Method for producing laminate and laminate

The laminate is designed with a hydrogel layer that adheres only in specific regions to the base material, allowing for controlled swelling and shape change, addressing the fragility and handling issues of previous hydrogel laminates, and enabling their use in diverse applications.

WO2024218855A1PCT designated stage expired Publication Date: 2024-10-24NT T INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/015453
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-18
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Existing hydrogel laminates used for simulating biological tissues are prone to damage and difficult to handle, necessitating a method for manufacturing a more robust and manageable laminate with reduced fragility.

Method used

A laminate is created by forming a pattern of adhesive functional groups on a substrate, applying a hydrogel precursor solution, and polymerizing it, while using a silane coupling agent and a mask film to create a base material with specific through holes and a hydrogel layer that adheres only in certain regions, allowing for controlled swelling and shape change.

Benefits of technology

The resulting laminate is easier to handle and less prone to damage, with a hydrogel layer that can swell and change shape in response to stimuli, enabling its use in various applications such as medicine and robotics without compromising structural integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023015453_24102024_PF_FP_ABST
    Figure JP2023015453_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a method for producing a laminate. The method comprises a step for forming a pattern of an adhesive functional group on one side of a substrate, a step for applying a precursor solution containing a hydrogel precursor to cover the pattern of the adhesive functional group, and a step for polymerizing the precursor. The precursor has an adhesive functional group and a polymerizable functional group. The step for forming the pattern includes a step for forming a surface treatment layer on one side using a silane coupling agent including the adhesive functional group, a step for bonding a mask film having a first opening portion onto the surface treatment layer, a step for removing the surface treatment layer exposed through the first opening portion, and a step for removing a portion of the mask film in an annular pattern along the first opening portion to form a second opening portion in the mask film.
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing laminate and laminate

[0001] The present invention relates to a method for manufacturing a laminate and a laminate.

[0002] Hydrogels are swollen materials containing polymeric materials with a three-dimensional network structure, with most of their volume filled with a solvent. The solvent typically contained in hydrogels is water. Hydrogels are known to exhibit properties such as a low coefficient of friction, high flexibility, and the ability to transmit substances through the solvent contained within.

[0003] The properties of hydrogels are similar to those of biological tissues. Therefore, hydrogels have attracted attention as materials with high affinity for living organisms. If hydrogels could be engineered into three-dimensional structures similar to those of biological tissues, or into structures that dynamically change shape in response to external stimuli, they could be used in a wide range of fields, including medicine, cell culture, and robotics.

[0004] Examples of "three-dimensional shapes similar to biological tissue" include hollow or channel-like shapes like blood vessels and curved shapes. Also, examples of "structures whose shape changes dynamically in response to external stimuli" include structures whose shape changes in response to changes in water content or osmotic pressure.

[0005] The inventors have previously proposed a laminate that uses a hydrogel as a forming material and that can obtain a hollow, flow-channel structure (see Patent Document 1). The laminate shown in Patent Document 1 is expected to be used in research and development, for example, as a model of biological tissue.

[0006] Japanese Patent Application Laid-Open No. 2020-062843

[0007] In the structure described in Patent Document 1, the structure made of hydrogel is easily damaged. Therefore, there has been a demand for a laminate that is easier to handle. There has also been a demand for a manufacturing method capable of manufacturing such a laminate.

[0008] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a novel laminate that is easy to handle and is less likely to break, as well as a method for producing such a laminate.

[0009] In order to solve the above-mentioned problems, one aspect of the present invention provides a method for manufacturing a laminate, comprising the steps of: forming a pattern of adhesive functional groups on one surface of a substrate; applying a precursor solution containing a hydrogel precursor so as to cover the pattern of adhesive functional groups; and polymerizing the precursor, wherein the precursor has a functional group polymerizable with the adhesive functional group; and the step of forming the pattern comprises the steps of forming a surface treatment layer on the one surface using a silane coupling agent having the adhesive functional group; laminating a mask film having a first opening onto the surface treatment layer; removing the surface treatment layer exposed from the first opening; and removing a portion of the mask film in a ring shape along the first opening to form a second opening in the mask film.

