Manufacturing method of portland cement clinker

By incorporating waste concrete materials and adjusting the MgO content in the cement clinker production process, the method addresses energy consumption and environmental concerns, enhancing initial strength development and reducing CO2 emissions while utilizing waste materials effectively.

WO2024219334A1PCT designated stage expired Publication Date: 2024-10-24TOKUYAMA CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014824
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-18
Filing Date
2024-04-12
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

The cement industry faces challenges in reducing energy consumption and environmental impact due to high clinker firing temperatures and the limited use of waste materials, particularly with conventional Portland cement clinker, which also affects initial strength development.

Method used

A method for producing cement clinker that utilizes waste concrete materials as raw materials, adjusts the MgO content to 1.1 to 1.5 mass%, and maintains a total AF content of 22 mass% or more, allowing for firing at lower temperatures while enhancing initial strength development.

Benefits of technology

This approach enables the effective use of waste materials, reduces energy consumption, and improves initial strength development of cement clinker, while minimizing CO2 emissions by using waste concrete as a substitute for limestone, thereby achieving better physical properties and reduced limestone usage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014824_24102024_PF_FP_ABST
    Figure JP2024014824_24102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a manufacturing method of a cement clinker, the method being capable of reducing a firing temperature in manufacturing and providing a product that exhibits excellent initial strength development even when containing MgO, while regulating CO2 emission. This method uses a waste concrete material as a part of a starting material. The starting material is conditioned so that the total amount of C3A and C4AF is 22 mass% or more and the amount of C3S is 60 mass% or more when calculated by the Bogue formula, the iron modulus (I.M.) is 1.3 or less, and the MgO content is 1.1-1.5 mass%. This starting material is fired at 1,300-1,400 °C to give a Portland cement clinker. 
Need to check novelty before this filing date? Find Prior Art

Description

Portland cement clinker manufacturing method

[0001] The present invention relates to a method for producing cement clinker. More specifically, the present invention relates to a method for producing cement clinker that can be fired at a lower temperature than conventional methods, that allows for the effective use of waste concrete materials, and that exhibits good early strength development.

[0002] The cement industry is a mass production and mass consumption industry, and in recent years, 2 Resource and energy conservation has become a top priority due to environmental issues such as emissions. For example, Portland cement, which is the most mass-produced cement, requires raw materials adjusted to a specific chemical composition to be burned at high temperatures of 1450 to 1550°C to produce clinker, and the burning process is the most energy-intensive process. In other words, if the burning temperature of clinker can be reduced, it will lead to energy savings. To reduce the burning temperature of clinker, it is necessary to reduce the C, the main mineral in clinker. 4 AF(4CaO・Al 2 O 3 Fe 2 O 3 A technology for increasing the C 4 By increasing AF, the molten phase increases, and the presence of the liquid phase increases C 2 S(2CaO・SiO 2 ) to C 3 S(3CaO・SiO 2 Since the reaction of producing minerals such as solid-state reactions that convert clinker into slag is promoted, the burning temperature of the clinker can be reduced.

[0003] In addition, from the viewpoint of resource circulation, the effective use of waste and by-products is an important issue. Taking advantage of the characteristics of the cement industry and cement manufacturing facilities, the effective use or treatment of waste as raw materials or thermal energy sources during cement manufacturing is considered effective from the viewpoint of safe and large-scale disposal. Waste and by-products are Al 2 O 3 Many of them have a high content of C 4 In the system for increasing AF, the Al content of the cement clinker 2 O 3Since the content is higher than that of conventional Portland cement clinker, it becomes possible to use more waste and by-products than with conventional Portland cement clinker. In this respect, the clinker described in Patent Document 1 is also superior.

[0004] C among clinker minerals 3 A (3CaO.Al 2 O 3 ) and C 4 Clinker with a high AF content has Al 2 O 3 This is advantageous in that a large amount of such waste can be used.

[0005] On the other hand, by utilizing waste and by-products, the components contained in the waste and by-products are brought into cement clinker. CaO, SiO, which are the main components of cement clinker, 2 , Al 2 O 3 , Fe 2 O 3 In addition, other minor components also affect the clinker's burnability, actual mineral composition, and cement properties, so appropriate management of minor components is required. For example, Patent Document 1 discloses that the clinker described therein shows a tendency for the initial strength development up to 7 days of age to decrease as the MgO content increases (Non-Patent Document 1).

