Copolyamide resin, and composition, molded article, film and monofilament containing same
The copolyamide resin, formulated with biomass-derived structural units, addresses the issues of high enthalpy change and crystallinity in traditional polyamide resins, achieving improved transparency and handleability, and aligns with sustainable development goals by using renewable resources.
Patent Information
- Application Number
- PCT/JP2024/014944
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2024-04-15
- Publication Date
- 2024-10-24
AI Technical Summary
Molded products using traditional polyamide resins derived from fossil materials often exhibit high enthalpy change upon melting, high crystallinity, and poor transparency, which are not suitable for applications requiring mechanical properties and aesthetic quality.
A copolyamide resin is developed using biomass-derived raw materials, specifically structural units derived from pentamethylene diamine and adipic acid/sebacic acid, with a mass ratio of 85/15 to 15/85, which reduces enthalpy change, crystallinity, and improves transparency through melt polymerization or other known polymerization methods.
The resulting copolyamide resin offers improved transparency, reduced crystallinity, and enhanced handleability, making it suitable for various applications while contributing to sustainable development by utilizing biomass-derived materials.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Copolymerized polyamide resin, and composition, molded article, film, and monofilament containing the same
[0001] The present invention relates to a copolyamide resin, and particularly to a copolyamide resin using a raw material derived from biomass.
[0002] Polyamides are polymers formed by assembling structural units containing amide bonds. The structural units of polyamides are generally derived from aminocarboxylic acids or lactams, or diamines and dicarboxylic acids. In particular, aliphatic polyamide resins derived from aliphatic species of these compounds have versatile and beneficial properties as resins, such as chemical resistance, toughness, heat resistance, and oil resistance. Therefore, aliphatic polyamide resins are useful as raw materials for molded products in a variety of applications. For example, they are used as substrates for monolayer or laminate films, particularly in packaging films that require pinhole resistance and gas barrier properties, particularly in the food packaging field, and as structural materials for multilayer films coextruded with other resins.
[0003] One of the advantages of resins is that their properties can be controlled in various ways by selecting the monomer or by using multiple types of monomers. Copolymer polyamide resins are produced by combining two or more types of structural units to give molded articles with properties suited to their intended use (Patent Document 1).
[0004] Polyamide resins provide molded products with excellent properties, and therefore are produced as homopolymers of various structural units or copolymers of combinations of structural units. However, many of the monomers used to produce polyamide resins are industrially derived from fossil fuels. For example, ε-caprolactam, a well-known raw material for Nylon (registered trademark), is synthesized from naphtha-derived benzene. With the recent rise in environmental awareness, which calls for the reduction of carbon dioxide emissions, there is a demand for a shift from fossil fuels to biomass-derived raw materials for polyamide resins. One known biomass-derived compound that can be used as a polyamide raw material is 1,5-pentanediamine, which can be obtained from starch or sugarcane through enzyme reactions, yeast reactions, fermentation reactions, and the like. Patent Document 2 attempts to produce polyamide resins with fewer biomass-derived impurities using 1,5-pentanediamine as a raw material. Patent Documents 3 and 4 attempt to produce polyamide resins for large molded products using 1,5-pentanediamine as a raw material, with improved thermal retention stability, etc.
[0005] International Publication No. 2022 / 071013 International Publication No. 2015 / 076233 JP 2006-348057 A JP 2007-332353 A
[0006] The replacement of conventional products with resins derived from biomass raw materials is one of the global efforts to build a sustainable society, and in Japan too, there are efforts to establish legislation such as setting certain standards for the content of bio-based polymers, establishing recycling processes, and reducing CO2 emissions. 2 Demonstration experiments are underway to achieve this. However, replacing raw resin materials often involves changes to the molecular structure of the resin, which inevitably leads to changes in physical properties. Consumers are highly concerned about the quality of resins, along with the price, and there is a strong demand for resins that are of equal or higher quality than the resins they are replacing.
[0007] The molded articles using the polyamide resins described in Patent Documents 1 to 4 exhibit certain mechanical properties (tensile modulus, tensile elongation, etc.), but have the problem of a high enthalpy change ΔH accompanying melting of the resin and poor transparency.
[0008] Therefore, an object of the present invention is to provide a copolymer polyamide resin that has a low enthalpy change ΔH upon melting, has a low degree of crystallinity and therefore excellent transparency, and is made using raw materials derived from biomass, as well as a composition containing the same and molded articles such as films and monofilaments.
[0009] The present invention relates to the following [1] to [7]: [1] A structural unit A represented by the following formula (A) derived from a reaction product of equimolar amounts of pentamethylenediamine and adipic acid: and structural unit B derived from a reaction product of equimolar amounts of pentamethylenediamine and sebacic acid, represented by the following formula (B): [2] The copolymer polyamide resin according to [1], wherein the copolymer polyamide resin has a melting point of 170 to 240°C as measured by DSC. [3] The copolymer polyamide resin according to [1] or [2], wherein the copolymer polyamide resin has a crystallization temperature of 115 to 195°C as measured by DSC. [4] A polyamide resin composition comprising the copolymer polyamide resin according to any one of [1] to [3]. [5] A molded article comprising the copolymer polyamide resin according to any one of [1] to [3]. [6] A film comprising the copolymer polyamide resin according to any one of [1] to [3]. [7] A monofilament comprising the copolymer polyamide resin according to any one of [1] to [3].
[0010] According to the present invention, it is possible to provide a copolymer polyamide resin which has a low enthalpy change ΔH upon melting, a low degree of crystallinity and therefore excellent transparency, and which uses a biomass-derived raw material, as well as a composition containing the same and a molded article such as a film or monofilament.
[0011] In the present invention, the polyamide resin refers to a resin having an acid amide bond (-CONH-) in the main chain and obtained by polymerizing or copolymerizing a lactam, an aminocarboxylic acid, or a nylon salt composed of a diamine and a dicarboxylic acid as a raw material by a known method such as melt polymerization, solution polymerization, or solid-state polymerization. As long as the effects of the present invention are not impaired, other components may be blended with the polyamide resin to form a polyamide resin composition.
