Phenolic resin
The phenolic resin, synthesized from phenols, dodecanediamine, and aldehydes, addresses the challenge of enhancing handling stability and fuel efficiency in run-flat tires by improving sidewall rigidity, thus meeting the performance requirements of run-flat tires at zero air pressure.
Patent Information
- Application Number
- PCT/JP2024/014274
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2024-04-08
- Publication Date
- 2024-10-24
AI Technical Summary
Run-flat tires require materials that enhance handling stability and fuel efficiency while maintaining sidewall rigidity at zero air pressure, which existing tire tread rubber compositions fail to adequately address.
A phenolic resin synthesized from phenols, dodecanediamine, and aldehydes is blended into the tire rubber composition, providing structural units with linear or branched carbon chains to improve handling stability and fuel efficiency, and enhance sidewall rigidity.
The phenolic resin improves steering stability, fuel efficiency, and maintains sidewall rigidity, ensuring the tire's performance and durability even at zero air pressure.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002
Abstract
Description
phenolic resin CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This international application claims priority based on Japanese Patent Application No. 2023-67595, filed with the Japan Patent Office on April 18, 2023, the entire contents of which are incorporated herein by reference.
[0002] The present disclosure relates to phenolic resins.
[0003] A tire tread is the part of an automobile tire that comes into contact with the road surface. Various tire tread patterns have been devised to achieve desired performance. Tire treads are made of tire tread rubber compositions. To achieve the desired performance, tire tread rubber compositions contain various materials.
[0004] Run-flat tires are tires that can be driven for a certain distance even if the tire pressure drops to 0 kPa due to a puncture or other reason. Even if the tire pressure drops to 0 kPa due to a puncture or other reason, if a run-flat tire is used, the vehicle can be moved to the nearest workshop without having to change to a spare tire. ISO stipulates that run-flat tires can be driven for 80 km at 0 kPa of air pressure at a speed of 80 km / h.
[0005] Run-flat tire structures can be broadly divided into those in which the tire sidewalls are reinforced with sidewall reinforcing rubber and those in which a ring-shaped core is inserted inside. The sidewall reinforcing rubber must have a certain degree of rigidity so that the sidewalls do not collapse even when the air pressure is 0 kPa. Note that one type of rubber composition can be used for both the tire tread rubber and the sidewall reinforcing rubber.
[0006] Patent Document 1 discloses a technology aimed at providing an inexpensive tire that has excellent durability, can suppress a decrease in complex modulus due to temperature rise, can improve handling stability over a wide speed range, and is inexpensive.
[0007] Patent Document 2 discloses a technology aimed at providing a tire tread rubber composition that can reduce rolling resistance (RR) and improve fuel economy without impairing the braking performance and cornering performance of an automobile on wet road surfaces, and a pneumatic tire that uses the rubber composition.
[0008] Patent Document 3 discloses a technique relating to a phenolic resin that has an excellent elastic modulus when compounded with rubber. Patent Document 4 discloses a technique relating to benzoxazine.
[0009] Japanese Patent Application Laid-Open No. 2008-050431 Japanese Patent Application Laid-Open No. 2000-080205 Japanese Patent Application Laid-Open No. 2021-004270 Japanese Patent Application Laid-Open No. 2008-222930
[0010] The performance required for automobile tires is steering stability and fuel economy. Run-flat tires must have sidewalls that are resistant to collapse even when the air pressure is 0 kPa.
[0011] In one aspect of the present disclosure, it is preferable to provide a phenolic resin that, when compounded in an automobile tire, can improve the handling stability and fuel economy of the automobile and make the sidewall of a run-flat tire less susceptible to crushing.
[0012] One aspect of the present disclosure is a phenolic resin (excluding benzoxazine-type phenolic resins) synthesized from raw materials including 100 parts by mass of a phenol, 20 to 80 parts by mass of dodecanediamine, and 1 to 20 parts by mass of an aldehyde, and having one or more structural units derived from dodecanediamine having a linear or branched carbon chain in the molecule.
[0013] When the phenolic resin according to one aspect of the present disclosure is compounded in an automobile tire, the steering stability and fuel economy of the automobile can be improved, and the sidewall of a run-flat tire can be made less susceptible to crushing.
