Variable resistance material, material for switch element, switch layer, switch element, and storage device
A Te-based resistance change material with defined current densities and carrier mobility is used to create a switch element with excellent OTS characteristics, addressing the need for stable switching in next-generation storage devices, thereby improving their capacity and integration density.
Patent Information
- Application Number
- PCT/JP2024/010661
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-07-12
- Filing Date
- 2024-03-19
- Publication Date
- 2024-10-24
AI Technical Summary
Next-generation nonvolatile storage devices require switch elements with excellent Ovonic Threshold Switch (OTS) characteristics, specifically large resistance change with respect to applied voltage, to achieve stable switching action and high integration density.
A resistance change material containing Te, with specific OFF and ON current densities, carrier mobility, and threshold voltage ranges, is used to form a switch element with a switch layer and electrodes, enabling stable OTS characteristics for use in cross-point storage devices.
The solution provides a switch element with a high ON/OFF current ratio and stable OTS characteristics, suitable for next-generation nonvolatile storage devices, enhancing their capacity and integration density.
Smart Images

Figure JP2024010661_24102024_PF_FP_ABST
Abstract
Description
Resistance change material, material for switch element, switch layer, switch element and storage device
[0001] The present invention relates to a variable resistance material, a material for a switching element, a switching layer, a switching element, and a memory device.
[0002] Next-generation nonvolatile memory devices have been attracting attention as replacements for NAND flash memories. Resistance-change and phase-change memory devices have been proposed as next-generation nonvolatile memory devices, and development is underway to achieve larger capacities and higher speeds.
[0003] Furthermore, cross-point memory devices have attracted attention as a next-generation nonvolatile memory device structure (see Patent Documents 1 and 2). A cross-point memory device includes word lines, bit lines that are orthogonal to the word lines in a planar view, and memory elements and switch elements that are arranged at the intersections of the word lines and bit lines in a planar view. While transistors and diodes have traditionally been used as switch elements, the use of ovonic threshold switches (OTS elements), whose resistance changes depending on the applied voltage, has attracted attention as memory devices become smaller, have larger capacities, and are more highly integrated.
[0004] JP 2006-086526 A JP 2018-164085 A
[0005] Lencer, D. et al., “A map for phase-change materials”, Nat. Mater. 7, 972-977 (2008)
[0006] In order to obtain a stable switching action, the OTS element is required to exhibit a large change in resistance with respect to the applied voltage (that is, to have excellent OTS characteristics).
[0007] In view of the above, an object of the present invention is to provide a variable resistance material, a material for a switching element, a switching layer, a switching element, and a memory device, all of which have excellent OTS characteristics.
[0008] A description will be given of various aspects of a resistance change material, a material for a switching element, a switching layer, a switching element, and a memory device that solve the above problems.
[0009] The variable resistance material of aspect 1 is a variable resistance material containing Te, and when a current density when a voltage that is ½ of the threshold voltage is applied is defined as an OFF current density, the OFF current density is 3.1 × 10 2 A / cm 2 The characteristics are as follows: Here, the threshold voltage refers to the voltage value at which the electrical resistance value suddenly changes from a high resistance state to a low resistance state, and the OFF current density refers to the value obtained by dividing the current value (OFF current value) that flows when a voltage half the threshold voltage is applied by the contact area with the electrode.
[0010] The variable resistance material of the second aspect is the same as that of the first aspect, except that the ON current density is 1×10 6 A / cm 2 Here, the ON current density means a value obtained by dividing the value of the current (ON current value) that flows when a voltage equal to or higher than the threshold voltage is applied by the contact area with the electrode.
[0011] The variable resistance material of aspect 3 is the same as that of aspect 1 or aspect 2, except that the carrier mobility is 5×10 -3 cm 2 It is preferable that the voltage Vs is not more than 1 / Vs.
[0012] The variable resistance material of Aspect 4 is any one of Aspects 1 to 3, wherein when a current density when a voltage equal to or higher than a threshold voltage is applied is defined as an ON current density, the ON / OFF current ratio obtained by dividing the ON current density by the OFF current density is 1×10 4 It is preferable that this is equal to or greater than this.
[0013] The variable resistance material of Aspect 5 is any one of Aspects 1 to 4, and preferably has a threshold voltage in the range of 0.5V to 10V.
[0014] The variable resistance material of Aspect 6 is any one of Aspects 1 to 5, and preferably contains, in atomic percent, 0.1% to 50% of Ge and 40% to 90% of Te.
[0015] The variable resistance material of Aspect 7 is any one of Aspects 1 to 6, and preferably contains, in atomic %, 1% to 59% of Si+Al+Ga+Sn+Bi+Cu+Ag+Zn+Y+In+Ca+Mg.
[0016] The variable resistance material of Aspect 8 is any one of Aspects 1 to 7, and preferably contains, in atomic percent, 0% to less than 5% of Sb.
[0017] The variable resistance material of Aspect 9 is any one of Aspects 1 to 7, and preferably does not substantially contain Sb, Se, or As.
[0018] The variable resistance material of Aspect 10 is any one of Aspects 1 to 9, and preferably has an oxygen content of less than 1 atomic %.
[0019] The variable resistance material of Aspect 11 is preferably a thin film in any one of Aspects 1 to 10.
[0020] A switching element material according to a twelfth aspect is characterized in that it is made of the variable resistance material according to any one of the first to eleventh aspects.
[0021] The switch layer of the thirteenth aspect is characterized in that it is made of the variable resistance material of any one of the first to eleventh aspects.
[0022] A switch element according to a fourteenth aspect of the present invention is characterized by comprising the switch layer according to the thirteenth aspect of the present invention and a first electrode disposed on the switch layer.
[0023] A switching element of aspect 15 includes a switching layer, a first electrode disposed on the switching layer, and a second electrode disposed opposite the first electrode with the switching layer sandwiched therebetween, wherein the switching layer contains Te, and the OFF current density is 3.1×10 when a voltage that is half the threshold voltage is applied. 2 A / cm 2 The present invention is characterized in that the resistive element is made of the following variable resistance material.
[0024] A switch element of Aspect 16 is preferably the same as Aspect 15, wherein the first electrode is disposed on an outer circumferential surface of the switch layer, and the second electrode is disposed on an inner circumferential surface of the switch layer.
[0025] The switching element of Aspect 17 is preferably the same as Aspect 15 or 16, wherein the first electrode and the second electrode are made of at least one material selected from the group consisting of tungsten, titanium, copper, platinum, tungsten nitride, and titanium nitride.
[0026] The switching element of Aspect 18 is the switching element of any one of Aspects 15 to 17, further comprising: an ionic r σ ' and hybridization π -1 It is preferable that r satisfies the following value: σ ´≧0.05r π -1 ≦2.0
[0027] The switching element of Aspect 19, in any one of Aspects 15 to 18, preferably satisfies a / b<1, where a is the carrier activation energy when a voltage of 0.15 V is applied to the switching layer, and b is the carrier activation energy when a voltage of 0.30 V is applied to the switching layer.
[0028] The storage device of aspect 20 preferably includes the switch element of any one of aspects 15 to 19.
[0029] The storage device of aspect 21 preferably includes the switch element of any one of aspects 15 to 19 and a storage element.
