Polyamide resin composition

The polyamide resin composition, featuring an aliphatic polyamide resin with a high methylene-to-amide group ratio and reactive polyolefin, addresses moldability and hydrolysis resistance issues, ensuring durable and compatible tubes for coolant transport.

WO2024219100A1PCT designated stage expired Publication Date: 2024-10-24UBE CORPORATION

Patent Information

Application Number
PCT/JP2024/008579
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-21
Filing Date
2024-03-06
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Polyamide resins used in coolant tubes face challenges with moldability and hydrolysis resistance, particularly in multi-layer tubes where interlayer adhesion is poor and compatibility issues arise, limiting their durability and suitability for automotive piping applications.

Method used

A polyamide resin composition comprising an aliphatic polyamide resin with a high methylene-to-amide group ratio and a polyolefin with reactive functional groups, optimized for molecular weight distribution and terminal group concentrations, to enhance moldability and hydrolysis resistance.

Benefits of technology

The composition achieves excellent moldability and hydrolysis resistance, making it suitable for producing durable tubes that can transport coolants, even in the presence of water, with improved interlayer adhesion and compatibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024008579_24102024_PF_FP_ABST
    Figure JP2024008579_24102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a polyamide resin composition containing an aliphatic polyamide resin and a polyolefin exhibiting reactivity with a terminal group of the polyamide resin, wherein: the aliphatic polyamide resin has a portion derived from a linear or branched hydrocarbon compound at a proportion of 80 mol% or more in all monomer units; and, in the aliphatic polyamide resin, the ratio of the high molecular weight component to the low molecular weight component is within a specific range in the molecular weight distribution curve of the polymethyl methacrylate equivalent. According to this resin composition, a resin composition having excellent moldability and high hydrolysis resistance is provided.
Need to check novelty before this filing date? Find Prior Art

Description

Polyamide resin composition

[0001] The present invention relates to a polyamide resin composition that is particularly useful for use as a coolant tube.

[0002] In the past, the main material for automotive piping tubing has been replaced by lightweight resins with excellent rust resistance, due to issues such as rust caused by road deicing agents, as well as the need to prevent global warming and conserve energy. Resins typically used for piping tubing include polyamide resins, saturated polyester resins, polyolefin resins, and thermoplastic polyurethane resins. Polyamide resins, among others, offer excellent properties such as gas barrier properties, toughness, pinhole resistance, heat resistance, and oil resistance, and are expected to provide tubing with excellent resistance to alcohols such as ethylene glycol contained in coolants.

[0003] Automotive piping tubes, such as coolant tubes, are required to have many properties, including durability against chemicals, temperature, and impact, as well as moldability into a tube. For resins such as polyamide, compositions that meet the required properties can be designed by rearranging the monomer units, blending with other polymers in some cases, or using different materials for the inner and outer layers (Patent Documents 1 to 4). Furthermore, because polymers are a collection of components with different molecular weights, controlling the molecular weight is also used as a means of controlling the properties (Patent Document 5).

[0004] International Publication No. 2015 / 033982 JP 57-147519 A JP 2008-507436 A JP 63-170460 A JP 2015-110764 A

[0005] Polyamide resins are highly useful as molding resins due to their flexibility in molecular structure design and the inherent physical properties of polyamides. However, when designing polymer molecules, there is often a trade-off between two or more physical properties. For example, the resin described in Patent Document 5 exhibits high fluidity, but there is still room for improvement in terms of moldability. Furthermore, from the perspective of moldability, resins for injection molding are not necessarily suitable for tube molding; resins must have moldability suited to the article to be manufactured or its purpose. Furthermore, polyamides contain amide bonds (-NHCO-) ​​as structural units, which can result in insufficient hydrolysis resistance. As in Patent Document 3, attempts have been made to use resins other than polyamides for the inner layer of tubes. However, in the case of tubes composed of multiple layers, high adhesion between the layers is required, and there is still room for improvement in the durability resulting from interlayer adhesion. Even when using a mixture of polymers as in Patent Document 4, it is impossible to prevent polyamides from coming into contact with water, and compatibility between polymers is also an issue, making it difficult to formulate a suitable resin composition.

[0006] From the viewpoint of weight reduction and resource conservation, there is always a demand for resins that have moldability that allows molding even with a small amount of resin used and a small thickness, and that have high durability even with a small thickness. From such a viewpoint, an object of the present invention is to provide a resin composition that has excellent moldability and high hydrolysis resistance.

[0007] The present invention relates to a resin composition or various molded articles using the same, as described in the following items: [1] A polyamide resin composition comprising an aliphatic polyamide resin and a polyolefin having a functional group reactive with an end group of the polyamide resin, wherein the aliphatic polyamide resin has a moiety derived from a linear or branched hydrocarbon compound of 80 mol % or more of all monomer units thereof, the mass ratio of the polyolefin content (B) to the total mass of the aliphatic polyamide resin content (A) and the polyolefin content (B) [(B) / {(A)+(B)}] is 0.15 to 0.40, and the aliphatic polyamide resin has the following characteristics in a molecular weight distribution curve calculated as polymethyl methacrylate: When the weight fraction of the mode of the molecular weight distribution curve is taken as 100%, S1 is the area of ​​the portion sandwiched between the molecular weight distribution curve from the highest molecular weight point among points corresponding to a weight fraction of 70% to the maximum molecular weight point and the horizontal axis corresponding to a weight fraction of 0%, and S2 is the area of ​​the portion sandwiched between the molecular weight distribution curve from the lowest molecular weight point among points corresponding to a weight fraction of 70% to the minimum molecular weight point and the horizontal axis corresponding to a weight fraction of 0%, the value of [{S2 / (S2+S1)}×100] is 64 to 90. [2] The polyamide resin composition according to [1] above, wherein the MFR measured when a 5,000 g quantity of the polyamide resin composition is heated to 300° C. in accordance with ISO 1133 is 0.01 g / 10 min or more and 20 g / 10 min or less. [3] The polyamide resin composition according to [1] or [2], wherein the amount of functional groups per 1 g of the polyolefin [C1] is more than 25 μmol / g and less than 100 μmol / g, and the amount of amino groups per 1 g of the aliphatic polyamide resin [A1] is more than 25 μmol / g and less than 100 μmol / g. [4] When the amount of functional groups in the polyolefin and the amount of amino groups in the aliphatic polyamide resin contained in 1 g of the polyamide resin composition are [C2] and [A2], respectively, the product [C2] x [A2] is 250 to 750 ((μmol / g) 2[5] The polyamide resin composition of any of [1] to [4] above, wherein the ratio [CH2] / [NHCO] of the number of methylene groups ([CH2]) to the number of amide groups ([NHCO]) in the aliphatic polyamide resin exceeds 5 on average. [6] The polyamide resin composition of any of [1] to [5] above, wherein the aliphatic polyamide resin comprises at least one selected from the group consisting of PA11, PA12, PA69, PA610, PA612, PA910, PA912, PA1010, PA1012, and PA1212. [7] The polyamide resin composition of any of [1] to [6] above, wherein the polyolefin has at least one functional group selected from the group consisting of a carboxy group, an acid anhydride group, a carboxylic acid ester group, a carboxylic acid imide group, a carboxylic acid amide group, and an epoxy group, or a salt thereof. [8] The polyamide resin composition of any of [1] to [7] above, wherein the polyolefin is at least one selected from the group consisting of copolymers having an (ethylene and / or propylene) / α-olefin copolymer as a main skeleton, at least a portion of which has a functional group reactive with an end group of an aliphatic polyamide resin, and (ethylene and / or propylene) / (α,β-unsaturated carboxylic acid and / or α,β-unsaturated carboxylic acid ester) copolymer. [9] The polyamide resin composition of any of [1] to [8] above, wherein the weight average molecular weight (Mw) of the polyamide resin is 50,000 to 80,000.

[10] The polyamide resin composition of any of [1] to [9] above, which is used for a blown molded article for transporting a coolant.

[11] A tube, hose, or pipe comprising the polyamide resin composition of any of [1] to [9] above.

[12] A blown molded article having a single-layer structure made of the polyamide resin composition of any of [1] to [9] above.

[0008] The present invention provides a polyamide resin composition having excellent moldability and high hydrolysis resistance, which can be used to produce molded articles such as tubes, hoses, and pipes that are particularly suitable for transporting coolants.

[0009] FIG. 1 is a schematic diagram of a GPC chart of an aliphatic polyamide resin.

[0010] The polyamide resin composition of the present invention will be described in detail below for each of its constituent components. In this specification, when a plurality of substances corresponding to each component are present in the composition, the content of each component refers to the total amount of the plurality of substances present in the composition, unless otherwise specified. In this specification, the symbol "to" indicating a numerical range means that the numerical values ​​before and after it are included as the lower and upper limits. For example, "50.00 to 90.00 mass%" means "50.00 mass% or more and 90.00 mass% or less."

[0011] <Aliphatic Polyamide Resin> Aliphatic polyamide resins are polymers having an amide bond (—NHCO—) in the main chain containing an aliphatic hydrocarbon group. Aliphatic polyamide resins are obtained by polymerizing or copolymerizing lactams, aminocarboxylic acids, or aliphatic diamines and aliphatic dicarboxylic acids, which are structural units of aliphatic polyamides, using known methods such as melt polymerization, solution polymerization, and solid-state polymerization. Herein, "aliphatic polyamide resin" refers to a polyamide resin essentially composed of monomer units derived from linear or branched hydrocarbon compounds. While this does not exclude the polyamide resin from containing monomer units derived from alicyclic structures or cyclic compounds such as aromatic hydrocarbons, the content of such monomer units in the aliphatic polyamide resin of the present invention is 20 mol % or less of the total monomer units. The aliphatic polyamide resin of the present invention is a polyamide resin in which 80 mol % or more of the total monomer units are derived from linear or branched hydrocarbon compounds, and preferably a polyamide resin composed of monomer units derived from linear or branched hydrocarbon compounds.

