Method for producing foam particles from a polycarbonate formulation
The process of using a chain extender with N2 and CO2 in the polycarbonate formulation, along with air cooling and water spraying, effectively produces foam particles with low bulk density and excellent weldability, addressing the need for lightweight components with improved mechanical properties.
Patent Information
- Application Number
- PCT/EP2024/060218
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-19
- Filing Date
- 2024-04-16
- Publication Date
- 2024-10-24
AI Technical Summary
There is a high demand for polycarbonate foam particles with low bulk densities and good weldability, which existing methods have not adequately addressed.
A process involving a polycarbonate formulation with a chain extender and a foaming agent comprising nitrogen (N2) and optionally carbon dioxide (CO2), combined with air cooling and water spraying during granulation, to produce foam particles with low bulk density and improved weldability.
The process results in foam particles with reduced bulk density and enhanced weldability, allowing for the production of lightweight components with complex geometries and improved mechanical properties, including high elongation at break and uniform surface welding.
Smart Images

Figure EP2024060218_24102024_PF_FP_ABST
Abstract
Description
[0001] Process for producing foam particles from a polycarbonate formulation
[0002] The present invention relates to a process for producing foam particles from a polycarbonate formulation, as well as to foam particles obtained or obtainable by the process according to the invention. Furthermore, the invention relates to the use of the foam particles according to the invention and to the use of a chain extender in combination with a foaming agent comprising or consisting of N2 and optionally CO2 in a polycarbonate formulation for producing foam particles.
[0003] State of the art
[0004] Foam particles (also called particle foams, expanded granules, foam particles, foamed beads, etc.), especially those made from thermoplastic polymers, are becoming increasingly important. Today's technology now makes it possible to provide foam particles of reliable quality and to manufacture components with advantageous properties from them. Due to their lower bulk density compared to "simple" thermoplastics, expanded materials open up new fields of application, while conventional applications can be realized with significant weight savings. Expanded thermoplastics are therefore an attractive material, especially for lightweight construction applications, provided their mechanical properties are also sufficiently good.Tool developments in recent years also make it possible to produce components with surfaces that are so aesthetically pleasing that even visible parts made of expanded thermoplastics are a viable alternative to corresponding injection-molded parts, while also being significantly lighter. Due to their lower material consumption, expanded materials are also attractive from a sustainability perspective. Furthermore, their generally good thermal insulation properties can also contribute to energy savings, for example, when used as thermal insulation material or as an additional effect when used as soundproofing material.
[0005] Polycarbonate foam particles have also been described. Foam particles made of engineering thermoplastics are of interest to the automotive industry, for example, due to properties such as high temperature resistance and good fire behavior. Expanded polycarbonate (EPC for short) is a foam particle for high-temperature applications where conventional foam particles such as expanded polypropylene (EPP for short) fail. DE 4100200 A1 describes a process for producing polycarbonate foam from polycarbonate, in which a transesterification catalyst is added to the aromatic polycarbonate in combination with aromatic polycarboxylic acids or water, optionally together with aliphatic hydroxycarboxylic acids and / or aliphatic alcohols. This results in a controlled, partial degradation of the polycarbonate with the release of CO2, which leads to the foaming of the remaining polycarbonate.The polycarbonate foams described in the document have densities of around 0.4 to 0.8 g / cm. 3 on.
[0006] WO 2021 / 106795 A1 discloses a process for producing foamed thermoplastic resin particles. The process consists of a melt-kneading step in which a thermoplastic resin, in particular polypropylene resins, and carbon dioxide gas as a foaming agent are melt-kneaded, and a granulation step in which the foamed thermoplastic resin particles are granulated by a hot-cutting process. In the hot-cutting process, the thermoplastic resin and the molten resin containing the blowing agent are extruded through the holes of the die, and the molten resin extruded from the holes of the die is cut into air with a cutting tool. This involves a step of cooling the molten resin in air during or after foaming, and the granulation step includes a step of ejecting a mixed mist of water and air toward the nozzle opening.
[0007] WO 2012 / 020112 A1 describes an expandable granulate comprising A) a polymer matrix consisting of A1) at least 55% by weight of polyester, 0 to 45% by weight of one or more thermoplastic polymers different from component A1); B) a physical blowing agent component and C) optionally further additives, which is suitable for producing particle foams for use in the automotive industry, aviation industry, construction industry, packaging industry, sports and leisure industry, transport, construction, lightweight construction and / or composite construction.
[0008] WO2014 / 198779 A1 discloses a process for producing expanded granules from a thermoplastic elastomer with an elongation at break of more than 100%, comprising the steps of: (a) pressing a polymer melt containing a blowing agent through a perforated plate heated to a temperature between 150°C and 280°C into a granulation chamber, (b) comminuting the polymer melt pressed through the perforated plate with a cutting device into individual expanding granules, (c) discharging the granules from the granulation chamber with a liquid stream, wherein the blowing agent contains CO2 or N2 or a combination of CO2 and N2 and the amount of blowing agent in the polymer melt containing a blowing agent is in the range from 0.5 to 2.5 wt.-% and wherein the granulation chamber is flowed through by a liquid tempered to a temperature between 5°C and 90°C, the pressure of which is 0.1 bar to 20 bar above the ambient pressure, wherein the pressure and temperature of the liquid in the granulation chamber, as well as the temperature of the perforated plate are selected such that the granules in the pressurised liquid are expanded by the propellant contained therein in such a way that expanded granules with a closed skin are produced.
[0009] WO 03 / 053651 A1 discloses a process for producing granules from expandable thermoplastic polymers by extrusion, comprising: i) melting the polymer in a single-screw or multi-screw extruder; ii) incorporating an expansion agent into the polymer in the molten state; iii) granulating the polymer thus obtained; iv) tempering the granules thus obtained; v) cooling the tempered granules to room temperature.
[0010] EP 3858906 A1 discloses expanded particles containing a polycarbonate-based resin as base resin, wherein the particles have a specified cell density X and a specified average cell wall thickness, as well as an expanded molded body.
[0011] Nevertheless, there is still a high demand for polycarbonate foam particles, especially aromatic polycarbonate, which have low bulk densities and at the same time good weldability.
[0012] Object of the invention
[0013] The object of the present invention was therefore to provide a process for producing foam particles from a polycarbonate formulation containing at least one aromatic polycarbonate, which have a low bulk density and / or good weldability.
[0014] Solution to the task and detailed description
[0015] Surprisingly, it was found that by using a chain extender in the polycarbonate formulation in combination with the use of a foaming agent which comprises or consists of nitrogen (N2) and optionally carbon dioxide (CO2) in certain amounts and total amounts, and air cooling and optionally water spraying during granulation, foam particles are obtained which have a low bulk density and improved weldability.
[0016] The object is therefore achieved by a process for producing foam particles from a polycarbonate formulation containing at least one aromatic polycarbonate, comprising or consisting of the following steps: i) feeding the polycarbonate formulation into an extrusion line and melting and homogenizing the polycarbonate formulation in the extrusion line; ii) introducing a foaming agent into the molten polycarbonate formulation, whereby a foaming agent-containing extrudate is formed; iii) discharging the foaming agent-containing extrudate from the extrusion line to form a foamed extrudate, wherein the foamed extrudate is cooled directly by means of a gaseous cooling medium which comprises or consists of air, and optionally a liquid cooling medium, and comminuted to form foam particles; wherein
[0017] • a chain extender is added to the polycarbonate formulation before step ii) and its content is from 0.20 wt.% to 0.90 wt.%, preferably 0.30 wt.% to 0.70 wt.%, more preferably from 0.40 wt.% to 0.70 wt.%, particularly preferably 0.40 wt.% to 0.50 wt.%, based on the mass of the polycarbonate formulation;
[0018] • the foaming agent comprises or consists of N2 and optionally CO2 and the content of N2 is from 0.05 wt.% to 0.23 wt.%, preferably from 0.18 wt.% to 0.21 wt.%, the content of CO2 is from 0 wt.% to 0.73 wt.%, preferably from 0.30 wt.% to 0.43 wt.% and the total content of N2 and CO2 is from 0.15 to 0.96 wt.%, preferably from 0.18 wt.% to 0.75 wt.%, in each case based on the mass of the polycarbonate formulation dissolved.
