Variable-resistance material, switch element material, switch layer, switch element, and storage device
A Te-Ge-Ga resistance change material with specific spectroscopic characteristics provides stable switching in next-generation memory devices, addressing the instability of traditional elements and enhancing memory performance.
Patent Information
- Application Number
- PCT/JP2024/010660
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-20
- Filing Date
- 2024-03-19
- Publication Date
- 2024-10-24
AI Technical Summary
Next-generation nonvolatile storage devices require stable switching action in resistance change materials, which traditional switch elements like transistors and diodes fail to provide, especially as memory devices become smaller and more integrated.
A resistance change material composed of 40% to 90% Te, 0% to 40% Ge, and 0% to 40% Ga, characterized by specific XPS and Raman spectroscopy peaks, is used to create a switch element with a stable amorphous state that maintains resistance changes without phase transition under applied voltage.
The material achieves a high ON/OFF current ratio and prolonged cycle count, ensuring stable switching action and increased memory device performance without crystalline state changes.
Smart Images

Figure JP2024010660_24102024_PF_FP_ABST
Abstract
Description
Resistance change material, material for switch element, switch layer, switch element and storage device
[0001] The present invention relates to a variable resistance material, a material for a switching element, a switching layer, a switching element, and a memory device.
[0002] Next-generation nonvolatile memory devices have been attracting attention as replacements for NAND flash memories. Resistance-change and phase-change memory devices have been proposed as next-generation nonvolatile memory devices, and development is underway to achieve larger capacities and higher speeds.
[0003] Furthermore, cross-point memory devices have attracted attention as a next-generation nonvolatile memory device structure (see Patent Documents 1 and 2). A cross-point memory device includes word lines, bit lines that are orthogonal to the word lines in a planar view, and memory elements and switch elements that are arranged at the intersections of the word lines and bit lines in a planar view. While transistors and diodes have traditionally been used as switch elements, the use of ovonic threshold switches (OTS elements), whose resistance changes depending on the applied voltage, has attracted attention as memory devices become smaller, have larger capacities, and are more highly integrated.
[0004] JP 2006-086526 A JP 2018-164085 A
[0005] In order to obtain a stable switching action, the OTS element is required to exhibit a stable resistance change with respect to the applied voltage.
[0006] In view of the above, an object of the present invention is to provide a variable resistance material, a material for a switching element, a switching layer, a switching element, and a memory device that are capable of achieving a stable switching action.
[0007] A description will be given of various aspects of a resistance change material, a material for a switching element, a switching layer, a switching element, and a memory device that solve the above problems.
[0008] The variable resistance material of aspect 1 is a variable resistance material containing, in atomic %, 40% to 90% Te, more than 0% to 40% Ge, and more than 0% to 40% Ga, and in an XPS spectrum measured by X-ray photoelectron spectroscopy, the apex of the XPS peak Px1 due to the Te3d5 / 2 orbital is the apex of amorphous GeTe. 5 The XPS peak Px1GT due to the Te3d5 / 2 orbital in the present invention is shifted to a lower energy side than the peak of the XPS peak Px1GT due to the Te3d5 / 2 orbital in the present invention. 5 " is a GeTe film produced by high-frequency magnetron sputtering using Ar gas. 5 means.
[0009] In the variable resistance material of Aspect 2, in Aspect 1, the apex of the XPS peak Px1 is preferably shifted to the lower energy side by 0.05 eV or more than the apex of the XPS peak Px1GT.
[0010] In the variable resistance material of Aspect 3, in Aspect 1 or Aspect 2, it is preferable that the half width Px1hw of the XPS peak Px1 is larger than the half width Px1GThw of the XPS peak Px1GT.
[0011] In the variable resistance material of Aspect 4, in Aspect 3, the ratio of the half width Px1hw of the XPS peak Px1 to the half width Px1GThw of the XPS peak Px1GT (Px1hw / Px1GThw) is preferably 1.01 or more.
[0012] The variable resistance material of Aspect 5 is any one of Aspects 1 to 4, further comprising, in the XPS spectrum, a half width Px2hw of an XPS peak Px2 due to a Ge 3d orbital, which is equal to or less than that of an amorphous GeTe 5 It is preferable that the full width at half maximum Px2GThw of the XPS peak Px2GT attributed to the Ge 3d orbital in the sample.
[0013] In the variable resistance material of Aspect 6, in Aspect 5, it is preferable that the ratio of the half width Px2hw of the XPS peak Px2 to the half width Px2GThw of the XPS peak Px2GT (Px2hw / Px2GThw) is 1.01 or more.
[0014] The variable resistance material of aspect 7 is a variable resistance material containing, in atomic %, 40% to 90% Te and more than 0% to 40% Ge, and is characterized in that it has at least three or more peaks in a binding energy range of 15 eV to 44 eV in an XPS spectrum measured by X-ray photoelectron spectroscopy.
[0015] The resistance change material of aspect 8 is a resistance change material containing, in atomic %, 40% to 90% Te, more than 0% to 40% Ge, and more than 0% to 40% Ga, and in a Raman spectrum measured by Raman spectroscopy, the apex of Raman peak Pr1, which is a combination of Raman peaks due to Ge—Te bonds and Te—Te bonds, is at a wavenumber of 118 cm -1 ~130cm -1 The half width Pr1hw of the Raman peak Pr1 is in the range of 5 is larger than the half-width Pr1GThw of the Raman peak Pr1GT in
[0016] The variable resistance material of Aspect 9 is preferably the same as Aspect 8, in which the ratio of the half width Pr1hw of the Raman peak Pr1 to the half width Pr1GThw of the Raman peak Pr1GT (Pr1hw / Pr1GThw) is 1.05 or more.
[0017] In the variable resistance material of Aspect 10, in Aspect 8 or Aspect 9, the apex of Raman peak Pr1 is preferably shifted to the higher wavenumber side than the apex of Raman peak Pr1GT.
[0018] The variable resistance material of aspect 11 is the same as that of aspect 10, except that the apex of the Raman peak Pr1 is 0.1 cm from the apex of the Raman peak Pr1GT. -1 It is preferable that the wavelength is shifted to the higher wavenumber side.
[0019] The variable resistance material of Aspect 12 is any one of Aspects 8 to 11, further comprising: a Raman peak Pr2 due to a Te—Te bond having a peak at a wavenumber of 135 cm -1 ~145cm -1 The apex of the Raman peak Pr2 is in the range of 5It is preferable that the peak of the Raman peak Pr2GT due to the Te-Te bond is shifted to the higher wavenumber side.
[0020] The variable resistance material of Aspect 13 is the variable resistance material of Aspect 12, wherein the apex of the Raman peak Pr2 is 0.1 cm from the apex of the Raman peak Pr2GT. -1 It is preferable that the wavelength is shifted to the higher wavenumber side.
[0021] The variable resistance material of Aspect 14 is a variable resistance material containing, in atomic %, 40% to 90% Te and more than 0% to 40% Ge, and is characterized in that the activation energy Ea when an amorphous thin film made of the variable resistance material crystallizes is 240 kJ / mol or more.
[0022] The variable resistance material of Aspect 15 is any one of Aspects 1 to 14, wherein the number of cycles is 5×10 2 It is preferable that the number of times is more than 1.
[0023] In the variable resistance material of Aspect 16, in any one of Aspects 1 to 15, it is preferable that the number of cycles x (times) and the activation energy Ea (kJ / mol) satisfy the relationship of the following formula (1): log 10 x≧0.011Ea+0.1 ... Equation (1)
[0024] The variable resistance material of Aspect 17 is any one of Aspects 1 to 16, and preferably contains, in atomic percent, 0% to 20% Sb.
[0025] The variable resistance material of Aspect 18 is any one of Aspects 1 to 17, and preferably contains substantially no Sb, Se, or As.
[0026] The variable resistance material of Aspect 19 is preferably a thin film in any one of Aspects 1 to 18.
[0027] A switching element material according to aspect 20 is characterized in that it is made of the variable resistance material according to any one of aspects 1 to 19.
[0028] The switch layer of Aspect 21 is characterized in that it is made of the variable resistance material of any one of Aspects 1 to 19.
[0029] A switch element of Aspect 22 is characterized by comprising a first electrode and the switch layer of Aspect 21 disposed on the first electrode.
[0030] The switching element of Aspect 23 is preferably the same as Aspect 22, further comprising a second electrode disposed opposite the first electrode with the switching layer interposed therebetween.
[0031] A storage device according to aspect 24 is characterized by comprising the switch element according to aspect 22 or aspect 23 and a storage element.
[0032] According to the present invention, it is possible to provide a variable resistance material, a material for a switching element, a switching layer, a switching element, and a memory device that are capable of achieving a stable switching action.