[0010] In addition, in order to solve the above-mentioned problems, one aspect of the present invention provides a laminate comprising a substrate and a gel layer formed on an upper surface of the substrate, the substrate having a first through hole and a second through hole penetrating the substrate in the thickness direction, the interface between the substrate and the gel layer having an adhesive region where the substrate and the gel layer are adhered to each other, and a non-adhesive region that is surrounded by the adhesive region in a closed ring shape in a planar view and where the substrate and the gel layer are not adhered to each other, the first through hole and the second through hole each opening into the non-adhesive region, and the substrate is exposed around the gel layer.

[0011] According to the present invention, it is possible to provide a novel laminate that is easy to handle and is prevented from being broken, and also to provide a method for producing such a laminate.

[0012] FIG. 1 is a perspective view of a laminate 10 of this embodiment. FIG. 2 is a cross-sectional view taken along line II-II in FIG. 1. FIG. 3 is a schematic perspective view of the laminate 10. FIG. 4 is a cross-sectional view taken along line IV-IV in FIG. 3. FIG. 5 is a cross-sectional view of the flow channel device 1 taken along line V-V in FIG. 3. FIG. 6 is a process diagram illustrating a method for manufacturing a laminate. FIG. 7 is a process diagram illustrating a method for manufacturing a laminate. FIG. 8 is a process diagram illustrating a method for manufacturing a laminate. FIG. 9 is a process diagram illustrating a method for manufacturing a laminate.

[0013] The laminate and the method for manufacturing the laminate according to this embodiment will be described below with reference to Figures 1 to 9. Note that in all the following figures, the dimensions and proportions of the components are appropriately changed to make the drawings easier to understand.

[0014] In the following explanation, an xyz Cartesian coordinate system is set, and the positional relationships of the components are explained with reference to this xyz Cartesian coordinate system. Here, a predetermined direction in a horizontal plane is defined as the x-axis direction, a direction perpendicular to the x-axis direction in the horizontal plane is defined as the y-axis direction, and a direction perpendicular to both the x-axis and y-axis directions (i.e., the vertical direction) is defined as the z-axis direction.

[0015] Furthermore, "up" refers to the +z direction, which is vertically upward, and "down" refers to the -z direction, which is vertically downward.

[0016] In the following description, "planar view" refers to viewing an object from vertically above (+z side) downward (-z direction).

[0017] 1 is a perspective view of a laminate 10 according to this embodiment. The laminate 10 includes a substrate 11 and a gel layer 12.

[0018] (Substrate) The substrate 11 supports the gel layer 12. The modulus of rigidity of the substrate 11 is different from the modulus of rigidity of the gel layer 12. For example, the modulus of rigidity of the substrate 11 is higher than the modulus of rigidity of the gel layer 12.

[0019] As long as the effects of the invention are not impaired, various materials, whether organic or inorganic, can be selected as the material for forming the substrate 11. The substrate 11 may or may not be optically transparent.

[0020] Examples of organic materials that form the substrate 11 include polymeric materials and elastomers. Examples of polymeric materials include thermoplastic resins such as polyvinyl chloride, polystyrene, ABS resin, and polylactic acid, and thermosetting resins such as polyimide and phenolic resin. Examples of elastomers include polysilicone and synthetic rubber.

[0021] The substrate 11 may be subjected to various processes by known microfabrication techniques on at least one of the surface and the interior thereof. For example, the substrate 11 may have irregularities or grooves on the surface.

[0022] The substrate 11 also has first through holes 111 and second through holes 112 that penetrate in the thickness direction (z-axis direction) of the substrate 11. In Fig. 1 , the substrate 11 is shown as having three first through holes 111 and three second through holes 112. The number of first through holes 111 and second through holes 112 is not limited to this as long as the number of first through holes 111 and second through holes 112 is the same, and may be one each, or may be a number other than three.

