Method for producing polycarbonate beads
A continuous process using aromatic polycarbonate with controlled OH end groups and chain extenders addresses the challenge of achieving low-density polycarbonate beads with good mechanical properties, resulting in beads suitable for high-performance molded parts and insulation applications.
Patent Information
- Application Number
- PCT/EP2024/060485
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-19
- Filing Date
- 2024-04-18
- Publication Date
- 2024-10-24
AI Technical Summary
Current processes for producing polycarbonate beads do not achieve low-density foams with good mechanical properties, as they either result in defective cells due to insufficient reaction or excessive reactivity, leading to poor mechanical performance.
A continuous process involving aromatic polycarbonate with a specific content of OH end groups and a chain extender, mixed at a particular molar ratio, is used to create polycarbonate beads with improved mechanical properties by controlling the foaming process at high melt temperatures and pressures.
The process produces polycarbonate beads with bulk densities between 150 to 250 g/L, exhibiting good mechanical properties and intact cell structures, enabling the production of molded parts with enhanced mechanical performance and thermal insulation.
Smart Images

Figure IMGF000005_0001 
Figure IMGF000011_0001 
Figure IMGF000013_0001
Abstract
Description
[0001] Process for producing polycarbonate beads
[0002] The invention relates to a process for producing polycarbonate beads, the polycarbonate beads obtainable by the process, and molded parts obtainable from the polycarbonate beads.
[0003] Particle foams, particularly EPS, EPP, and E-TPU, are becoming increasingly important. Modern technology now allows for the production of reliable quality particle foams and the manufacture of components with advantageous properties from these particle foams. Their lower bulk density compared to "simple" thermoplastics opens up new fields of application for expanded materials, while allowing conventional applications to be realized with significant weight savings. Expanded thermoplastics are therefore an attractive material, particularly for lightweight construction applications, provided their application-specific properties are sufficiently good. Tool developments in recent years have made it possible to produce components with surfaces that exhibit such an appearance that even visible parts made of expanded thermoplastics are a viable alternative to corresponding injection-molded parts, while remaining significantly lighter.Due to the lower material consumption, the expanded materials are also attractive from a sustainability perspective and can also contribute to energy savings due to their generally good thermal insulation properties, for example when used as thermal insulation material or as an additional effect when used as an insulating material for noise suppression.
[0004] Particle foams made of polycarbonate have also been described. Particle foams made of engineering thermoplastics are of interest to the automotive industry, for example, due to properties such as high temperature resistance and good fire behavior. EPC is a particle foam for high-temperature applications where conventional polymer foams such as EPP fail. DE 4100200 A1 describes a process for producing polycarbonate foam from polycarbonate, in which a transesterification catalyst is added to the aromatic polycarbonate in combination with aromatic polycarboxylic acids or water, optionally together with aliphatic hydroxycarboxylic acids and / or aliphatic alcohols. This results in a controlled, partial degradation of the polycarbonate with the release of CO2, which serves to foam the remaining polycarbonate. The polycarbonate foams described in the document have densities of around 0.4 to 0.8 g / cm³ 3 on.
[0005] EP 3858906 A1 describes a process for producing expandable particles from aromatic polycarbonate by extruding aromatic polycarbonate, granulating, impregnating with carbon dioxide as a blowing agent, and expanding the particles, followed by shaping the particles to obtain an expanded molded article. EP 2603549 A1 describes polyester foams and explicitly includes polycarbonate foams in these, which, in addition to low density, exhibit good processability. To produce these particle foams, a starting polymer material is selected in which crystallinity, reflected by the enthalpy of fusion, glass transition temperature, and melting temperature lie within a specific range. The process for producing the particle foams comprises providing appropriate starting polymer components in a molten state, mixing in a blowing agent component, and optionallyof one or more additives into the melt, extrusion, and granulation of the blowing agent-containing melt under water at elevated pressure of 1 to 20 bar. EP 2603549 A1 also describes the basic possibility of adding chain extenders, for example, to stabilize the extrusion process by increasing the molecular weight, although no specific quantity is specified. Nor are any further requirements placed on the polymer used.
[0006] The task was therefore to provide improved low-density polycarbonate beads compared to the state of the art via a continuous process, from which molded parts with better mechanics can be produced.
[0007] Surprisingly, it has now been discovered that molded parts made of polycarbonate particle foams, so-called foamed "polycarbonate beads," with sufficiently good mechanical properties are only accessible if a chain extender in a certain amount is reacted with polycarbonate containing a certain amount of OH end groups. Only then is the process control required for good mechanical properties with reactive particle foam extrusion possible, so that foaming at high melt temperatures T of Ti = (T g + 110°C) to T2 = (T g + 170 °C) (with T gequal to the glass transition temperature of the aromatic polycarbonate-based composition) over the usual temperature range for foam production via extrusion of thermoplastics with physical blowing agents for expansion to low-density foams, and at simultaneously high pressures. According to the prior art, a "particle foam extrusion" is understood by the person skilled in the art to mean a complete or partial extrusion process with the addition of a blowing gas with final granulation and cooling to form expanded particles, in the case of amorphous thermoplastics at melt temperatures of T g + 10 °C to T g + 70 °C with T g = the glass transition temperature of the polymer material.
[0008] The invention therefore relates to a process, in particular a continuous process, for producing polycarbonate beads, comprising the following steps, preferably in this order: a) Providing a composition based on aromatic polycarbonate, wherein the aromatic polycarbonate, based on the total weight of the aromatic polycarbonate, has a content of OH end groups of at least 350 ppm, determined by 'H-NMR spectroscopy with dichloromethane as solvent at room temperature, b) Mixing the aromatic polycarbonate-based composition with a chain extender suitable for OH groups in a molar ratio such that 0.64 to 1.10 mol of the reactive group of the chain extender are used per 1 mol of OH end groups of the polycarbonate, c) Providing the mixture in a plasticized state, d) Mixing a physical blowing agent into the melt,e) Particle foam extrusion of the plasticized mixture at a temperature of the plasticized mixture T of Ti = (T, g + 110°C) to T2 = (T g + 170°C), where T g is the glass transition temperature of the aromatic polycarbonate-based composition, f) granulating the blowing agent-containing melt.
[0009] The final granulation produces foamed polycarbonate beads.
[0010] The content of OH end groups is determined by 'H-NMR spectroscopy with dichloromethane as solvent at room temperature by evaluating the ratio of the integrals of the signals at 6.68 ppm (two aromatic protons ortho to phenolic OH groups) and at 1.68 ppm (six methyl protons of the bisphenol-A unit).
[0011] The glass transition temperature is determined according to DIN EN ISO 11357-1:2017.
[0012] “Providing the mixture in a plasticized state” means that a polymer melt is present.
[0013] Unless expressly stated otherwise, all ppm amounts in the present invention are to be understood as parts by weight.
[0014] There is a minimum value for both the amount of OH end groups and the concentration of chain extender, but also a maximum concentration for foam extrusion at high melt temperatures T of Ti = (T g + 110 °C) to T2 = (T g + 170 °C), preferably T of Ti = (T g + 120 °C) to T2 = (T g + 160 °C), particularly preferably in the range of Ti = (T g + 130 °C) to T2 = (T g+ 150 °C) for particle foam production to obtain a polycarbonate particle foam with good mechanical properties in the bulk density range of 150 to 250 g / L, determined in accordance with DIN EN ISO 60:2000-01. "In accordance with" means that instead of the standardized aluminum container with a known volume, a 1 L beaker was used, and its contents were weighed to determine the density of the material.
[0015] The number of OH groups in the aromatic polycarbonate has a significant influence on whether beads with low density and good mechanical properties can be obtained in the resulting molded parts. Too many OH groups in the polycarbonate result in excessive reactivity of the polycarbonate, which ultimately leads to rearrangement reactions in the polycarbonate chain, a reduction in molecular weight due to excessively rapid branching, with the associated excessively rapid increase in viscosity (excessive shear input), and yellowing. Too few OH groups in the polycarbonate, however, result in insufficient reaction with the chain extender or even no reaction at all. This also means that a good particle foam with sufficient mechanical properties cannot be obtained. Instead, the particle foam will exhibit a large number of defective, collapsed cells.
[0016] According to the invention, the OH end group content of the aromatic polycarbonate used in the process is at least 350 ppm, preferably 350 ppm to 600 ppm, more preferably 380 ppm to 580 ppm, particularly preferably 400 ppm to 550 ppm, very particularly preferably 450 to 550 ppm, based on the total weight of aromatic polycarbonate used. The reference value here is the pure aromatic polycarbonate, not the aromatic polycarbonate-based composition. To achieve such an end group content, preferably more than 70 wt. % SPC, based on the total weight of the aromatic polycarbonate used, is used, more preferably at least 80 wt. % SPC, based on the total weight of the aromatic polycarbonate used, very particularly preferably exclusively SPC is used as the aromatic polycarbonate for the production of the polycarbonate beads.
[0017] The concentration of the chain extender is also crucial. Too much chain extender leads to the material being unprocessable due to the resulting excessive viscosity caused by the excessive molecular weight buildup of the polycarbonate. Too little chain extender results in no significant molecular weight buildup and thus insufficient pressure buildup (the viscosity of PC without / with insufficient CE at 300 °C is too low) and ultimately poorer mechanical properties, with the reaction of the chain extender with the polycarbonate being a function of time and temperature. For example, the foam extrusion process for bisphenol-A-based homopolycarbonate is preferably carried out at a housing temperature of TceMuse of TiHousing = T g + 100 °C to = T g + 150 °C and a melting temperature T of approx.