[0033] FIG. 1 is a schematic cross-sectional view of a switching element according to one embodiment of the present invention. FIG. 2 is a schematic cross-sectional view of a memory element according to one embodiment of the present invention. FIG. 3 is a schematic three-dimensional view of a memory device according to a first embodiment of the present invention. FIG. 4 is a schematic three-dimensional view of an enlarged memory device according to the first embodiment of the present invention. FIG. 5 is a schematic three-dimensional view of a modified memory device according to the first embodiment of the present invention. FIG. 6 is a schematic three-dimensional view of a memory device according to a second embodiment of the present invention. FIG. 7 is a schematic three-dimensional view of a modified memory device according to the second embodiment of the present invention. FIG. 8 is a diagram showing XPS spectra of the Te3d5 / 2 orbital in the resistance change materials of the examples and comparative examples. FIG. 9 is a diagram showing XPS spectra of the Ge3d orbital in the resistance change materials of the examples and comparative examples. FIG. 10 is a diagram showing XPS spectra of the Te4d orbital in the resistance change materials of the examples and comparative examples. FIG. 11 is a diagram showing XPS spectra of the Ga3d orbital in the resistance change materials of the examples and comparative examples. FIG. 12 is a diagram showing Raman spectra in the resistance change materials of the examples and comparative examples. FIG. 13 is a diagram showing the relationship between the activation energy and the number of cycles for the variable resistance materials and switching elements of the examples and comparative examples.
[0034] Preferred embodiments will be described below, but the following embodiments are merely examples and the present invention is not limited to the following embodiments.
[0035] <Variable Resistance Material> [XPS Spectrum] (First Invention) In a broad aspect of the variable resistance material of the present invention, there is provided a variable resistance material containing, in atomic %, 40% to 90% Te, more than 0% to 40% Ge, and more than 0% to 40% Ga, wherein in an XPS spectrum measured by X-ray photoelectron spectroscopy (XPS), the apex of the XPS peak Px1 due to the Te3d5 / 2 orbital is 40% to 90% Te, and the apex of the XPS peak Px1 due to the Te3d5 / 2 orbital is 40% to 90% Ge, and the apex of the XPS peak Px1 due to the Te3d5 / 2 orbital is 40% to 90% Ga ... 5 The variable resistance material having this structure is characterized by a shift to a lower energy side than the apex of the XPS peak Px1GT due to the Te3d5 / 2 orbital in GeTe (first invention). The electron density around Te is high. Therefore, the covalent bond of the Te bond is 5 The resistance change material of the present invention exhibits a higher value than the value of the reference value, and the amorphous state is highly stable. Therefore, the variable resistance material of the present invention does not undergo a phase change to a crystalline state in response to an applied voltage, and can achieve a stable switching action. In the present invention, the switching action refers to the property of changing the resistance in response to an applied voltage. In the following description, the switching action may also be referred to as the switching characteristic or the OTS characteristic. In the following description, the binding energy values of the XPS spectra refer to values corrected using the XPS peak Px1C due to the C1s orbital. In the present invention, "C" refers to hydrocarbon.
[0036] The apex of the XPS peak Px1 due to the Te3d5 / 2 orbital is in the binding energy range of 570 eV to 580 eV. More specifically, the apex of the XPS peak Px1 is preferably at 570 eV or higher, particularly preferably at 571 eV or higher, and more preferably at 580 eV or lower, 578 eV or lower, 576 eV or lower, particularly preferably at 574 eV or lower.
[0037] The apex of the XPS peak Px1 is preferably shifted to a lower energy side by 0.05 eV or more, 0.06 eV or more, 0.08 eV or more, particularly 0.10 eV or more, relative to the apex of the XPS peak Px1GT. By shifting the apex of the XPS peak Px1 to a lower energy side, the covalent bond of the Te bond is further enhanced, and the stability of the amorphous state is further increased. The upper limit of the shift amount is not particularly limited, but may be, for example, 0.3 eV or less.
[0038] The half-value width Px1hw of the XPS peak Px1 is preferably larger than the half-value width Px1GThw of the XPS peak Px1. In a variable resistance material having this configuration, the electron distribution around Te is broadened, and the electrons in the orbitals overlap more strongly. This increases the covalent bond strength, further increasing the stability of the amorphous state. Therefore, a more stable switching action can be achieved.
[0039] The half-width ratio (Px1hw / Px1GThw) is preferably 1.01 or more, 1.02 or more, 1.04 or more, 1.06 or more, 1.08 or more, 1.10 or more, particularly preferably 1.12 or more. As the half-width Px1hw increases, the covalent bond of the Te bond is further enhanced, and the stability of the amorphous state is further increased. The upper limit of the half-width ratio is not particularly limited, but may be, for example, 1.20 or less.
[0040] The resistance change material of the present invention is a resistance change material containing, in atomic %, 40% to 90% Te, more than 0% to 40% Ge, and more than 0% to 40% Ga, and in an XPS spectrum measured by X-ray photoelectron spectroscopy (XPS), the energy difference |Px1-Px1C| between the apex of the XPS peak Px1 due to the Te3d5 / 2 orbital and the apex of the XPS peak Px1C due to the C1s orbital is smaller than that of amorphous GeTe. 5 In the variable resistance material having this structure, the covalent bond of the Te bond is preferably smaller than the energy difference |Px1GT-Px1C| between the apex of the XPS peak Px1GT and the apex of the XPS peak Px1C due to the Te3d5 / 2 orbital. 5The temperature is higher than that of the amorphous state, and the stability of the amorphous state is even higher. Therefore, a more stable switching action can be obtained.
[0041] The apex of the XPS peak Px1C due to the C1s orbital is in the binding energy range of 279 eV to 294 eV. More specifically, the apex of the XPS peak Px1C is preferably at 281 eV or higher, particularly preferably at 282 eV or higher, and is preferably at 288 eV or lower, particularly preferably at 286 eV or lower.
[0042] The energy difference ratio |Px1-Px1C| / |Px1GT-Px1C| is preferably 0.9999 or less, 0.9998 or less, and particularly preferably 0.9997 or less. When the energy difference ratio satisfies the above value, the stability of the amorphous state is further increased. The lower limit of the energy difference ratio is not particularly limited, but may be, for example, 0.98 or more.
[0043] In the resistance change material of the present invention, the half width Px2hw of the XPS peak Px2 due to the Ge 3d orbital in the XPS spectrum is 5 It is preferable that the half-width Px2GThw of the peak Px2GT attributed to the Ge 3d orbital in the variable resistance material is larger than that of the peak Px2GThw attributed to the Ge 3d orbital in the variable resistance material. In the variable resistance material having this structure, the electron distribution around the Ge becomes wider, and the electrons in the orbitals overlap more strongly. This increases the covalent bond of the Ge bond, further increasing the stability of the amorphous state. Therefore, a more stable switching action can be obtained.
[0044] The apex of the XPS peak Px2 due to the Ge 3d orbital is in the binding energy range of 25 eV to 37 eV. More specifically, the apex of the XPS peak Px2 is preferably at 25 eV or higher, 27 eV or higher, particularly 29 eV or higher, and is preferably at 35 eV or lower, 33 eV or lower, particularly 31 eV or lower.
[0045] The half-width ratio (Px2hw / Px2GThw) is preferably 1.01 or more, 1.015 or more, particularly 1.02 or more. As the half-width Px2hw increases, the covalent bond of the Ge bond is further enhanced, and the stability of the amorphous state is further increased. The upper limit of the half-width ratio is not particularly limited, but may be, for example, 1.20 or less.
[0046] In the resistance change material of the present invention, in the XPS spectrum, the apex of the XPS peak Px3 due to the Te4d5 / 2 orbital is 5 The electron density around Te is high in the variable resistance material having such a structure. Therefore, the covalent bond of the Te bond is high in GeTe. 5 Therefore, the amorphous state is more stable, and a more stable switching action can be obtained.
[0047] The apex of the XPS peak Px3 due to the Te4d5 / 2 orbital is in a binding energy range of 35 eV to 44 eV. More specifically, the apex of the XPS peak Px3 is preferably at 35 eV or higher, 37 eV or higher, particularly 39 eV or higher, and is preferably at 44 eV or lower, 43 eV or lower, particularly 42 eV or lower. Note that within the binding energy range of 35 eV to 44 eV, an XPS peak due to the Te4d3 / 2 orbital is present on the higher energy side than the peak due to the Te4d5 / 2 orbital.
[0048] The apex of the XPS peak Px3 is preferably shifted to a lower energy side by 0.05 eV or more, 0.06 eV or more, 0.08 eV or more, 0.10 eV or more, particularly 0.11 eV or more, relative to the apex of the XPS peak Px3GT. By shifting the apex of the XPS peak Px3 to a lower energy side, the covalent bond of the Te bond is further enhanced, and the stability of the amorphous state is further increased. The upper limit of the shift amount is not particularly limited, but may be, for example, 0.3 eV or less.
[0049] The variable resistance material of the present invention further has an XPS peak Px3 attributable to the Te4d5 / 2 orbital whose half width Px3hw is smaller than that of amorphous GeTe. 5 The full width at half maximum Px3GT is preferably larger than the full width at half maximum Px3GThw of the peak Px3GT due to the Te4d5 / 2 orbital in the variable resistance material. A variable resistance material having this structure has a wider electron distribution around Te, resulting in stronger electron overlap between orbitals. This increases the covalent bond strength, further increasing the stability of the amorphous state. Therefore, a more stable switching action can be achieved.
[0050] The half-width ratio (Px3hw / Px3GThw) is preferably 1.01 or more, 1.02 or more, 1.04 or more, 1.06 or more, 1.08 or more, 1.10 or more, 1.12 or more, particularly preferably 1.15 or more. By increasing the half-width Px3hw, the covalent bond of the Te bond is further enhanced, and the stability of the amorphous state is further increased. The upper limit of the half-width ratio is not particularly limited, but may be, for example, 1.25 or less.