[0012] The copolymerized polyamide resin of the present invention comprises a structural unit A derived from a reaction product of equimolar amounts of pentamethylenediamine and adipic acid, represented by the following formula (A): and structural unit B derived from a reaction product of equimolar amounts of pentamethylenediamine and sebacic acid, represented by the following formula (B): and the mass ratio of structural unit A / structural unit B is 85 / 15 to 15 / 85. By including structural units A and B in the copolymerized polyamide resin in the above ratio, it is possible to increase the bio content while lowering the enthalpy change ΔH associated with melting, thereby decreasing the degree of crystallinity and improving transparency.
[0013] [Structural Unit A] Structural unit A is a unit derived from the equimolar reaction product of pentamethylenediamine and adipic acid, as represented by the above formula (A). Structural unit A is formed by polymerizing an equimolar salt or equimolar mixture of pentamethylenediamine and adipic acid. The pentamethylenediamine and adipic acid that constitute this unit may be condensed directly or via another unit or a diamine or dicarboxylic acid that constitutes another unit. By including structural unit A, the copolymerized polyamide resin can shorten the time until solidification during heat molding, improve handleability and work efficiency, and increase the bio content.
[0014] Examples of pentamethylenediamines include 1,5-pentamethylenediamine, 1,4-pentamethylenediamine, and 1,3-pentamethylenediamine, but 1,5-pentamethylenediamine is preferred from the viewpoints of availability and the strength of the resulting polyamide resin. Pentamethylenediamines may be used alone or in combination of two or more.
[0015] Pentamethylenediamine may be derived from a fossil raw material or a biomass-derived raw material, but from the viewpoint of increasing the bio content of the copolyamide resin, it is preferably a biomass-derived raw material. Examples of biomass-derived pentamethylenediamine include WO 2015 / 076233, JP 2006-348057, JP 2007-332353, JP 2002-223771, JP 2004-000114, JP 2004-208646, JP 2004-290091, JP 2004-298034, JP 2002-223770, JP 2004-222569, JP 2005-6650, JP 2019-154313, and JP 2019-205423. Those obtained by the production methods disclosed in such publications can be used.
[0016] Specifically, it is known that 1,5-pentamethylenediamine can be produced by decarboxylating lysine through an enzymatic reaction, and 1,5-pentamethylenediamine can be produced from lysine using, for example, lysine decarboxylase, cells producing lysine decarboxylase, a processed product of the cells, a microorganism expressing lysine decarboxylase, etc. Alternatively, the enzymatic decarboxylation of lysine can be carried out while adding an acid such as adipic acid to the lysine solution so as to maintain a pH suitable for the enzymatic decarboxylation.
[0017] Adipic acid may be derived from a fossil raw material or a biomass-derived raw material, but from the viewpoint of availability, adipic acid is preferably derived from a fossil raw material.
[0018] [Structural Unit B] Structural unit B is a unit derived from the reaction product of equimolar amounts of pentamethylenediamine and sebacic acid, as represented by the above formula (B). Structural unit B is formed by polymerizing an equimolar salt or equimolar mixture of pentamethylenediamine and sebacic acid. The pentamethylenediamine and sebacic acid that constitute this unit may be condensed directly or via another unit or a diamine or dicarboxylic acid that constitutes another unit. By including structural unit B in a copolymerized polyamide resin, the water absorption of the molded article can be reduced while increasing the bio content.
[0019] Examples of pentamethylenediamine include the same ones as those exemplified for the structural unit A, and preferred embodiments are also the same.
[0020] Sebacic acid may be derived from fossil fuels or biomass, but is preferably derived from biomass in order to increase the bio content of the copolymerized polyamide resin. Biomass-derived sebacic acid can be synthesized, for example, from ricinoleic acid triglyceride, which is the main component of castor oil obtained from castor bean seeds.
[0021] [Mass Ratio of Structural Unit A and Structural Unit B] The mass ratio of structural unit A / structural unit B in the copolymerized polyamide resin is 85 / 15 to 15 / 85, preferably 80 / 20 to 20 / 80, more preferably 70 / 30 to 25 / 75, even more preferably 60 / 40 to 30 / 70, and particularly preferably 55 / 45 to 35 / 65. By setting the mass ratio of structural unit A / structural unit B to 15 / 85 or more, the time until solidification during heat molding is shortened, improving handleability and work efficiency, and the transparency of the molded article is also improved. By setting the mass ratio to 85 / 15 or less, the water absorption of the molded article is reduced and transparency is improved.
[0022] The total amount of the structural unit A and the structural unit B is preferably 80 to 100% by mass, more preferably 90 to 100% by mass, and even more preferably 95 to 100% by mass, relative to 100% by mass of the copolymerized polyamide resin. In one embodiment, the total amount of the structural unit A and the structural unit B is 100% by mass, relative to 100% by mass of the copolymerized polyamide resin.
[0023] [Other Structural Units] As long as the copolymerized polyamide resin does not impair its properties, it may contain structural units other than structural unit A and structural unit B. Examples of such structural units include structural units derived from a reaction product of equimolar amounts of pentamethylenediamine with a dicarboxylic acid other than adipic acid and sebacic acid; structural units derived from a reaction product of equimolar amounts of a diamine other than pentamethylenediamine with adipic acid or sebacic acid; structural units derived from a reaction product of equimolar amounts of a diamine other than pentamethylenediamine with a dicarboxylic acid other than adipic acid and sebacic acid; and structural units derived from aminocarboxylic acids and / or lactams.