[0030] A memory device of aspect 22 is a memory device including a stacked body in which a switch element and a memory element are stacked, the switch element including a switch layer and a first electrode disposed on the switch layer, and the switch layer has an OFF current density of 3.1×10 when a current density when a voltage of ½ of a threshold voltage is applied is defined as the OFF current density. 2 A / cm 2The memory element is characterized in that it is made of the following resistance change material, and the memory element is one of a resistance change memory element, a magnetoresistive memory element, a phase change memory element, and a ferroelectric memory element.
[0031] According to the present invention, it is possible to provide a variable resistance material, a material for a switching element, a switching layer, a switching element, and a memory device, all of which have excellent OTS characteristics.
[0032] FIG. 1 is a schematic cross-sectional view of a switch element according to one embodiment of the present invention. FIG. 2 is a schematic cross-sectional view of a memory element according to one embodiment of the present invention. FIG. 3 is a schematic three-dimensional view of a memory device according to a first embodiment of the present invention. FIG. 4 is a schematic three-dimensional view of an enlarged memory device according to the first embodiment of the present invention. FIG. 5 is a schematic three-dimensional view of a modified memory device according to the first embodiment of the present invention. FIG. 6 is a schematic three-dimensional view of a memory device according to a second embodiment of the present invention. FIG. 7 is a schematic three-dimensional view of a modified memory device according to the second embodiment of the present invention. FIG. 8 is a schematic three-dimensional view of an ionic r of a switch layer. σ ' and hybridization π -1 This is a graph plotting
[0033] Preferred embodiments are described below. However, the following embodiments are merely examples, and the present invention is not limited to the following embodiments. In the following description, "%" means "atomic %" unless otherwise specified. Furthermore, in the present invention, "x + y + z + ..." means the total content of each component. Here, each component does not necessarily have to be contained as an essential component, and it is acceptable for there to be components that are not contained (content 0%). Furthermore, "x + y + z + ... A% to B%" includes, for example, cases where "x = 0%, y + z + ... A% to B%" and "x = 0%, y = 0%, z + ... A% to B%" are included.
[0034] <Resistance change material> The resistance change material of the present invention is a resistance change material containing Te, and has an OFF current density of 3.1×10 2 A / cm 2 The present invention is characterized by the following:
[0035] The inventors have discovered that excellent OTS characteristics can be obtained from variable resistance materials whose OFF current density satisfies a predetermined value. The OTS characteristic refers to the characteristic of a chalcogenide-based thin film in which the resistance value changes with the application of voltage. More specifically, the variable resistance material exhibits high resistance in its initial state (OFF state). When a voltage is applied to this state, it maintains the high resistance state until it exceeds a threshold voltage, at which point it suddenly switches to a low resistance state (ON state). When the applied voltage is reduced from the ON state, it returns to the OFF state. Variable resistance materials with excellent OTS characteristics have a large difference in resistance between the high resistance state and the low resistance state. In other words, the difference between the current density in the low resistance state and the current density in the high resistance state (ON / OFF current ratio) is large. Therefore, they can be stably used as switch layers and switch elements. Here, the ON / OFF current ratio refers to the value obtained by dividing the ON current density by the OFF current density.
[0036] In the variable resistance material of the present invention, when a voltage half the threshold voltage is applied, the OFF current density is defined as the current density, and the upper limit of the OFF current density is 3.1×10 2 A / cm 2 is less than or equal to 3×10 2 A / cm 2 Below, 2.8 x 10 2 A / cm 2 Below, especially 2.6 x 10 2 A / cm 2 When the OFF current density satisfies the above value, it becomes easy to increase the ON / OFF current ratio. Therefore, it becomes possible to obtain stable OTS characteristics. The lower limit of the OFF current density is not particularly limited, but is preferably 5×10 -3 A / cm 2 That's it, 6 x 10 -3 A / cm 2 That's it, 1 x 10 -2 A / cm 2 It may be more than that.
[0037] In the variable resistance material of the present invention, when a voltage equal to or higher than a threshold voltage is applied, the current density is defined as the ON current density, and the lower limit of the ON current density is 1×10 6 A / cm2 That's it, 2 x 10 6 A / cm 2 That's it, 3.1 x 10 6 A / cm 2 That's it, 3.2 x 10 6 A / cm 2 That's it, 3.5 x 10 6 A / cm 2 That's it, 4.1 x 10 6 A / cm 2 That's it, 4.2 x 10 6 A / cm 2 That's it, 4.3 x 10 6 A / cm 2 That's it, 4.4 x 10 6 A / cm 2 Above, especially 4.5 x 10 6 A / cm 2 By satisfying the above-mentioned value for the ON current density, the ON / OFF current ratio can be further increased. The upper limit of the ON current density is not particularly limited, but it is preferably 1×10 9 A / cm 2 Below, 1 x 10 8 A / cm 2 Below, 1 x 10 7 A / cm 2 The following may also be used.
[0038] The variable resistance material of the present invention has a lower limit of the ON / OFF current ratio of 1×10 4 That's it, 1.2 x 10 4 That's it, 1.5 x 10 4 That's it, 1.8 x 10 4 That's it, 5 x 10 4 That's it, 1 x 10 5 That's it, 1.5 x 10 5 That's it, 3.1 x 10 5 That's it, 3.9 x 10 5 That's it, 5 x 10 5 That's it, 6.3 x 10 5 Above, especially 1 x 10 6 Or, when the ON / OFF current ratio is x, log 10The lower limit of x is preferably 4 or more, 4.1 or more, 4.2 or more, 4.3 or more, 4.7 or more, 5 or more, 5.2 or more, 5.5 or more, 5.6 or more, 5.7 or more, 5.8 or more, and particularly preferably 6 or more. Such a large ON / OFF current ratio increases the difference between the current density in the low resistance state and the current density in the high resistance state (ON / OFF current ratio). In other words, an excellent OTS effect can be obtained. The upper limit of the ON / OFF current ratio is not particularly limited, but may be, for example, 2×10 10 Below, 1 x 10 9 Below, 1 x 10 8 Below, especially 1 x 10 7 It can be expressed as follows: Also, log 10 The upper limit of the value of x is preferably 10.3 or less, 9 or less, 8 or less, and particularly preferably 7 or less.
[0039] The variable resistance material of the present invention preferably has a threshold voltage in the range of 0.5 V to 10 V. More specifically, the upper limit of the threshold voltage is preferably 10 V or less, 8 V or less, 6 V or less, and particularly preferably 5 V or less. By having the threshold voltage in the above range, a switching element or the like can be driven with less energy. The lower limit of the threshold voltage is not particularly limited, but may be 0.5 V or more, 0.8 V or more, 1 V or more, 1.2 V or more, and particularly preferably 1.5 V or more.
[0040] The OFF current density, ON current density, ON / OFF current ratio, and threshold voltage can be determined as follows. First, a voltage of 0 V to 10 V is applied to the switching element, and the current value flowing through the switching element and the threshold voltage are measured. The applied voltage may be a DC voltage, an AC voltage, a pulse voltage, or any other voltage. However, from the viewpoint of preventing heat accumulation in the switching element, it is preferable to measure using a pulse voltage. The threshold voltage can be the voltage value at which the electrical resistance value abruptly changes from a high resistance state to a low resistance state. The OFF current density can be the value obtained by dividing the current value (OFF current value) flowing when a voltage equal to or equal to half the threshold voltage is applied by the contact area with the first electrode or the second electrode. The ON current density can be the value obtained by dividing the current value (ON current value) flowing when a voltage equal to or greater than the threshold voltage is applied by the contact area with the first electrode or the second electrode. The ON / OFF current ratio can be determined by dividing the ON current value by the OFF current value. When the contact area between the switch element and the first electrode and the contact area between the switch element and the second electrode are the same, the current density can be calculated using the contact area of the first electrode or the second electrode, as described above. When the contact area between the switch element and the first electrode and the contact area between the switch element and the second electrode are different in size, the current density can be calculated using the smaller contact area.