[0023] 1, the first through holes 111 are arranged at equal intervals in the y direction on the +x side of the substrate 11. The second through holes 112 are arranged at equal intervals in the y direction on the −x side of the substrate 11.

[0024] (Gel Layer) The gel layer 12 is made of hydrogel and is provided on one surface 11a of the substrate 11. The gel layer 12 is provided to overlap a pair of a first through hole 111 and a second through hole 112 that are aligned in the x-axis direction, and one surface 11a of the substrate 11 is exposed around the gel layer 12. That is, in the laminate 10, three gel layers 12 are formed in the shape of strips extending in the x-axis direction.

[0025] Examples of polymeric materials that make up hydrogels include water-soluble polymers such as polyacrylamide and polyvinyl alcohol, polysaccharides such as chitosan and alginic acid, and proteins such as collagen and albumin. These materials have a three-dimensional network structure and swell by absorbing a solvent to fill most of their volume. A typical solvent that swells the polymeric materials that make up hydrogels is water.

[0026] The material for forming the gel layer 12 may be a stimuli-responsive gel that can adjust its swelling degree in response to an external stimulus.

[0027] For example, gels that respond to heat (thermoresponsive gels) include gels made of poly(N-isopropylacrylamide) and poly(methyl vinyl ether). A photothermal conversion material (metal nanomaterials, carbon nanomaterials, conductive polymers, etc.) may be dispersed in the thermoresponsive gel, and the heat generated by light irradiation may be used as a trigger to cause the gel to respond to stimuli.

[0028] Gels that respond to pH (pH-responsive gels) include gels made of polyelectrolytes synthesized from anionic or cationic monomers.

[0029] Gels that respond to light (photoresponsive gels) include gels made of polymers with spiropyran or azobenzene in the skeleton. Photoresponsive gels may incorporate a mechanism that changes the degree of swelling in response to light stimulation, using an inclusion complex of azobenzene and cyclodextrin as a crosslinking point.

[0030] Other examples of materials for forming the gel layer 12 include molecularly imprinted gels in which specific molecules bound to the hydrogel skeleton serve as crosslinking points in the gel network. Examples of protein-responsive gels include biomolecular crosslinked gels in which biomolecular complexes serve as crosslinking points in the gel network, and antigen-responsive gels in which antigen-antibody complexes are introduced into the network as crosslinking points in the gel.

[0031] The material for forming the gel layer 12 may be a mixture of these polymer materials to form a hydrogel that responds to multiple stimuli. Furthermore, the material for forming the gel layer 12 may also be a tough hydrogel such as a double network gel, a slide-ring gel, a Tetra-PEG gel, or a nanoclay gel.

[0032] Various known methods can be used to synthesize the polymer material that constitutes the hydrogel. For example, when the polymer material that constitutes the hydrogel is an acrylic polymer material, a three-dimensional network structure may be formed by crosslinking acrylic groups during polymerization of acrylic monomers.

[0033] The type of polymerization reaction when polymerizing the acrylic monomer is not particularly limited, but an example thereof is radical polymerization using a water-soluble photopolymerization initiator. Examples of the water-soluble photoinitiator include 2-oxoglutaric acid, 4'-(2-hydroxyethoxy)-2-hydroxy-2-methylpropiophenone (trade name: Irgacure 2959), lithium phenyl(2,4,6-trimethylbenzoyl)phosphinate (abbreviation: LAP), and 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide] (trade name: VA-086).

[0034] During radical polymerization, a deoxidizer may be added to the reaction system to prevent polymerization inhibition by oxygen. Examples of the deoxidizer include a combination of glucose and glucose oxidase. Radical polymerization may also be carried out under an inert gas atmosphere such as nitrogen or argon.