[0024] Examples of diamines other than pentamethylenediamine include ethylenediamine, trimethylenediamine, tetramethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, tridecanediamine, tetradecanediamine, pentadecanediamine, hexadecanediamine, heptadecanediamine, octadecanediamine, nonadecanediamine, eicosanediamine, 2-methyl-1,8-octanediamine, and 2,2,4 / 2,4,4-trimethylhexamethylenediamine. Aliphatic diamines; alicyclic diamines such as 1,3- / 1,4-cyclohexyldiamine, bis(4-aminocyclohexyl)methane, bis(4-aminocyclohexyl)propane, bis(3-methyl-4-aminocyclohexyl)methane, bis(3-methyl-4-aminocyclohexyl)propane, 1,3- / 1,4-bisaminomethylcyclohexane, 5-amino-2,2,4-trimethyl-1-cyclopentanemethylamine, 5-amino-1,3,3-trimethylcyclohexanemethylamine, bis(aminopropyl)piperazine, bis(aminoethyl)piperazine, and norbornanedimethylenediamine; and the like.
[0025] Examples of dicarboxylic acids other than adipic acid and sebacic acid include aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, pimelic acid, suberic acid, azelaic acid, undecanedioic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid, pentadecanedioic acid, hexadecanedioic acid, heptadecanedioic acid, octadecanedioic acid, nonadecanedioic acid, and eicosanedioic acid; and alicyclic dicarboxylic acids such as 1,3- / 1,4-cyclohexanedicarboxylic acid, dicyclohexanemethane-4,4'-dicarboxylic acid, and norbornanedicarboxylic acid.
[0026] Examples of aminocarboxylic acids include 6-aminocaproic acid, 7-aminoheptanoic acid, 9-aminononanoic acid, 10-aminodecanoic acid, 11-aminoundecanoic acid, 12-aminododecanoic acid, etc. Examples of lactams include ε-caprolactam, enantholactam, decalactam, undecalactam, dodecalactam, α-pyrrolidone, α-piperidone, etc.
[0027] The amount of each structural unit of the copolymerized polyamide resin corresponds to the amount of each component charged during the production of the copolymerized polyamide resin, but can also be determined by measuring the obtained copolymerized polyamide resin as is or after hydrolysis using high performance liquid chromatography, gas chromatography, gas chromatograph / atomic emission detector (GC / AED), gel permeation chromatography, etc. The amount of each structural unit of the copolymerized polyamide resin described in this specification and claims is calculated from the charge ratio (mass ratio) of the raw materials, assuming that all of the raw materials for the copolymerized polyamide resin have reacted. In the examples, taking into consideration that condensation water is lost during polymerization, the amount of each structural unit was calculated as follows: contribution of 1,5-pentamethylenediamine to a molecular weight of 102.18 = 100.18 (= 102.18 - 2.00) g / mol; contribution of adipic acid to a molecular weight of 146.14 = 112.14 (= 146.14 - 34.00) g / mol; and contribution of sebacic acid to a molecular weight of 202.25 = 168.25 (= 202.25 - 34.00) g / mol.
[0028] [Physical Properties of Copolymer Polyamide Resin] From the viewpoint of moldability, the melting point of the copolymer polyamide resin measured by differential scanning calorimetry (DSC) is preferably 170 to 240°C, more preferably 175 to 230°C, even more preferably 180 to 220°C, and particularly preferably 180 to 210°C. The melting point of the copolymer polyamide resin measured by DSC can be increased or decreased depending on the ratio of constituent units, the molecular weight of the copolymer polyamide resin, etc. Furthermore, from the viewpoint of the transparency of molded articles, the heat of fusion (enthalpy change accompanying melting) ΔH corresponding to the melting point is preferably 40 J / g or less, more preferably 1 to 40 J / g, even more preferably 5 to 40 J / g, even more preferably 5 to 30 J / g, and particularly preferably 5 to 20 J / g. In this specification, the melting point measured by DSC is the top temperature of the endothermic peak in the DSC curve in the second heating process when a copolymer polyamide resin is heated to 300°C at a rate of 10°C / min in a nitrogen gas atmosphere, held at that temperature for 1 minute, cooled to 30°C at a rate of 10°C / min, and then heated again to 300°C at a rate of 10°C / min. The heat of fusion corresponding to the melting point is calculated from the endothermic peak in the DSC curve in the second heating process.
[0029] From the viewpoint of moldability, the crystallization temperature of the copolymer polyamide resin measured by differential scanning calorimetry (DSC) is preferably 115 to 195°C, more preferably 115 to 170°C, even more preferably 115 to 160°C, and particularly preferably 115 to 150°C. The crystallization temperature of the copolymer polyamide resin measured by DSC can be increased or decreased depending on the ratio of constituent units, the molecular weight of the copolymer polyamide resin, etc. In this specification, the crystallization temperature measured by DSC is the top temperature of the exothermic peak in the DSC curve during the cooling process when the copolymer polyamide resin is heated to 300°C at a rate of 10°C / min in a nitrogen gas atmosphere, held at that temperature for 1 minute, and then cooled to 30°C at a rate of 10°C / min.
[0030] The copolyamide resin is preferably a random copolymer from the viewpoint of obtaining a preferable melting point and crystallization temperature. A random copolymer is a copolymer in which structural units A and B are arranged randomly. A copolyamide resin obtained by mixing and polymerizing each unit in the monomer state is usually a random copolymer. On the other hand, for example, a copolyamide resin obtained by mixing and further polymerizing polyamide resin A obtained by polymerizing a monomer that is the raw material for structural unit A and polyamide resin B obtained by polymerizing a monomer that is the raw material for structural unit B is usually not a random copolymer but a block copolymer. A block copolymer is a copolymer formed by polymerizing blocks in which a certain number of structural units A or structural units B are arranged consecutively. A random copolymer can be confirmed by a nuclear magnetic resonance spectrometer. 13 This can also be confirmed by examining the bonding probability of each structural unit from a C-NMR spectrum.
[0031] The biomass ratio of the copolyamide resin measured in accordance with ASTM D6866 is preferably 40% or more, more preferably 50% or more. The biomass ratio is determined by the radioactive carbon ( 14 Specifically, if all of the carbon in the copolyamide resin is derived from fossil raw materials, the biomass degree is 0%, and if all of the carbon is derived from biomass, the biomass degree is 100%.