[0041] The variable resistance material of the present invention has an upper limit of carrier mobility of 5×10 -3 cm 2 / Vs or less, 4.5×10 -3 cm 2 / Vs or less, 4×10 -3 cm 2 / Vs or less, 3.5×10 -3 cm 2 / Vs or less, especially 3×10 -3 cm 2 / Vs or less. When the carrier mobility satisfies the above value, the OFF current density is likely to decrease. Therefore, the ON / OFF current ratio can be easily increased. The lower limit of the carrier mobility is not particularly limited, but is, for example, 1×10 -8 cm 2 / Vs or more, 1×10 -7 cm 2 / Vs or more, 1×10 -6 cm 2 / Vs or more. The carrier mobility can be measured using a resistivity / Hall measurement system.
[0042] The variable resistance material of the present invention contains Te. Te constitutes the variable resistance material and is an essential component for obtaining OTS characteristics. The Te content is preferably 40% to 90%. More specifically, the lower limit of the Te content is preferably 40% or more, 42% or more, 47% or more, 50% or more, more than 50%, 51% or more, 53% or more, 55% or more, 60% or more, 61% or more, 65% or more, 67% or more, 70% or more, and particularly preferably 71% or more. The upper limit of the Te content is preferably 90% or less, 89% or less, 85% or less, 82.5% or less, 80% or less, 75% or less, and particularly preferably 72.5% or less. If the Te content is too low, the amorphous state tends to become unstable. Furthermore, it becomes difficult to obtain OTS characteristics. If the Te content is too high, the amorphous state tends to become unstable. Moreover, the carrier mobility becomes too high, and the OFF current density tends to become large.
[0043] The variable resistance material of the present invention may contain components other than Te. For example, it preferably contains, in atomic percent, 0.1% to 50% Ge and 40% to 90% Te. Furthermore, it may contain components other than Ge and Te.
[0044] Ge is a component that stabilizes the amorphous state of the resistance change material. The Ge content is preferably 0.1% to 50%. More specifically, the lower limit of the Ge content is preferably 0.1% or more, 1% or more, 3% or more, 5% or more, 7% or more, 10% or more, 11% or more, and particularly preferably 13% or more. The upper limit of the Ge content is preferably 50% or less, 40% or less, 30% or less, and particularly preferably 20% or less. If the Ge content is too low, the amorphous state tends to become unstable. If the Ge content is too high, it becomes difficult to obtain OTS characteristics. Furthermore, the manufacturing cost tends to increase.
[0045] The lower limit of the Ge+Te content (total amount of Ge and Te) is preferably 41% or more, 45% or more, 50% or more, 60% or more, 65% or more, 70% or more, 75% or more, particularly 80% or more. The upper limit of the Ge+Te content is preferably 99% or less, 98% or less, 97% or less, particularly 95% or less. If the Ge+Te content is too low, the amorphous state tends to become unstable. Also, it becomes difficult to obtain OTS characteristics. If the Ge+Te content is too high, it becomes difficult to obtain OTS characteristics.
[0046] Si, Al, Ga, Sn, Bi, Cu, Ag, Zn, Y, In, Ca, and Mg are components that stabilize the amorphous state of the variable resistance material. They also tend to increase the ON / OFF current ratio by reducing the OFF current density. Therefore, the variable resistance material of the present invention preferably has a Si+Al+Ga+Sn+Bi+Cu+Ag+Zn+Y+In+Ca+Mg content (the total amount of Si, Al, Ga, Sn, Bi, Cu, Ag, Zn, Y, In, Ca, and Mg) of 1% to 59%. More specifically, the lower limit of the Si+Al+Ga+Sn+Bi+Cu+Ag+Zn+Y+In+Ca+Mg content is preferably 1% or more, particularly 2% or more. The upper limit of the content of Si+Al+Ga+Sn+Bi+Cu+Ag+Zn+Y+In+Ca+Mg is preferably 59% or less, 58% or less, 55% or less, 50% or less, 45% or less, 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, 15% or less, 14% or less, 13% or less, 10% or less, and particularly preferably 9% or less. The above content can also be rephrased as "containing one or more components selected from Si, Al, Ga, Sn, Bi, Cu, Ag, Zn, Y, In, Ca, and Mg." If the content of these components is too low, the above effects are difficult to achieve. If the content of these components is too high, the amorphous state tends to become unstable. Furthermore, OTS characteristics are difficult to achieve. The lower limit of the content of each of the components Si, Al, Ga, Sn, Bi, Cu, Ag, Zn, Y, In, Ca, and Mg is preferably 0% or more, more than 0%, 0.1% or more, 0.5% or more, 1% or more, and particularly preferably 2% or more. The upper limit of the content of each of the components Si, Al, Ga, Sn, Bi, Cu, Ag, Zn, Y, In, Ca, and Mg is preferably 59% or less, 58% or less, 55% or less, 50% or less, 45% or less, 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, 15% or less, 14% or less, 13% or less, 10% or less, and particularly preferably 9% or less.
[0047] Among the above components, Ga and Ag are components that tend to reduce carrier mobility and lower OFF current density, thereby particularly contributing to improving the ON / OFF current ratio. They are also components that particularly tend to stabilize the amorphous state. The lower limit of the Ga+Ag content (total amount of Ga and Ag) is preferably 0% or more, more than 0%, 0.1% or more, 0.5% or more, 1% or more, 2% or more, 3% or more, and particularly 5% or more. The upper limit of the Ga+Ag content is preferably 59% or less, 58% or less, 55% or less, 50% or less, 45% or less, 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, 15% or less, 14% or less, 13% or less, 10% or less, and particularly 9% or less. If the Ga+Ag content is too high, the amorphous state tends to become unstable.
[0048] In particular, from the viewpoint of reducing the OFF current density, the lower limit of Ga / (Ga+Ag) is preferably 0.1 or more, particularly 0.2 or more, and the upper limit of Ga / (Ga+Ag) is preferably 1.2 or less, less than 1.2, particularly 1.1 or less. Here, Ga / (Ga+Ag) is the value obtained by dividing the Ga content by the combined amount of Ga and Ag.
[0049] In particular, from the viewpoint of increasing the number of cycles described later, the lower limit of Ag / (Ga+Ag) is preferably 0.1 or more, particularly 0.2 or more, and the upper limit of Ag / (Ga+Ag) is preferably 1.2 or less, less than 1.2, particularly preferably 1.1 or less. Here, Ag / (Ga+Ag) is the value obtained by dividing the Ag content by the combined amount of Ga and Ag.
[0050] Sb is a component that easily destabilizes the amorphous state at high temperatures. Therefore, the Sb content is preferably 0% to less than 5%. More specifically, the upper limit of the Sb content is preferably less than 5%, 4% or less, 3% or less, or 2% or less, and it is particularly preferable that Sb is not contained substantially. In this specification, "substantially not contained" means that Sb is not intentionally contained in the raw materials, and does not exclude contamination at the impurity level. Objectively, this refers to a content of each component of less than 0.1%.
