A heat treatble glass article with an enamel coating

The use of a high temperature degradable polymeric binder in enamel coatings for glass substrates creates uniformly scattered voids, overcoming the limitations of conventional coatings to achieve enhanced opacity and stability, resulting in a durable, opaque, and weather-resistant glass article suitable for various applications.

WO2024218787A1PCT designated stage expired Publication Date: 2024-10-24SAINT GOBAIN VITRAGE SA +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/IN2024/050332
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-19
Filing Date
2024-03-28
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Conventional enamel coatings for glass substrates face limitations in achieving high opacity due to the maximum amount of inorganic pigments and extenders that can be used, leading to instability during storage and blending issues, which restricts the maximum achievable opacity and hiding power.

Method used

A heat treatable glass article with an enamel coating comprising a high temperature degradable polymeric binder that forms uniformly scattered voids upon curing and firing, enhancing opacity without the traditional challenges of formulation stability.

Benefits of technology

The solution results in a substantially opaque glass article with minimal visible light transmission, allowing for handling and tempering at high temperatures, and improved mechanical and optical properties, including durability and resistance to scratches and weathering.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IN2024050332_24102024_PF_FP_ABST
    Figure IN2024050332_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The present application provides a heat treatable glass substrate coated with an enamel formulation The enamel formulation comprises inorganic components, pigment, diluents and a high temperature degradable polymeric organic binder. The high temperature degradable polymeric organic binder post curing and firing of the glass substrate opacifies the glass substrate such that the glass substrate has substantially minimal visible light transmission, by forming uniformly scattered voids. Further the application also provides a method of making the heat treatable glass substrate thereof.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] A HEAT TREATBLE GLASS ARTICLE WITH AN ENAMEL COATING

[0002] TECHNICAL FIELD

[0003] The present disclosure in general relates to glass substrates coated with an enamel to improve opacity of the glass substrate. Specifically, the present disclosure relates to heat treatable glass substrates provided with an enamel coating comprising a high temperature degradable polymeric binder such that the said coating during a heat treatment process forms scattered voids. Further disclosed is a method of making a glass substrate thereof.

[0004] BACKGROUND

[0005] Glass articles coated with enamel, find their application in interior and exterior applications in buildings which must be opaque, optically distortion-free, tenaciously adherent, reasonably hard and resistant to sunlight, sun heat, chemicals and moisture, and several other functional properties. Specifically, glasses with opaque properties are intended for decorative building walls, or interior furniture fronts, and decorating glass sheets. For example, the enamel coatings on glass substrates may be used to form wardrobes, as privacy doors, decorative furniture, as partitions, in tables, shelves, in bathrooms, in shops displays, as wall covering, in outdoor environments, etc.

[0006] It is very well established in the state of art to form an enamel coating layer on a glass sheet by applying a paste or paint prepared by dispersing an inorganic pigment and a finely powdered glass frit in a mixed solution of an organic binder and an organic solvent onto a surface of the glass sheet. And by further using the known techniques of screen-printing, roller coating or digital printing, a paint layer is formed on the glass surface which is further dried and fired to fuse the glass frit contained in the paint layer. Conventionally, enamel coated glass sheets for increasing the opacity may be produced according to various other processes. Conventional enamel-based commercial formulations are known to have high concentration of inorganic pigments and glass frits, with a relatively low concentration of organic binders or additives. The increased content of the inorganic pigments and extenders could generally improve opacity. However, the traditional enamel coatings systems are limited by the maximum amount of the pigments and extenders that can be used to allow for consistent deposition of the coatings on the glass substrate. Increased pigment usage to improve opacity also results in poor coating deposition.

[0007] Patent document WO2011051459A1 discloses enamel coatings with increased organic resin content to improve the green strength of the enamel coating with glass. The enamel coating in this application comprises between 11 and 40 % of organic material. However, coatings with the higher organic content have not been reported to improve the opacity over conventional enamel systems.

[0008] Patent application EP3140261A1 discloses glass or glass-ceramic substrate, covered with an enamel layer. An organic resin is used as an undercoat underneath an enamel layer to impart higher adhesion and water resistance. Similarly, patent application US20090220778A1 teaches an organic resin being used as an overcoat on top of the enamel layer to impart higher green strength to the coating. The organic resin could potentially offer good green strength but does not offer any further improvements in opacity over the conventional enamel systems.

