Semiconductor catalyst, catalyst electrode, method for producing reduced product, and device for producing reduced product
The use of nitrogen-containing diamond particle catalysts in thin films addresses durability and light efficiency issues in hydrogen production, enabling effective hydrogen generation from visible light and expanding environmental applicability for clean energy production.
Patent Information
- Application Number
- PCT/JP2024/014429
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-02
- Filing Date
- 2024-04-09
- Publication Date
- 2024-10-24
AI Technical Summary
Existing semiconductor catalysts for hydrogen production, such as those using n-type gallium nitride and nickel oxide, face challenges in durability due to degradation issues and require ultraviolet light, which limits their efficiency and environmental applicability, especially since only a small percentage of ultraviolet rays reach the Earth's surface.
A semiconductor catalyst composed of a thin film with nitrogen-containing diamond particles, which are physically and chemically stable, allowing for efficient electron release under visible light irradiation and promoting reduction reactions, thereby enabling hydrogen production even in environments with limited ultraviolet light exposure.
The nitrogen-containing diamond particle catalyst exhibits excellent durability and enhances hydrogen production efficiency using visible light, making it suitable for various environments and improving the utilization of solar energy for clean energy generation while reducing carbon dioxide emissions.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Semiconductor catalyst, catalytic electrode, method for producing reduced product, and reduced product generating device
[0001] The present disclosure relates to a novel semiconductor catalyst, a method for producing a reduced product using the semiconductor catalyst, a reduced product generator for producing a reduced product using the semiconductor catalyst, a catalytic electrode for hydrogen generation including the semiconductor catalyst, a method for producing hydrogen using the catalytic electrode, and a hydrogen generator for producing hydrogen using the catalytic electrode. This application claims priority to Japanese Patent Application No. 2023-68141 filed in Japan on April 18, 2023, Japanese Patent Application No. 2023-91246 filed in Japan on June 1, 2023, and Japanese Patent Application No. 2023-91950 filed in Japan on June 2, 2023, the contents of which are incorporated herein by reference.
[0002] To prevent global warming, it is urgent to reduce emissions of greenhouse gases such as carbon dioxide. In this situation, there is a need to switch energy sources from fossil fuels such as coal and oil to non-fossil fuels. Hydrogen is attracting attention as a non-fossil fuel. This is because power generation using hydrogen as an energy source does not emit carbon dioxide, thereby reducing the environmental burden.
[0003] Hydrogen can be produced by steam reforming of fossil fuels such as coal and petroleum, but from the perspective of reducing the burden on the environment, a method of producing hydrogen by electrolyzing water has attracted attention, and studies are being conducted on the use of solar energy to electrolyze water.
[0004] Patent Document 1 discloses that hydrogen is generated when a semiconductor photoelectrode is obtained by laminating a honeycomb pattern of titanium and aluminum as a current collector layer on the surface of an n-type gallium nitride thin film, which is a semiconductor film, and then laminating a catalyst layer containing a metal oxide such as nickel oxide, and the resulting semiconductor photoelectrode is immersed in an aqueous sodium hydroxide solution and irradiated with light from the catalyst layer side.
[0005] Japanese Patent Application Laid-Open No. 2018-90887
[0006] Because n-type gallium nitride has a large band gap, it requires irradiation with ultraviolet light to be excited by light. However, since only 5-6% of sunlight reaching the Earth's surface contains ultraviolet light, it is difficult to efficiently utilize solar energy. Therefore, by providing a separate catalyst layer (e.g., a metal catalyst layer such as nickel oxide), the band gap can be reduced and visible light responsiveness can be achieved. However, metal catalyst layers such as n-type gallium nitride and nickel oxide are prone to deterioration due to elution, decomposition, corrosion, etc., which limits the environment in which they can be used.
[0007] Therefore, an object of the present disclosure is to provide a semiconductor catalyst having excellent durability and exhibiting the effect of promoting a reduction reaction when irradiated with visible light. Another object of the present disclosure is to provide a method for producing the semiconductor catalyst. Another object of the present disclosure is to provide a method for producing a reduced product, in which a reducible substance is reduced using the semiconductor catalyst to obtain a corresponding reduced product. Another object of the present disclosure is to provide a reduced product generation device using the semiconductor catalyst.
[0008] As a result of intensive research into solving the above problems, the present inventors have found the following: 1. A thin film containing nitrogen-containing diamond particles, which are extremely stable physically and chemically, is highly durable; 2. A semiconductor catalyst made of a thin film containing nitrogen-containing diamond particles in the plane and height directions has a donor level formed at a position close to the conduction band in the band gap of diamond, so that when irradiated with visible light, it easily transitions to an excited state, releases electrons, and exhibits a catalytic effect of promoting the reduction reaction of a substance to be reduced; 3. When a stack of the semiconductor catalyst and conductive member is used as a working electrode and irradiated with visible light while in contact with water together with a counter electrode, the reduction reaction of water proceeds efficiently and hydrogen is produced. The present disclosure has been completed based on these findings.
[0009] That is, the present disclosure provides a semiconductor catalyst comprising a thin film containing nitrogen-containing diamond particles in the planar and height directions.
[0010] The present disclosure also provides the semiconductor catalyst, wherein the thin film has a configuration in which nitrogen-containing diamond particles are arranged in a plane direction and a height direction, and adjacent diamond particles in the plane direction and the height direction are in close contact with each other.
[0011] The present disclosure also provides a method for manufacturing a thin film having a nitrogen atomic concentration of 10×10 18 atoms / cm 3 The semiconductor catalyst as described above is provided.
[0012] The present disclosure also provides the semiconductor catalyst, wherein the thickness of the thin film is 5 nm or more.
[0013] The present disclosure also provides the semiconductor catalyst, the surface of which has a negative electron affinity.
[0014] The present disclosure also provides the semiconductor catalyst, which is a visible light responsive catalyst.
[0015] The present disclosure also provides the semiconductor catalyst as a reduction catalyst.
[0016] The present disclosure also provides the semiconductor catalyst, which is a catalyst for producing hydrogen.
[0017] The present disclosure also provides a method for producing a semiconductor catalyst, which comprises carrying out the following step 1, and then carrying out the following step 2 at least once to obtain the semiconductor catalyst: Step 1: fixing nitrogen-containing diamond particles having a positive or negative charge, the nitrogen-containing diamond particles having a charge opposite to that of the substrate, on a substrate having a positive or negative charge; Step 2: stacking nitrogen-containing diamond particles having a positive or negative charge, the nitrogen-containing diamond particles having a charge opposite to that of the fixed nitrogen-containing diamond particles, on the fixed nitrogen-containing diamond particles.
[0018] The present disclosure also provides a method for producing a reduction product, which comprises reducing a reducible substance under irradiation with visible light and in the presence of the semiconductor catalyst to obtain the corresponding reduction product.
[0019] The present disclosure also provides a reduction product generating device including the semiconductor catalyst.
[0020] The present disclosure also provides a catalytic electrode for hydrogen generation, comprising a catalytic layer (1) and a conductive layer (2), wherein the catalytic layer (1) contains the semiconductor catalyst.
[0021] The present disclosure also provides the catalytic electrode for generating hydrogen, wherein the conductive layer (2) is a layer having a diamond crystal structure in which some of the carbon atoms are substituted with boron atoms.
[0022] The present disclosure also provides a method for manufacturing a conductive layer (2) having a boron atomic concentration of 1×10 19 atoms / cm 3 The present invention provides the above-described catalytic electrode for generating hydrogen.
[0023] The present disclosure also provides the catalytic electrode for generating hydrogen, wherein the thickness of the catalytic layer (1) is 1 nm to 100 μm, and the thickness of the conductive layer (2) is 1 μm or more.
[0024] The present disclosure also provides a method for producing hydrogen, which comprises reducing water using the catalytic electrode for hydrogen generation under visible light irradiation to produce hydrogen.
[0025] The present disclosure also provides a hydrogen generation device including a water electrolysis cell having a water container, the hydrogen generation catalytic electrode arranged to be in contact with the water in the container, and a counter electrode.
[0026] The semiconductor catalyst disclosed herein is formed from diamond particles, which are extremely physically and chemically stable, resulting in excellent durability and no environmental limitations. Furthermore, while diamond particles themselves have a large band gap and require ultraviolet irradiation for photoexcitation, the semiconductor catalyst disclosed herein uses nitrogen-containing diamond particles. The nitrogen-containing diamond particles form donor levels close to the conduction band. Therefore, the semiconductor catalyst can easily release electrons when irradiated with visible light or sunlight, thereby promoting reduction reactions. Because of the above properties, the semiconductor catalyst can be suitably used as a reduction catalyst or a visible-light-responsive catalyst. The semiconductor catalyst can also be suitably used as a catalyst for promoting the reaction of generating hydrogen from water (e.g., a hydrogen generation catalyst). Furthermore, a laminate obtained by stacking the semiconductor catalyst on a conductive material can be suitably used as a catalytic electrode in the reaction of electrolyzing water to generate hydrogen. Furthermore, using the semiconductor catalyst as an electrode allows for efficient use of inexhaustible solar energy to perform water electrolysis, thereby producing clean energy hydrogen while suppressing carbon dioxide generation.