[0051] In the variable resistance material of the present invention, the apex of the XPS peak Px4a due to the Ga 3d orbital is preferably shifted to a lower energy side in the XPS spectrum than the apex of the XPS peak Px4b due to the Ga 3d orbital in a variable resistance material that does not contain Ag. A variable resistance material having this configuration has a high electron density around Ga. Therefore, the covalent bonding of the Ga bond is higher than in a variable resistance material that does not contain Ag, and the stability of the amorphous state is even higher. Therefore, a more stable switching action can be obtained.
[0052] The apex of the XPS peak Px4a due to the Ga 3d orbital is in the binding energy range of 15 eV to 25 eV. More specifically, the apex of the XPS peak Px4a is preferably at 15 eV or higher, 17 eV or higher, particularly preferably at 18 eV or higher, and is preferably at 25 eV or lower, 23 eV or lower, 21 eV or lower, particularly preferably at 20 eV or lower.
[0053] The apex of the XPS peak Px4a is preferably shifted to a lower energy side by 0.05 eV or more, 0.06 eV or more, particularly 0.08 eV or more, relative to the apex of the XPS peak Px4b. The shift of the apex of the XPS peak Px4a to a lower energy side further enhances the covalent bond of the Ga bond, thereby further increasing the stability of the amorphous state. The upper limit of the shift is not particularly limited, but may be, for example, 0.3 eV or less.
[0054] (Second Invention) In another broad aspect of the variable resistance material of the present invention, there is provided a variable resistance material containing, in atomic percent, 40% to 90% Te and greater than 0% to 40% Ge, characterized in that an XPS spectrum measured by X-ray photoelectron spectroscopy (XPS) has at least three peaks within a binding energy range of 15 eV to 44 eV (second invention). Variable resistance materials with peaks within this binding energy range have a high electron density around the Te and Ge, as well as a broader electron distribution and stronger electron orbital overlap. This results in a stronger covalent bond and a more stable amorphous state. This allows for a stable switching action.
[0055] Peaks observed within the binding energy range of 15 eV to 44 eV are preferably the XPS peak Px2 (binding energy 25 eV to 35 eV) due to the Ge3d orbital, the XPS peak Px3 (binding energy 35 eV to 44 eV) due to the Te4d orbital, and the XPS peak Px4a (binding energy 15 eV to 25 eV) due to the Ga3d orbital. However, the variable resistance material may also include XPS peaks due to orbitals other than those mentioned above within the binding energy range of 15 eV to 44 eV in the XPS spectrum. Note that in any element, the same electron orbital may split into two peaks due to spin-orbit interaction, in which case the number of peaks is counted as one. For example, the Te4d orbital splits into two peaks, the Te4d5 / 2 orbital and the Te4d3 / 2 orbital, but this is counted as one peak.
[0056] [Raman Spectrum] (Third Invention) In another broad aspect of the resistance change material of the present invention, there is provided a resistance change material containing, in atomic %, 40% to 90% Te, more than 0% to 40% Ge, and more than 0% to 40% Ga, wherein in a Raman spectrum measured by Raman spectroscopy, a Raman peak Pr1, which is a combination of Raman peaks due to Ge—Te bonds and Te—Te bonds, has a vertex at a wavenumber of 118 cm -1 ~130cm -1 The half width Pr1hw of the Raman peak Pr1 is in the range of 5 The Raman peak Pr1 is characterized by being larger than the half-width Pr1GTw of the Raman peak Pr1GT in (3rd invention). A variable resistance material having this configuration has a high covalent bond in the Te-Te bond, increasing the stability of the amorphous state. Therefore, a stable switching action can be obtained. Because the Raman peaks resulting from the Ge-Te bond and the Te-Te bond overlap, making peak separation difficult, the Raman peak Pr1 is treated as a peak resulting from both the Ge-Te bond and the Te-Te bond.
[0057] The apex of the Raman peak Pr1 is at a wavenumber of 118 cm -1 ~130cm -1 More specifically, the apex of the Raman peak Pr1 is in the range of 118 cm -1 Above, 120cm -1 Above, especially 123cm -1 It is preferable that the temperature is above 130 cm -1 Below, 128cm -1 Below, especially 126cm -1 It is preferred that the following be present:
[0058] The half-width ratio (Pr1hw / Pr1GThw) is preferably 1.01 or more, 1.05 or more, 1.10 or more, 1.15 or more, particularly preferably 1.20 or more. As the half-width Pr1hw increases, the covalent bond property of the Te-Te bond is further enhanced, and the stability of the amorphous state is further increased. The upper limit of the half-width ratio is not particularly limited, but may be, for example, 1.40 or less.
[0059] In the variable resistance material of the present invention, the peak of the Raman peak Pr1 is preferably shifted to a higher wave number side than the peak of the Raman peak Pr1GT. 5 Therefore, the amorphous state is more stable, and a more stable switching action can be obtained.
[0060] The apex of the Raman peak Pr1 is 0.1 cm from the apex of the Raman peak Pr1GT. -1 More than 0.4cm -1 More than 0.7cm -1 Above, especially 1 cm -1 By shifting the apex of the Raman peak Pr1 to the high wavenumber side, the covalent bond of the Te-Te bond is further enhanced, and the stability of the amorphous state is further increased. There is no particular restriction on the upper limit of the shift amount, but it is preferably 2 cm, for example. -1 The following may also be used.
[0061] The resistance change material of the present invention further has a Raman peak Pr2 due to Te—Te bonds at a wavenumber of 135 cm -1 ~145cm -1 The apex of the Raman peak Pr2 is in the range of 5 In the variable resistance material having such a structure, the covalent bonding of the Te-Te bond is preferably shifted to the high wave number side relative to the peak of the Raman peak Pr2GT due to the Te-Te bond. 5 Therefore, the amorphous state is more stable, and a more stable switching action can be obtained.
[0062] The apex of the Raman peak Pr2 is 0.1 cm from the apex of the Raman peak Pr2GT. -1 More than 0.4cm -1 More than 0.7cm -1 Above, especially 1 cm -1By shifting the apex of the Raman peak Pr1 to the high wavenumber side, the covalent bond of the Te-Te bond is further enhanced, and the stability of the amorphous state is further increased. The upper limit of the shift amount is not particularly limited, but is, for example, 3.5 cm -1 The following may also be used.
[0063] [Activation Energy Ea] (Fourth Invention) In another broad aspect of the variable resistance material of the present invention, there is provided a variable resistance material containing, in atomic %, 40% to 90% Te and more than 0% to 40% Ge, wherein the activation energy Ea at which an amorphous thin film made of the variable resistance material crystallizes is 240 kJ / mol or more (fourth invention).
[0064] The activation energy Ea can be determined using the Kissinger method. Specifically, the method is as follows: First, a 150-nm-thick amorphous thin film made of a variable resistance material is prepared. Next, the electrical resistance of the amorphous thin film is measured using the two-terminal method while heating it at varying heating rates within the range of 5 to 15°C / min. Next, the temperature at which the electrical resistance suddenly drops is taken as the crystallization temperature, and the activation energy at the time of crystallization is calculated using the following formula (2). Note that the measurement can be performed not only in an inert atmosphere such as argon gas or nitrogen gas, but also in air. Here, α is the heating rate of the sample, Tx is the crystallization temperature, R is the gas constant, and C is a constant.
[0065] ln(α / Tx 2 )=-(Ea / RTx)+C...Formula (2)
[0066] The lower limit of the activation energy Ea is 240 kJ / mol or more, and is preferably 250 kJ / mol or more, 270 kJ / mol or more, 285 kJ / mol or more, 300 kJ / mol or more, 330 kJ / mol or more, 350 kJ / mol or more, and particularly preferably 360 kJ / mol or more. A variable resistance material that satisfies the above activation energy has a high activation energy during crystallization and high stability in the amorphous state. Therefore, variable resistance materials having the above activation energy are particularly useful from the perspective of further improving cycle characteristics. The upper limit of the activation energy Ea is not particularly limited, but may be, for example, 500 kJ / mol or less, particularly 450 kJ / mol or less.
[0067] The first to fourth inventions can be implemented individually. However, the first to fourth inventions may be implemented in combination with some or all of them. Hereinafter, the first to fourth inventions may be collectively referred to as the present invention.
[0068] Since the variable resistance material of the present invention is stable in an amorphous state, it is possible to increase the number of cycles when used as a switching element. That is, the ON / OFF current ratio can be maintained even when ON and OFF are repeatedly switched on and off. Specifically, the lower limit of the number of cycles (the number of times ON / OFF switching is repeated until the ON / OFF current ratio becomes 10% of the initial measurement value) is 5×10 2 More than once, 1 x 10 3 More than once, especially 1 x 10 4 If the number of cycles is too small, it becomes difficult to use the device as a switching element. The upper limit of the number of cycles is not particularly limited, but is, for example, 1×10 10 times or less, 1×10 9 times or less, 1×10 8 times or less, especially 1 x 10 7 It may be less than once.