[0009] Patent application US20090099287A1 teaches the use of polysiloxane coating in heat- treatable coating and is shown to withstand greater than 500°C exposure with no deterioration of the coating or the polysiloxane. The invention is intended towards a pyrolysis-resistant coating paint. The polysiloxane coating is entirely retained in its polymer form during the heat-treatment with the use of the heat-dissipating inorganic pigments. However, there is no suggestion of increase in opacity or hiding power of the coatings.

[0010] PCT publication WO2007135192 discloses a glass sheet having a coating comprising enamel provided on at least part of its surface characterized in that the enamel is curable under infrared rays and the contact angle between a water droplet and the coating at a portion of the glass sheet carrying the coating is greater than 75°. Similarly, PCT publication WO2011051459 discloses glass sheet having a coating of enamel provided on at least one surface of said glass sheet, characterized in that the coating comprises between 11 and 40 % of organic material, expressed in weight percentage, and in that the coating is in direct contact with the glass sheet. However, again these documents focus on the enamel coating that provides for the necessary green strength for processability prior to tempering, and no suggestion of increase in opacity or hiding power of the coatings.

[0011] More recently, preceramic polymers or ceramic precursors have been known as starting materials for the manufacture of ceramic materials, but these materials have, however, not been known to be used in enamel formulations or coatings to increase the opacity. The patent publication WO2022195612A1 discloses a heat treatable glass substrates provided with an enamel coating comprising a ceramic precursor, such that the said coating during a heat treatment process opacifies the glass substrate. However, the ceramic precursors do not undergo complete decomposition and leave behind inorganic residues after high temperature treatment. Moreover, the typical ceramic precursors based on silicones, silazanes etc., have challenges during mixing and storage leading to phase separation and agglomeration.

[0012] In the established works in the state of art, there is a maximum limit on the inorganic pigments or extenders available for use, that can allow for a homogenous enamel coating deposition. This in turn limits the maximum achievable opacity (or hiding power) at a given enamel film thickness. Summarily, in the state of art, the opacity of the glass frit enamel-based paints is provided by the incorporation of pigments, extenders, hollow microspheres, or ceramic precursors. However, excessive incorporation of any of these components causes problems with blending and formulation stability during storage.

[0013] Therefore, it is desirable to develop glass articles with enamel coatings having the desired opacity and as well ensuring that a homogeneous deposition of the coating is achieved. With the proposed invention, this problem is circumvented with the use of a high temperature degradable polymeric binder that allows for good blending in the formulation, creates uniformly scattered voids on curing and firing the coating and homogenous deposition on glass. After curing followed by a high temperature heattreatment during glass toughening, the enamel coating improves the opacity of the coated glass article. The present invention allows for improving opacity of the enamel coatings without the traditional challenges of formulation stability.

[0014] OBJECT OF INVENTION

[0015] The main object of the present invention is to provide a heat treatable coated article, specifically a glass article. Said article coated with an enamel, the enamel particularly comprises a high temperature degradable polymeric binder, which while undergoing curing and firing, forms coating with uniformly scattered voids.

[0016] Another object of the present invention is to provide a heat treatable coated glass article, said article coated with an enamel, the enamel coating opacifies the glass substrate and provides a substantially opaque glass article, thereby ensuring nil or minimal visible light transmission. Yet, another object of the present invention is to provide a method for making a heat treatable coated article, with an enamel in accordance with the disclosure. A glass article produced by the method in accordance with the disclosure forms a coating with uniformly scattered voids, withstands the high tempering temperatures during the making of the glass substrate along with improving the opacity during the heat treatment.

[0017] Further, yet another object of the present invention is to provide a heat treatable coated glass article, in accordance with the method disclosed, such that the glass substrate can optionally be handled and / or transported without mechanical damages to the enamel coating and further be tempered at temperatures as high as 750 °C after being handled and / or transported.

[0018] The present disclosure was developed by outlining the above objectives.

[0019] SUMMARY OF THE DISCLOSURE

[0020] In one aspect of the present disclosure, a heat treatable coated article is disclosed, specifically a glass article. The article comprises a glass substrate, and an enamel coating applied directly onto a surface of the glass substrate. The enamel coating comprises pigments, inorganic component, diluents, and high temperature degradable polymeric organic binder, which when once cured and fired at a high temperature, forms coating with uniformly scattered voids.

