Low thermal expansion steel casting product and method for manufacturing same
The low thermal expansion cast steel product with a specific composition and cryo treatment method addresses the issue of coarse grains in existing products, achieving superior ultrasonic flaw detection by maintaining a low thermal expansion coefficient and fine crystal structure, enhancing defect detection capabilities.
Patent Information
- Application Number
- PCT/JP2024/014670
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-20
- Filing Date
- 2024-04-11
- Publication Date
- 2024-10-24
AI Technical Summary
Low thermal expansion cast steel products exhibit coarse austenite crystal grains, leading to inferior ultrasonic flaw detection due to scattering and attenuation of ultrasonic waves at grain boundaries, making defect detection difficult.
A low thermal expansion cast steel product with a specific composition (C: 0.040% or less, Si: 0.30% or less, Mn: 0.05-0.50%, S: 0.005% or less, Ni: 31.00-34.00%, Co: 2.00-6.00%, Al: 0.035-0.100%) and a manufacturing method involving cryo treatment and recrystallization, resulting in an average austenite crystal grain size of 200 μm or less and an ultrasonic attenuation coefficient of 2.0 dB/cm or less.
The solution enables excellent ultrasonic flaw detection properties by maintaining a low thermal expansion coefficient of 1.0×10^-6 /°C and achieving a fine equiaxed crystal structure, improving the ability to detect defects non-destructively.
Smart Images

Figure JP2024014670_24102024_PF_FP_ABST
Abstract
Description
Low thermal expansion cast steel products and their manufacturing method
[0001] The present invention relates to a low thermal expansion cast steel product having a low thermal expansion coefficient and a method for producing the same.
[0002] Thermally stable invar alloys are widely used as materials for components in electronics and semiconductor-related equipment, laser processing machines, and ultra-precision processing equipment.
[0003] Patent Document 1 describes a steel sheet containing 29.5 to 35% Ni, 2.0 to 7.0% Co, and 0.001 to 2.0% Cr, with a thermal expansion coefficient of 0.5 × 10 -6 / ℃ ~ 2.0 × 10 -6 This alloy is obtained by homogeneous solution treatment, followed by quenching or annealing by cooling at a rate of 1°C / sec or less, and then cold rolling by 10% or more.
[0004] Patent Document 2 discloses a low thermal expansion wire containing 65% or less Co, 30% or less Ni, and 10% or less Cr, with the total content of Co and Ni being 25 to 65%. Patent Document 2 also discloses a method of transforming the low thermal expansion wire into a strain-induced martensite phase by cold working a part of the austenite phase.
[0005] Patent Document 3 discloses a low thermal expansion alloy containing 0.03 to 1.5% Ni, 53 to 55% Ni and Co combined, and 9 to 10% Cr. Patent Document 3 discloses a method of annealing the alloy at 650 to 900°C and then cooling it in a furnace at a rate of less than 20°C / min.
[0006] Patent No. 2796966 Japanese Patent Publication No. 6-279945 Patent No. 5534150
[0007] In low-thermal expansion cast steel products, austenite grains tend to coarsen, making ultrasonic testing less effective than forged products. In other words, ultrasonic waves are scattered and attenuated at grain boundaries, making it difficult to detect defects using ultrasonic testing, a non-destructive test.
[0008] An object of the present invention is to solve the above problems and to provide a low thermal expansion cast steel product having excellent ultrasonic flaw detection properties.
[0009] The present inventors have conducted extensive research into methods for improving ultrasonic flaw detection performance and have achieved the present invention. The present invention includes the following aspects.
[0010] (1) A low thermal expansion cast steel product having a component composition, in mass%, of C: 0.040% or less, Si: 0.30% or less, Mn: 0.05 to 0.50%, S: 0.005% or less, Ni: 31.00 to 34.00%, Co: 2.00 to 6.00%, Al: 0.035 to 0.100%, with the balance being Fe and unavoidable impurities, the average crystal grain size of the austenitic structure being 200 μm or less, and the attenuation coefficient of the ultrasonic bottom echo being 2.0 dB / cm or less.