[0014] Exemplary embodiments of the present disclosure will now be described.
[0015] 1. Composition of Phenolic Resin The phenolic resin of the present disclosure is synthesized from raw materials including 100 parts by mass of a phenol (P), 20 to 80 parts by mass of dodecanediamine (D), and 1 to 20 parts by mass of an aldehyde (F). The phenolic resin of the present disclosure has one or more structural units derived from dodecanediamine (D) having a linear or branched carbon chain in the molecule.
[0016] The phenolic resin of the present disclosure is preferably synthesized from raw materials containing 100 parts by mass of a phenol (P) and 30 to 70 parts by mass of dodecanediamine (D).
[0017] Examples of the phenols (P) include phenol, cresol, xylenol, nonylphenol, para-tertiary-butylphenol, para-secondary-butylphenol, naphthol, catechol, resorcinol, hydroquinone, methylhydroquinone, dimethylhydroquinone, etc. Phenol is preferred as the phenol (P).
[0018] The two amino groups contained in the dodecanediamine (D) may be any positional isomer. The dodecane skeleton contained in the dodecanediamine (D) may be linear or branched. The dodecane skeleton contained in the dodecanediamine (D) may have an unsaturated bond. As the dodecanediamine (D), dodecanediamine having a linear dodecane skeleton and no unsaturated bond is preferred. As the dodecanediamine (D), 1,12-dodecanediamine is more preferred.
[0019] Examples of the aldehydes (F) include aldehydes (F) that can be used in the production of phenolic resins. Examples of the aldehydes (F) include formaldehyde, paraformaldehyde, and trioxane (metaformaldehyde). These aldehydes (F) can be used alone or in combination of two or more. Alternatively, the aldehydes (F) may be dissolved in water in advance.
[0020] The phenolic resin of the present disclosure is preferably synthesized from raw materials containing 100 parts by mass of a phenol (P) and 5 to 15 parts by mass of an aldehyde (F).
[0021] In this specification, the amount of aldehydes (F) refers to the amount of the active ingredient. The active ingredient is aldehydes (F). For example, in a 37% formaldehyde aqueous solution, the mass ratio of the active ingredient is 37 mass%. For example, if a raw material contains W g of a 37% formaldehyde aqueous solution, the amount of formaldehyde in the raw material (i.e., the amount of the active ingredient) is 0.37 × W g.
[0022] The phenolic resin of the present disclosure excludes, for example, benzoxazine-type phenolic resins. That is, the phenolic resin of the present disclosure is preferably a phenolic resin other than benzoxazine-type phenolic resins.
[0023] 2. Method for Producing Phenolic Resin The phenolic resin of the present disclosure is synthesized from raw materials including 100 parts by mass of a phenol (P), 20 to 80 parts by mass of dodecanediamine (D), and 1 to 20 parts by mass of an aldehyde (F).
[0024] When producing the phenolic resin of the present disclosure, pure water can be added for dilution. The amount of pure water added is preferably 25 to 125 parts by mass, more preferably 50 to 100 parts by mass, per 100 parts by mass of the phenol (P).
[0025] The method for producing a phenolic resin according to the present disclosure is, for example, as follows: Predetermined amounts of phenols (P), dodecanediamine (D), and pure water are mixed and heated to 100°C while stirring. A specified amount of aldehydes (F) is added dropwise to the mixture, and the mixture is allowed to react. The dropwise addition time is preferably 0.5 to 3.5 hours, more preferably 1 to 3 hours. The reaction time is preferably 2 to 6 hours, more preferably 3 to 5 hours.
[0026] Next, the heater is set to a temperature of 200°C, and the reaction is carried out for 0.5 to 3.5 hours, more preferably 1 to 3 hours. Next, the heater is set to a temperature of 180°C, and the mixture is distilled under vacuum to remove unreacted monomers. Through these steps, the phenolic resin of the present disclosure is obtained.
[0027] Although the detailed mechanism of the above reaction is not clear, it is believed to be a resin formed by a three-component reaction of dodecanediamine (D), aldehydes (F), and phenols (P).
