Electrode catalyst layer, membrane electrode assembly, and polymer electrolyte fuel cell
The electrode catalyst layer with a conductive carrier, metal particles, ionic liquid, and inorganic film enhances proton conductivity and durability in polymer electrolyte fuel cells, addressing issues of low humidification and long-term performance.
Patent Information
- Application Number
- PCT/JP2024/012903
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-20
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-24
AI Technical Summary
Polymer electrolyte fuel cells face challenges in maintaining high power generation performance and durability, particularly under low humidification conditions and during long-term operation, where proton transport decreases and catalyst coarsening occurs, limiting output and durability.
An electrode catalyst layer comprising catalyst particles with a conductive carrier, metal particles, an ionic liquid, and an inorganic film containing Si, where the ionic liquid is an imidazolium salt, such as 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, and a fibrous material with electron or proton conductivity, which enhances proton conduction and prevents catalyst coarsening.
The solution improves proton conductivity and maintains high power generation performance over long periods by preventing ionic liquid outflow and catalyst coarsening, achieving excellent durability and output in polymer electrolyte fuel cells.
Smart Images

Figure JP2024012903_24102024_PF_FP_ABST
Abstract
Description
Electrode catalyst layer, membrane electrode assembly, and polymer electrolyte fuel cell
[0001] The present invention relates to an electrode catalyst layer, a membrane electrode assembly, and a polymer electrolyte fuel cell.
[0002] Fuel cells are power generation systems that generate electricity from the chemical reaction between hydrogen and oxygen. Compared to conventional power generation methods, fuel cells are characterized by high efficiency, low environmental impact, and low noise, and are attracting attention as a clean energy source of the future. In particular, solid polymer fuel cells, which can be used at around room temperature, are seen as promising for use in automotive power sources and stationary power sources for homes, and in recent years, various research and development efforts have been conducted on solid polymer fuel cells. Challenges for their practical application include improving cell performance such as power generation characteristics and durability, establishing infrastructure, and reducing manufacturing costs.
[0003] A polymer electrolyte fuel cell is generally constructed by stacking a large number of unit cells. A unit cell has a structure in which a membrane electrode assembly, in which a fuel electrode (anode) for supplying fuel gas and an oxygen electrode (cathode) for supplying oxidant are bonded to both sides of a polymer electrolyte membrane, is sandwiched between separators having gas flow paths and cooling water flow paths. The fuel electrode (anode) and oxygen electrode (cathode) are mainly composed of an electrode catalyst layer containing at least a catalytic material such as a platinum-based noble metal, a conductive support, and a polymer electrolyte, and a gas diffusion layer that is both gas permeable and electrically conductive.
[0004] In a polymer electrolyte fuel cell, electricity can be generated through the following electrochemical reaction. First, in the fuel electrode-side electrode catalyst layer, hydrogen contained in the fuel gas is oxidized by a catalytic substance to produce protons and electrons. The generated protons pass through the polymer electrolyte in the electrode catalyst layer and the polymer electrolyte membrane in contact with the electrode catalyst layer, and reach the oxygen electrode-side electrode catalyst layer. At the same time, the generated electrons pass through the conductive support in the fuel electrode-side electrode catalyst layer, the gas diffusion layer in contact with the fuel electrode-side electrode catalyst layer, the separator, and an external circuit, and reach the oxygen electrode-side electrode catalyst layer. Finally, in the oxygen electrode-side electrode catalyst layer, the protons and electrons react with oxygen contained in an oxidant gas, such as air, to produce water. In this series of reactions, the proton conduction resistance is greater than the electron conduction resistance. Therefore, efficient proton conduction is important for improving reactivity and fuel cell performance.
[0005] Currently, fuel cells with high output and durability are desired to reduce the cost of fuel cells. However, under low humidification conditions, proton transport in the polymer electrolyte in the catalyst layer decreases, resulting in a decrease in output. Furthermore, the catalyst in the catalyst layer coarsens during long-term operation, resulting in a decrease in output.
[0006] To address the above-mentioned problems, Patent Document 1 proposes a catalyst layer containing an ionic liquid.
[0007] Patent No. 7026669
[0008] Patent Document 1 describes that the inclusion of an ionic liquid in an electrode catalyst layer provides excellent proton transport capacity even under low-humidity conditions, and is expected to improve output. However, the ionic liquid gradually leaks out during long-term operation, causing a gradual decrease in output, resulting in durability issues when used as a fuel cell. Furthermore, the inclusion of an ionic liquid does not prevent catalyst coarsening during long-term operation. In other words, even if the inclusion of an ionic liquid alone improves output, it is limited to a short period of time and does not solve the durability issue.
[0009] The present invention has been made in light of the above-mentioned points, and an object of the present invention is to provide an electrode catalyst layer, a membrane electrode assembly, and a polymer electrolyte fuel cell that are excellent in power generation performance and durability.
[0010] [1] An electrode catalyst layer for a polymer electrolyte fuel cell, the electrode catalyst layer comprising catalyst particles, a polymer electrolyte, and a fibrous material, the catalyst particles comprising a conductive support, a plurality of metal particles supported on the conductive support, an ionic liquid in contact with the surfaces of the metal particles and the conductive support, and an inorganic film covering the surfaces of the metal particles and the conductive support via the ionic liquid, the inorganic film containing Si, and the ratio of the number of silicon atoms to the total number of atoms of carbon, nitrogen, oxygen, fluorine, silicon, sulfur, and platinum elements, as determined by energy dispersive X-ray spectroscopy of the electrode catalyst layer, is 0.5 at% or more and 10 at% or less. [2] The electrode catalyst layer according to [1], wherein the inorganic film contains silica. [3] The electrode catalyst layer according to [1] or [2], wherein the ionic liquid is an imidazolium salt. [4] The electrode catalyst layer according to [3], wherein the ionic liquid is 1-alkyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide. [5] The electrode catalyst layer according to [3], wherein the ionic liquid is 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide. [6] The electrode catalyst layer according to any one of [1] to [5], wherein the fibrous material exhibits at least one of electron conductivity and proton conductivity. [7] The electrode catalyst layer according to any one of [1] to [6], wherein the fibrous material has an azole structure. [8] A polymer electrolyte membrane and a membrane electrode assembly provided on at least one surface of the polymer electrolyte membrane. [9] A solid polymer fuel cell comprising the membrane electrode assembly according to [8].
[0011] According to the present invention, it is possible to provide an electrode catalyst layer, a membrane electrode assembly, and a polymer electrolyte fuel cell that are excellent in power generation performance and durability.
[0012] Fig. 4(a) is a plan view of the membrane electrode assembly as viewed from the oxygen electrode side of the electrode catalyst layer, and Fig. 4(b) is a schematic cross-sectional view taken along line X-X' in Fig. 4(a). Fig. 4(b) is an exploded perspective view showing an example of the configuration of a polymer electrolyte fuel cell.