[0006] JP 2012-224504 A

[0007] Masami Ota et al., Abstracts of the 74th Cement Technology Conference, pp. 114-115 (2020)

[0008] The clinker described in Patent Document 1 can be burned at a low temperature and contains Al 2 O 3 and Fe 2 O 3 However, as described in Non-Patent Document 1, an increase in the MgO content may reduce the initial strength development, potentially limiting its use. Therefore, an object of the present invention is to provide a method for producing clinker that has good initial cement strength development even when it contains MgO.

[0009] The present inventors have conducted extensive research to solve the above problems, and have found that by using waste concrete material as part of the clinker raw material with the above composition and adjusting the MgO content to 1.1 to 1.5 mass%, a better early strength development is achieved than in the case of a clinker with a conventional MgO content, leading to the completion of the present invention. 3 A and C 4 The total amount of AF is 22 mass% or more, C 3 This method for producing cement clinker involves blending raw materials so that the S content is 60 mass% or more, the iron content (I.M.) is 1.3 or less, and the MgO content is 1.1 to 1.5 mass%, and then firing the mixture at 1300 to 1400°C. In this specification, when a range is indicated by "to", such as "1.1 to 1.5 mass%, the range includes both the upper and lower limits.

[0010] According to the present invention, it is possible to obtain a clinker that can be fired at a lower temperature than conventional cement clinkers, that can effectively utilize waste concrete materials, and that exhibits better early strength development (after 7 days of age) than clinkers with a conventional MgO content. Furthermore, the present invention allows waste concrete materials to be used as part of the cement clinker raw materials and to replace the CaO source made from limestone. This allows the amount of limestone in the cement clinker raw materials to be reduced, thereby reducing the amount of CO2 generated from the raw materials during the firing of the cement clinker.

[0011] In this specification, waste concrete material refers to, for example, ready-mixed concrete sludge, returned concrete, residual concrete, waste concrete, etc., and may also include waste mortar. When generated, waste concrete material contains aggregates such as sand and gravel, but it is preferable to remove the aggregates by crushing and sieving. This is because the aggregate contains, for example, between 3 mass% and 6 mass% NaO and KO in total, and by using components derived from cement clinker in the waste concrete material, more waste concrete material can be used in place of limestone in the cement clinker raw material, thereby reducing the amount of CO2 generated from the raw materials. After crushing, the waste concrete material may also be used without sieving.

[0012] The MgO concentration of fresh concrete sludge is, for example, between 2 and 4 mass%, while the MgO concentration of aggregate is, for example, between 1 and 3 mass%. The MgO concentration of waste concrete material is somewhere between these two values. The MgO concentration of ordinary Portland cement clinker is, for example, about 0.9 mass%, and the high MgO concentration of waste concrete material is due to the inclusion of components derived from blast furnace cement, which contains a large amount of MgO, in the waste concrete material, as well as MgO derived from the aggregate. According to the inventor's experience, when waste concrete is crushed and then classified using a sieve, the under-sieve component of a 1.2 mm sieve has a higher MgO concentration than the under-sieve component of a 5 mm sieve.

[0013] C in the Portland cement clinker (hereinafter simply referred to as "cement clinker") produced by the production method of the present invention 3 A, C 4 AF and C 3 The amount of S is determined by the Bogue formula.

[0014] The Bogue formula is used alongside coefficients and ratios to calculate the approximate composition of major compounds using major chemical analysis values, and is well known to those skilled in the art. However, just to be sure, the method for calculating the amount of each mineral in cement clinker using the Bogue formula is described below. 3 S amount = (4.07 x CaO) - (7.60 x SiO 2) - (6.72 x Al 2 O 3 ) - (1.43 x Fe 2 O 3 ) C 2 S amount = (2.87×SiO 2 ) - (0.754 x C 3 S) C 3 A amount = (2.65×Al 2 O 3 ) - (1.69 x Fe 2 O 3 ) C 4 AF amount = 3.04×Fe 2 O 3