[0028] 3. Rubber Composition The rubber composition is, for example, a tire tread rubber composition or a sidewall reinforcing rubber for a run-flat tire. The rubber composition contains the phenolic resin of the present disclosure and a diene-based rubber.
[0029] Examples of diene rubbers include styrene butadiene rubber (SBR), butadiene rubber (BR), isoprene rubber (IR), butyl rubber, natural rubber (NR), etc. These diene rubbers can be used alone or in combination of two or more.
[0030] The amount of the phenolic resin in the rubber composition is preferably 0.5 to 30 parts by mass, and more preferably 5 to 20 parts by mass, per 100 parts by mass of the total amount of diene rubber.
[0031] The rubber composition contains, for example, silica, which is known as white carbon in the tire industry. The amount of silica in the rubber composition is preferably 1 to 200 parts by mass, and more preferably 20 to 120 parts by mass, per 100 parts by mass of the total amount of diene rubber.
[0032] The rubber composition contains, for example, carbon black. The amount of carbon black in the rubber composition is preferably 0.5 to 200 parts by mass, and more preferably 1 to 120 parts by mass, per 100 parts by mass of the total amount of diene rubber.
[0033] The rubber composition contains, for example, silica and carbon black. The total amount of silica and carbon black in the rubber composition is preferably 1 to 200 parts by mass, and more preferably 20 to 120 parts by mass, per 100 parts by mass of the total amount of diene rubber.
[0034] The rubber composition contains, for example, a coupling agent. When the rubber composition contains silica, the rubber composition preferably contains a coupling agent. The amount of the coupling agent in the rubber composition is preferably 0.5 to 20 parts by mass, and more preferably 2 to 10 parts by mass, per 100 parts by mass of the total amount of diene rubber.
[0035] The rubber composition contains, for example, an antioxidant. The amount of the antioxidant in the rubber composition is preferably 0.1 to 10 parts by mass, and more preferably 0.5 to 5 parts by mass, per 100 parts by mass of the total amount of diene rubber.
[0036] The rubber composition contains, for example, zinc white. The amount of zinc white in the rubber composition is preferably 0.1 to 10 parts by mass, and more preferably 0.5 to 5 parts by mass, per 100 parts by mass of the total amount of diene rubber.
[0037] The rubber composition contains, for example, stearic acid. The amount of stearic acid in the rubber composition is preferably 0.1 to 10 parts by mass, and more preferably 0.5 to 5 parts by mass, per 100 parts by mass of the total amount of diene rubber.
[0038] The rubber composition contains, for example, an extender oil. The amount of the extender oil in the rubber composition is preferably 1 to 50 parts by mass, and more preferably 5 to 30 parts by mass, per 100 parts by mass of the total amount of diene rubber.
[0039] The rubber composition contains, for example, oil sulfur. The amount of oil sulfur in the rubber composition is preferably 0.1 to 10 parts by mass, and more preferably 0.5 to 5 parts by mass, per 100 parts by mass of the total amount of diene rubber.
[0040] The rubber composition contains, for example, a vulcanization accelerator. The amount of the vulcanization accelerator in the rubber composition is preferably 0.1 to 10 parts by mass, and more preferably 0.5 to 5 parts by mass, per 100 parts by mass of the total amount of diene rubber.
[0041] 4. Example (4-1) Synthesis of Phenolic Resin A 100 g of phenol, 42 g of dodecanediamine, and 75 g of pure water were charged into a reactor equipped with a stirrer, reflux condenser, and thermometer. The temperature was then raised to 100°C. 32 g of a 37% aqueous formaldehyde solution was then added dropwise over 2 hours. The amount of formaldehyde (i.e., the amount of active ingredient) was calculated by multiplying 32 g by 0.37.
[0042] Next, the mixture was reacted under reflux conditions for 4 hours. Next, the temperature was raised to 200°C and the mixture was reacted for 2 hours. Next, the temperature was lowered to 180°C. Next, the mixture was distilled under vacuum. Next, unreacted monomers were removed. Next, phenolic resin A, which was a reactive product, was extracted. Through the above steps, phenolic resin A was obtained.