[0018] T g+ (110 to 170 °C) after blowing agent mixing and dissolution. Particle foam production without cooling results in collapsed particles with high density. Depending on the process, the stabilization and solidification of the foam structure through cooling can lead to foam expansion being suppressed too quickly. The high temperatures in the process make it possible to utilize the full foaming potential of the formulation under cooling by compensating for the excessively rapid cooling / solidification. At these temperature profiles, however, the pressure at the die plate without chain extenders is 80 - 90 bar (despite the melt pump). The use of chain extenders increases the pressure at the die plate to 140 - 180 bar, preferably 150 - 160 bar. Without appropriate chain extension and thus without the additional increase in viscosity, particle foam production is not possible under these process conditions (temperatures).
[0019] In order to obtain polycarbonate beads with good properties, it has been found to be essential to the invention that a molar ratio (in a continuous process, a throughput-related addition takes place) of 1 mol of OH end groups of the polycarbonate to 0.64 - 1.10 mol, preferably 0.71 to 1.0 mol, more preferably up to 0.96 mol, even more preferably 0.8 to 0.9 mol, in particular 0.82 to 0.90 mol of the reactive group of the chain extender is used.
[0020] Preferably, if the content of OH end groups in the aromatic polycarbonate is 400 to 550 ppm, determined by 'H-NMR spectroscopy with dichloromethane as solvent at room temperature, 0.71 to 0.96 mol of the reactive group of the chain extender are used per 1 mol of OH end groups of the polycarbonate.
[0021] The use of a chain extender results in a molecular weight increase of the polycarbonate to a range of 40,000 to 230,000 g / mol, preferably up to 100,000 g / mol, which is associated with an additional pressure build-up on the perforated plate of approximately 60 to 100 bar at the temperatures at which polycarbonate is in its plasticized state.
[0022] In a particularly preferred embodiment according to the invention, the process is carried out continuously and comprises the following steps, preferably in this order: a) Providing a composition based on aromatic polycarbonate, wherein the aromatic polycarbonate, based on the total weight of the aromatic polycarbonate, has a content of OH end groups of at least 350 ppm, preferably from 400 to 550 ppm, determined by 'H-NMR spectroscopy with dichloromethane as solvent at room temperature, b) Mixing the aromatic polycarbonate-based composition with a chain extender suitable for OH groups in an amount such that 0.64 to 1.10 mol, preferably 0.71 to 1.0 mol, more preferably up to 0.96 mol, even more preferably 0.8 to 0.9 mol, in particular 0.82 to 0.90 mol of the reactive group of the chain extender (adjusted based on throughput) is present per 1 mol of OH end groups of the polycarbonate. be used,wherein an epoxy-functionalized chain extender is used, preferably a styrene-acrylic-based polymer comprising epoxy reactive groups, in particular one with an epoxy equivalent weight (EEW) of 285 to 485 g / mol, determined according to DIN EN 1877-1:2000. c) providing the mixture in a plasticized state, d) mixing a physical blowing agent into the melt in a concentration of 0.1 - 2.3 wt.%, based on the polymer melt, wherein the physical blowing agent is nitrogen, carbon dioxide or a mixture of these, preferably carbon dioxide, e) particle foam extrusion of the plasticized mixture at a melting temperature T of Ti = (T, g + 110°C) to T2= (T g + 170°C), preferably at T of Ti = (T g + 120 °C) to T2= (T g + 160 °C), where T gis the glass transition temperature of the aromatic polycarbonate-based composition, f) granulation of the blowing agent-containing melt, preferably as underwater granulation without pressurization.
[0023] The individual steps of the process according to the invention can be carried out using tools and machines known to those skilled in the art and available in plastics technology. Individual steps can also be carried out in combination, if necessary.
[0024] The process for producing polycarbonate beads can be carried out continuously or batchwise. The polymer melt can, for example, be taken directly from the polymerization reactor as freshly polymerized material or fed directly from the reactor into a mixing extruder, where ketene extender, blowing agent, and optionally additives are ultimately fed at various points. The process according to the invention is preferably carried out continuously, because a batchwise process carries the risk of the polycarbonate crystallizing.
[0025] It goes without saying that the specified specifications regarding the ratio of the molar amounts of OH end groups of the polycarbonate and the reactive group of the ketene extender must be adjusted according to the process. In a continuous process, a throughput-related concentration adjustment (mol / h : mol / h ratio) is advantageous.
[0026] The process according to the invention can be a single-stage or two-stage extrusion process in which, in a first extrusion step, the molecular weight of the polymer is increased in the presence of the ketene extender, producing polycarbonate granules as the first product. Foaming then takes place with the physical blowing agent, preferably carbon dioxide, in a second extrusion step. The subsequent underwater granulation ultimately results in the polycarbonate beads according to the invention. At the end of the first extrusion step, granulation can then take place. For this purpose, the melt is extruded through a mold at an outlet opening of the extruder and then cut to length. Cutting to length is performed by a cutting device, which is usually located immediately downstream of the mold through which the material is extruded.The cutting device can be in contact with the mold or positioned at a certain distance from the mold. The subsequent blowing agent addition can also take place in the same extruder, either after a certain residence time of the polycarbonate and chain extender mixture, or simultaneously with the chain extender addition.
[0027] The process according to the invention makes it possible to obtain polycarbonate beads, a particle foam. Due to the material's low weight and impact-resistant properties, combined with higher continuous service temperatures (e.g., resistance to cathodic dip-painting processes) compared to PP, ABS, PE, or PA6, the use of particle-foamed polycarbonate makes it possible to significantly reduce the weight of some vehicle components, as well as lower fuel consumption and CCE emissions, while maintaining mechanical properties even at higher temperatures. Furthermore, the availability of foamed polycarbonate is expected to open up a whole range of additional applications, especially wherever insulation tasks are required at higher temperatures.
[0028] The invention thus also relates to polycarbonate beads produced by the process according to the invention. A "bead" refers to granules (= particle foam) foamed according to the invention, which typically have a maximum density of a maximum of 50% of the unfoamed starting material (the aromatic polycarbonate-based composition). The polycarbonate beads obtainable by the process according to the invention preferably have an average molecular weight, measured here as the absolute molecular weight, of the aromatic polycarbonate of at least 140 kDa (highly branched), particularly preferably at least 150 kDa, determined by GPC-MALLS measurement (multi-angle laser light scattering) according to DIN EN ISO 16014-5:2019-09.The molecular weights and molecular dimensions of the molecules are determined simultaneously, allowing conclusions to be drawn about the degree of branching of the materials, as branching influences the separation mechanism of GPC, which is evident from the rising molecular weight curve. The linear starting material serves as a reference for comparison with the foamed samples. The more branched (smaller hydrodynamic volume at the same molecular weight) the sample is, the further the curve deviates from the ideal line of an unbranched polycarbonate. Polycarbonate material with a corresponding minimum degree of branching can be foamed well, resulting in polycarbonate beads with good morphology, from which molded parts with good mechanical properties can then be produced.
[0029] The particles of expanded polycarbonate, the "polycarbonate beads", produced by the process according to the invention, have the following properties: a bulk density, depending on the continuous process, of 150 g / L to 250 g / L, preferably 180 g / L to 200 g / L, determined in-process via the bulk density in accordance with DIN EN ISO 60: 1999. "In accordance with" here means that instead of the standardized aluminum container with a known volume, a 1 L beaker is used and its contents are weighed to determine the density of the material. a nominal diameter (depending on the process) in the range of 2 to 7 mm, preferably 2.5 to 5 mm, particularly preferably 3 mm ± 0.2 mm, whereby the exact determination of the size distribution is preferably carried out using a Camsizer; the thermal properties (T g of 145-150 °C) and mechanical properties of polycarbonate, e.g. at a component density of 200 kg / m 3of at least a flexural modulus of 70 MPa, a flexural strength of 2.5 MPa (ISO 6603-2:2000); a compressive modulus of 59 MPa and a compressive strength (at 10% compression) of 1.73 MPa (ISO 844-11:2014); a tensile strength of at least 1.97 MPa and an elongation at break of 8 - 14% (ISO 1926:2009); an average equivalent circle diameter of the cells to the circle of equal projection area of a maximum of 150 pm, preferably a maximum of 100 pm, particularly preferably a maximum of 80 pm, determined by SEM (ASTM E1508-12a:2019).
[0030] The size of the beads depends on the process and can be influenced by factors such as the selected nozzle size, throughput, blade speed, and composition of the blowing agent-containing melt. An example process with a nozzle size of 1.2 mm produces beads with a nominal diameter in the range of 1.8 to 3 mm. The maximum frequency distribution is at 2.5 mm with a distribution width of 28% of the mean. A nozzle of 2.2 mm produces a particle size distribution with an average diameter of 5 mm and a distribution width of 40% of the mean.
[0031] The polycarbonate beads are weldable over a wide range, preferably at a steam pressure of 7 bar to 11 bar, particularly preferably 8 bar to 10 bar. They have a high molecular weight M w in the range from 40 000 g / mol up to 230 000 g / mol, determinable by GPC, as described in the examples section.
[0032] The polycarbonate beads show good mechanical properties and low thermal conductivity (DIN EN 12667:2001) in the range of 45 - 47 mW / (m*K) at 10 °C and a component density of 200 ± 10 kg / m 3 .
[0033] The beads have intact ("closed-cell") or at least predominantly intact cells, which is why foam moldings with very uniform, flat surfaces and homogeneous bead bonding can be produced from the polycarbonate beads. "Predominantly" means that preferably > 85% of the cells, more preferably > 90% of the cells in a bead are intact, i.e., in these beads, the individual cell structure is shared by at least three other structural elements (cells), and there are no more than two broken cell walls per individual cell.
