x 100 (Table 2). Negative values ​​indicate that the molded body was larger than the original shape after curing.

[0051] The density was determined using the density meter DMA 38 (trade name of Anton Paar) at 23°C.

[0052] The water absorption was determined according to DIN EN ISO 62.

[0053] The test results are summarized in Table 2. Table 1: Crosslinkable polymer compositions:

[0054] *: Palapreg® 18-03: Trade names of AOC AG;

[0055] **: Curox® 1-200: Trade name of United Initiators.

[0056] The following low-profile additives (LPA) were used:

[0057] LPAV1 (comparison example): Vinnapas® C 501 (trade name of Wacker Chemie, carboxylated polyvinyl acetate, Mw = 135,000 g / mol) with approx. 1% crotonic acid in the polymer, T g 43°C;

[0058] LPA1 : Example 1 (15% IBOA, 1% crotonic acid);

[0059] LPA2 : Example 2 (30% IBOA, 1% crotonic acid);

[0060] LPA3 : Example 3 (50% IBOA, 1% crotonic acid);

[0061] Table 2: Shrinkage of the moldings:

[0062] Table 2 shows that the inventive solid resins LPA 1-3 provide comparable shrinkage compensation to Comparative Example 1 with LPAV1, but advantageously significantly reduce water absorption. 2) Production of BMC boards

[0063] First, the UP resin and all additives (see Tables 3 and 4) except for the glass fibers and the filler (calcium carbonate) were premixed in a container using a dissolver for 2 minutes (resin paste). In a second step, this resin paste was premixed with the glass fibers and calcium carbonate in a small laboratory mixer for 15 minutes.

[0064] The BMC compound (Bulk Moulding Compound) was then wrapped in suitable styrene-tight foil and stored for 2 days at 23°C (ripening time) and then placed in a Wickert press (pressing conditions: 3 minutes, 160°C, 730 kN pressing force, 3 mm plate thickness).

[0065] The BMC plates obtained in this way were tested after cooling to room temperature as follows:

[0066] - mechanical properties: determination of the flexural modulus of elasticity according to DIN EN ISO 1425;

[0067] - Shrinkage values ​​(linear shrinkage): determined by measuring and specifying in percentage values;

[0068] - Water absorption of BMC boards according to DIN EN ISO 62.

[0069] The results of the testing are shown in Table 4.

[0070] Table 3: crosslinkable polymer composition: *: Palapreg® 18-03: Trade name of AOC AG; Luperox® P: Trade name of Arkema; ​​Luvatol® MK 35: Trade name of Lehmann&Voss; Plasticolors® CF-20737: Trade name of Chromaflo Technologies (black pigment paste for BMC / SMC).

[0071] Compared with the non-inventive BMC V with VINNAPAS® C 501, the BMC 1-3 with the inventive additives LPA 1-3 show significantly lower values ​​for water absorption and improved values ​​for the flexural elastic modulus, which is a measure of the stiffness of the composite components.

[0072] In addition, a linear shrinkage of 0.05% and less could be achieved in all examples according to the invention.

[0073] Table 4: Test results:

[0074] *: Vinnapas® C 501: Trade name of Wacker Chemie, carboxylated polyvinyl acetate, Mw = 135,000 g / mol.

Claims

Patent claims:

1. Use of vinyl acetate-isobornyl acrylate copolymers as low-profile additives, characterized in that the vinyl acetate-isobornyl acrylate copolymers are based on 2 to 98 wt.% vinyl acetate, 2 to 98 wt.% isobornyl acrylate and optionally one or more further ethylenically unsaturated monomers, each based on the total weight of the vinyl acetate-isobornyl acrylate copolymers.

2. Use of vinyl acetate-isobornyl acrylate copolymers as low-profile additives according to claim 1, characterized in that the vinyl acetate-isobornyl acrylate copolymers are based on 20 to 97 wt. % vinyl acetate, based on the total weight of the vinyl acetate-isobornyl acrylate copolymers.

3. Use of vinyl acetate-isobornyl acrylate copolymers as low-profile additives according to claim 1 or 2, characterized in that the vinyl acetate-isobornyl acrylate copolymers are based on 2 to 80 wt. % isobornyl acrylate, based on the total weight of the vinyl acetate-isobornyl acrylate copolymers.

4. Use of vinyl acetate-isobornyl acrylate copolymers as low-profile additives according to claims 1 to 3, characterized in that one or more further ethylenically unsaturated monomers are selected from the group comprising ethylenically unsaturated carboxylic acids, ethylenically unsaturated sulfonic acids and ethylenically unsaturated phosphonic acids and the salts of the aforementioned acids.

5. Use of vinyl acetate-isobornyl acrylate copolymers as low-profile additives according to claims 1 to 4, characterized in that one or more further ethylenically unsaturated monomers are selected from the group comprising acrylic acid, methacrylic acid, crotonic acid, itaconic acid and fumaric acid, maleic acid, monoesters of fumaric acid and maleic acid or salts thereof.

6. Use of vinyl acetate-isobornyl acrylate copolymers as low-profile additives according to claims 1 to 5, characterized in that the vinyl acetate-isobornyl acrylate copolymers are based on 0 to 5 wt. % of further ethylenically unsaturated monomers, based on the total weight of the vinyl acetate-isobornyl acrylate copolymers.

7. Use of vinyl acetate-isobornyl acrylate copolymers as low-profile additives according to claims 1 to 6, characterized in that the vinyl acetate-isobornyl acrylate copolymers have a glass transition temperature Tg of 30 to 100°C (determined by means of differential scanning calorimetry).

8. Use of vinyl acetate-isobornyl acrylate copolymers as low-profile additives according to claims 1 to 7, characterized in that the vinyl acetate-isobornyl acrylate copolymers have a Höppler viscosity of 1 to 100 mPas (determined by Höppler, according to DIN 53015, at 20°C, in 10% solution in ethyl acetate).

9. Radically crosslinkable polymer compositions comprising a) at least one crosslinkable, unsaturated polyester resin or vinyl ester resin, b) at least one monomer having an ethylenically unsaturated group, c) at least one initiator, d) optionally one or more accelerators, e) optionally fiber materials, f) optionally fillers and g) optionally additives, characterized in that one or more vinyl acetate-isobornyl acrylate copolymers from claims 1 to 8 are additionally present.

10. Composite components obtainable by curing the radically crosslinkable polymer compositions according to claim 9.

Citation Information

Patent Citations

  • unsaturated POLYESTER MOLDING COMPOUND

    DE2163089A1

  • Use of carboxyl-functional polyvinyl acetates for producing BMC parts

    US20090182090A1

  • Improvement in scoop-excavators or dredging-machines for removing mud from the bottoms

    US3718A

  • Jambs secoe

    US714A

  • Use of vinyl ester copolymers as low-profile additives (LPAs)

    DE102009001498A1