[0035] When the polymeric material constituting the hydrogel is a polysaccharide or a protein, the three-dimensional network structure may be formed by physical bonding of the polysaccharide or protein, or by crosslinking the polysaccharide or protein using a crosslinking agent, such as glutaraldehyde.

[0036] The shape of the gel layer 12 is not particularly limited, and various shapes can be selected depending on the usage form. For example, the gel layer 12 may be in the form of a film, a plate, a block, etc. Among these, the shape of the gel layer 12 is preferably in the form of a film.

[0037] The thickness of the gel layer 12 is not particularly limited, but is preferably a thickness that provides sufficient structural strength to prevent the gel layer 12 from collapsing under its own weight. For example, when a hydrogel containing polyacrylamide is used as the material for forming the gel layer 12, the thickness of the gel layer 12 is preferably 50 μm to 1000 μm, and more preferably 120 μm to 200 μm.

[0038] The strength of the gel layer 12 can be improved by increasing the crosslinking of the polymer material that constitutes the hydrogel by chemical crosslinking or physical crosslinking, or by increasing the concentration of the polymer material that constitutes the hydrogel.

[0039] For example, when preparing a hydrogel containing polyacrylamide by polymerizing acrylamide monomers (precursors), the monomer concentration is preferably 0.8 mol / L to 8 mol / L, more preferably 2 mol / L to 4 mol / L.

[0040] Furthermore, when methylenebisacrylamide is used as a chemical crosslinking agent when polymerizing acrylamide monomers, the concentration of the crosslinking agent is preferably 0.01 mol % to 2.0 mol % relative to the monomer, and more preferably 0.03 mol % to 1 mol %.

[0041] Hydrogels can contain various additives. The type of additive is not particularly limited as long as it does not inhibit hydrogel formation. Examples of additives include biomolecules that improve biocompatibility, silver nanoparticles or surfactants that exhibit antibacterial properties, ionic liquids or conductive polymers that increase conductivity, and magnetic nanoparticles that react to magnetic fields. Adding these additives to hydrogels can impart desired functions to the hydrogels.

[0042] (Interface Structure) Figure 2 is a cross-sectional view taken along line II-II in Figure 1. As shown in Figure 2, laminate 10 has, at the interface between substrate 11 and gel layer 12, adhesive region 10a where substrate 11 and gel layer 12 are adhered to each other, and non-adhesive region 10b where substrate 11 and gel layer 12 are not adhered to each other.

[0043] The non-adhesive region 10b is formed in a band shape extending in the x-axis direction and is surrounded by the adhesive region 10a in a closed ring shape in plan view. The shape of the non-adhesive region 10b is an example, and various shapes can be used depending on the design.

[0044] A layer 121 of a silane coupling agent having adhesive functional groups is formed in the adhesive region 10a. The "adhesive functional groups" refer to functional groups that can polymerize with the monomers (precursors) of the polymeric material that constitutes the hydrogel. In the adhesive region 10a, the gel layer 12 is bonded to the adhesive functional groups of the layer 121.

[0045] For example, when an acrylic monomer is used as the monomer, the adhesive functional group can be a (meth)acrylic group, and in this case, the silane coupling agent can be, for example, 3-(methacryloyloxy)propyltrimethoxysilane.

[0046] The first through-hole 111 and the second through-hole 112 each open to the non-adhesive region 10b.

[0047] 3 to 5 show the state in which the gel layer 12 of the laminate 10 has been swollen. FIG. 3 is a schematic perspective view of the laminate 10, and corresponds to FIG. 1. FIG. 4 is a cross-sectional view taken along line IV-IV in FIG. 3, and corresponds to FIG. 2. FIG. 5 is a cross-sectional view of the flow channel device 1 taken along line V-V in FIG. 3. In the following description, the swollen gel layer is designated by the reference numeral 15.