[0034] The starting material for the production of the beads according to the invention in the process according to the invention is a composition based on aromatic polycarbonate.
[0035] "Aromatic polycarbonate" in the sense of the invention refers to both aromatic homopolycarbonates and aromatic copolycarbonates. The polycarbonates can be linear or branched in a known manner.
[0036] The polycarbonates contained in the compositions are prepared in a known manner from dihydroxyaryl compounds, carbonic acid derivatives, optionally chain terminators and branching agents.
[0037] Details of the production of polycarbonates have been documented in numerous patents published over the past 40 years. Examples include Schnell, "Chemistry and Physics of Polycarbonates," Polymer Reviews, Volume 9, Interscience Publishers, New York, London, Sydney 1964; D. Freitag, U. Grigo, PR Müller, H. Nouvertne, BAYER AG, "Polycarbonates" in Encyclopedia of Polymer Science and Engineering, Volume 11, Second Edition, 1988, pages 648-718; and finally, U. Grigo, K. Kirchner, and PR Müller, "Polycarbonates" in Becker / Braun, Kunststoff-Handbuch, Volume 3 / 1, Polycarbonates, Polyacetals, Polyesters, Cellulose Esters, Carl Hanser Verlag Munich, Vienna 1992, pages 117 to 299.
[0038] Aromatic polycarbonates are produced, for example, by reacting dihydroxyaryl compounds with carbonic acid halides, preferably phosgene, and / or with aromatic dicarboxylic acid dihalides, preferably benzenedicarboxylic acid dihalides, by the interfacial process, optionally using chain terminators and optionally using trifunctional or more than trifunctional branching agents. Production via a melt polymerization process is also possible by reacting dihydroxyaryl compounds with, for example, diphenyl carbonate. According to the invention, preference is given to using polycarbonate produced by the melt polymerization process, also called the "transesterification process." Polycarbonate used according to the invention has 350 to 600 ppm of OH end groups, whereby this information refers to the polycarbonate as such, to the polymer itself, without any added additives.The amount of OH end groups refers to the total polycarbonate used. A mixture of polycarbonate obtained by melt polymerization and polycarbonate obtained by interfacial polymerization can also be used, as long as the concentration of OH end groups in the polycarbonate used is within the specified range. However, it is particularly preferred to use only polycarbonate produced by melt polymerization.
[0039] Dihydroxyaryl compounds suitable for the production of polycarbonates are, for example, hydroquinone, resorcinol, dihydroxydiphenyls, bis-(hydroxyphenyl)-alkanes, bis-(hydroxyphenyl)-cycloalkanes, bis-(hydroxyphenyl)-sulfides, bis-(hydroxyphenyl)-ethers, bis-(hydroxyphenyl)-ketones, bis-(hydroxyphenyl)-sulfones, bis-(hydroxyphenyl)-sulfoxides, a-a'-bis-(hydroxyphenyl)-diisopropylbenzenes, phthalimidines derived from isatin or phenolphthalein derivatives, as well as their core-alkylated, core-arylated and core-halogenated compounds.
[0040] Preferred dihydroxyaryl compounds are 4,4'-dihydroxydiphenyl, 2,2-bis-(4-hydroxyphenyl)-propane (bisphenol A), 2,4-bis-(4-hydroxyphenyl)-2-methylbutane, 1,1-bis-(4-hydroxyphenyl)-p-diisopropylbenzene, 2,2-bis-(3-methyl-4-hydroxyphenyl)-propane, dimethyl bisphenol A, bis-(3,5-dimethyl-4-hydroxyphenyl)-methane, 2,2-bis-(3,5-dimethyl-4-hydroxyphenyl)-propane, bis-(3,5-dimethyl-4-hydroxyphenyl)-sulfone, 2,4-bis-(3,5-dimethyl-4-hydroxyphenyl)-2-methylbutane, 1,1- Bis-(3,5-dimethyl-4-hydroxyphenyl)-p-diisopropylbenzene and 1, l-Bis-(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, as well as the bisphenols (I) to (III) in which R' is each C1-C4-alkyl, aralkyl or aryl, preferably methyl or phenyl, most preferably methyl.
[0041] Particularly preferred bisphenols are 2,2-bis-(4-hydroxyphenyl)-propane (bisphenol A), 2,2-bis-(3,5-dimethyl-4-hydroxyphenyl)-propane, 1, l-bis-(4-hydroxyphenyl)-cyclohexane, 1, l-bis-(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 4,4'-dihydroxydiphenyl and dimethyl-bisphenol A as well as the bisphenols of the formulas (I), (II) and (III).
[0042] These and other suitable dihydroxyaryl compounds are described, for example, in US 3 028 635 A, US 2 999 825 A, US 3 148 172 A, US 2 991 273 A, US 3 271 367 A, US 4 982 014 A and US 2 999 846 A, in DE 1 570 703 A, DE 2 063 050 A, DE 2 036 052 A, DE 2 211 956 A and DE 3 832 396 A, in FR 1 561 518 A, in the monograph "H. Schnell, Chemistry and Physics of Polycarbonates, Interscience Publishers, New York 1964" and in JP 62039 / 1986 A, JP 62040 / 1986 A and JP 105550 / 1986 A. In the case of homopolycarbonates, only one dihydroxyaryl compound is used; in the case of copolycarbonates, several dihydroxyaryl compounds are used.
[0043] Suitable carbonic acid derivatives include phosgene or diphenyl carbonate.
[0044] Suitable chain terminators that can be used in the production of polycarbonates are monophenols. Examples of suitable monophenols include phenol itself, alkylphenols such as cresols, p-tert-butylphenol, isooctylphenol, cumylphenol, and mixtures thereof.
[0045] Preferred chain terminators are phenols that are mono- or polysubstituted by C1- to C30-alkyl radicals, linear or branched, preferably unsubstituted, or by tert-butyl. Particularly preferred chain terminators are phenol, cumylphenol, and / or p-tert-butylphenol.
[0046] The amount of chain terminator to be used is preferably 0.1 to 5 mol%, based on the moles of dihydroxyaryl compounds used. The chain terminators can be added before, during, or after the reaction with a carbonic acid derivative.
[0047] Suitable branching agents are the tri- or more than trifunctional compounds known in polycarbonate chemistry, in particular those with three or more than three phenolic OH groups.
[0048] Suitable branching agents are, for example, l,3,5-tri-(4-hydroxyphenyl)benzene, l,l,l-tri-(4-hydroxyphenyl)ethane, tri-(4-hydroxyphenyl)phenylmethane, 2,4-bis-(4-hydroxyphenylisopropyl)phenol, 2,6-bis-(2-hydroxy-5'-methyl-benzyl)-4-methylphenol, 2-(4-hydroxyphenyl)-2-(2,4-dihydroxyphenyl)propane, tetra-(4-hydroxyphenyl)methane, tetra-(4-(4-hydroxyphenylisopropyl)phenoxy)methane and l,4-bis-((4',4"-dihydroxytriphenyl)methyl)benzene and 3,3-bis-(3-methyl-4-hydroxyphenyl)-2-oxo-2,3-dihydroindole.
[0049] The amount of branching agents to be used optionally is preferably 0.05 mol% to 2.00 mol%, based on moles of dihydroxyaryl compounds used.
[0050] The branching agents can either be added together with the dihydroxyaryl compounds and the chain terminators in the aqueous alkaline phase or dissolved in an organic solvent before phosgenation. In the case of the transesterification process, the branching agents are used together with the dihydroxyaryl compounds.
[0051] Particularly preferred polycarbonates are the homopolycarbonate based on bisphenol A, the copolycarbonates based on l,l-bis-(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane and 4,4'-dihydroxydiphenyl as well as the copolycarbonates based on the two monomers bisphenol A and l,l-bis-(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, as well as the dihydroxyaryl compounds of the formulas (I), (II) and (III) in which R' is each C1- to C2-alkyl, aralkyl or aryl, preferably methyl or phenyl, very particularly preferably methyl, derived homo- or copolycarbonates, in particular with bisphenol A. Very particularly preferably, the polycarbonate-based compositions contain bisphenol A-based polycarbonate, most preferably the polycarbonate in the polycarbonate-based compositions is bisphenol A-based homopolycarbonate.
[0052] Also preferred are copolycarbonates for the preparation of which diphenols of the general formula (la) were used:
[0053] (la), where
[0054] R 5 represents hydrogen or C1- to C4-alkyl, C1- to C5-alkoxy, preferably hydrogen;
[0055] methoxy or methyl,
[0056] R 6 , R 7 , R 8 and R 9each independently represents Ci- to C-alkyl or Ce- to Cn-aryl, preferably methyl or phenyl,
[0057] Y represents a single bond, SO2-, -S-, -CO-, -O-, C1- to C6-alkylene, C2- to C5-alkylidene, C1- to C12-arylene, which may optionally be condensed with further aromatic rings containing heteroatoms or represents a C5- to C6-cycloalkylidene radical which may be mono- or polysubstituted by C1- to C4-alkyl, preferably a single bond, -O-, isopropylidene or represents a C5- to C6-cycloalkylidene radical which may be mono- or polysubstituted by C1- to C4-alkyl, V represents oxygen, C2- to C6-alkylene or C3- to C6-alkylidene. preferably represents oxygen or Cs-alkylene, p, q and r each independently represent 0 or 1 when q = 0, W represents a single bond when q = 1 and r = 0, W represents oxygen, C2- to C (, -alkylene or C3- to C6-alkylidene, preferably oxygen or Cs-alkylene, when q = 1 and r = 1, W and V each independently represent C2- to C6-alkylene or C3- to C6-alkylidene, preferably C3-alkylene,
[0058] Z represents a C1- to C12-alkylene, preferably C5-alkylene, o represents an average number of repeating units from 10 to 500, preferably 10 to 100, and m represents an average number of repeating units from 1 to 10, preferably 1 to 6, more preferably 1.5 to 5. It is also possible to use diphenols in which two or more siloxane blocks of the general formula (Ia) are linked to one another via terephthalic acid and / or isophthalic acid to form ester groups.