[0021] The high temperature degradable organic binder forming the scattered voids, opacifies the glass substrate during the firing of the enamel on the glass substrate, and such that the glass substrate after the heat treatment has substantially minimal visible light transmission. Optionally, the glass substrate can also be handled and / or transported without mechanical damages to the enamel coating and further be tempered at temperatures as high as 750 °C after being handled and / or transported.

[0022] In another aspect of the present disclosure, a method for making a heat treatable coated article, specifically a glass article is disclosed. The method involves the steps of: cleaning a glass substrate having a first surface and a second surface; applying the enamel coating on one of the surfaces of the glass substrate, wherein the enamel comprises pigments, inorganic component, diluents and high temperature degradable polymeric organic binder; drying in an infrared oven for about 10 - 20 minutes at a temperature of less than 250 °C; and heat treating the enamel coated glass substrate at a temperature of about 600 to 750 °C. The enamel coating comprising the high temperature degradable polymeric organic binder upon curing and firing forms a coating with uniformly scattered voids.

[0023] Other features and aspects of this disclosure will be apparent from the following description and the accompanying drawings.

[0024] BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Embodiments are illustrated by way of example and are not limited in the accompanying figures.

[0026] FIG. 1 illustrates a cross-sectional view of a heat treatable glass article, in accordance with one embodiment of the present disclosure.

[0027] FIG. 2 illustrates a graphical representation of the change in the thickness of the enamel coating after tempering, in accordance with an embodiment of the present disclosure. FIG. 3(a), 3(b) and 3(c) illustrate the SEM micrographs of the cross-section of the coatings post tempering / fusion with a polymeric binder concentration of 4%, 10% and 16%, in accordance with one embodiment of the present disclosure.

[0028] FIG. 4 illustrates a graphical representation of a thermogravimetric analysis of different binders showing the impact of high temperature degradable polymers and low temperature degradable polymers on the pyrolysis temperatures, in accordance with one embodiment of the present disclosure.

[0029] FIG. 5 illustrates a graphical representation of the opacity of the coatings expressed as AE* as a function of the dry film thickness for coatings with two different binder chemistries as per Inventive Example 1 and Comparative Example 1, in accordance with one embodiment of the present disclosure.

[0030] FIG. 6(a), 6(b) and 6(c) illustrates the SEM micrographs of the enamel coating with an enamel formulation having a binder with a low pyrolysis temperature, according to comparative example 1, for different film thicknesses measured before frit fusion, in accordance with one embodiment of the present disclosure.

[0031] FIG. 6(d), 6(e) and 6(f) illustrates the SEM micrographs of the enamel coating with the enamel formulation having a binder with a high pyrolysis temperature according to inventive example 1, for different film thicknesses measured before frit fusion, in accordance with one embodiment of the present disclosure.

[0032] Skilled artisans appreciate that elements in the figures are illustrated for simplicity and clarity and have not necessarily been drawn to scale. For example, the dimensions of some of the elements in the figures may be exaggerated relative to other elements to help to improve understanding of embodiments of the invention. DETAILED DESCRIPTION

[0033] As used herein, in every embodiment, it must be understood that the terms or phrases ‘high temperature degradable polymer’ or ‘high pyrolysis polymer’ or ‘high temperature pyrolysis polymer’, can be used interchangeably. Said phrases refer to a polymer material that has not completely pyrolyzed or decomposed at temperatures in excess 450°C.

[0034] The term ‘high temperature heat treatment’ or ‘firing’ can be used interchangeably, refers to a heat treatment of glass substrate at a temperature above 600° C and less than 750°C.

[0035] The term ‘curing’ as used herein, refers to a step of hardening of a polymer material by cross-linking of polymer chains.

[0036] The term ‘firing’ as used herein, refers to a step of the fusion of the inorganic frits at temperatures in excess of 450°C.

[0037] The term ‘crosslinked polymer’, is well known to a person skilled in the art, refers to long polymer chains formed when cross-linked together to create a three-dimensional network.

[0038] The term ‘non-crosslinked polymer’, is well known to a person skilled in the art, refers to linear polymers which are held together by weaker van der Waals forces.

[0039] As used herein, the term or phrases ‘voids’ or ‘scattered voids’ or ‘uniformly scattered voids’ can be used interchangeably, refers to closed pores within the matrix of the enamel coating post-firing or high temperature treatment. The term ‘article’, as used herein, refers to a final product, which comprises a glass or a transparent substrate provided with the enamel coating thereof.