[0027] 1 is a diagram showing the results of concentration analysis of boron atoms and nitrogen atoms of the laminate obtained in Example 1. FIG. 2 is a schematic diagram of an H-type cell used for measuring the amount of hydrogen produced using a catalytic electrode. FIG. 3 is a diagram showing the results of LSV measurement of the catalytic electrode obtained in Example 2.
[0028] [Semiconductor catalyst] The semiconductor catalyst of the present disclosure is made of a thin film containing nitrogen-containing diamond particles in the plane direction and height direction. The semiconductor catalyst contains nitrogen-containing diamond particles on the surface. Therefore, the semiconductor catalyst has a large surface area and can efficiently utilize solar energy to promote the reduction reaction.
[0029] The nitrogen-containing diamond particles contain carbon atoms and nitrogen atoms as atoms other than carbon atoms (i.e., heteroatoms), and have a structure in which some of the carbon atoms that make up the diamond crystal structure are substituted with nitrogen atoms.
[0030] The thin film includes the following structures: 1. A thin film in which nitrogen-containing diamond particles are arranged in the plane direction and the height direction, and diamond particles adjacent in the plane direction and the height direction are in close contact with each other. 2. A thin film in which nitrogen-containing diamond particles are dispersed in the plane direction and the height direction in a solid dispersion medium (e.g., resin, etc.).
[0031] As the thin film, the thin film having the structure 1 is preferable in particular, in that it has excellent durability and significantly improves the catalytic effect of the reduction reaction (i.e., the reaction in which a reducible substance is subjected to a reduction treatment to produce a corresponding reduced product), and in particular, a thin film is preferable in which nitrogen-containing diamond particles are arranged in the surface direction and height direction, and adjacent diamond particles in the surface direction and height direction are adhered to each other by Coulomb force and / or van der Waals force.
[0032] The thickness of the thin film is, for example, 1 nm or more and 100 μm or less. From the viewpoint of exhibiting sufficient electron emission ability, the lower limit of the thickness is preferably 3 nm, more preferably 5 nm, even more preferably 10 nm, even more preferably 15 nm, even more preferably 30 nm, even more preferably 40 nm, particularly preferably 45 nm, most preferably 50 nm, and particularly preferably 60 nm. From the viewpoint of suppressing electrical resistance, the upper limit of the thickness is preferably 10 μm, particularly preferably 1 μm, and most preferably 100 nm. If the thickness of the thin film is below the above range, the efficiency of use of visible light for electron excitation decreases, and the electron emission ability tends to be insufficient. On the other hand, if the thickness of the thin film exceeds the above range, the amount of electron excitation by visible light irradiation saturates, and the electrical resistance increases, which tends to reduce the reducing ability.
[0033] The nitrogen atom concentration of the thin film is, for example, 5×10 18 atoms / cm 3 or more, preferably 1×10 19 atoms / cm 3 More preferably, 5×10 19 atoms / cm 3 More preferably, 1×10 20 atoms / cm 3 The upper limit of the nitrogen atom concentration is, for example, 5×1022 atoms / cm 3 , preferably 1 × 10 22 atoms / cm 3 , particularly preferably 5 × 10 21 atoms / cm 3 , most preferably 4×10 21 atoms / cm 3 Since the thin film contains nitrogen atoms in the above range, it has visible light responsiveness, and electrons are easily excited and emitted when irradiated with visible light. If the nitrogen atom concentration is below the above range, the electron emission ability tends to be insufficient. On the other hand, if the nitrogen atom concentration is above the above range, the diamond crystal structure tends to collapse, and the electron emission performance tends to decrease.
[0034] The nitrogen atomic concentration of the thin film may be uniform or may be graded from the center to the surface. When the nitrogen atomic concentration of the thin film increases from the center to the surface, the electron emission ability tends to be further improved. The surface of the thin film refers to, for example, the portion of the thin film from the surface (depth 0) to a depth of 150 nm.
[0035] The nitrogen atom concentration in the surface layer of the thin film is, for example, 1×10 19 atoms / cm 3 or more, preferably 5 × 10 19 atoms / cm 3 More preferably, 1×10 20 atoms / cm 3 More preferably, 2 × 10 20 atoms / cm 3 More preferably, 3×10 20 atoms / cm 3 or more, most preferably 4 x 10 20 atoms / cm 3 The upper limit of the nitrogen atom concentration is, for example, 5×10 22 atoms / cm 3 , preferably 1 × 10 21 atoms / cm 3 , more preferably 5×10 21 atoms / cm 3 is.
[0036] The thin film has a nitrogen atom concentration of 1×10 19 atoms / cm 3 The thickness of the portion having a thickness of 5 nm or more (for example, 5 to 150 nm, preferably 5 to 100 nm, particularly preferably 5 to 50 nm) is preferably 10 nm or more, more preferably 15 nm or more, particularly preferably 20 nm or more, most preferably 25 nm or more, and particularly preferably 30 nm or more.
[0037] The thin film may contain heteroatoms other than nitrogen atoms, such as boron atoms.
[0038] When the thin film contains boron atoms, the concentration of boron atoms is, for example, 1×10 13 atoms / cm 3 or more, preferably 1×10 14 atoms / cm 3 or more, more preferably 1×10 15 atoms / cm 3 More preferably, 1×10 16 atoms / cm 3 More preferably, 1×10 17 atoms / cm 3 More preferably, 1×10 18 atoms / cm 3 More preferably, 1×10 19 atoms / cm 3 More preferably, 5×10 19 atoms / cm 3 More preferably, 3×10 20 atoms / cm 3 or more, most preferably 5 × 10 20 atoms / cm 3 More preferably, 1×10 21 atoms / cm 3 The upper limit of the boron atom concentration is, for example, 5×10 22 atoms / cm 3 , preferably 3 × 10 22 atoms / cm 3 , particularly preferably 1 × 10 22 atoms / cm3 is.
[0039] The thin film may contain other heteroatoms in addition to boron atoms and nitrogen atoms, but the concentration of the other heteroatoms should not exceed 5×10 21 atoms / cm 3 It is preferable that the number of electrons emitted is 5×10 or less in terms of high electron emission ability, and more preferably 5×10 20 atoms / cm 3 More preferably, 5 × 10 19 atoms / cm 3 More preferably, 5 × 10 18 atoms / cm 3 Below, particularly preferably 1 × 10 18 atoms / cm 3 Below, most preferably 1 × 10 17 atoms / cm 3 Below, particularly preferably 1 × 10 16 atoms / cm 3 The following is the result.
[0040] The heteroatom contents (nitrogen atom content and boron atom content) in the thin film and the thickness of the thin film can be determined by secondary ion mass spectrometry (SIMS) or the like.
[0041] The surface roughness Rms (root mean square roughness) of the thin film is, from the viewpoint of increasing the specific surface area, for example, 1 nm or more, preferably 5 nm or more, particularly preferably 10 nm or more. The upper limit of the surface roughness Rms is, for example, 100 nm, preferably 80 nm, particularly preferably 50 nm, and most preferably 30 nm.
[0042] Furthermore, the surface layer of the thin film is preferably hydrogen-terminated, which gives the surface of the thin film a negative electron affinity, making it easier to release electrons from the surface of the thin film, and significantly improving the catalytic effect of the reduction reaction.
[0043] The thin film may contain other components in addition to the nitrogen-containing diamond particles and resin, such as components derived from the substrate used in the manufacturing process (e.g., silicon compounds such as silicon carbide).
[0044] The semiconductor catalyst is substantially composed of only the thin film. When the semiconductor catalyst contains components other than the thin film, the content of the components other than the thin film is, for example, 10% by weight or less, preferably 5% by weight or less, more preferably 3% by weight or less, particularly preferably 1% by weight or less, most preferably 0.5% by weight or less, and particularly preferably 0.1% by weight or less, based on the total amount of the semiconductor catalyst.
[0045] As described above, the semiconductor catalyst has the function of releasing electrons when irradiated with visible light, and therefore can be suitably used as a visible light-responsive catalyst. As will be described in detail later, the use of the semiconductor catalyst makes it possible to reduce a reducible substance under visible light irradiation to obtain a corresponding reduced product. For example, when HO is used as the reducible substance, hydrogen can be produced as the corresponding reduced product. Therefore, the semiconductor catalyst can be suitably used as a reduction catalyst or a hydrogen production catalyst.
[0046] [Method for Producing Semiconductor Catalyst] The semiconductor catalyst (or the thin film) can be produced, for example, through the following steps: Step 1: Fixing nitrogen-containing diamond particles on a substrate; and Step 2: Removing the substrate.
[0047] (Step 1) Step 1 is a step of fixing nitrogen-containing diamond particles on a substrate.
[0048] In the present disclosure, "nitrogen-containing diamond particles" refer to diamond particles containing nitrogen atoms, and there are no restrictions on the portion containing the nitrogen atoms. The diamond particles are composed of a core portion made of sp3 carbon and a shell portion made of sp2 carbon, and the nitrogen atoms may be contained in the core portion or the shell portion. Furthermore, they may be contained in the boundary between the core portion and the shell portion.
[0049] The shape of the nitrogen-containing diamond particles is not particularly limited, and examples include spherical (perfect spherical, nearly perfect spherical, ellipsoidal, etc.), polyhedral, rod-shaped (cylindrical, prismatic, etc.), plate-shaped, flaky, irregular, etc.