[0012] (Methylene Group Number / Amide Group Number Ratio) The aliphatic polyamide resin used in the present invention preferably has a ratio [CH2] / [NHCO] of the number of methylene groups ([CH2]) to the number of amide groups ([NHCO]) of more than 5 on average. The number of methylene groups can be determined from the raw materials, lactam, aminocarboxylic acid, aliphatic diamine, and aliphatic dicarboxylic acid. When a branched hydrocarbon compound is contained in the monomer unit of the polyamide resin, the number of methylene groups is calculated by regarding the carbon atom at the branch point of the carbon chain and the methyl group at the branch chain end as methylene groups. Generally, when lactam or aminocarboxylic acid is used as the raw material, the number of methylene groups contained in the lactam or aminocarboxylic acid is the methylene group number / amide group number ratio. When aliphatic diamine and aliphatic dicarboxylic acid are used as the raw materials, the sum of the number of methylene groups contained in the aliphatic diamine and the aliphatic dicarboxylic acid divided by 2 is the methylene group number / amide group number ratio. Without being bound by any particular theory, it is believed that when the methylene group number / amide group number ratio exceeds a certain value, the proportion of methylene chains in the polyamide resin increases. It is believed that the inclusion of a large number of hydrophobic aliphatic hydrocarbon groups enhances hydrophobicity, and furthermore, improves compatibility with polyolefins, as described below, resulting in a polyamide resin composition with higher hydrolysis resistance. The [CH2] / [NHCO] ratio is preferably 6 or more, and even more preferably 7 or more. Furthermore, while the use of long-chain polyamides with a high [CH2] / [NHCO] ratio allows for the production of molded products with superior durability, it is preferable to select raw materials for the polyamide resin so that the [CH2] / [NHCO] ratio is 12 or less, from the perspective of raw material availability and using more environmentally friendly resins.

[0013] Among the raw materials for the aliphatic polyamide resin described below, there are some monomers in which the number of methylene groups when considered alone is 5 or less. However, in a preferred embodiment of the present invention, such monomers can also be used as long as they are combined with a monomer having a larger number of methylene groups to make the ratio of the number of methylene groups to the number of amide groups exceed 5 on average.

[0014] (Raw materials for aliphatic polyamide resin) The aliphatic polyamide resin used in the present invention preferably satisfies the above-mentioned condition of the methylene group / amide group number ratio, but any raw material that is a compound having a linear or branched hydrocarbon in its molecular skeleton and is used in the production of aliphatic polyamide resins can be used. In a preferred embodiment of the present invention, even if the raw material has 5 or less methylene groups, it can be used in an amount that satisfies the above-mentioned condition for the total aliphatic polyamide resin. Examples of such compounds having a linear or branched hydrocarbon in its molecular skeleton that can be used as raw materials for polyamide resin are listed below.

[0015] Examples of lactams include caprolactam, enantholactam, undecane lactam, dodecane lactam, α-pyrrolidone, α-piperidone, etc. Examples of aminocarboxylic acids include 6-aminocaproic acid, 7-aminoheptanoic acid, 9-aminononanoic acid, 11-aminoundecanoic acid, 12-aminododecanoic acid, etc. These can be used alone or in combination of two or more.

[0016] Examples of aliphatic diamines include 1,2-ethanediamine, 1,3-propanediamine, 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine, 1,12-dodecanediamine, 1,13-tridecanediamine, 1,14-tetradecanediamine, 1,15-pentadecanediamine, 1,16 1,17-hexadecanediamine, 1,18-octadecanediamine, 1,19-nonadecanediamine, 1,20-eicosanediamine, 2-methyl-1,5-pentanediamine, 3-methyl-1,5-pentanediamine, 2-methyl-1,8-octanediamine, 2,2,4-trimethyl-1,6-hexanediamine, 2,4,4-trimethyl-1,6-hexanediamine, 5-methyl-1,9-nonanediamine, etc. These may be used alone or in combination.

[0017] Examples of the aliphatic dicarboxylic acid include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid, pentadecanedioic acid, hexadecanedioic acid, octadecanedioic acid, and eicosane diacid, and these may be used alone or in combination.

[0018] Examples of aliphatic polyamide resins that satisfy the above-mentioned condition of the methylene group / amide group number ratio include polyundecaneamide (PA11), polydodecanamide (PA12), polytetramethylene azelamide (PA49), polytetramethylene sebacamide (PA410), polytetramethylene dodecamide (PA412), polypentamethylene suberamide (PA58), polypentamethylene azelamide (PA59), polypentamethylene sebac ... Polypentamethylene sebacamide (PA510), polypentamethylene dodecamide (PA512), polyhexamethylene suberamide (PA68), polyhexamethylene azelamide (PA69), polyhexamethylene sebacamide (PA610), polyhexamethylene dodecamide (PA612), polyhexamethylene tetradecamide (PA614), polyhexamethylene hexadecamide (PA616), polyhexamethylene octadecamide (PA618), Cutadecamide (PA618), polynonameethylene adipamide (PA96), polynonameethylene suberamide (PA98), polynonameethylene azelamide (PA99), polynonameethylene sebacamide (PA910), polynonameethylene dodecamide (PA912), polydecamethylene adipamide (PA106), polydecamethylene suberamide (PA108), polydecamethylene azelamide (PA109), polydecamethylene Examples of the polyamide include homopolymers such as polydodecamethylene sebacamide (PA1010), polydecamethylene dodecamide (PA1012), polydodecamethylene adipamide (PA126), polydodecamethylene suberamide (PA128), polydodecamethylene azelamide (PA129), polydodecamethylene sebacamide (PA1210), and polydodecamethylene dodecamide (PA1212), as well as copolymers made from several of the raw materials used to form these polymers. Here, "PA" means "polyamide."

[0019] Among these, from the viewpoints of economy and availability, polyundecaneamide (PA11), polydodecanamide (PA12), polyhexamethylene azelamide (PA69), polyhexamethylene sebacamide (PA610), polyhexamethylene dodecamide (PA612), polynonamethylene decamide (PA910), polynonamethylene dodecamide (PA912), polydecamethylene sebacamide (PA1010), polydecamethylene dodecamide (PA1010), and polydecamethylene dodecamide (PA1012) are preferred. Preferred are polyundecaneamide (PA1012), polydodecanamide (PA1212), and copolymers using several of the raw materials forming these. More preferred are at least one homopolymer selected from the group consisting of polyundecaneamide (PA11), polydodecanamide (PA12), polyhexamethylenedecamide (PA610), and polyhexamethylenedodecanamide (PA612), and / or copolymers using several of the raw materials forming these.

[0020] The aliphatic polyamide resin used in the present invention preferably has a methylene group / amide group ratio of more than 5 in the entire resin, but an aliphatic polyamide or an aromatic polyamide having a methylene group / amide group ratio of 5 or less may also be used in combination. Examples of such aliphatic polyamides include polyvaleroamide (PA5), polycaproamide (PA6), polyethylene adipamide (PA26), polytetramethylene succinamide (PA44), polytetramethylene glutamide (PA45), polytetramethylene adipamide (PA46), polytetramethylene suberamide (PA48), polypentamethylene succinamide (PA54), polypentamethylene glutamide (PA55), polypentamethylene adipamide (PA56), polyhexamethylene succinamide (PA64), polyhexamethylene glutamide (PA65), polyhexamethylene adipamide (PA66), and copolymers formed from several of the raw materials used to form these. Examples of aromatic polyamides include PA4T, PA6T, PA9T, PA10T, PA6I, PAMXD6, and copolymers formed from several of the raw materials used to form these. However, the aromatic polyamide is used in an amount such that the content of the monomer unit of the aliphatic hydrocarbon compound in the polyamide resin is 80 mol % or more.

[0021] The aliphatic polyamide resin used in the present invention may be a copolymer of an aliphatic polyamide having a methylene group / amide group ratio of more than 5 and an aliphatic polyamide having a methylene group / amide group ratio of 5 or less, and is preferably designed so that the aliphatic polyamide resin as a whole has a methylene group / amide group ratio of more than 5. Examples of such copolymers include PA6 / 69, PA6 / 610, PA6 / 611, PA6 / 612, PA6 / 11, PA6 / 12, PA6 / 66 / 12, PA6 / 66 / 610, PA6 / 66 / 612, etc., which contain a high proportion of aliphatic polyamides having a methylene group / amide group ratio of more than 5.

[0022] Polyamide resins are obtained by the reaction of amino groups with carboxy groups, and therefore have amino or carboxy groups at the molecular terminals. When the amount of amino groups per gram of polyamide resin is [A1] (μmol / g) and the amount of carboxy groups per gram of polyamide resin is [B1] (μmol / g), [A1] and [B1] are preferably greater than 25 μmol / g and less than 100 μmol / g, more preferably 35 μmol / g or greater but less than 95 μmol / g, and even more preferably 40 μmol / g or greater but less than 90 μmol / g. When the polyamide resin is obtained from a lactam or aminocarboxylic acid, [B1] is approximately the same amount as [A1]. The amount of amino groups [A1] can be measured by dissolving the polyamide resin in a phenol / methanol mixed solution and titrating with 0.05 N hydrochloric acid. The amount of carboxyl group [B1] can be measured by dissolving the polyamide resin in benzyl alcohol and titrating the solution with a 0.05N sodium hydroxide solution.