[0051] Se is a component that easily stabilizes the amorphous state of the resistance change material. The upper limit of the Se content is preferably 58% or less, 55% or less, particularly 50% or less. The lower limit of the Se content is preferably 0% or more, 1% or more, 5% or more, 10% or more, particularly 20% or more. If the Se content is too high, the amorphous state tends to become unstable. Se is also a toxic component. Therefore, from the viewpoint of reducing the burden on the environment, it is preferable that the upper limit of the Se content be 40% or less, 30% or less, 20% or less, or 10% or less, particularly that substantially no Se is contained.
[0052] As is a component that easily stabilizes the amorphous state of the resistance change material. However, because As is a toxic component, from the viewpoint of reducing the environmental impact, the As content is preferably 0% to 30%. More specifically, the upper limit of the As content is preferably 30% or less, 25% or less, 20% or less, 10% or less, 5% or less, or 3% or less, and it is particularly preferable that As is not contained substantially.
[0053] The variable resistance material of the present invention preferably contains substantially no Sb, Se, or As, which further facilitates reducing the environmental load.
[0054] If the content of B, C, N, F, Cl, Br, and I is too high, the amorphous state tends to become unstable. Furthermore, weather resistance tends to decrease. Therefore, the upper limit of the content of B + C + N + F + Cl + Br + I (the total amount of B, C, N, F, Cl, Br, and I) is preferably 50% or less, 45% or less, 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, 15% or less, 14% or less, 12% or less, 10% or less, 8% or less, 6% or less, and particularly preferably 5% or less. Furthermore, the upper limit of the content of each of the components B, C, N, F, Cl, Br, and I is preferably 50% or less, 45% or less, 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, 15% or less, 14% or less, 12% or less, 10% or less, 8% or less, 6% or less, and particularly preferably 5% or less. However, from the viewpoint of increasing the crystallization temperature, B, C, N, F, Cl, Br and I may be contained in a total amount of 0% or more, 1% or more, particularly 2% or more.
[0055] If the content of P, Cr, Mn, Ti, or Fe is too high, the amorphous state tends to become unstable. Therefore, the content of P + Cr + Mn + Ti + Fe (the total amount of P, Cr, Mn, Ti, and Fe) is preferably 0% to 10%. More specifically, the upper limit of the content of P + Cr + Mn + Ti + Fe is preferably 10% or less, 5% or less, 1% or less, less than 1%, or 0.1% or less, and it is particularly preferred that these components are not contained substantially. If the content of these components is too high, the amorphous state tends to become unstable. Note that the content of each of P, Cr, Mn, Ti, and Fe is preferably 0% to 10%. More specifically, the upper limit of the content of each of P, Cr, Mn, Ti, and Fe is preferably 10% or less, 5% or less, 1% or less, less than 1%, or 0.1% or less, and it is particularly preferred that these components are not contained substantially.
[0056] From the viewpoint of reducing the environmental load, it is preferable that Cd, Tl, and Pb are not substantially contained.
[0057] The variable resistance material of the present invention preferably has an oxygen content of less than 1 atomic %. More specifically, the upper limit of the oxygen content is preferably 0.8% or less, 0.5% or less, 0.3% or less, 0.1% or less, 0.09% or less, 0.05% or less, and particularly preferably 0.02% or less, in atomic %. If the oxygen content is too high, the ON current density is likely to decrease and the threshold voltage is likely to increase. From the viewpoint of raw material refining costs, the lower limit of the oxygen content is 1×10 -6 % or more, 1 x 10 -5 % or more, 5 x 10 -5 % or more, 1 x 10 -4 % or more, especially 2 × 10 -4 % or more is preferable.
[0058] The composition of the variable resistance material can be evaluated using energy dispersive X-ray spectroscopy (EDX), electron probe microanalyzer (EPMA), X-ray fluorescence analysis (XRF), or the like. EDX may be evaluated using a TEM-EDX or SEM-EDX device attached to a transmission electron microscope (TEM) or a scanning electron microscope (SEM), or the like. The oxygen content can be evaluated using an inert gas fusion-infrared absorption method, or the like.
[0059] The variable resistance material of the present invention preferably has a crystallization temperature Tx of 150°C or higher, 160°C or higher, and particularly preferably 170°C or higher. When the crystallization temperature Tx satisfies the above value, crystallization due to heat generated during switching is less likely to occur, making it easier to further increase the number of cycles described below. The upper limit of the crystallization temperature Tx is not particularly limited, but may be, for example, 500°C or lower, 450°C or lower, and particularly preferably 400°C or lower.
[0060] The crystallization temperature Tx of the variable resistance material can be evaluated using differential thermal analysis (DTA) or differential scanning calorimetry (DSC). Alternatively, the temperature dependence of electrical resistance may be measured in a two-terminal electrical resistance measurement, and the temperature at which the electrical resistance drops sharply may be evaluated as the crystallization temperature Tx. Furthermore, the obtained variable resistance material may be heat-treated at a predetermined temperature, and the point at which a crystallization peak appears in XRD may be evaluated as the crystallization temperature Tx. It is preferable that the crystallization temperature Tx evaluated by any of the above methods satisfies the preferred value of the crystallization temperature Tx described above. In particular, it is preferable that the crystallization temperature Tx evaluated in terms of the temperature dependence of electrical resistance satisfies the preferred value of the crystallization temperature Tx described above.
[0061] Since the variable resistance material of the present invention is stable in an amorphous state, it is possible to increase the number of cycles when used as a switching element. That is, the ON / OFF current ratio can be maintained even when ON and OFF are repeated. Specifically, the lower limit of the number of cycles (the number of times the ON / OFF current is repeatedly switched until the ON / OFF current ratio becomes 10% of the initial measured value) is 5×10 2 More than once, 1 x 10 3 More than once, especially 1 x 10 4 If the number of cycles is too small, it becomes difficult to use the device as a switching element. The upper limit of the number of cycles is not particularly limited, but may be, for example, 1×10 10 times or less, 1×10 9 times or less, 1×10 8 times or less, 1×10 7 It may be less than once.
[0062] The variable resistance material of the present invention is preferably used as a thin film (variable resistance film). The thin film (variable resistance film) is particularly suitable for use as a switch layer or a switch memory layer, which will be described later. However, the variable resistance material is not limited to a thin film.
[0063] The film thickness of the thin film (resistance change film) is preferably 1 nm to 300 nm. More specifically, the lower limit of the film thickness of the resistance change film is preferably 1 nm or more, 2 nm or more, 5 nm or more, 10 nm or more, 30 nm or more, and particularly preferably more than 50 nm, and the upper limit of the film thickness of the resistance change film is preferably 300 nm or less, 200 nm or less, and particularly preferably 100 nm or less. If the film thickness is too small, the current value (OFF current) in the high resistance state tends to be high. If the film thickness is too large, the threshold voltage tends to be high.
[0064] The material for a switching element of the present invention is preferably made of the variable resistance material of the present invention described above. Furthermore, the switching layer of the present invention is preferably made of the variable resistance material of the present invention described above. As described above, the variable resistance material of the present invention has excellent OTS characteristics, and therefore can be suitably used as a material for a switching layer and a switching element.