[0032] The proportion (by mass) of biomass raw material in the copolyamide resin is preferably 40% or more, and more preferably 50% or more. The proportion of biomass raw material is the proportion of the amount (by mass) of biomass-derived raw materials charged in 100% by mass of the total amount of raw materials charged, assuming that all of the raw materials for the copolyamide resin have reacted. The upper limit of the proportion of biomass raw material is 100%, and can be, for example, 90% or less. When the biomass raw materials consist only of 1,5-pentamethylenediamine and sebacic acid, the proportion of biomass raw material is the proportion of the amounts of 1,5-pentamethylenediamine and sebacic acid charged in 100% by mass of the total amount of raw materials charged. In the examples, the proportion of biomass raw materials was calculated as follows: contribution of 1,5-pentamethylenediamine to a molecular weight of 102.18 = 100.18 (= 102.18 - 2.00) g / mol; contribution of adipic acid to a molecular weight of 146.14 = 112.14 (= 146.14 - 34.00) g / mol; contribution of sebacic acid to a molecular weight of 202.25 = 168.25 (= 202.25 - 34.00) g / mol.
[0033] [Method for producing copolymerized polyamide resin] For the production of copolymerized polyamide resin, known polymerization methods such as melt polymerization, solution polymerization, interfacial polymerization, solid-state polymerization, and combinations thereof can be used. Usually, melt polymerization carried out at a temperature higher than the melting point of the copolymerized polyamide resin to be obtained is preferably used. For the production of copolymerized polyamide resin, known polymerization equipment can be used, and the copolymerized polyamide resin can be produced by appropriately combining operations such as normal pressure, reduced pressure, and increased pressure in a batch or continuous manner as needed. For example, the monomer that is the raw material for structural unit A and the monomer that is the raw material for structural unit B can be introduced at the same time.
[0034] Furthermore, although not particularly limited, since copolymerized polyamide resins have high viscosity, in some cases, in order to avoid difficulties in extracting the resin during polymerization, it is possible to synthesize a copolymerized polyamide resin having low viscosity by melt polymerization, and then obtain a copolymerized polyamide resin having increased viscosity by solid-state polymerization.
[0035] [Uses of Copolymer Polyamide Resins] Copolymer polyamide resins can increase the bio content, which can contribute to achieving Goal 12 of the SDGs (Sustainable Development Goals), and when formed into molded articles, they have excellent transparency. Copolymer polyamide resins can be used for polyamide resin compositions and molded articles such as films and monofilaments.
[0036] <Polyamide Resin Composition> One aspect of the present invention is a polyamide resin composition containing a copolymerized polyamide resin. The polyamide resin composition may contain other components in addition to the copolymerized polyamide resin, provided that the effects of the present invention are not impaired. Examples of other components include polyamide resins other than copolymerized polyamide resins; any resin other than polyamide resins, such as modified or unmodified polyolefin resins; and functionality-imparting agents such as plasticizers, heat resistance agents, foaming agents, antioxidants, UV absorbers, weathering agents, crystal nucleating agents, crystallization accelerators, mold release agents, lubricants, antistatic agents, antifogging agents, flame retardants, flame retardant assistants, pigments, and dyes. The polyamide resin composition containing these other components can be formed into molded articles such as pellets, films, and monofilaments.
[0037] The method for producing the polyamide resin composition is not particularly limited, and the composition can be produced, for example, by mixing the copolymer polyamide resin and other components using a known melt kneader such as a single-screw or twin-screw extruder, a Banbury mixer, a kneader, or a mixing roll.
[0038] <Molded Article> One aspect of the present invention is a molded article containing a copolymer polyamide resin or a polyamide resin composition. The method for producing the molded article is not particularly limited, and examples include injection molding, press molding, blow molding, extrusion molding, and rotational molding.
[0039] (Uses of Molded Articles) Molded articles containing copolymerized polyamide resins or polyamide resin compositions take advantage of their excellent properties and are used in a variety of applications, including films, monofilaments, electronic components, electrical components, household goods, office supplies, automobile and vehicle-related parts, building materials, sporting goods, etc. Preferred electronic component applications include, for example, connectors, coils, sensors, LED lamps, sockets, resistors, relay cases, small switches, coil bobbins, capacitors, variable capacitor cases, optical pickup chassis, oscillators, various terminal boards, transformers, plugs, printed circuit boards, tuners, speakers, microphones, headphones, small motors, magnetic head bases, power modules, semiconductors, liquid crystal displays, FDD carriages, FDD chassis, motor brush holders, transformer components, parabolic antennas, and computer-related parts. Preferred applications for electrical components include generators, motors, transformers, current transformers, voltage regulators, rectifiers, inverters, relays, power contacts, switches, circuit breakers, knife switches, opposite-pole rods, electrical components, motor cases, notebook computer housings and internal components, CRT display housings and internal components, printer housings and internal components; portable terminal housings and internal components for mobile phones, mobile personal computers, handheld mobile devices, etc.; various gears, various cases, cabinets, etc. Preferred applications for household and office supplies include VTR parts, television parts, irons, hair dryers, rice cooker parts, microwave oven parts; audio and video equipment parts such as acoustic components, audio equipment, laser discs (registered trademark), compact discs, and DVDs; lighting parts, refrigerator parts, air conditioner parts, typewriter parts, word processor parts, electronic device housings for personal computers and notebook computers, etc., office computer-related parts, telephone-related parts, facsimile-related parts, copier-related parts, cleaning jigs, motor parts, lighters, typewriters, microscopes, binoculars, cameras, clocks, etc.Automotive and vehicle-related part applications include, for example, alternator terminals, alternator connectors, IC regulators, light dimmer potentiometer bases, various valves such as exhaust gas valves, various pipes, hoses, and tubes for fuel, cooling, brake, wiper, exhaust, and intake systems, air intake nozzle snorkels, intake manifolds, fuel pumps, engine coolant joints, carburetor main bodies, carburetor spacers, exhaust gas sensors, coolant sensors, oil temperature sensors, brake pad wear sensors, throttle position sensors, crankshaft position sensors, air flow meters, brake pad wear sensors, battery peripherals, air conditioner thermostat bases, heating hot air flow control valves, radiator motor brush holders, water pump impellers, turbine vanes, wiper motor-related parts, distributors, starter switches, starter relays, transmission wire harnesses, transmission oil pans, windshield washer nozzles, air conditioners, etc. Preferred uses include engine panel switch boards, coils for fuel-related electromagnetic valves; various connectors such as wire harness connectors, SMJ connectors, PCB connectors, door grommet connectors, and fuse connectors; horn terminals, insulating plates for electrical components, step motor rotors, lamp sockets, lamp reflectors, lamp housings, brake pistons, solenoid bobbins, engine oil pans, engine oil filters, ignition device cases, torque control levers, safety belt parts, register blades, washer levers, window regulator handles, window regulator handle knobs, passing light levers, sun visor brackets, instrument panels, airbag peripheral parts, door pads, pillars, console boxes, various motor housings, roof rails, fenders, garnishes, roof panels, hood panels, trunk lids, door mirror stays, spoilers, hood louvers, wheel covers, wheel caps, grill apron cover frames, lamp bezels, door handles, door moldings, rear finishers, and wipers.Preferred applications for building materials include, for example, wall, roof, and ceiling-related parts for civil engineering buildings; window-related parts, heat-insulating parts, flooring-related parts, seismic isolation and vibration-damping member-related parts, lifeline-related parts, etc. Preferred applications for sporting goods include, for example, golf-related goods such as golf clubs and shafts; personal protective equipment for sports such as masks, helmets, breast pads, elbow pads, and knee pads for American football, baseball, softball, etc.; shoe-related goods such as soles for sports shoes; fishing tackle-related goods such as fishing rods and fishing lines; summer sports-related goods for surfing, etc.; winter sports-related goods for skiing and snowboarding, etc.; and other indoor and outdoor sports-related goods.