[0013] Hereinafter, embodiments of the present invention will be described with reference to the drawings. Note that the present invention is not limited to the embodiments described below, and modifications such as design changes can be made based on the knowledge of those skilled in the art. Such modified embodiments are also included in the scope of the present invention. In addition, the drawings are appropriately exaggerated to facilitate understanding.
[0014] [Configuration of Electrode Catalyst Layer] The specific configuration of the electrode catalyst layer according to this embodiment will be described below with reference to the drawings. As shown in the schematic diagram of FIG. 1 , the electrode catalyst layer 10 according to this embodiment is configured to include catalyst particles 12, a polymer electrolyte 13, and a fibrous material 14. The electrode catalyst layer 10 may have voids in the portions where none of the above components are present. The electrode catalyst layer 10 is fixed to the surface of a polymer electrolyte membrane 11 by bonding or the like.
[0015] (Catalyst Particle 12) First, the catalyst particle 12 according to this embodiment will be described. As shown in the schematic diagrams of Figures 2 and 3, the catalyst particle 12 includes a conductive support 15, a plurality of metal particles 16 supported on the conductive support 15, an ionic liquid 17, and an inorganic film 18.
[0016] (Conductive Support) The conductive support 15 may be made of a support material that is conductive and capable of supporting the catalyst particles 12 without being eroded by the metal particles 16. Carbon particles may be used for the conductive support 15. Examples of the carbon particles that may be used include carbon black, graphite, activated carbon, carbon nanotubes, carbon nanofibers, and fullerenes.
[0017] The particle size of the conductive support is preferably about 10 nm or more and 1000 nm or less, and more preferably about 10 nm or more and 100 nm or less. When the particle size is 10 nm or more, the conductive support does not pack too densely in the electrode catalyst layer 10, thereby preventing a decrease in the gas diffusibility of the electrode catalyst layer 10. When the particle size is 1000 nm or less, the occurrence of cracks in the electrode catalyst layer 10 is prevented. The particle size of the conductive support is a volume average diameter measured by a laser diffraction / scattering method.
[0018] When the conductive support 15 is a carbon particle, the peak intensity ratio (G / D ratio) of the G band to the D band of the conductive support 15 by Raman spectroscopy is preferably 1.6 or more and 2.2 or less, more preferably 1.8 or more and 2.0 or less. If the G / D ratio is within the above range, the crystallinity of the conductive support 15 is suitable, and therefore, a decrease in the durability of the electrode catalyst layer 10 can be suppressed. In this specification, the wavelength of the laser light used in Raman spectroscopy is 532 nm. The G band is defined as a wavelength of 1580 cm -1 The D band refers to the Raman peak located around 1360 cm -1 This refers to the Raman peaks located near the
[0019] (Metal Particles) The material of the metal particles 16 can be, for example, a metal included in the platinum group, a metal other than the platinum group, or an alloy, oxide, double oxide, or carbide of these metals. Metals included in the platinum group include platinum, palladium, ruthenium, iridium, rhodium, and osmium. Metals other than the platinum group can include iron, lead, copper, chromium, cobalt, nickel, manganese, vanadium, molybdenum, gallium, and aluminum. In particular, the metal particles 16 are preferably particles of platinum or a platinum alloy. The constituent material of the metal particles 16 contained in the electrode catalyst layer can be one type or two or more types.
[0020] The average particle size of the metal particles 16 is preferably 0.5 nm or more and 20 nm or less, and more preferably 1 nm or more and 5 nm or less. If the average particle size of the metal particles 16 is 0.5 nm or more, the stability as a catalyst is improved. If the average particle size of the metal particles 16 is 20 nm or less, the activity as a catalyst is improved. The particle size of the metal particle 16 conductive support is the average diameter determined by analysis of a TEM image (e.g., JIS H7804:2005).
[0021] (Ionic Liquid) As shown in Figures 2 and 3, the ionic liquid 17 is in contact with the surfaces of the conductive support 15 and the metal particles 16. It is sufficient that the ionic liquid 17 is in contact with a portion of the surface of the conductive support 15, and it is sufficient that the ionic liquid 17 is in contact with a portion of the surface of the metal particles 16. When the conductive support 15 has gaps such as pores therein, the ionic liquid may permeate at least a portion of the interior of the conductive support 15. When the inorganic film 18 has gaps such as pores therein, the ionic liquid 17 may also permeate at least a portion of the interior of the inorganic film 18. The ionic liquid 17 can permeate any gaps in the conductive support 15 and the inorganic film 18.
[0022] Although there is no particular limitation on the ionic liquid 5, it is preferably an imidazolium salt. An imidazolium salt is a salt of a cation having an imidazole ring structure and a counter anion. Examples of the cation are as follows: R and R' are independently -CH 3 , -C 2 H 5 , -C 3 H 7 , -C 4 H 9 , -C 6 H 13 , -CH 2 -CH=CH 2 is. An example of a counter anion is Cl. - ,Br - , I - , BF 4 - , P.F. 6 - , FSI ((FSO 2 ) 2 N -), TFSI((CF 3 SO 2 ) 2 N - ) Ionic liquid 17 is preferably an imidazolium salt, and specifically, ionic liquid 17 preferably contains 1-alkyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide. Examples of the alkyl group contained in this compound include a methyl group, an ethyl group, a butyl group, a pentyl group, a heptyl group, an octyl group, a nonyl group, and a decyl group. Of these, the alkyl group is preferably a butyl group. That is, ionic liquid 17 preferably contains 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide. In this case, ionic liquid 17 is preferably composed only of 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, but may also contain other 1-alkyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imides in addition to this compound. When ionic liquid 17 contains multiple types of 1-alkyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, it is preferable that the content of 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide is 50% or more of the total mass of ionic liquid 17.
[0023] In the catalyst particles 12, the volume of the ionic liquid 17 is preferably 10% to 50% of the mesopore volume of the conductive support 15, and more preferably 10% to 30%. The mesopore volume, i.e., the pore volume of the mesopore region, is the total volume of pores from 2 nm to 100 nm. The mesopore volume can be determined, for example, by low-temperature nitrogen adsorption. The mesopore volume in the conductive support may be 2 to 50 nm.