[0065] The variable resistance material of the present invention can be produced, for example, as follows. First, raw materials are mixed to obtain the desired composition. Next, the mixed raw materials are placed in a quartz glass ampoule that has been heated and evacuated, and the ampoule is sealed with an oxygen burner while evacuating. Next, the sealed quartz glass ampoule is kept at approximately 650°C to 1000°C for 6 to 12 hours. After that, the bulk variable resistance material can be obtained by rapidly cooling to room temperature.
[0066] The raw materials may be elemental raw materials (Ge, Ga, Si, Te, Ag, I, etc.), or compound raw materials (GeTe 4 , Ga 2 Te 3 , AgI, etc.) may be used. These may also be used in combination.
[0067] A thin film (resistance change film) having the above-described composition can be formed by physical vapor deposition (PVD) using the obtained resistance change material as a target.
[0068] It is also possible to form a thin film (resistance change film) having the above-described composition by adjusting the film formation output appropriately using a multi-target sputtering method using a pure element M target (Ge, Te, Sb, Si, Al, Ga, Sn, Bi, Cu, Ag, Zn, Y, In, Ca, and Mg), a binary alloy target, or a ternary or higher alloy target as the target, and adjusting the components.
[0069] The method for producing the thin film is not particularly limited, and a sputtering method, a vacuum deposition method, or an ion plating method can be used as a PVD method. Alternatively, a CVD (Chemical Vapor Deposition) method, an ALD (Atomic Layer Deposition) method, or the like may be selected as a method for producing the thin film. In particular, the sputtering method is preferred because it allows for easy composition control and film thickness control.
[0070] <Switching element> Fig. 1 is a schematic cross-sectional view of a switching element according to one embodiment of the present invention. The switching element 10 includes a first electrode 1, a second electrode 2, and a switching layer 3 disposed on a major surface of the first electrode 1. The second electrode 2 is disposed opposite the first electrode 1. In this embodiment, the switching layer 3 is disposed between the first electrode 1 and the second electrode 2. In other words, the switching element 10 of this embodiment includes the switching layer 3 and the first electrode 1 disposed on the switching layer 3. In further words, the switching element 10 of this embodiment preferably includes the second electrode 2 disposed opposite the first electrode 1, with the switching layer 3 sandwiched between them. In this case, if the switching layer 3 contains Te and a current density when a voltage half the threshold voltage is applied is defined as the OFF current density, the OFF current density is 3.1 x 10 2 A / cm 2 It is preferable that the resistance change material is one of the following:
[0071] The switch element 10 of this embodiment can be suitably used in a cross-point type memory device or a BiCS (Bit-Cost Scalable) type memory device, which will be described later. In the case of a BiCS type memory device, the switch element 10 of this embodiment preferably has the first electrode 1 disposed on the outer circumferential surface of the switch layer 3 and the second electrode 2 disposed on the inner circumferential surface of the switch layer 3.
[0072] The first electrode 1 and the second electrode 2 can be made of an inorganic material. Examples of inorganic materials that can be used include metal materials and ceramic materials. For example, the first electrode 1 and the second electrode 2 are preferably made of at least one material selected from tungsten, titanium, copper, platinum, tungsten nitride, and titanium nitride. Tungsten, titanium, copper, and platinum are preferred metal materials. Furthermore, tungsten nitride and titanium nitride are preferred ceramic materials.
[0073] The thicknesses of the first electrode 1 and the second electrode 2 can be designed as appropriate. For example, the upper limit of the thickness of the first electrode 1 and the second electrode 2 is preferably 200 nm or less, 100 nm or less, 80 nm or less, 60 nm or less, and particularly preferably 50 nm or less, respectively. The smaller the thickness of the first electrode 1 and the second electrode 2, the more advantageous it is for increasing the capacity of the memory device. The lower limit of the thickness of the first electrode 1 and the second electrode 2 is preferably 1 nm or more, and particularly preferably 2 nm or more, respectively, for example.
[0074] The upper limit of the area of the first electrode 1 and the second electrode 2 is, for example, 1,000,000 nm 2 Below, 562500nm 2 Below, 250000nm 2 Below, 62500nm 2 Below, 10000nm 2 Below, 6400nm 2 Below, 2500nm 2 Below, especially 1600 nm 2 The lower limit of the area of the first electrode 1 and the second electrode 2 is not particularly limited, but from the viewpoint of manufacturing costs, it is preferably 1 nm or less. 2 Above 2 nm, especially 2 The upper limit of the contact area between the first electrode 1 and the switch layer 3 or the contact area between the second electrode 2 and the switch layer 3 may be 1,000,000 nm or more. 2 Below, 562500nm 2 Below, 250000nm 2 Below, 62500nm 2 Below, 10000nm 2 Below, 6400nm 2 Below, 2500nm 2 Below, especially 1600 nm 2 It is preferable that the contact area between the first electrode 1 and the switch layer 3 or the contact area between the second electrode 2 and the switch layer 3 is 1 nm or less, which is advantageous for increasing the capacity of the memory device. There is no particular lower limit to the contact area between the first electrode 1 and the switch layer 3 or the contact area between the second electrode 2 and the switch layer 3. However, from the viewpoint of manufacturing costs, it is preferable that the contact area be 1 nm or less. 2 Above 2 nm, especially 2With regard to the contact area between the electrode and the switch layer 3, it is sufficient that at least one of the contact area between the first electrode 1 and the switch layer 3 and the contact area between the second electrode 2 and the switch layer 3 satisfies the above value, and it is more preferable that both contact areas satisfy the above value.
[0075] The switch layer 3 is formed from the resistance change material of the present invention and exhibits OTS characteristics. More specifically, the switch layer 3 is preferably made of a thin film (resistance change film). The resistance state of the switch layer 3 changes depending on the applied voltage. That is, when a voltage equal to or greater than the threshold voltage is applied, the switch layer 3 enters a low resistance state (ON state). Furthermore, when a voltage equal to half the threshold voltage is applied, the switch layer 3 enters a high resistance state (OFF state). In this embodiment, the switch layer 3 is in an amorphous state, and no phase change occurs due to the application of a voltage. In other words, the switch layer 3 does not undergo a phase change to a crystalline state due to the application of a voltage.
[0076] The switch layer 3 is disposed in contact with at least one electrode. In other words, the switch layer 3 is preferably disposed on the first electrode 1. In yet another expression, the first electrode 1 is preferably disposed on the switch layer 3. In addition, it is preferable to include a second electrode 2 disposed at a position facing the first electrode 1 with the switch layer 3 interposed therebetween.
[0077] The thickness of the switch layer 3 can be appropriately designed depending on the desired threshold voltage. The upper limit of the thickness of the switch layer 3 is preferably, for example, 300 nm or less, 200 nm or less, particularly 100 nm or less. If the thickness is too large, the threshold voltage is likely to become too high. The lower limit of the thickness of the switch layer 3 is preferably, for example, 1 nm or more, 2 nm or more, 5 nm or more, 10 nm or more, 30 nm or more, particularly more than 50 nm.