[0050] The average particle size of the nitrogen-containing diamond particles is, for example, 1 nm to 100 μm. The upper limit of the average particle size is preferably 10 μm, more preferably 1 μm, particularly preferably 100 nm, most preferably 50 nm, and particularly preferably 20 nm. If the average particle size is below the above range, when removing the substrate in step 2, the nitrogen-containing diamond particles may be removed together with the substrate, making it difficult to form a thin film. On the other hand, if the average particle size exceeds the above range, the obtained thin film tends to be thick, the electrical resistance increases, and the reducibility tends to decrease. The average particle size is the median diameter (d50) measured by laser diffraction and scattering method.
[0051] Nitrogen-containing diamond particles can be obtained, for example, by adding a nitrogen source to the raw material when producing nanodiamond particles using a detonation method, by obtaining a growth film containing nitrogen-doped diamond obtained by a CVD method and then pulverizing the obtained growth film, or by doping undoped nanodiamond particles with nitrogen atoms using an ion implantation method.
[0052] There are no particular limitations on the method for fixing nitrogen-containing diamond particles onto a substrate, but one example is a method in which a paint containing nitrogen-containing diamond particles is applied to the substrate and dried to fix the nitrogen-containing diamond particles onto the substrate.
[0053] The coating material contains a solvent together with nitrogen-containing diamond particles. Examples of the solvent include water; alcohols such as ethanol and propanol; hydrocarbons such as toluene; cyclic ethers such as tetrahydrofuran; ketones such as methyl isobutyl ketone. These can be used alone or in combination of two or more. Among them, water and / or alcohol are preferred as the solvent because they have excellent dispersibility of nitrogen-containing nanodiamond particles.
[0054] The coating material may further contain a thickener, a dispersant, a buffering agent, and the like.
[0055] The content of the nitrogen-containing diamond particles in the coating material is, for example, 0.001 to 5.0% by weight, preferably 0.1 to 1.0% by weight.
[0056] Examples of the substrate include silicon substrates, quartz substrates, ceramic substrates, glass substrates, metal substrates (e.g., aluminum substrates, copper substrates, iron substrates, stainless steel substrates, brass substrates, etc.), plastic substrates (e.g., polyimide substrates, polyamide substrates, etc.), etc. Among these, silicon substrates are preferred because of their excellent heat resistance, mass productivity, thermal shock resistance, etc.
[0057] The surface of the substrate may be subjected to ultrasonic cleaning using acetone, ethanol, pure water, etc. Furthermore, it may be subjected to acid cleaning using hydrochloric acid, hydrofluoric acid, etc. Furthermore, fine irregularities may be formed on the surface of the substrate.
[0058] The coating material can be applied by, for example, a printing method, a coating method, etc. Specific examples include screen printing, mask printing, offset printing, inkjet printing, flexographic printing, gravure printing, spin coating, stamping, dispensing, squeegee printing, silk screen printing, spraying, brush coating, etc.
[0059] The coating of the coating material may be carried out only once or may be repeated multiple times. In particular, it is preferable to repeatedly apply the coating material multiple times to form a coating film of appropriate thickness, as this improves the electron emission ability and is particularly effective in promoting the reduction reaction of the reducible substance. The number of applications is preferably, for example, 2 or more, more preferably 5 or more, particularly preferably 8 or more, and most preferably 10 or more. The upper limit of the number of applications is, for example, 20, preferably 15.
[0060] The thickness of the coating film is, for example, 1 nm or more and 100 μm or less, and from the viewpoint of improving the electron emission ability and being excellent in the effect of promoting the reduction reaction of the reducible substance, the lower limit of the thickness is preferably 3 nm, more preferably 10 nm, particularly preferably 30 nm, most preferably 50 nm, and particularly preferably 70 nm. The upper limit of the thickness is preferably 10 μm, particularly preferably 1 μm, and most preferably 100 nm, from the viewpoint of suppressing an increase in electrical resistance.
[0061] When the coating of the coating material is repeated multiple times, the following method A or method B can be employed. Method A: A method of repeatedly applying a coating material containing nitrogen-containing diamond particles having a positive or negative charge, the nitrogen-containing diamond particles having a charge opposite to that of the substrate, onto a substrate having a positive or negative charge, and drying the coating material multiple times. Method B: A method of performing the following step I once, and then performing the following step II at least once. Step I: A step of applying a coating material containing nitrogen-containing diamond particles having a positive or negative charge, the nitrogen-containing diamond particles having a charge opposite to that of the substrate, onto a substrate having a positive or negative charge, to fix the diamond particles onto the substrate. Step II: A step of applying a coating material containing nitrogen-containing diamond particles having a positive or negative charge, the nitrogen-containing diamond particles having a charge opposite to that of the fixed nitrogen-containing diamond particles, onto the fixed nitrogen-containing diamond particles, to stack the nitrogen-containing diamond particles having the opposite charge on the fixed nitrogen-containing diamond particles.
[0062] In the step I, when the coating material containing nitrogen-containing diamond particles having the opposite charge to that of the substrate is applied onto the substrate, the nitrogen-containing diamond particles in the coating material migrate toward the substrate due to Coulomb force. Then, when the nitrogen-containing diamond particles approach the substrate, the van der Waals force is added to the Coulomb force, and the nitrogen-containing diamond particles are adsorbed and fixed on the substrate.
[0063] In addition, in step II, the nitrogen-containing diamond particles in the aqueous dispersion migrate toward the fixed nitrogen-containing diamond particles due to Coulomb force, and when they approach each other, they are adsorbed and fixed by the addition of van der Waals force to the Coulomb force.
[0064] The larger the amplitude of the zeta potential of the fixed nitrogen-containing diamond particles and the zeta potential of the nitrogen-containing diamond particles having an opposite charge to that of the nitrogen-containing diamond particles, the larger the Coulomb force and van der Waals force that are generated, which is preferable in that the nitrogen-containing diamond particle layer can be stacked uniformly and densely.
[0065] Said amplitude is represented by the sum of the absolute value of the zeta potential of said fixed nitrogen-containing diamond particle and the absolute value of the zeta potential of the nitrogen-containing diamond particle that has the opposite charge to the charge of said nitrogen-containing diamond particle, and is for example 40mV or more, preferably 50mV or more, more preferably 60mV or more, particularly preferably 65mV or more, most preferably 70mV or more, particularly preferably 80mV or more.The upper limit of the sum of the absolute value of said zeta potential is for example 120mV.
[0066] Before carrying out the step II, the substrate coated with the coating material containing nitrogen-containing diamond particles may be washed with water, etc. By washing, excess coating material is removed, so that a thin film with a uniform thickness (preferably a thin film with a uniform thickness and in-plane uniformity) can be formed.
[0067] Through this process, a thin film containing nitrogen-containing diamond particles in the planar and vertical directions can be formed on the surface of the substrate.
[0068] (Step 2) Step 2 is a step of removing the substrate from the substrate provided with the thin film obtained through step 1.
[0069] The method for removing the substrate can be appropriately selected depending on the type of substrate. For example, when a silicon substrate is used as the substrate, a method of dissolving and removing the substrate with a mixture of hydrofluoric acid and nitric acid can be selected.
[0070] Through this process, a thin film containing nitrogen-containing diamond particles in the plane and height directions (preferably a thin film containing nitrogen-containing diamond particles uniformly in the plane and height directions) is obtained.
[0071] The thin film containing nitrogen-containing diamond particles in the plane and height directions obtained by removing the substrate through this step may then be subjected to the following step 3. Step 3: A step of performing a hydrogenation treatment and / or an sp2 carbon removal treatment
[0072] The treatment can be carried out by, for example, irradiating the thin film with hydrogen plasma.
[0073] By irradiating hydrogen plasma onto the thin film, obtain a thin film that contains nitrogen-containing diamond particles in the plane direction and height direction, and the nitrogen-containing diamond particles contained in the thin film are bonded to each other adjacently, and the bond existing on the surface of the thin film is hydrogen-terminated.Furthermore, obtain a thin film that contains nitrogen-containing diamond particles in the plane direction and height direction, and the sp2 carbon is removed.
[0074] The above method uses nitrogen-containing diamond particles, which allows the nitrogen atom concentration to be increased without damaging the diamond crystal structure, resulting in a thin film (or thin-film catalyst) that combines the electron emission ability derived from the diamond crystal structure with good visible light response.
[0075] [Method for Producing a Reduced Product] The method for producing a reduced product according to the present disclosure is a method for reducing a reducible substance under irradiation with visible light and in the presence of the catalyst (or the thin film) to obtain the corresponding reduced product.
[0076] The reduction reaction is preferably carried out in an aqueous electrolyte. When the reduction reaction is carried out in an aqueous electrolyte, electrons released from the catalyst react with water to form hydrated electrons (e aq - The formed hydrated electrons can exist stably in the aqueous electrolyte solution, and can reduce the reducible substance in the aqueous electrolyte solution to efficiently produce the corresponding reduced product.
[0077] The aqueous electrolyte solution is an electrolyte solution containing water as a solvent. Examples of electrolytes contained in the aqueous electrolyte solution include potassium chloride, sodium chloride, lithium chloride, potassium hydroxide, sodium hydroxide, lithium hydroxide, potassium sulfate, sodium sulfate, zinc sulfate, zinc nitrate, zinc phosphate, zinc acetate, iron hydroxide, and manganese chloride. These may be used alone or in combination of two or more.