[0011] (2) The average thermal expansion coefficient at 25 to 100°C is 1.0 x 10 -6 / °C or less.
[0012] (3) A method for producing a low thermal expansion cast steel product according to (1) or (2), comprising the steps of: a cryo-treatment step of cooling a cast steel product having a composition, in mass%, of C: 0.040% or less, Si: 0.30% or less, Mn: 0.05 to 0.50%, S: 0.005% or less, Ni: 31.00 to 34.00%, Co: 2.00 to 6.00%, and Al: 0.035 to 0.100%, with the balance being Fe and unavoidable impurities; and a recrystallization step of heating the cryo-treated cast steel product to 800 to 1100°C and maintaining the temperature for 0.5 to 5 hours.
[0013] According to the present invention, it is possible to obtain a low thermal expansion cast steel product having excellent ultrasonic flaw detection properties.
[0014] 1 shows an example of the structure of a cast steel product after cryo-treatment. 2 shows an example of the structure of a cast steel product after recrystallization treatment.
[0015] The present invention will be described in detail below.
[0016] <Composition> First, the composition of the cast steel product of the present invention will be described. Hereinafter, "%" regarding the composition of the components represents "mass %" unless otherwise specified.
[0017] (C: 0.040% or less) C dissolves in austenite and contributes to increasing strength. However, C dissolves in the matrix during the recrystallization process and precipitates during cooling, increasing the thermal expansion coefficient. The average thermal expansion coefficient at 25 to 100°C is 1.0 x 10 -6 / °C or less, it is necessary to reduce the amount of C precipitated. Therefore, the C content is set to 0.040% or less. The C content may be 0.035% or less, 0.030% or less, 0.025% or less, or 0.020% or less. C is not an essential element, and the C content may be 0%. The C content may be 0.001% or more, 0.002% or more, 0.004% or more, 0.008% or more, 0.010% or more, or 0.015% or more.
[0018] (Si: 0.30% or less) Si is added as a deoxidizer. In the present invention, in order to produce a sound cast steel product without blowing, it is sufficient to add the minimum amount necessary for deoxidation. The final cast steel product does not need to contain Si, and the lower limit of the Si content is 0%. Si may be contained in a range of 0.30% or less. Since deoxidation can also be performed with Al, Si does not need to be added. The Si content may be 0.25% or less, 0.20% or less, 0.15% or less, or 0.10% or less. The Si content may be 0.01% or more, 0.02% or more, 0.03% or more, 0.04% or more, 0.05% or more, or 0.07% or more.
[0019] (Mn: 0.05 to 0.50%) Mn is added as a deoxidizer. It is also added to react with S to form MnS, thereby fixing S. In the present invention, to obtain this effect, the Mn content is set to 0.05% or more. If the Mn content is too high, the effect will saturate, so the Mn content is set to 0.50% or less. The Mn content may be 0.10% or more, 0.15% or more, 0.20% or more, 0.25% or more, or 0.30% or more. The Mn content may be 0.48% or less, 0.45% or less, 0.40% or less, or 0.35% or less.
[0020] (S: 0.005% or less) S is contained as an impurity. When S segregates at grain boundaries, it inhibits recrystallization and reduces ultrasonic flaw detection properties, so the lower the S content, the better. In the low thermal expansion cast steel product of the present invention, the S content is 0.005% or less. The S content may be 0.004% or less, or 0.003% or less. The lower the S content, the better, and the lower limit of the S content is 0%. However, since setting the S content to 0% increases costs, the S content may be 0.001% or more, or 0.002% or more.