[0078] In the switching element 10, the ionic r σ ' and hybridization π -1 It is preferable that the ionic r σ It is preferable that ' is 0.05 or more. σThe upper limit of the hybridization ratio r′ is not particularly limited, but can be set to, for example, 0.30 or less, 0.25 or less, and particularly 0.20 or less. π -1 It is preferable that the hybridization ratio is 2.0 or less, and particularly 1.9 or less. π -1 The lower limit of the ionic r of the switch layer 3 is not particularly limited, but is preferably 1.0 or more, 1.1 or more, 1.2 or more, and particularly preferably 1.3 or more. σ ´ and hybridization π -1 By satisfying the above value, it is possible to reduce the OFF current density while maintaining the stability of the amorphous state. σ ' and hybridization π -1 can be calculated by the following formulas 1 and 2 described in Non-Patent Document 1. s and r p are the orbital radii of s and p, and n i , n j means the number of atoms per formula unit of chemical species i (anion) and chemical species j (cation).
[0079]
[0080]
[0081] In the switching element 10 of this embodiment, it is preferable that the carrier activation energy increases with increasing applied voltage. For example, when the carrier activation energy when a voltage of 0.15 V is applied to the switching layer 3 is a (eV), and the carrier activation energy when a voltage of 0.30 V is applied to the switching layer 3 is b (eV), the switching element 10 preferably satisfies a / b<1. By exhibiting the above characteristics, even when the applied voltage increases, the OFF current density is less likely to increase, and the ON / OFF current ratio increases. Here, the carrier activation energy refers to the energy required for electrons to transition to a conductive state, and can be calculated as follows. First, voltages are applied to the switching element 10 at different temperatures, and the current values at these times are measured. The temperature and applied voltage ranges are not limited, but the temperature can be 30°C to 80°C, and the applied voltage can be 0V to 0.30V, for example. Next, the carrier activation energy can be calculated from the current value at an arbitrary voltage value and the temperature at the time of measurement using the following formula (3): where I is the current, E a denotes the carrier activation energy, k denotes the Boltzmann constant, T denotes the absolute temperature, and C denotes a constant.
[0082]
[0083] The switching element 10 of this embodiment preferably exhibits a tendency for its threshold voltage to increase with heating. For example, the threshold voltage of the switching element 10 at 80° C. is preferably 1.05 times or more, particularly 1.1 times or more, of the threshold voltage at room temperature of 25° C. By exhibiting the above characteristics, the OFF current density is unlikely to increase even at high temperatures where the kinetic energy of electrons is large, and a high ON / OFF current ratio is maintained even at high temperatures, thereby exhibiting excellent heat resistance.
[0084] In the switch element 10 of this embodiment, it is preferable that the Schottky barrier height increases with increasing temperature. For example, it is preferable that the Schottky barrier height of the switch element 10 at 80°C is 1.01 times or more, particularly 1.02 times or more, of the Schottky barrier height at 30°C. By exhibiting the above characteristics, carrier movement is hindered, thereby making it possible to reduce the OFF current density. Therefore, it becomes easier to increase the ON / OFF current ratio. Note that the Schottky barrier height φ B can be calculated by the following formula (4): s is the saturation current, A is the contact area, A * is Richardson's constant, q is the elementary charge, k is Boltzmann's constant, and T is the absolute temperature.
[0085]
[0086] <Memory Element> Fig. 2 is a schematic cross-sectional view of a memory element according to one embodiment of the present invention. The memory element 21 includes a first electrode 11, a second electrode 12, and a switch memory layer 4 disposed on a major surface of the first electrode 11. The second electrode 12 is disposed opposite the first electrode 11. In this embodiment, the switch memory layer 4 is disposed between the first electrode 11 and the second electrode 12. In other words, the memory element 21 of this embodiment includes the switch memory layer 4, the first electrode 11 disposed on one major surface of the switch memory layer 4, and the second electrode 12 disposed on the other major surface of the switch memory layer 4. The switch memory layer 4 is made of a resistance change film.
[0087] The first electrode 11 and the second electrode 12 can be made of an inorganic material. Examples of inorganic materials that can be used include metal materials and ceramic materials. Examples of metal materials that can be used include tungsten, titanium, copper, and platinum. Examples of ceramic materials that can be used include tungsten nitride and titanium nitride.
[0088] The thickness of the first electrode 11 and the second electrode 12 can be designed as appropriate. For example, it is preferable that the thickness of the first electrode 11 and the second electrode 12 is 200 nm or less, 100 nm or less, 80 nm or less, 60 nm or less, and particularly 50 nm or less, respectively. The smaller the thickness of the first electrode 11 and the second electrode 12, the more advantageous it is for increasing the capacity of the memory device. The lower limit of the thickness of the first electrode 11 and the second electrode 12 is, for example, preferably 1 nm or more, and particularly preferably 2 nm or more.
[0089] The memory element 21 is a resistance change memory element and includes a switch memory layer 4 that functions as both a memory and a switch element. For example, applying a predetermined voltage or higher to the switch memory layer 4 changes the state to a low resistance state LR1, allowing information to be recorded. Furthermore, decreasing the applied voltage from the low resistance state LR1 results in a state in which information is recorded, where the state becomes a high resistance state HR1. Furthermore, applying a read voltage without performing an erase operation changes the state to a low resistance state LR2. On the other hand, applying a read voltage in a high resistance state in which no information is recorded or an erase operation has been performed results in a high resistance state HR2. At this time, information can be recorded by associating 1 and 0 with LR2 and HR2, respectively. Furthermore, the operation method is not limited to the above-described method. For example, after recording information, the applied voltage can be reduced to 0, and then a read voltage can be applied, resulting in LR2. On the other hand, applying a read voltage after an erase operation results in HR2, whereby information can be recorded by associating 1 and 0 with each.
[0090] The upper limit of the area of the first electrode 11 and the second electrode 12 is, for example, 1,000,000 nm 2 Below, 562500nm 2 Below, 250000nm 2 Below, 62500nm 2 Below, 10000nm 2 Below, 6400nm 2 Below, 2500nm 2 Below, especially 1600 nm 2 The lower limit of the area of the first electrode 11 and the second electrode 12 is not particularly limited, but from the viewpoint of manufacturing costs, it is preferable that the lower limit be 1 nm or less. 2 Above 2 nm, especially 2The upper limit of the contact area between the first electrode 11 and the switch memory layer 4 or the contact area between the second electrode 12 and the switch memory layer 4 may be 1,000,000 nm 2 Below, 562500nm 2 Below, 250000nm 2 Below, 62500nm 2 Below, 10000nm 2 Below, 6400nm 2 Below, 2500nm 2 Below, especially 1600 nm 2 The lower limit of the contact area between the first electrode 11 and the switch memory layer 4 and / or the contact area between the second electrode 12 and the switch memory layer 4 is not particularly limited, but from the viewpoint of manufacturing costs, it is preferably 1 nm or less. 2 Above 2 nm, especially 2 With regard to the contact area between the electrode and the switch memory layer 4, it is sufficient that at least one of the contact area between the first electrode 11 and the switch memory layer 4 and the contact area between the second electrode 12 and the switch memory layer 4 satisfies the above value, and it is more preferable that both contact areas satisfy the above value.
[0091] <Memory Device> (First Embodiment) The memory device of this embodiment preferably includes a switch element, and more preferably includes a switch element and a memory element. Furthermore, when including a switch element and a memory element, the memory device of the present invention is preferably made of a laminate in which the switch element and the memory element are stacked. More specifically, the memory device of this embodiment is a memory device including a laminate in which the switch element and the memory element are stacked, the switch element includes a switch layer and a first electrode disposed on the switch layer, and the switch layer has an OFF current density of 3.1×10 when the current density when a voltage half the threshold voltage is applied is defined as the OFF current density. 2 A / cm 2 It is preferable that the memory element is made of the following resistance change material, and the memory element is one of a resistance change memory element, a magnetoresistive memory element, a phase change memory element, and a ferroelectric memory element.