[0078] The reduction reaction includes the following modes: [1] The reducible substance only receives electrons from hydrated electrons (decomposition reaction is not included); [2] The reducible substance receives electrons from hydrated electrons and decomposes; [3] The hydrated electrons react with water molecules to generate hydrogen radicals, and the generated hydrogen radicals reduce the reducible substance.
[0079] Examples of the reducible substance include HO, CO, O, N, NO, NO, pollutants (e.g., organic or inorganic compounds), organic fluorine compounds (or fluorinated hydrocarbons), metal ions, and metal complex ions.
[0080] The reducible substances and the corresponding reduction products are shown below.
[0081] en: ethylenediamine
[0082] The method for reducing the reducible substance may be any method in which electrons released from a catalyst under visible light irradiation react with the reducible substance. Among these, from the viewpoint of efficiently bringing the electrons released from the catalyst into contact with the reducible substance, it is preferable to use an electrolytic cell having the catalyst on the electrode and to carry out the electrolysis reaction in a state in which the reducible substance is contained in an electrolyte. The method for containing the reducible substance in the electrolyte can be appropriately performed depending on the type of the reducible substance. For example, when the reducible substance is a liquid or solid, it can be dissolved or dispersed in the electrolyte. When the reducible substance is a gas, it can be bubbling in the electrolyte.
[0083] For example, when H2O is used as the substance to be reduced, hydrogen is generated as the corresponding reduction product, and therefore the catalytic electrode can be used as a catalytic electrode for generating hydrogen.
[0084] The catalyst is responsive to visible light (light having a wavelength of more than 400 nm and less than 830 nm), so the reduction reaction can be promoted using sunlight. Furthermore, the reduction reaction can be promoted even in an environment with low levels of ultraviolet light, such as indoor spaces.
[0085] [Catalytic Electrode] The catalytic electrode of the present disclosure includes a catalytic layer (1) and a conductive layer (2), and the catalytic layer (1) includes the semiconductor catalyst (or the thin film).
[0086] The catalytic electrode can be used as an electrode (for example, a cathode) in a reaction in which a reducible substance is reduced by electrical energy to obtain a corresponding reduced product.
[0087] (Catalyst Layer (1)) The catalyst layer (1) contains the semiconductor catalyst (that is, a thin film containing nitrogen-containing diamond particles in the planar and vertical directions).
[0088] The thickness of the catalyst layer (1) is, for example, 1 nm or more and 100 μm or less. From the viewpoint of exhibiting sufficient electron emission ability, the lower limit of the thickness is preferably 3 nm, more preferably 5 nm, even more preferably 10 nm, even more preferably 15 nm, even more preferably 30 nm, and even more preferably 35 nm. From the viewpoint of suppressing electrical resistance, the upper limit of the thickness is preferably 10 μm, particularly preferably 1 μm, most preferably 100 nm, and particularly preferably 50 nm. If the thickness of the catalyst layer (1) is below the above range, the efficiency of use of visible light for electron excitation decreases, and the electron emission ability tends to be insufficient. On the other hand, if the thickness of the catalyst layer (1) exceeds the above range, the amount of electron excitation by visible light irradiation saturates, and the electrical resistance increases, so the reducing ability tends to decrease.
[0089] (Conductive Layer (2)) The conductive layer (2) is a layer containing a conductive member.
[0090] The conductive material constituting the conductive member is not particularly limited, and examples thereof include metals such as platinum, titanium, tantalum, nickel, copper, and aluminum; carbon materials (e.g., conductive diamonds such as boron-doped diamond, graphene, carbon nanotubes, carbon black, and graphite); and semiconductors such as silicon compounds (e.g., silicon carbide). These may be used alone or in combination of two or more.
[0091] Of the conductive materials, carbon materials are preferred because they are inexpensive, have high mechanical strength and excellent durability, and have a small linear expansion coefficient. Conductive diamond is particularly preferred, and boron-doped diamond is most preferred.
[0092] Therefore, the conductive layer (2) is preferably a layer having a diamond crystal structure in which some of the carbon atoms are substituted with boron atoms (hereinafter, this may be referred to as "conductive layer (2-1)").
[0093] The conductive layer (2-1) contains carbon atoms and boron atoms as heteroatoms, and the boron atom concentration is, for example, 1×10 19 atoms / cm 3 or more, preferably 5 × 10 19 atoms / cm 3 More preferably, 3×10 20 atoms / cm 3 More preferably, 1×10 21 atoms / cm 3 The upper limit of the boron atom concentration is, for example, 5×10 22 atoms / cm 3 , preferably 3 × 10 22 atoms / cm 3 , particularly preferably 1 × 10 22 atoms / cm 3 , most preferably 5×10 21 atoms / cm 3 , particularly preferably 3×10 21 atoms / cm 3 When the conductive layer (2-1) contains boron atoms in the above range, it has excellent conductivity. When the boron atom concentration of the conductive layer (2-1) is below the above range, the conductivity tends to be insufficient. On the other hand, when the boron atom concentration of the conductive layer (2-1) is above the above range, the diamond crystal structure tends to be easily broken.
[0094] The conductive layer (2-1) may contain heteroatoms other than boron atoms, but the concentration of heteroatoms other than boron atoms is, for example, 5×10 21 atoms / cm 3From the viewpoint of providing high conductivity, it is preferable that the 20 atoms / cm 3 More preferably, 5 × 10 19 atoms / cm 3 More preferably, 1×10 19 atoms / cm 3 Below, particularly preferably 1 × 10 18 atoms / cm 3 Below, most preferably 1 × 10 17 atoms / cm 3 Below, particularly preferably 1 × 10 16 atoms / cm 3 The following is the result.
[0095] When the conductive layer (2-1) contains nitrogen atoms, the nitrogen atom concentration is, for example, 5×10 20 atoms / cm 3 It is preferably equal to or less than 1×10 20 atoms / cm 3 More preferably, 1×10 19 atoms / cm 3 More preferably, 5 × 10 18 atoms / cm 3 less than 1×10 18 atoms / cm 3 Below, particularly preferably 1 × 10 17 atoms / cm 3 The lower limit of the nitrogen atom concentration is, for example, 1×10 16 atoms / cm 3 is.
[0096] The thickness of the conductive layer (2) (total thickness when it is composed of multiple layers) is not particularly limited, but is, for example, 1 μm or more, preferably 50 μm or more, and particularly preferably 100 μm or more. A thickness of 100 μm or more of the conductive layer (2) is preferable in that it has sufficient strength to be formed into a free-standing film and is easy to handle. The upper limit of the thickness is, for example, 1 mm, and from the viewpoint of suppressing an increase in electrical resistance, it is preferably 500 μm, particularly preferably 300 μm, most preferably 250 μm, and particularly preferably 200 μm.
[0097] (Other Layers) The catalytic electrode may include components other than the catalytic layer (1) and the conductive layer (2).
[0098] The proportion of the total weight of the catalyst layer (1) and the conductive layer (2) in the total amount of the catalyst electrode (100 wt%) is, for example, 60 wt% or more, preferably 70 wt% or more, more preferably 80 wt% or more, particularly preferably 90 wt% or more, and most preferably 95 wt% or more. The upper limit is 100 wt%. In other words, the catalyst electrode may be composed of only the catalyst layer (1) and the conductive layer (2).
[0099] The thickness of the catalytic electrode is, for example, 1001 nm or more, preferably 1010 nm or more, particularly preferably 1050 nm or more. The upper limit of the thickness is, for example, 1 mm, preferably 500 μm, particularly preferably 300 μm, and most preferably 200 μm.
[0100] When the catalytic electrode and a counter electrode are placed in a container that contains a reducible substance so as to be in contact with the reducible substance and visible light is irradiated onto the catalytic electrode, the reducible substance (e.g., HO) can be efficiently electrolyzed and reduced to produce a corresponding reduced product (H when the reducible substance is HO).
[0101] That is, by using the catalytic electrode, solar energy can be converted into electrical energy, and by using this electrical energy to reduce a reducible substance (for example, HO), it is possible to produce a corresponding reduced product (H, which is useful as clean energy when the reducible substance is HO) while suppressing carbon dioxide emissions.
[0102] [Method for Manufacturing Catalyst Electrode] The catalyst electrode can be manufactured by laminating a catalyst layer (1) containing the catalyst and a conductive layer (2).
[0103] The catalytic electrode can be manufactured by fixing nitrogen-containing diamond particles on a conductive substrate to form a catalytic layer (1).
[0104] There are no particular restrictions on the conductive substrate as long as it is a substrate made of a conductive material, but among them, a conductive diamond substrate is particularly preferred because it is inexpensive, has high mechanical strength and excellent durability, and has a small linear expansion coefficient, and a conductive substrate having a boron-doped diamond crystal structure is most preferred.
[0105] Among the catalytic electrodes, a catalytic electrode in which the conductive layer (2) is a conductive layer (2-1) having a boron-doped diamond crystal structure can be manufactured, for example, through the following steps (Method 1): Step A: A step of fixing nitrogen-containing diamond particles on a substrate to form a catalytic layer (1); Step B: A step of forming a conductive layer (2-1) having a boron-doped diamond crystal structure on the catalytic layer (1) by a vapor phase growth method.