[0021] (Ni: 31.00 to 34.00%) Ni is an element that lowers the thermal expansion coefficient. If the Ni content is too high or too low, the thermal expansion coefficient will not be sufficiently small. Also, if the Ni content is too high, it becomes difficult to cause martensitic transformation by cooling, and the proportion of equiaxed crystals after recrystallization decreases. The average thermal expansion coefficient at 25 to 100°C is 1.0 x 10 -6 / °C or less, it is necessary to control the Ni content within a narrow range. Specifically, the Ni content is set to a range of 31.00 to 34.00%. The Ni content may be 31.10% or more, 31.20% or more, 31.30% or more, 31.40% or more, 31.50% or more, 31.60% or more, or 31.70% or more. The Ni content may be 33.80% or less, 33.50% or less, 33.00% or less, or 32.50% or less.
[0022] (Co: 2.00 to 6.00%) Co contributes to lowering the thermal expansion coefficient in combination with Ni. The average thermal expansion coefficient at 25 to 100°C is 1.0 x 10 -6 / °C or less, the Co content is in the range of 2.00 to 6.00%. The Co content may be 2.30% or more, 2.50% or more, 2.70% or more, 3.00% or more, 3.50% or more, or 4.00% or more. The Co content may be 5.80% or less, 5.60% or less, 5.40% or less, 5.20% or less, or 5.00% or less.
[0023] Furthermore, to reduce the thermal expansion coefficient, it is preferable that the Ni content (mass%) [Ni] and the Co content (mass%) [Co] satisfy the relationship 34.00≦[Ni]+0.8×[Co]≦38.00. [Ni]+0.8×[Co] may be 34.20% or more, 34.50% or more, 34.70% or more, 35.00% or more, or 35.50% or more. [Ni]+0.8×[Co] may be 37.80% or less, 37.60% or less, 37.20% or less, 36.80% or less, or 36.50% or less.
[0024] (Al: 0.035 to 0.100%) Al is added as a deoxidizer. If the Al content is low, deoxidation is insufficient and Mn oxides are formed, which prevents the formation of MnS and makes it easier for S to segregate at grain boundaries, inhibiting recrystallization. As a result, ultrasonic flaw detection performance deteriorates. Therefore, the Al content is set to 0.035% or more. If the Al content is too high, the effect saturates, so the Al content is set to 0.100% or less. The Al content may be 0.040% or more, or 0.045% or more. The Al content may be 0.090% or less, 0.080% or less, 0.070% or less, or 0.060% or less.
[0025] The remainder of the composition is Fe and inevitable impurities. The inevitable impurities refer to elements that are not intentionally added to steel but are inevitably mixed in due to raw materials, the manufacturing environment, etc., when industrially manufacturing a steel having the composition specified in the present invention. Examples of inevitable impurities include P and Cu, which are elements that are not intentionally added in the manufacturing process. The content of the impurities is not limited as long as it is within a range that does not affect the effects of the present invention. The total content of the impurities, in mass %, may be 0.50% or less, 0.40% or less, 0.30% or less, 0.20% or less, 0.15% or less, 0.10% or less, 0.05% or less, or 0%.
[0026] <Structure of Cast Steel Product> The structure of the cast steel product of the present invention is an austenite structure with an average grain size of 200 μm or less. The structure is centered on fine equiaxed crystals. When the proportion of equiaxed crystals is low, the average grain size of austenite becomes large. Although it is not necessary for all of the structure to be equiaxed crystals, it is preferable that the proportion of equiaxed crystals is 60% or more in terms of area ratio. The proportion of equiaxed crystals may be 70% or more, 80% or more, 85% or more, 90% or more, or 95% or more in terms of area ratio.
[0027] The average grain size of austenite was determined as the average circle-equivalent diameter of crystal grains observed under an optical microscope after cutting a specimen for microstructure observation from near the center of the cast steel product, mirror-polishing the observation surface, and etching with Marble reagent. Among the crystal grains observed under the optical microscope, those with a ratio of the long side to the short side of 3 or more were judged to be columnar crystals, and those with a ratio of less than 3 were judged to be equiaxed crystals.