[0092] Fig. 3 is a schematic three-dimensional view of a memory device according to a first embodiment of the present invention, and Fig. 4 is a schematic three-dimensional view of an enlarged memory device according to the first embodiment of the present invention. As shown in Figs. 3 and 4, the memory device 100 includes a switch element 10, a memory element 20, a word line 30, and a bit line 40. The bit line 40 is orthogonal to the word line 30 in a planar view. The switch element 10 and the memory element 20 are disposed at the intersection of the word line 30 and the bit line 40 in a planar view. In other words, the memory device 100 of this embodiment is a so-called cross-point memory device.
[0093] 5 is a schematic three-dimensional diagram of a modified example of the memory device according to the first embodiment of the present invention. The memory device 200 includes a switch element 10, a memory element 20, a word line 30, and a bit line 40. The bit line 40 is disposed in a through-hole formed in the word line 30. The memory element 20 and the switch element 10 are disposed on the outer periphery of the bit line 40. The switch element 10 has a first electrode 1 disposed on the outer periphery of the switch layer 3, and a second electrode 2 disposed on the inner periphery opposite the first electrode 1, with the switch layer 3 sandwiched therebetween. In other words, the memory device 200 of this modified example is a so-called BiCS type memory device. As such, the memory device of the present invention is not limited to a cross-point type memory device, and may be various other memory devices.
[0094] The memory element 20 can be any memory element such as a resistance change memory element, a magnetoresistive memory element, a phase change memory element, or a ferroelectric memory element. Preferred embodiments of each memory element will be described below.
[0095] The resistance change memory element includes a resistance change layer. More specifically, the resistance change memory element preferably includes a stacked body in which a resistance change layer is sandwiched between an upper electrode and a lower electrode. The resistance change layer is preferably made of a metal oxide material, a metal nitride material, or a chalcogenide material. The metal oxide material is, for example, NiO x , NbO x , TiO x , TaO x , HfO x , ZrO x , MoO x , W.O. x , Pr 1-xCa x MnO 3 (PCMO). The metal nitride material is preferably at least one selected from, for example, SiN x , AlN x , ZrN x , NiN x , CuN x , CrN x The chalcogenide material is preferably at least one selected from the group consisting of Ge—Te, Sb—Te, Ge—Sb—Te, Si—Sb—Te, Ge—Ga—Te, In—Sb—Te, Ge—Se—As, and Ge—Se—As—Te. The resistance change layer may be made of carbon nanotubes.
[0096] In the resistance change memory element, the upper electrode and / or the lower electrode are preferably made of at least one selected from tungsten, titanium, copper, platinum, tungsten nitride, and titanium nitride. Tungsten, titanium, copper, and platinum are preferred as metal materials. Tungsten nitride and titanium nitride are preferred as ceramic materials.
[0097] The magnetoresistive memory element includes a stack (TMR element) in which an insulating layer is sandwiched between ferromagnetic layers. The insulating layer is made of an insulating material, such as MgO, CaO, SrO, or Al. 2 O 3 The insulating layer preferably comprises at least one material selected from the group consisting of CoFeB, FeB, NiFe, MnIr, Fe, CoPt, CoNi, Co, Ni, Pt, Ni, and Mn. The insulating layer preferably comprises at least one material selected from the group consisting of CoFeB, FeB, NiFe, MnIr, Fe, CoPt, CoNi, Co, Ni, Pt, Ni, and Mn.
[0098] The ferroelectric memory element includes a ferroelectric layer. More specifically, the ferroelectric memory element preferably includes a stacked body in which a ferroelectric layer is sandwiched between an upper electrode and a lower electrode. The ferroelectric layer is preferably composed of a ferroelectric material containing hafnium oxide, and is preferably composed of hafnium oxide doped with at least one element selected from Si, Zr, Ge, Gd, La, Y, and Yb. The ferroelectric layer may also be composed of at least one material selected from lead zirconate titanate (PZT), strontium bismuthate tantalate (SBT), and bismuth ferrite (BFO).
[0099] The phase-change memory element is a memory layer made of a phase-change material. More specifically, the phase-change memory element preferably includes a stacked body having a phase-change layer sandwiched between an upper electrode and a lower electrode. The phase-change layer is preferably made of a chalcogenide material. The chalcogenide material is preferably at least one selected from, for example, Ge—Te, Sb—Te, Ge—Sb—Te, Si—Sb—Te, Ge—Ga—Te, In—Sb—Te, Cu—Ge—Te, Cr—Ge—Te, Mn—Te, Ge—Se—As, and Ge—Se—As-Te.
[0100] Second Embodiment The storage device of the present invention is not limited to a configuration including a switch layer and a storage element separately. For example, the storage device of the present invention may be configured to include only a switch element. In this case, the switch element may function as both a switch element and a storage element. For example, the storage device of this embodiment preferably includes a resistance change storage element (storage element 21) having the above-described memory function and switch element function. In this embodiment, by using a resistance change storage element having a memory function and a switch element function, it is possible to record information in the storage element even if a switch element is not provided. However, the storage device of this embodiment may include any switch element.
[0101] 6 is a schematic three-dimensional diagram of a memory device according to a second embodiment of the present invention. As shown in FIG. 6, the memory device 101 includes a memory element 21, a word line 30, and a bit line 40. The bit line 40 is orthogonal to the word line 30 in a plan view. The memory element 21 is disposed at the intersection of the word line 30 and the bit line 40 in a plan view. In other words, the memory device 101 of this embodiment is a so-called cross-point memory device.
[0102] 7 is a schematic three-dimensional diagram of a modified example of a memory device according to the second embodiment of the present invention. As shown in FIG. 7, a memory device 201 includes a memory element 21, a word line 30, and a bit line 40. The bit line 40 is disposed in a through hole provided in the word line 30. The memory element 21 is disposed on the outer periphery of the bit line 40. In other words, the memory device 201 of this embodiment is a so-called BiCS type memory device. As such, in this embodiment, the memory device is not limited to a cross-point type memory device, and various other memory devices may be used.
[0103] The present invention will be described below based on examples, but the present invention is not limited to these examples.
[0104]
[0105]
[0106]
[0107]
[0108] The examples and comparative examples were prepared as follows. First, a quartz glass ampoule was heated and evacuated, and then raw materials were mixed to obtain the composition shown in Table 1 and placed in the quartz glass ampoule. Next, the quartz glass ampoule was sealed with an oxygen burner. Next, the sealed quartz glass ampoule was placed in a melting furnace, and the temperature was raised to 650°C to 1000°C at a rate of 10°C to 40°C / hour, and then held for 6 to 12 hours. During this holding time, the quartz glass ampoule was turned upside down to stir the molten material. Finally, the quartz glass ampoule was removed from the melting furnace and rapidly cooled to room temperature to obtain a variable resistance material.
[0109] The oxygen content of the obtained variable resistance material was measured by inert gas fusion-infrared absorption method. The results are shown in Table 1.