[0015] The iron ratio (I.M.), along with the hydraulic ratio (H.M.), silica ratio (S.M.), activity index (A.I.), and lime saturation (LSD), is calculated using the values ​​of the main chemical components and is used as one of the number of times and ratios as a characteristic value for managing cement clinker production. It is a coefficient well known to those skilled in the art, but just to be sure, the calculation method for the iron ratio will be listed below along with other coefficient values. Hydraulic ratio (H.M.) = CaO / (SiO 2 +Al 2 O 3 +Fe 2 O 3 ) Silicate ratio (S.M.) = SiO 2 / (Al 2 O 3 +Fe 2 O 3 ) Iron rate (I.M.) = Al 2 O 3 / Fe 2 O 3 Activity Coefficient (A.I.) = SiO 2 / Al 2 O 3 Lime saturation (L.S.D.) = CaO / (2.8×SiO 2 +1.2 x Al 2 O 3 +0.65 x Fe 2 O 3 )

[0016] In addition, "CaO" and "SiO 2 ", "Al 2O 3 " and "Fe 2 O 3 " can be measured by a method conforming to JIS R 5202 "Chemical analysis method for Portland cement" or JIS R 5204 "Fluorescence X-ray analysis method for cement", respectively.

[0017] As described above, in the present invention, the C of cement clinker 3 A, C 4 The total amount of AF must be 22 mass% or more. If these amounts are less than 22 mass%, it becomes difficult to obtain cement clinker with good physical properties such as strength development by firing at a low temperature. A more preferable total amount is 24 mass% or more. As will be described later, in order to obtain high strength development, C 3 S must be 60 mass% or more. 3 A and C 4 The upper limit of the total amount of AF is 40 mass%, preferably 35 mass% or less, more preferably 32 mass% or less, and particularly preferably 28 mass% or less. 4 AF is preferably present alone in an amount of 15 mass% or more, since it allows sufficient sintering even at low temperatures and reduces the amount of f-CaO in the cement clinker.

[0018] C 3 The amount of S is extremely important for the strength development of a cement composition (hereinafter simply referred to as "cement") using the cement clinker obtained by the present invention. If this amount is less than 60%, the C 3 A and C 4 Even if the total amount of AF and the iron content described later are within the specified ranges, good strength development cannot be obtained. 3 The amount of S is preferably 62 mass% or more, and particularly preferably 63 mass% or more. 3 A and C 4 Since the total amount of AF is at least 22%, C 3 The upper limit of the amount of S is 78%. In order to ensure a certain amount of time from the start to the end of coagulation, the amount of S is preferably 70% by mass or less, and more preferably 65% ​​by mass or less.

[0019] In the present invention, the cement clinker further contains C 2 S may be contained. The amount of S is preferably 18 mass% or less and 3 mass% or more. From the viewpoint of obtaining long-term strength, C is particularly preferable. 3 The total amount of S and the amount of C is 69 mass% or more.

[0020] In the present invention, the iron ratio (I.M.) of the cement clinker is 1.3 or less. If the iron ratio exceeds 1.3, sufficient strength development (more specifically, mortar strength development, for example) cannot be obtained even if the other requirements of the resulting cement clinker are satisfied. Furthermore, if the iron ratio exceeds 1.3, the time from the start to the end of setting tends to become too long, and for this reason too, the iron ratio is set to 1.3 or less. A more preferable range of the iron ratio is 1.0 to 1.3, and particularly preferably 1.14 to 1.27.

[0021] The hydraulic ratio and silicic acid ratio are not particularly limited, but in order to obtain an excellent balance of various physical properties, the hydraulic ratio is preferably 1.8 to 2.2, more preferably 1.9 to 2.1, and the silicic acid ratio is preferably 1.0 to 2.0, more preferably 1.1 to 1.7.

[0022] The most important aspect of this invention is that waste concrete materials are used as part of the raw materials, resulting in an MgO content of 1.1 to 1.5 mass%. Examples of waste concrete materials include ready-mixed concrete sludge, returned concrete, residual concrete, waste concrete, and waste mortar. These materials may be used alone or in combination of two or more. Ready-mixed concrete sludge is obtained by separating ready-mixed concrete recovered by washing a concrete mixer truck into sludge primarily composed of aggregate and cement, and then subjecting the solids in the sludge to solid-liquid separation. Returned concrete refers to ready-mixed concrete that is returned to a construction site without being used. Residual concrete includes returned concrete and is a general term for concrete that was not used due to reasons such as failure to pass inspection or excessive production. Waste concrete refers to discarded concrete resulting from the demolition of a building.