[0019] The invention further relates to foam particles obtained or obtainable by the process according to the invention. Furthermore, the invention relates to the use of the foam particles according to the invention for producing lightweight components; automotive components, in particular body components, insulation components, and / or soundproofing elements; body-supporting elements, in particular seats, automotive seats, and / or bicycle seats; insulating layers; composite components, in particular sandwich elements; wind turbine components; and / or protective helmets, in particular bicycle helmets, construction helmets, and / or industrial safety helmets.
[0020] Furthermore, the invention relates to the use of a chain extender in combination with a foaming agent comprising or consisting of N2 and optionally CO2 in a polycarbonate formulation which contains at least one aromatic polycarbonate for producing foam particles, in particular with reduced bulk density and improved weldability, wherein the production is preferably carried out by a process according to one of claims 1 to 16, wherein
[0021] • the N2 content is from 0.05 wt.% to 0.23 wt.%, preferably from 0.18 wt.% to 0.21 wt.%, the CO2 content is from 0 wt.% to 0.73 wt.%, preferably from 0.30 wt.% to 0.43 wt.%, and the total N2 and CO2 content is from 0.15 to 0.96 wt.%, preferably from 0.18 wt.% to 0.75 wt.%, in each case based on the mass of the polycarbonate formulation; and
[0022] • the content of chain extender is from 0.20 to 0.90 wt.%, preferably from 0.30 wt.% to 0.70 wt.%, more preferably from 0.40 wt.% to 0.70 wt.%, particularly preferably from 0.40 wt.% to 0.50 wt.%, based on the mass of the polycarbonate formulation.
[0023] Good or very good weldability means that the beads (foam particles) can be welded under steam at low pressures of 4-6 bar in a standard hot steam diffusion welding process. "Standard" here means that it is an established process in machines that are already used to produce molded parts from other polymer foams using the hot steam diffusion welding process. Preferably, this is a drop-in technology for the EPP welding process, i.e. the post-expandable polycarbonate foam particles can be processed into molded parts on systems that are normally used to produce molded parts from expanded polypropylene; the process known from EPP can also be used.The polycarbonate foam particles can thus be converted into molded parts, even those with complex geometries, by filling corresponding cavities, whereby ultimately only a single corresponding work step is required. The subsequent cutting to size, which is often still required for extrusion foams and which therefore generates waste, is no longer necessary. For good and very good weldability, the welded end product should also have a uniform surface. The beads are completely welded together on the surface, with no cavities present or visible. The welded sheet can preferably not be broken (depending on the density) or can only be broken with great force and / or with severe deflection (dimensions of the sheet in these tests: 300 x 200 x 15 mm). 3) and preferably has good mechanical properties, such as a high elongation at break. The elongation at break can be determined according to ISO 1209-2:2007. The weldability evaluations used in the context of this invention are presented in Figure 3 and Figure 4 and Table 1 below. Accordingly, “very good” weldability exists, for example, if the welded foam particles have a surface similar to A1 in Figure 3, a surface profile similar to A2 in Figure 3 and a closed surface. In contrast, “very poor” weldability exists, for example, if the welded foam particles have a surface similar to D1 in Figure 4, a surface profile similar to D2 in Figure 4 and no closed surface. Photos were taken of the foamed sheets. The photos were converted into a 16-bit grayscale image and a representative area of 2 cm x 2 cm was selected.A 3D surface plot of this area was created with a maximum grit size of 1024 and a smoothing level of 200 (top view), as well as a surface plot (elevation profile image) as a wireframe with a polygon multiplier of 100%. The corresponding elevation profile was created using the image processing software Image-J.
[0024] These exemplary photos and the corresponding elevation profile images were used for the visual assessment of weldability.
[0025] Table 1: For good weldability, it is advantageous if the foam particles exhibit no coalescence (coalescence occurs when five or more foam cells coalesce to form a large cell, determined by scanning electron microscopy according to ASTM E1 508-12a:2019) and an average cell diameter in the range of 100 to 200 pm. In addition, the foam particles should have average particle diameters of 1.0 to 7.0 mm, preferably 2.5 to 5.0 mm, determined according to the method outlined below.
[0026] The polycarbonate formulation preferably has a melt volume flow rate (MVR) of up to 14 cm 3 / (10 min), more preferably up to 12 cm 3 / (10 min), especially preferably 5 cm 3 / (10 min) to 9 cm 3 / (10 min), especially preferably 5.5 cm 3 / (10 min) to 6.5 cm 3 / (10 min), determined according to ISO 1133:2012-3 (test temperature 300°C, mass 1.2 kg).
[0027] "Aromatic polycarbonate" in the sense of the invention refers to both aromatic homopolycarbonates and aromatic copolycarbonates. The polycarbonates can be linear or branched in a known manner. The aromatic polycarbonate used in the process according to the invention can be a single polycarbonate or a mixture of two or more aromatic polycarbonates. Polycarbonate that is a post-consumer or post-industrial recyclate can also be used. Corresponding recyclates can be fed to the extruder as granules or ground material. It is also possible to use recyclate only as part of the aromatic polycarbonate.The aromatic polycarbonate preferably has an OH end group content of at least 350 ppm, preferably 350 ppm to 600 ppm, more preferably 380 ppm to 580 ppm, particularly preferably 400 ppm to 550 ppm, and most preferably 450 to 550 ppm, based on the total weight of the aromatic polycarbonate. The OH end group content is determined according to DIN EN ISO 4629:2016-2 using 1H NMR spectroscopy with dichloromethane as the solvent at room temperature, evaluating the ratio of the integrals of the signals at 6.68 ppm (two aromatic protons ortho to phenolic OH groups) and at 1.68 ppm (six methyl protons of the bisphenol A unit).
[0028] The polycarbonate formulation may contain additives, in particular pigments, talc, carbon black, or mixtures thereof. Additives may further include, for example, thermal stabilizers, flame retardants, antioxidants, mold-release agents, colorants, anti-drip agents, UV absorbers, IR absorbers, nucleating agents, impact modifiers, antistatic agents, optical brighteners, light scattering agents, transesterification inhibitors, compatibilizers, and / or additives for laser marking. The additives are preferably added to the polycarbonate formulation before step ii). Accordingly, the additives may already be present in the polycarbonate formulation when it is fed into the extrusion line and / or may be added to the polycarbonate formulation in the extrusion line. The additives can be used in low concentrations of 0.1 to 1.0 wt.%, preferably 0.15 to 0.5 wt.%, particularly preferably in concentrations of 0.2 to 0.3 wt.% are added, based on the mass of the polycarbonate formulation including the chain extender. By adding nucleating agents, the metered amount of gas must be adjusted (reduced) depending on the type, amount, and nucleation efficiency of the additive. To initiate foam cell formation for a finer and more homogeneous cell morphology, nucleating agents such as nano-talc, graphite, carbon black, pigments, etc. are preferably added in low concentrations of 0.1 to 1.0 wt. %, more preferably 0.15 to 0.5 wt. %, particularly preferably in concentrations of 0.2 to 0.3 wt. %, whereby the stated amounts refer to the resulting total composition of polycarbonate-based composition and chain extender.