[0043] The phenolic resin A is a phenolic resin synthesized from raw materials containing 100 parts by mass of a phenol (P), 20 to 80 parts by mass of dodecanediamine (D), and 1 to 20 parts by mass of an aldehyde (F).
[0044] The phenolic resin A is a phenolic resin having one or more structural units derived from dodecanediamine in the molecule, the carbon chain of which is linear or branched. The phenolic resin A is a phenolic resin excluding benzoxazine-type phenolic resins.
[0045] (4-2) Synthesis of Phenolic Resin B: 100 g of phenol, 48.2 g of dodecanediamine, and 75 g of pure water were charged into a reactor equipped with a stirrer, reflux condenser, and thermometer. The temperature was then raised to 100°C. 36 g of a 37% aqueous formaldehyde solution was then added dropwise over 2 hours. The amount of formaldehyde (i.e., the amount of active ingredient) was calculated by multiplying 36 g by 0.37.
[0046] Next, the mixture was reacted under reflux conditions for 4 hours. Next, the temperature was raised to 200°C and the mixture was reacted for 2 hours. Next, the temperature was lowered to 180°C. Next, the mixture was distilled under vacuum. Next, unreacted monomers were removed. Next, the reaction product, phenolic resin B, was taken out. Through the above steps, phenolic resin B was obtained.
[0047] The phenolic resin B is a phenolic resin synthesized from raw materials containing 100 parts by mass of a phenol (P), 20 to 80 parts by mass of dodecanediamine (D), and 1 to 20 parts by mass of an aldehyde (F).
[0048] The phenolic resin B is a phenolic resin having one or more structural units derived from dodecanediamine in the molecule, the carbon chain of which is linear or branched. The phenolic resin B is a phenolic resin excluding benzoxazine-type phenolic resins.
[0049] (4-3) Synthesis of Phenolic Resin C 100 g of phenol, 31 g of triethylenetetramine, and 75 g of pure water were charged into a reactor equipped with a stirrer, reflux condenser, and thermometer. The temperature was then raised to 100°C. 43.3 g of a 37% aqueous formaldehyde solution was then added dropwise over 2 hours. The amount of formaldehyde (i.e., the amount of active ingredient) was calculated by multiplying 43.3 g by 0.37.
[0050] Next, the mixture was reacted under reflux conditions for 4 hours. Next, the temperature was raised to 200°C and reacted for 2 hours. Next, the temperature was lowered to 180°C. Next, the mixture was distilled under vacuum. Next, unreacted monomers were removed. Next, the reaction product, phenolic resin C, was extracted. Through the above steps, phenolic resin C was obtained. Phenolic resin C is not a phenolic resin having one or more structural units derived from dodecanediamine in the molecule.
[0051] (4-4) Preparation of Tire Tread Rubber Composition Tire tread rubber compositions of Examples 1 and 2 and Comparative Examples 1 to 4 were prepared by the following method. First, the materials shown in Table 1, excluding vulcanization accelerators 1 and 2 and oil sulfur, were mixed in the amounts shown in Table 1, and kneaded for 10 minutes in an internal Banbury mixer. Next, vulcanization accelerators 1 and 2 and oil sulfur were added in the amounts shown in Table 1, and kneaded for an additional 2 minutes. Through the above steps, tire tread rubber compositions of Examples 1 and 2 and Comparative Examples 1 to 4 were obtained.
[0052] The blend amounts in Table 1 are in parts by mass. The materials shown in Table 1 were as follows.