[0023] Examples of equipment for producing aliphatic polyamide resins include known polyamide production equipment, such as batch-type reaction vessels, single- or multi-vessel continuous reaction vessels, tubular continuous reaction vessels, and kneading reaction extruders such as single-screw kneading extruders and twin-screw kneading extruders. Known polymerization methods, such as melt polymerization, solution polymerization, and solid-phase polymerization, can be used, and polymerization can be carried out by repeating operations under normal pressure, reduced pressure, and increased pressure. These polymerization methods can be used alone or in appropriate combination.

[0024] Aliphatic polyamide resins are produced by polymerization using the above-mentioned raw materials. For example, they are produced by polymerizing or copolymerizing the polyamide raw materials using known methods such as melt polymerization, solution polymerization, or solid-state polymerization. Here, in the production of aliphatic polyamide resins, additional amines may be added in addition to the polyamide raw materials and polymerized or copolymerized. When additional amines are added, the aliphatic polyamide resin may be produced by adding the amines after polymerization and melt-kneading. Thus, the amines can be added at any stage during polymerization or at any stage during melt-kneading after polymerization. Examples of the amines include monoamines, diamines, triamines, and polyamines. Furthermore, in addition to the amines, carboxylic acids such as monocarboxylic acids, dicarboxylic acids, and tricarboxylic acids may be added as needed, as long as the end group concentration does not deviate from the range of the above-mentioned conditions. These amines and carboxylic acids may be added simultaneously or separately. Furthermore, the amines and carboxylic acids exemplified below can be used singly or in combination. By adjusting the amounts of amines and carboxylic acids, it is possible to adjust the molecular weight, the amount of terminal amino groups, and the amount of terminal carboxy groups of the aliphatic polyamide to be produced.

[0025] Specific examples of the monoamine to be added include aliphatic monoamines such as methylamine, ethylamine, propylamine, butylamine, pentylamine, hexylamine, heptylamine, octylamine, 2-ethylhexylamine, nonylamine, decylamine, undecylamine, dodecylamine, tridecylamine, tetradecylamine, pentadecylamine, hexadecylamine, octadecylamine, octadecyleneamine, eicosylamine, and docosylamine; alicyclic monoamines such as cyclohexylamine and methylcyclohexylamine; benzylamine, β- Examples of such amines include aromatic monoamines such as phenylmethylamine, symmetric secondary amines such as N,N-dimethylamine, N,N-diethylamine, N,N-dipropylamine, N,N-dibutylamine, N,N-dihexylamine, and N,N-dioctylamine, and mixed secondary amines such as N-methyl-N-ethylamine, N-methyl-N-butylamine, N-methyl-N-dodecylamine, N-methyl-N-octadecylamine, N-ethyl-N-hexadecylamine, N-ethyl-N-octadecylamine, N-propyl-N-hexadecylamine, and N-propyl-N-benzylamine. These amines may be used alone or in combination.

[0026] Specific examples of the diamine to be added include 1,2-ethanediamine, 1,3-propanediamine, 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine, 1,12-dodecanediamine, 1,13-tridecanediamine, 1,14-tetradecanediamine, 1,15-tetradecanediamine, 1,16-tetradecanediamine, 1,17-tetradecanediamine, 1,18-tetradecanediamine, 1,19-tetradecanediamine, 1,20-tetradecanediamine, 1,21-tetradecanediamine, 1,22-tetradecanediamine, 1,23-tridecanediamine, 1,24-tetradecanediamine, 1,25-tetradecanediamine, 1,26-tetradecanediamine, 1,27-tetradecanediamine, 1,28-tetradecanediamine, 1,29-tetradecanediamine, 1,30-tetradecanediamine, 1,31-tetradecanediamine, 1,32-tetradecanediamine, 1,33-tridecanediamine, 1,34-tetradecanediamine, 1,35-tetradecanediamine, 1,36-tetradecanediamine, 1,37-tetradecanediamine, 1,38-tetradecanediamine, 1,39-tetradecanediamine, 1,40-tetradecanediamine, 1,41-tetradecanediamine, 1,42-tetradecanediamine, 1,43-tetradecanediamine, 1,44-tetradecanediamine, aliphatic amines such as 1,15-pentadecanediamine, 1,16-hexadecanediamine, 1,17-heptadecanediamine, 1,18-octadecanediamine, 2-methyl-1,5-pentanediamine, 3-methyl-1,5-pentanediamine, 2-methyl-1,8-octanediamine, 2,2,4-trimethyl-1,6-hexanediamine, 2,4,4-trimethyl-1,6-hexanediamine, and 5-methyl-1,9-nonanediamine Diamines include alicyclic diamines such as 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, bis(4-aminocyclohexyl)methane, 2,2-bis(4-aminocyclohexyl)propane, bis(3-methyl-4-aminocyclohexyl)methane, 2,2-bis(3-methyl-4-aminocyclohexyl)propane, 5-amino-2,2,4-trimethyl-1-cyclopentanemethylamine, 5-amino-1,3,3-trimethylcyclohexanemethylamine, bis(aminopropyl)piperazine, bis(aminoethyl)piperazine, 2,5-bis(aminomethyl)norbornane, 2,6-bis(aminomethyl)norbornane, 3,8-bis(aminomethyl)tricyclodecane, and 4,9-bis(aminomethyl)tricyclodecane; and aromatic diamines such as m-xylylenediamine and p-xylylenediamine. These may be used alone or in combination.

[0027] Specific examples of the triamine to be added include 1,2,3-triaminopropane, 1,2,3-triamino-2-methylpropane, 1,2,4-triaminobutane, 1,2,3,4-tetraminobutane, 1,3,5-triaminocyclohexane, 1,2,4-triaminocyclohexane, 1,2,3-triaminocyclohexane, 1,2,4,5-tetraminocyclohexane, 1,3,5-triaminobenzene, 1,2,4-triaminobenzene, 1,2,3-triaminobenzene, 1,2,4,5-tetraminobenzene, 1,2,4-triaminonaphthalene, 2,5,7-triaminonaphthalene, 2,4,6-triaminopyridine, 1,2,7,8-tetraminonaphthalene, and 1,4,5,8-tetraminonaphthalene. These may be used alone or in combination.

[0028] The polyamine to be added has a primary amino group (-NH 2 Any compound having a plurality of primary and secondary amino groups (—NH—) may be used, and examples thereof include polyalkyleneimines, polyalkylenepolyamines, polyvinylamines, and polyallylamines. The amino groups having active hydrogens are reaction sites for polyamines.

[0029] Polyalkyleneimines are produced by ionic polymerization of alkyleneimines such as ethyleneimine and propyleneimine, or by polymerizing alkyloxazoline and then partially or completely hydrolyzing the polymer. Examples of polyalkylenepolyamines include diethylenetriamine, triethylenetetramine, pentaethylenehexamine, and reaction products of ethylenediamine with polyfunctional compounds. Polyvinylamines can be obtained, for example, by polymerizing N-vinylformamide to form poly(N-vinylformamide) and then partially or completely hydrolyzing the polymer with an acid such as hydrochloric acid. Polyallylamines are generally obtained by polymerizing the hydrochloride of an allylamine monomer and then removing the hydrochloric acid. These can be used alone or in combination. Among these, polyalkyleneimines are preferred.

[0030] Examples of polyalkyleneimines include homopolymers and copolymers obtained by polymerizing one or more alkyleneimines having from 2 to 8 carbon atoms, such as ethyleneimine, propyleneimine, 1,2-butyleneimine, 2,3-butyleneimine, and 1,1-dimethylethyleneimine, using a conventional method. Among these, polyethyleneimine is more preferred. The polyalkyleneimine may be a branched polyalkyleneimine containing primary amines, secondary amines, and tertiary amines obtained by ring-opening polymerization of an alkyleneimine as a raw material, a linear polyalkyleneimine containing only primary amines and secondary amines obtained by polymerizing an alkyloxazoline as a raw material, or a polyalkyleneimine having a three-dimensional crosslinked structure. Furthermore, the polyalkyleneimine may contain ethylenediamine, propylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, dipropylenetriamine, tripropylenetetramine, dihexamethylenetriamine, aminopropylethylenediamine, bisaminopropylethylenediamine, or the like. Polyalkyleneimines usually have, in addition to tertiary amino groups, primary amino groups and secondary amino groups (imino groups) having active hydrogen atoms due to the reactivity of the active hydrogen atoms on the nitrogen atoms contained therein.

[0031] The number of nitrogen atoms in the polyalkyleneimine is not particularly limited, and is preferably from 4 to 3,000, more preferably from 8 to 1,500, and even more preferably from 11 to 500. The number average molecular weight of the polyalkyleneimine is preferably from 100 to 20,000, more preferably from 200 to 10,000, and even more preferably from 500 to 8,000.