[0040] The term ‘glass substrate’ or ‘transparent substrate’, as used herein, interchangeably, refers to a solid-like and transparent material that is used in numerous applications in our daily lives. As referred herein, the substrate is glass which is made from natural and abundant raw materials (sand, soda ash and limestone) that are melted at very high temperature to form a new material

[0041] The present application provides a heat treatable coated article, specifically the article being a glass article. The coated article in accordance with the present disclosure comprises a glass substrate, and an enamel coating applied directly onto a surface of the glass substrate. In accordance with the present disclosure the enamel coated article, post curing and firing has uniformly scattered voids. Beneficially, the scattered voids resulted in enhanced opacity of the coated glass article, in accordance with the present disclosure. Further, beneficially the disclosed enamel coating in accordance with the present disclosure allows for a good blending and homogeneous deposition over the glass substrate.

[0042] FIG. 1 illustrates a cross-sectional view of a heat treatable glass article 100 in accordance with one embodiment of the present disclosure. As shown, the heat treatable glass article 100 includes a glass substrate 101 having a first surface 102 and a second surface 103. The glass substrate 101 is directly provided with an enamel coating 104 in accordance with the present disclosure, on a first surface 102 of the glass substrate 101. In one embodiment of the present disclosure, the enamel coating provided on the first surface 102 of the glass substrate 101 comprises pigments, inorganic component, diluents. In accordance with every embodiment of the present disclosure, the enamel coating 104 comprises high temperature degradable polymeric organic binder.

[0043] In one embodiment of the present disclosure, the heat treatable glass substrate 101 is coated with an enamel 104 on the entire first surface 102 of the glass substrate 101 or in parts of the first surface 102 of the glass substrate 101. In a few other embodiments the enamel coating 104 can be provided as a design pattern that can cover the surface area of the first surface 102 of the glass substrate 101 in varying extents, from 0.1 to 100%. In such an embodiment, the enamel coating 104 may be provided in the form of a decorative pattern using screen printing techniques to obtain various shapes and sizes. In an alternate embodiment, the enamel coating 104 can also be provided on the second surface 103 of the glass substrate 101.

[0044] In one embodiment of the present disclosure, the heat treatable glass substrate 101 is provided with an enamel coating 104. The enamel coating formulation comprises the inorganic component in the range of 40 to 70 weight %; pigments in the range of 0 to 50 weight %; diluents in the range of 10 to 40 weight %; and high temperature degradable polymeric organic binder in the range of 2 to 25 weight %.

[0045] The glass substrate coated with an enamel 104 in accordance with the present disclosure comprising, the inorganic component further consists of frits. The inorganic component is preferably present in the enamel coating 104 in the range of 40 to 70 weight%. In a most preferred embodiment, the inorganic material is present in the range of 45 to 70 weight%. The inorganic frit is selected from the group comprising but not limited to oxides of zinc, bismuth, lithium, boron, sodium, aluminum, silicon, potassium, calcium, titanium, chromium, iron, cobalt, copper, strontium, zirconium, barium. In accordance with an embodiment of the present disclosure, the pigment is selected from the group consisting of but not limited to titanium dioxide, zinc oxide, iron or other metal ion doped titania, copper oxide, chromium oxide, cobalt oxide, lithium niobate, manganates, beryllium oxide, cadmium sulfide or cadmium telluride.

[0046] The diluents and polymeric binder constitute to organic components in the enamel coating 104. In a preferred embodiment the organic component in the enamel coating 104 is present in the range of 10 to 60 weight%. In a preferred embodiment the organic component is present in the range of 15 to 40 weight%.

[0047] In a specific embodiment the diluent is present in the range of 10 to 40 weight % of the enamel coating 104. The diluents present in the enamel coating 104 is selected form the group comprising but not limited to alkanes, alkyl acetates, ketones, di-acetone alcohol, ether glycol, xylene, toluene or ethyl methyl ketone and their combinations thereof.