[0059] Particularly preferred are (poly)siloxanes of the formulas (2) and (3) where RI is hydrogen, Ci- to C4-alkyl, preferably hydrogen or methyl and particularly preferably hydrogen,
[0060] R2 independently represent aryl or alkyl, preferably methyl,
[0061] X represents a single bond, -SO2-, -CO-, -O-, -S-, C1- to C12-alkylene, C2- to C5-alkylidene or C1- to C18-arylene, which may optionally be condensed with further aromatic rings containing heteroatoms, X preferably represents a single bond, C1- to C5-alkylene, C2- to C5-alkylidene, C5- to C12-cycloalkylidene, -O-, -SO-, -CO-, -S-, -SO2-, particularly preferably X represents a single bond, isopropylidene, C5- to C12-cycloalkylidene or oxygen, and very particularly preferably isopropylidene, n represents an average number from 10 to 400, preferably 10 and 100, particularly preferably 15 to 50 and m represents an average number from 1 to 10, preferably from 1 to 6 and particularly preferably from 1.5 to 5 stands.
[0062] Likewise preferably, the siloxane block can be derived from the following structure where a in formula (IV), (V) and (VI) represents an average number from 10 to 400, preferably 10 to 100 and particularly preferably 15 to 50.
[0063] It is also preferred that at least two identical or different siloxane blocks of the general formulas (IV), (V) or (VI) are linked to one another via terephthalic acid and / or isophthalic acid to form ester groups. It is also preferred if, in formula (Ia), p = 0, V is Cs-alkylene, r = 1, Z is Cs-alkylene, R 8 and R 9 represents methyl, q = 1, W represents Cs-alkylene, m = 1, R 5 represents hydrogen or Ci- to C4-alkyl, preferably hydrogen or methyl, R 6 and R 7 each independently represents Ci- to C-alkyl, preferably methyl, and o represents 10 to 500.
[0064] Copolycarbonates with monomer units of formula (Ia) and in particular their preparation are described in WO 2015 / 052106 A2.
[0065] Copolycarbonates with monomer units of formula (IV) and in particular their preparation are described in WO 2015 / 052106 A2.
[0066] The aromatic polycarbonate used in the process according to the invention can be a single polycarbonate or a mixture of two or more aromatic polycarbonates, as long as the content of OH end groups of the total polycarbonate used is within the range according to the invention. Polycarbonate that is a post-consumer or post-industrial recyclate can also be used. Such recyclates can be fed to the extruder as granules or ground material. It is also possible to use recyclate only as part of the aromatic polycarbonate.
[0067] In principle, one or more additives can be added to the aromatic polycarbonate, specifically to the polycarbonate as it is used as the starting material in the process according to the invention. However, one or more additives can also be added to the aromatic polycarbonate in the extruder during the process according to the invention, preferably together with the chain extender. Mixing via the side extruder is not possible in the process according to the invention if only one extrusion stage is used, since the blowing agent is present in the melt and would therefore escape via the side feed. However, a gas-tight side feed would allow the additives to be introduced in this way. Additives can also be introduced using powder premixes or as a masterbatch.Liquid additives can generally be injected at any point in the process, as long as sufficient homogenization can still be achieved, preferably in the area of static or dynamic mixing units. Additives can also be added in a first stage, followed by the blowing agent in a second stage. Here, the additives can also be metered via a side extruder.
[0068] The mixture of aromatic polycarbonate, optional blend partner, and optional additives as starting material is referred to as an "aromatic polycarbonate-based composition." The use of an "aromatic polycarbonate-based composition" in process step a is therefore to be understood as the use of the pure polymer, but also as the use of additized aromatic polycarbonate. If an additized polycarbonate composition is used, it preferably contains at least 70 wt. %, more preferably at least 80 wt. %, even more preferably at least 90 wt. %, particularly preferably at least 95 wt. %, most preferably at least 98 wt. % aromatic polycarbonate, based on the total weight of the polycarbonate composition.Most preferably, the “aromatic polycarbonate-based composition” does not contain any blend partners to the polycarbonate, but in the process according to the invention for producing polycarbonate beads, only aromatic polycarbonate is used, apart from any additives customary for polycarbonate.
[0069] Such further additives, as are usually added to polycarbonates, are in particular thermal stabilizers, flame retardants, antioxidants, mold release agents, anti-drip agents, such as polytetrafluoroethylene (Teflon) or SAN-encapsulated PTFE (e.g. Blendex 449), UV absorbers, IR absorbers, impact modifiers, antistatic agents, optical brighteners, fillers such as talc, light scattering agents, transesterification inhibitors, compatibilizers, nucleating agents, colorants, pigments, e.g. titanium dioxide, carbon black, chemical blowing agents and / or additives for laser marking, in particular in the amounts customary for polycarbonate-based compositions. Such additives are described, for example, in EP-A 0 839 623, WO-A 96 / 15102, EP-A 0 500 496, or in the "Plastics Additives Handbook," Hans Zweifel, 5th Edition 2000, Hanser Verlag, Munich. These additives can be added individually or in mixtures.It is understood that only such additives and only in such quantities may be added if they do not have a significantly negative effect on the production of the beads according to the process according to the invention.
[0070] The additives are preferably selected from the group of thermal stabilizers, flame retardants, antioxidants, mold release agents, colorants, pigments, anti-drip agents, UV absorbers, IR absorbers, nucleating agents, impact modifiers, antistatic agents, optical brighteners, light scattering agents, transesterification inhibitors, compatibilizers and / or additives for laser marking.
[0071] The aromatic polycarbonate-based composition preferably has a melt volume flow rate MVR of up to 14 cm 3 / (10 min), more preferably up to 12 cm 3 / (10 min), especially preferably 5 cm 3 / (10 min) to 9 cm 3 / (10 min), especially preferably 5.5 cm 3 / (10 min) to 6.5 cm 3 / (10 min), determined according to ISO 1133:2012-3 (test temperature 300°C, mass 1.2 kg).
[0072] As part of the process according to the invention, sufficient chain extender is added to the aromatic polycarbonate used so that the molar ratio of the OH end groups of the polycarbonate is 1 to 0.64 to 1.1, preferably to 0.71 to 1.0, more preferably to 0.96, even more preferably 0.8 to 0.9, in particular 0.82 to 0.90 of the reactive groups of the chain extender. The amount of substance is preferably adjusted based on the throughput per hour. This results in polymer buildup, and the molecular weight of the aromatic polycarbonate is increased through the formation of long-chain branches.
[0073] Suitable chain extenders are generally amines, carboxyl compounds, maleic anhydride-modified compounds, epoxy-functionalized compounds, oxazolines, carbodiimides, and / or functionalized polymers, for example based on acrylate and / or styrene, which have the corresponding functional group. Such compounds can be used alone or in a mixture. Such groups include, for example, amine functions in the amines, carboxyl functions in the carboxyl compounds, anhydride functions in maleic anhydride-modified compounds, epoxy functions in epoxy-functionalized compounds, or other functions that can react with the OH end groups of the polycarbonate to form a chain. Epoxy-functionalized compounds are particularly preferred as chain extenders, most preferably epoxy-functionalized styrene-acrylic-based polymers, which are available, for example, from BASF SE as Joncryl additives.Joncryl ADR 4368, ADR 4400, ADR 4468 are offered. The amount / weight of chain extender must be adapted to the aromatic polycarbonate, so that 0.64 to 1.10 mol, preferably 0.71 to 1.0 mol, more preferably up to 0.96 mol, even more preferably 0.8 to 0.9 mol, in particular 0.82 to 0.90 mol of the reactive group of the chain extender is used per 1 mol of OH end groups of the polycarbonate. Starting, for example, from an aromatic polycarbonate with 350 - 600 ppm OH end groups, reacted with a chain extender with an epoxy equivalent weight of 310 g / mol, e.g. with Joncryl ADR 4468, in concentrations of 0.4 - 1.2 wt.%, preferably 0.5 - 1.0 wt.%, particularly preferably in concentrations of 0.7 - 0.9 wt.%, wherein the amount of chain extender is based on the resulting total composition (composition based on aromatic polycarbonate, ie including any blend partner and anyBy specifically adjusting the molar ratio from 1 mol to 0.64 to 1.10 mol, molecular weight ranges of 40,000 to 230,000 g / mol, preferably 50,000 to 150,000 g / mol, and particularly preferably 75,000 to 100,000 g / mol, determined as described, can be achieved. The broad processing window enables the production of components from particles with molecular weights between 40,000 and 230,000 g / mol with different properties.
[0074] The following configurations can be used to carry out reactive particle foam extrusion, but are not limited to them: a) Polymerization reactor / (static) extruder / mixer / gas dosing / melt pump / granulation b) Extruder (twin / single screw) / gas dosing / granulator c) Extruder (twin / single screw) / gas dosing / static mixer / granulator d) Extruder (twin / single screw) / gas dosing / heat exchanger / granulator e) Extruder (twin / single screw) / gas dosing / static mixer / heat exchanger / granulator f) Twin-screw extruder / gas dosing / single-screw extruder / granulator g) Twin-screw extruder / gas dosing / heat exchanger / granulator h) Twin-screw extruder / gas dosing / single-screw extruder / melt pump / granulator i) Twin-screw extruder / Gas dosing / heat exchanger / melt pump / granulator.