[0024] If the volume fraction of the ionic liquid 17 is 10% or more, proton conduction between the polymer electrolyte 13 and the metal particles 16 via the ionic liquid 17 is likely to be favorable. In particular, sufficient oxygen reduction activity can be obtained in the electrode catalyst layer of the air electrode. Furthermore, if the volume fraction of the ionic liquid 17 is 50% or less, the amount of the ionic liquid 17 is not too large. Although the ionic liquid 17 has the function of passing protons, its degree of permeability is secondary compared to the polymer electrolyte 13. If the amount of the ionic liquid 17 becomes too large, the separation between the catalyst particles 12 and the polymer electrolyte 13 increases, which can increase resistance. In contrast, if the volume fraction of the ionic liquid 17 is 50% or less, an increase in resistance due to an excess of the ionic liquid 17 is favorably suppressed. By including the ionic liquid 17 in the electrode catalyst layer 10 as described above, it is possible to suppress a decrease in proton transport to the catalyst even under low-humidification conditions.
[0025] (Inorganic film 18) The inorganic film 18 covers the surfaces of the conductive support 15 and the surfaces of the metal particles 16 via the ionic liquid 17 that is in contact with the surfaces of the conductive support 15 and the metal particles 16. It is sufficient that only a portion of the surface of the conductive support is covered with the inorganic film 18, and it is sufficient that only a portion of the surface of the metal particles is covered with the inorganic film 18. The inorganic film 18 covers the metal particles 16 mainly via the ionic liquid 17. The thickness of the inorganic film 18 may be uniform or non-uniform.
[0026] The material of the inorganic film 18 is an inorganic material containing Si. In particular, the material of the inorganic film 18 preferably contains silica (silicon oxide), and in particular, it is preferable that the material contains silica obtained by hydrolysis and dehydration condensation of tetraethoxysilane. By using such silica, the inorganic film 18 is formed into a multilayer structure made of silica films, which makes it easier to retain the ionic liquid 17 inside the inorganic film 18. The composition of silica generated from tetraethoxysilane is (SiO 2 ) n is.
[0027] The thickness of the inorganic film 18 may be 1 nm or more and 100 nm or less, preferably 10 nm or more and 50 nm or less, and more preferably 20 nm or more and 40 nm or less. If the thickness of the inorganic film 18 is 1 nm or more, the inorganic film 18 is easily formed. Furthermore, if the thickness of the inorganic film 18 is 100 nm or less, sufficient gaps between layers in the multilayer structure are easily secured. The thickness of the inorganic film 18 may be uniform or non-uniform.
[0028] (Composition of Catalyst Particles) There are no particular limitations on the ratio of the mass of the metal particles to the total mass of the conductive carrier and metal particles of the catalyst particles, but it can be, for example, 10 to 70 mass %.
[0029] (Polymer Electrolyte) The polymer electrolyte 13 contained in the electrode catalyst layer 10 can be a proton-conductive electrolyte. For example, a fluorine-based polymer electrolyte or a hydrocarbon-based polymer electrolyte can be used as the polymer electrolyte. For example, a polymer electrolyte having a tetrafluoroethylene skeleton can be used as the fluorine-based polymer electrolyte. An example of a polymer electrolyte having a tetrafluoroethylene skeleton is Nafion (registered trademark) manufactured by DuPont. For example, a sulfonated polyether ketone, sulfonated polyether sulfone, sulfonated polyether ether sulfone, sulfonated polysulfide, and sulfonated polyphenylene can be used as the hydrocarbon-based polymer electrolyte.
[0030] The polymer electrolyte contained in the polymer electrolyte membrane 11 and the polymer electrolyte 13 contained in the electrode catalyst layer 10 may be the same electrolyte or different electrolytes. However, taking into consideration the interfacial resistance at the interface between the polymer electrolyte membrane 11 and the electrode catalyst layer 10 and the rate of dimensional change in the polymer electrolyte membrane 11 and the electrode catalyst layer 10 when humidity changes, it is preferable that the polymer electrolyte contained in the polymer electrolyte membrane 11 and the polymer electrolyte 13 contained in the electrode catalyst layer 10 be the same electrolyte or polymer electrolytes with similar thermal expansion coefficients.
[0031] The content of the polymer electrolyte 13 in the electrode catalyst layer 10 is preferably 40 parts by mass or more and 140 parts by mass or less, when the content of the conductive support 15 in the electrode catalyst layer 10 is taken as 100 parts by mass. If the content of the polymer electrolyte 13 is 40 parts by mass or more, it is possible to suppress a decrease in proton conductivity due to a defect in the proton conduction pathway. As a result, it becomes easier to ensure a balance between proton conductivity and electron conductivity in the electrode catalyst layer 10. Furthermore, if the content of the polymer electrolyte 13 is 140 parts by mass or less, a three-phase interface is more likely to be formed in the electrode catalyst layer 10, thereby enhancing catalytic activity.
[0032] (Fibrous Material) Any material may be used as the fibrous material 14 as long as it can maintain its fibrous shape without being affected by the metal particles 16 and the polymer electrolyte 13. In order to reduce the resistance of the electrode catalyst layer 10, the fibrous material 14 preferably exhibits electron conductivity and / or proton conductivity.
[0033] As the electron-conductive fibrous material 14, carbon fibers such as carbon fibers, carbon nanofibers, and carbon nanotubes can be used. Carbon nanofibers and carbon nanotubes are preferred.
[0034] Examples of the fibrous material 14 exhibiting proton conductivity include fibers obtained by processing a polymer electrolyte into a fibrous form. As the polymer electrolyte, fluororesins and hydrocarbon-based resins can be used. For example, the fluororesin is Nafion (a registered trademark, manufactured by Chemours), and the hydrocarbon-based resin is engineering plastics or copolymers thereof into which sulfonic acid groups have been introduced. Acid-doped polybenzazoles, which exhibit proton conductivity by being doped with an acid, can also be suitably used.
[0035] The fibrous material 14 may also be a resin fiber having a basic functional group in the main chain or side chain functional group that can interact with an acidic substance. These interact with the acidic substance contained in the polymer electrolyte 13, thereby coating the surface of the resin fiber with the polymer electrolyte and enabling proton conductivity. Examples of basic functional groups that can interact with acidic substances include =N- groups, -NH2 groups, >NH groups, >N- groups, ammonium groups, amine derivatives, pyridine derivatives, imidazole derivatives, and imidazolium groups. Specific examples of resin fibers include polybenzimidazole (PBI), polybenzoxazole, polybenzthioazole, polyvinylimidazole, and polyallylamine. In particular, polybenzimidazole (PBI) having an azole structure is preferred from the standpoints of proton conductivity and processability.