[0029] Suitable chain extenders are generally amines, carboxyl compounds, maleic anhydride-modified compounds, epoxy-functionalized compounds, oxazolines, carbodiimides and / or functionalized polymers, for example based on acrylate and / or styrene, which have the corresponding functional group. Such compounds can be used alone or in a mixture. Such groups include, for example, amine functions in the amines, carboxyl functions in the carboxyl compounds, anhydride functions in maleic anhydride-modified compounds, epoxy functions in epoxy-functionalized compounds or other functions that can react with the OH end groups of the polycarbonate to form a chain. Epoxy-functionalized compounds are particularly preferred as chain extenders, most preferably epoxy-functionalized styrene-acrylic-based polymers, which are available, for example, from BASF SE as Joncryl® additives, e.g.Joncryl ADR 4368, ADR 4400, ADR 4468 are offered. The chain extender preferably comprises or consists of at least one epoxy-functionalized compound, preferably with an epoxy equivalent weight (EEW) of 285 to 485 g / mol, determined according to DIN EN 1877-1:2000.
[0030] The extrusion system preferably comprises or consists of a twin-screw extruder or a co-kneader, at least one single-screw extruder or a melt cooler, optionally at least one melt pump, and / or at least one perforated plate. More preferably, the extrusion system comprises or consists of a twin-screw extruder or a co-kneader, at least one single-screw extruder or a melt cooler, optionally at least one melt pump, and at least one perforated plate.
[0031] In detail, the process can be implemented in various configurations. Preferably, the twin-screw extruder or the co-kneader, optionally another melt pump, the single-screw extruder or the melt cooler, optionally the melt pump, and the die plate are arranged consecutively. Preferably, steps i) and ii) are carried out in the twin-screw extruder or co-kneader, the single-screw extruder or melt cooler generates a residence time for the foaming agent-containing extrudate, and the melt pump(s) generate(s) pressure to retain the blowing agent in the foaming agent-containing extrudate and discharge(s) the foaming agent-containing extrudate through the die plate according to step iii). Residence time is understood to be the time between the supply of the polycarbonate formulation and the discharge of the foaming agent-containing extrudate.The residence time generated for the foaming agent-containing extrudate should be long enough to allow the chain extender to react sufficiently, and short enough to ensure no or only insignificant polymer degradation. The residence time generated for the foaming agent-containing extrudate is preferably 4 to 15 minutes. The diameter of the holes for a perforated plate is preferably in the range of 0.8 to 3.0 mm, more preferably 1.0 to 2.4 mm. The perforated plate can be a single-hole plate or a multi-hole plate.
[0032] Granulation (discharging the foaming agent-containing extrudate and cooling and comminuting the foamed extrudate) at the conclusion of the process according to the invention preferably takes place without additional pressurization, i.e., at atmospheric pressure. When the foaming agent-containing extrudate is discharged from the extrusion line, the foamed extrudate is formed. This occurs—without being bound to any theory—as a result of the expansion of the foaming agent, whereby after a certain time, a complete or almost complete gas exchange has taken place, so that only the normal air composition remains in the then granulated, expanded polycarbonate beads (foam particles).Therefore, a constant pressure should be maintained at least from the time the blowing agent is added until discharge (preferably upstream of the die plate). This allows the foaming agent to dissolve completely in the polycarbonate formulation, thus preserving the foaming agent-containing extrudate. In other words, the pressure should be selected so that it is above the critical solution pressure of the foaming agent. This pressure is preferably at least 74 bar, especially if the foaming agent comprises or consists of N2 and CO2.
[0033] The foaming agent-containing extrudate is discharged from the extrusion line, preferably through a die plate, preferably at a melt temperature T of TI = (Tg + 110 °C) to T2 = (Tg + 170 °C), more preferably from TI = (Tg + 120 °C) to T2 = (Tg + 160 °C), particularly preferably in the range of TI = (Tg + 130 °C) to T2 = (Tg + 150 °C). The temperature of the die plate is also preferably set to a temperature of Tg + (130 to 150 °C) in order to prevent the die holes from freezing due to cooling extrudate and thus ensure a homogeneous granule size (foam particle size) and good granule quality (foam particle quality), as well as to achieve corresponding foam expansion with the highest possible expansion potential.Cooling begins immediately after the foaming agent-containing extrudate is dispensed or - if dispensed through a perforated plate - at the perforated plate and is continued via a cooling section.
[0034] It is further preferred that the air used as gaseous cooling medium has a pressure of 40-48 m 3Air is introduced per kilogram of foamed extrudate. The liquid cooling medium preferably comprises or consists of water, glycerol or mixtures thereof, preferably water. The liquid medium, in particular if it comprises or consists of water, is preferably sprayed in. Furthermore, it is preferred that the liquid cooling medium is introduced by means of spray nozzles at an amount of 0.06 to 0.26 l of liquid cooling medium per kilogram of foamed extrudate. Furthermore, it is preferred that the flow of the gaseous cooling medium and / or the liquid cooling medium is guided substantially transversely to the outflow direction of the foamed extrudate. Preferably, the foamed extrudate is cooled in step iii) directly by means of a gaseous cooling medium which comprises or consists of air, and a liquid cooling medium which in particular comprises or consists of water.
[0035] The comminution in step iii) is preferably carried out by means of a cutting device. The cutting device can, for example, comprise rotating blades.
[0036] The foaming agent can be introduced at various points, such as by liquid dosing or high-pressure dosing. If the foaming agent comprises or consists of N2 and CO2, it is preferred that the mass ratio of N2 to CO2 be between 0.9:1 and 2.6:1.
[0037] The bulk density of the foam particles obtained by the process according to the invention is preferably 50 to 160 g / l, more preferably 50 to 100 g / l. The bulk density is determined in accordance with DIN EN ISO 60:2000-01. "In accordance" here means that instead of the standardized aluminum container with a known volume, a 1 L beaker was filled and its contents were weighed to determine the density of the material.
[0038] Furthermore, the foam particles according to the invention preferably have an average particle diameter of 1.0 to 7.0 mm, more preferably 2.5 to 5.0 mm. The average particle diameter of the foam particles was determined using a Camsizer according to ISO 13322-2.
[0039] Furthermore, the foam particles according to the invention preferably have an average cell diameter of 100 to 200 pm. The average cell diameter represents the average equivalent diameter of the cells to a circle with the same projection area and is determined by scanning electron microscopy (SEM) according to ASTM E1508-12a:2019.
[0040] Embodiments
[0041] The present invention particularly relates to the following embodiments:
[0042] According to a first embodiment, the invention relates to a process for producing foam particles 12 from a polycarbonate formulation containing at least one aromatic polycarbonate, comprising or consisting of the following steps: i) feeding the polycarbonate formulation into an extrusion line and melting and homogenizing the polycarbonate formulation in the extrusion line; ii) introducing a foaming agent into the molten polycarbonate formulation, whereby a foaming agent-containing extrudate is formed; iii) discharging the foaming agent-containing extrudate from the extrusion line to form a foamed extrudate, wherein the foamed extrudate is cooled directly by means of a gaseous cooling medium which comprises or consists of air, and optionally a liquid cooling medium, and comminuted to form foam particles 12; wherein
[0043] • a chain extender is added to the polycarbonate formulation before step ii) and its content is from 0.20 wt.% to 0.90 wt.%, based on the mass of the polycarbonate formulation;
[0044] • the foaming agent comprises or consists of N2 and optionally CO2 and the N2 content is from 0.05 wt.% to 0.23 wt.%, the CO2 content is from 0 wt.% to 0.73 wt.% and the total N2 and CO2 content is from 0.15 to 0.96 wt.%, in each case based on the mass of the polycarbonate formulation.