[0048] The heat treatable glass substrate 101 provided with the enamel coating 104 in accordance with the present disclosure further comprises the high temperature degradable polymeric organic binder. In accordance with a specific embodiment of the present disclosure, the high temperature degradable polymeric organic binder, in the enamel coating is present in the range of 2 to 25 weight %. In a most preferred embodiment the high temperature degradable polymeric organic binder, in the enamel coating is present in the range of 5 to 15 weight %. The high temperature degradable polymeric organic binder is selected from the group comprising, but not limited to polyacrylics, polyesters, polyacrylates, polyurethanes, polysilicones, polysilazanes, epoxies, melamines and their combinations thereof. In a specific embodiment the high temperature degradable polymeric organic binder is a polyurethane. The high temperature degradable polymeric organic binder in accordance with a preferred embodiment of the present disclosure is a crosslinked polymer. In a most preferred embodiment high temperature degradable polymeric organic binder is a polyurethane system. For example, an acrylic polyol and a blocked poly-isocyanate cured at temperatures in excess of 140°C during the curing of the paint provides a polyurethane coating.

[0049] In some embodiments the high temperature degradable polymeric organic binder is also a non-crosslinked polymer. In accordance with the present disclosure crosslinked polymer includes any polyol linked to an isocyanate group, polymers with hydroxyl groups that condense to form a linkage with or without the presence of a catalyst, polyols that react with an amine-functional molecule or any self-crosslinking polymer. In another embodiment in accordance with the present disclosure the non-crosslinked polymer includes polyacrylics, polyesters, polyacrylates, polyurethanes, polysilicones, polysilazanes, epoxies, melamines, urea formaldehyde, phenol formaldehyde, polyamides, polyimides, fluoropolymers, their combinations thereof.

[0050] In multiple embodiments of the present disclosure, the enamel coating 104 inclusive of the high temperature degradable polymeric organic binder enhances the opacity of the enamel coatings. The enamel coating 104 in accordance with the present disclosure form scattered voids 105 once the coating is cured and fired at a temperature of in excess of 450°C. During the firing, the inorganic frits soften and fuse and form a continuous inorganic matrix. In a conventional system, the organic binders burn off completely prior to frit fusion, resulting in a homogenous coating post the glass toughening process. The inventors in accordance with the present disclosure incorporated the high temperature degradable polymeric organic binder in the enamel coating 104 which resulted in concurrent occurrence of the glass frit fusion and the thermal degradation of the organic binder which resulted in uniform scattered voids 105. The scattered voids in accordance with the present disclosure are a result of entrapped organic vapor from the pyrolysis of the polymeric organic binder. The voids filled with vapor have a refractive index (~1) that is lower than the surrounding inorganic matrix (-1.5-1.6) and the pigments (> 3) incorporated therein. This leads to reflections of light waves at the interface of the voids and the surrounding matrix resulting in scattering in different directions. The light scattering thus reduces direct transmission of light through the inorganic matrix. In every embodiment of the present disclosure the uniformly scattered voids 105 act as light scattering sites thereby providing higher opacity than the conventional formulations.

[0051] The extent of the formation of the scattered voids 105 in the fused frit network due to the entrapment of vapor depends on the concentration of the high temperature degradable polymeric organic binder used in the enamel coating 104. This can be inferred from the change in the enamel coating 104 thickness during the frit fusion. In the absence of any vapor entrapment, the glass frits fuse and shrink thereby reducing the overall thickness of the coating. In accordance with the present disclosure, in the presence of a high temperature degradable polymeric organic binder, which undergoes at least part of its decomposition at temperatures similar as that of frit fusion, there is an increase in the enamel coating thickness due to the vapor expansion, in addition to the decrease in the enamel coating thickness due to frit fusion. Referring to FIG. 2 which depicts a plot of the change in the thickness of the enamel coating 104 after tempering as a function of the organic binder concentration. It is seen that the extent of enamel coating shrinkage post tempering decreases with increasing the binder concentration and eventually results in an increase in coating thickness. At lower organic binder concentrations, the shrinkage associated with frit fusion dominates over any coating expansion due to vapor buildup. As the concentration of the organic binder increases, coating expansion due the vapor buildup is higher than the shrinkage due to frit fusion, resulting in a net increase in coating thickness post-tempering. In an example embodiment, the crosslinked high temperature degradable polymeric organic binder is a polyurethane system. The polyurethane system resulted from the crosslinking of an acrylic polyol and a polyisocyanate crosslinker. In accordance with the present disclosure the acrylic polyol and a polyisocyanate crosslinker is mixed in a 1: 1 ratio. In another example embodiment, the non-crosslinked high temperature degradable polymeric organic binder is an acrylic polyol. Referring to FIG. 4 which depicts a thermogravimetric analysis of two different binders in accordance with the present disclosure showing the difference in the temperatures of complete pyrolysis. The high temperature degradable polymeric organic binder in accordance with a preferred embodiment, undergoes complete pyrolysis only at temperatures exceeding 450°C. The low temperature degradable polymeric organic binder, in accordance with another preferred embodiment, has a complete burn out at temperatures around 400°C. In every embodiment of the present disclosure, the increase in the temperature for complete pyrolysis has surprisingly and beneficially expected to result in the entrapment of the organic vapor in the fused frit system.