[0106] The following steps may be carried out after the step B: Step C: A step of removing the substrate to obtain a laminate of the catalyst layer (1) and the conductive layer (2-1); and Step D: A step of subjecting the surface of the catalyst layer (1) of the obtained laminate to a hydrogenation treatment and / or sp2 carbon removal treatment.
[0107] The steps A, C, and D are the same as steps 1, 2, and 3, respectively, in the method for producing the catalyst.
[0108] The step A may be, for example, a step of forming a catalyst layer (1) by carrying out the following step 1 and then carrying out the following step 2 at least once: Step 1: A step of fixing nitrogen-containing diamond particles having a positive or negative charge, the nitrogen-containing diamond particles having a charge opposite to that of the substrate, on a substrate having a positive or negative charge; Step 2: A step of stacking nitrogen-containing diamond particles having a positive or negative charge, the nitrogen-containing diamond particles having a charge opposite to that of the fixed nitrogen-containing diamond particles, on the fixed nitrogen-containing diamond particles.
[0109] Step A may also be a process of repeatedly applying a coating material containing nitrogen-containing diamond particles having a positive or negative charge, the nitrogen-containing diamond particles having a charge opposite to that of the substrate, to a substrate having a positive or negative charge, and drying the coating material.
[0110] (Step B) Step B is a step of forming boron-doped diamond crystal structure (=the growth film having boron-doped diamond crystal structure) by vapor phase epitaxy on the surface of the catalyst layer (1) of the substrate / catalyst layer (1) laminate obtained through step A.
[0111] Vapor phase growth methods (CVD methods) include microwave plasma CVD methods, plasma CVD methods, hot filament CVD methods, photo CVD methods, etc. Among these, microwave plasma CVD methods are preferred because they can rapidly form a diamond crystal structure with excellent crystallinity.
[0112] The microwave plasma CVD method is a method for growing a boron-doped diamond crystal structure by introducing microwaves into a plasma generation chamber, decomposing a carbon source and a boron source to form plasma, and introducing this onto a substrate heated to 300 to 900° C. The boron atom content in the resulting diamond crystal structure can be controlled by adjusting the amount of boron source added to the carbon source.
[0113] Examples of the carbon source include hydrocarbons such as methane, ethane, propane, ethylene, and acetylene; alcohols such as methanol and ethanol; and ketones such as acetone. These may be used alone or in combination of two or more.
[0114] As the boron source, for example, diborane, trimethylboron, trimethoxyborane, boron oxide, etc. can be used.
[0115] Through this step, a laminate of substrate / catalyst layer (1) / conductive layer (2-1) is obtained.
[0116] The catalytic electrode can also be manufactured through the following steps (Method 2): Step A': Forming a conductive layer (2-1) having a boron-doped diamond crystal structure on a substrate by vapor deposition; Step B': Fixing nitrogen-containing diamond particles on the conductive layer (2-1) to form a catalytic layer (1).
[0117] The following steps may be carried out after the step B': Step C: A step of removing the substrate to obtain a laminate of the catalyst layer (1) and the conductive layer (2-1); and Step D: A step of subjecting the surface of the catalyst layer (1) of the obtained laminate to a hydrogenation treatment and / or sp2 carbon removal treatment.
[0118] Step A' can be carried out in the same manner as step B above, except that instead of forming the boron-doped diamond crystal structure on a substrate having nitrogen-containing diamond particles fixed to its surface, the boron-doped diamond crystal structure is formed on a substrate having seed crystals (e.g., nitrogen-free diamond particles) fixed to its surface.
[0119] Step B' can be carried out in the same manner as step A above, except that instead of applying a coating material containing nitrogen-containing diamond particles onto a substrate, a coating material containing nitrogen-containing diamond particles is applied onto the boron-doped diamond crystal structure obtained in step A'.
[0120] The catalytic electrode can also be manufactured through the following steps (Method 3): Step A": A step of fixing nitrogen-containing diamond particles on a conductive substrate having a boron-doped diamond crystal structure to form a catalytic layer (1); Step D': A step of performing sp2 carbon removal treatment on the surface of the catalytic layer (1) of the obtained laminate.
[0121] Step A" can be carried out in the same manner as above-mentioned step A, except that the paint containing nitrogen-containing diamond particles is applied onto the conductive substrate having boron-doped diamond crystal structure.In addition, as the conductive substrate having boron-doped diamond crystal structure, a conductive layer having boron-doped diamond crystal structure can be formed on a substrate by the same method as above-mentioned step A', and then the substrate can be removed, or a commercially available product can be used.
[0122] The step A" is, for example, a step of forming a catalyst layer (1) by carrying out the following step 1' and then carrying out the following step 2 at least once. Step 1': A step of fixing nitrogen-containing diamond particles having a positive or negative charge, the nitrogen-containing diamond particles having a charge opposite to that of the substrate, to a conductive substrate having a boron-doped diamond crystal structure. Step 2: A step of stacking nitrogen-containing diamond particles having a positive or negative charge, the nitrogen-containing diamond particles having a charge opposite to that of the fixed nitrogen-containing diamond particles, on the fixed nitrogen-containing diamond particles.
[0123] The step A" may also be a step of repeatedly applying a coating material containing nitrogen-containing diamond particles having a positive or negative charge, the nitrogen-containing diamond particles having a charge opposite to that of the substrate, to a substrate having a positive or negative charge, and drying the coating material.
[0124] As the conductive substrate with boron-doped diamond crystal structure, for example, can be used the growth film that contains boron-doped diamond formed by CVD method or the growth film that has been subjected to surface treatment.The growth film that is formed by CVD method has the boron-doped diamond crystal structure that is hydrogen-terminated, so it has positive charge.In addition, when the surface of the growth film that is formed by CVD method is subjected to acid treatment, the surface of the growth film is oxygen-terminated, and has negative charge.
[0125] Step D' is a step of carrying out sp2 carbon removal treatment on the catalyst layer (1) obtained through step A. This treatment can be carried out, for example, by irradiating the obtained catalyst layer (1) with hydrogen plasma. By carrying out this treatment, dangling bonds are generated on the surface of the catalyst layer (1), and the nitrogen-containing diamond particles are bonded to each other using the generated dangling bonds as starting points, and further the nitrogen-containing diamond particles are bonded to the conductive substrate. As a result, the nitrogen-containing diamond particles are firmly adhered to the conductive substrate, and are given the strength that can withstand use as an electrode.
[0126] According to Method 3, a catalyst layer (1) / conductive layer (2-1) laminate can be obtained without the step of removing the substrate, and damage that would occur in the step of removing the substrate can be avoided.
[0127] The conductive substrate used in method 3 can be any shape that can be coated with a coating material containing nitrogen-containing diamond particles, and the shape can be freely selected according to the application and design.In addition, the conductive substrate may have irregularities or may be curved.On the other hand, in method 1 and method 2, when forming the conductive layer (2-1) having a boron-doped diamond crystal structure by vapor phase epitaxy, it is important to maintain the surface temperature of the substrate uniform in order to form the conductive layer (2-1) with a uniform thickness.Therefore, it is preferable to use a substrate with a smooth surface and a uniform thickness.
[0128] Furthermore, in Method 3, instead of the conductive substrate having a boron-doped diamond crystal structure, a substrate made of a conductive material can be used without particular restrictions.
[0129] [Reduction Product Generator] The reduction product generator of the present disclosure is a device including a means for reducing a reducible substance in the presence of the catalyst to generate a corresponding reduction product. The reduction product generator includes at least the catalyst.
[0130] The device preferably includes a reaction section (i.e., a section where a reduction reaction takes place) in which the catalyst is disposed. The device may also include a supply section that supplies a substance to be reduced to the reaction section, a visible light irradiation section, a recovery section that recovers the generated reduction product, and the like.
[0131] From the viewpoint of efficiently bringing the electrons released from the catalyst by irradiation with visible light into contact with the reducible substance, the device is preferably an electrolysis cell in which the reaction section is provided with a storage section that stores the reducible substance and an electrolyte solution, an electrode containing the catalyst (= a catalyst electrode including a catalyst layer (1) containing the catalyst and a conductive layer (2)) and a counter electrode that are arranged so as to be in contact with the reducible substance and the electrolyte solution in the storage section.
[0132] The electrolytic solution is preferably an aqueous electrolytic solution containing water as a solvent. Examples of the electrolyte contained in the electrolytic solution include potassium chloride, sodium chloride, lithium chloride, potassium hydroxide, sodium hydroxide, lithium hydroxide, potassium sulfate, sodium sulfate, zinc sulfate, zinc nitrate, zinc phosphate, zinc acetate, iron hydroxide, and manganese chloride. These may be used alone or in combination of two or more.
[0133] When the substance to be reduced is water, the device is a hydrogen generation device, and includes, for example, an electrolysis cell (=water electrolysis cell) including a storage section that stores water (preferably water containing an electrolyte), an electrode containing the catalyst (=catalytic electrode including a catalyst layer (1) containing the catalyst and a conductive layer (2)) that is arranged so as to be in contact with the water in the storage section, and a counter electrode (for example, a platinum electrode, etc.).
[0134] The electrolytic cell may further include a separator and a power source for applying an external voltage.