[0053] *1 SBR rubber: SBR-1502 (product name) manufactured by ENEOS Materials Corporation *2 BR rubber: BR01 (product name) manufactured by ENEOS Materials Corporation *3 Silica: Nipsil AQ (product name) manufactured by Tosoh Silica Corporation *4 Carbon black: Seast 6 (product name) manufactured by Tokai Carbon Co., Ltd. *5 Phenolic resin D: Cashew-modified phenolic resin, BRM-845 (product name) manufactured by AICA Kogyo Co., Ltd. *6 Phenolic resin E: KORESIN resin (product name) manufactured by BASF Corporation *7 Phenolic resin F: Phenolic resin sold as a tackifier. Manufactured by AICA Corporation, CRM-973 (trade name) *8 Stearic acid: NOF Corporation, Tsubaki (trade name) *9 Antioxidant: Seiko Chemical Co., Ltd., Ozonone 6C (trade name) *10 Zinc oxide: Seido Chemical Industry Co., Ltd., zinc oxide 3 types *11 Coupling agent: bis[3-(triethoxysilyl)propyl]tetrasulfide, Evonik Corporation, Si69 (trade name) *12 Extender oil: ENEOS Corporation, Aromax 3 (trade name) *13 Oil sulfur: dispersible powder sulfur, Yabu Shoten Co., Ltd. *14 Vulcanization accelerator 1: Sanselaer CM-G (trade name) manufactured by Sanshin Chemical Industry Co., Ltd. *15 Vulcanization accelerator 2: Sanselaer D (trade name) manufactured by Sanshin Chemical Industry Co., Ltd. (4-5) Preparation of vulcanized rubber test pieces Vulcanized rubber test pieces were prepared for each of the tire tread rubber compositions of each example and each comparative example. The vulcanized rubber test pieces were prepared by press-vulcanizing the tire tread rubber composition in a predetermined mold at 170° C. for 10 minutes.
[0054] (4-6) Method for Measuring Softening Point of Phenolic Resin The softening point of each of the phenolic resins A to F was measured using a vapor phase softening point measuring device EX-719PD manufactured by Elex Scientific Co., Ltd. The heating rate during the softening point measurement was 2.5°C / min.
[0055] The softening point is preferably 70° C. or higher and 150° C. or lower. When the softening point is 70° C. or higher, the effect of the phenolic resin in reinforcing the rubber composition is further enhanced. When the softening point is 150° C. or lower, the workability when using the phenolic resin is good.
[0056] (4-7) Method for Measuring Type A Hardness The Type A hardness of vulcanized rubber test pieces was measured for each of the Examples and Comparative Examples. The measurement temperature was 23±2°C. The Type A hardness was a 0.5 second value. The Type A hardness is preferably 68 or more.
[0057] (4-8) Method for measuring storage modulus E' at 20°C For each of the Examples and Comparative Examples, the storage modulus E' at 20°C of the vulcanized rubber test pieces was measured using a VR-7130 fully automatic viscoelasticity analyzer manufactured by Ueshima Seisakusho Co., Ltd. The measurement conditions were as follows:
[0058] Initial strain: 10% Amplitude: ±2% Frequency: 10 Hz Temperature: 20°C The storage modulus E' at 20°C is an index representing hardness. The storage modulus E' at 20°C is preferably 6.5 GPa or more. When the storage modulus E' at 20°C is 6.5 GPa or more, a tire manufactured using the rubber composition has excellent steering stability.
[0059] (4-9) Method for Measuring Tan δ at 60° C. For each of the Examples and Comparative Examples, the tan δ at 60° C. of the vulcanized rubber test pieces was measured under the following measurement conditions.
[0060] Conditions: Initial strain: 10%, Amplitude: ±2%, Frequency: 10 Hz, Temperature: 60°C Tan δ at 60°C is an index showing rolling resistance. Tan δ at 60°C is preferably less than 0.1. When Tan δ at 60°C is less than 0.1, a tire manufactured using the rubber composition is excellent in fuel economy.
[0061] (4-10) Evaluation Method of Steering Stability For each of the Examples and Comparative Examples, a prototype tire was produced using the tire tread rubber composition. The prototype tire was a pneumatic tire. The prototype tire size was 195 / 65 R15.
[0062] Four prototype tires were mounted on a vehicle, and a test driver conducted a driving sensory test. The test driver changed lanes while driving at 120 km / h, and evaluated the vehicle's controllability on a scale of 1 to 5. The higher the score, the better the controllability. A score of 3 or higher is preferable.
[0063] (4-11) Evaluation Results For each of the tire tread rubber compositions of the Examples and Comparative Examples, the measurement results of the softening point, Type A hardness, storage modulus E' at 20°C, and Tan δ at 60°C are shown in Table 2. Furthermore, for each of the tire tread rubber compositions of the Examples and Comparative Examples, the evaluation results of the steering stability are shown in Table 2.