[0040] <Film> Another aspect of the present invention is a film containing a copolymer polyamide resin or a polyamide resin composition. The film may be a monolayer film consisting of only a copolymer polyamide resin layer, or a laminate film of two or more layers including a copolymer polyamide resin layer and another layer. Examples of the other layer include a layer containing a resin other than the copolymer polyamide resin, such as a thermoplastic resin or a thermosetting resin, or a layer made of a metal such as aluminum. Examples of resins other than the copolymer polyamide resin include ethylene-based resins such as low-density polyethylene, linear low-density polyethylene, ionomers, ethylene-vinyl alcohol copolymer (EVOH), ethylene-acrylic acid copolymer, ethylene-vinyl acetate copolymer, ethylene-acrylic acid ester copolymer, and ethylene-methacrylic acid copolymer; polyolefins such as polypropylene, modified polyolefins, polyesters, polyvinyl alcohol, polyamides other than copolymer polyamide resins, polyamide elastomers; and biomass plastics such as polylactic acid (PLA) and polyhydroxyalkanoates (PHA).
[0041] The thickness of the film can be appropriately selected depending on the application. For example, in the case of a monolayer film, the thickness is preferably 5 to 200 μm, more preferably 10 to 50 μm. In the case of a laminated film, the total thickness is preferably 10 to 1000 μm, more preferably 20 to 500 μm; and the thickness of the layer containing the copolymerized polyamide resin or polyamide resin composition is preferably 5 to 100 μm, more preferably 10 to 50 μm.
[0042] The film may be an unstretched film or a stretched film obtained by stretching the unstretched film. The stretching method is not particularly limited, and examples thereof include uniaxial stretching using heated rolls, simultaneous biaxial stretching using a tubular method, and sequential biaxial stretching using heated rolls or a tenter.
[0043] (Film Manufacturing Method) The method for manufacturing the film is not particularly limited, and for example, known manufacturing methods can be applied. For example, a copolymerized polyamide resin or a polyamide resin composition can be melt-kneaded using an extruder, and a monolayer film can be produced by a molding method such as a T-die molding method, an air-cooled inflation molding method, a water-cooled inflation molding method, or a triple bubble molding method. The laminated film can be directly laminated by coextrusion, lamination, or the like, or can be laminated via an adhesive or adhesive resin layer. Coextrusion is preferred because of its excellent productivity. When a laminated film is produced by a coextrusion method, for example, a coextrusion T-die molding method in which a copolymerized polyamide resin or a composition thereof, a thermoplastic resin or a composition thereof, etc. are melted in separate extruders and continuously extruded through a T-die and cooled with a casting roll to form a film; a coextrusion air-cooled inflation molding method in which the resins are continuously extruded through a circular die and cooled by air; or a coextrusion water-cooled inflation molding method in which the resins are continuously extruded through a circular die and cooled by contact with water, etc., can be used to produce a substantially unoriented unstretched film.
[0044] Of these, air-cooled inflation molding and water-cooled inflation molding (also simply referred to as "inflation molding" or "inflation molding") require simple equipment and allow the film width to be easily changed simply by adjusting the blow-up ratio, resulting in good workability and high productivity in film production. When used in air-cooled or water-cooled inflation molding or co-extrusion air-cooled or water-cooled inflation molding, copolymerized polyamide resins can suppress film curling. In particular, when a multilayer film containing a layer containing a copolymerized polyamide resin and a low-melting-point thermoplastic resin layer is produced by co-extrusion air-cooled or water-cooled inflation molding, thermal degradation and curling of the film can be suppressed, making this method preferred.
[0045] The conditions for forming an inflation-molded film are not particularly limited, but the resin temperature is preferably above the melting point of the raw resin used and below 300°C. In the present invention, the resin temperature can be, for example, 160°C to 250°C, preferably 160°C to 220°C. The blow-up ratio (also referred to as the blow ratio) refers to the ratio of the maximum bubble diameter to the die diameter. The blow-up ratio is preferably 1.1 to 3.0, more preferably 1.2 to 2.5. The take-up speed is determined by the thickness and width of the film and the extrusion rate, and can be adjusted within a range that maintains film formation stability. Generally, the take-up speed is preferably 1 to 150 m / min, more preferably 5 to 100 m / min.