[0075] The extrusion process can be carried out in one or two stages.
[0076] In detail, the process can be implemented in various configurations. Key process steps include: melting the aromatic polycarbonate-based composition, optionally adding nucleating agents (talc, especially nano-talc, graphite, carbon black, pigments, etc.), dosing of the blowing agent via liquid dosing devices (e.g., from Lewa GmbH in Germany) or compression units (high-pressure units) (e.g., from Frima Maximator GmbH in Germany), optionally building up pressure up to the die plate via, for example, cooling, adding reactive macromonomers, or using technical aids such as breaker plates or melt pumps (preferably, pressure buildup is achieved by adding reactive macromonomers or using technical aids), and finally, cutting off the granules / beads via granulation in a liquid medium, hot cutting off, or sub-gas granulation, whereby gas mixtures can also be used.It should be noted that not only water can be used as the liquid medium, but also an alternative medium such as glycerin or glycerol.
[0077] A tandem configuration consisting of a twin-screw and a single-screw extruder is particularly preferred for carrying out the process according to the invention. The twin-screw extruder is more preferably used for plasticizing the aromatic polycarbonate-based composition and for mixing in the physical blowing agent and the chain extender, while the single-screw extruder is subsequently used for melt tempering. The molecular weight buildup already takes place in the twin-screw extruder / first extruder and continues until the extrusion exits the die (end of the extrusion line).
[0078] The physical blowing agent is particularly preferably added to the melt containing the aromatic polycarbonate and the chain extender that reacts during the entire process in the last third of the first extrusion unit (depending on the design). Mixing is preferably carried out such that the polymer melt ultimately contains the blowing agent in homogeneous distribution, wherein the proportion of physical blowing agent in the mixture is preferably 1.0 to 2.3 wt.% for CO2, more preferably 1.2 to 1.7 wt.%, particularly preferably 1.3-1.5 wt.% for N2, preferably 0.1 to 0.5 wt.%, more preferably 0.1 to 0.3 wt.%, particularly preferably 0.15 to 0.25 wt.%, and very particularly preferably 0.15 to 0.2 wt.%, based on the total weight of polymer melt (= polycarbonate-based composition) with chain extender. It should be noted that the method according to the invention does not require that step d be carried out after step b.It is also possible that the mixing of the physical blowing agent into the melt begins at the same time as or overlaps with the addition of the chain extender.
[0079] To initiate foam cell formation for a finer and more homogeneous cell morphology, nucleating agents such as talc, in particular nano-talc, graphite, carbon black, pigments and etc. are preferably added in low concentrations of 0.1 to 1.0 wt.%, more preferably 0.15 to 0.5 wt.%, particularly preferably in concentrations of 0.2 to 0.3 wt.%, wherein the amounts refer to the resulting total composition of polycarbonate-based composition and chain extender.
[0080] In principle, any blowing agent commonly used for foaming thermoplastics can be used as a physical blowing agent. Examples include propane, butane, n-pentane, isopentane, as well as similar aliphatic hydrocarbons, aromatic hydrocarbons, alicyclic hydrocarbons, aliphatic alcohols, carbon dioxide, nitrogen, air, inert gases such as argon or helium, and others. Combinations of two or more of these blowing agents can also be used as a physical blowing agent. Carbon dioxide, one or more inert gases, nitrogen, air, or mixtures thereof are preferably used as physical blowing agents, as these are not only toxicologically and ecologically safe, but also do not promote combustion. Nitrogen, carbon dioxide, or a mixture of these is particularly preferred, with carbon dioxide being the most preferred.
[0081] If nitrogen is used as a physical blowing agent, preferably 0.1 to 0.5 wt.%, more preferably 0.1 to 0.3 wt.%, particularly preferably 0.15 to 0.25 wt.% and very particularly preferably 0.15 to 0.2 wt.% nitrogen is used, based on the polymer melt including chain extender and additives (ie polycarbonate-based composition plus chain extender).
[0082] If carbon dioxide is used as a physical blowing agent, preferably 1.0 to 2.3 wt.%, more preferably 1.2 to 1.7 wt.%, particularly preferably 1.3 - 1.5 wt.% carbon dioxide, based on the polymer melt including chain extenders and additives, are used.
[0083] During the manufacturing process, shown here using the example of a tandem system (setup h), various physical blowing agents can be introduced into the polymer melt at various points, for example by liquid dosing or high-pressure dosing. Physical blowing gases are preferably added to the first extruder, but in the last third of the extruder for the best possible homogenization. Dosing at the end of the tandem system would also enable particles to be produced, but the process would be less stable and the resulting particles would be inhomogeneous. Carbon dioxide is the most preferred blowing agent because, compared to other blowing agents used in the production of expanded thermoplastics, it has the advantage of being non-flammable and is also more cost-effective than inert gases and nitrogen.Furthermore, it can be converted relatively easily into the supercritical state (T > 31.0 °C and p > 73.8 bar), which promotes miscibility and dissolution in polycarbonate due to its low compressibility and rapid diffusivity. When carbon dioxide is used as a blowing agent in the manufacturing process according to the invention, the polycarbonate beads according to the invention can therefore also be used without concern for components used in applications that involve a certain fire hazard or that must not outgas (interior). In particular, applications in the field of e-mobility are therefore also conceivable, for example as body components, e.g., for composite parts. In particular, soundproofing elements integrated into the floor area of the vehicle or insulating layers in the body are possible applications.
[0084] The melt pressure must be selected so that it is above the critical solution pressure of the physical blowing agent.
[0085] The extrusion of the melt at the outlet of the extruder through a nozzle plate takes place after blowing agent mixing and dissolution, usually with a melt temperature T of Ti = (T g + 110 °C) to T2= (T g + 170 °C), preferably Ti = (T g + 120 °C) to T2 = (Tg + 160 °C), particularly preferably in the range of Ti = (T g + 130 °C) to T2= (T g + 150 °C). The temperature of the nozzle plate is also preferably kept at a temperature of T g + (130 to 150 °C) to prevent freezing of the nozzle due to cooling polymer melt and thus ensure flowing polymer granulation, as well as to achieve appropriate foam expansion with the highest possible expansion potential.
[0086] The diameter of the nozzle opening for a single-hole nozzle is preferably in the range of 0.8 to 2.2 mm, more preferably 1.0 to 1.5 mm. For multi-hole nozzles, nozzle diameters of 0.4 to 0.8 mm are preferred, particularly preferably 0.6 mm.
[0087] The granulation of the melt at the end of the process according to the invention is preferably carried out by underwater granulation and more preferably without additional pressurization, i.e., at atmospheric pressure. Granulation at atmospheric pressure allows the desired low densities of the polycarbonate beads to be achieved. As the melt exits the nozzle, the polycarbonate material experiences a pressure drop from 140 to 180 bar, preferably from 150 to 160 bar, to atmospheric pressure of approximately 1 bar, at which point the material begins to foam. The physical blowing agent, for example, carbon dioxide, inflates the polycarbonate material, while the gas diffuses out of the polymer melt. After a certain time, complete or almost complete gas exchange has taken place, so that only the normal air composition can be found in the then granulated, expanded polycarbonate, the polycarbonate beads.
[0088] The invention also relates to a process for producing molded parts from the polycarbonate beads produced by the process according to the invention, and to such molded parts.
[0089] The polycarbonate beads can be transferred into molded parts, even those with complex geometries, by filling appropriate cavities, ultimately requiring only one corresponding process step. The subsequent cutting and associated waste, often required with extrusion foams, is eliminated. Polycarbonate beads are also easier to transport than the often bulky sheets of available extrusion foams.
[0090] Corresponding molded parts according to the invention can be used in the automotive industry, transportation, construction, aviation, aerospace, packaging, and generally in lightweight and / or composite construction. Possible molded parts made from the polycarbonate beads include not only sheets but also complex, three-dimensionally shaped parts.
[0091] Molded parts consisting of or comprising the polycarbonate beads according to the invention are in particular visible parts in various fields of application, wherein finishing with laser textures is also possible, such as dashboards or interior trim elements, soundproofing elements, foamed elements, e.g. in carpets in the footwell of cars, a core material or load-bearing foam part of composite materials, for example for body insulation for vehicles, in particular electric vehicles, in the HVAC (heating, air conditioning, ventilation) sector as insulating material, as high-temperature insulation in industry, home and building technology or in the transport sector, insulating materials, packaging, lightweight construction elements, rotor blades of wind turbines, facade components.
[0092] In general, molded parts made of polymer foams are primarily subjected to compression. Another relevant type of loading for polymer foams is bending. Here, the component is subjected to a complex load by subjecting the upper side to a compressive load and the underside to a tensile load. Compression tests provide information about the application-relevant mechanical performance, while tensile and bending tests provide information about the welding quality. The components made from the polycarbonate beads obtained by the process according to the invention can exhibit a thermo-mechanical (T g of 145 - 150 °C) profile of polycarbonate, e.g. with a component density of 200 kg / m 3 of a flexural modulus of 59.1 ± 11.4 MPa, a flexural strength of
[0093] 2.2 ± 0.3MPa (at 23°C, ISO 1209-1:2007, modified geometry to 120 x 25 x 10 mm 3); compression modulus of 54.7 ± 5 MPa and a compressive strength (at 10% compression) of 1.61 ± 0.12 MPa (at 23°C, DIN EN ISO 844-11:2014); a tensile strength of at least 1.97 MPa and an elongation at break of 8.4% (DIN EN ISO 1926:2009) with simultaneous good insulation effect of
[0094] 45.2 ± 2 mW / (m K) at 10°C (EN ISO 8301-8: 1991). The commercially available particle foam EPP has a density of 200 kg / m 3 approximately a flexural modulus of 56.1 ± 10.8 MPa, a flexural strength of 1.85 ± 0.25 MPa, a compressive modulus of 48.4 ± 3.6 MPa, and a compressive strength (at 10% compression) of 1.51 ± 0.5 MPa. In addition, EPP has a tensile strength of 2.49 MPa and an elongation at break of 20.2%, while simultaneously exhibiting an insulation effect of 54 ± 0.2 mW / (m*K) (10 °C). These values are determined as described above for the EPC, a noticeably lower performance.