[0045] According to a second embodiment, the invention relates to a process according to embodiment 1, characterized in that the aromatic polycarbonate, based on the total weight of the aromatic polycarbonate, has a content of OH end groups of at least 350 ppm, preferably from 350 to 600 ppm, more preferably from 380 to 580 ppm, particularly preferably from 400 to 550 ppm, most particularly preferably from 450 to 550 ppm, determined by means of 'H-NMR spectroscopy with dichloromethane as solvent at room temperature, and / or the polycarbonate formulation has a melt volume flow rate MVR of up to 12 cm 3 / (10 min), determined according to ISO 1133:2012-3 (test temperature 300°C, mass 1.2 kg).
[0046] According to a third embodiment, the invention relates to a process according to embodiment 1 or 2, characterized in that additives, in particular pigments, talc, carbon black or mixtures thereof, are contained in the polycarbonate formulation or are added to the polycarbonate formulation before step ii).
[0047] According to a fourth embodiment, the invention relates to a method according to one of the preceding embodiments, characterized in that the extrusion plant comprises or consists of at least one twin-screw extruder or a co-kneader 1, at least one single-screw extruder or a melt cooler 4, optionally at least one melt pump 5 and / or at least one perforated plate 6).
[0048] According to a fifth embodiment, the invention relates to a process according to embodiment 4, characterized in that the twin-screw extruder or the co-kneader 1, optionally a further melt pump 5, the single-screw extruder or the melt cooler 4, optionally the melt pump 5 and the perforated plate 6 are connected consecutively downstream, wherein preferably steps i) and ii) take place in the twin-screw extruder or co-kneader 1, the single-screw extruder or melt cooler 4 generates a residence time for the foaming agent-containing extrudate and the melt pump or the melt pumps 5 generate / generate a pressure in order to keep the blowing agent in the foaming agent-containing extrudate and to discharge the foaming agent-containing extrudate through the perforated plate 6 according to step iii).
[0049] According to a sixth embodiment, the invention relates to a method according to one of the preceding embodiments, characterized in that the air used as gaseous cooling medium has a pressure of 40 to 48 m 3 Air is introduced per kilogram of foamed extrudate.
[0050] According to a seventh embodiment, the invention relates to a process according to one of the preceding embodiments, characterized in that the liquid cooling medium comprises or consists of water, glycerol or mixtures thereof, preferably water, wherein the liquid cooling medium is preferably introduced by means of spray nozzles at an amount of 0.06 to 0.26 l of liquid cooling medium per kilogram of foamed extrudate.
[0051] According to an eighth embodiment, the invention relates to a method according to one of the preceding embodiments, characterized in that the flow of the gaseous cooling medium and / or the liquid cooling medium is guided substantially transversely to the outflow direction of the foamed extrudate. According to a ninth embodiment, the invention relates to a method according to one of the preceding embodiments, characterized in that the comminution in step iii) is carried out by means of a cutting device 8.
[0052] According to a tenth embodiment, the invention relates to a process according to one of the preceding embodiments, characterized in that the content of chain extender is from 0.30 wt.% to 0.70 wt.%, preferably from 0.40 wt.% to 0.70 wt.%, more preferably 0.40 wt.% to 0.50 wt.%, based on the mass of the polycarbonate formulation.
[0053] According to an eleventh embodiment, the invention relates to a process according to one of the preceding embodiments, characterized in that the mass ratio of N2 to CO2 is from 0.9:1 to 2.6:1.
[0054] According to a twelfth embodiment, the invention relates to a process according to one of the preceding embodiments, characterized in that the N2 content is from 0.18 wt.% to 0.21 wt.%, the CO2 content is from 0.30 wt.% to 0.43 wt.% and / or the total N2 and CO2 content is from 0.18 wt.% to 0.75 wt.%, in each case based on the mass of the polycarbonate formulation.
[0055] According to a thirteenth embodiment, the invention relates to a process according to one of the preceding embodiments, characterized in that the chain extender comprises or consists of at least one epoxy-functionalized compound, preferably at least one epoxy-functionalized compound having an epoxy equivalent weight of 285 to 485 g / mol, determined according to DIN EN 1877-1:2000.
[0056] According to a fourteenth embodiment, the invention relates to a process according to one of the preceding embodiments, characterized in that the bulk density of the foam particles (12) is 50 to 160 g / l, preferably 50 to 100 g / l, determined by means of the method set out above.
[0057] According to a fifteenth embodiment, the invention relates to a process according to any one of the preceding embodiments, characterized in that the foam particles 12 have an average particle diameter of 1.0 to 7.0 mm, preferably 2.5 to 5.0 mm, determined by the method set out above. According to a sixteenth embodiment, the invention relates to a process according to any one of the preceding embodiments, characterized in that the foam particles 12 have an average cell diameter of 100 to 200 pm, determined by the method set out above.
[0058] According to a seventeenth embodiment, the invention relates to foam particles 12 obtained or obtainable by a process according to any one of embodiments 1 to 16.
[0059] According to an eighteenth embodiment, the invention relates to the use of the foam particles 12 according to embodiment 17 for the production of lightweight components; automotive components, in particular body components, insulation components and / or soundproofing elements; body-supporting elements, in particular seats, automotive seats and / or bicycle seats; insulating layers; composite components, in particular sandwich elements; wind power components and / or protective helmets, in particular bicycle helmets, construction helmets and / or industrial protective helmets.
[0060] According to a nineteenth embodiment, the invention relates to the use of a chain extender in conjunction with a foaming agent, comprising or consisting of N2 and optionally CO2, in a polycarbonate formulation which contains at least one aromatic polycarbonate, for producing foam particles 12, in particular with reduced bulk density and improved weldability, wherein the production is preferably carried out by a process according to one of embodiments 1 to 16, wherein
[0061] • the N2 content is from 0.05 wt% to 0.23 wt%, the CO2 content is from 0 wt% to 0.73 wt% and the total N2 and CO2 content is from 0.15 to 0.96 wt%, in each case based on the mass of the polycarbonate formulation; and
[0062] • the chain extender content is from 0.20 to 0.90 wt.%, based on the mass of the polycarbonate formulation.
[0063] Figures and examples
[0064] The present invention is explained below with reference to Figures 1, 2, 3 and 4 as well as the following examples, but is not limited to these. Figure 1 shows a schematic representation of an inventive
[0065] Extrusion plant for producing foam particles from a polycarbonate formulation;
[0066] Figure 2: a schematic representation of another inventive
[0067] Extrusion plant for producing foam particles from a polycarbonate formulation;
[0068] Figure 3: exemplary photos (Al and Bl) and surface profiles (A2 and B2) of the surface of foamed sheets with very good (Al, A2) or good weldability (Bl, B2); and
[0069] Figure 4: exemplary photos (CI and Dl) and surface profiles (C2 and D2) of the surface of foamed sheets with poor (Cl, C2) and very poor (Dl, D2) weldability.