[0036] The fiber diameter of the fibrous material 14 is preferably 100 to 400 nm, more preferably 150 to 250 nm, and even more preferably 180 to 220 nm, with the average fiber diameter and / or the peak of the fiber diameter distribution being 100 to 400 nm, more preferably 150 to 250 nm, and even more preferably 180 to 220 nm. By setting the fiber diameter within this range, when the polymer fibers are incorporated into an electrode catalyst layer, the voids in the electrode catalyst layer can be increased and a decrease in proton conductivity can be suppressed, enabling higher output. If the average fiber diameter and / or the peak of the fiber diameter distribution of the polymer fibers is smaller than the above range, the voids may become narrow and sufficient drainage and gas diffusion properties may not be ensured. In this case, water may remain in the electrode catalyst layer 10, reducing output and promoting deterioration of the electrode catalyst layer. If the average fiber diameter and / or the peak of the fiber diameter distribution of the polymer fibers is larger than the above range, the proton conduction pathways through the polymer electrolyte 13 and the electron conduction pathways through the conductive carrier 15 may be blocked, resulting in increased resistance.
[0037] Furthermore, the fiber length of the fibrous material 14 preferably has a peak in the fiber length distribution of 1 to 100 μm, more preferably 5 to 50 μm, and even more preferably 5 to 30 μm. By setting the peak of the fiber length distribution within this range, it is possible to suppress the occurrence of cracks when forming the electrode catalyst layer 10, thereby increasing the durability of the electrode catalyst layer and the membrane electrode assembly. In addition, it is possible to increase the voids within the electrode catalyst layer, enabling higher output.
[0038] The fiber diameter of the fibrous material 14 can be obtained, for example, by observing the cross section of the electrode catalyst layer 10 using a scanning electron microscope (SEM) and measuring the diameter of the fibrous material 14 exposed at the cross section. When the fibrous material 14 is cut obliquely, the shape of the exposed cross section may be elliptical. In this case, the fiber diameter of the fibrous material 14 can be obtained by measuring the diameter of a perfect circle fitted along the minor axis. The average fiber diameter and / or the peak of the fiber diameter distribution can be obtained by measuring the fiber diameters of the fibrous material 14 at multiple locations, for example, 50 locations, and creating an arithmetic mean and / or frequency distribution.
[0039] The content of the fibrous material 14 in the electrode catalyst layer 10 is preferably equal to or less than 100 parts by mass of the conductive support 15, and can be about 5 to 100 parts by mass. If the content of the fibrous material 14 in the electrode catalyst layer 10 is small, the effects of reducing proton conduction resistance and improving gas diffusibility cannot be sufficiently obtained, and cracks may occur when the electrode catalyst layer 10 is formed, reducing durability during long-term operation. On the other hand, if the content of the fibrous material 14 in the electrode catalyst layer 10 is large, the catalytic reaction may be inhibited, resulting in a decrease in cell performance.
[0040] By including the fibrous material 14 in the electrode catalyst layer 10 as described above, cracks do not occur during the formation of the electrode catalyst layer 10, and it is possible to increase the number of pores in the electrode catalyst layer 10.
[0041] (Si Amount in Electrode Catalyst Layer) In this embodiment, the ratio of the number of silicon atoms to the total number of atoms of carbon, nitrogen, oxygen, fluorine, silicon, sulfur, and platinum elements in the electrode catalyst layer obtained by energy dispersive X-ray spectroscopy is 0.5 at % or more and 10 at %.
[0042] The ratio of the number of silicon atoms to the total number of carbon, nitrogen, oxygen, fluorine, silicon, sulfur, and platinum atoms can be measured by elemental mapping using, for example, a transmission electron microscope (TEM-EDX) equipped with an energy dispersive X-ray spectrometer. The X-ray acceleration voltage in TEM-EDX is preferably 200 kV. This acceleration voltage allows the electron beam to penetrate to a thickness of about 100 nm in a specific region, thereby obtaining elemental information for the electrode catalyst layer. The shape of the region (observation area) where elemental mapping is performed using TEM-EDX can be rectangular, for example, a square of 150 nm x 150 nm or a rectangle of 30 nm x 50 nm. The shape of the region (observation area) where elemental mapping is performed using TEM-EDX is preferably an observation area where the catalyst particles 12 occupy 20% or more of the area.
[0043] The catalyst layer to be subjected to TEM-EDX is processed into thin sections of about 100 nm. For processing into thin sections, known methods such as focused ion beam and ultramicrotome can be used. When processing into thin sections, it is particularly preferable to perform the processing while cooling the electrode catalyst layer 10 in order to reduce damage to the polymer electrolyte 13 that constitutes the electrode catalyst layer 10.
[0044] (Function) As a result of extensive research into the power generation performance and durability of polymer electrolyte fuel cells, the inventors have found that the proton conductivity in the electrode catalyst layer has a significant effect on power generation performance, and that coating the metal particles serving as catalysts and the conductive carrier supporting the catalyst with an ionic liquid improves proton conductivity. Furthermore, they have found that coating the metal particles and the conductive carrier with an inorganic film containing Si suppresses the outflow of the ionic liquid and the coarsening of catalyst particles, thereby achieving high power generation performance over the long term.
[0045] According to this embodiment, as shown in FIG. 3 , the inorganic film 18 covers the metal particles 16, thereby preventing the metal particles 16 from eluting into the polymer electrolyte 13 surrounding the catalyst particles 12 in the electrode catalyst layer. On the other hand, if the inorganic film 18 directly covers each metal particle 16, contact between the proton-conducting polymer electrolyte 13 and the metal particles 16 acting as a catalyst for the electrode reaction would be prevented. In contrast, in the configuration of this embodiment, an ionic liquid 17 that allows protons to pass through is interposed between the inorganic film 18 and the metal particles 16, so that protons are conducted via the ionic liquid 17. Furthermore, if the ionic liquid 17 penetrates into the gaps in the inorganic film 18, the ionic liquid 17 in the inorganic film 18 also contributes to proton conduction. It is advantageous from the standpoint of electron conduction if the metal particles 16 have exposed portions that are not covered by the ionic liquid 17 and the inorganic film 18.
[0046] 2, contact of the surface of the conductive support 15 with the ionic liquid 17 contributes to improving the proton conductivity in the electrode catalyst layer 10, and coating the conductive support 15 with the inorganic film 18 via the ionic liquid hinders the movement of the metal particles 16, thereby contributing to suppressing coarsening of the metal particles 16. Furthermore, if the conductive support 15 has exposed portions that are not covered by the ionic liquid 17 and the inorganic film 18, this is advantageous from the viewpoint of electron conduction.
[0047] Furthermore, by setting the ratio of the number of silicon atoms to the total number of atoms of carbon, nitrogen, oxygen, fluorine, silicon, sulfur, and platinum elements, as determined by energy dispersive X-ray spectroscopy of the electrode catalyst layer, to 0.5 at% or more and 10 at% or less, a polymer electrolyte fuel cell that exhibits high power generation performance and is excellent in durability can be obtained.
