Copolymerized polyamide resin, and composition, molded article, film, and monofilament containing same

The copolyamide resin, formulated with biomass-derived structural units, addresses the issues of high water absorption and poor abrasion resistance in conventional polyamide resins, offering improved performance and sustainability through optimized structural unit ratios.

WO2024219348A1PCT designated stage expired Publication Date: 2024-10-24UBE CORPORATION
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014948
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-10-13
Filing Date
2024-04-15
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Conventional polyamide resins derived from fossil raw materials exhibit high water absorption and poor abrasion resistance, making them unsuitable for applications requiring low water absorption and high abrasion resistance, such as films and monofilaments.

Method used

A copolyamide resin is developed using biomass-derived raw materials, specifically structural units derived from pentamethylene diamine and sebacic acid, combined with aminocarboxylic acids and lactams, to achieve low water absorption and high abrasion resistance, with a preferred mass ratio of structural units optimized for improved properties.

Benefits of technology

The copolyamide resin demonstrates reduced water absorption and enhanced abrasion resistance, making it suitable for applications like films and monofilaments, while also contributing to a sustainable society by utilizing biomass-derived materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

Provided is a copolymerized polyamide resin which has low water absorption and excellent abrasion resistance when made into molded articles, and in which a biomass-derived material is used. Also provided are a composition and molded articles such as a film and a monofilament containing the copolymerized polyamide resin. The present invention can contribute to the achievement of Goal 12, etc. of the Sustainable Development Goals (SDGs). The copolymerized polyamide resin contains: a structural unit A selected from the group consisting of a structural unit A1 derived from the product of an equimolar reaction between pentamethylenediamine and adipic acid, and a structural unit A2 derived from the product of an equimolar reaction between pentamethylenediamine and sebacic acid; and a structural unit B derived from at least one aminocarboxylic acid selected from among 10-aminodecanoic acid, 11-aminoundecanoic acid and 12-aminododecanoic acid, and / or at least one lactam selected from among decalactam, undecalactam and dodecalactam.
Need to check novelty before this filing date? Find Prior Art

Description

Copolymerized polyamide resin, and composition, molded article, film, and monofilament containing the same

[0001] The present invention relates to a copolyamide resin, and particularly to a copolyamide resin using a raw material derived from biomass.

[0002] Polyamides are polymers formed by assembling structural units containing amide bonds. The structural units of polyamides are generally derived from aminocarboxylic acids or lactams, or diamines and dicarboxylic acids. In particular, aliphatic polyamide resins derived from aliphatic species of these compounds have versatile and beneficial properties as resins, such as chemical resistance, toughness, heat resistance, and oil resistance. Therefore, aliphatic polyamide resins are useful as raw materials for molded products in a variety of applications. For example, they are used as substrates for monolayer or laminate films, particularly in packaging films that require pinhole resistance and gas barrier properties, particularly in the food packaging field, and as structural materials for multilayer films coextruded with other resins.

[0003] One of the advantages of resins is that their properties can be controlled in various ways by selecting the monomer or by using multiple types of monomers. Copolymer polyamide resins are produced by combining two or more types of structural units to give molded articles with properties suited to their intended use (Patent Document 1).

[0004] Polyamide resins provide molded products with excellent properties, and therefore are produced as homopolymers of various structural units or copolymers of combinations of structural units. However, many of the monomers used to produce polyamide resins are industrially derived from fossil fuels. For example, ε-caprolactam, a well-known raw material for Nylon (registered trademark), is synthesized from naphtha-derived benzene. With the recent rise in environmental awareness, which calls for the reduction of carbon dioxide emissions, there is a demand for a shift from fossil fuels to biomass-derived raw materials for polyamide resins. One known biomass-derived compound that can be used as a polyamide raw material is 1,5-pentanediamine, which can be obtained from starch or sugarcane through enzyme reactions, yeast reactions, fermentation reactions, and the like. Patent Document 2 attempts to produce polyamide resins with fewer biomass-derived impurities using 1,5-pentanediamine as a raw material. Patent Documents 3 and 4 attempt to produce polyamide resins for large molded products using 1,5-pentanediamine as a raw material, with improved thermal retention stability, etc.