[0135] By using the device, solar energy can be efficiently converted into electrical energy, and this electrical energy can be used to reduce a reducible substance (for example, HO). Therefore, it is possible to produce the corresponding reduced product (when the reducible substance is HO, H, which is useful as clean energy), while suppressing carbon dioxide emissions.
[0136] When HO is reduced using the electrolytic reaction apparatus under visible light irradiation by the method described in the Examples, the amount of H produced is, for example, 0.1 ppm or more (e.g., 0.1 to 5 ppm), preferably 0.5 ppm or more, particularly preferably 1 ppm or more, and most preferably 1.5 ppm or more.
[0137] When H2O is reduced using the electrolytic reaction device under visible light irradiation by the method described in the Examples, the faradaic efficiency of H2 generation is, for example, 10% or more, preferably 15% or more, particularly preferably 20% or more, and most preferably 40% or more.
[0138] When HO was reduced using the electrolytic reaction device under visible light irradiation according to the method described in the Examples, the total reduction current density was, for example, 1.0 × 10 -2mA / cm 2 or more, preferably 2.5 × 10 -2 mA / cm 2 More preferably, 5.0 × 10 -2 mA / cm 2 or more, most preferably 10.0 x 10 -2 mA / cm 2 More preferably, 15.0 × 10 -2 mA / cm 2 That's all.
[0139] The above-described configurations and combinations thereof of the present disclosure are merely examples, and additions, omissions, substitutions, and modifications of the configurations can be made as appropriate without departing from the spirit of the present disclosure.
[0140] The present disclosure will be described in more detail below using examples, but the present disclosure is not limited to these examples and is limited only by the claims.
[0141] Example 1 (Formation of catalyst layer (1)) A SiO2 / Si substrate was used as the substrate. The SiO2 / Si substrate was a laminate of SiO2 (thickness 100 nm) with a diameter of 8 mm and n-type Si (thickness 0.45 mm). The SiO2 / Si substrate was subjected to ultrasonic cleaning treatment with acetone, ethanol, and pure water, and acid cleaning treatment.
[0142] A suspension of nitrogen-containing ζ+ nanodiamond particles (particle diameter D50: 5 nm) (N-ζ+ nD particle concentration: 1.0%, solvent: water, zeta potential: +50 mV) was applied to the treated SiO2 / Si substrate, the substrate surface was thoroughly rinsed with pure water, and the remaining water on the surface was blown off with air. Next, a suspension of nitrogen-containing ζ- nanodiamond particles (particle diameter D50: 5 nm) (N-ζ- nD particle concentration: 1.0%, solvent: water, zeta potential: -40 mV) was applied to the treated SiO2 / Si substrate at room temperature, the substrate surface was thoroughly rinsed with pure water, and the remaining water on the surface was blown off with air.
[0143] The process of immersing the substrate in the nitrogen-containing ζ+ nanodiamond particle suspension, washing with pure water, immersing the substrate in the nitrogen-containing ζ- nanodiamond particle suspension, and drying was repeated four more times to form 10 nitrogen-containing nanodiamond particle layers, thereby obtaining a N-nD particle film / SiO2 / Si substrate laminate.
[0144] (Formation of Conductive Layer (2)) Then, on the N-nD particle film of the N-nD particle film / SiO2 / Si substrate laminate, a 2.45 GHz microwave plasma chemical vapor deposition apparatus (manufactured by Arios) with a spherical resonator structure was used to grow boron-doped nanodiamond (BDD) under the following conditions. This resulted in a BDD / N-nD particle film / SiO2 / Si substrate laminate. <CVD Conditions> Plasma output: 900 W Reaction pressure: 50 kPa Substrate temperature: 890°C Hydrogen flow rate: 100 sccm Carbon source: methane (flow rate: 2 sccm) Boron source: hydrogen-diluted 1% trimethylboron (flow rate: 1 sccm) Growth time: 80 hours
[0145] Thereafter, a hydrofluoric acid / nitric acid mixture (pure water: HF stock solution: nitric acid = 20 g / 20 g / 20 g) was used to completely dissolve and remove the SiO 2 / Si substrate from the BDD / N-nD particle film / SiO 2 / Si substrate laminate, yielding an N-nD particle film / BDD laminate. The resulting N-nD particle film / BDD laminate had a film thickness of 0.15 mm and was freestanding. Thereafter, a hydrogen plasma treatment (2) (650 W, 40 kPa, 5 minutes, substrate temperature 850°C, hydrogen flow rate 100 sccm) was performed on the N-nD particle film side surface of the N-nD particle film / BDD laminate to perform hydrogen termination and removal of sp2 carbon. Through the above treatments, a hydrogen-terminated N-nD particle film / BDD laminate (1) was obtained. The surface roughness Rms of the hydrogen-terminated N-nD particle film was 2 nm to 3 nm.
[0146] Furthermore, the concentrations of nitrogen atoms and boron atoms in the laminate (1) were measured by secondary ion mass spectrometry under the following conditions. The results are shown in Figure 1. <Secondary ion mass spectrometry conditions> Apparatus: PHI ADEPT-1010™ (manufactured by ULVAC-PHI, INC.) Measurement conditions: primary acceleration voltage, 5.0 kV Detection area: 54 x 54 µm 2 Primary ion species: Cs +
[0147] The resulting hydrogen-terminated NnD particle film / BDD laminate (1) was used as a catalytic electrode (1).
[0148] Comparative Example 1 (Formation of Catalyst Layer (1)) A SiO2 / Si substrate was used as the substrate. The SiO2 / Si substrate was a laminate of SiO2 (thickness 100 nm) with a diameter of 8 mm and n-type Si (thickness 0.45 mm). The SiO2 / Si substrate was subjected to ultrasonic cleaning treatment with acetone, ethanol, and pure water, and acid cleaning treatment.
[0149] A suspension of nitrogen-containing nanodiamond particles (N-nD, particle diameter D50: 5 nm, product name "DINNOVARE", manufactured by Daicel Corporation) (N-nD particle concentration: 1.0%, solvent: water) was applied to the treated SiO2 / Si substrate and dried to form an N-nD particle film having a single layer structure. This resulted in an N-nD particle film / SiO2 / Si substrate laminate.
[0150] The surface of the N-nD particle film of the obtained N-nD particle film / SiO2 / Si substrate laminate was subjected to hydrogen plasma treatment (1) (900 W, 50 kPa, substrate temperature 890°C, hydrogen flow rate 100 sccm) for any time within 1 hour to remove sp2 carbon from the N-nD particle film.
[0151] (Formation of Conductive Layer (2)) A BDD / N-nD particle film / SiO2 / Si substrate laminate (2) was obtained in the same manner as in Example 1, except that the boron atom and nitrogen atom concentrations were changed as shown in Table 3 below and the hydrogen plasma treatment (1) was not performed.
[0152] Thereafter, the SiO2 / Si substrate was removed in the same manner as in Example 1, and the surface of the N-nD particle film was subjected to hydrogen plasma treatment to hydrogen-terminate and remove sp2 carbon. Through these treatments, a hydrogen-terminated N-nD particle film / BDD laminate (2) was obtained.
[0153] The resulting hydrogen-terminated NnD particle film / BDD laminate (2) was used as a catalytic electrode (2).
[0154] (Evaluation) For the catalytic electrodes (1) and (2) obtained in the examples and comparative examples, the amount of hydrogen produced, the electron release flow rate in the hydrogen production reaction, the total reduction current density in the hydrogen production reaction, and the Faraday efficiency of H production in the hydrogen production reaction (H-F efficiency) were measured by the following methods.
[0155] <Measurement of Hydrogen Production Amount> The catalytic electrodes (1) and (2) were used to carry out a reduction reaction of HO, and the amount of hydrogen produced was measured. As shown in FIG. 2, a catalytic electrode (with an area of 0.2 cm2 in contact with the electrolyte) was attached to the working electrode 1. 2 ) was used as the counter electrode 2, and a platinum mesh electrode was used as the counter electrode 2. A silver-silver chloride (Ag / AgCl) electrode 3a immersed in a saturated potassium chloride aqueous solution 3b in a glass tube with a porous glass liquid junction 3c was used as the reference electrode 3. One side of an H-type cell (manufactured by EC Frontier Co., Ltd.) was designated as the anode chamber 6, and the other side as the cathode chamber 7. The working electrode 1 and reference electrode 3 were installed in the anode chamber 6, and the counter electrode 2 was installed in the cathode chamber 7. The two chambers were separated by a diaphragm 5 (Nafion 117), and 30 mL of electrolyte (100 mM potassium chloride aqueous solution) was added to each of the anode chamber 6 and the cathode chamber 7. After sealing the H-type cell, a sample bag 8 (Smart Bag PA, CEK-1, GL Science) was attached, and a constant potential of -1.0 V (vs. Ag / AgCl) was immediately applied to the working electrode 1 using an electrochemical measurement system (HSV-110, Hokuto Denko). Simultaneously with the application of the potential, the light emitted from a mercury xenon light source (not shown, L9588-04, Hamamatsu Photonics) was filtered with an optical filter (not shown, A9616-09, Hamamatsu Photonics) to cut out ultraviolet light, and only the visible light was introduced into a quartz optical fiber (A10014-70-0110, manufactured by Hamamatsu Photonics K.K.), and the visible light emitted from the fiber end 4 was irradiated toward the surface of the working electrode 1 (the surface on the catalyst layer (1) side). The application of the constant potential and the light irradiation were continued for 15 minutes, and then both were stopped simultaneously. Thereafter, the hydrogen concentration (ppm) in the mixed gas collected in the sample bag 8 was measured.