[0032] On the other hand, examples of the carboxylic acids to be added include aliphatic monocarboxylic acids such as acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, enanthic acid, caprylic acid, capric acid, pelargonic acid, undecanoic acid, lauric acid, tridecanoic acid, myristic acid, myristoleic acid, palmitic acid, stearic acid, oleic acid, linoleic acid, arachic acid, behenic acid, and erucic acid; alicyclic monocarboxylic acids such as cyclohexanecarboxylic acid and methylcyclohexanecarboxylic acid; aromatic monocarboxylic acids such as benzoic acid, toluic acid, ethylbenzoic acid, and phenylacetic acid; malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecane diacid, dodecanedioic acid, hexadecanedioic acid, hexadecenedioic acid, octadecanedioic acid, octadecenedioic acid, eicosanedioic acid, and hydroxybenzoic acid. Aliphatic dicarboxylic acids such as senedioic acid, docosanedioic acid, diglycolic acid, 2,2,4-trimethyladipic acid, and 2,4,4-trimethyladipic acid; alicyclic dicarboxylic acids such as 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, and norbornanedicarboxylic acid; aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, m-xylylenedicarboxylic acid, p-xylylenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, and 2,7-naphthalenedicarboxylic acid; and tricarboxylic acids such as 1,2,4-butanetricarboxylic acid, 1,3,5-pentanetricarboxylic acid, 1,2,6-hexanetricarboxylic acid, 1,3,6-hexanetricarboxylic acid, 1,3,5-cyclohexanetricarboxylic acid, and trimesic acid. These can be used alone or in combination.

[0033] The amount of amines to be added can be appropriately determined by a known method within the range of the above-mentioned end group concentration condition. Usually, the amount of amines added per mole of polyamide raw material (1 mole of monomer or monomer unit constituting a repeating unit) is preferably 0.5 meq / mol to 20 meq / mol, more preferably 1.0 meq / mol to 10 meq / mol, from the viewpoint of obtaining sufficient reactivity and facilitating the production of polyamide having the desired viscosity (the equivalent weight (eq) of an amino group is defined as the amount of an amino group that reacts with a carboxyl group in a 1:1 ratio to form an amide group). The amount of carboxylic acids to be used can also be appropriately determined within the range of the above-mentioned end group concentration condition.

[0034] In the case of aliphatic polyamide resins, among the amines exemplified above, it is preferable to add a diamine and / or a polyamine during polymerization. From the viewpoint of suppressing gel formation, it is more preferable to add at least one selected from the group consisting of an aliphatic diamine, an alicyclic diamine, and a polyamine during polymerization. In order to simultaneously satisfy the desired relative viscosity for extrusion applications and the terminal amino group concentration conditions of the present invention, it is even more preferable to add a polyamine during polymerization.

[0035] The aliphatic polyamide resin may be a two-component mixture or a copolymer. If it is a copolymer, it may be a block copolymer or a random copolymer.

[0036] The weight average molecular weight (Mw) of the aliphatic polyamide resin is preferably 50,000 or more, more preferably 60,000 or more, from the viewpoint of obtaining hydrolysis resistance. On the other hand, from the viewpoint of tube formability, Mw is preferably 80,000 or less, more preferably 70,000 or less. When multiple polyamide resins are contained, it is preferable that the Mw of the entire polyamide resin is within the above range. Here, the Mw of the polyamide resin is a value calculated by gel permeation chromatography (GPC) under the conditions described below.

[0037] (Molecular Weight Distribution Curve of Aliphatic Polyamide Resin) The aliphatic polyamide resin of the present invention has the following characteristic in its molecular weight distribution curve: In other words, in a molecular weight distribution curve calculated in terms of polymethyl methacrylate, when the weight fraction of the mode of the molecular weight distribution curve is taken as 100%, S1 is the area sandwiched between the molecular weight distribution curve from the highest molecular weight point among points corresponding to a weight fraction of 70% to the maximum molecular weight and the horizontal axis corresponding to a weight fraction of 0%, and S2 is the area sandwiched between the molecular weight distribution curve from the lowest molecular weight point among points corresponding to a weight fraction of 70% to the minimum molecular weight and the horizontal axis corresponding to a weight fraction of 0%, the value of [{S2 / (S2+S1)}×100] is 64 to 90.

[0038] S1 represents the area of ​​the molecular weight distribution curve of an aliphatic polyamide resin between the point corresponding to the highest molecular weight among the points corresponding to a weight fraction of 70% to the maximum molecular weight, when the weight fraction of the mode of the molecular weight distribution curve is taken as 100%, and the horizontal axis corresponding to a weight fraction of 0%. S2 represents the area of ​​the molecular weight distribution curve between the point corresponding to the lowest molecular weight among the points corresponding to a weight fraction of 70% to the minimum molecular weight, and the horizontal axis corresponding to a weight fraction of 0%. S1 represents the proportion of high molecular weight components in the aliphatic polyamide resin, and S2 represents the proportion of lower molecular weight components in the aliphatic polyamide resin. Therefore, the larger the value of the area ratio [{S2 / (S2+S1)}×100], the higher the proportion of lower molecular weight components in the aliphatic polyamide resin. For the regions represented by S1 and S2, please also refer to Figure 1, which is a schematic diagram of an example of a molecular weight distribution curve obtained by GPC.

[0039] The polymethyl methacrylate-equivalent molecular weight distribution of an aliphatic polyamide resin is determined by injecting 20 μL of a solution of the aliphatic polyamide resin in 1,1,1,3,3,3-hexafluoro-2-propanol (HFIP) into a gel permeation chromatography (GPC) equipped with a TSKgel Super AW3000 and AW5000 (manufactured by Tosoh Corporation) column at a temperature of 40°C, measuring the sample at a flow rate of 0.3 mL / min and an injection volume of 20 μL, and converting the measured value into polymethyl methacrylate equivalents. The weight-average molecular weight of the aliphatic polyamide resin can also be determined by the same method. A weight-average molecular weight of 1,000 or more, calculated as polymethyl methacrylate, is used as the molecular weight distribution curve.

[0040] The aliphatic polyamide resin of the present invention has an area ratio [{S2 / (S2+S1)}×100] of 64 to 90. This means that the aliphatic polyamide resin contains a higher proportion of low-molecular-weight components than high-molecular-weight components. When the value of [{S2 / (S2+S1)}×100] is within this range, the proportion of lower-molecular-weight components increases, tending to moderately reduce fluidity. As a result, the MFR (melt flow rate) can be kept within a range suitable for tube molding. The value of [{S2 / (S2+S1)}×100] is preferably 65 or greater, more preferably 66 or greater. Furthermore, the value of [{S2 / (S2+S1)}×100] is preferably 95 or less, more preferably 90 or less.

[0041] Examples of means for adjusting the value of [{S2 / (S2+S1)}×100] within the above range include a method of quickly completing the polymerization of the polyamide resin to increase the amount of low-molecular-weight components, a method of mixing at least two kinds of aliphatic polyamide resins with different molecular weights, etc. Since it is possible to finely adjust the value of [{S2 / (S2+S1)}×100] by changing the blending amount of the aliphatic polyamide resin with a relatively low weight-average molecular weight, it is preferable to mix two or more kinds of aliphatic polyamide resins.

[0042] The aliphatic polyamide resin preferably has a melting point of 170°C or higher and 190°C or lower as measured by differential scanning calorimetry (DSC). The lower limit of the melting point is more preferably 172°C or higher, and particularly preferably 175°C or higher. The upper limit of the melting point is more preferably 188°C or lower, even more preferably 187°C or lower, and particularly preferably 185°C or lower. Having a melting point within this range makes it possible to achieve both tube formability and hydrolysis resistance. The melting point of the aliphatic polyamide resin as measured by differential scanning calorimetry (DSC) can be increased or decreased depending on the composition ratio, relative viscosity, and molecular weight of each component.

[0043] The aliphatic polyamide resin preferably has a crystallization temperature of 130°C or higher and 160°C or lower as measured by differential scanning calorimetry (DSC). The lower limit of the crystallization temperature is more preferably 135°C or higher, and particularly preferably 140°C or higher. The upper limit of the crystallization temperature is more preferably 157°C or lower, and particularly preferably 155°C or lower. This allows for stable tube moldability. The crystallization temperature of the aliphatic polyamide resin as measured by differential scanning calorimetry (DSC) can be increased or decreased depending on the composition ratio, relative viscosity, and molecular weight of each component.

[0044] The aliphatic polyamide resin preferably has a relative viscosity of 1.80 or more and 2.10 or less. The lower limit of the relative viscosity is more preferably 1.85 or more, particularly preferably 1.90 or more. The upper limit of the relative viscosity is more preferably 2.09 or less, particularly preferably 2.08 or less. When the relative viscosity is equal to or less than the above upper limit, the tube formability is excellent. When the relative viscosity is equal to or more than the above lower limit, the hydrolysis resistance is excellent. In this specification, ηr (relative viscosity) is the measured value (JIS K 6920) at 25°C of 100 ml of 96% by mass concentrated sulfuric acid as a solvent, with a polyamide concentration of 1 g / 100 ml.

[0045] <Polyolefin> The polyamide resin composition of the present invention contains a polyolefin. Known materials can be used as the polyolefin, but the polyolefin of the present invention preferably functions as an impact resistance agent. The polyolefin preferably has a surface hardness (Shore A) of 80 or less as measured in accordance with ASTM D2240.