[0069] The threshold voltage refers to the voltage value at which the electrical resistance of the variable resistance material changes suddenly from a high resistance state to a low resistance state. The voltage applied (applied voltage) at this time is not limited to DC voltage, AC voltage, pulse voltage, etc., but pulse voltage is preferred from the viewpoint of preventing heat accumulation in the switching element. The ON current value refers to the current value (ON current value) that flows when a voltage equal to or greater than the threshold voltage is applied. The OFF current value refers to the current value (OFF current value) that flows when a voltage equal to half the threshold voltage is applied. The ON / OFF current ratio refers to the value obtained by dividing the ON current value by the OFF current value. The upper limit of the threshold voltage is preferably 10 V or less, 8 V or less, 6 V or less, and particularly 5 V or less. By having the threshold voltage within the above range, it is possible to drive the device with less energy. The lower limit of the threshold voltage is not particularly limited, but may be 0.5 V or more, 1 V or more, particularly 1.5 V or more.
[0070] The variable resistance material of the present invention preferably satisfies the relationship of the following formula (1), where x is the number of cycles and Ea is the activation energy (kJ / mol). A variable resistance material that satisfies this relationship is particularly suitable as a switching element.
[0071] log 10 x≧0.011Ea+0.1 ... Equation (1)
[0072] The variable resistance material of the present invention contains, in atomic percent, 40% to 90% Te and more than 0% to 40% Ge. In particular, the variable resistance materials of the first and third inventions contain, in atomic percent, 40% to 90% Te, more than 0% to 40% Ge, and more than 0% to 40% Ga. The variable resistance materials of the second and fourth inventions may contain more than 0% to 40% Ga, or may not contain Ga at all. The reasons for specifying the composition in this way and the content of each component are explained below. In the following explanation, "%" means "atomic percent" unless otherwise specified. Furthermore, in the present invention, "x + y + z + ..." refers to the total content of each component. Here, each component does not necessarily have to be contained as an essential component, and it is acceptable for a component not to be contained (content 0%). Furthermore, "x+y+z+... A% to B%" includes, for example, "x=0%, y+z+... A% to B%" and "x=0%, y=0%, z+... A% to B%".
[0073] The variable resistance material of the present invention contains at least Te. Te is a component that constitutes the variable resistance material and provides switching action. The Te content is 40% to 90%. More specifically, the lower limit of the Te content is preferably 40% or more, 42% or more, 47% or more, 50% or more, more than 50%, 51% or more, 53% or more, 55% or more, 60% or more, 61% or more, 65% or more, 67% or more, 70% or more, and particularly 71% or more. The upper limit of the Te content is preferably 90% or less, 89% or less, 85% or less, 82.5% or less, 80% or less, 75% or less, and particularly 72.5% or less. If the Te content is too low, the amorphous state tends to become unstable. Furthermore, it becomes difficult to obtain switching action. If the Te content is too high, the amorphous state tends to become unstable. Furthermore, the OFF current density tends to increase.
[0074] Ge is a component that stabilizes the amorphous state of the resistance change material. The Ge content is greater than 0% to 40%. More specifically, the lower limit of the Ge content is preferably greater than 0%, 0.1% or more, 1% or more, 3% or more, 5% or more, 7% or more, 10% or more, 11% or more, and particularly 13% or more. The upper limit of the Ge content is preferably 40% or less, 30% or less, and particularly 20% or less. If the Ge content is too low, the amorphous state tends to become unstable. If the Ge content is too high, it becomes difficult to obtain a switching action. Furthermore, the manufacturing cost tends to increase.
[0075] The lower limit of the Ge+Te content (total amount of Ge and Te) is preferably more than 40%, 41% or more, 45% or more, 50% or more, 60% or more, 65% or more, 70% or more, 75% or more, and particularly 80% or more. The upper limit of the Ge+Te content is preferably 99% or less, 98% or less, 97% or less, and particularly 95% or less. If the Ge+Te content is too low, the amorphous state tends to become unstable. Also, it becomes difficult to obtain a switching action. If the Ge+Te content is too high, it becomes difficult to obtain a switching action.
[0076] Ga is a component that easily increases the electron density around Te when introduced into the glass network. Therefore, it can reduce the OFF current and particularly contribute to improving the ON / OFF current ratio. The lower limit of the Ga content is preferably 0% or more, more than 0%, 1% or more, 2% or more, 3% or more, and particularly 5% or more. The upper limit of the Ga content is preferably 59% or less, 58% or less, 55% or less, 50% or less, 45% or less, 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, 15% or less, 14% or less, 13% or less, and particularly 10% or less. If the Ga content is too high, the amorphous state tends to become unstable.
[0077] Ag is a component that particularly stabilizes the amorphous state, easily increases the activation energy, and contributes to improving the number of cycles. The lower limit of the Ag content is preferably 0% or more, more than 0%, 1% or more, 2% or more, 3% or more, 5% or more, and particularly 6% or more. The upper limit of the Ag content is preferably 59% or less, 58% or less, 55% or less, 50% or less, 45% or less, 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, 15% or less, 14% or less, 13% or less, 11% or less, and particularly 10% or less. If the Ag content is too high, the amorphous state tends to become unstable.
[0078] From the viewpoint of further stabilizing the amorphous state, the lower limit of the Ga+Ag content (total amount of Ga and Ag) is preferably 0% or more, more than 0%, 0.1% or more, 0.5% or more, 1% or more, 2% or more, 3% or more, and particularly preferably 5% or more, and the upper limit of the Ga+Ag content is preferably 59% or less, 58% or less, 55% or less, 50% or less, 45% or less, 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, 15% or less, 14% or less, 13% or less, 10% or less, and particularly preferably 9% or less.
[0079] From the viewpoint of further reducing the OFF current value, the lower limit of Ga / (Ga+Ag) is preferably 0.1 or more, particularly preferably 0.2 or more, and the upper limit of Ga / (Ga+Ag) is preferably 1.2 or less, particularly preferably less than 1.2, particularly preferably 1.1 or less. Here, Ga / (Ga+Ag) is the value obtained by dividing the Ga content by the combined amount of Ga and Ag.
[0080] From the viewpoint of further increasing the number of cycles, the lower limit of Ag / (Ga+Ag) is preferably 0.1 or more, particularly 0.2 or more, and the upper limit of Ag / (Ga+Ag) is preferably 1.2 or less, less than 1.2, particularly preferably 1.1 or less, where Ag / (Ga+Ag) is the value obtained by dividing the Ag content by the combined amount of Ga and Ag.
[0081] The variable resistance material of the present invention may contain the following components in addition to the above components.
[0082] Si, Al, Sn, Bi, Cu, Zn, Y, In, Ca, and Mg are components that stabilize the amorphous state of the variable resistance material and tend to improve the number of cycles. In the present invention, the number of cycles refers to the number of times the ON / OFF current is repeatedly switched until the ON / OFF current ratio becomes 10% of the initial measured value. These components also tend to increase the ON / OFF current ratio by decreasing the OFF current. Therefore, the variable resistance material of the present invention preferably has a Si+Al+Sn+Bi+Cu+Zn+Y+In+Ca+Mg content (the total amount of Si, Al, Sn, Bi, Cu, Zn, Y, In, Ca, and Mg) of 0 to 59%. More specifically, the lower limit of the Si+Al+Sn+Bi+Cu+Zn+Y+In+Ca+Mg content is preferably 0% or more, 1% or more, and particularly 2% or more. The upper limit of the content of Si+Al+Sn+Bi+Cu+Zn+Y+In+Ca+Mg is preferably 59% or less, 58% or less, 55% or less, 50% or less, 45% or less, 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, 15% or less, 14% or less, 13% or less, 10% or less, and particularly preferably 9% or less. The above content can also be rephrased as "containing one or more components selected from Si, Al, Sn, Bi, Cu, Zn, Y, In, Ca, and Mg." If the content of these components is too low, the above effects are difficult to achieve. If the content of these components is too high, the amorphous state tends to become unstable. Furthermore, the switching action is difficult to achieve. The lower limit of the content of each of the components Si, Al, Sn, Bi, Cu, Zn, Y, In, Ca, and Mg is preferably 0% or more, more than 0%, 0.1% or more, 0.5% or more, 1% or more, and particularly preferably 2% or more. The upper limit of the content of each of the components Si, Al, Sn, Bi, Cu, Zn, Y, In, Ca, and Mg is preferably 59% or less, 58% or less, 55% or less, 50% or less, 45% or less, 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, 15% or less, 14% or less, 13% or less, 10% or less, and particularly preferably 9% or less.
[0083] Sb is a component that easily destabilizes the amorphous state at high temperatures. Therefore, the Sb content is preferably 0% to 20%. More specifically, the upper limit of the Sb content is preferably 20% or less, 15% or less, 10% or less, 9% or less, less than 5%, 4% or less, 3% or less, or 2% or less, and it is particularly preferable that Sb is not contained substantially. In this specification, "substantially not contained" means that Sb is not intentionally contained in the raw materials, and does not exclude contamination at the impurity level. Objectively, this refers to a content of each component of less than 0.1%.
[0084] Se is a component that easily stabilizes the amorphous state of the resistance change material. The upper limit of the Se content is preferably 58% or less, 55% or less, particularly 50% or less. The lower limit of the Se content is preferably 0% or more, 1% or more, 5% or more, 10% or more, particularly 20% or more. If the Se content is too high, the amorphous state tends to become unstable. Se is also a toxic component. Therefore, from the viewpoint of reducing the burden on the environment, it is preferable that the upper limit of the Se content be 40% or less, 30% or less, 20% or less, 10% or less, particularly substantially none.