[0070] The extrusion system shown in Figure 1 comprises a twin-screw extruder 1 for carrying out steps i) and ii), which has an inlet for supplying the polycarbonate formulation 2 and an injection point for introducing the foaming agent 3. Furthermore, additives or a chain extender, for example, can be added via the inlet 2, provided they are not already contained in the polycarbonate formulation. Following the twin-screw extruder 1 are a single-screw extruder 4 for generating a residence time for the foaming agent-containing extrudate, as well as a melt pump 5. The melt pump 5 serves to generate pressure to retain the blowing agent in the foaming agent-containing extrudate and to extrude the foaming agent-containing extrudate through a perforated plate 6 further downstream according to step iii).On the side of the exit point of the perforated plate 6, there is a directly adjacent cutting chamber 7 in which the foamed extrudate and the foam particles 12 are formed. Within the cutting chamber 7 and immediately behind the exit point of the perforated plate 6, a cutting device 8 is arranged for comminuting the foamed extrudate, thereby obtaining the foam particles 12. Furthermore, both an air cooling system 9 and a water spray system 10 are provided in the cutting chamber 7, essentially transverse to the outflow direction of the foamed extrudate, in order to provide both air and, if necessary, water for cooling the foamed extrudate during comminution and to transport the resulting foam particles 12 in the direction of the outflowing air.The foam particles 12 can then be fed into a cyclone 11, which is adjacent to the cutting chamber and is located in the outflow direction of the air cooling 9, for drying the foam particles 12, whereby the dried foam particles 12 are obtained.
[0071] The extrusion system shown in Figure 2 differs from that in Figure 1 only in that an additional melt pump 5 is connected between the twin-screw extruder and the single-screw extruder.
[0072] Examples and comparison examples:
[0073] Raw materials used:
[0074] PCI: An aromatic polycarbonate based on bisphenol A with an MVR of 6 cm 3 / 10 min (300°C / l.2 kg, ISO 1133-1:2011) and a softening temperature (VST / B 120; ISO 306:2013) of 149°C. M w, determined as described below, approximately 30,900 g / mol at 28 kDa (MALLS). Contains 0.06% thermal stabilizer and 0.1% UV stabilizer. OH end group content, determined by 'H NMR spectroscopy with dichloromethane as solvent at room temperature (as described above): 470 ppm.
[0075] Manufactured using the melt condensation process (SPC).
[0076] Chain extender 1: A commercially available and multifunctional chain extender from BASF SE (Joncryl ADR 4468) based on epoxy-reactive group-containing styrene-acrylic polymer with a medium molecular weight (gel permeation chromatography in ortho-dichlorobenzene at 150 °C with polystyrene calibration) M w = 7,250 g / mol, an epoxy equivalent weight of 310 g / mol, determined according to DIN EN 1877-1:2000-12, a glass transition temperature T g of 59 °C and a decomposition temperature of 350 °C, determined according to DIN EN ISO 11357-1:2017.
[0077] Methods: The mean particle diameter, bulk density, mean cell diameter, weldability and coalescence of the foam particles were determined as described above.
[0078] Experimental procedure:
[0079] For the tests described below, two different process setups were used: a) Twin-screw extruder-gas dosing-single-screw extruder - optional melt pump-air granulation
[0080] A co-rotating twin-screw extruder (twin-screw extruder 1) from Reifenhäuser (Troisdorf, Germany) with a 43 D diameter was operated at a throughput of 25-30 kg / h, a screw speed of 100 rpm, and profile temperatures of 100-160 °C (barrels 1 to 3), 240 °C (barrel 4) to 280 °C (barrels 5-10). PCI granules and optionally chain extender 1 were metered through the main feed (feed for the polycarbonate formulation 2). CO2 was metered via a LEWA liquid metering station, and N2 was metered via a Maximator via an injection point in barrel 6 (injection point for the introduction of foaming agent 3). The twin-screw extruder 1 used here has 10 consecutive heated zones / barrels in the direction of travel with corresponding temperature control and pressure detection, with zone 1 being located on the feed side and zone 10 near the outlet side of the twin-screw extruder 1.The chain extender and blowing agent contents used in the experiments are listed in Tables 2 to 4 along with the test results obtained. The melt was conveyed via a heated transfer pipe (290 °C) into a single-screw extruder (single-screw extruder 4) from Reifenhäuser. Single-screw extruder 4 was also operated at a continuous barrel temperature of 280 °C and features four heatable zones with appropriate temperature control and pressure sensors. The speed of the single-screw extruder was 26 rpm. A melt pump 5 was installed at the end of single-screw extruder 4 in some of the experiments. Melt pump 5 was operated under pressure control at an inlet pressure of 110 bar and a temperature of 280 °C. The use of melt pump 5 resulted in higher solubilities of the blowing agents. Behind melt pump 5 there was an EWA50 Air air granulator from ECON.A die plate 6 with 8 holes, a hole diameter of 1 mm, and a stirrup length of 2.5 mm was used. The melt residence time between inlet and outlet was approximately 7-10 minutes. The cutter head was equipped with three knives (cutting device 8). The cutting chamber 7 is continuously flushed with an air stream from an air cooling system 9 of the ECON EWA50 Air air pelletizer. The air flow was 1200 m³. 3 / h at a fan speed of 3000 rpm. A water injection system with two spray nozzles (water injection 10) was also installed in the cutting chamber. These sprayed water from the front onto an area below the die plate. The injected water volume was 6.4 l / h. This water injection system could be operated in various ways, either in continuous operation or in cyclic operation with a spray time of 1 s and a pause time of 2 s. The start-up switch and the die plate were heated to 260 °C. Melt pump 5 was heated to 280 °C. The cut granules (foam particles) were blown into a cyclone by an air stream.
[0081] The schematic process setup is shown in Fig. 1, where the melt pump 5 is optional. b) Twin-screw extruder-gas dosing-single-screw extruder-melt pump-underwater pelletizing
[0082] Process structure as in a) with the following difference:
[0083] An underwater pelletizing unit from Econ (EWA 50) (E) was installed behind the melt pump. A perforated plate with five holes, each 1.5 mm in diameter and 3 mm long, was used. The melt's residence time between inlet and outlet was approximately 7-10 minutes. After exiting, the melt was separated in the cutting chamber by a rotating cutter head. The cutter head was equipped with five knives. The resulting pellets were processed in a 70-80 °C cold water circuit at a water flow rate of 28 m³. 3 / h and conveyed into a centrifuge instead of a cyclone, where the water was separated from the granules.
[0084] Inventive Example 1
[0085] For Example 1 according to the invention, process setup a) with air pelletizing was used. No melt pump was installed. Water was continuously sprayed into the area below the die plate via the two spray nozzles at a flow rate of 6.4 l / h.
[0086] The throughput was 25 kg / h. The pelletizer speed was 3000 rpm. The melt temperature was 305 °C. The melt pressure in the twin-screw extruder increased gradually from 45 bar at barrel 5 to 320 bar at the tip of the twin-screw extruder. The melt pressure upstream of the die plate was 240 bar.
[0087] The foam particles in this example were round and had an average particle diameter of 3.2–3.9 mm. The bulk density of the foam particles was 160 g / l. The average cell diameter was 124 μm, and the cell structure showed no coalescence. The foam particles could be easily welded.
[0088] Inventive Example 2
[0089] Inventive Example 2 was carried out using the same process setup as Inventive Example 1. No melt pump was installed. Water was continuously sprayed onto the area below the die plate via the two spray nozzles.