[0046] Furthermore, in order to improve printability, lamination ability, or adhesive applicability, the film may be subjected to surface treatment such as corona discharge treatment, plasma treatment, flame treatment, acid treatment, etc. After such treatment, if necessary, the film may be subjected to secondary processing steps such as printing, lamination, adhesive application, and heat sealing, and then used for the respective intended applications.
[0047] (Applications of the film) The film has excellent handling properties and work efficiency during thermoforming, and is also highly transparent, making it suitable for use as a food packaging film. The film is also suitable for use as an inflation-molded film. Furthermore, the film can be used in a variety of applications, including the applications of molded products, such as electronic components, electrical components, household goods, office supplies, automobile and vehicle-related parts, building materials, and sporting goods.
[0048] <Monofilament> Yet another aspect of the present invention is a monofilament comprising a copolymer polyamide resin or a polyamide resin composition. The diameter of the monofilament is not particularly limited, but is preferably 0.5 to 20 mm, more preferably 1 to 5 mm. The monofilament may be a continuous fiber or a staple fiber.
[0049] (Monofilament Manufacturing Method) Monofilaments can be obtained by known manufacturing methods using copolymerized polyamide resins or polyamide resin compositions. Examples of methods for manufacturing monofilaments include melting polyamide resin pellets in an extruder or the like, extruding them through a spinning nozzle, and cooling them in a refrigerant bath such as water or trichloroethylene to produce undrawn yarns. In this case, the distance between the filament outlet of the spinning nozzle and the refrigerant liquid level is preferably maintained at approximately 10 to 300 mm.
[0050] The undrawn yarn may be further drawn and heat-set. Here, two-stage drawing, in which drawing is performed in two stages, is preferred. In the first stage of the two-stage drawing, the undrawn yarn is preferably drawn 2 to 5 times, more preferably 3 to 4 times, in steam or hot water. If the draw ratio is within this range, the knot strength tends to be further improved.
[0051] When stretching is performed in water vapor, the temperature range is preferably 95 to 120° C., more preferably 100 to 110° C. When the temperature of the water vapor is within this temperature range, the knot strength and transparency of the obtained monofilament tend to be further improved.
[0052] When stretching is performed in hot water, the temperature of the hot water is preferably 50 to 95° C., more preferably 60 to 90° C. When the temperature of the hot water is within this range, the knot strength and transparency of the obtained monofilament tend to be further improved.
[0053] In the second-stage drawing, the monofilament is preferably drawn 1.1 to 2.5 times, more preferably 1.2 to 2.5 times, in a gas atmosphere. The gas is not particularly limited, and examples thereof include inert gases such as helium, nitrogen, and argon, and air. The temperature of the gas atmosphere in the second-stage drawing is preferably 120 to 300°C, more preferably 180 to 250°C. When the second-stage drawing is performed within the above-mentioned temperature range and draw ratio, the knot strength and transparency of the resulting monofilament tend to be further improved.
[0054] The two-stage drawn monofilament is preferably heat-set. The two-stage drawn monofilament can be heat-set in a gas atmosphere at preferably 160 to 350°C, more preferably 160 to 320°C, while being subjected to a 0 to 10% relaxation treatment. When the temperature is within this range, the knot strength tends to be further improved.
[0055] In the above two-stage drawing and heat setting, the total draw ratio is preferably in the range of 4.0 to 7.0 times, more preferably 4.5 to 6.5 times, and even more preferably 5.5 to 6.0 times.
[0056] (Uses of Monofilaments) Monofilaments have low water absorption and excellent abrasion resistance, and therefore can be used as filaments, multifilaments, nets, and other structures for applications in fishing, industry, clothing, medicine, etc. Furthermore, monofilaments can be used in a variety of applications, including electronic components, electrical components, household goods, office supplies, automobile and vehicle-related parts, building materials, and sporting goods, which are exemplified as uses of molded products.
[0057] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.
[0058] [Physical Property Measurement] (1) Melting Point (Tm) and Heat of Fusion (ΔH) Using a Hitachi High-Tech Science DSC7020 model, the polyamide resins of the Examples and Comparative Examples were heated to 300°C at a rate of 10°C / min under a nitrogen gas atmosphere, held at that temperature for 1 minute, cooled to 30°C at a rate of 10°C / min, and then heated again to 300°C at a rate of 10°C / min. The top temperature of the endothermic peak in the DSC curve during the second heating process was taken as the melting point (Tm), and the corresponding heat of fusion was taken as ΔH (unit: J / g). If ΔH was 40 J / g or less, the molded article was judged to have low crystallinity and excellent transparency.
[0059] (2) Crystallization Temperature (Tc) Using a DSC7020 model manufactured by Hitachi High-Tech Science Corporation, the polyamide resins of the Examples and Comparative Examples were heated to 300°C at a rate of 10°C / min under a nitrogen gas atmosphere, held at that temperature for 1 minute, and then cooled to 30°C at a rate of 10°C / min. The top temperature of the exothermic peak in the DSC curve during the cooling process was taken as the crystallization temperature (Tc).
[0060] (3) Calculation of the proportion of each structural unit and biomass raw material The proportion of each structural unit and biomass raw material in the polyamide resins of the Examples and Comparative Examples was calculated from the amount of raw material charged, assuming that all of the raw materials for the polyamide resin had reacted. The proportion of biomass raw material is the proportion of the amount (mass) of raw material derived from biomass charged in 100% by mass of the total amount of raw materials charged, assuming that all of the raw materials for the polyamide resin had reacted. Specifically, the proportions of each structural unit and biomass raw material were calculated taking into account the loss of condensation water during polymerization, with the following assumptions: contribution of 1,5-pentamethylenediamine to a molecular weight of 102.18 = 100.18 (= 102.18 - 2.00) g / mol; contribution of adipic acid to a molecular weight of 146.14 = 112.14 (= 146.14 - 34.00) g / mol; and contribution of sebacic acid to a molecular weight of 202.25 = 168.25 (= 202.25 - 34.00) g / mol. The proportion of biomass raw material was defined as the proportion of structural units derived from biomass-derived 1,5-pentamethylenediamine and sebacic acid relative to 100% by mass of all structural units in the polymer.