[0095] However, due to the sometimes quite large polycarbonate beads with average diameters equivalent to a projection-equivalent circle (i.e., nominal diameters) of approximately 4 to 6 mm, it is necessary to overfill the cavity in the mold by 10–20% volume-related. The vapor-based welding process for particle foams follows the same mechanism for all particles and is described in detail in the literature, for example, in Raps et al. 2015; DOI: 10.1016 / j.polymer.2014.10.078.
[0096] To produce molded parts / components, foam particles are welded together in an automatic steam molding machine or variothermally (thermally by heating). In automatic steam molding, the particle surface is melted or softened using high-pressure steam (i.e. steam at a high temperature), which leads to interdiffusion of polymer chains between different beads and resulting cohesion of the beads. Good cohesion between the particles and a low proportion of macropores / interstitial spaces, i.e. voids between particles in the component due to poor packing, are necessary to ensure favorable mechanical properties. The processing of foam beads into the finished part takes place in an automatic molding machine in five steps: 1) Complete or partial closing of the mold, 2) Filling the mold with, if necessary,Subsequently, complete closure, 3) welding of the particles, 4) cooling and stabilization, 5) ejection of the molded part. Two processes are distinguished: the crack-gap method and the pressure-fill method. With the pressure-fill method, the mold is first closed, then the particles are drawn from a container using air pressure and blown into the mold by an injector at approximately 3 bar, where they are compressed. The particles relax in the mold and fill the cavities more effectively (corresponding to an overfill of approximately 10% with the crack-gap method). With the crack-gap method, the mold is not completely closed, but a certain gap (%) remains open. Then, the filling with particles takes place so that the mold is overfilled by a certain percentage (10-20% by volume with EPC). The mold is then closed, and the particles are compressed to the target thickness.For a target component thickness of, for example, 20 mm, the mold cavity is opened by 4 mm for filling (= 20 vol%), filled with the polycarbonate beads and then the mold is retracted to a component thickness of 20 mm. This step is crucial to achieve a homogeneous distribution of the beads in the mold. In the third step, the beads are fused together using hot steam that flows through the mold according to a fixed sequence. During vapor deposition, the beads form physical bonds due to the interdiffusion of polymer chains of neighboring particles. To ensure high welding quality between the particles, 7 to 11 bar, particularly 8 to 10 bar, are preferred for EPC. In the steam-based welding process, the air between the beads is first flushed out and the mold is preheated. Steam flows in parallel to the mold with the valves open.In the second step, the steam flows through the mold, a process known as cross-steaming. During this step, the opposing steam inlet and outlet valves are open. To ensure the most homogeneous temperature distribution and consistent weld quality across the entire part, the tool is preferably steamed from both sides. Finally, with the outlet valves closed, steam is fed into the steam chamber at a specific pressure to improve the surface quality by forming a skin (autoclave steaming). In the fourth step, the molded part is cooled, which is crucial for dimensional accuracy. If the part is ejected without cooling, further expansion of the particles is possible, leading to a deviation from the original dimension. To cool it, the mold is sprayed with water until a temperature of approximately 80°C is reached.After forming and cooling, the part is finally ejected in the final step, preferably by compressed air and mechanical ejectors.
[0097] The invention is illustrated by the following figures.
[0098] They show:
[0099] Fig. 1: Flow diagram of the process according to the invention for producing polycarbonate beads.
[0100] Fig. 2a: SEM image of the foam morphology of a polycarbonate bead obtainable by the process according to the invention (molar reactive group ratio OH:epoxy of 1 mol:0.82 mol for a PC 1 component with an OH end group content of 470 ppm (El)). The OH end group content, based on the total weight of the aromatic polycarbonate used, was 470 ppm.
[0101] Fig. 2b: SEM image of the foam morphology of another polycarbonate bead obtainable by the process according to the invention (molar reactive group ratio OH:epoxy of 1 mol:0.90 mol (based on the throughput per hour) for a PC 1 component with an OH end group content of 470 ppm (E2)). The OH end group content, based on the total weight of the aromatic polycarbonate used, was 429 ppm.
[0102] Fig. 2c: SEM image of the foam morphology of a non-inventive polycarbonate bead (molar reactive group ratio OH:epoxy of 1 mol:1.12 mol (based on the throughput per hour) for a PC 1 component with an OH end group content of 470 ppm (V4)). The OH end group content, based on the total weight of the aromatic polycarbonate used, was 346 ppm.
[0103] Fig. 2d: SEM image of the foam morphology of another non-inventive polycarbonate bead (molar reactive group ratio OH:epoxy of 1 mol:1.47 mol (based on the throughput per hour) for a PC 1 component with an OH end group content of 470 ppm (V6)). The OH end group content, based on the total weight of the aromatic polycarbonate used, was 264 ppm.
[0104] The system shown in Figure 1 for carrying out the process according to the invention is a tandem design. It consists of a co-rotating twin-screw extruder (A). The screws are optimized for the foaming process (e.g., two left-handed elements for gas tightness towards the feed). In the exemplary representation, the twin-screw extruder has 10 heated zones with corresponding temperature control and pressure sensing, with the gas metering in this example taking place at position 1.6. After homogenization of the melt, it is forced into the single-screw (C) via the bypass (B). The single-screw extruder here has 4 heatable zones with corresponding temperature control and pressure sensors. The gas-melt mixture is primarily conveyed to the melt pump and maintained at the same temperature throughout this process.The downstream melt pump (D) is responsible for generating backpressure into the upstream system (improving gas solubility) and controlling the pressure in front of the die plate. The homogenized melt is forced through the die plate, foams, and is separated by a rotating knife and transported away from the water circuit (E) (dried and separated).
[0105] Figures 2a to 2d show SEM images of the morphologies of various polycarbonate beads produced according to the process steps of the inventive method, but with different molar ratios of OH end groups of the polycarbonate to epoxy groups of the chain extender ("OH to epoxy"). While aromatic polycarbonate was used in the production of the beads from Figures 2a and 2b, in which the molar ratio OH:epoxy is within the inventive range, this does not apply to the materials from Figures 2c and 2d. Here, the molar ratio OH:epoxy of the formulation used was 1:1.12 and 1.47, respectively. The partially destroyed cell morphology and cell coalescence are clearly visible in these comparison beads. The resulting material cannot be processed into molded parts with good mechanical properties.However, the polycarbonate beads according to the invention, produced by the process according to the invention, have largely intact foam cells, with the quality of the foam structure being significantly improved in the particularly preferred range of the reactive group equivalents of the formulation.
[0106] Examples
[0107] 1. Description of raw materials and test methods a) Raw materials
[0108] Polymers:
[0109] PCI: An aromatic polycarbonate based on bisphenol A with an MVR of 6 cm 3 / (10 min) (300°C / l.2 kg, ISO 1133-1:2011) and a softening temperature (VST / B 120; ISO 306:2013) of 149°C. T g , determined according to DIN EN ISO 11357-1:2017: 148°C. M w, determined as described below, approximately 30,900 g / mol at 28 kDa (MALLS). Contains 0.06% thermal stabilizer and 0.1% UV stabilizer. OH end group content, determined by 'H NMR spectroscopy with dichloromethane as solvent at room temperature (as described above): 470 ppm. Produced by the melt condensation process (SPC).
[0110] PC2: An aromatic polycarbonate based on bisphenol A with an MVR of 6 cm 3 / (10 min) (300°C / l.2 kg, ISO 1133-1:2011) and a softening temperature (VST / B 120; ISO 306:2013) of 150°C. T g , determined according to DIN EN ISO 11357-1:2017: 148°C. M w , determined as described below, approximately 30,900 g / mol at 28 kDa (MALLS). OH end group content, determined by 'H NMR spectroscopy with dichloromethane as solvent at room temperature (as described above): 60 ppm.
[0111] Manufactured using the interfacial condensation (LPC) process.