[0028] <Attenuation Coefficient> The attenuation coefficient of the ultrasonic bottom echo of the cast steel product of the present invention is 2.0 dB / cm or less. Here, the attenuation coefficient is defined as the value (dB / cm) calculated by (B1-B2) / L, where B1 (dB) is the height of the first bottom echo, B2 (dB) is the height of the second bottom echo, and L (cm) is the distance from the sample surface to the bottom of the cast steel product when the output is adjusted so that the height of the first bottom echo is 75-85% of 100% ultrasonic output in the vertical method of bottom echo detection. The attenuation coefficient is preferably 1.8 dB / cm or less, 1.5 dB / cm or less, 1.2 dB / cm or less, or 1.0 dB / cm or less. A small attenuation coefficient is advantageous for detecting defects by ultrasonic flaw detection, a non-destructive test. Such an attenuation coefficient can be obtained by producing a low-thermal expansion cast steel product with a chemical composition within the above-mentioned range and using the manufacturing method described below.
[0029] <Coefficient of thermal expansion> The cast steel product of the present invention has an average coefficient of thermal expansion of 1.0 × 10 at 25 to 100°C. -6 / °C or less. The thermal expansion coefficient is measured by taking a thermal expansion measurement specimen from near the center of the cast steel product and heating it from 0°C to 130°C at a temperature increase rate of 3°C / min using a thermal expansion measuring instrument, and measuring the average thermal expansion coefficient from 25 to 100°C. A DIL 402C manufactured by NETZSCH can be used as the thermal expansion measuring instrument. The average thermal expansion coefficient from 25 to 100°C is 1.00 x 10 -6 / ℃ or less, 0.90 × 10 -6 / °C or less, 0.80 x 10 -6 / °C or less, 0.70 x 10 -6 / °C or less, 0.60 x 10 -6 / °C or less, or 0.50 x 10 -6 / °C or less.
[0030] <<Manufacturing Method>> Next, a method for manufacturing a low thermal expansion cast steel product of the present invention will be described. The low thermal expansion cast steel product of the present invention can be obtained by the casting and heat treatment described below. Note that in the manufacturing method of a low thermal expansion cast steel product of the present invention, no forging is performed.
[0031] (Casting) First, molten steel is produced so that the cast steel product has the aforementioned chemical composition. The method for producing molten steel is not particularly limited, and known devices and methods may be used. Next, the molten steel is poured into a mold and solidified to obtain the cast steel product. The mold, the device for pouring the molten steel into the mold, and the method for pouring are not particularly limited, and known devices and methods may be used. The structure of the cast steel product produced in the mold will be a structure centered on columnar crystals. The obtained cast steel product is subjected to the following heat treatment.
[0032] (Cryo-treatment step) Next, the cast steel product is rapidly cooled to below the Ms point, held at a temperature below the Ms point for 0.5 to 3 hours, and then heated to room temperature (cryo-treatment step). The cooling method is not particularly limited. Generally, the Ms point can be estimated using the steel composition according to the following formula:
[0033] Ms (°C) = 521 - 353C - 22Si - 24.3Mn - 7.7Cu - 17.3Ni - 17.7Cr - 25.8Mo where C, Si, Mn, Cu, Ni, Cr, and Mo are the contents (mass%) of each element. Elements that are not contained are set to 0.
[0034] For the low-thermal-expansion cast steel product of the present invention, the Ms point calculated by the above formula will be approximately -10°C to -70°C, depending on the Ni content in particular. Therefore, methods such as immersion in dry ice and methyl alcohol or ethyl alcohol, liquid nitrogen, or spraying with liquid nitrogen can be used as cooling media. This results in the formation of a structure containing fine martensite. Furthermore, the temperature can be raised by lifting the material into room-temperature air. Figure 1 shows an example of the structure after the cryo-treatment process. The black areas in the structure photograph are martensite. The formation of a large amount of martensite refines the austenite grain size in the subsequent recrystallization process.