[0046] The polyolefin used has a functional group that exhibits reactivity with the end group of the polyamide resin. Specific examples include copolymers having an (ethylene and / or propylene) / α-olefin copolymer as the main skeleton, at least a portion of which has a functional group that exhibits reactivity with the end group of the aliphatic polyamide resin, and (ethylene and / or propylene) / (α,β-unsaturated carboxylic acid and / or α,β-unsaturated carboxylic acid ester) copolymers. These can be used alone or in combination of two or more. The polyolefin preferably has an ethylene / α-olefin copolymer as the main skeleton.

[0047] The (ethylene and / or propylene) / α-olefin copolymer is a polymer obtained by copolymerizing ethylene and / or propylene with an α-olefin having 3 or more carbon atoms or 4 or more carbon atoms. Examples of the α-olefins having 3 or more carbon atoms include propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, 1-eicosene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene, 3-ethyl-1-hexene, 9-methyl-1-decene, 11-methyl-1-dodecene, and 12-ethyl-1-tetradecene. These may be used alone or in combination of two or more.

[0048] The copolymer may also be one obtained by copolymerizing a polyene such as a non-conjugated diene. Examples of the non-conjugated diene include 1,4-pentadiene, 1,4-hexadiene, 1,5-hexadiene, 1,4-octadiene, 1,5-octadiene, 1,6-octadiene, 1,7-octadiene, 2-methyl-1,5-hexadiene, 6-methyl-1,5-heptadiene, 7-methyl-1,6-octadiene, 4-ethylidene-8-methyl-1,7-nonadiene, 4,8-dimethyl-1,4,8-decatriene (DMDT), and dicyclopentadiene. Examples of the alkyl acrylate include butyl acrylate, butyl acrylate, butyl acrylate, butyl acrylate, butyl acrylate (VBA), ...

[0049] The (ethylene and / or propylene) / (α,β-unsaturated carboxylic acid and / or α,β-unsaturated carboxylic acid ester) copolymer is a polymer obtained by copolymerizing ethylene and / or propylene with an α,β-unsaturated carboxylic acid and / or α,β-unsaturated carboxylic acid ester monomer. Examples of the α,β-unsaturated carboxylic acid monomer include acrylic acid and methacrylic acid. Examples of the α,β-unsaturated carboxylic acid ester monomer include the methyl ester, ethyl ester, propyl ester, butyl ester, pentyl ester, hexyl ester, heptyl ester, octyl ester, nonyl ester, and decyl ester of these α,β-unsaturated carboxylic acids. These may be used alone or in combination of two or more.

[0050] Furthermore, it is preferable that at least a portion of the (ethylene and / or propylene) / α-olefin copolymer has a functional group that reacts with a terminal amino group of the aliphatic polyamide resin. The (ethylene and / or propylene) / (α,β-unsaturated carboxylic acid and / or α,β-unsaturated carboxylic acid ester) copolymer already has the functional group, but may further have a different functional group.

[0051] Examples of the functional group include a carboxyl group, an acid anhydride group, a carboxylic acid ester group, a metal carboxylic acid salt, a carboxylic acid imide group, a carboxylic acid amide group, and an epoxy group. These groups may be in the form of a corresponding salt if they can form a salt. Acidic functional groups can form metal salts with typical metals or transition metals, and basic functional groups can form ammonium salts.

[0052] Examples of compounds containing these functional groups include acrylic acid, methacrylic acid, maleic acid, fumaric acid, itaconic acid, crotonic acid, mesaconic acid, citraconic acid, glutaconic acid, cis-4-cyclohexene-1,2-dicarboxylic acid, endobicyclo-[2.2.1]-5-heptene-2,3-dicarboxylic acid, and metal salts of these carboxylic acids, monomethyl maleate, monomethyl itaconate, methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, hydroxyethyl acrylate, methyl methacrylate, and methacrylic acid. Examples of suitable alkyl acrylates include 2-ethylhexyl, hydroxyethyl methacrylate, aminoethyl methacrylate, dimethyl maleate, dimethyl itaconate, maleic anhydride, itaconic anhydride, citraconic anhydride, endobicyclo-[2.2.1]-5-heptene-2,3-dicarboxylic anhydride, maleimide, N-ethylmaleimide, N-butylmaleimide, N-phenylmaleimide, acrylamide, methacrylamide, glycidyl acrylate, glycidyl methacrylate, glycidyl ethacrylate, glycidyl itaconate, and glycidyl citraconate. These may be used alone or in combination of two or more. Of these, maleic anhydride, itaconic anhydride, and citraconic anhydride are preferred.

[0053] Methods for introducing these functional groups into polymers used in polyolefins include (i) copolymerizing a copolymerizable monomer having a functional group during polymerization of the polymer, (ii) introducing a functional group into the molecular chain or molecular end of the polymer using a polymerization initiator, a chain transfer agent, etc., and (iii) grafting a compound having a functional group and a graftable functional group (graft compound) onto the polymer, etc. These introduction methods can be used alone or in appropriate combination.

[0054] The content of functional groups such as acid anhydride groups and carboxylic acid ester groups (functional group amount [C1]) contained per gram of polyolefin is preferably more than 25 μmol / g and less than 100 μmol / g, more preferably 35 μmol / g or more and less than 95 μmol / g, and even more preferably 40 μmol / g or more and 90 μmol / g or less. A content of more than 25 μmol / g can produce a composition with a high melt viscosity, allowing the target wall thickness to be achieved in tube molding. Furthermore, a content of less than 100 μmol / g can prevent the melt viscosity from becoming too high, reducing the load on the extruder and enabling good molding processing. For example, when a polyolefin contains a carboxy group, acid anhydride group, or carboxylic acid ester group, the content of the functional groups is measured by neutralization titration with a 0.1 N KOH ethanol solution using a sample solution prepared using a xylene / ethanol mixed solution and phenolphthalein as an indicator. The polyolefin may be used in combination with a polyolefin that does not have a functional group that is reactive with the terminal group of the polyamide resin, but it is preferable to use an amount such that the content of the functional group relative to the total polyolefin falls within the above range.

[0055] In the polyamide resin composition of the present invention, the product of the functional group amount [C1] of the polyolefin and the amino group amount [A1] of the aliphatic polyamide resin is 1000 to 5000 ((μmol / g) 2 It is preferable that the amounts of the functional groups in both components are controlled so that

[0056] The polyolefin preferably has an MFR of 2 g / 10 min or less as measured in accordance with ISO 1133 at a temperature of 190°C and a load of 2.16 kg. If the MFR is within this range, it becomes easier to maintain the MFR of the entire polyamide resin composition within a good range.

[0057] <Polyamide Resin Composition> The polyamide resin composition of the present invention is a composition containing the above-mentioned aliphatic polyamide resin and polyolefin. The mass ratio of the polyolefin content (B) to the total mass of the aliphatic polyamide resin content (A) and the polyolefin content (B), [(B) / {(A) + (B)}], is 0.15 to 0.40. That is, the amount of the aliphatic polyamide resin is in the range of 60 to 85 mass% relative to 100 mass% of the total of the aliphatic polyamide resin and polyolefin. The aliphatic polyamide resin content, [(B) / {(A) + (B)}], is preferably 0.17 to 0.38, more preferably 0.18 to 0.37, and particularly preferably 0.20 to 0.36. That is, the aliphatic polyamide resin content is preferably 62 mass% or more, more preferably 63 mass% or more, and particularly preferably 64 mass% or more. The content of the aliphatic polyamide resin is preferably 83% by mass or less, more preferably 82% by mass or less, and particularly preferably 80% by mass or less.

[0058] (Amount of Functional Groups [C2] of Polyolefin in Polyamide Resin Composition) The amount of functional groups [C2] of polyolefin in the polyamide resin composition is preferably 5 μmol / g or more but less than 70 μmol / g, more preferably 7 μmol / g or more but less than 50 μmol / g, and even more preferably 8 μmol / g or more but less than 40 μmol / g. A content of more than 5 μmol / g can produce a composition with a high melt viscosity, allowing the target wall thickness to be achieved in tube molding. Furthermore, a content of less than 100 μmol / g can prevent the melt viscosity from becoming too high, reducing the load on the extruder and enabling good molding processing. The amount of functional groups [C2] of polyolefin in the polyamide resin composition is measured by neutralization titration with a 0.1N KOH ethanol solution using a sample solution prepared from the polyamide resin composition using benzyl alcohol and phenolphthalein as an indicator. Alternatively, it can be determined from the composition ratio and the amount of functional groups of each polyolefin.

[0059] (Amino Group Amount [A2] of Aliphatic Polyamide in Polyamide Resin Composition) From the viewpoint of improving the fluidity of the polyamide resin composition, the amino group amount [A2] of the aliphatic polyamide resin in the polyamide resin composition is preferably more than 20 μmol / g and less than 95 μmol / g, more preferably 30 μmol / g or more and less than 90 μmol / g, and even more preferably 35 μmol / g or more and 85 μmol / g or less. [A2] is generally smaller than the amino group amount [A1] of the aliphatic polyamide resin. The amino group amount of the aliphatic polyamide resin in the polyamide resin composition is measured by dissolving the polyamide resin composition in a phenol / methanol mixed solution and titrating with 0.05 N hydrochloric acid. Alternatively, it may be determined from the composition ratio and the functional group amount of each polyolefin.