[0048] If the ratio of the number of silicon atoms to the total number of atoms of carbon, nitrogen, oxygen, fluorine, silicon, sulfur, and platinum elements obtained by energy dispersive X-ray spectroscopy of the electrode catalyst layer 10 is less than 0.5 at%, this means that the amount of inorganic film 18 that suppresses the outflow of ionic liquid 17 that improves the proton conductivity of the electrode catalyst layer 10 and the coarsening of metal particles 16 is too small. If the ratio of the number of silicon atoms to the total number of atoms of carbon, nitrogen, oxygen, fluorine, silicon, sulfur, and platinum elements obtained by energy dispersive X-ray spectroscopy of the electrode catalyst layer is more than 10 at%, this means that the amount of inorganic film 18 is too large. If the amount of inorganic film 18 is too large, it may inhibit the conduction of protons and electrons.
[0049] The weight ratio of the inorganic film 18 to the catalyst particles 12 is preferably 0.01 or more and 0.2 or less. When the weight ratio of the inorganic film 18 is 0.01 or more, the inorganic film 18 is formed on the surface of the catalyst particles 12 to a degree that sufficiently suppresses the elution of the metal particles 16. Furthermore, the ionic liquid 17 is easily retained within the inorganic film 18. When the weight ratio of the inorganic film 18 is 0.2 or less, the thickness and area of the inorganic film 18 are not too large, ensuring sufficient contact between the metal particles 16 and the ionic liquid 17 to achieve suitable proton conduction. The weight ratio of the inorganic film 18 can be determined, for example, using inductively coupled plasma (ICP) atomic emission spectroscopy (ICP-OES or ICP-AES), X-ray fluorescence spectroscopy (XRF), or X-ray photoelectron spectroscopy (XPS). As described above, the inclusion of the inorganic film 18 can suppress the coarsening of the metal particles 16 and the outflow of the ionic liquid 17, thereby improving durability.
[0050] (Polymer Electrolyte Membrane) Examples of the polymer electrolyte used in the polymer electrolyte membrane 11 are the same as the polymer electrolyte in the electrode catalyst layer. That is, the polymer electrolyte may be any polymer electrolyte having proton conductivity, such as a fluorine-based polymer electrolyte or a hydrocarbon-based polymer electrolyte. Examples of fluorine-based polymer electrolytes are Nafion (registered trademark: manufactured by DuPont), Flemion (registered trademark: manufactured by Asahi Glass Co., Ltd.), and Gore-Select (registered trademark: manufactured by Gore Japan LLC). Examples of hydrocarbon-based polymer electrolytes are engineering plastics and engineering plastics into which sulfonic acid groups have been introduced.
[0051] (Method for Producing Catalyst Particles) The catalyst particles 12 can be produced by supporting metal particles 16 on a conductive support 15 by a known method to produce a catalyst-supported support, impregnating the catalyst-supported conductive support with an ionic liquid 17 to form a precursor, and then forming an inorganic film 18 on the surface of the precursor. A known film formation method, such as a sol-gel method, is used to form the inorganic film 18. By using a method in which the inorganic film 18 is formed after impregnating the catalyst-supported support with the ionic liquid 17, it is possible to form the inorganic film 18 without requiring a surfactant. Therefore, it is possible to avoid heat treatment and suppress deterioration of the conductive support 15, thereby suppressing a decrease in the durability of the electrode catalyst layer 10. Furthermore, the inorganic film can be coated on the surfaces of the conductive support and the metal particles via the ionic liquid.
[0052] [Configuration of Membrane Electrode Assembly] Next, with reference to FIG. 4, a specific configuration of a membrane electrode assembly 1 including an electrode catalyst layer 10 according to this embodiment will be described. FIG. 4 shows an example of the configuration of a membrane electrode assembly according to this embodiment, where (a) is a plan view of the membrane electrode assembly as viewed from the oxygen electrode side of the electrode catalyst layer 10, and (b) is a cross-sectional view taken along line X-X' in (a). As shown in FIG. 4, the membrane electrode assembly 1 includes a polymer electrolyte membrane 11 and electrode catalyst layers 10C and 10A bonded to either side of the polymer electrolyte membrane 11. In this embodiment, the electrode catalyst layer 10C formed on the upper surface of the polymer electrolyte membrane 11 is a cathode-side electrode catalyst layer constituting the oxygen electrode, and the electrode catalyst layer 10A formed on the lower surface of the polymer electrolyte membrane 11 is an anode-side electrode catalyst layer constituting the fuel electrode. Hereinafter, the pair of electrode catalyst layers 10C and 10A may be abbreviated as "electrode catalyst layer 10" when there is no need to distinguish between them. The outer periphery of the electrode catalyst layer 10 may be sealed by a gasket 21 or the like.
[0053] [Method for Manufacturing Electrode Catalyst Layer and Membrane Electrode Assembly] The following describes a method for manufacturing the electrode catalyst layer 10 and membrane electrode assembly 1 described above. First, a catalyst ink is prepared. At least the catalyst particles 12, polymer electrolyte 13, and fibrous material 14 described above are mixed in a dispersion medium, and the mixture is then subjected to a dispersion treatment to prepare the catalyst ink. The dispersion treatment can be performed using, for example, a planetary ball mill, a bead mill, or an ultrasonic homogenizer. The solvent used as the dispersion medium for the catalyst ink may be any solvent that does not corrode the conductive support 15, metal particles 16, ionic liquid 17, inorganic membrane 18, polymer electrolyte 13, and fibrous material 14, and that can dissolve or disperse the polymer electrolyte 13 as a fine gel in a highly fluid state. The solvent may contain water. It is desirable for the catalyst ink to contain at least a volatile liquid organic solvent. However, because lower alcohols used as solvents have a high risk of ignition, it is preferable to use such solvents in a mixed solvent with water. The amount of water to be added is not particularly limited as long as it is an amount that does not cause the polymer electrolyte 13 to separate and become cloudy or gel.
[0054] The prepared catalyst ink is applied to a substrate and then dried, thereby removing the solvent component from the catalyst ink coating, and forming an electrode catalyst layer 10 on the substrate. The substrate may be a polymer electrolyte membrane 11, a transfer substrate, a gas diffusion layer 22, or the like. When the polymer electrolyte membrane 11 is used as the substrate, for example, the catalyst ink is applied directly to the surface of the polymer electrolyte membrane 11, and the solvent is then removed from the catalyst ink coating to form the electrode catalyst layer 10C. Thereafter, the catalyst ink is applied directly to the surface opposite the polymer electrolyte membrane 11 so as to face the electrode catalyst layer 10A across the polymer electrolyte membrane 11, and the solvent is then removed from the catalyst ink coating to form the electrode catalyst layer 10A, thereby obtaining the membrane electrode assembly 1.