[0023] The waste concrete material is a mixture of conventional cement raw materials (CaO source such as limestone, SiO source such as silica stone, etc.) 2 Al from sources, clay, etc. 2 O 3 Fe source, iron source, etc. 2 O 3 It has the characteristic of having a higher MgO content than waste concrete materials (such as blast furnace cement). This is presumably due to the inclusion of components derived from blast furnace cement in waste concrete materials and the fact that concrete aggregates contain a large amount of MgO. The MgO content in cement clinker can be measured using methods conforming to JIS R 5202 "Chemical analysis of Portland cement" and JIS R 5204 "X-ray fluorescence analysis of cement," etc.

[0024] Furthermore, limestone (calcium carbonate), which is used as a CaO raw material in the production of cement clinker, emits carbon dioxide when burned. However, the waste concrete material used in the present invention contains calcium oxide, which can be used as a CaO raw material. Therefore, by using the waste concrete material, the amount of limestone used, which causes carbon dioxide emissions, can be reduced, and carbon dioxide emissions during the production of cement clinker can be suppressed.

[0025] When cement clinker with the above composition is prepared using general raw materials that do not contain waste concrete material, the resulting cement clinker contains a maximum of approximately 0.90 mass% MgO. In contrast, although the mechanism is unclear, by using waste concrete material as part of the raw materials and adjusting the MgO content to 1.1 to 1.5 mass%, the cement clinker exhibits better early strength development than cement clinker with a conventional MgO content. Adjusting the MgO content using something other than waste concrete material, such as a reagent, does not exhibit good early strength development. Because an increased MgO content promotes the effective use of waste concrete material, a more preferred MgO content is 1.2 to 1.5 mass%, with a particularly preferred MgO content being 1.35 to 1.50 mass%.

[0026] As described above, the cement clinker containing a large amount of MgO obtained by using waste concrete material as part of the raw materials according to the present invention has the characteristic of exhibiting better initial strength development than cement clinker having a conventional level of MgO content.

[0027] Preferably, the waste concrete material is added to the raw materials so that the content of MgO derived from the waste concrete material in the Portland cement clinker after firing is 0.25 mass % or more and 1.0 mass % or less.

[0028] Preferably, the waste concrete material is added to the raw material at a concentration of 10 mass % or more and 30 mass % or less.

[0029] According to the present invention, it is possible to produce clinker by firing at a lower temperature than conventional ordinary Portland cement clinker. That is, conventional ordinary Portland cement clinker requires a temperature of around 1450°C for firing, but according to the present invention, cement clinker can be obtained by firing at a temperature of 1300 to 1400°C.

[0030] The method for producing cement clinker in the present invention is not particularly limited except that waste concrete material is used as part of the raw materials and the raw materials are mixed so as to achieve the above-mentioned specific mineral ratios and coefficients. Similar to known cement (clinker) raw materials, the cement clinker can be obtained by preparing and mixing waste concrete material in predetermined proportions so as to achieve the above-mentioned mineral ratios and coefficients, and then firing it in an SP kiln, NSP kiln, or the like.

[0031] The cement raw materials may be prepared and mixed by a known method. For example, waste materials, by-products, and other raw materials (CaO sources such as limestone, quicklime, and slaked lime, SiO sources such as silica stone) may be prepared in advance. 2 Al from sources, clay, etc. 2 O 3 Fe source, iron source, etc. 2 O 3 The composition of the waste concrete material and the waste concrete material is measured, and the mixing ratio of each raw material is calculated from the proportion of each component in these raw materials so that the ratio falls within the above range, and the raw materials are mixed in that ratio.

[0032] The raw materials used in the production of the cement clinker of the present invention are the same as those used in the production of conventional cement clinker, and are not particularly limited. Of course, waste materials, by-products, etc. can also be used.

[0033] In the production of the cement clinker used in the present invention, it is preferable to use one or more waste materials, by-products, etc., from the viewpoint of promoting the effective utilization of waste materials, by-products, etc. Specific examples of usable waste materials and by-products include blast furnace slag, steelmaking slag, non-ferrous slag, coal ash, sewage sludge, water purification sludge, papermaking sludge, construction waste soil, foundry sand, soot and dust, incineration fly ash, molten fly ash, chlorine bypass dust, wood chips, waste clay, slag, waste tires, shells, municipal waste and its incineration ash (some of these can be used as both a cement raw material and a thermal energy source).

[0034] Coal ash contains, for example, 1 mass % to 2 mass % of MgO. 2 O 3 Because of its high concentration, adding a large amount makes it difficult to maintain the composition of cement clinker within the specified range. 2 Therefore, in the present invention, the MgO concentration in cement clinker is controlled mainly by using waste concrete materials.