[0156] <Measurement of electron emission flow rate in hydrogen generation reaction> The electron emission efficiency of the catalytic electrodes (1) and (2) when irradiated with visible light was measured by the following method. That is, a measurement chamber (manufactured by Riko Boeki Co., Ltd., i series ultra-high vacuum microprobe and chamber, vacuum degree 10 -4 A gold foil was placed on an insulating base (at a pressure of 100 Pa or less, measurement temperature of 23 to 40°C), and the catalytic electrode was placed on top of it, with the BDD side in contact with the gold foil. Using a semiconductor parameter analyzer (KEITHLEY SEMICONDUCTOR CHARACTERIZATION SYSTEM 4200-SCS), a voltage of -20 V was applied to the back surface of the catalytic electrode, a collector voltage (0 to 100 V) was applied at a position 100 μm above the surface of the catalytic electrode, and visible light was applied from a position 35 mm away from the laminate (1) in the same manner as in <Measurement of hydrogen production amount> above, to measure the amount of current generated.
[0157] <Measurement of total reduction current density in hydrogen generation reaction> Using the same device and conditions as in the above <Measurement of hydrogen generation amount>, a constant potential was applied for 15 minutes, and the change in reduction current was recorded. The average value was divided by the electrode area to calculate the total reduction current density.
[0158] <Measurement of H2-F efficiency in hydrogen generation reaction> Using the same device and conditions as in the <Measurement of hydrogen generation amount>, a constant potential was applied for 15 minutes, and the change in reduction current value was recorded, and the total amount of electricity due to the reduction reaction was calculated. In addition, the amount of electricity used for hydrogen generation was calculated from the amount of hydrogen generated obtained in the <Measurement of hydrogen generation amount>, and the proportion of the total amount of electricity used for hydrogen generation in the reduction reaction, expressed as a percentage, was defined as the H2-F efficiency.
[0159] The results are summarized in the table below.
[0160] Example 2 (Formation of catalyst layer (1)) A conductive diamond electrode [a laminate (diameter 8 mm) of BDD (thickness approximately 10 μm) and conductive Si (thickness: 0.7 mm) manufactured by Matsuo Sangyo Co., Ltd.] was used as the conductive BDD substrate. The conductive BDD substrate was subjected to ultrasonic cleaning treatment using acetone, ethanol, and pure water, and acid cleaning treatment. Thereafter, a hydrogen plasma treatment was performed using a microwave plasma CVD device to further clean and hydrophilize the surface of the conductive BDD substrate.
[0161] A 40 μL suspension of nitrogen-containing ζ nanodiamond particles (particle diameter D50: 5 nm) (N-ζ nD particle concentration: 1.0%, solvent: water, zeta potential: +50 mV) was applied to the conductive BDD substrate after the treatment. The coated conductive BDD substrate was then spun at 1000 rpm for 30 seconds using a spin coater (MS-B100, manufactured by Mikasa Co., Ltd.) to spread the applied suspension. The rotation speed of the spin coater was then increased to 6000 rpm and held for 2 minutes to remove moisture from the conductive BDD substrate and dry it.
[0162] The process of applying, spreading, and drying the suspension of nitrogen-containing ζ+ nanodiamond particles was repeated three more times. Thereafter, the substrate was dried in air at 60°C for 10 minutes using a hot plate (AS ONE Corporation, CHP-1700F). This resulted in a laminate (N-nD particle film / conductive BDD substrate laminate (3)) in which multiple nitrogen-containing nanodiamond particle layers were stacked on a conductive BDD substrate. The surface roughness Rms of the N-nD particle film was 5 nm to 20 nm. This was designated catalytic electrode (3).
[0163] (Evaluation) The catalytic electrode (3) obtained in Example 2 was measured for the amount of hydrogen produced, the total reduction current density in the hydrogen production reaction, the LSV in the hydrogen production reaction, the amount of CO produced, and the total reduction current density in the CO production reaction by the following methods. In addition, the measurements were carried out in the same manner as above except that visible light irradiation was not performed, and this was used as a blank.
[0164] <Measurement of Hydrogen Production Amount> The catalytic electrode (3) was used to carry out a reduction reaction of HO, and the amount of hydrogen produced was measured. As shown in FIG. 2, a laminate (1) (with an area of 0.2 cm2 in contact with the electrolyte) was attached to a working electrode 1. 2 ) was used as the electrode, and a platinum mesh electrode was used as the counter electrode 2. A silver-silver chloride (Ag / AgCl) electrode 3a immersed in a saturated potassium chloride aqueous solution 3b in a glass tube with a porous glass liquid junction 3c was used as the reference electrode 3. One side of an H-type cell (manufactured by EC Frontier Co., Ltd.) was designated as the cathode chamber 9, and the other side as the anode chamber 10. The working electrode 1 and reference electrode 3 were installed in the cathode chamber 9, and the counter electrode 2 was installed in the anode chamber 10. The two chambers were separated by a diaphragm 5 (Nafion 117), and 30 mL of 0.1 M potassium chloride aqueous solution was added to each chamber as the electrolyte. After sealing the H-type cell, argon gas was bubbled through the inlet 6 at a flow rate of 80 mL / min for 30 minutes and released from the gas outlet 8, thereby degassing the electrolyte. While maintaining the argon gas flow rate at 80 mL / min, a sample bag 7 (Smart Bag PA, CEK-1, manufactured by GL Sciences Co., Ltd.) was attached, and a constant potential of −2.0 V (vs. Ag / AgCl) was immediately applied to the working electrode 1 using an electrochemical measurement system (HSV-110, manufactured by Hokuto Denko Co., Ltd.). When light irradiation was performed, radiation from a mercury-xenon light source (not shown, manufactured by Hamamatsu Photonics K.K.) was filtered out of ultraviolet light with an optical filter (not shown, manufactured by Hamamatsu Photonics K.K.), and only visible light was introduced into a quartz optical fiber (A10014-70-0110, manufactured by Hamamatsu Photonics K.K.), and the visible light emitted from the fiber end 4 was irradiated toward the surface of the working electrode 1 (the surface on the electron excitation layer (1) side). The argon gas flow, application of a constant potential, and light irradiation were continued for 10 minutes, and then all of these were stopped. After that, quantitative analysis of the components contained in the mixed gas collected in the sample bag 7 and the electrolyte in the cathode chamber 9 was performed, and the amount of hydrogen produced was calculated.
[0165] <Measurement of total reduction current density in hydrogen generation reaction> Using the same device and conditions as in the above <Measurement of hydrogen generation amount>, a constant potential was applied for 15 minutes, and the change in reduction current was recorded. The average value was divided by the electrode area to calculate the total reduction current density.
[0166] <LSV Measurement> Using the same device as in the above <Hydrogen Production Amount Measurement>, the change in reduction current when the potential of the working electrode 1 was linearly swept from 0 V to −2.0 V was recorded. The results are shown in Figure 3. From Figure 3, it can be seen that the catalytic electrode of the present disclosure has the effect of reducing the applied voltage when irradiated with visible light.
[0167] The results of the measurement of the amount of hydrogen produced and the measurement of the total reduction current density in the hydrogen production reaction are summarized in the table below.
[0168] From Table 4, it can be seen that when visible light is irradiated, the total reduction current density increases by about 1.5 times, and accordingly the efficiency of water reduction improves, resulting in more efficient production of hydrogen than when no visible light is irradiated.
[0169] <Measurement of CO Production Amount> A reduction reaction of carbon dioxide was carried out using the catalytic electrode (3), and the amount of carbon monoxide produced was measured. As shown in FIG. 2, a laminate (1) (with an area of 0.2 cm2 in contact with the electrolyte) was attached to a working electrode 1. 2) was used as the electrode, and a platinum mesh electrode was used as the counter electrode 2. The reference electrode 3 was a silver-silver chloride (Ag / AgCl) electrode 3a immersed in a saturated potassium chloride aqueous solution 3b in a glass tube with a porous glass liquid junction 3c. One side of an H-type cell (manufactured by EC Frontier Co., Ltd.) served as the cathode chamber 9, and the other as the anode chamber 10. The working electrode 1 and reference electrode 3 were installed in the cathode chamber 9, and the counter electrode 2 was installed in the anode chamber 10. The two chambers were separated by a diaphragm 5 (Nafion 117), and 30 mL of 0.1 M potassium chloride aqueous solution was added to each chamber as the electrolyte. After sealing the H-type cell, CO gas was bubbled through the inlet 6 at a flow rate of 80 mL / min for 30 minutes and released from the gas outlet 8, thereby degassing the electrolyte and dissolving CO to a saturated concentration. While maintaining a CO2 gas flow rate of 80 mL / min, a sample bag 7 (Smart Bag PA, CEK-1, manufactured by GL Sciences Co., Ltd.) was attached, and a constant potential of -2.0 V (vs. Ag / AgCl) was immediately applied to the working electrode 1 using an electrochemical measurement system (HSV-110, manufactured by Hokuto Denko Corporation). When light irradiation was performed, radiation from a mercury-xenon light source (not shown, manufactured by Hamamatsu Photonics K.K.) was filtered out of ultraviolet light with an optical filter (not shown, manufactured by Hamamatsu Photonics K.K.), and only visible light was introduced into a quartz optical fiber (A10014-70-0110, manufactured by Hamamatsu Photonics K.K.), and the visible light emitted from the fiber end 4 was irradiated toward the surface of the working electrode 1 (the surface on the electron excitation layer (1) side). The CO flow, constant potential application, and light irradiation were continued for 10 minutes, and then all of these were stopped. After that, quantitative analysis of the components contained in the mixed gas collected in the sample bag 7 and the electrolyte in the cathode chamber 9 was performed, and the amounts of hydrogen and CO produced were calculated.