[0110] Next, a switching element was fabricated using the variable resistance material as a target. 2 A W electrode with a thickness of 50 nm was formed on the substrate. Next, a 100 nm thick SiO 2 An insulating layer was then formed. Then, a focus ion beam device (JEOL, JIB-4600F) was used to form a SiO 2 Holes of 500 nm in diameter were formed in the insulating layer and the W electrode layer. Next, a 150 nm thick film of variable resistance material was deposited in the formed holes to form a switch layer. Finally, a 150 nm thick W electrode was deposited on the switch layer to fabricate a switch element. The film deposition was performed by Ar sputtering under reduced pressure.
[0111] The OFF current density, ON current density, ON / OFF current ratio, and threshold voltage of the obtained switching element were measured. The results are shown in Table 2.
[0112] The OFF current density, ON current density, ON / OFF current ratio, and threshold voltage were determined as follows. First, a voltage of 0 V to 10 V was applied to the switching element, and the current value and threshold voltage flowing through the switching element were measured. The voltage applied at this time is not limited to DC voltage, AC voltage, pulse voltage, etc., but pulse voltage was used to prevent heat accumulation in the switching element. The threshold voltage was defined as the voltage value at which the electrical resistance value abruptly changes from a high resistance state to a low resistance state. The OFF current density was defined as the current value (OFF current value) flowing when a voltage equal to or greater than the threshold voltage was applied, divided by the contact area with the electrode. The ON current density was defined as the current value (ON current value) flowing when a voltage equal to or greater than the threshold voltage was applied, divided by the contact area with the electrode. The ON / OFF current ratio was determined by dividing the ON current value by the OFF current value.
[0113] The thin film sample for carrier mobility measurement was Si / SiO 2A 150 nm thick variable resistance material film was formed on a substrate by Ar sputtering. The carrier mobility of the obtained thin film sample was measured at 30°C using a resistivity / Hall measurement system (ResiTest 8308, manufactured by Toyo Corporation). The results are shown in Table 2.
[0114] The ionic r of the switch layer is shown in FIG. σ ' and hybridization π -1 As shown in FIG. 8, the ionic r σ ´ is 0.05 or more, hybridization r π -1 was 2.0 or less.
[0115] As shown in Tables 1 and 2, the variable resistance materials of Examples 1 to 7 have a carrier mobility of 2.6×10 -3 cm 2 / Vs or less, and the OFF current density is 2.55×10 2 A / cm 2 The logarithm of the ON / OFF current ratio x is log 10 On the other hand, the carrier mobility of Comparative Example 1 was 5.1×10 -3 cm 2 / Vs, and the OFF current density is 3.57 × 10 2 A / cm 2 The logarithm of the ON / OFF current ratio x is 10 x was small at 3.9.
[0116] Table 3 shows the change in carrier activation energy when a voltage is applied to the switching element, and Table 4 shows the relationship between the absolute temperature of the switching element and the Schottky barrier height. As shown in Table 3, in Example 2, when the carrier activation energy when a voltage of 0.15 V is applied to the switching layer is a (eV), and the carrier activation energy when a voltage of 0.30 V is applied to the switching layer is b (eV), the relationship a / b<1 was satisfied. Furthermore, as shown in Table 4, in Example 2, the Schottky barrier height φ B80℃ is the Schottky barrier height φ at 30°C B30℃ This was 1.04 times the previous figure.
[0117] The resistance change material of the present invention can be suitably used for a switching element that can be used in a resistance change type, magnetoresistive type, phase change type, ferroelectric type, or other memory device.
[0118] 1, 11 First electrode 2, 12 Second electrode 3 Switch layer 4 Switch memory layer 10 Switch element 20, 21 Memory element 30 Word line 40 Bit line 100, 101, 200, 201 Memory device
Claims
1. A variable resistance material containing Te, wherein the OFF current density is defined as the current density when a voltage that is 1 / 2 the threshold voltage is applied, and the OFF current density is 3.1×10 2 A / cm 2 A resistive change material, which is:
2. Furthermore, when a voltage equal to or higher than the threshold voltage is applied, the current density is defined as an ON current density, and the ON current density is 1×10 6 A / cm 2 The variable resistance material according to claim 1 .
3. Carrier mobility is 5×10 -3 cm 2 The variable resistance material according to claim 1 or 2, wherein the Vref is 0.1 V or less.
4. When the current density when a voltage equal to or higher than the threshold voltage is applied is defined as the ON current density, the ON / OFF current ratio obtained by dividing the ON current density by the OFF current density is 1×10 4 The variable resistance material according to claim 1 or 2.
5. The variable resistance material according to claim 1 or 2, wherein the threshold voltage is within a range of 0.5V to 10V.
6. The variable resistance material according to claim 1 or 2, containing, in atomic percent, 0.1% to 50% of Ge and 40% to 90% of Te.
7. The variable resistance material according to claim 1 or 2, containing, in atomic percent, 1% to 59% of the following elements: Si+Al+Ga+Sn+Bi+Cu+Ag+Zn+Y+In+Ca+Mg.
8. The variable resistance material according to claim 1 or 2, containing, in atomic percent, 0% to less than 5% of Sb.
9. The variable resistance material according to claim 1 or 2, which is substantially free of Sb, Se and As.
10. The variable resistance material according to claim 1 or 2, having an oxygen content of less than 1 atomic %.
11. The variable resistance material according to claim 1 or 2, which is a thin film.
12. A switching element material comprising the variable resistance material according to claim 1 or 2.
13. A switch layer comprising the variable resistance material according to claim 1 or 2.
14. A switch element comprising: a switch layer according to claim 13; and a first electrode disposed on the switch layer.
15. A semiconductor device comprising: a switch layer; a first electrode disposed on the switch layer; and a second electrode disposed at a position facing the first electrode with the switch layer interposed therebetween, wherein the switch layer contains Te, and when a current density when a voltage that is 1 / 2 a threshold voltage is applied is defined as an OFF current density, the OFF current density is 3.1×10 2 A / cm 2 A switching element made of a variable resistance material, which is as follows:
16. The switch element according to claim 15, wherein the first electrode is disposed on an outer circumferential surface of the switch layer, and the second electrode is disposed on an inner circumferential surface of the switch layer.
17. The switch element according to claim 15 or 16, wherein the first electrode and the second electrode are made of at least one material selected from the group consisting of tungsten, titanium, copper, platinum, tungsten nitride, and titanium nitride.
18. Ionic r of the switch layer σ ' and hybridization π -1 The switching element according to claim 15 or 16, wherein r satisfies the following value. σ ´≧0.05r π -1 <=2.0 19. A switching element according to claim 15 or 16, wherein a / b<1 is satisfied, where a is a carrier activation energy when a voltage of 0.15 V is applied to the switching layer, and b is a carrier activation energy when a voltage of 0.30 V is applied to the switching layer.
20. A storage device comprising the switch element according to claim 15 or 16.
21. A memory device comprising: a switch element according to claim 15 or 16; and a memory element.
22. A memory device including a laminate in which a switch element and a memory element are laminated, the switch element including a switch layer and a first electrode disposed on the switch layer, the switch layer having an OFF current density of 3.1×10 2 A / cm 2 A storage device comprising the following resistance change material, wherein the memory element is any one of a resistance change memory element, a magnetoresistive memory element, a phase change memory element, and a ferroelectric memory element.
Citation Information
Patent Citations
Nonvolatile semiconductor memory device and method of manufacturing the same
JP2010287872A
Rectifier element for crosspoint-based memory array architecture
JP2010519762A
Switch element and memory device
JP2015135917A
Memory element including variable resistance material layer
JP2018164085A