[0048] 3 to 5 , the gel layer 15 is not fixed to the substrate 11 in the non-adhesive region 10b. The gel layer 15 is fixed to the substrate 11 in the adhesive region 10a. Therefore, the portion of the gel layer 15 that overlaps with the non-adhesive region 10b in a planar manner can freely increase in volume in the extension direction of the non-adhesive region 10b and in a direction away from the substrate 11 when the volume increases due to swelling. On the other hand, the portion of the gel layer 15 that overlaps with the non-adhesive region 10b in a planar manner is restricted from increasing in volume in a direction intersecting the extension direction of the non-adhesive region 10b.

[0049] As a result, in order to mitigate the increase in internal pressure due to the increase in volume, the portion of gel layer 15 that overlaps non-adhesive region 10b in plan view swells and deforms significantly in the direction away from substrate 11. As a result, a tubular flow path 10x surrounded by gel layer 15 and substrate 11 is formed in laminate 10.

[0050] The shape of the flow channel 10x can be controlled by controlling the pattern shapes of the adhesive region 10a and the non-adhesive region 10b.

[0051] The shape of the flow channel 10x can be controlled by adjusting the type of gel layer 15, the modulus of rigidity of the gel layer 15, the thickness of the gel layer 15, etc. The modulus of rigidity and the swelling rate of the gel layer 15 can be controlled by changing the type of monomer of the polymer material constituting the gel layer 15, the type and amount of the cross-linking agent used, etc.

[0052] The change in shape described above occurs due to the difference in the swelling rate of the gel layer 12 before swelling and the swelling rate of the gel layer 15 after swelling. The change between the gel layer 12 and the gel layer 15 is reversible. Therefore, in the flow channel device 1, the shape of the flow channel 10x can be controlled by controlling the swelling rate of the gel layer. The swelling rate of the gel layer can be controlled by bringing the gel layer into contact with water to cause swelling, drying the gel layer, or the like.

[0053] In such a laminate 10, when connecting piping to the flow path 10x, it is not necessary to directly connect the piping to the flow path 10x made of hydrogel by connecting the piping to the first through-hole 111 and the second through-hole 112 of the substrate 11. Therefore, damage to the flow path 10x (damage to the gel layer 15) can be suppressed.

[0054] The laminate 10 having the above-described configuration can provide a novel device that is easy to handle and is less susceptible to breakage.

[0055] <<Laminate Manufacturing Method>> Figures 6 to 9 are process diagrams illustrating a laminate manufacturing method. Figures 6 to 8 are explanatory diagrams of the "pattern forming step" of the present invention, and Figure 9 is an explanatory diagram of the "precursor solution applying step" and the "precursor polymerizing step" of the present invention.

[0056] First, as shown in FIG. 6, one surface of the substrate 11 is treated with a silane coupling agent S to form a layer of the silane coupling agent (surface treatment layer) on the one surface 11a (step of forming a surface treatment layer).

[0057] The base material 11 has a plurality of (three in the drawing) first through holes 111 penetrating the base material 11 in the thickness direction, and the same number of second through holes 112 as the first through holes 111 .

[0058] The silane coupling agent used herein is a silane coupling agent having an adhesive functional group. In this specification, the term "adhesive functional group" refers to a functional group that can polymerize with a monomer (precursor) of the polymer material that constitutes the hydrogel.

[0059] For example, when an acrylic monomer is used as the monomer, the adhesive functional group can be a (meth)acrylic group, and in this case, the silane coupling agent can be, for example, 3-(methacryloyloxy)propyltrimethoxysilane.

[0060] The surface treatment layer formed is a monomolecular layer of a silane coupling agent, and adhesive functional groups are introduced into the surface 11 a of the substrate 11 by the surface treatment layer.

[0061] Next, as shown in FIG. 7, a mask film 50 having first openings 50a is attached to the surface treatment layer of the first surface 11a (attaching step).