[0090] The throughput was 30 kg / h. The granulator speed was 3000 rpm. The melt temperature was 305 °C. The melt pressure at the tip of the twin-screw extruder was 302 bar. The melt pressure upstream of the die plate was 243 bar.
[0091] The foam particles in this example were round and had an average particle diameter of 3.9–4.5 mm. The bulk density of the foam particles was 100 g / l. The average cell diameter was 193 μm, and the cell structure showed no coalescence. The foam particles could be welded very well.
[0092] Inventive Example 3
[0093] Inventive Example 3 was carried out using the same process setup as Inventive Example 1. A melt pump was installed. Water was continuously sprayed onto the area below the perforated plate via the two spray nozzles.
[0094] The throughput was 30 kg / h. The granulator speed was 3000 rpm. The melt temperature was 305 °C. The melt pressure at the tip of the twin-screw extruder was 303 bar. The melt pressure upstream of the die plate was 240 bar.
[0095] The foam particles in this example were round and had an average particle diameter of 3.9–4.5 mm. The bulk density of the foam particles was 88 g / l. The average cell diameter was 112 μm, and the cell structure showed no coalescence. The foam particles could be easily welded.
[0096] Comparison example 4
[0097] Comparative Example 4 was carried out using the same process setup as Inventive Example 1. No melt pump was installed. Unlike Example 1, no water was sprayed into the cutting chamber via the spray nozzles. This led to the foam particles sticking together. The foam particles were therefore not processable using this process.
[0098] The throughput was 25 kg / h. The granulator speed was 2500 rpm.
[0099] Melt temperature was 305 °C. The melt pressure at the top of the
[0100] The twin-screw extruder's pressure was 320 bar. The melt pressure upstream of the die plate was 260 bar.
[0101] Comparison example 5
[0102] Comparative Example 5 was carried out using the same process setup and the same process parameters as Comparative Example 4. No melt pump was installed. In contrast to Comparative Example 4, water was sprayed intermittently via the spray nozzles in the cutting chamber (2 s pause; 1 s water injection). This amount of water was also insufficient to prevent the foam particles from sticking together. The foam particles could not be processed using this process.
[0103] Comparison example 6
[0104] Comparative Example 6 was carried out using the same process setup as Comparative Example 4. No melt pump was installed. Water was continuously sprayed onto the area below the die plate via the two spray nozzles. The throughput was 25 kg / h. The granulator speed was 2500 rpm.
[0105] The melt temperature was 305 °C. The melt pressure at the tip of the twin-screw extruder was 260 bar. The melt pressure before the die plate was 190 bar.
[0106] The foam particles in this comparative example were round and had an average particle diameter of 3.5–4 mm. The bulk density of the foam particles was 140 g / l. However, the average cell diameter of 370 pm was relatively large, and the cell structure exhibited coalescence. The foam particles were very difficult to weld.
[0107] Comparison example 7
[0108] Comparative Example 7 was carried out using the same process setup as Inventive Example 1. No melt pump was installed. Water was continuously sprayed onto the area below the die plate via the two spray nozzles.
[0109] The throughput was 25 kg / h. The granulator speed was 2500 rpm.
[0110] Melt temperature was 305 °C. The melt pressure at the top of the
[0111] The twin-screw extruder's pressure was 260 bar. The melt pressure upstream of the die plate was 190 bar.
[0112] The foam particles in this comparative example were elongated and had an average particle diameter of 1.9–2.4 mm. The bulk density of the foam particles was very high at 310 g / l. The average cell diameter was 59 μm, and the cell structure showed coalescence. The foam particles were very difficult to weld. The blowing agent concentration was too high for this process window.
[0113] Comparison example 8
[0114] Comparative Example 8 was carried out using the same process setup as Inventive Example 1. No melt pump was installed. Water was continuously sprayed onto the area below the die plate via the two spray nozzles.
[0115] The throughput was 25 kg / h. The granulator speed was 2500 rpm.
[0116] Melt temperature was 305 °C. The melt pressure at the top of the
[0117] The pressure of the twin-screw extruder was 320 bar. The melt pressure upstream of the die plate was 260 bar. The foam particles in this comparative example were round and had an average particle diameter of 3.7–4.2 mm. The bulk density of the foam particles was 180 g / l. The average cell diameter was 374 μm, and the cell structure showed coalescence. The foam particles were very difficult to weld.
[0118] Comparison example 9
[0119] Comparative Example 9 was carried out using the same process setup as Inventive Example 1. No melt pump was installed. Water was continuously sprayed onto the area below the die plate via the two spray nozzles.
[0120] The throughput was 25 kg / h. The granulator speed was 2500 rpm.
[0121] Melt temperature was 305 °C. The melt pressure at the top of the
[0122] The twin-screw extruder's pressure was 360 bar. The melt pressure upstream of the die plate was 276 bar.
[0123] The foam particles in this comparative example were round and had an average particle diameter of 4.1–5.4 mm. The bulk density of the foam particles was 60 g / l. The average cell diameter was 193 μm, and the cell structure showed coalescence. The foam particles were difficult to weld.
[0124] Comparison example 10
[0125] Comparative Example 10 was carried out using the same process setup as Inventive Example 1. No melt pump was installed. Water was continuously sprayed onto the area below the die plate via the two spray nozzles.
[0126] The throughput was 25 kg / h. The granulator speed was 3000 rpm.
[0127] Melt temperature was 303 °C. The melt pressure at the top of the
[0128] The twin-screw extruder's pressure was 246 bar. The melt pressure upstream of the die plate was 203 bar.
[0129] The foam particles in this comparative example were elongated and had an average particle diameter of 3.2–3.6 mm. The bulk density of the foam particles was 160 g / l. The average cell diameter was 124 μm, and the cell structure showed coalescence. The foam particles were very difficult to weld.
[0130] Comparative Example 11 Comparative Example 11 was carried out using the same process setup as Inventive Example 1. No melt pump was installed. Water was continuously sprayed onto the area below the die plate via the two spray nozzles.
[0131] The throughput was 25 kg / h. The granulator speed was 3000 rpm.
[0132] Melt temperature was 303 °C. The melt pressure at the top of the
[0133] The twin-screw extruder's pressure was 246 bar. The melt pressure upstream of the die plate was 203 bar.
[0134] The foam particles in this comparative example were elongated and had an average particle diameter of 2.8–3.0 mm. The bulk density of the foam particles was 220 g / l. The average cell diameter was 70 μm, and the cell structure showed coalescence. The foam particles were very difficult to weld. The blowing agent concentration was too high for this process window.
[0135] Comparison example 12
[0136] Comparative Example 12 was carried out using the same process setup as Inventive Example 1. No melt pump was installed. Water was continuously sprayed onto the area below the die plate via the two spray nozzles.
[0137] The throughput was 30 kg / h. The granulator speed was 3000 rpm. The melt temperature was 305 °C. The melt pressure at the tip of the twin-screw extruder was 215 bar. The melt pressure upstream of the die plate was 185 bar.
[0138] The foam particles in this comparative example were slightly elongated and had an average particle diameter of 3.3–3.6 mm. The bulk density of the foam particles was 150 g / l. The average cell diameter was 225 μm, and the cell structure showed coalescence. The foam particles were very difficult to weld.
[0139] Comparison example 13
[0140] Comparative Example 13 was carried out using the same process setup as Inventive Example 1. A melt pump was installed. Water was continuously injected into the area below the die plate via the two spray nozzles. The throughput was 30 kg / h. The granulator speed was 3000 rpm. The melt temperature was 305 °C. The melt pressure at the tip of the twin-screw extruder was 247 bar. The melt pressure upstream of the die plate was 270 bar.