[0170] <Measurement of total reduction current density in CO production reaction> Using the same device and conditions as in the above <Measurement of CO production amount>, a constant potential was applied for 15 minutes, and the change in reduction current was recorded. The average value was divided by the electrode area to calculate the total reduction current density.
[0171] The results are summarized in the table below.
[0172] Table 5 shows that when the catalytic electrode of the present disclosure is irradiated with visible light, the efficiency of carbon dioxide reduction is improved, and approximately 10 times as much carbon monoxide is produced as compared to when it is not irradiated with visible light.
[0173] In summary, the configuration of the present disclosure and its variations are described below. [1] A semiconductor catalyst comprising a thin film containing nitrogen-containing diamond particles in the plane direction and the height direction. [2] The semiconductor catalyst according to [1], wherein the thin film has a configuration in which the nitrogen-containing diamond particles are arranged in the plane direction and the height direction, and diamond particles adjacent in the plane direction and the height direction are in close contact with each other. [3] A semiconductor catalyst according to [1], wherein the nitrogen atom concentration of the thin film is 10×10 18 atoms / cm 3[4] The semiconductor catalyst according to any one of [1] to [3], wherein the thickness of the thin film is 5 nm or more. [5] The semiconductor catalyst according to any one of [1] to [4], wherein the surface has a negative electron affinity. [6] The semiconductor catalyst according to any one of [1] to [5], wherein the semiconductor catalyst is a visible light responsive catalyst. [7] The semiconductor catalyst according to any one of [1] to [6], wherein the semiconductor catalyst is a reduction catalyst. [8] The semiconductor catalyst according to any one of [1] to [7], wherein the semiconductor catalyst is a hydrogen generation catalyst. [9] A method for producing a semiconductor catalyst, comprising carrying out the following step 1, and then carrying out the following step 2 at least once, to obtain the semiconductor catalyst according to any one of [1] to [8].
[10] A method for producing a reduced product by reducing a substance to be reduced under irradiation with visible light and in the presence of the semiconductor catalyst according to any one of [1] to [8] to obtain a corresponding reduced product.
[11] A reduction product generating device comprising the semiconductor catalyst according to any one of [1] to [8].
[12] A catalytic electrode for generating hydrogen, comprising a catalyst layer (1) and a conductive layer (2), wherein the catalyst layer (1) comprises the semiconductor catalyst according to any one of [1] to [8].
[13] A catalytic electrode for hydrogen generation, comprising a catalytic layer (1) and a conductive layer (2), wherein the catalytic layer (1) comprises a thin film containing nitrogen-containing diamond particles in the plane direction and height direction.
[14] A catalytic electrode for hydrogen generation, comprising a catalytic layer (1) and a conductive layer (2), wherein the catalytic layer (1) comprises a thin film having a configuration in which the nitrogen-containing diamond particles are arranged in the plane direction and height direction, and diamond particles adjacent in the plane direction and height direction are in close contact with each other.
[15] A catalytic electrode for hydrogen generation, wherein the nitrogen atom concentration of the thin film is 10 x 10 18 atoms / cm 3
[16] The catalytic electrode for hydrogen generation according to any one of
[12] to
[15] , wherein the conductive layer (2) is a layer having a diamond crystal structure in which a part of carbon atoms is substituted with boron atoms.
[17] The catalytic electrode for hydrogen generation according to
[13] or
[14] , wherein the concentration of boron atoms in the conductive layer (2) is 1×10 or more. 19 atoms / cm 3
[18] The hydrogen generation catalytic electrode according to any one of
[12] to
[17] , wherein the thickness of the catalytic layer (1) is 1 nm to 100 μm, and the thickness of the conductive layer (2) is 1 μm or more.
[19] A method for producing hydrogen, comprising reducing water to produce hydrogen using the hydrogen generation catalytic electrode according to any one of
[12] to
[18] under visible light irradiation.
[20] A hydrogen production method, comprising generating hydrogen using an apparatus including a water electrolysis cell comprising a water storage section, the hydrogen generation catalytic electrode according to any one of
[12] to
[18] , arranged so as to contact the water in the storage section, and a counter electrode.
[21] A hydrogen generation device including a water electrolysis cell comprising a water storage section, the hydrogen generation catalytic electrode according to any one of
[12] to
[18] , arranged so as to contact the water in the storage section, and a counter electrode.
[0174] The semiconductor catalyst of the present disclosure is formed from diamond particles, which are extremely physically and chemically stable, and therefore has excellent durability and is not limited in its usage environment. Furthermore, the semiconductor catalyst of the present disclosure easily releases electrons when irradiated with visible light or sunlight, thereby exhibiting the effect of promoting reduction reactions. Because of the above-mentioned properties, the semiconductor catalyst can be suitably used as a reduction catalyst or a visible-light-responsive catalyst. Furthermore, by using the semiconductor catalyst in an electrode, it is possible to efficiently utilize inexhaustible solar energy to perform a water electrolysis reaction, thereby producing clean energy hydrogen while suppressing the generation of carbon dioxide.
[0175] 1 Working electrode 2 Counter electrode 3 Reference electrode 3a Ag / AgCl electrode 3b Saturated potassium chloride aqueous solution 3c Porous glass liquid junction 4 Fiber end 5 Diaphragm 6 Anode chamber 7 Cathode chamber 8 Sample bag
Claims
1. A semiconductor catalyst consisting of a thin film containing nitrogen-containing diamond particles in the planar and vertical directions.
2. The semiconductor catalyst according to claim 1, wherein the thin film is a thin film having a configuration in which nitrogen-containing diamond particles are arranged in the planar and height directions, and adjacent diamond particles in the planar and height directions are in close contact with each other.
3. The nitrogen atomic concentration of the thin film is 10×10 18 atoms / cm 3 The semiconductor catalyst according to claim 1 or 2.
4. The semiconductor catalyst according to claim 1 or 2, wherein the thin film has a thickness of 5 nm or more.
5. The semiconductor catalyst according to claim 1 or 2, wherein the surface has a negative electron affinity.
6. The semiconductor catalyst according to claim 1 or 2, which is a visible light responsive catalyst.
7. The semiconductor catalyst according to claim 1 or 2, which is a reduction catalyst.
8. The semiconductor catalyst according to claim 1 or 2, which is a catalyst for generating hydrogen.
9. A method for producing a semiconductor catalyst, comprising carrying out the following step 1, and then carrying out the following step 2 at least once to obtain the semiconductor catalyst according to claim 1 or 2. Step 1: Fixing nitrogen-containing diamond particles having a positive or negative charge on a substrate having a positive or negative charge, the nitrogen-containing diamond particles having an opposite charge to the charge of the substrate. Step 2: Laminating nitrogen-containing diamond particles having a positive or negative charge on the fixed nitrogen-containing diamond particles, the nitrogen-containing diamond particles having an opposite charge to the fixed nitrogen-containing diamond particles.
10. A method for producing a reduced product, comprising reducing a reducible substance under irradiation of visible light and in the presence of the semiconductor catalyst according to claim 1 or 2 to obtain the corresponding reduced product.
11. A reduction product generating device comprising the semiconductor catalyst according to claim 1 or 2.
12. A catalytic electrode for generating hydrogen, comprising a catalytic layer (1) and a conductive layer (2), the catalytic layer (1) comprising the semiconductor catalyst according to claim 1 or 2.
13. The catalyst electrode for generating hydrogen according to claim 12, wherein the conductive layer (2) is a layer having a diamond crystal structure in which a portion of carbon atoms is substituted with boron atoms.
14. The boron atom concentration in the conductive layer (2) is 1×10 19 atoms / cm 3 The hydrogen generation catalyst electrode according to claim 13 .
15. The catalyst electrode for generating hydrogen according to claim 12, wherein the thickness of the catalyst layer (1) is 1 nm to 100 μm, and the thickness of the conductive layer (2) is 1 μm or more.
16. A method for producing hydrogen, comprising reducing water and producing hydrogen using the hydrogen generation catalyst electrode according to claim 12 under irradiation with visible light.
17. A hydrogen generating device including a water electrolysis cell comprising: a water storage section; the hydrogen generating catalytic electrode according to claim 12 arranged in contact with the water in the storage section; and a counter electrode.
Citation Information
Patent Citations
Semiconductor photoelectrode
JP2018090887A
PRS resource allocation method, measurement interval allocation method and related equipment
JP2023068141A
Hybrid vehicle control device
JP2023091246A
Water treatment method and water treatment system
JP2023091950A
Nitrogen-doped hydrogen terminal diamond and preparation method thereof
CN113731459A