[0035] In particular, the cement clinker of the present invention is 3 A and C 4 AF Al 2 O 3 Therefore, compared to conventional cement clinker, it contains a lot of minerals whose constituent elements are Al. 2 O 3 This has the advantage that it can be produced using a larger amount of waste and by-products that are rich in minerals.

[0036] The MgO content in cement clinker can be adjusted by analyzing the above-mentioned waste, by-products, natural raw materials, and waste concrete materials, and adjusting the blending ratio of each raw material so that the above-mentioned specified MgO content is achieved. The Mg component contained in the raw materials is present in the form of oxide, composite oxide, or in some cases magnesium alloy or metallic magnesium, which is almost non-volatile at the clinker firing temperature. Therefore, calculations to determine the blending ratio can be performed assuming that the entire amount of Mg component contained in the raw materials is transferred to the clinker. If it is known that there is Mg component that volatilizes during the raw material crushing process or the firing process and does not transfer to the clinker, this amount must be taken into account in the calculation.

[0037] The cement clinker of the present invention can be made into cement by crushing it together with gypsum or crushing it separately and then mixing it, just like conventionally known cement clinkers. Examples of such cement include ordinary Portland cement, high-early-strength Portland cement, and ultra-high-early-strength Portland cement. In addition to being used as Portland cement, it can also be used as a component of various blended cements and solidifying materials such as soil solidifying materials.

[0038] When gypsum is added to prepare a cement composition, the gypsum used may be any known gypsum used as a raw material for cement production, such as gypsum dihydrate, gypsum hemihydrate, anhydrous gypsum, etc., without any particular limitation. In the case of Portland cement, the amount of gypsum added is determined by the amount of SO 3 It is preferable to add it so that the amount is 1.5 to 5.0 mass%, and more preferably 1.8 to 3 mass%. As for the method for crushing the cement clinker and gypsum, known techniques can be used without particular limitation.

[0039] The cement composition may be mixed and ground with an appropriate admixture or grinding aid, such as blast furnace slag, siliceous admixture, fly ash, calcium carbonate, or limestone, or may be mixed with the admixture after grinding. Chlorine bypass dust or the like may also be mixed.

[0040] The fineness of the cement composition is not particularly limited, but the Blaine specific surface area is preferably 2800 to 4500 cm2 It is preferable that the SiO2 content is adjusted to 1 / g.

[0041] Furthermore, if necessary, after pulverization, blast furnace slag, fly ash, etc. can be mixed to produce blast furnace slag cement, fly ash cement, etc.

[0042] 1 is a characteristic diagram showing the relationship between the MgO concentration in cement clinker and the compressive strength of mortar in the examples.

[0043] The configuration and effects of the present invention will be explained below using examples, but the present invention is not limited to these examples.

[0044] (Reference Example, Comparative Example 1, Examples 1-3) Raw materials were prepared using industrial raw materials, including waste (limestone, silica, coal ash, and kalami (iron slag)), and raw concrete sludge from waste concrete. The raw materials were then calcined at 1,360°C for 100 minutes to obtain cement clinker. The raw concrete sludge was collected at a ready-mix concrete plant, where aggregate was separated from the returned concrete and dehydrated using a filter press. The sample was then immediately dried to bone dryness before use. Table 1 shows the chemical composition of the raw concrete sludge used after heating to 1,000°C. Table 2 shows the blending ratio (mass%) of the raw concrete sludge to the raw materials and the chemical composition (mass%) of the clinker obtained after calcination. Table 3 shows the mineral composition (mass%) calculated by the Bogue method, as well as coefficients and ratios. Because the mineral composition calculated by the Bogue method ignores impurities, the total is slightly less than 100% by mass.

[0045] 100 parts by mass of this cement clinker was mixed with 2.2 parts by mass of gypsum dihydrate and 1.8 parts by mass of gypsum hemihydrate to obtain a Blaine specific surface area of ​​3200±100 cm 2 The mortar compressive strength of each cement was calculated as 100% by pulverizing the clinker to a value of 1 / g, and the resulting cement was crushed to a value of 1 / g. The mortar compressive strength of each cement is shown in Table 4 and Figure 1 as a mortar compressive strength (%), relative to the mortar compressive strength of a cement produced using a reference cement clinker obtained without using the waste concrete material, fresh concrete sludge, and without adjusting the MgO content. The various measurement methods were as follows.