[0005] International Publication No. 2022 / 071013 International Publication No. 2015 / 076233 JP 2006-348057 A JP 2007-332353 A

[0006] The replacement of conventional products with resins derived from biomass raw materials is one of the global efforts to build a sustainable society, and in Japan too, there are efforts to establish legislation such as setting certain standards for the content of bio-based polymers, establishing recycling processes, and reducing CO2 emissions. 2 Demonstration experiments are underway to achieve this. However, replacing raw resin materials often involves changes to the molecular structure of the resin, which inevitably leads to changes in physical properties. Consumers are highly concerned about the quality of resins, along with the price, and there is a strong demand for resins that are of equal or higher quality than the resins they are replacing.

[0007] Although molded articles using the polyamide resins described in Patent Documents 1 to 4 exhibit certain mechanical properties (such as tensile modulus and tensile elongation), they have problems such as high water absorption and poor abrasion resistance, and are insufficient for applications requiring low water absorption and high abrasion resistance, such as films and monofilaments. Therefore, there is a demand for polyamide resins that combine low water absorption and high abrasion resistance.

[0008] Therefore, an object of the present invention is to provide a copolymerized polyamide resin that has low water absorption and excellent abrasion resistance when formed into a molded article, and that uses a biomass-derived raw material, as well as a composition containing the same and molded articles such as a film and a monofilament.

[0009] The present invention relates to the following [1] to

[12] . [1] A structural unit A1 derived from a reaction product of equimolar amounts of pentamethylenediamine and adipic acid, represented by the following formula (A1): and structural unit A2 derived from a reaction product of equimolar amounts of pentamethylenediamine and sebacic acid, represented by the following formula (A2): and a structural unit B derived from at least one aminocarboxylic acid selected from 10-aminodecanoic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid, and / or at least one lactam selected from decalactam, undecalactam, and dodecalactam. [2] The copolymer polyamide resin according to [1], wherein structural unit B is a unit derived from 12-aminododecanoic acid and / or dodecalactam. [3] The copolymer polyamide resin according to [1] or [2], wherein the proportion of biomass raw material in the copolymer polyamide resin is 3% or more by mass. [4] The copolymer polyamide resin according to any one of [1] to [3], wherein structural unit A is structural unit A1, and the mass ratio of structural unit A1 / structural unit B is 95 / 5 to 9 / 91. [5] The copolymer polyamide resin according to any one of [1] to [3], wherein the structural unit A is structural unit A2, and the mass ratio of structural unit A2 / structural unit B is 97 / 3 to 7 / 93. [6] The copolymer polyamide resin according to any one of [1] to [4], wherein the structural unit A is structural unit A1, and the melting point of the copolymer polyamide resin as measured by DSC is 130 to 250°C. [7] The copolymer polyamide resin according to [1], [2], [3], or [5], wherein the structural unit A is structural unit A2, and the melting point of the copolymer polyamide resin as measured by DSC is 100 to 250°C. [8] The copolymer polyamide resin according to [1], [2], [3], [4], or [6], wherein the structural unit A is structural unit A1, and the crystallization temperature of the copolymer polyamide resin as measured by DSC is 110 to 200°C. [9] A polyamide resin composition comprising the copolymer polyamide resin according to any one of [1] to [8].

[10] A molded article comprising the copolymer polyamide resin according to any one of [1] to [8].

[11] A film comprising the copolymer polyamide resin according to any one of [1] to [8].

[12] A monofilament comprising the copolymer polyamide resin according to any one of [1] to [8].

[0010] According to the present invention, it is possible to provide a copolymerized polyamide resin which, when formed into a molded article, has low water absorption and excellent abrasion resistance, and which uses a biomass-derived raw material, as well as a composition containing the same and molded articles such as a film and a monofilament.