[0112] Chain extender 1: A commercially available and multifunctional chain extender from BASF SE (Joncryl ADR 4468) based on epoxy-reactive group-containing styrene-acrylic polymer with a medium molecular weight (gel permeation chromatography in ortho-dichlorobenzene at 150 °C with polystyrene calibration) M w = 7,250 g / mol, an epoxy equivalent weight of 310 g / mol, determined according to DIN EN 1877-1:2000-12, a glass transition temperature T g of 59 °C and a decomposition temperature of 350 °C, determined according to DIN EN ISO 11357-1:2017. b) Carrying out the procedure for the examples
[0113] The process according to the invention can, in principle, be carried out using various machine setups, as previously described. The experiments described below were carried out using setups i), ii), iii) twin-screw extruder with gas dosing, single-screw extruder with melt pump and underwater pelletizer, also shown in Figure 1.Example i) describes a successful particle production within the scope of the claim, example ii) describes a failed particle production due to exceeding the maximum chain extender concentration, example iii) describes a failed particle production due to the absence of the reactive component, example iv) describes a series of tests with the same setup and process parameters as in i) but with successive reduction of the OH concentration of the melt (ppm) PCs at constant reactive component and example v) describes a successful particle production using an alternative setup twin-screw extruder - static mixer / heat exchanger - melt pump - underwater granulation. i) A twin screw extruder from Reifenhäuser (Troisdorf, Germany) with 43 D was operated at a throughput of 35 kg / h, at profile temperatures of 100 - 160 °C (positions 1 to 3), 240 °C (position 4) to 280 °C (positions 5 - 10) and a speed of 100 rpm.Chain extender 1 was also added to the PCI melt at a low concentration of 0.7 wt.%. This corresponds to a molar ratio of OH to epoxy of 1:0.82 (mol / mol). The melt temperature was 10–20 °C higher than the barrel temperature. The blowing agent was added via a Maximator (Maximator GmbH, Germany) and / or a dosing station (Lewa GmbH, Germany) at position 6 with a CO2 content of 1.2 to 1.5 wt.%. The pressure profiles in the twin screw increased successively from position 5 onwards from 45 bar to the extruder tip at 310 bar. The melt was conveyed via the transfer pipe (290 °C) into the single screw (Reifenhäuser). The extruder was also operated at a continuous barrel temperature of 280 °C, a throughput of 35 kg / h, and a speed of 26 rpm. The melt pressure gradually decreased via the screw to the melt pump (from 250 to 120 bar).The melt pump was operated under pressure control at a back pressure of 110 bar and a temperature of 280 °C. The pressure downstream of the melt pump during this process was in the range of 160–180 bar (pressure at the die plate). The start-up switch and die plate were also set to a temperature of 280 °C, and the melt temperature was (T). g + 140 °C) to (T g + 150 °C). The UWG (EUP 50) and the perforated plate were manufactured by ECON (Econ GmbH, Austria). The perforated plate consisted of five individual hole inserts with a diameter of 2.2 mm and a stirrup length of 3.49 mm. The residence time of the melt between inlet and outlet was approximately 7-10 minutes. After the outlet, the melt was separated with a rotating 6-blade knife at 1500 rpm and conveyed by a 70-80 °C cold water circuit (28 m 3 / h). The resulting particles were round with a bulk density of 150 - 180 g / L and could be easily welded in the range of 8 - 10 bar. ii) A 43 D twin screw from Reifenhäuser (Troisdorf, Germany) was operated at a throughput of 17 kg / h, at prof temperatures of 160 - 240 °C (positions 1 to 3), 260 - 270 °C (positions 4 and 5) to 280 °C (positions 6 - 10) and a speed of 86 rpm. Additionally, the chain extender 1 was added in a high concentration of 1.5 wt.%. This corresponds to a reactive group ratio OH:epoxy of 1 mol:1.78 mol. The melt temperature was 10 - 20 °C higher than the barrel temperature. The propellant supply took place via a Maximator (Maximator GmbH, Germany) and / or via a dosing station (Lewa GmbH, Germany) at position 6 with a content of 2 to 2.3 wt% CO2.The pressure profiles in the twin screw increased gradually from position 5 from 67 bar to the tip of the extruder at 250 bar. The melt was conveyed via the transfer pipe (290 °C) into the single screw (tire houses). The extruder was also operated at a continuous barrel temperature of 280 °C, a throughput of 17 kg / h and a speed of 15 rpm. The melt pressure gradually decreased via the screw until it reached the melt pump (from 250 to 115 bar). The melt pump was operated with pressure control at a back pressure of 110 bar and a temperature of 280 °C. The pressure downstream of the melt pump in this process was 230 bar (pressure at the die plate). The start-up diverter was also set to a temperature of 280 °C and the die plate to 320 °C. The melt temperature was (T. g + 150 °C) to (T g+ 160 °C). Due to an overdose of the reactive component, the throughput had to be significantly reduced and the die plate temperature increased to prevent an emergency shutdown due to critical system pressure. The UWG (EUP 50) and the die plate were manufactured by ECON (Econ GmbH, Austria). The die plate consisted of five individual hole inserts with a diameter of 2.2 mm and a stirrup length of 15 mm. The residence time of the melt between inlet and outlet was approximately 7-10 minutes. After the exit, the melt was separated with a rotating 6-blade knife at 1500 rpm and conveyed by a 70-80 °C cold water circuit (28 m 3 / h). The production process was unstable and resulted in collapsed and shriveled particles (bulk density > 500 g / L) that could not be welded. iii) A 43 D twin screw from Reifenhäuser (Troisdorf, Germany) was operated at a throughput of 15 kg / h, at profile temperatures of 160 - 240 °C (positions 1 to 3), 260 - 270 °C (positions 4 and 5) to 280 °C (positions 6 - 10), and a speed of 85 rpm. This series of tests was conducted without chain extenders. The melt temperature was 10 - 20 °C higher than the barrel temperature. The gas supply was via a Maximator (Maximator GmbH, Germany) and / or a dosing station (Lewa GmbH, Germany) at position 6 with a CO2 content of 2 to 2.3 wt.%. The pressure profiles in the twin screw gradually increased from position 5 onwards from 73 bar to 94 bar at the extruder tip.The melt was conveyed via the transfer pipe (290 °C) into the single-screw extruder (tire houses). The extruder was also operated at a continuous barrel temperature of 280 °C, a throughput of 15 kg / h, and a speed of 15 rpm. The melt pressure gradually decreased via the screw down to the melt pump (from 94 to 87 bar). The melt pump was operated under pressure control at a back pressure of 110 bar and a temperature of 280 °C. The pressure downstream of the melt pump in this process was 90 bar (pressure at the die plate). The start-up diverter and die plate were set to a temperature of 280 °C, and the melt temperature was (T. g + 140 °C) to (T g+ 150 °C). Despite the lack of a reactive component, the process was kept as similar as possible to ii). The UWG (EUP 50) and the perforated plate were manufactured by ECON (Econ GmbH, Austria). The perforated plate consisted of five individual hole inserts with a diameter of 2.2 mm and a stirrup length of 15 mm. The residence time of the melt between inlet and outlet was approximately 7-10 minutes. After the outlet, the melt was separated with a rotating 6-blade knife at 1500 rpm and conveyed by a 70-80 °C cold water circuit (28 m 3 / h). The manufacturing process was not possible under the given conditions and resulted in barely expanded round particles with a very high density of 500 - 600 kg / m 3These were very difficult or impossible to weld into components. iv) A 43 D twin screw from Reifenhäuser (Troisdorf, Germany) was operated at a throughput of 35 kg / h, at profile temperatures of 100 - 160 °C (positions 1 to 3), 240 °C (position 4) to 280 °C (positions 5 - 10) and a speed of 100 rpm. In addition, chain extender 1 was added in a fixed concentration of 0.7 wt.%. In this series, the molar reactive group ratio OH:epoxy was varied by varying the proportion of a second polycarbonate, namely between 1 : 0.82 and 1 : 1.47 (OH:epoxy, each in mol) (Table 1). The melt temperature was 10 - 20 °C higher than the barrel temperature. The propellant supply took place via a Maximator (Maximator GmbH, Germany) and / or via a dosing station (Lewa GmbH, Germany) at position 6 with a content of 1.3 wt% CO2.The pressure profiles in the twin screw gradually increased from position 5 from 45 bar to the top of the extruder at 270 bar for 100 wt.% SPC. By adding a PC component low in OH end groups, PC-2, the pressure profiles initially increased slightly to 275 bar at a content of 10%. Further addition of the PC component low in OH end groups beyond 20 wt.% led to decreasing pressure profiles. The melt was conveyed via the transfer pipe (290 °C) into the single screw (tire houses). The extruder was also operated at a continuous barrel temperature of 280 °C, a throughput of 35 kg / h, and a speed of 26 rpm. The melt pump was operated under pressure control at a back pressure of 110 bar and a temperature of 280 °C. The pressure after the melt pump was determined by the content of the reactive polycarbonate and was reduced by the foreign matrix content (detailed in Table 1).The start-up switch and the perforated plate were also set to a temperature of 280 °C and the melt temperature was T. g + 140 °C to T g + 150 °C. The UWG (EUP 50) and the perforated plate were manufactured by ECON (Econ GmbH, Austria). The perforated plate consisted of five individual hole inserts with a diameter of 2.2 mm and a stirrup length of 3.49 mm. The residence time of the melt between inlet and outlet was approximately 7-10 minutes. After the outlet, the melt was separated with a rotating 6-blade knife at 1500 rpm and conveyed by a 70-80 °C cold water circuit (28 m 3 / h). The roundness of the particles gradually decreased and the foam density increased.