[0035] (Recrystallization Treatment Step) Next, the cast steel product is reheated to 800-1100°C, held at 800-1100°C for 0.5-5 hours, and then cooled. This causes the martensite-formed structure to revert to an austenite structure. The grain size of the structure formed by normal solidification is approximately 1-10 mm, but by undergoing the above-mentioned cryo-treatment step and the subsequent recrystallization treatment step, the austenite structure becomes a fine structure with an average grain size of 200 μm or less, centered on equiaxed crystals. Figure 2 shows an example of the structure after the recrystallization treatment step. It can be seen that the structure after the recrystallization treatment step has become a fine structure with an average grain size of 200 μm or less.
[0036] (Solution Treatment Step) After the cryo-treatment, a solution treatment step may be performed in which the cast steel product is heated to 800 to 1100°C, held at that temperature for 0.5 to 5 hours, and then rapidly cooled. The solution treatment step is not an essential step and may be performed as needed. The solution treatment step dissolves precipitates that precipitated during casting, improving ductility and toughness.
[0037] (Diffusion Treatment Step) A diffusion treatment step may be further provided before the cryo-treatment step, in which the steel castings are held at 1100 to 1300°C for 5 to 50 hours. The diffusion treatment step is not an essential step and may be performed as needed. This eliminates the segregation of Ni and impurities in the steel, and allows for the more stable production of steel castings with a low thermal expansion coefficient, even for large-sized steel castings.
[0038] (Tempering Treatment Step) Between the cryo-treatment step and the recrystallization treatment step, the cast steel product may be subjected to martensite tempering treatment in which the cast steel product is heated to 300 to 400°C, just below the AC3 point, and held at 300 to 400°C for 1 to 10 hours, in order to further refine the recrystallized austenite grains. The tempering treatment step is not an essential step and may be performed as needed.
[0039] Example 1 of the Invention Using a high-frequency melting furnace, a molten metal was poured into a mold to produce a Y-type test material adjusted to have the composition shown in No. 1 in Table 1. The produced Y-type test material was subjected to cryo-treatment by cooling to -196°C and holding for 1.5 hours, and then reheated to 900°C, held for 2.0 hours, and then subjected to recrystallization treatment by allowing to cool in the air, thereby obtaining a low thermal expansion cast steel product.
[0040] <Invention Examples 2 to 7, Comparative Examples 1 to 6> Low thermal expansion cast steel products were obtained in the same manner as in Example 1, except that the chemical composition, cryo-treatment, and recrystallization treatment temperatures were set to the conditions shown in Tables 1 and 2. For each treatment temperature in Table 2, "-" indicates that the corresponding step was not performed. Note that Comparative Example 6 is a forged product that was forged after casting.
[0041] (Average Austenite Grain Size and Average Thermal Expansion Coefficient from 25 to 100° C.) The average austenite grain size and average thermal expansion coefficient from 25 to 100° C. were determined for the obtained low thermal expansion cast steel products by the above-mentioned method.
[0042] (Attenuation coefficient) A 25 x 25 x 100L sample was taken from the Y-shaped test material, and the bottom echo height was measured in a direction perpendicular to the longitudinal direction using the vertical method. The ultrasonic frequency was 2 MHz, and the first bottom echo height of the sample was adjusted to 80%, and the second bottom echo height B2 (dB) was obtained. The first height B1 (dB) and the sample height (L) were used to calculate (B1-B2) / L, which was used as the attenuation coefficient.
[0043] The results are shown in Table 2. In Table 2, the attenuation coefficient "≧2.70" means that the attenuation was too large to measure. The Ms point is a value calculated using the above-mentioned estimation formula.