[0011] In the present invention, the polyamide resin refers to a resin having an acid amide bond (-CONH-) in the main chain and obtained by polymerizing or copolymerizing a lactam, an aminocarboxylic acid, or a nylon salt composed of a diamine and a dicarboxylic acid as a raw material by a known method such as melt polymerization, solution polymerization, or solid-state polymerization. As long as the effects of the present invention are not impaired, other components may be blended with the polyamide resin to form a polyamide resin composition.

[0012] The copolymerized polyamide resin of the present invention comprises a structural unit A1 derived from a reaction product of equimolar amounts of pentamethylenediamine and adipic acid, represented by the following formula (A1): and structural unit A2 derived from a reaction product of equimolar amounts of pentamethylenediamine and sebacic acid, represented by the following formula (A2): and a structural unit B derived from at least one aminocarboxylic acid selected from 10-aminodecanoic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid, and / or at least one lactam selected from decalactam, undecalactam, and dodecalactam. By including structural units A and B in the copolymerized polyamide resin, it is possible to increase the bio content while achieving low water absorption and high abrasion resistance in the resulting molded article.

[0013] [Structural Unit A] The structural unit A is selected from the group consisting of structural unit A1, which is derived from the reaction product of equimolar amounts of pentamethylenediamine and adipic acid, as shown in the above formula (A1), and structural unit A2, which is derived from the reaction product of equimolar amounts of pentamethylenediamine and sebacic acid, as shown in the above formula (A2). By including structural unit A in the copolymerized polyamide resin, the obtained molded article can maintain low water absorption and high abrasion resistance while increasing the bio content. As the structural unit A, only one of structural units A1 and A2 may be used, or both may be used in combination.

[0014] [Structural Unit A1] The structural unit A1 is a unit derived from the reaction product of equimolar amounts of pentamethylenediamine and adipic acid, as represented by the above formula (A1). The structural unit A1 is formed by polymerizing an equimolar salt or equimolar mixture of pentamethylenediamine and adipic acid. The pentamethylenediamine and adipic acid that constitute this unit may be condensed directly or via another unit or a diamine or dicarboxylic acid that constitutes another unit. By including the structural unit A1 in the copolymerized polyamide resin, the resulting molded article can maintain low water absorption and high abrasion resistance while increasing the bio content.

[0015] Examples of pentamethylenediamines include 1,5-pentamethylenediamine, 1,4-pentamethylenediamine, and 1,3-pentamethylenediamine, but 1,5-pentamethylenediamine is preferred from the viewpoints of availability and the strength of the resulting polyamide resin. Pentamethylenediamines may be used alone or in combination of two or more.

[0016] Pentamethylenediamine may be derived from a fossil raw material or a biomass-derived raw material, but from the viewpoint of increasing the bio content of the copolyamide resin, it is preferably a biomass-derived raw material. Examples of biomass-derived pentamethylenediamine include WO 2015 / 076233, JP 2006-348057, JP 2007-332353, JP 2002-223771, JP 2004-000114, JP 2004-208646, JP 2004-290091, JP 2004-298034, JP 2002-223770, JP 2004-222569, JP 2005-6650, JP 2019-154313, and JP 2019-205423. Those obtained by the production methods disclosed in such publications can be used.

[0017] Specifically, it is known that 1,5-pentamethylenediamine can be produced by decarboxylating lysine through an enzymatic reaction, and 1,5-pentamethylenediamine can be produced from lysine using, for example, lysine decarboxylase, cells producing lysine decarboxylase, a processed product of the cells, a microorganism expressing lysine decarboxylase, etc. Alternatively, the enzymatic decarboxylation of lysine can be carried out while adding an acid such as adipic acid to the lysine solution so as to maintain a pH suitable for the enzymatic decarboxylation.

[0018] Adipic acid may be derived from a fossil raw material or a biomass-derived raw material, but from the viewpoint of availability, adipic acid is preferably derived from a fossil raw material.