[0060] (Product of Amount of Functional Groups in Polyolefin [C2] and Amount of Amino Groups in Aliphatic Polyamide Resin [A2]) The polyamide resin composition of the present invention has a polyamide resin composition in which the product of the amount of functional groups in polyolefin [C2] and the amount of amino groups in the aliphatic polyamide resin [A2] per 1 g of the polyamide resin composition is 250 to 750 ((μmol / g) 2 It is preferable that the amounts of the functional groups of both the polymers are designed so that the ratio of the functional groups of both the polymers satisfies the above.

[0061] The method for mixing the aliphatic polyamide resin and the polyolefin is not particularly limited, and various additives may be added as necessary, and various conventionally known methods may be employed. For example, the aliphatic polyamide resin and the polyolefin may be dry-blended uniformly using a tumbler or mixer to achieve the above-mentioned mixing ratio, or the aliphatic polyamide resin and the polyolefin may be dry-blended in advance with other components added as necessary at the concentration to be used during molding, followed by melt-kneading. The melt-kneading may be carried out using a kneader such as a single-screw extruder, a twin-screw extruder, a kneader, or a Banbury mixer.

[0062] (Additives) Furthermore, if necessary, the polyamide resin composition may contain additives such as antioxidants, heat stabilizers, ultraviolet absorbers, light stabilizers, weathering agents, lubricants, inorganic fillers, antistatic agents, flame retardants, crystallization accelerators, plasticizers, colorants, and lubricants. As these additives, various commercially available materials known to those skilled in the art can be used.

[0063] It is preferable to add an antioxidant to the polyamide resin composition. Examples of organic antioxidants include phenolic antioxidants, phosphorus-based antioxidants, and sulfur-based antioxidants.

[0064] Preferred examples of the phenolic antioxidant include hindered phenolic antioxidants. In this specification, a hindered phenol refers to a compound having a substituent at the ortho-position (hereinafter also referred to as the "o-position") of the phenolic hydroxyl group. The substituent at the o-position is not particularly limited, but examples include an alkyl group, an alkoxy group, an amino group, and a halogen atom. Among these, alkyl groups such as a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, a sec-butyl group, an i-butyl group, and a tert-butyl group are preferred, with bulky i-propyl group, sec-butyl group, an i-butyl group, and a tert-butyl group being more preferred, and a tert-butyl group being most preferred. Furthermore, with regard to the o-position, it is preferred that both of the two o-positions relative to the phenolic hydroxyl group have a substituent.

[0065] The hindered phenol having a tert-butyl group at the o-position may be a commercially available product, and specific examples thereof include N,N'-(hexane-1,6-diyl)bis[4-hydroxy-3,5-bis(tert-butyl)benzenepropanamide (Irganox (registered trademark) 1098; manufactured by BASF Japan Ltd.), pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4'-hydroxyphenyl)propionate (Irganox (registered trademark) 1010; manufactured by BASF Japan Ltd.), and the like. ), ethylene bis(oxyethylene) bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate] (Irganox (registered trademark) 245; manufactured by BASF Japan Ltd.), 3,9-bis[2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane (Sumilizer (registered trademark) GA-80; manufactured by Sumitomo Chemical Co., Ltd.). These may be used alone or in combination of two or more.

[0066] As the phosphorus-based antioxidant, a phosphite compound of a hindered phenol or a hypophosphite compound of a hindered phenol is preferred, a phosphite compound of a hindered phenol having a tert-butyl group at the o-position or a hypophosphite compound of a hindered phenol having a t-butyl group at the o-position is more preferred, and a phosphite compound of a hindered phenol having a t-butyl group at the o-position is even more preferred. These may be commercially available products, and a specific example of a phosphite compound of a hindered phenol having a t-butyl group at the o-position is tris(2,4-di-tert-butylphenyl)phosphite (Irgafos (registered trademark) 168; manufactured by BASF Japan Ltd.). Specific examples of the hypophosphite ester compound of a hindered phenol having a tert-butyl group at the o-position include 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane (ADK STAB (registered trademark) PEP-36; manufactured by ADEKA Corporation), and a reaction product of biphenyl, phosphorus trichloride, and 2,4-di-tert-butylphenol, the main component of which is p,p,p',p'-tetrakis(2,4-di-tert-butylphenoxy)-4,4' (or 3',4)-biphenyldiphosphine (Hostanox (registered trademark) P-EPQ (registered trademark) P; manufactured by Clariant Japan Co., Ltd.). These may be used alone or in combination of two or more.

[0067] Examples of sulfur-based antioxidants include distearyl-3,3-thiodipropionate, pentaerythrityl tetrakis(3-laurylthiopropionate), and didodecyl(3,3'-thiodipropionate). These may be used alone or in combination of two or more. These organic antioxidants may be used alone or in combination of two or more.

[0068] Other polyamide resins or other thermoplastic resins may be added to the polyamide resin composition. Examples of such resins that can be added include the polyamide resins and thermoplastic resins described in paragraphs 0054 and 0055 of WO 2015 / 033982. These resins can be used alone or in combination of two or more.

[0069] The polyamide resin composition of the present invention has an MFR of 0.01 g / 10 min or more and 20 g / 10 min or less at 300°C and 5000 g. By setting the MFR within this range, the resin does not exhibit excessive fluidity and is suitable for molding into a tube. The MFR is preferably 0.05 g / 10 min or more, and more preferably 0.10 g / 10 min or more. The MFR is preferably 15 g / 10 min or less, and more preferably 10 g / 10 min or less. The MFR is a value measured in accordance with ISO 1133 by heating 5000 g of the resin composition to 300°C.

[0070] <Molded Articles> The polyamide resin composition of the present invention can be used to produce hollow molded articles, particularly those for transporting cooling liquids. As long as the hollow molded article is produced, its shape is not limited, and it can take various forms, including tubes, hoses, and pipes. Generally, even resins that can be injection molded without any problems tend to be unsuitable for tube molding. The production of hollow molded articles such as tubes and hoses differs from injection molding, which is based on pouring the resin into a mold, in that a constant amount of resin must be continuously extruded from an extruder and the extruded resin must solidify in the same shape. Resin pulsation during the extrusion process can result in inconsistent tube wall thickness and weak spots against pressure. Furthermore, if the resin's fluidity is too high, dripping occurs before curing, preventing the formation of a hollow molded article with a uniform shape. Therefore, resins for tube molding are required to have an appropriate range of fluidity and be capable of being molded uniformly and continuously. The inventors have discovered that the polyamide resin composition of the present invention is a resin with properties that meet these requirements and is suitable for tube molding.

[0071] The polyamide resin composition of the present invention can be formed into a single-layer hollow molded article. Polyamides are essentially susceptible to hydrolysis, and even in the case of a single layer, the polyamide resin composition of the present invention is extremely effective in that it can be used to transport fluids, even when the coolant contains water.

[0072] The polyamide resin composition of the present invention can basically be used as a single layer, but in some cases, it may be formed into a molded article having a layer structure of two or more layers. The layer containing the polyamide resin composition of the present invention can be used as any of the inner layer, outer layer, and intermediate layer, and can be designed according to the application of the resin used as the second layer. Resins that can be used in combination in the laminate tube include fluorine-containing polymers having functional groups reactive to amino groups introduced into the molecular chain, polyolefin polymers, thermoplastic resin compositions optionally containing conductive fillers, polyamides other than the above-mentioned aliphatic polyamide resins, for example, aromatic polyamides such as PA6T using terephthalic acid, and aliphatic polyamides mainly composed of short-chain alkylene groups. Resins known to those skilled in the art can be used depending on the location and desired properties.

[0073] When a laminate tube is produced, the thickness of the layer of the polyamide resin composition of the present invention is not particularly limited and can be adjusted depending on the type of polymer constituting each layer, the total number of layers in the laminate tube, the intended use, etc. In general, the thickness of the layer of the polyamide resin composition of the present invention is preferably 3% or more and 90% or less of the total thickness of the laminate tube.

[0074] Tubes can be manufactured by known methods such as extrusion molding or blow molding, and molding can be performed in accordance with conventional methods. In extrusion molding, a molten resin is extruded into a circular mold and cooled to form a tube. Because a tube of any length can be manufactured using a relatively simple process, extrusion molding is easy and preferable for general infusion tubes. Single- or multi-screw extruders can be used. In blow molding, a hollow body called a parison is formed and then molded using internal air pressure. These methods can also be used to mold complex shapes.

[0075] When the tube is multilayered, examples of the method include a method in which an extruder corresponding to the number of layers or materials is used to melt extrude and simultaneously laminate the layers inside or outside a die (coextrusion method), or a method in which a single-layer tube or a laminated tube produced by the above method is first produced in advance, and then resins are laminated on the outside in sequence, if necessary using an adhesive, to integrate the resins (coating method).

[0076] Furthermore, when the tube to be obtained has a complex shape or when a molded product is to be formed by heat bending after molding, the tube may be heat-treated after formation at a temperature below the melting point of the resin constituting the tube for 0.01 to 10 hours in order to remove residual strain in the molded product, thereby obtaining the desired molded product.

[0077] The tube may have a corrugated region. The corrugated region is a region formed in a wave shape, bellows shape, accordion shape, corrugated shape, or the like. The corrugated region may exist not only over the entire length of the laminated tube, but also partially in an appropriate region along the length. The corrugated region can be easily formed by first forming a straight tube and then molding it to form a predetermined corrugated shape. The presence of such a corrugated region provides impact absorption and facilitates installation. Furthermore, it is possible to add necessary parts such as connectors or to form L- or U-shapes by bending.