[0046] As is clear from Table 4 and Figure 1, by adjusting the MgO concentration in cement clinker to 1.1 mass% or more and 1.5 mass% or less, the early compressive strength of mortar at 3 and 7 days of age increased. There was a large difference in the early compressive strength of mortar between MgO concentrations of 1.03 mass% and 1.16 mass%. Adding MgO as a reagent did not improve the early strength.

[0047] (1) Measurement of MgO and other chemical compositions of raw materials and cement clinker: Measured by fluorescent X-ray analysis in accordance with JIS R 5204. (2) Measurement of mortar compressive strength: Measured by a method in accordance with JIS R 5201.

[0048]

[0049] (Comparative Example 2) To adjust the MgO content, a special grade reagent (MgO) was used instead of fresh concrete sludge from waste concrete material, and tests were conducted in the same manner as in Comparative Example 1 and Examples 1 to 3. Table 2 shows the chemical composition of the clinker obtained after burning, and Table 3 shows the mineral composition, coefficients, and ratios according to the Bogue method. Table 4 also shows the compressive strength (%) of cement mortar.

[0050]

[0051]

[0052]

[0053] The Reference Example is a cement clinker obtained without using ready-mixed concrete sludge, which is a waste concrete material, and without adjusting the MgO content. The MgO content is 0.90 mass%, which is the same as the conventional content. In other words, the results of each Example and Comparative Example will be discussed based on the results of this Reference Example.

[0054] In Comparative Example 1, the MgO content was less than 1.1 mass %, and it was found that the compressive strength of the mortar up to 7 days after the age was approximately the same as that of the Reference Example.

[0055] Although Examples 1 to 3 are based on the present invention and have a higher MgO content than conventional examples, the initial compressive strength of the mortar up to 7 days after application exceeds that of the Reference Example. It is also clear that this does not affect the compressive strength of the mortar after 28 days.

[0056] In Comparative Example 2, no waste concrete material was used, but instead special-grade reagent MgO was used, with the MgO content being within the range of 1.1 to 1.5 mass%. The compressive strength of the mortar at an age of 3 days was comparable to that of the Reference Example, but the compressive strength of the mortar at an age of 7 days was lower than that of the Reference Example. Therefore, it can be seen that when a special-grade reagent is used to adjust the MgO content to the range of the present invention, the same effect as that of the present invention is not exhibited in terms of initial strength development.

Claims

1. C calculated by the Borg formula 3 A and C 4 The total amount of AF is 22 mass% or more, C 3 A method for producing Portland cement clinker by firing a raw material having an S content of 60 mass% or more and an iron content (I.M.) of 1.3 or less at 1300°C to 1400°C, characterized in that waste concrete material is added to the raw material as an MgO source, thereby making the MgO content of the Portland cement clinker after firing 1.1 mass% to 1.5 mass%.

2. The method for producing Portland cement clinker according to claim 1, wherein the waste concrete material is at least one member selected from the group consisting of ready-mixed concrete sludge, returned concrete, residual concrete, waste concrete, and waste mortar.

3. C 4 3. The method for producing Portland cement clinker according to claim 1 or 2, wherein the AF content is 15 mass% or more.

4. C 3 S and C 2 2. The method for producing Portland cement clinker according to claim 1, wherein the total amount of S is 69 mass% or more.

5. A method for producing Portland cement clinker according to claim 1, characterized in that gypsum is added to the Portland cement clinker after burning.

6. A method for producing Portland cement clinker according to claim 5, characterized in that at least one admixture selected from the group consisting of blast furnace slag, siliceous admixtures, fly ash and limestone is further added to the Portland cement clinker after burning.

7. A method for producing Portland cement clinker according to claim 1 or 2, characterized in that waste concrete material is added to the raw materials so that the content of MgO derived from the waste concrete material in the Portland cement clinker after firing is 0.25 mass% or more and 1.0 mass% or less.

8. A method for producing Portland cement clinker according to claim 7, characterized in that waste concrete material is added to the raw materials in a concentration of 10 mass% to 30 mass%.

Citation Information

Patent Citations

  • Cement clinker

    JP2012224504A

  • Treatment of concrete waste material

    JP1994285454A

  • Artificial lightweight aggregate and its production

    JP1998152356A

  • Method of producing hydraulic material utilizing concrete scrap