[0141] The foam particles in this comparative example were round and had an average particle diameter of 3.8–4.7 mm. The bulk density of the foam particles was 83 g / l. The average cell diameter was 109 μm, and the cell structure showed coalescence. The foam particles were difficult to weld.
[0142] Comparison example 14
[0143] In Comparative Example 14, setup b) with underwater pelletizing (UWG) was used instead of air pelletizing. A melt pump was installed.
[0144] The throughput was 29 kg / h. The pelletizer speed was 2100 rpm. The melt temperature was 306 °C. The melt pressure at the tip of the twin-screw extruder was 296 bar. The melt pressure upstream of the die plate was 194 bar.
[0145] The foam particles in this comparative example were round and had an average particle diameter of approximately 4 mm. The bulk density of the foam particles was 170 g / l. The component density of a resulting component after welding was 270 kg / m 3 The average cell diameter was 84 pm, and the cell structure showed no coalescence. The foam particles could be easily welded. The comparative example shows the significantly higher bulk density with UWG compared to air granulation under comparable parameters.
[0146] The material parameters (content of chain extender and blowing agent) were varied in the tests, as shown in Tables 2 to 4 below together with the test results obtained.
[0147] Comparison example 15
[0148] In Comparative Example 15, setup b) with underwater pelletizing (UWG) was used instead of air pelletizing. A melt pump was installed.
[0149] The throughput was approximately 15 kg / h. The granulator speed was 1500 rpm. The melt temperature was 290 °C. The melt pressure at the tip of the twin-screw extruder was 94 bar. The melt pressure upstream of the die plate was 90 bar. The foam particles in this comparative example were slightly elongated and had an average particle diameter of 3.5–4 mm. The bulk density of the foam particles was 340 g / l. The average cell diameter and cell structure were not determined. The foam particles were very difficult to weld.
[0150] Comparison example 16
[0151] In Comparative Example 16, setup b) with underwater pelletizing (UWG) was used instead of air pelletizing. A melt pump was installed.
[0152] The throughput was approximately 15 kg / h. The granulator speed was 1500 rpm. The melt temperature was 296 °C. The melt pressure at the tip of the twin-screw extruder was just under 143 bar. The melt pressure upstream of the die plate was 160 bar.
[0153] The foam particles in this comparative example were slightly elongated and had an average particle diameter of 3.5–4 mm. The bulk density of the foam particles was 237 g / l. The average cell diameter and cell structure were not determined. The foam particles had moderate weldability.
[0154] Comparison example 17
[0155] In Comparative Example 17, setup b) with underwater pelletizing (UWG) was used instead of air pelletizing. A melt pump was installed.
[0156] The throughput was approximately 15 kg / h. The pelletizer speed was 1500 rpm. The melt temperature was 300 °C. The melt pressure at the tip of the twin-screw extruder was 225 bar. The melt pressure upstream of the die plate was 193 bar.
[0157] The foam particles in this comparative example were slightly elongated and had an average particle diameter of 3.5–5 mm. The bulk density of the foam particles was 265 g / l. The average cell diameter and cell structure were not determined. The foam particles were difficult to weld.
[0158] Comparison example 18
[0159] In Comparative Example 18, setup b) with UWG (underwater pelletizing) was used instead of air pelletizing. A melt pump was installed. TI
[0160] The throughput was just under 15 kg / h. The granulator speed was 1500 rpm. The melt temperature was 295 °C. The melt pressure at the tip of the twin-screw extruder was 250 bar. The melt pressure upstream of the die plate was 230 bar.
[0161] The foam particles in this comparative example were slightly elongated and had an average particle diameter of 4-5 mm. The bulk density of the foam particles was 280 g / l. The average cell diameter and cell structure were not determined. The foam particles were very difficult to weld.
[0162] Comparison example 19
[0163] Comparative Example 19 was carried out using the same process setup as Inventive Example 1. A melt pump was installed. Water was continuously sprayed onto the area below the perforated plate via the two spray nozzles.
[0164] The throughput was 20 kg / h. The granulator speed was 4000 rpm. The melt temperature was 295 °C. The melt pressure at the tip of the twin-screw extruder was 196 bar. The melt pressure upstream of the die plate was 245 bar.
[0165] The foam particles in this comparative example were round and had an average particle diameter of 4–4.5 mm. The bulk density of the foam particles was 78 g / l. The particles exhibited cell coalescence. The average cell diameter was not determined. The foam particles were difficult to weld.
[0166] Comparison example 20
[0167] In Comparative Example 20, setup b) with underwater pelletizing (UWG) was used instead of air pelletizing. A melt pump was installed.
[0168] The throughput was 30 kg / h. The granulator speed was 1900 rpm. The melt temperature was 300 °C. The melt pressure at the tip of the twin-screw extruder was 260 bar. The melt pressure upstream of the die plate was 116 bar.
[0169] The foam particles in this comparative example were slightly elongated and angular, with an average particle diameter of 4.5–6.3 mm. The bulk density of the foam particles was 186 g / l. The particles exhibited cell coalescence. The average cell diameter was not determined. The foam particles were difficult to weld. Comparative Example 21
[0170] Comparative Example 21 was carried out using the same process setup as Inventive Example 1. A melt pump was installed. Water was continuously sprayed onto the area below the die plate via the two spray nozzles.
[0171] The throughput was 30 kg / h. The granulator speed was 3000 rpm. The melt temperature was 302 °C. The melt pressure at the tip of the twin-screw extruder was 240 bar. The melt pressure upstream of the die plate was 200 bar.
[0172] The foam particles in this comparative example were round and had an average particle diameter of 3.9–4.0 mm. The bulk density of the foam particles was 160 g / l. The particles exhibited cell coalescence. The average cell diameter was not determined. The foam particles were difficult to weld.
[0173] Comparison example 22
[0174] Comparative Example 22 was carried out using the same process setup as Inventive Example 1. A melt pump was installed. Water was continuously sprayed onto the area below the perforated plate via the two spray nozzles.
[0175] The throughput was 30 kg / h. The granulator speed was 3000 rpm. The melt temperature was 300 °C. The melt pressure at the tip of the twin-screw extruder was 230 bar. The melt pressure upstream of the die plate was 170 bar.
[0176] The foam particles in this comparative example were round and had an average particle diameter of 2.2–2.7 mm. The bulk density of the foam particles was 296 g / l. The average cell diameter was 20 μm, and the particles exhibited cell coalescence. The foam particles were very difficult to weld. Table 2: Chain extender and blowing agent contents and obtained test results.
[0177] Ex = Inventive example; Cf. = Comparative example; Not determined = Material was not processable due to the formation of agglomerates, so that no
[0178] Determination was possible.
[0179] Table 3: Contents of chain extender and blowing agent and obtained test results.
[0180] Ex = Inventive example; Cf. = Comparative example; UWG = Underwater granulation; Not determined = Material could not be processed due to the formation of agglomerates, so no determination was possible.