[0078] Taking into consideration stone chipping, abrasion with other parts, and flame resistance, the outer periphery of the thus molded tube is coated with one of the following rubbers on all or part of the outer periphery: natural rubber (NR), butadiene rubber (BR), isoprene rubber (IR), butyl rubber (IIR), chloroprene rubber (CR), carboxylated butadiene rubber (XBR), carboxylated chloroprene rubber (XCR), epichlorohydrin rubber (ECO), acrylonitrile butadiene rubber (NBR), hydrogenated acrylonitrile butadiene rubber (HNBR), carboxylated acrylonitrile butadiene rubber (XNBR), a mixture of NBR and polyvinyl chloride, acrylonitrile isoprene rubber (NIR), chlorinated polyethylene rubber (CM), chlorosulfonated polyethylene rubber (CSM), ethylene propylene rubber (E A solid or sponge-like protective member (protector) can be provided, which is made of, for example, ethylene propylene diene rubber (EPDM), ethylene vinyl acetate rubber (EVM), a rubber mixture of NBR and EPDM, acrylic rubber (ACM), ethylene acrylic rubber (AEM), acrylate butadiene rubber (ABR), styrene butadiene rubber (SBR), carboxylated styrene butadiene rubber (XSBR), styrene isoprene rubber (SIR), styrene isoprene butadiene rubber (SIBR), urethane rubber, silicone rubber (MQ, VMQ), fluororubber (FKM, FFKM), fluorosilicone rubber (FVMQ), or a thermoplastic elastomer such as a vinyl chloride-based, olefin-based, ester-based, urethane-based, or amide-based protective member. The protective member may also be made into a sponge-like porous body by known techniques. By making the protective member porous, a lightweight protective portion with excellent heat insulation can be formed. Material costs can also be reduced. Alternatively, glass fibers or the like may be added to improve its strength. The shape of the protective member is not particularly limited, but it is usually a block-shaped member with a recess for receiving a cylindrical member or a laminated tube. In the case of a cylindrical member, the tube can be inserted into a prefabricated cylindrical member, or the cylindrical member can be coated and extruded onto the tube, and the two can be tightly attached to each other. To bond the two, an adhesive is applied to the inner surface or the recessed surface of the protective member as needed, and the tube is inserted or fitted into this, and the two are tightly attached to form an integrated structure of the tube and protective member. It is also possible to reinforce the protective member with metal or the like.

[0079] The outer diameter of the tube is designed taking into consideration the flow rate of the chemical (e.g., fuel such as alcohol-containing gasoline) and the wall thickness is designed to be such that the amount of chemical permeation does not increase, the burst pressure of a normal tube can be maintained, and flexibility is maintained to an extent that the tube is easy to assemble and has good vibration resistance during use, but is not limited thereto. Preferably, the outer diameter is 4 mm to 300 mm, the inner diameter is 3 mm to 250 mm, and the wall thickness is 0.5 mm to 25 mm.

[0080] Tubes using the polyamide resin composition of the present invention can be used for a variety of applications, including automobile parts, internal combustion engine applications, mechanical parts such as power tool housings, industrial materials, industrial supplies, electric and electronic parts, medical products, food products, household and office supplies, building materials, and furniture parts.

[0081] Furthermore, a tube using the polyamide resin composition of the present invention has excellent chemical solution permeation prevention properties and is therefore suitable as a chemical solution transport tube. Examples of chemical solutions include aromatic hydrocarbon solvents such as benzene, toluene, and xylene; alcohols and phenolic solvents such as methanol, ethanol, propanol, butanol, pentanol, ethylene glycol, propylene glycol, diethylene glycol, phenol, cresol, polyethylene glycol, and polypropylene glycol; ether solvents such as dimethyl ether, dipropyl ether, methyl tert-butyl ether, ethyl tert-butyl ether, dioxane, and tetrahydrofuran; chloroform, methylene chloride, trichloroethylene, ethylene dichloride, perchloroethylene, monochloroethane, dichloroethane, tetrahydrofuran; Examples of suitable solvents include halogen-based solvents such as dichloroethane, perchloroethane, and chlorobenzene; ketone-based solvents such as acetone, methyl ethyl ketone, diethyl ketone, and acetophenone; gasoline, kerosene, diesel gasoline, alcohol-containing gasoline, oxygenated ethyl-t-butyl ether blend gasoline, amine-containing gasoline, sour gasoline, castor oil-based brake fluid, glycol ether-based brake fluid, borate ester-based brake fluid, brake fluid for extremely cold regions, silicone oil-based brake fluid, mineral oil-based brake fluid, power steering oil, hydrogen sulfide-containing oil, windshield washer fluid, coolant for vehicle engines, urea solution, pharmaceuticals, ink, and paint. The laminated tube of the present invention is suitable as a tube for transporting the above-mentioned chemical liquids, and specific examples thereof include fuel tubes such as feed tubes, return tubes, evaporative tubes, fuel filler tubes, ORVR tubes, reserve tubes, and vent tubes; oil tubes, oil drilling tubes, brake tubes, tubes for windshield washer fluid, engine coolant (LLC) tubes, reservoir tank tubes, urea solution transport tubes, cooler tubes for cooling water, refrigerants, etc., tubes for air conditioner refrigerants, heater tubes, road heating tubes, floor heating tubes, infrastructure supply tubes, tubes for fire extinguishers and fire extinguishing equipment, tubes for medical cooling equipment, tubes for spraying ink and paint, and other chemical liquid tubes.In particular, it is suitable as a tube for conveying automotive coolants containing ethylene glycol and water.

[0082] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. The components used in the examples and comparative examples and the methods for measuring the physical properties of the molded articles are shown below.

[0083] [Constituent Components] (A) Aliphatic Polyamide Resin (A-1) Polyamide 12 (manufactured by UBE Corporation, [CH2] / [NHCO]=11, relative viscosity=2.23, amino group amount (terminal amino group amount)=58 μmol / g) (A-2) Polyamide 12 (manufactured by UBE Corporation, [CH2] / [NHCO]=11, relative viscosity=1.90, amino group amount (terminal amino group amount)=81 μmol / g) (A-3) Polyamide 12 (manufactured by UBE Corporation, [CH2] / [NHCO]=11, relative viscosity=1.68, amino group amount (terminal amino group amount)=24 μmol / g) The relative viscosity was measured at 25°C in accordance with JIS K 6920 using a solution obtained by dissolving 1 g of the polyamide resin in 100 ml of 96% sulfuric acid. The amount of amino groups is measured by dissolving the polyamide resin in a phenol / methanol (7 / 3 (volume ratio)) mixed solution and titrating with 0.05 N hydrochloric acid. The amount of amino groups [A1] of the aliphatic polyamide resin shown in Table 1 was calculated from the composition ratio and the amount of each amino group. (B) Polyolefins (B-1) Maleic anhydride-modified ethylene / 1-butene copolymer (Mitsui Chemicals, Inc., Tafmer (registered trademark) MH5010, functional group amount (maleic anhydride group amount) = 50 μmol / g) (B-2) Maleic anhydride-modified ethylene / 1-butene copolymer (Mitsui Chemicals, Inc., Tafmer (registered trademark) MH5020, functional group amount (maleic anhydride group amount) = 100 μmol / g) (B-3) Unmodified ethylene / 1-butene copolymer (Mitsui Chemicals, Inc., Tafmer (registered trademark) DF740) The functional group amount of the polyolefin is measured by neutralization titration with a 0.1 N KOH ethanol solution using a sample solution prepared using a xylene / ethanol (9 / 1 (volume ratio)) mixed solution and phenolphthalein as an indicator. In addition, the amount of functional groups [C1] of the polyolefin shown in Table 1 was calculated from the composition ratio and the amount of each functional group.In addition to the polyamide and polyolefin, a hindered phenol-based antioxidant (Irganox (registered trademark) 245 manufactured by BASF Japan Ltd.), a phosphorus-based processing stabilizer (Irgafos (registered trademark) 168 manufactured by BASF Japan Ltd.), and an organic sulfur-based secondary antioxidant (Sumilizer (registered trademark) TP-D manufactured by Sumitomo Chemical Co., Ltd.) were used as antioxidants, and carbon black (VULCAN (registered trademark) 9A32 manufactured by Cabot Corporation) was used as a colorant.

[0084] Examples: Aliphatic polyamide resin, polyolefin, and additives were melt-kneaded in a twin-screw melt kneader in the compositions shown in Table 1 to produce pellets of a polyamide resin composition. As comparative examples, pellets of polyamide resin composition were produced in the same manner in the compositions shown in Table 1, except that no polyolefin was added (Comparative Example 1), the amount of polyolefin was reduced to 10 parts by mass (Comparative Example 2), and the type and amount of aliphatic polyamide were changed (Comparative Examples 3 to 8). The composition of each component in the compositions of the examples and comparative examples is shown in Table 1. The values ​​are in mass%.

[0085] <Measurement and Evaluation of Physical Properties> The physical properties and evaluation of the polyamide resin compositions obtained in the examples and comparative examples were carried out as follows.