[0064] The softening points shown in Table 2 are the softening points of the phenolic resins contained in the tire tread rubber compositions of each Example and Comparative Example. In Examples 1 and 2, the softening points, Type A hardness, storage modulus E' at 20°C, Tan δ at 60°C, and handling stability were all within the preferred ranges.
[0065] When the tire tread rubber compositions of Examples 1 and 2 are used as tire treads, the tire is excellent in handling stability and fuel economy. When the tire tread rubber compositions of Examples 1 and 2 are used as sidewall reinforcing rubber for run-flat tires, the sidewall has sufficient rigidity.
[0066] Phenolic resin C is not a phenolic resin having one or more structural units derived from dodecanediamine having a linear or branched carbon chain in the molecule. In Comparative Example 1 using phenolic resin C, the softening point, storage modulus E' at 20°C, and handling stability were within the preferred ranges, but the type A hardness and Tan δ at 60°C were outside the preferred ranges.
[0067] Phenolic resin D is a cashew-modified phenolic resin. In Comparative Example 2 using Phenolic resin D, similarly to Comparative Example 1, the softening point, storage modulus E′ at 20°C, and handling stability were within the preferred ranges, but the Type A hardness and Tan δ at 60°C were outside the preferred ranges.
[0068] The tires manufactured using the tire tread rubber compositions of Comparative Examples 1 and 2 are judged to be inferior in fuel economy. Furthermore, when the tire tread rubber compositions of Comparative Examples 1 and 2 are used as sidewall reinforcing rubber for run-flat tires, the rigidity of the sidewall is judged to be insufficient.
[0069] Phenolic resin E is KORESIN, which is sold as a tackifier. Comparative Example 3, which used phenolic resin E, had a softening point within the preferred range, but the type A hardness, storage modulus E' at 20°C, Tan δ at 60°C, and handling stability were outside the preferred ranges.
[0070] Phenolic resin F is CRM-973, a benzoxazine type phenolic resin. In Comparative Example 4, in which phenolic resin F was used, only the softening point was within the preferred range, but the other evaluation results were outside the preferred ranges.
[0071] 5. Effects of the Phenolic Resin The phenolic resin of the present disclosure can be used to produce a tire that improves the handling stability of an automobile and achieves low fuel consumption. The phenolic resin of the present disclosure can be used as a phenolic resin for compounding in a tire tread. In this case, the performance of the automobile tire is improved. The phenolic resin of the present disclosure can be used in the sidewall reinforcing rubber of a run-flat tire. In this case, the sidewall of the run-flat tire has high rigidity.
[0072] 6. Other Embodiments Although the embodiments of the present disclosure have been described above, the present disclosure is not limited to the above-described embodiments and can be implemented in various modifications.
[0073] (6-1) The function of one component in each of the above embodiments may be shared among multiple components, or the functions of multiple components may be performed by one component. Also, part of the configuration of each of the above embodiments may be omitted. Furthermore, at least part of the configuration of each of the above embodiments may be added to or substituted for the configuration of another of the above embodiments.
[0074] (6-2) In addition to the above-described phenolic resin, the present disclosure can also be realized in various forms, such as a composition containing the phenolic resin, a tire, a run-flat tire, a method for producing a phenolic resin, a method for producing a composition, a method for producing a tire, and a method for producing a run-flat tire.
Claims
1. A phenolic resin (excluding benzoxazine-type phenolic resins) synthesized from raw materials containing 100 parts by mass of phenols, 20 to 80 parts by mass of dodecanediamine, and 1 to 20 parts by mass of aldehydes, and having one or more structural units derived from dodecanediamine with a linear or branched carbon chain in the molecule.
2. The phenol resin according to claim 1, wherein the structural unit is derived from 1,12-dodecanediamine, and the softening point of the phenol resin is 70°C or higher and 150°C or lower.
Citation Information
Patent Citations
Resin composition comprising benzoxadine ring-containing thermosetting resin
JP2010053324A
Thermosetting resin comprising copolymer having benzoxazine ring
JP2010053325A
Rubber composition containing main chain benzoxazine and method for producing the same
JP2018524438A