[0055] When a transfer substrate is used, for example, a catalyst ink is applied to the transfer substrate and then dried to produce a transfer substrate with a catalyst layer. Thereafter, the surface of the electrode catalyst layer 10 on the transfer substrate with the catalyst layer is brought into contact with the polymer electrolyte membrane 11, and the electrode catalyst layer 10 and the polymer electrolyte membrane 11 are bonded together by applying heat and pressure. The electrode catalyst layers 10 are bonded to both sides of the polymer electrolyte membrane 11, and the transfer substrate is then removed, thereby producing a membrane / electrode assembly 1.
[0056] When a gas diffusion layer is used as the substrate, a catalyst ink is applied to the surface of the gas diffusion layer and then dried to produce a gas diffusion layer with a catalyst layer. The surface of the electrode catalyst layer 10 in the catalyst-layer-equipped gas diffusion layer is then brought into contact with the polymer electrolyte membrane 11, and the electrode catalyst layer 10 and the polymer electrolyte membrane 11 are then bonded together by applying heat and pressure. The membrane / electrode assembly 1 can be produced by bonding the electrode catalyst layers 10 to both sides of the polymer electrolyte membrane 11.
[0057] Various coating methods can be used to apply the catalyst ink to the substrate. Examples of coating methods include die coating, roll coating, curtain coating, spray coating, and squeegee coating. Die coating is preferred as the coating method. Die coating is preferred because it stabilizes the film thickness during the coating period and allows for intermittent coating. Methods for drying the catalyst ink coating include drying using a hot air oven, IR (far infrared) drying, drying using a hot plate, and reduced pressure drying. The drying temperature is 40°C or higher and 200°C or lower, and preferably approximately 40°C or higher and 120°C or lower. The drying time is 0.5 minutes to 1 hour, and preferably approximately 1 minute to 30 minutes.
[0058] When forming the electrode catalyst layer 10 on a transfer substrate or a gas diffusion layer, the pressure and temperature applied to the electrode catalyst layer 10 during transfer of the electrode catalyst layer 10 affect the power generation performance of the membrane electrode assembly 1. To obtain a membrane electrode assembly 1 with high power generation performance, the pressure applied to the electrode catalyst layer 10 is preferably 0.1 MPa or more and 20 MPa or less. A pressure of 20 MPa or less prevents the electrode catalyst layer 10 from being excessively compressed. A pressure of 0.1 MPa or more prevents a decrease in power generation performance due to a decrease in the bonding strength between the electrode catalyst layer 10 and the polymer electrolyte membrane 11. Considering the improvement of the bonding strength at the interface between the polymer electrolyte membrane 11 and the electrode catalyst layer 10 and the suppression of interfacial resistance, the temperature during bonding is preferably near the glass transition point of the polymer electrolyte membrane 11 or the polymer electrolyte 13 contained in the electrode catalyst layer 10.
[0059] The transfer substrate can be, for example, a polymer film or a sheet formed from a fluorine-based resin. Fluorine-based resins have excellent transferability. Examples of fluorine-based resins include ethylene tetrafluoroethylene copolymer (ETFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroperfluoroalkyl vinyl ether copolymer (PFA), and polytetrafluoroethylene (PTFE). Examples of polymers that form the polymer film include polyimide, polyethylene terephthalate, polyamide (Nylon (registered trademark)), polysulfone, polyethersulfone, polyphenylene sulfide, polyether ether ketone, polyetherimide, polyarylate, and polyethylene naphthalate.
[0060] The thickness of the electrode catalyst layer 10 is preferably 2 μm or more and 20 μm or less. If the thickness is greater than 20 μm, cracks are likely to occur, and when used in a fuel cell, the diffusibility and conductivity of gas and generated water are reduced, resulting in a decrease in output. Furthermore, if the thickness is less than 2 μm, the layer thickness is likely to vary, and the catalyst particles 12 and polymer electrolyte 13 inside are likely to become non-uniform. Cracks on the surface of the electrode catalyst layer 10 and non-uniform thickness are likely to adversely affect the durability of the fuel cell when used and operated over a long period of time, and are therefore undesirable.
[0061] The thickness of the electrode catalyst layer 10 can be measured, for example, by observing the cross section of the membrane electrode assembly 1 using a scanning electron microscope (SEM). For example, it can be measured by measuring the thickness of the electrode catalyst layer within a field of view that includes the entire electrode catalyst layer at an observation magnification of approximately 1000 to 10000 times. In order to grasp the thickness uniformly within the catalyst layer, it is preferable to perform similar measurements at at least 20 or more observation points. As a method for exposing the cross section of the membrane electrode assembly 1, for example, known methods such as ion milling and ultramicrotome can be used.
[0062] Here, by adjusting the blending ratio of the fibrous material, the blending ratio of the polymer electrolyte, the solvent composition of the catalyst ink, the dispersion strength when preparing the catalyst ink, the heating temperature and heating rate of the applied catalyst ink, etc., the electrode catalyst layer 10 can be made to have sufficient gas diffusibility and proton conductivity.
[0063] [Configuration of Polymer Electrolyte Fuel Cell] Next, a specific configuration example of a polymer electrolyte fuel cell 3 including the membrane electrode assembly 1 according to this embodiment will be described with reference to Fig. 5. Fig. 5 is an exploded perspective view showing a configuration example of a polymer electrolyte fuel cell 3 equipped with the membrane electrode assembly 1. Note that Fig. 5 shows an example of the configuration of a single cell, and the polymer electrolyte fuel cell 3 is not limited to this configuration and may have a configuration in which a plurality of single cells are stacked.
[0064] As shown in Figure 5, the polymer electrolyte fuel cell 3 includes a membrane electrode assembly 1, a gas diffusion layer 22C, and a gas diffusion layer 22A. The gas diffusion layer 22C is disposed opposite an electrode catalyst layer 10C, which is a cathode-side electrode catalyst layer on the oxygen electrode side of the membrane electrode assembly 1. The gas diffusion layer 22A is disposed opposite an electrode catalyst layer 10A, which is an anode-side electrode catalyst layer on the fuel electrode side of the membrane electrode assembly 1. The electrode catalyst layer 10C and the gas diffusion layer 22C constitute an oxygen electrode 2C, and the electrode catalyst layer 10A and the gas diffusion layer 22A constitute a fuel electrode 2A. In addition, a gasket 16C on the oxygen electrode side and a gasket 16A on the fuel electrode side are disposed to prevent gas leakage from the outer peripheral portion of the polymer electrolyte membrane 11 to which the electrode catalyst layer 10 is not bonded are disposed.