[0086] (Value of [{S2 / (S2+S1)}×100] (GPC)) As an index of compatibility between tube moldability and long-term LLC (coolant) resistance, the molecular weight distribution of the polyamide resin composition in terms of polymethyl methacrylate was calculated by gel permeation chromatography (GPC). In the molecular weight distribution curve in terms of polymethyl methacrylate, when the weight fraction of the mode of the molecular weight distribution curve is taken as 100%, S1 is the area sandwiched between the molecular weight distribution curve from the highest molecular weight point corresponding to a weight fraction of 70% to the maximum molecular weight point and the horizontal axis corresponding to a weight fraction of 0%, and S2 is the area sandwiched between the molecular weight distribution curve from the lowest molecular weight point corresponding to a weight fraction of 70 to the minimum molecular weight point and the horizontal axis corresponding to a weight fraction of 0%, and the value of [{S2 / (S2+S1)}×100] was calculated as an index of the content of low molecular weight components. (Amount of functional groups [C2] of polyolefin in polyamide resin composition) The amount of functional groups [C2] of polyolefin in polyamide resin composition is measured by neutralization titration with 0.1N KOH ethanol solution using phenolphthalein as an indicator, using a sample solution prepared by dissolving the polyamide resin composition in a xylene / ethanol mixture. Alternatively, it may be determined from the composition ratio and the amount of functional groups of each polyolefin. (Amount of amino groups [A2] of aliphatic polyamide resin in polyamide resin composition) The amount of amino groups of aliphatic polyamide resin in polyamide resin composition is measured by dissolving the polyamide resin composition in a phenol / methanol mixture and titrating with 0.05N hydrochloric acid. Alternatively, it may be determined from the composition ratio and the amount of functional groups of each polyolefin. (Amount of functional groups in polyolefin in polyamide resin composition [C2] × amount of amino groups in aliphatic polyamide resin) The amount of functional groups in polyolefin in polyamide resin composition [C2] × amount of amino groups in aliphatic polyamide resin is the product of the amount of functional groups in polyolefin in the polyamide resin composition and the amount of amino groups in the aliphatic polyamide resin in the polyamide resin composition.

[0087] [Mixing Stability] In the pellet production of Examples 1 to 6 and Comparative Examples 1 to 5, the kneading stability when the melt-kneaded material was extruded into a strand shape using a twin-screw melt kneader was evaluated according to the following criteria: ∘ (Good): Stable strand extrusion was possible. × (Poor): Stable strand extrusion was impossible. (For example, the material could not be extruded into a strand shape, or even if it could be extruded into a strand shape, the strand became thin or thick, or was broken midway.)

[0088] [Resin Pressure] The resin pressure was measured when melt-kneaded in a twin-screw melt-kneader at a barrel temperature of 240°C. The measurement was performed by attaching a pressure gauge to the kneader and reading the value. A low pressure reduces the burden on the device and allows for stable pellet production. It was determined that a resin pressure of 10 MPa or less indicates good productivity, and a resin pressure of 8 MPa or less indicates particularly excellent productivity.

[0089] [Tube formability] The formability of tubes using an extrusion molding machine was evaluated according to the following criteria: ○ (Good): Continuous molding was possible, and tubes could be formed stably without pulsation. △ (Fair): Pulsation occurred, and the tube dimensions were somewhat unstable, but continuous molding was fully possible. × (Unacceptable): Continuous molding of tubes was not possible, and pulsation occurred.

[0090] [Flowability (MFR)] As an index of the flowability of a polyamide resin composition, MFR (temperature: 300°C, load: 5,000 g) was measured by a method in accordance with ISO 1133. If the MFR was 0.1 to 20 g / 10 min, the flowability was determined to be good.

[0091] [Preparation of Test Pieces] Test pieces were prepared from the polyamide resin composition in accordance with ISO 294-1 using an injection molding machine SE100D-C160S manufactured by Sumitomo Heavy Industries, Ltd.

[0092] [Toughness (Tensile Breaking Elongation)] The tensile breaking elongation of the obtained test specimens was measured by a method in accordance with ISO 527-1 and 2. If the tensile breaking elongation was 150% or more, it was determined that the toughness was sufficient, and if it was 170% or more, it was determined that the toughness was particularly excellent.

[0093] (Hydrolysis Resistance) The obtained test specimens were sealed and immersed in an autoclave filled with coolant (water / ethylene glycol = 50 / 50 mass ratio) and heated at 120°C for 1000 hours. Thereafter, the test specimens were removed and the tensile breaking elongation was measured according to ISO 527-1 and 2. The tensile breaking elongation after immersion was defined as the tensile breaking elongation retention rate, where the tensile breaking elongation before immersion was 100%. The hydrolysis resistance was evaluated according to the following criteria. ○ (Good): Cases where both the tensile breaking elongation after the coolant immersion test was 40% or more and the tensile breaking retention rate after the coolant immersion test was 15% or more were satisfied. × (Fail): Cases where either the tensile breaking elongation after the coolant immersion test was 40% or more and the tensile breaking retention rate after the coolant immersion test was 15% or more were not satisfied.

[0094]

[0095] As shown in Table 1, the polyamide resin composition of the present invention exhibited excellent stability during kneading and moldability when formed into a tube, while also exhibiting high hydrolysis resistance over a long period of time, making it extremely suitable as a material for tubes for transporting liquids such as coolants. A [{S2 / (S2+S1)}×100] value of 64 to 90 resulted in a relatively high and appropriate content of low-molecular-weight components, which is thought to achieve both fluidity and hydrolysis resistance. On the other hand, Comparative Examples 1 and 2, which contained no polyolefin or only a small amount of it, and Comparative Examples 3 to 5, which had small [{S2 / (S2+S1)}×100] values, had such low viscosity that the MFR could not be measured, resulting in problems with tube moldability.

Claims

1. A polyamide resin composition comprising an aliphatic polyamide resin and a polyolefin having a functional group exhibiting reactivity with an end group of the polyamide resin, wherein the aliphatic polyamide resin has a portion derived from a linear or branched hydrocarbon compound of 80 mol % or more of all monomer units thereof, the mass ratio [(B) / {(A)+(B)}] of the polyolefin content (B) to the total mass of the aliphatic polyamide resin content (A) and the polyolefin content (B) is 0.15 to 0.40, and the aliphatic polyamide resin has the following characteristics in a molecular weight distribution curve calculated as polymethyl methacrylate: When the weight fraction of the most frequent value on the molecular weight distribution curve is taken as 100%, the area of ​​the portion sandwiched between the molecular weight distribution curve from the highest molecular weight point among the points corresponding to a weight fraction of 70% to the maximum molecular weight point and the horizontal axis corresponding to a weight fraction of 0% is taken as S1, and the area of ​​the portion sandwiched between the molecular weight distribution curve from the lowest molecular weight point among the points corresponding to a weight fraction of 70% to the minimum molecular weight point and the horizontal axis corresponding to a weight fraction of 0% is taken as S2, the value of [{S2 / (S2+S1)}×100] is 64 to 90.

2. The polyamide resin composition according to claim 1, wherein the MFR of the polyamide resin composition is 0.01 g / 10 min or more and 20 g / 10 min or less when a 5,000 g quantity of the polyamide resin composition is heated to 300° C. in accordance with ISO 1133.

3. The polyamide resin composition according to claim 1, wherein the amount of functional groups [C1] per 1 g of the polyolefin is more than 25 μmol / g and less than 100 μmol / g, and the amount of amino groups [A1] per 1 g of the aliphatic polyamide resin is more than 25 μmol / g and less than 100 μmol / g.

4. When the amount of functional groups of the polyolefin contained in 1 g of the polyamide resin composition is [C2] and the amount of amino groups of the aliphatic polyamide resin is [A2], the product [C2] x [A2] is 250 to 750 ((μmol / g) 2 2. The polyamide resin composition according to claim 1, wherein 5. The polyamide resin composition according to claim 1, wherein the ratio [CH2] / [NHCO] of the number of methylene groups ([CH2]) to the number of amide groups ([NHCO]) in the aliphatic polyamide resin exceeds 5 on average.

6. The polyamide resin composition according to claim 1, wherein the aliphatic polyamide resin is at least one selected from the group consisting of PA11, PA12, PA69, PA610, PA612, PA910, PA912, PA1010, PA1012 and PA1212.

7. The polyamide resin composition according to claim 1, wherein the polyolefin has at least one functional group selected from the group consisting of a carboxy group, an acid anhydride group, a carboxylic acid ester group, a carboxylic acid imide group, a carboxylic acid amide group and an epoxy group, or a salt thereof.

8. The polyamide resin composition according to claim 1, wherein the polyolefin is at least one selected from the group consisting of copolymers having an (ethylene and / or propylene) / α-olefin copolymer as the main skeleton, at least a portion of which has a functional group exhibiting reactivity with an end group of an aliphatic polyamide resin, and (ethylene and / or propylene) / (α,β-unsaturated carboxylic acid and / or α,β-unsaturated carboxylic acid ester) copolymers.

9. The polyamide resin composition according to claim 1, wherein the weight average molecular weight (Mw) of said polyamide resin is 50,000 to 80,000.

10. The polyamide resin composition according to any one of claims 1 to 9, which is used for a hollow molded article for transporting a cooling liquid.

11. A tube, hose or pipe comprising the polyamide resin composition according to any one of claims 1 to 9.

12. A blown molded article having a single-layer structure of the polyamide resin composition according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • refrigerant pipe

    JP2008507436A

  • Optical communication device, optical communication system and light radiation element

    JP2025147519A

  • Substrate cleaning composition, method for manufacturing cleaned substrate using the same, and method for manufacturing device

    JP2025170460A

  • Laminated tube

    WO2015033982A1

  • Production of thermoplastic resin composition

    JP1997169903A

Cited By

  • Polyamide resin composition

    WO2026205514A1