[0181] Table 4: Variation of the blowing agent content and obtained test results
[0182] Ex. = Inventive example; Cf. = Comparative example;
[0183] As Comparative Example 14 shows compared to Example 9, air granulation is advantageous over underwater granulation because lower bulk densities can be achieved with air granulation. This is also evident when considering the two Comparative Examples 19 and 20, which differ only in the type of granulation. When underwater granulation is used, the bulk density is more than twice as high. Comparative Examples 4 and 5 show that sufficient water spraying during air granulation is particularly advantageous for obtaining beads (foam particles) that do not stick together. Furthermore, Comparative Examples 6, 7, 10 and 12 show, in comparison to the examples according to the invention, that a chain extender is necessary to achieve good weldability. Comparative Examples 15 to 18 demonstrate the influence of the amount of chain extender. If the proportion is within the inventive range (cf. 16.), the weldability is best and, at the same time, the bulk density is lowest. Comparative Examples 6, 7, 8, and 9 show that too low a nitrogen content has disadvantages with regard to weldability. Comparative Examples 11 and 13, as well as 21 and 22, however, show that too high a blowing agent content also has a negative impact on weldability and bulk density. The effect of the blowing agent content at a constant proportion of chain extender is shown in Table 4.
[0184] List of reference symbols
[0185] 1 twin-screw extruder
[0186] 2 Inlet for the supply of the polycarbonate formulation
[0187] 3 Injection point for the introduction of the foaming agent 4 Single-screw extruder or melt cooler
[0188] 5 Melt pump
[0189] 6 hole plate
[0190] 7 Cutting chamber
[0191] 8 Cutting device
[0192] 9 Air cooling
[0193] 10 Water spray
[0194] 11 Cyclone
[0195] 12 foam particles
Claims
Patent claims 1. A process for producing foam particles (12) from a polycarbonate formulation containing at least one aromatic polycarbonate, comprising or consisting of the following steps: i) feeding the polycarbonate formulation into an extrusion line and melting and homogenizing the polycarbonate formulation in the extrusion line; ii) introducing a foaming agent into the molten polycarbonate formulation, whereby a foaming agent-containing extrudate is formed; iii) discharging the foaming agent-containing extrudate from the extrusion line to form a foamed extrudate, wherein the foamed extrudate is cooled directly by means of a gaseous cooling medium which comprises or consists of air, and optionally a liquid cooling medium, and comminuted to form foam particles (12); wherein • a chain extender is added to the polycarbonate formulation before step ii) and its content is from 0.20 wt.% to 0.90 wt.%, based on the mass of the polycarbonate formulation; • the foaming agent comprises or consists of N2 and optionally CO2 and the N2 content is from 0.05 wt.% to 0.23 wt.%, the CO2 content is from 0 wt.% to 0.73 wt.% and the total N2 and CO2 content is from 0.15 to 0.96 wt.%, in each case based on the mass of the polycarbonate formulation.
2. Process according to claim 1, characterized in that the aromatic polycarbonate, based on the total weight of the aromatic polycarbonate, has a content of OH end groups of at least 350 ppm, preferably from 350 to 600 ppm, more preferably from 380 to 580 ppm, particularly preferably from 400 to 550 ppm, most particularly preferably from 450 to 550 ppm, determined by means of 'H-NMR spectroscopy with dichloromethane as solvent at room temperature, and / or the polycarbonate- Formulation a melt volume flow rate MVR of up to 12 cm 3 / (10 min), determined according to ISO 1133:2012-3 (test temperature 300°C, mass 1.2 kg).
3. Process according to claim 1 or 2, characterized in that additives, in particular pigments, talc, carbon black or mixtures thereof, are contained in the polycarbonate formulation or are added to the polycarbonate formulation before step ii).
4. Method according to one of the preceding claims, characterized in that the extrusion plant comprises or consists of at least one twin-screw extruder or a co-kneader (1), at least one single-screw extruder or a melt cooler (4), optionally at least one melt pump (5) and / or at least one perforated plate (6).
5. The method according to claim 4, characterized in that the twin-screw extruder or the co-kneader (1), optionally a further melt pump (5), the single-screw extruder or the melt cooler (4), optionally the melt pump (5) and the perforated plate (6) are arranged consecutively downstream, wherein preferably steps i) and ii) take place in the twin-screw extruder or co-kneader (1), the single-screw extruder or melt cooler (4) generates a residence time for the foaming agent-containing extrudate and the melt pump or the melt pumps (5) generate / generate a pressure in order to keep the blowing agent in the foaming agent-containing extrudate and to discharge the foaming agent-containing extrudate through the perforated plate (6) according to step iii).
6. Method according to one of the preceding claims, characterized in that the air used as gaseous cooling medium has a pressure of 40 to 48 m 3 Air is introduced per kilogram of foamed extrudate.
7. Process according to one of the preceding claims, characterized in that the liquid cooling medium comprises or consists of water, glycerol or mixtures thereof, preferably water, wherein the liquid cooling medium is preferably introduced by means of spray nozzles at an amount of 0.06 to 0.26 l of liquid cooling medium per kilogram of foamed extrudate.
8. Method according to one of the preceding claims, characterized in that the comminution in step iii) is carried out by means of a cutting device (8).
9. Process according to one of the preceding claims, characterized in that the content of chain extender is from 0.30 wt.% to 0.70 wt.%, preferably from 0.40 wt.% to 0.70 wt.%, more preferably 0.40 wt.% to 0.50 wt.%, based on the mass of the polycarbonate formulation.
10. Process according to one of the preceding claims, characterized in that the N2 content is from 0.18 wt.% to 0.21 wt.%, the CO2 content is from 0.30 wt.% to 0.43 wt.% and / or the total N2 and CO2 content is from 0.18 wt.% to 0.75 wt.%, in each case based on the mass of the polycarbonate formulation.
11. Process according to one of the preceding claims, characterized in that the chain extender comprises or consists of at least one epoxy-functionalized compound, preferably at least one epoxy-functionalized compound having an epoxy equivalent weight of 285 to 485 g / mol, determined according to DIN EN 1877-1:2000.
12. The method according to any one of the preceding claims, characterized in that the bulk density of the foam particles (12) is 50 to 160 g / l, preferably 50 to 100 g / l, the foam particles have an average particle diameter of 1.0 to 7.0 mm, preferably 2.5 to 5.0 mm and / or the foam particles have an average cell diameter of 100 to 200 pm, in each case determined by means of the methods set out in the description.
13. Foam particles (12) obtained or obtainable by a process according to any one of claims 1 to 12.
14. Use of the foam particles (12) according to claim 13 for the production of lightweight components; automotive components, in particular body components, insulation components and / or soundproofing elements; body-supporting elements, in particular seats, automotive seats and / or bicycle seats; insulating layers; Composite components, in particular sandwich elements; wind turbine components and / or protective helmets, in particular bicycle helmets, construction helmets and / or industrial safety helmets.
15. Use of a chain extender in combination with a foaming agent comprising or consisting of N2 and optionally CO2 in a polycarbonate formulation containing at least one aromatic polycarbonate for producing foam particles (12), in particular with reduced bulk density and improved weldability, wherein the production is preferably carried out by a process according to one of claims 1 to 12, wherein • the N2 content is from 0.05 wt% to 0.23 wt%, the CO2 content is from 0 wt% to 0.73 wt% and the total N2 and CO2 content is from 0.15 to 0.96 wt%, in each case based on the mass of the polycarbonate formulation; and • the chain extender content is from 0.20 to 0.90 wt.%, based on the mass of the polycarbonate formulation.
Citation Information
Patent Citations
Thermoplastic polycarbonate(s) - useful as a source of carbon di:oxide blowing agent for prodn. of thermoplastic polycarbonate foam
DE4100200A1
Manufacturing device and manufacturing method for thermoplastic resin foam particles
WO2021106795A1
Expanded particles and expanded molded article
EP3858906A1
Process and equipment for the production of granules of expandable thermoplastic polymers
WO2003053651A1
Polyester-based expandable beads
WO2012020112A1