[0085] As is a component that easily stabilizes the amorphous state of the resistance change material. However, because As is a toxic component, from the viewpoint of reducing the environmental impact, the As content is preferably 0% to 30%. More specifically, the upper limit of the As content is preferably 30% or less, 25% or less, 20% or less, 10% or less, 5% or less, or 3% or less, and it is particularly preferable that As is not contained substantially.
[0086] The variable resistance material of the present invention preferably contains substantially no Sb, Se, or As, which further facilitates reducing the environmental load.
[0087] If the content of B, C, N, F, Cl, Br, and I is too high, the amorphous state tends to become unstable. Furthermore, weather resistance tends to decrease. Therefore, the upper limit of the content of B + C + N + F + Cl + Br + I (the total amount of B, C, N, F, Cl, Br, and I) is preferably 50% or less, 45% or less, 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, 15% or less, 14% or less, 12% or less, 10% or less, 8% or less, 6% or less, and particularly preferably 5% or less. Furthermore, the upper limit of the content of each of the components B, C, N, F, Cl, Br, and I is preferably 50% or less, 45% or less, 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, 15% or less, 14% or less, 12% or less, 10% or less, 8% or less, 6% or less, and particularly preferably 5% or less. However, from the viewpoint of increasing the crystallization temperature, B, C, N, F, Cl, Br and I may be contained in a total amount of 0% or more, 1% or more, particularly 2% or more.
[0088] If the content of P, Cr, Mn, Ti, and Fe is too high, the amorphous state tends to become unstable. Therefore, the content of P + Cr + Mn + Ti + Fe (the total amount of P, Cr, Mn, Ti, and Fe) is preferably 0% to 10%. More specifically, the upper limit of the content of P + Cr + Mn + Ti + Fe is preferably 10% or less, 5% or less, 1% or less, less than 1%, or 0.1% or less, and it is particularly preferred that they are not substantially contained. Note that the content of each of the P, Cr, Mn, Ti, and Fe components is preferably 0% to 10%. More specifically, the upper limit of the content of each of the P, Cr, Mn, Ti, and Fe components is preferably 10% or less, 5% or less, 1% or less, less than 1%, or 0.1% or less, and it is particularly preferred that they are not substantially contained.
[0089] From the viewpoint of reducing the environmental load, it is preferable that Cd, Tl, and Pb are not substantially contained.
[0090] The composition of the variable resistance material can be evaluated using energy dispersive X-ray spectroscopy (EDX), electron probe microanalyzer (EPMA), X-ray fluorescence analysis (XRF), etc. EDX may also be evaluated using a TEM-EDX or SEM-EDX device attached to a transmission electron microscope (TEM) or a scanning electron microscope (SEM), etc.
[0091] The variable resistance material of the present invention has a large ON / OFF current ratio and exhibits a stable switching action. Specifically, the ON / OFF current ratio is 1×10 4 That's it, 1 x 10 5 Above, especially 1 x 10 6 By satisfying the above values, better OTS characteristics can be obtained.
[0092] The variable resistance material of the present invention preferably has a crystallization temperature Tx of 150° C. or higher, 160° C. or higher, particularly 170° C. or higher. When the crystallization temperature Tx satisfies the above value, crystallization due to heat generated during switching is less likely to occur, making it easier to further increase the number of cycles. The upper limit of the crystallization temperature Tx is not particularly limited, but may be, for example, 500° C. or lower, 450° C. or lower, particularly 400° C. or lower.
[0093] The crystallization temperature Tx of the variable resistance material can be evaluated using differential thermal analysis (DTA) or differential scanning calorimetry (DSC). Alternatively, the temperature dependence of electrical resistance may be measured in a two-terminal electrical resistance measurement, and the temperature at which the electrical resistance drops sharply may be evaluated as the crystallization temperature Tx. Furthermore, the obtained variable resistance material may be heat-treated at a predetermined temperature, and the point at which a crystallization peak appears in XRD may be evaluated as the crystallization temperature Tx. It is preferable that the crystallization temperature Tx evaluated by any of the above methods satisfies the preferred value of the crystallization temperature Tx described above. In particular, it is preferable that the crystallization temperature Tx evaluated in terms of the temperature dependence of electrical resistance satisfies the preferred value of the crystallization temperature Tx described above.
[0094] The variable resistance material of the present invention is preferably used as a thin film (variable resistance film). The thin film (variable resistance film) is particularly suitable for use as a switch layer or a switch memory layer, which will be described later. However, the variable resistance material is not limited to a thin film.
[0095] The film thickness of the thin film (resistance change film) is preferably 1 nm to 300 nm. More specifically, the lower limit of the film thickness of the resistance change film is preferably 1 nm or more, 2 nm or more, 5 nm or more, 10 nm or more, 30 nm or more, and particularly preferably more than 50 nm, and the upper limit of the film thickness of the resistance change film is preferably 300 nm or less, 200 nm or less, and particularly preferably 100 nm or less. If the film thickness is too small, the current value (OFF current) in the high resistance state tends to be high. If the film thickness is too large, the threshold voltage tends to be high.
[0096] The material for a switching element of the present invention is preferably made of the above-described variable resistance material of the present invention. Furthermore, the switching layer of the present invention is preferably made of the above-described variable resistance material of the present invention. As described above, the variable resistance material of the present invention has an excellent switching action, and therefore can be suitably used as a material for a switching layer and a switching element having a switching layer.
[0097] The variable resistance material of the present invention can be produced, for example, as follows. First, raw materials are mixed to obtain the desired composition. Next, the mixed raw materials are placed in a quartz glass ampoule that has been heated and evacuated, and the ampoule is sealed with an oxygen burner while evacuating. Next, the sealed quartz glass ampoule is kept at approximately 650°C to 1000°C for 6 to 12 hours. After that, the bulk variable resistance material can be obtained by rapidly cooling to room temperature.
[0098] The raw materials may be elemental raw materials (Ge, Ga, Si, Te, Ag, I, etc.), or compound raw materials (GeTe 4 , Ga 2 Te 3 , AgI, etc.) may be used. These may also be used in combination.
[0099] By using the obtained variable resistance material as a target, a thin film (variable resistance film) having the above-described composition can be formed.
[0100] It is also possible to form a thin film (resistance change film) having the above-described composition by adjusting the film formation output appropriately using a multi-sputtering method using a pure element M target (Ge, Te, Sb, Si, Al, Ga, Sn, Bi, Cu, Ag, Zn, Y, In, Ca, and Mg), a binary alloy target, or a ternary or higher alloy target as the target, and adjusting the components.
[0101] The method for producing the thin film is not particularly limited, and examples of the PVD method that can be used include sputtering, vacuum deposition, and ion plating. Alternatively, examples of the thin film production method that can be selected include CVD (Chemical Vapor Deposition), ALD (Atomic Layer Deposition), and the like. In particular, it is preferable to use the sputtering method because it allows for easy composition control and film thickness control.
[0102] <Switch Element> Fig. 1 is a schematic cross-sectional view of a switch element according to one embodiment of the present invention. The switch element 10 includes a first electrode 1, a second electrode 2, and a switch layer 3 disposed on a major surface of the first electrode 1. The second electrode 2 is disposed opposite the first electrode 1. In this embodiment, the switch layer 3 is disposed between the first electrode 1 and the second electrode 2. In other words, the switch element 10 of this embodiment includes the switch layer 3, the first electrode 1 disposed on one major surface of the switch layer 3, and the second electrode 2 disposed on the other major surface of the switch layer 3.
[0103] The switch element 10 of the present invention can be suitably used in a cross-point type memory device or a BiCS (Bit-Cost Scalable) type memory device, which will be described later. In the case of a BiCS type memory device, the switch element 10 of the present invention preferably has the first electrode 1 disposed on the outer circumferential surface of the switch layer 3 and the second electrode 2 disposed on the inner circumferential surface of the switch layer 3.
[0104] The first electrode 1 and the second electrode 2 can be made of an inorganic material. Examples of inorganic materials that can be used include metal materials and ceramic materials. For example, the first electrode 1 and the second electrode 2 are preferably made of at least one material selected from tungsten, titanium, copper, platinum, tungsten nitride, and titanium nitride. Tungsten, titanium, copper, and platinum are preferred metal materials. Furthermore, tungsten nitride and titanium nitride are preferred ceramic materials.
[0105] The thicknesses of the first electrode 1 and the second electrode 2 can be designed as appropriate. For example, the upper limit of the thickness of the first electrode 1 and the second electrode 2 is preferably 200 nm or less, 100 nm or less, 80 nm or less, 60 nm or less, and particularly preferably 50 nm or less, respectively. The smaller the thickness of the first electrode 1 and the second electrode 2, the more advantageous it is for increasing the capacity of the memory device. The lower limit of the thickness of the first electrode 1 and the second electrode 2 is preferably 1 nm or more, and particularly preferably 2 nm or more, respectively, for example.
[0106] The switch layer 3 is formed from the resistance change material of the present invention and exhibits OTS characteristics. More specifically, the switch layer 3 is preferably made of a thin film (resistance change film). The resistance state of the switch layer 3 changes depending on the applied voltage. That is, when a voltage equal to or greater than the threshold voltage is applied, the switch layer 3 enters a low resistance state (ON state). Furthermore, when a voltage equal to half the threshold voltage is applied, the switch layer 3 enters a high resistance state (OFF state). In the present invention, the switch layer 3 is amorphous, and no phase change occurs due to the application of a voltage. In other words, the switch layer 3 does not undergo a phase change to a crystalline state due to the application of a voltage.