[0114] If the polycarbonate concentration of OH end groups is too low, namely < 350 ppm, the manufacturing process collapses with a molar reactive group ratio (OH:epoxy, each in mol) of 1:1.12 (outside the scope of the claim). The molecular weight buildup no longer occurs sufficiently, so that the viscosities of the melt mixture and thus the pressures at the die plate are no longer sufficient for a homogeneous particle foam. The resulting particles have a more elongated shape and are inhomogeneous in shape and appearance (due to lower viscosity and thus altered flow properties) at higher foam densities (lower pressure drop) (Table 2). The particles can no longer be sufficiently welded in the stressed pressure range of 7–11 bar.The components have no closed surface and numerous sink marks / cavities, resulting in poorer thermal conductivity, increased rigidity, significantly reduced maximum flexural strain, and poorer penetration performance (Table 2 and Table 3). v) A Coperion ZSK 26 MC twin-screw extruder with 44 D was operated at a throughput of 20 kg / h, barrel temperatures of 280°C (from the melting zone), a torque of 60%, and a speed of 230 rpm. Additionally, chain extender 1 was added in low concentrations of 0.9 wt.%. This corresponds to a molar reactive group ratio OH:epoxy of 1:0.9-1.1 for a PC component in the composition with a particularly preferred OH end group content of 450 to 550 ppm, and is thus within the range according to the invention.The blowing agent CO2 was introduced into barrel 7 of 10 of the twin-screw extruder via a gas dosing station (Promix Solutions GmbH, Germany) at concentrations ranging from 1.2 to 1.5 wt.%. The melt temperature of the gas-polymer mixture was 280°C (= T). g+130°C). The homogenized gas-polymer mixture was forced into the static mixer. The residence time in this mixer was 6-8 minutes. The mixer was also operated at a process temperature of 280°C. At the end of the static mixer, a melt pump from Maag-Germany GmbH regulated the backpressure at the melt pump inlet to 90 bar. A pressure of 198 bar was applied upstream of the die plate. The melt was granulated using an underwater pelletizer (from Gala). The gas-melt mixture was forced through a die plate with two holes into the water-filled cutting chamber. The hole diameter of the die plate was 2.4 mm. In the cutting chamber, the melt was cut into pellets by rotating knives. The knife speed was 3500 rpm. The pressure drop behind the die plate caused the pellets to foam. A pressure of 2 bar was applied to the 80 - 90°C hot process water flowing through the cutting chamber.Finally, the granules were dried in a centrifuge and separated. The resulting particles were round, had a smooth, homogeneous surface, a bulk density of 220-250 g / L, and were very easy to weld. c) Test methods.
[0115] The produced particles were formed into components with a density of 200 ± 10 kg / m using a Teubert TVZ162 / 100PP molding machine (Teubert Maschinenbau GmbH, Germany). 3 and a geometry of 300 x 200 x 15 mm 3The required pressure for welding the EPC was in the range of 7 to 10 bar. Finally, the properties of the components were determined. Scanning electron microscopy measurements (SEM, Model: JEOL JSM-6510, Borken, Germany) were performed on graphite-sputtered samples to visualize their morphology. A dynamic mechanical analysis (DMA) was performed on a Gabo Eplexor 500N from NETZSCH GmbH (Selb, Germany) in pressure mode on 15 x 15 x 15 mm 3Samples were tested in a temperature range of -25 to 250 °C at a heating rate of 1 K / min in pressure-regulated mode with an amplitude of 5% (static) and 2% (dynamic) of the sample height at a frequency of 1 Hz. Mechanical characterization was performed using compression, tensile, and 3-point bending tests (room temperature, 80 and 110 °C), as well as puncture tests (room temperature). Compression tests were conducted according to DIN EN ISO 844:2014-11 on a Zwick Z020 universal testing machine from Zwick & Roell (Ulm, Germany) using samples with a geometry of 15 x 15 x 15 mm. 3 and a 10 kN load cell up to 60% compression. A 3-point bending test was performed based on ISO 1209-1:2007-05 using the same universal testing machine at 10 mm / min and a 20 kN load cell. The specimens were skinned to eliminate the influence of the compact surface layer and to limit the geometry to 120 x 25 x 10 mm. 3Tensile measurements on the components were carried out according to ISO 1926:2009 on a Zwick Z050 universal testing machine (Zwick & Roell, Ulm, Germany) with a specimen geometry of 140 (30±80±30) x 80 x 15 mm 3 and a 20 kN load cell. Puncture characterization was performed using a Fractovis Plus dart testing machine from Instron Ceast (Pianezza, Italy) with a maximum energy of 40 J and a penetration speed of 4.4 m / s (based on DIN EN ISO 6603-2:2002-04) with a specimen geometry of 60 x 60 x 15 mm. 3 All mechanical characterizations were performed at room temperature, 80 °C, and 110 °C, each with a 10-minute temperature adjustment period prior to measurement. All components were tested at the same density of approximately 200 kg / m 3Thermal conductivity measurements were performed on a HFM 446 Lambda measuring device from NETZSCH (Selb, Germany) at -10 °C, 10 °C, 25 °C, 50 °C, and 70 °C.
[0116] The average molecular weight Mw for PC-1 and PC-2 was determined using gel permeation chromatography. Calibration was performed against bisphenol A polycarbonate standards using dichloromethane as the eluent. Calibration was performed with linear polycarbonates (made from bisphenol A and phosgene) of known molecular weight distribution from PSS Polymer Standards Service GmbH, Germany. Calibration was performed according to method 2301-0257502-09D (from 2009 in German) from Currenta GmbH & Co. OHG, Leverkusen. The eluent was dichloromethane. Column combinations consisted of cross-linked styrene-divinylbenzene resins. Analytical column diameter: 7.5 mm; length: 300 mm. Particle sizes of the column material: 3 mm to 20 mm. Solution concentration: 0.2 wt.%. Flow rate: 1.0 ml / min; solution temperature: 30°C. Injection volume: 100 ml. Detection via UV detector.For the highly branched polycarbonate resulting from the molecular weight increase through the addition of a chain extender, the determination was carried out using GPC-MALLS, as described below. Not all highly branched / partially crosslinked fractions could be dissolved (XYZ% insoluble), so that particularly high molecular weight fractions cannot be characterized using existing analytical methods. This is a problem known to those skilled in the art, so the accuracy of determining the molecular weight for highly branched polymers is limited. The aforementioned molecular weight ranges refer accordingly to the fractions soluble in dichloromethane.
[0117] The OH number of the polymers was determined by 'H-NMR spectroscopy with dichloromethane as solvent at room temperature, evaluating the ratio of the integrals of the signals at 6.68 ppm (2 aromatic protons ortho to phenolic OH groups) and at 1.68 ppm (6 methyl protons of the bisphenol A unit). 2. Results
[0118] Compositions and analytics
[0119] Tab. 1: Detailed compositions and analytical results of the molar ratio study according to Example iv) Tab. 2: Detailed parameters of the compression tests, bending tests and puncture tests for the comparative study in example iv) of the EPC particle foam components
[0120] Note: Component made of EPC (V-4) has a foam density of 230 kg / m 3 The parameters here are original and would have to be adjusted with a factor of 0.85 for simple %-normalization.
[0121] Tab. 3: Complete data for the thermal conductivity of EPC (El) and (V4).
[0122] # Thermal conductivity data of the non-expanded starting material
Claims
1. A process for producing foamed polycarbonate beads, comprising the following steps: a) providing a composition based on aromatic polycarbonate, wherein the aromatic polycarbonate, based on the total weight of the aromatic polycarbonate, has a content of OH end groups of at least 350 ppm, determined by 'H-NMR spectroscopy with dichloromethane as solvent at room temperature, b) mixing the aromatic polycarbonate-based composition with a chain extender suitable for OH groups in a molar ratio such that 0.64-1.10 mol of the reactive group of the chain extender is used per 1 mol of OH end groups of the polycarbonate, c) providing the mixture in a plasticized state, d) mixing a physical blowing agent into the melt, e) particle foam extrusion of the plasticized mixture at a temperature T of Ti = (T g+ 110°C) to T2 = (T g + 170°C), where T g is the glass transition temperature of the aromatic polycarbonate-based composition, f) granulating the blowing agent-containing melt.
2. The process according to claim 1, wherein carbon dioxide is used as the blowing agent.
3. The process according to claim 1 or 2, wherein the process is conducted as a continuous process.
4. A process according to any one of the preceding claims, wherein the aromatic polycarbonate-based composition of step a has a melt volume flow rate MVR of up to 12 cm 3 / (10 min), determined according to ISO 1133:2012-3 (test temperature 300°C, mass 1.2 kg).
5. A process according to any one of the preceding claims, wherein the granulation is carried out as granulation in a liquid medium, as hot die granulation or as sub-air granulation.
6. Process according to one of the preceding claims, wherein the granulation is carried out as underwater granulation without pressure application.
7. Process according to one of the preceding claims, wherein one or more epoxy-functionalized compounds are used as chain extenders.
8. A process according to any one of the preceding claims, wherein 0.1 - 2.3 wt.% of physical blowing agent is admixed in step d, the amount being based on the total weight of aromatic polycarbonate-based composition and ketene extender.
9. A process according to any one of the preceding claims, wherein the aromatic polycarbonate of the composition from step a has, based on the total weight of the aromatic polycarbonate, a content of OH end groups of 350 to 600 ppm, determined by means of 1 H- NMR spectroscopy with dichloromethane as solvent at room temperature, 10. Process according to one of the preceding claims, wherein the aromatic polycarbonate of the composition from step a has, based on the total weight of the aromatic polycarbonate, a content of OH end groups of at least 380 ppm, determined by 'H-NMR spectroscopy with dichloromethane as solvent at room temperature.
11. Method according to one of the preceding claims, wherein step b and step d occur in an overlapping manner.
12. The method according to any one of claims 1 to 10, wherein steps a to f take place in the order mentioned.
13. The process according to any one of the preceding claims, wherein the ketene extender used is an epoxy-functionalized ketene extender having an epoxy equivalent weight of 285 to 485 g / mol.
14. Polycarbonate beads produced by the process according to any one of the preceding claims.
15. A process for producing molded parts from the polycarbonate beads according to claim 14, wherein the cracking method or the pressure filling method is used.
Citation Information
Patent Citations
Hydrolytically stable polycarbonates and processes for their production
DE1570703A1
Working up of additives in fat and protein - contng foodstuffs
DE2036052A1
Saponification-resistant polycarbonates, processes for their production and their use
DE2063050A1
PROCESS FOR THE MANUFACTURE OF SAPFONATION-STABLE BLOCKCOPOLYCARBONATES
DE2211956A1
Dihydroxydiphenylcycloalkanes, their preparation, and their use for the preparation of high-molecular-weight polycarbonates
DE3832396A1