[0065] The polymer electrolyte fuel cell 3 further includes a separator 23C disposed opposite the oxygen electrode 2C and a separator 23A disposed opposite the fuel electrode 2A. The separator 23C includes a gas flow path 24C for flowing reactant gas formed on the surface facing the gas diffusion layer 22C, and a cooling water flow path 25C for flowing cooling water formed on the surface opposite to the surface on which the gas flow path 24C is formed. The separator 23A has a similar configuration to the separator 23C, and includes a gas flow path 24A formed on the surface facing the gas diffusion layer 22A, and a cooling water flow path 25A formed on the surface opposite to the surface on which the gas flow path 24A is formed. The separators 23C and 23A are made of a conductive and gas-impermeable material. In the polymer electrolyte fuel cell 3, an oxidant such as air or oxygen is supplied to the oxygen electrode 2C through the gas flow path 24C of the separator 23C, and a fuel gas containing hydrogen or an organic fuel is supplied to the fuel electrode 2A through the gas flow path 24A of the separator 23A, thereby generating electricity.
[0066] By employing the membrane electrode assembly 1 according to this embodiment, it is possible to provide sufficient drainage, gas diffusibility, and proton conductivity, and to exhibit high power generation performance over the long term. That is, according to this embodiment, it is possible to provide an electrode catalyst layer 10, a membrane electrode assembly 1, and a polymer electrolyte fuel cell 3 that have sufficient proton conductivity during operation of the polymer electrolyte fuel cell and are capable of exhibiting high power generation performance over the long term. Therefore, the present invention can be suitably used in stationary cogeneration systems and fuel cell vehicles that use polymer electrolyte fuel cells, as well as in hydrogen production electrolysis systems that use membrane electrode assemblies, and has great industrial utility value.
[0067] Hereinafter, a membrane electrode assembly according to an embodiment of the present invention will be described.
[0068] Example 1 Production of Catalyst Particles Platinum-supported carbon (Pt mass ratio: 50% by mass), in which platinum particles were supported on a highly crystallized carbon support, was added to acetonitrile, and an ionic liquid was added in an amount equivalent to 60% of the mesopore volume of the platinum-supported carbon. The mesopore volume of the platinum-supported carbon (conductive support) was substantially the same as that of the conductive support. This mixture was subjected to ultrasonic dispersion for 30 minutes, stirred overnight with a stirrer, and then the acetonitrile was removed using an evaporator to obtain platinum-supported carbon impregnated with the ionic liquid. The ionic liquid used was a liquid consisting solely of 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide. The mesopore volume of the platinum-supported carbon was determined using a low-temperature nitrogen adsorption method, targeting pores ranging from 2 nm to 100 nm.
[0069] Next, the platinum-supported carbon impregnated with the ionic liquid was added to water, and after ultrasonic stirring, a mixed solution containing tetraethoxysilane (TEOS) and ethanol was added. Sodium hydroxide was then added and stirred for two hours, after which a separated product was obtained using a centrifuge. The separated product was then dried at 80°C for six hours to obtain catalyst particles of Example 1. These catalyst particles have an inorganic film made of silica. The amount of inorganic film coating on the catalyst particles was adjusted by the amount of TEOS, so that the weight ratio of the inorganic film (weight of silica / total weight of silica and platinum-supported carbon) was 0.1.
[0070] <Preparation of membrane electrode assembly> A catalyst ink was prepared by dispersing a mixture of the catalyst particles of Example 1, a polymer electrolyte, a fibrous material, and a dispersion medium. The materials other than the catalyst particles were as follows:
[0071] Polymer electrolyte: Fluorine-based polymer electrolyte (Nafion (registered trademark) dispersion, manufactured by Wako Pure Chemical Industries, Ltd.) Fibrous material: Resin fiber having an azole structure (average fiber length 20 μm, average fiber diameter 220 nm) Dispersion medium: Mixture of water and 1-propanol in a mass ratio of 1:1
[0072] The blending amounts of the polymer electrolyte and fibrous material were 70 parts by mass and 20 parts by mass, respectively, with the blending amount of the conductive carrier in the catalyst particles in the catalyst ink being 100 parts by mass. The blending amount of the dispersion medium was such that the solids concentration in the catalyst ink was 10% by mass. The dispersion treatment was carried out using a planetary ball mill at a rotation speed of 600 rpm for 60 minutes. During this treatment, zirconia balls with a diameter of 2 mm were added to approximately one-third of the zirconia container.
[0073] Next, the catalyst ink was applied to one side of a polymer electrolyte membrane (Nafion (registered trademark) 211, manufactured by DuPont) using a die coater to a thickness of 100 μm to form a coating film. The coating film had a square shape with a side length of 50 mm. A drying process was then carried out in an oven at 80°C to volatilize the dispersion medium contained in the coating film, thereby forming an air electrode catalyst layer.
[0074] Next, a catalyst ink was applied to a surface of the polymer electrolyte membrane opposite the surface on which the air electrode catalyst layer was formed, to a thickness of 30 μm, to form a coating film. The coating film had a square shape with a side length of 50 mm and was formed in a position opposite the air electrode catalyst layer. A drying process was then carried out in an oven at 80°C to volatilize the dispersion medium contained in the coating film, thereby forming an anode catalyst layer. This resulted in a membrane electrode assembly equipped with the electrode catalyst layer of Example 1.
[0075] Example 2 A membrane electrode assembly of Example 2 was obtained using the same materials and steps as in Example 1, except that in the catalyst particle production step, the amount of TEOS added was changed so that the weight ratio of the inorganic membrane was 0.2.
[0076] Example 3 A membrane electrode assembly of Example 3 was obtained using the same materials and steps as in Example 1, except that in the catalyst particle production step, the amount of TEOS added was changed so that the weight ratio of the inorganic membrane was 0.01.
[0077] Example 4 A membrane electrode assembly of Example 4 was obtained in the same manner as in Example 1, except that carbon nanofibers (VGCF-H (registered trademark), manufactured by Showa Denko Packaging, average fiber length 7 μm, average fiber diameter 150 nm) were added as the fibrous material in the step of preparing the catalyst ink.
[0078] Comparative Example 1 A membrane electrode assembly of Comparative Example 1 was obtained using the same materials and steps as in Example 1, except that in the catalyst particle production step, the amount of TEOS added was changed so that the weight ratio of the inorganic membrane was 0.3.
[0079] (Comparative Example 2) A membrane electrode assembly of Comparative Example 2 was obtained using the same materials and steps as in Example 1, except that no inorganic film was formed on the platinum-supported carbon. That is, the catalyst particles of Comparative Example 2 did not have an inorganic film.
[0080] (Comparative Example 3) A membrane electrode assembly of Comparative Example 3 was obtained using the same materials and steps as in Example 1, except that the platinum-supported carbon was not impregnated with an ionic liquid and the inorganic membrane was not formed. That is, the catalyst particles of Comparative Example 3 consisted only of platinum-supported carbon, and did not have an ionic liquid or an inorganic membrane.