[0044]
[0045]
[0046] As shown in Table 2, the low thermal expansion cast steel products of the present invention have a low thermal expansion coefficient at 25 to 100°C, and also have a small attenuation coefficient in the as-cast state, similar to that of forged products, i.e., they have excellent ultrasonic flaw detection properties.
[0047] Comparative Example 1 is an example in which neither cryo-treatment nor recrystallization treatment was performed, and the specimen had coarse austenite grains as cast, resulting in a large damping coefficient.
[0048] Comparative Example 2 is an example in which the Al content was low, and it is thought that the formation of Mn oxides prevented the formation of MnS, which led to the segregation of S at grain boundaries and inhibited recrystallization, resulting in an increase in the average grain size of austenite and an increase in the damping coefficient.
[0049] Comparative Example 3 is an example in which the S content was high and the Al content was low, and it is believed that the formation of Mn oxides prevented the formation of MnS, and the high S content also made S more likely to segregate at grain boundaries, inhibiting recrystallization. As a result, the average grain size of austenite increased, and the damping coefficient also increased.
[0050] Comparative Example 4 is an example in which the Ni content was high, the Co content was high, and the Al content was low. The inappropriate Ni and Co contents resulted in a high thermal expansion coefficient. Furthermore, the formation of Mn oxides prevented the formation of MnS, which facilitated segregation of S at grain boundaries and inhibited recrystallization. Furthermore, the high Ni content stabilized austenite, reducing the amount of martensitic transformation by cryo-treatment and reducing the number of equiaxed crystals after recrystallization. As a result, the average grain size of austenite increased, resulting in a high damping coefficient.
[0051] Comparative Example 5 is an example in which the Ni content, Co content, and Al content were low, and it is believed that the inappropriate Ni and Co contents increased the thermal expansion coefficient, and the formation of Mn oxides prevented the formation of MnS, making it easier for S to segregate at grain boundaries and inhibiting recrystallization, resulting in an increase in the average grain size of austenite and an increase in the damping coefficient.
[0052] Comparative Example 6 is an example of a forged product that was forged without undergoing cryo-treatment or recrystallization treatment. Because it is a forged product, it has a processed structure and is different from the low thermal expansion cast steel product of the present invention, which is cast steel.
Claims
1. A low thermal expansion cast steel product having a composition, in mass%, of C: 0.040% or less, Si: 0.30% or less, Mn: 0.05-0.50%, S: 0.005% or less, Ni: 31.00-34.00%, Co: 2.00-6.00%, Al: 0.035-0.100%, with the balance being Fe and unavoidable impurities, the average crystal grain size of the austenitic structure being 200 μm or less, and the attenuation coefficient of the ultrasonic bottom echo being 2.0 dB / cm or less.
2. The average thermal expansion coefficient at 25 to 100°C is 1.0 x 10 -6 2. The low thermal expansion cast steel product according to claim 1, characterized in that the thermal expansion coefficient is 0.1 / °C or less.
3. A method for producing a low thermal expansion cast steel product according to claim 1 or 2, comprising the steps of: a cryo-treatment step of cooling a cast steel product having a composition, in mass %, of C: 0.040% or less, Si: 0.30% or less, Mn: 0.05-0.50%, S: 0.005% or less, Ni: 31.00-34.00%, Co: 2.00-6.00%, Al: 0.035-0.100%, with the balance being Fe and unavoidable impurities, to the Ms point or below, holding the temperature at the Ms point or below for 0.5-3 hours, and then raising the temperature to room temperature; and a recrystallization step of heating the cryo-treated cast steel product to 800-1100°C and holding the temperature for 0.5-5 hours.
Citation Information
Patent Citations
Parts for precise device and its manufacture, and precise device using the same
JP1998237595A
Fe-ni-co alloy for electron gun parts, electron gun press punched work piece and electron gun electrode
JP1999269616A
High tensile steel material and its manufacturing method
JP2005113249A
High-rigidity low-thermal expansion casting and method for producing the same
JP2016027187A
Low thermal expansion alloy