[0107] The switch layer 3 is disposed in contact with at least one electrode. In other words, the switch layer 3 is preferably disposed on the first electrode 1. In yet another expression, the first electrode 1 is preferably disposed on the switch layer 3. In addition, it is preferable to include a second electrode 2 disposed at a position facing the first electrode 1 with the switch layer 3 interposed therebetween.
[0108] The thickness of the switch layer 3 can be appropriately designed depending on the desired threshold voltage. The upper limit of the thickness of the switch layer 3 is preferably, for example, 300 nm or less, 200 nm or less, particularly 100 nm or less. If the thickness is too large, the threshold voltage is likely to become too high. The lower limit of the thickness of the switch layer 3 is preferably, for example, 1 nm or more, 2 nm or more, 5 nm or more, 10 nm or more, 30 nm or more, particularly more than 50 nm.
[0109] <Memory Element> Fig. 2 is a schematic cross-sectional view of a memory element according to one embodiment of the present invention. The memory element 21 includes a first electrode 11, a second electrode 12, and a switch memory layer 4 disposed on a major surface of the first electrode 11. The second electrode 12 is disposed opposite the first electrode 11. In this embodiment, the switch memory layer 4 is disposed between the first electrode 11 and the second electrode 12. In other words, the memory element 21 of this embodiment includes the switch memory layer 4, the first electrode 11 disposed on one major surface of the switch memory layer 4, and the second electrode 12 disposed on the other major surface of the switch memory layer 4. The switch memory layer 4 is made of a resistance change film.
[0110] The first electrode 11 and the second electrode 12 can be made of an inorganic material. Examples of inorganic materials that can be used include metal materials and ceramic materials. Examples of metal materials that can be used include tungsten, titanium, copper, and platinum. Examples of ceramic materials that can be used include tungsten nitride and titanium nitride.
[0111] The thickness of the first electrode 11 and the second electrode 12 can be designed as appropriate. For example, it is preferable that the thickness of the first electrode 11 and the second electrode 12 is 200 nm or less, 100 nm or less, 80 nm or less, 60 nm or less, and particularly 50 nm or less, respectively. The smaller the thickness of the first electrode 11 and the second electrode 12, the more advantageous it is for increasing the capacity of the memory device. The lower limit of the thickness of the first electrode 11 and the second electrode 12 is, for example, preferably 1 nm or more, and particularly preferably 2 nm or more, respectively.
[0112] The memory element 21 is a resistance change memory element and includes a switch memory layer 4 that functions as both a memory and a switch element. For example, applying a predetermined voltage or higher to the switch memory layer 4 changes the state to a low resistance state LR1, allowing information to be recorded. Furthermore, decreasing the applied voltage from the low resistance state LR1 results in a state in which information is recorded, where the state becomes a high resistance state HR1. Furthermore, applying a read voltage without performing an erase operation changes the state to a low resistance state LR2. On the other hand, applying a read voltage in a high resistance state in which no information is recorded or an erase operation has been performed results in a high resistance state HR2. At this time, information can be recorded by associating 1 and 0 with LR2 and HR2, respectively. Furthermore, the operation method is not limited to the above-described method. For example, after recording information, the applied voltage can be reduced to 0, and then a read voltage can be applied, resulting in LR2. On the other hand, applying a read voltage after an erase operation results in HR2, whereby information can be recorded by associating 1 and 0 with each.
[0113] <Storage Device> (First Embodiment) A storage device of this embodiment preferably includes a switch element and a storage element.
[0114] 3 is a schematic three-dimensional view of the memory device according to the first embodiment of the present invention, and FIG. 4 is a schematic three-dimensional view of an enlarged version of the memory device according to the first embodiment of the present invention. As shown in FIGS. 3 and 4, the memory device 100 includes a switch element 10, a memory element 20, a word line 30, and a bit line 40. The bit line 40 is orthogonal to the word line 30 in a plan view. The switch element 10 and the memory element 20 are disposed at the intersection of the word line 30 and the bit line 40 in a plan view. In other words, the memory device 100 of this embodiment is a so-called cross-point memory device.
[0115] 5 is a schematic three-dimensional diagram of a modified example of the memory device according to the first embodiment of the present invention. The memory device 200 includes a switch element 10, a memory element 20, a word line 30, and a bit line 40. The bit line 40 is disposed in a through hole provided in the word line 30. The memory element 20 and the switch element 10 are disposed on the outer periphery of the bit line 40. The switch element 10 has a first electrode 1 disposed on the outer periphery of the switch layer 3, and a second electrode 2 disposed on the inner periphery opposite the first electrode 1, with the switch layer 3 sandwiched therebetween. In other words, the memory device 200 of this modified example is a so-called BiCS type memory device. As such, the memory device of the present invention is not limited to a cross-point type memory device, and may be various other memory devices.
[0116] Any memory element such as a resistance change memory element, a magnetoresistive memory element, a phase change memory element, or a ferroelectric memory element can be used as the memory element 20. Preferred embodiments of each memory element will be described below.
[0117] The resistance change memory element includes a resistance change layer. More specifically, the resistance change memory element preferably includes a stacked body in which a resistance change layer is sandwiched between an upper electrode and a lower electrode. The resistance change layer is preferably made of a metal oxide material, a metal nitride material, or a chalcogenide material. The metal oxide material is, for example, NiO x , NbO x , TiO x , TaO x , HfO x , ZrO x , MoO x , W.O. x , and Pr 1-x Ca x MnO 3 (PCMO). The metal nitride material is preferably at least one selected from, for example, SiN x , AlN x , ZrN x , NiN x , CuN x , CrN xThe chalcogenide material is preferably at least one selected from the group consisting of Ge—Te, Sb—Te, Ge—Sb—Te, Si—Sb—Te, Ge—Ga—Te, In—Sb—Te, Ge—Se—As, and Ge—Se—As—Te. The resistance change layer may be made of carbon nanotubes.
[0118] In the resistance change memory element, the upper electrode and / or the lower electrode are preferably made of at least one selected from tungsten, titanium, copper, platinum, tungsten nitride, and titanium nitride. Tungsten, titanium, copper, and platinum are preferred as metal materials. Tungsten nitride and titanium nitride are preferred as ceramic materials.
[0119] The magnetoresistive memory element includes a stack (TMR element) in which an insulating layer is sandwiched between ferromagnetic layers. The insulating layer is made of an insulating material, such as MgO, CaO, SrO, and Al. 2 O 3 The insulating layer preferably comprises at least one material selected from the group consisting of CoFeB, FeB, NiFe, MnIr, Fe, CoPt, CoNi, Co, Ni, Pt, Ni, and Mn. The insulating layer preferably comprises at least one material selected from the group consisting of CoFeB, FeB, NiFe, MnIr, Fe, CoPt, CoNi, Co, Ni, Pt, Ni, and Mn.
[0120] The phase-change memory element is a memory layer made of a phase-change material. More specifically, the phase-change memory element preferably includes a stacked body having a phase-change layer sandwiched between an upper electrode and a lower electrode. The phase-change layer is preferably made of a chalcogenide material. The chalcogenide material is preferably at least one selected from, for example, Ge—Te, Sb—Te, Ge—Sb—Te, Si—Sb—Te, Ge—Ga—Te, In—Sb—Te, Cu—Ge—Te, Cr—Ge—Te, Mn—Te, Ge—Se—As, and Ge—Se—As-Te.
[0121] The ferroelectric memory element includes a ferroelectric layer. More specifically, the ferroelectric memory element preferably includes a stacked body in which a ferroelectric layer is sandwiched between an upper electrode and a lower electrode. The ferroelectric layer is preferably composed of a ferroelectric material containing hafnium oxide, and is preferably composed of hafnium oxide doped with at least one element selected from Si, Zr, Ge, Gd, La, Y, and Yb. The ferroelectric layer may also be composed of at least one element selected from lead zirconate titanate (PZT), strontium bismuthate tantalate (SBT), and bismuth ferrite (BFO).
[0122] Second Embodiment The storage device of the present invention is not limited to a configuration including a switch layer and a storage element separately. For example, the storage device of the present invention may be configured to include only a switch element. In this case, the switch element may function as both a switch element and a storage element. For example, the storage device of this embodiment preferably includes a resistance change storage element (storage element 21) having the above-described memory function and switch element function. In this embodiment, by using a resistance change storage element having a memory function and a switch element function, it is possible to record information in the storage element even if a switch element is not provided. However, the storage device of this embodiment may include any switch element.
[0123] 6 is a schematic three-dimensional diagram of a memory device according to a second embodiment of the present invention. As shown in FIG. 6, the memory device 101 includes a memory element 21, a word line 30, and a bit line 40. The bit line 40 is orthogonal to the word line 30 in a plan view. The memory element 21 is disposed at the intersection of the word line 30 and the bit line 40 in a plan view. In other words, the memory device 101 of this embodiment is a so-called cross-point memory device.
[0124] 7 is a schematic three-dimensional diagram of a modified example of a memory device according to the second embodiment of the present invention. As shown in FIG. 7, a memory device 201 includes a memory element 21, a word line 30, and a bit line 40. The bit line 40 is disposed in a through hole provided in the word line 30. The memory element 21 is disposed on the outer periphery of the bit line 40. In other words, the memory device 201 of this embodiment is a so-called BiCS type memory device. As such, in this embodiment, the memory device is not limited to a cross-point type memory device, and various other memory devices may be used.