[0052] The present disclosure further provides a method for making a heat treatable coated article 100, which is coated with the enamel 104, as per the teachings of the present disclosure. The method comprises the steps of cleaning a glass substrate having a first surface 102 and a second surface 103. The first surface 102 of the glass substrate 101 is applied with the enamel coating 104.

[0053] The enamel coating 104 is applied directly on the glass substrate 101 covering its surface area in entirety or in parts using a variety of wet-coating deposition techniques including but not limiting to Meyer rod coating, screen printing, embossed roller coating, digital printing, curtain coating, gravure coating, ink-jetting, spray painting, spin coating, bar coating or dip coating. The enamel coating 104 can be provided in any form, size, shape and / or color in such a way that it covers the surface area of the glass substrate 101, in entirety or in parts thus making a patterned design.

[0054] In an embodiment, the enamel coating 104 according to the present disclosure when applied by any of the known wet application processes such as spraying, dipping, flow coating, and electrodeposition, the coating is dried prior to firing. Drying is typically accomplished using IR lamps. The thickness of the enamel coating 104 typically depends on the requisite function and opacity to be achieved.

[0055] Further, the glass substrate coated with an enamel 104 is dried in an infrared oven for about 10 to 20 minutes at a temperature of less than 250 °C followed by heat treating the enamel coated glass substrate at a temperature of about 600 to 750 °C.

[0056] In accordance with the present disclosure, the thickness of the enamel coating 104 ranges from 1 to 200 pm. In a preferred embodiment the thickness of the enamel coating 104 ranges from 5 to 100 pm, and in a most preferred embodiment the thickness of the enamel coating 104 ranges from 10 to 50 pm. The enamel coating 104 can be used to cover the first surface 102 of the glass substrate 101 in its entirety or in parts as a decorative pattern. The patterns formed by the enamel coating 104, printed on the glass substrate 101 are selected from the various patterns including but not limited to logos, lines, polka dots, circles, square, triangle, oval, rectangle, octagon, parallelogram, trapezoid, pentagon, hexagon, stars, gradients, abstract shapes or a combination thereof, with varying diameters and depths. The surface area to be covered by the enamel coating 104 in the present disclosure is varied based on the requirement and shape of the pattern.

[0057] During the heat treatment step, the enamel coating 104 is fused onto the glass substrate 101. The high temperature degradable polymeric organic binder in accordance with the present disclosure leaves behind voids in the enamel coating 104 during its bum-off and the concurrent fusion of the inorganic enamel frits. The introduction of voids in the enamel coating 104 leads to increasing the opacity or the hiding power of the glass substrate. The glass articles 100 thus formed are substantially opaque with nil or minimal visible light transmission. The glass substrate with the enamel coating 104 of the disclosure does not yellow on curing and gives a hard, durable, scratch-resistant, gasoline-resistant, weatherresistant, alkali-resistant coating which is suitable for all interior and exterior glass applications including but not limited to partitions, wall cladding, spandrels, facades, and decorative purposes that necessitate having bright, opaque colors and improved aesthetics.

[0058] Further the enamel coated 104 glass substrate 101 thus obtained according to the teachings of the present disclosure can also be transported, cut, stored and / or washed and made to undergo other post-processing steps such as those not limited to edge grinding, bending etc., before subsequently being tempered or toughened at tempering temperature as high as 750°C for a specified duration of time. In few other embodiments, the enamel coated glass substrate thus obtained according to the teachings of the present disclosure cannot be handled before tempering.

[0059] EXAMPLES

[0060] Inventive Example 1

[0061] Table 1 discloses an enamel coating [incorporated with a high temperature degradable polymer], according to an inventive Example 1 :

[0062] Table 1

[0063] Preparation of an enamel coated glass substrate: Sample A is prepared in accordance with the present disclosure.