[0061] (4) Equilibrium Water Absorption Using polyamide resin pellets from the Examples and Comparative Examples, a heat press manufactured by Shinto Metal Industries Co., Ltd. was used. The pellets were preheated at a temperature of melting point + 30°C for 3 minutes, then heat-pressed at 5 MPa for 1 minute, and then cooled and pressed at 30°C and 5 MPa for 3 minutes to produce unstretched polyamide sheets measuring 20 mm x 80 mm x 2 mm. The resulting sheets were vacuum-dried at 80°C for 48 hours, and their masses were measured. The sheets were then immersed in water at 23°C for 800 hours. The surface moisture of the removed sheets was lightly absorbed with a cloth, and their masses were then measured. The equilibrium water absorption was calculated from the masses of the sheets before and after immersion in water using the following formula: Equilibrium Water Absorption = [(Sheet Mass After Immersion in Water - Sheet Mass Before Immersion in Water) / Sheet Mass Before Immersion in Water] x 100. An equilibrium water absorption of 14.5% or less was considered to be low water absorbency.
[0062] (5) Abrasion Volume Using the polyamide resin pellets of the Examples and Comparative Examples, a heat press manufactured by Shinto Metal Industries Co., Ltd. was used. The pellets were preheated at a temperature of melting point +30°C for 3 minutes, then heat-pressed at 5 MPa for 1 minute, and then cooled and pressed at 30°C and 5 MPa for 3 minutes to produce two 45 mm x 45 mm x 1 mm unstretched polyamide sheets. The resulting sheets were vacuum-dried at 80°C for 48 hours and sealed in an aluminum bag. One of the two sheets was used as a sample for the abrasion test, and the other was used as a sample for measuring water absorption to correct the water absorption of the sample (dried sheet) during the abrasion test. First, the aluminum bag was opened, and the masses of the two samples were measured. G (garnet)-50 abrasive paper cut to a length of 157 mm and a width of 12 mm was attached to the abrasion wheel of a reciprocating flat abrasion tester manufactured by Suga Test Instruments Co., Ltd., and an abrasion test was performed on the abrasion test samples under conditions of a load of 3000 g, a stroke of 30 mm, and 120 reciprocations. After the test, resin powder generated on the sample due to abrasion was brushed off, and the mass of the sample was measured. At approximately the same time, the mass of the sample for measuring water absorption was measured. The mass difference between the mass of the sample for abrasion test before and after the abrasion test plus the mass increase (apparent water absorption) of the sample for measuring water absorption was taken as the abrasion amount. Abrasion amounts of less than 11.6 mg were considered to be excellent in abrasion resistance.
[0063] [Raw materials used] (1) Diamine 1,5-pentamethylenediamine: manufactured by CJ Research (derived from biomass, purity: 99.90% by mass) (2) Dicarboxylic acid Adipic acid: manufactured by Asahi Kasei Corporation (derived from fossil raw materials, purity: 99.8% by mass) Sebacic acid: manufactured by Casda Biomaterials (derived from biomass, purity: 99.5% by mass) (3) Organic solvent 2-propanol: manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. (purity: 99.7% by mass)
[0064] Synthesis of Nylon 56 Salt: 32.42 kg of adipic acid and 273 kg of 2-propanol were placed in a 700 L reaction vessel and heated to 40°C to dissolve the adipic acid. 22.67 kg of 1,5-pentamethylenediamine was then slowly added over 71 minutes. Heat of neutralization and crystallization was generated, but the solution temperature was adjusted to fall within the range of 40°C to 50°C during the addition. After the addition of 1,5-pentamethylenediamine was completed, the solution was stirred for 30 minutes while maintaining the temperature at 35°C to 40°C, and then cooled and stirred for 2 hours while maintaining the temperature at 0°C to 5°C. The precipitated nylon 56 salt was collected as a filter cake and then dried under reduced pressure at 60°C for 48 hours to obtain 54.8 kg of nylon 56 salt.
[0065] Synthesis of Nylon 510 Salt: 24.27 kg of sebacic acid and 184 kg of 2-propanol were placed in a 700 L reaction vessel and heated to 40°C to dissolve the sebacic acid. Then, 12.27 kg of 1,5-pentamethylenediamine was slowly added over 65 minutes. Heat of neutralization and crystallization was generated, but the solution temperature was adjusted to fall within the range of 40°C to 50°C during the addition. After the addition of 1,5-pentamethylenediamine was completed, the solution was stirred for 30 minutes while maintaining the temperature at 35°C to 40°C, and then cooled and stirred for 2 hours while maintaining the temperature at 0°C to 5°C. The precipitated nylon 510 salt was collected as a filter cake and then dried under reduced pressure at 60°C for 48 hours to obtain 36.3 kg of nylon 510 salt.
[0066] Example 1 A 1 L polymerization vessel was charged with 200.0 g of nylon 56 salt, 50.0 g of nylon 510 salt, and 50.0 g of degassed ion-exchanged water. The atmosphere inside the polymerization vessel was replaced with nitrogen, then sealed and heated to 200°C. The pressure inside the polymerization vessel was then adjusted to 1.3 MPa with stirring, and polymerization was carried out for 3 hours. The temperature inside the polymerization vessel was raised to 280°C, and the pressure was released to atmospheric pressure over 40 minutes. After pressure release, polymerization was carried out for 2 hours under a nitrogen stream of 200 mL / min, after which the stirrer was stopped and nitrogen was introduced to pressurize to 1.0 MPa. After pressurization, the mixture was extracted as strands and pelletized. The polyamide pellets were dried under reduced pressure at 90°C for 48 hours to obtain the copolymerized polyamide resin of Example 1. The randomness of the copolymerized polyamide resin of Example 1 was investigated. 13 The C-NMR spectrum confirmed that the copolymer was a random copolymer.