[0062] The mask film 50 has the same number of first openings 50a as the number of first through holes 111. The first openings 50a are strip-shaped and extend in the x-axis direction, and are formed in three locations. In addition, the mask film 50 has a circular cutting line 50x formed along the first openings 50a.

[0063] In this step, the mask film 50 is attached while exposing the first through holes 111 and the second through holes 112 from the plurality of first openings 50 a, respectively. One surface of the base material 11, more specifically, the surface treatment layer provided on the one surface, is exposed from the first openings 50 a.

[0064] The mask film 50 may be made of, for example, a known backgrind tape.

[0065] Thereafter, the surface treatment layer exposed from the first opening 50a is removed (removing step). Specifically, oxygen plasma treatment is performed using oxygen plasma O on one surface (surface treatment layer) of the base material exposed through the first opening 50a via the mask film 50. This removes the surface treatment layer (silane coupling agent) exposed in the first opening 50a. Other methods for removing the surface treatment layer include ashing using ozone decomposed by ultraviolet light and vapor-phase etching of glass using a fluorine-based gas.

[0066] Next, as shown in FIG. 8, a portion 501 of the mask film 50 is removed in a ring shape along the first opening 50a to form a second opening 50b in the mask film 50 (step of forming a second opening).

[0067] The portion 501 of the mask film 50 is formed by cutting the mask film 50 along the cutting line 50x. As a result, two types of regions are formed in the area exposed from the second opening 50b: a first region 11x where the portion 501 of the mask film 50 overlapped, and a second region 11y where the surface treatment layer has been removed. The surface treatment layer remains in the first region 11x. The surface treatment layer remaining in the first region 11x corresponds to the above-mentioned layer 121.

[0068] 9, an easily removable tape (not shown) is applied to the bottom surface (the surface opposite to the surface 11a) of the substrate 11 to block the first through-holes 111 and the second through-holes 112, and then a monomer solution of a polymer material constituting the hydrogel is dripped onto the area exposed from the second opening 50b (a precursor solution application step). The monomer solution corresponds to the precursor solution of the present invention.

[0069] The monomer solution contains a monomer of the polymer material constituting the hydrogel described above, a photopolymerization initiator, and, if necessary, an organic solvent. The monomer used has a functional group that can polymerize with the adhesive functional group contained in layer 121. For example, an acrylic monomer having an acrylic group can be used as the monomer contained in monomer solution 20A.

[0070] Examples of organic solvents that may be contained in the monomer solution include dimethyl sulfoxide (DMSO), dimethylformamide (DMF), dimethylacetamide (DMA), and ethylene carbonate (EC).

[0071] Next, a glass substrate (not shown) is placed on top of the mask film 50. As a result, excess monomer solution is discharged from the substrate 11, and the monomer solution remains only in the space surrounded by the substrate 11, the mask film 50, and the glass substrate.

[0072] Next, the monomer solution is irradiated with ultraviolet light to polymerize the precursor (precursor polymerizing step). The peak wavelength of the irradiated ultraviolet light is included in the absorption wavelength band of the photopolymerization initiator contained in the monomer solution. The peak wavelength of the ultraviolet light is, for example, 365 nm.

[0073] The ultraviolet irradiation polymerizes the monomers contained in the monomer solution, yielding a polymeric material. At this time, functional groups of the monomers polymerize with adhesive functional groups of the silane coupling agent in the first region 11x (layer 121), causing the monomer solution overlapping the layer 121 to adhere to the surface 11a of the substrate 11. In contrast, in the second region 11y of the substrate 11 where the layer 121 is not formed, the monomers contained in the monomer solution polymerize with each other without bonding to the substrate 11.

[0074] As a result, the gel layer 12 is formed so as to overlap the second opening 50b. The thickness of the gel layer 12 is the same as the gap between the base material 11 and the glass substrate, i.e., the same as the thickness of the mask film 50. The mask film 50 may be peeled off as necessary (a step of removing the mask film).