[0081] <Measurement of the ratio of silicon atoms> The ratio of the number of silicon atoms to the total number of atoms of carbon, nitrogen, oxygen, fluorine, silicon, sulfur, and platinum elements obtained by energy dispersive X-ray spectroscopy of the electrode catalyst layer was measured. Specifically, a thin section of the electrode catalyst layer was first obtained using a cryo-ultramicrotome, which processes the electrode catalyst layer while cooling it. Next, elemental mapping was performed using a transmission electron microscope (TEM-EDX) equipped with energy dispersive X-ray spectroscopy to obtain the elemental ratio of each element and calculate the ratio of silicon atoms. The acceleration voltage was 200 kV. The observation area was 150 nm × 150 nm in size, and the platinum-supported carbon occupied 20% or more of the area of the field of view.
[0082] <Evaluation of Power Generation Performance> The power generation performance was measured in accordance with the "Cell Evaluation and Analysis Protocol" published by the New Energy and Industrial Technology Development Organization (NEDO). A JARI standard cell was used as the evaluation unit cell. The unit cell was configured with gas diffusion layers (SIGRACET® 22BB, manufactured by SGL), gaskets, and separators arranged on both sides of a membrane electrode assembly and clamped to a predetermined surface pressure. An IV measurement was then performed as described in the "Cell Evaluation and Analysis Protocol." The cell temperature during the measurement was set to 80°C. The humidification conditions were a relative humidity of 88% RH at the anode and 42% RH at the cathode. Hydrogen was used as the fuel gas, and air was used as the oxidant gas. Hydrogen was flowed at a flow rate that provided a hydrogen utilization rate of 70%, and air was flowed at a flow rate that provided an oxygen utilization rate of 40%.
[0083] <Evaluation of durability> For each example and comparative example, a load response simulated potential cycle test described in "Cell Evaluation and Analysis Protocol" published by the New Energy and Industrial Technology Development Organization (NEDO) was carried out using the evaluation unit cell used in the above-mentioned evaluation of power generation performance. IV measurements were carried out before and after the test under the same conditions as those for the evaluation of power generation performance.
[0084] <Comparison Results> Table 1 shows the ratio of the number of silicon atoms in the cathode-side electrode catalyst layer of fuel cells including the membrane electrode assemblies of Examples 1 to 4 and the membrane electrode assemblies 1 of Comparative Examples 1 to 3, as well as the power generation performance and durability. With regard to power generation performance, a case in which the voltage was 0.65 V or higher at a current of 35 A was marked with "◎", a case in which the voltage was less than 0.65 V at a current of 35 A but 0.65 V or higher at a current of 25 A was marked with "◯", and a case in which the voltage was less than 0.65 V at a current of 25 A was marked with "×". With regard to durability, a case in which the voltage drop rate after the test compared to before the test at a current density of 1.5 A / cm2 was less than 20% was marked with "◎", a case in which the voltage drop rate was 20% or more but less than 30% was marked with "◯", and a case in which the voltage drop rate was 30% or more was marked with "×".
[0085]
[0086] As shown in Table 1, in all of Examples 1 to 4, the ratio of the number of silicon atoms in the electrode catalyst layer was 0.5 at % or more and 10 at % or less. The power generation performance and durability were all rated as "◎" or "◯." That is, in Examples 1 to 4, membrane electrode assemblies capable of constituting fuel cells with excellent power generation performance and durability were obtained.
[0087] On the other hand, in all of Comparative Examples 1 to 3, the ratio of the number of silicon atoms in the electrode catalyst layer was outside the range of 0.5 at% or more and 10 at% or less. At least one of the power generation performance and durability was rated "x." That is, when the ratio of the number of silicon atoms in the electrode catalyst layer was outside the above range, at least one of the power generation performance and durability was reduced.
[0088] Therefore, it was found that when the ratio of the number of silicon atoms in the electrode catalyst layer is 0.5 at % or more and 10 at % or less, a membrane electrode assembly capable of constituting a fuel cell with excellent power generation performance and durability can be obtained.
[0089] 1...membrane electrode assembly, 2C...oxygen electrode, 2A...fuel electrode, 3...solid polymer fuel cell, 10, 10C, 10A...electrode catalyst layer, 11...polymer electrolyte membrane, 12...catalyst particles, 13...polymer electrolyte, 14...fibrous material, 15...conductive support, 16...metal particles, 17...ionic liquid, 18...inorganic membrane, 21C, 21A...gasket, 22C, 22A...gas diffusion layer, 23C, 23A...separator, 24C, 24A...gas flow path, 25C, 25A...cooling water flow path.
Claims
1. An electrode catalyst layer for a polymer electrolyte fuel cell, the electrode catalyst layer comprising catalyst particles, a polymer electrolyte, and a fibrous material, the catalyst particles having a conductive support, a plurality of metal particles supported on the conductive support, an ionic liquid in contact with surfaces of the metal particles and the conductive support, and an inorganic film covering the surfaces of the metal particles and the conductive support via the ionic liquid, the inorganic film containing Si, and a ratio of the number of silicon atoms to the total number of atoms of carbon, nitrogen, oxygen, fluorine, silicon, sulfur, and platinum elements in the electrode catalyst layer, as measured by energy dispersive X-ray spectroscopy, is 0.5 at% or more and 10 at% or less.
2. The electrocatalyst layer according to claim 1, wherein the inorganic film comprises silica.
3. The electrode catalyst layer according to claim 1 or 2, wherein the ionic liquid is an imidazolium salt.
4. The electrode catalyst layer according to claim 3, wherein the ionic liquid is 1-alkyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide.
5. The electrode catalyst layer according to claim 3, wherein the ionic liquid is 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide.
6. The electrode catalyst layer according to claim 1 or 2, wherein the fibrous material exhibits at least one of electronic conductivity and proton conductivity.
7. The electrode catalyst layer according to claim 1 or 2, wherein the fibrous material has an azole structure.
8. A membrane electrode assembly comprising a polymer electrolyte membrane and the electrode catalyst layer according to claim 1 or 2 provided on at least one surface of the polymer electrolyte membrane.
9. A polymer electrolyte fuel cell comprising the membrane electrode assembly according to claim 8.
Citation Information
Patent Citations
Novel catalyst layer compositions for improving the performance of membrane electrode assemblies with ionic liquids
JP7026669B2
Electrode catalyst, fuel cell using it, and methods of manufacturing them
JP2008282635A
Coated fuel cell catalyst materials
JP2022128440A
Ionic liquid-impregnated silica-coated catalyst particles, membrane electrode assembly, and fuel cell
JP2024057940A
Substrate processing apparatus
KR102662926B1
Cited By
Membrane electrode assembly and solid polymer fuel cell
WO2026155260A1