[0125] The present invention will be described below based on examples, but the present invention is not limited to these examples.
[0126] (First Invention to Third Invention)
[0127]
[0128]
[0129] The samples were prepared as follows. First, a quartz glass ampoule was evacuated while being heated, and then raw materials were mixed to obtain the composition shown in Table 1 and placed in the quartz glass ampoule. Next, the quartz glass ampoule was sealed with an oxygen burner. Next, the sealed quartz glass ampoule was placed in a melting furnace, and the temperature was raised to 650°C to 1000°C at a rate of 10°C to 40°C / hour, and then held for 6 to 12 hours. During this holding time, the quartz glass ampoule was turned upside down to stir the molten material. Finally, the quartz glass ampoule was removed from the melting furnace and rapidly cooled to room temperature to obtain a variable resistance material.
[0130] Next, the prepared variable resistance material was used as a target by high frequency magnetron sputtering to obtain an amorphous thin film variable resistance material.
[0131] [XPS Measurement] The obtained amorphous thin film variable resistance material was etched to a depth of about 20 nm from the sample surface under the following conditions in order to remove the oxide layer on the sample surface. After etching, XPS measurement was performed under the following conditions. The specific measurement conditions are as follows:
[0132] [Dry etching conditions] Ion species: Ar +Acceleration voltage: 4 kV Etching time: 0.4 min Raster range: 2 × 2 mm
[0133] [XPS Measurement Conditions] Measurement equipment: PHI 5000 Versa Probe III (manufactured by ULVAC-PHI) Excitation X-rays: Al Kα1,2 rays (monochromated X-rays, 1486.6 eV) X-ray source power: 25 W (15 kV) Pass energy: 69 eV Measurement step: 0.05 eV Analysis area (beam diameter): 100 μm diameter Photoelectron acceptance angle (tilt of the detector relative to the sample surface): 45° Charge neutralization: Dual beam of electron beam and Ar ion Peak shift correction: After etching the sample surface, peak shift was corrected using C in the sample measurement section, with the C1s main peak (CHx, C-C) set to 284.6 eV. Smoothing: 9-point smoothing was performed using analysis software Multi Pak (manufactured by ULVAC-PHI).
[0134] The intensities of the spectra after peak shift correction were normalized, and the apex and half-width of the XPS peak were determined. The results are shown in Table 2 and Figures 8 to 11.
[0135] The half-width of the spectrum obtained by XPS was determined by drawing a tangent to the point where the first derivative value of the shoulder of the normalized spectrum peak was maximized, and the width of the binding energy at which the spectrum intensity was 1 / 2 (0.5) was defined as the width.
[0136] [Raman Measurement] Raman spectroscopy was performed on the obtained amorphous thin film variable resistance material. Specific measurement conditions are as follows. However, the measurement is not limited to the measurement conditions described below, and any conditions may be used as long as the variable resistance material is not altered by the laser light and a sufficient S / N ratio is obtained.
[0137] [Raman measurement conditions] Measurement device: Laser Raman microscope RAMAN touch (manufactured by Nanophoton Co., Ltd.) Laser wavelength: 532 nm Spectrometer entrance slit width: 50 μm Diffraction grating groove count: 1200 gr / mm Laser output: 300 W / cm 2Ratio of the attenuated light intensity to the maximum laser light intensity of the N / D filter: 144 / 255 Smoothing: Moving average method
[0138] The wave number of the laser light was measured by measuring the spectrum of a standard sample of silicon and was 520 cm -1 The Raman spectrum obtained for the variable resistance material was normalized in intensity, and the apex and half-width of the Raman peak were determined. The results are shown in Table 2 and FIG. 12.
[0139] The half-width of the spectrum obtained by the laser Raman microscope was determined by drawing a tangent to the point where the first derivative value of the shoulder of the normalized spectrum peak was maximum, and the width of the wavenumber at which the spectral intensity was 1 / 2 (0.5).
[0140] [XPS Measurement Results] As shown in Figure 8 and Table 2, in Examples 1-1 and 1-2 and Comparative Example 1, XPS peaks Px1 and Px1GT due to the Te3d5 / 2 orbital were confirmed near 573 eV. More specifically, the apex of the XPS peak Px1 was confirmed in the range of 572.79 to 572.80 eV. Furthermore, the apex of the XPS peak Px1 in Examples 1-1 and 1-2 was shifted to the lower energy side by 0.10 eV or more compared to the apex of the peak Px1GT in Comparative Example 1.
[0141] 9 and Table 2, in Examples 1-1 and 1-2, the half widths Px2hw of the XPS peaks due to the Ge 3d orbitals were 1.25 eV or more, which was larger than the half width Px2GThw of Comparative Example 1. In this case, the ratios of the half widths of the XPS peaks of Examples 1-1 and 1-2 to the half width of the XPS peak of Comparative Example 1 (Px2hw / Px2GThw) were 1.02 or more.
[0142] As shown in FIG. 10 and Table 2, in Examples 1-1, 1-2, and Comparative Example 1, XPS peaks due to the Te4d orbital were observed near 40 eV and 42 eV. More specifically, an XPS peak Px3 due to the Te4d5 / 2 orbital was observed in the range of 40.28 to 40.32 eV. Note that an XPS peak due to the Te4d3 / 2 orbital was observed near 42 eV. The apex of the XPS peak Px3 due to the Te4d3 / 2 orbital in Examples 1-1 and 1-2 was shifted to the lower energy side by 0.13 eV or more compared to the apex of the peak Px3GT in Comparative Example 1. Furthermore, the half-width Px3hw of the XPS peak in Examples 1-1 and 1-2 was 1.22 eV, which was larger than that of Comparative Example 1. At this time, the ratio of the half width of the XPS peak of Examples 1-1 and 1-2 to the half width of the XPS peak of Comparative Example 1 (Px3hw / Px3GThw) was 1.184.
[0143] 11 and Table 2, in Examples 1-1 and 1-2, XPS peaks Px4a and Px4b due to Ga 3d orbitals were observed near 19.5 eV. More specifically, the apexes of the XPS peaks Px4a and Px4b were observed in the range of 19.44 to 19.53 eV. Furthermore, the apex of the XPS peak Px4a in Example 1-2 was shifted to the lower energy side by 0.09 eV compared to the apex of peak Px4b in Example 1-1.
[0144] [Raman Measurement Results] As shown in FIG. 12 and Table 2, in Examples 1-1 and 1-2 and Comparative Example 1, -1 Raman peaks Pr1 and Pr1GT, which are the overlapping of Raman peaks due to Ge-Te bonds and Te-Te bonds, were confirmed near 124.99 cm. -1 In Examples 1-1 and 1-2, the half-width Pr1hw of the Raman peak was 15.8 cm -1 or more, which is larger than the half width Pr1GThw1 of Comparative Example 1. In addition, in Examples 1-1 and 1-2 and Comparative Example 1, -1 Raman peaks Pr2 and Pr2GT due to Te-Te bonds were confirmed around 136.50 to 137.55 cm -1At this time, the apex of the Raman peak Pr2 in Examples 1-1 and 1-2 was 1.04 cm apart from the apex of the Raman peak Pr2GT in Comparative Example 1. -1 The above shifted toward higher wavenumbers.
[0145] [Switching element] Next, a switching element was fabricated using a variable resistance material as a target. 2 A W electrode with a thickness of 50 nm was formed on the substrate. Next, a 100 nm thick SiO 2 An insulating layer was then formed. Then, a focus ion beam device (JEOL, JIB-4600F) was used to form a SiO 2 Holes of 500 nm in diameter were formed in the insulating layer and the W electrode layer. Next, a 150 nm thick film of variable resistance material was deposited in the holes to form a switch layer. Finally, a 150 nm thick W electrode was deposited on the switch layer to fabricate a switch element. The deposition was performed by Ar sputtering under reduced pressure.
[0146] The ON / OFF current ratio was measured using the obtained switch element. The ON / OFF current ratio was determined as follows. First, a voltage of 0 V to 10 V was applied to the switch element, and the current value flowing through the switch element and the threshold voltage were measured. The voltage applied at this time is not limited to DC voltage, AC voltage, pulse voltage, etc., but pulse voltage was used for the measurement from the perspective of preventing heat accumulation in the switch element. Next, the ON / OFF current ratio was determined by dividing the ON current value by the OFF current value. The ON current value was defined as the current value flowing when a voltage equal to or greater than the threshold voltage was applied. The OFF current value was defined as the current value flowing when a voltage equal to or greater than the threshold voltage was applied. The results are shown in Table 2.
[0147] As shown in Table 2, in Examples 1-1 and 1-2, the ON / OFF current ratio was 1×10 5.1 This is larger than that of Comparative Example 1.
[0148] (Fourth Invention)
[0149]
[0150]
[0151] The samples were prepared in the same manner as in the first to third inventions. Specifically, they were prepared as follows. First, a quartz glass ampoule was heated and evacuated, and then raw materials were mixed to obtain the composition shown in Table 3 and placed in the quartz glass ampoule. Next, the quartz glass ampoule was sealed with an oxygen burner. Next, the sealed quartz glass ampoule was placed in a melting furnace, where the temperature was raised to 650°C to 1000°C at a rate of 10°C to 40°C / hour and then held for 6 to 12 hours. During this holding time, the quartz glass ampoule was turned upside down to stir the molten material. Finally, the quartz glass ampoule was removed from the melting furnace and rapidly cooled to room temperature to obtain a variable resistance material.