[0067] Example 2 A 1 L polymerization vessel was charged with 175.0 g of nylon 56 salt, 75.0 g of nylon 510 salt, and 50.0 g of degassed ion-exchanged water. The atmosphere inside the polymerization vessel was replaced with nitrogen, then sealed and heated to 200°C. The pressure inside the polymerization vessel was then adjusted to 1.3 MPa with stirring, and polymerization was carried out for 3 hours. The temperature inside the polymerization vessel was raised to 250°C, and the pressure was released to atmospheric pressure over 40 minutes. After pressure release, polymerization was carried out for 2 hours under a nitrogen stream of 200 mL / min, after which the stirrer was stopped and nitrogen was introduced to pressurize to 1.0 MPa. After pressurization, the mixture was extracted as strands and pelletized. The polyamide pellets were dried under reduced pressure at 90°C for 48 hours to obtain the copolymerized polyamide resin of Example 2. The randomness of the copolymerized polyamide resin of Example 2 was investigated. 13 The C-NMR spectrum confirmed that the copolymer was a random copolymer.
[0068] Example 3 A 1-L polymerization vessel was charged with 150.0 g of nylon 56 salt, 100.0 g of nylon 510 salt, and 50.0 g of degassed ion-exchanged water, and polymerization was carried out in the same manner as in Example 2. The mixture was pelletized to obtain a copolymer polyamide resin of Example 3.
[0069] Example 4 A 1-L polymerization vessel was charged with 125.0 g of nylon 56 salt, 125.0 g of nylon 510 salt, and 50.0 g of degassed ion-exchanged water, and polymerization was carried out in the same manner as in Example 2. The mixture was pelletized to obtain a copolymer polyamide resin of Example 4.
[0070] Example 5 A 1-L polymerization vessel was charged with 100.0 g of nylon 56 salt, 150.0 g of nylon 510 salt, and 50.0 g of degassed ion-exchanged water, and polymerization was carried out in the same manner as in Example 2. The mixture was pelletized to obtain a copolymer polyamide resin of Example 5.
[0071] Example 6 A 1 L polymerization vessel was charged with 75.0 g of nylon 56 salt, 175.0 g of nylon 510 salt, and 50.0 g of degassed ion-exchanged water, and polymerization was carried out in the same manner as in Example 2. The mixture was pelletized to obtain a copolymer polyamide resin of Example 6.
[0072] Example 7 A 1 L polymerization vessel was charged with 50.0 g of nylon 56 salt, 200.0 g of nylon 510 salt, and 50.0 g of degassed ion-exchanged water, and polymerization was carried out in the same manner as in Example 2. The mixture was pelletized to obtain a copolyamide resin of Example 7.
[0073] Comparative Example 1 A 1 L polymerization vessel was charged with 225.0 g of nylon 56 salt, 25.0 g of nylon 510 salt, and 50.0 g of degassed ion-exchanged water, and polymerization was carried out in the same manner as in Example 1. The mixture was pelletized to obtain a copolymer polyamide resin of Comparative Example 1.
[0074] Comparative Example 2 A 1-L polymerization vessel was charged with 25.0 g of nylon 56 salt, 225.0 g of nylon 510 salt, and 50.0 g of degassed ion-exchanged water, and polymerization was carried out in the same manner as in Example 2. The mixture was pelletized to obtain a copolymer polyamide resin of Comparative Example 2.
[0075] Table 1 shows the mass ratio of each constituent unit calculated from the amount of raw material charged in Examples 1 to 7 and Comparative Examples 1 and 2, the ratio of constituent units derived from each monomer component, the proportion of biomass raw material, and DSC measurement data.
[0076]
[0077] The equilibrium water absorption and abrasion data for the copolyamide resins of Example 2 and Comparative Examples 1 and 2 are shown in Table 2.
[0078]
[0079] Table 1 shows that Examples 1 to 7, which contain structural units A derived from equimolar amounts of a reactant between pentamethylenediamine and adipic acid and structural units B derived from equimolar amounts of a reactant between pentamethylenediamine and sebacic acid, and in which the mass ratio of structural units A / structural units B is in the range of 85 / 15 to 15 / 85, have a smaller heat of fusion, i.e., a smaller enthalpy change ΔH upon melting, a lower degree of crystallinity, and excellent transparency, compared to Comparative Examples 1 and 2. In particular, Example 4, in which the mass ratio of structural units A / structural units B was 49 / 51, and Example 5, in which the mass ratio of structural units A / structural units B was 39 / 61, had an even smaller ΔH and were particularly excellent in transparency.
[0080] The copolyamide resin of the present invention can be suitably used for applications such as molded articles produced by various molding methods, food packaging films, etc. The copolyamide resin can contribute to the achievement of Goal 12 of the SDGs (Sustainable Development Goals), etc.
Claims
1. A structural unit A derived from a reaction product of equimolar amounts of pentamethylenediamine and adipic acid, represented by the following formula (A): and a structural unit B derived from a reaction product of equimolar amounts of pentamethylenediamine and sebacic acid represented by the following formula (B): and the mass ratio of structural unit A / structural unit B is 85 / 15 to 15 / 85.
2. The copolyamide resin according to claim 1, wherein the melting point of the copolyamide resin as measured by DSC is 170 to 240°C.
3. The copolyamide resin according to claim 1, wherein the crystallization temperature of the copolyamide resin as measured by DSC is 115 to 195°C.
4. A polyamide resin composition comprising the copolymer polyamide resin according to any one of claims 1 to 3.
5. A molded article comprising the copolymer polyamide resin according to any one of claims 1 to 3.
6. A film comprising the copolymer polyamide resin according to any one of claims 1 to 3.
7. A monofilament comprising the copolyamide resin according to any one of claims 1 to 3.
Citation Information
Patent Citations
Host and method for producing cadaverine
JP2002223770A
Method for producing cadaverine
JP2002223771A
Method for producing cadaverine
JP2004000114A
Cadaverine-dicarboxylic acid salt and method for producing the same
JP2004208646A
Corynebacterium, and cadaverine or salt thereof and method for producing the same
JP2004222569A
Cited By
Bio-based polyamide composition material for automobile air conditioner pipe and preparation method of bio-based polyamide composition material
CN120865703A