[0064] Table 1 discloses Sample A, which was prepared following the steps produced below:

[0065] 1) Cleaning a clear glass substrate having a first surface and a second surface. The clear glass substrate has a thickness of 6 mm.

[0066] 2) Preparing an enamel coating, comprising inorganic component, pigments, diluents and a crosslinked high temperature degradable polymeric organic binder. The enamel coating formulation has about 60wt.% of inorganic components that include glass frits, pigments, 30 wt.% of organic components, a diluent and about 10wt.% of the high pyrolysis polymer.

[0067] 3) Depositing an enamel coating inclusive of the high temperature degradable polymeric organic binder over one first surface of the clear glass substrate.

[0068] 4) Drying in an infrared oven for less than 20 minutes at a temperature of less than 250 °C. After drying, the enamel coating has a thickness ranging from about 1 pm to about 100 pm.

[0069] 5) Heat treating the coated clear glass substrate at a temperature of about 600 to 750 °C to obtain a glass substrate.

[0070] 6) Quenching the obtained coated clear glass substrate to toughen the glass.

[0071] Comparative Example 1

[0072] Table 2 discloses an enamel coating [incorporated with a low temperature degradable polymer], according to a comparative Example 1:

[0073] Table 2 Referring to FIG. 5 which depicts a plot of the opacity of the coatings expressed as AE* as a function of the dry film thickness for coatings with two different binder chemistries [Inventive Example 1 - Table 1 & Comparative Example 1 - Table 2],

[0074] The opacity of coated glasses were measured in a spectrophotometer by measuring the L*,a* and b* values against a black background and a white background. The difference in the L*, a* and b* values against the two backgrounds were represented as the contrast AE*, with a higher value denoting poorer hiding power.

[0075] The dry film thickness was measured on the coating prior to the glass tempering, while the opacity AE* was measured on the same substrate after the glass tempering. As shown in the figure, as the thickness of the coatings increases, the AE* decreases showing improved opacity. Moreover, the graph also indicates a difference in opacity at a given thickness for a coating containing a binder that has a lower pyrolysis temperature [comparative example 1] and a binder that has a higher pyrolysis temperature [inventive example 1], The improvement in opacity (lower AE*) with a high temperature pyrolysis binder [inventive example 1] is a direct result of the entrapment of the voids in the coating, which act as light scattering sites.

[0076] It has also been further inferred that the improvement in opacity with the incorporation of a high temperature degradable polymeric organic binder, in accordance with inventive example 1, allows for a reduced usage of enamel formulation to achieve the same target opacity. Furthermore, referring to FIGS. 3a, 3b and 3c which show the SEM micrographs of the cross-section of the coatings post tempering / fusion. FIG. 3a indicates a polymeric binder concentration of 4%, FIG. 3b indicates a polymeric binder concentration of 10% and FIG. 3c indicates a polymeric binder concentration of 16%. The concentration and the size of the voids in the coating increase with increasing binder concentration. This correlation between the size / distribution of voids and the concentration of the binder allows for an optimized design of the formulation that provides the desired optical and mechanical properties.

[0077] Further referring to FIGS. 6(a), 6(b) and 6(c) which indicate the SEM micrographs of the enamel coating with a conventional enamel formulation having a binder with a low pyrolysis temperature, according to comparative example 1, for different film thicknesses measured before frit fusion. Similarly, FIGS. 6(d), 6(e) and 6(f) indicate the SEM micrographs of the enamel coating with the enamel formulation having a high temperature degradable polymeric organic binder according to inventive example 1, for different film thicknesses measured before frit fusion.

[0078] It is clearly indicated that in Figure 6a, Figure 6b and Figure 6c in the coating with a low pyrolysis temperature, discrete frit particles in the coating fuse to form a continuous network. There are some isolated voids that form due to the entrapment of the vapor from the binder burnout, but these voids do not seem to contribute significantly to the overall opacity of the coatings. In contrast, Figure 6d, Figure 6e and Figure 6f [according to inventive example 1] show the cross-sectional micrographs, where the high temperature degradable polymeric organic binder used results in a large number of entrapped vapour in the fused frit network.