[0075] Either before or after peeling off the mask film 50, the polymer of the monomer solution is immersed in a large excess of pure water to remove unreacted monomers and to cause the polymer material produced by polymerization to swell with water, thereby obtaining a gel layer 15 in which the polymer material is swollen with water.

[0076] Furthermore, the portions of gel layer 15 that overlap layer 121 become adhesive regions 10a, and the portions of gel layer 15 that do not overlap layer 121 become non-adhesive regions 10b. As described above, the portions of gel layer 15 that overlap non-adhesive regions 10b of the hydrogel layer deform depending on the degree of swelling, and flow channels 10x are formed. In this manner, laminate 10 is obtained.

[0077] The laminate 10 having the above-described configuration can provide a novel device that is easy to handle and is less susceptible to breakage.

[0078] Furthermore, according to the method for manufacturing a laminate as described above, the above-mentioned laminate can be easily manufactured.

[0079] While the preferred embodiments of the present invention have been described above with reference to the accompanying drawings, the present invention is not limited to these examples. The shapes and combinations of the components shown in the above examples are merely examples, and various modifications can be made based on the design, specifications, etc., without departing from the spirit of the present invention.

[0080] DESCRIPTION OF SYMBOLS 10...Laminate, 10a...Adhesive region, 10b...Non-adhesive region, 11...Substrate, 11a...One surface, 12, 15...Gel layer, 50...Mask film, 50a...First opening, 50b...Second opening, 111...First through hole, 112...Second through hole, 121...Layer, O...Oxygen plasma, S...Silane coupling agent

Claims

1. A method for manufacturing a laminate, comprising: forming a pattern of adhesive functional groups on one surface of a substrate; applying a precursor solution containing a hydrogel precursor to cover the pattern of adhesive functional groups; and polymerizing the precursor, the precursor having a functional group polymerizable with the adhesive functional group; the pattern-forming step comprising: forming a surface treatment layer on the one surface using a silane coupling agent having an adhesive functional group; laminating a mask film having a first opening onto the surface treatment layer; removing the surface treatment layer exposed from the first opening; and removing a portion of the mask film in a ring shape along the first opening to form a second opening in the mask film.

2. A method for manufacturing a laminate as described in claim 1, wherein the substrate has a first through hole and a second through hole penetrating in a thickness direction of the substrate, and in the bonding step, the mask film is bonded while exposing the first through hole and the second through hole from the first opening.

3. A method for manufacturing a laminate as described in claim 2, wherein the mask film has a plurality of first through holes and a number of second through holes equal to the number of the first through holes, the mask film has a number of first openings equal to the number of the first through holes, and in the bonding step, the mask film is bonded while exposing the first through holes and the second through holes in each of the first openings.

4. A method for producing a laminate according to any one of claims 1 to 3, wherein in the removing step, an oxygen plasma treatment is performed on one side of the substrate through the mask film.

5. A method for producing a laminate according to any one of claims 1 to 4, further comprising a step of removing the mask film after the polymerization step.

6. A laminate comprising: a substrate; and a gel layer formed on an upper surface of the substrate, the substrate having a first through hole and a second through hole penetrating the substrate in a thickness direction; at the interface between the substrate and the gel layer, there is formed an adhesive region where the substrate and the gel layer are adhered to each other, and a non-adhesive region which is surrounded by the adhesive region in a closed ring shape in a plan view and where the substrate and the gel layer are not adhered to each other; the first through hole and the second through hole each open into the non-adhesive region; and the substrate is exposed around the gel layer.

Citation Information

Patent Citations

  • Suspended optical waveguide and preparation method thereof

    CN111061009A

  • Temperature responsive valve and its manufacturing method

    JP2007170469A

  • Microchannels with open and / or closed and / or pumping devices

    JP2015511181A

  • Microfluidic transportation structure where through hole and flow channel are integrated, and method for manufacturing the same

    JP2018130676A

  • Cross-linked polymer structure and use thereof

    JP2018148918A