[0152] Next, the prepared variable resistance material was used as a target by high frequency magnetron sputtering to obtain an amorphous thin film variable resistance material.
[0153] The crystallization temperature Tx of the obtained variable resistance material was determined by measuring the change in electrical resistance when the variable resistance material was heated, and determining the temperature at which the electrical resistance suddenly decreased. Specifically, an amorphous thin film with a thickness of 150 nm was prepared using the variable resistance material, and the electrical resistance of the amorphous thin film was measured using a two-terminal method while heating the amorphous thin film at a temperature increase rate of 10°C / min. The measurement was performed in an air atmosphere. The temperature at which the electrical resistance suddenly decreased was determined to be the temperature at which the first differential value of the electrical resistance with respect to temperature was maximized.
[0154] [Activation Energy] The activation energy Ea of the obtained variable resistance material was determined using the Kissinger method. Specifically, an amorphous thin film with a thickness of 150 nm was prepared using the variable resistance material, and then the electrical resistance of the amorphous thin film was measured using the two-terminal method while heating it at a temperature increase rate varying between 5°C / min and 15°C / min. The temperature at which the electrical resistance suddenly decreased was taken as the crystallization temperature, and the activation energy at the time of crystallization was calculated using the following formula (2). The measurement was performed in an air atmosphere. Here, α is the temperature increase rate of the sample, Tx is the crystallization temperature, R is the gas constant, and C is a constant. The results are shown in Table 4 and FIG. 13.
[0155] ln(α / Tx 2 )=-(Ea / RTx)+C...Formula (2)
[0156] [Switching element] Next, a switching element was fabricated in the same manner as in the first to third inventions. Specifically, the process is as follows. First, Si / SiO 2 A W electrode with a thickness of 50 nm was formed on the substrate. Next, a 100 nm thick SiO 2 An insulating layer was then formed. Then, a focus ion beam device (JEOL, JIB-4600F) was used to form a SiO 2 Holes of 500 nm in diameter were formed in the insulating layer and the W electrode layer. Next, a 150 nm thick film of variable resistance material was deposited in the holes to form a switch layer. Finally, a 150 nm thick W electrode was deposited on the switch layer to fabricate a switch element. The deposition was performed by Ar sputtering under reduced pressure.
[0157] The number of cycles was measured using the obtained switching element. First, a voltage of 0 V to 10 V was applied to the switching element, and the current value and threshold voltage flowing through the switching element were measured. The applied voltage was a pulse voltage to prevent heat accumulation in the switching element. The threshold voltage was defined as the voltage value at which the electrical resistance value abruptly changes from a high resistance state to a low resistance state. The current value flowing when a voltage equal to or greater than the threshold voltage was applied was defined as the OFF current, and the current value flowing when a voltage equal to or greater than the threshold voltage was applied was defined as the ON current. The ON current was measured by applying a 3 μs trapezoidal pulse voltage, and the OFF current was measured by applying a 22 μs trapezoidal pulse voltage. The number of cycles was defined as the number of times the ON / OFF current was repeatedly switched until the ON / OFF current ratio reached 10% of the initial measured value. The results are shown in Table 4.
[0158] 13 and Table 4, the activation energies of Examples 2-1 to 2-6 were as high as 251 kJ / mol or more. In addition, the switching elements fabricated using the variable resistance materials of Examples 2-1 to 2-6 were cycled to 8×10 2 At this time, as shown in FIG. 13, the resistance change materials of Examples 2-1 to 2-6 exhibited a log 10 The relationship x≧0.011Ea+0.1 was satisfied.
[0159] The resistance change material of the present invention can be suitably used for a switching element that can be used in a resistance change type, phase change type, or other memory device.
[0160] 1, 11 First electrode 2, 12 Second electrode 3 Switch layer 4 Switch memory layer 10 Switch element 20, 21 Memory element 30 Word line 40 Bit line 100, 101, 200, 201 Memory device
Claims
1. A variable resistance material containing, in atomic percent, 40% to 90% Te, more than 0% to 40% Ge, and more than 0% to 40% Ga, wherein in an XPS spectrum measured by X-ray photoelectron spectroscopy, the apex of the XPS peak Px1 due to the Te3d5 / 2 orbital is the same as that of amorphous GeTe. 5 The resistance change material is shifted to a lower energy side than the apex of the XPS peak Px1GT due to the Te3d5 / 2 orbital in 2. The variable resistance material according to claim 1, wherein the apex of the XPS peak Px1 is shifted to the lower energy side by 0.05 eV or more than the apex of the XPS peak Px1GT.
3. The variable resistance material according to claim 1 or 2, wherein a half width Px1hw of the XPS peak Px1 is larger than a half width Px1GThw of the XPS peak Px1GT.
4. The variable resistance material according to claim 3, wherein the ratio of the half width Px1hw of the XPS peak Px1 to the half width Px1GThw of the XPS peak Px1 (Px1hw / Px1GThw) is 1.01 or more.
5. In the XPS spectrum, the half-width Px2hw of the XPS peak Px2 due to the Ge3d orbital is 5 3. The variable resistance material according to claim 1, wherein the full width at half maximum Px2GT is greater than the full width at half maximum Px2GTw of an XPS peak Px2GT attributed to a Ge 3d orbital in the sample.
6. The variable resistance material according to claim 5, wherein the ratio of the half width Px2hw of the XPS peak Px2 to the half width Px2GThw of the XPS peak Px2GT (Px2hw / Px2GThw) is 1.01 or more.
7. A variable resistance material containing, in atomic percent, 40% to 90% Te and more than 0% to 40% Ge, which has at least three or more peaks in a binding energy range of 15 eV to 44 eV in an XPS spectrum measured by X-ray photoelectron spectroscopy.
8. A variable resistance material containing, in atomic percent, 40% to 90% Te, more than 0% to 40% Ge, and more than 0% to 40% Ga, wherein in a Raman spectrum measured by Raman spectroscopy, the apex of Raman peak Pr1, which is a combination of Raman peaks due to Ge-Te bonds and Te-Te bonds, is at a wavenumber of 118 cm -1 ~130cm -1 the half width Pr1hw of the Raman peak Pr1 is in the range of 5 The resistance change material has a half-width Pr1GThw greater than that of the Raman peak Pr1GT at 9. The variable resistance material according to claim 8, wherein the ratio of the half width Pr1hw of the Raman peak Pr1 to the half width Pr1GThw of the Raman peak Pr1 (Pr1hw / Pr1GThw) is 1.05 or more.
10. The variable resistance material according to claim 8 or 9, wherein the peak of the Raman peak Pr1 is shifted to a higher wavenumber side than the peak of the Raman peak Pr1GT.
11. The apex of the Raman peak Pr1 is 0.1 cm away from the apex of the Raman peak Pr1GT. -1 The variable resistance material according to claim 10 , wherein the wavelength is shifted to a higher wave number side by at least one of the above.
12. Furthermore, the apex of the Raman peak Pr2 due to the Te-Te bond is at a wavenumber of 135 cm -1 ~145cm -1 The apex of the Raman peak Pr2 is in the range of 5 10. The variable resistance material according to claim 8, wherein the peak of the Raman peak Pr2GT due to Te-Te bonds is shifted to a higher wavenumber side.
13. The apex of the Raman peak Pr2 is 0.1 cm from the apex of the Raman peak Pr2GT -1 The variable resistance material according to claim 12 , wherein the wavelength is shifted to a higher wave number side by at least one of the above.
14. A variable resistance material containing, in atomic %, 40% to 90% Te and more than 0% to 40% Ge, wherein the activation energy Ea when an amorphous thin film made of the variable resistance material crystallizes is 240 kJ / mol or more.
15. The number of cycles is 5 x 10 2 The variable resistance material according to claim 14 , wherein the resistance is at least 100 times.
16. The variable resistance material according to claim 14 or 15, wherein the number of cycles x (times) and the activation energy Ea (kJ / mol) satisfy the relationship of the following formula (1): log 10 x≧0.011Ea+0.1 ... Equation (1) 17. The variable resistance material according to claim 1, 7, 8 or 14, containing, in atomic percent, 0% to 20% of Sb.
18. The variable resistance material according to claim 1, 7, 8 or 14, which is substantially free of Sb, Se and As.
19. The variable resistance material according to claim 1, 7, 8 or 14, which is a thin film.
20. A material for a switching element, comprising the variable resistance material according to claim 1, 7, 8 or 14.
21. A switch layer made of the variable resistance material according to claim 1, 7, 8 or 14.
22. A switch element comprising: a first electrode; and a switch layer according to claim 21 disposed on the first electrode.
23. The switch element according to claim 22, further comprising a second electrode disposed opposite the first electrode with the switch layer interposed therebetween.
24. A memory device comprising: a switch element according to claim 23; and a memory element.
Citation Information
Patent Citations
Ge-RICH GST-212 PHASE CHANGE MATERIALS
JP2013008948A
Switch element and memory device
JP2015135917A
Diamine compound, and polyimide precursor and polyimide film prepared by using the same
KR102319883B1
Etching process for phase-change films
US20090246964A1
Phase change material and phase change memory element
WO2011030916A1