[0079] Reference Numerals

[0080] 100 Glass Article

[0081] 101 Glass substrate

[0082] 102 First Surface

[0083] 103 Second Surface

[0084] 104 Enamel coating

[0085] 105 Scattered Voids

Claims

We Claim:1) A heat treatable coated article 100 comprising: a glass substrate 101, an enamel coating 104 applied directly onto a surface 102 of the glass substrate 101; wherein the coating comprising pigments, inorganic component, diluents, and high temperature degradable polymeric organic binder once cured and fired at a high temperature, forms coating with uniformly scattered voids 105.2) The heat treatable coated article 100 as claimed in claim 1, wherein the high temperature degradable polymeric organic binder is a crosslinked or non-crosslinked polymer.3) The heat treatable coated article 100 as claimed in claim 1, wherein the high temperature degradable organic binder is selected from the group consisting of, but not limited to, polyacrylics, polyesters, polyacrylates, polyurethanes, polysilicones, polysilazanes, epoxies, melamines, urea formaldehyde, phenol formaldehyde, polyamides, polyimides, fluoropolymers and their combinations thereof.4) The heat treatable coated article 100 as claimed in claim 1, wherein the high temperature degradable polymeric organic binder, in the enamel coating is in the range of 2 to 25 weight %.5) The heat treatable coated article 100 as claimed in claim 1, wherein the inorganic component comprising frits, in the enamel coating is in the range of 40 to 70 weight %.6) The heat treatable coated article 100 as claimed in claim 1 , wherein the pigments in the enamel coating is in the range of 0 to 50 weight %.The heat treatable coated article 100 as claimed in claim 1, wherein the diluents in the enamel coating is in the range of 10 to 40 weight %.8) The heat treatable coated article 100 as claimed in claim 1, wherein the coated article can optionally be handled and / or transported without mechanical damages to the enamel coating and further be tempered at temperatures as high as 750 °C, after being handled and / or transported.9) The heat treatable coated article 100 as claimed in claim 5, wherein the frits are selected from the group comprising but not limited to oxides of zinc, bismuth, lithium, boron, sodium, aluminum, silicon, potassium, calcium, titanium, chromium, iron, cobalt, copper, strontium, zirconium, barium.10) The heat treatable coated article 100 as claimed in claim 6, wherein the pigment is selected from the group comprising but not limited to titanium dioxide, zinc oxide, iron or other metal ion doped titania, copper oxide, chromium oxide, cobalt oxide, lithium niobate, manganates, berilium oxide, cadmium sulfide or cadmium telluride.11) The heat treatable coated article 100 as claimed in claim 7, wherein the diluent is selected from the group comprising but not limited to alkanes, alkyl acetates, ketones, di-acetone alcohol, ether glycol, xylene, toluene or ethyl methyl ketone and their combinations thereof.12) The heat treatable coated article 100 as claimed in claim 1, wherein the enamel coating 104 deposited on the glass substrate has a thickness in the range of 1 to 200pm.13) The heat treatable coated article 100 as claimed in claim 1, has an opacity measured via black / white contrast card -AE* - value in the range of 0 to 0.5.14) A method for making a heat treatable coated article 100, comprising the step of:cleaning a glass substrate 101 having a first surface 102 and a second surface 103; applying the enamel coating 104 as claimed in claim 1 on one of the surfaces of the glass substrate, wherein the enamel comprises pigments, inorganic component, diluents and high temperature degradable polymeric organic binder; drying in an infrared oven for a duration not exceeding 20 minutes at a temperature of less than 250 °C; and heat treating the enamel coated glass substrate 101 at a temperature of about 600 to 750 °C; wherein the enamel coating 104 once cured and fired forms a coating with uniformly scattered voids 105.15) The method as claimed in claim 14, wherein the enamel coating 104 is applied over the glass substrate by screen printing, embossed roller coating, digital printing, curtain coating, gravure coating, ink-jetting, spray painting or dip coating.16) The method as claimed in claim 14, wherein the heat treatment causes the inorganic component and the polymeric binder of the enamel to concurrently fuse and thermally degrade.17) The method as claimed in claim 14, wherein the voids 105 formed in the coating post curing contain entrapped organic vapor from the pyrolysis of the organic binder.18) The method as claimed in claim 14, wherein the voids 105 act as light scattering sites which provide improved opacity.

Citation Information

Patent Citations

  • A patterned functionally coated glass article

    WO2020065664A1

  • A heat treatble glass article with an enamel coating