[0019] [Structural Unit A2] The structural unit A2 is a unit derived from the reaction product of equimolar amounts of pentamethylenediamine and sebacic acid, as represented by the above formula (A2). The structural unit A2 is formed by polymerizing an equimolar salt or equimolar mixture of pentamethylenediamine and sebacic acid. The pentamethylenediamine and sebacic acid that constitute this unit may be condensed directly or via another unit or a diamine or dicarboxylic acid that constitutes another unit. By including the structural unit A2 in the copolymerized polyamide resin, the resulting molded article can maintain low water absorption and high abrasion resistance while increasing the bio content.

[0020] As the pentamethylenediamine, those exemplified for the structural unit A1 can be used. Preferred embodiments of the pentamethylenediamine and the method for producing the same are also as described for the structural unit A1.

[0021] Sebacic acid may be derived from fossil fuels or biomass, but is preferably derived from biomass in order to increase the bio content of the copolyamide resin. Biomass-derived sebacic acid can be synthesized, for example, from ricinoleic acid triglyceride, which is the main component of castor oil obtained from castor bean seeds.

[0022] [Structural Unit B] Structural unit B is a unit derived from at least one aminocarboxylic acid selected from 10-aminodecanoic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid, and / or at least one lactam selected from decalactam, undecalactam, and dodecalactam. These aminocarboxylic acids and lactams may be derived from fossil raw materials or biomass-derived raw materials, but from the viewpoint of ease of availability, fossil raw materials are preferred. By including structural unit B in the copolymerized polyamide resin, molded articles with low water absorption and excellent abrasion resistance can be obtained.

[0023] From the viewpoint of reducing the water absorption of the molded article, the structural unit B is preferably a unit derived from 12-aminododecanoic acid and / or dodecalactam.

[0024] [Mass Ratio of Structural Unit A and Structural Unit B] The mass ratio of structural unit A / structural unit B in the copolymerized polyamide resin is preferably 97 / 3 to 7 / 93, more preferably 95 / 5 to 9 / 91, even more preferably 93 / 7 to 10 / 90, and particularly preferably 90 / 10 to 20 / 80. By setting the mass ratio within this range, handling during molding is good, and the molded product maintains low water absorption and has high abrasion resistance.

[0025] When the structural unit A is the structural unit A1, the mass ratio of the structural unit A1 / structural unit B in the copolymerized polyamide resin is preferably 95 / 5 to 9 / 91, more preferably 93 / 7 to 10 / 90, and particularly preferably 90 / 10 to 20 / 80. By setting the mass ratio within this range, handling during molding is easy, and the molded product maintains low water absorption and has high abrasion resistance.

[0026] When the structural unit A is the structural unit A2, the mass ratio of the structural unit A2 / structural unit B in the copolymerized polyamide resin is preferably 97 / 3 to 7 / 93, more preferably 95 / 5 to 9 / 91, even more preferably 93 / 7 to 10 / 90, and particularly preferably 90 / 10 to 20 / 80. By setting the mass ratio within this range, handling during molding is good, and the molded product maintains low water absorption and has high abrasion resistance.

[0027] The total amount of the structural unit A and the structural unit B is preferably 80 to 100% by mass, more preferably 90 to 100% by mass, and even more preferably 95 to 100% by mass, relative to 100% by mass of the copolymerized polyamide resin. In one embodiment, the total amount of the structural unit A and the structural unit B is 100% by mass, relative to 100% by mass of the copolymerized polyamide resin.

[0028] [Other Structural Units] As long as the properties of the copolymerized polyamide resin are not impaired, it may contain structural units other than structural unit A and structural unit B. Examples of such structural units include a structural unit derived from a reaction product of equimolar amounts of pentamethylenediamine with a dicarboxylic acid other than adipic acid and sebacic acid; a structural unit derived from a reaction product of equimolar amounts of a diamine other than pentamethylenediamine with adipic acid or sebacic acid; a structural unit derived from a reaction product of equimolar amounts of a diamine other than pentamethylenediamine with a dicarboxylic acid other than adipic acid and sebacic acid; and a structural unit derived from an aminocarboxylic acid and / or lactam other than the aminocarboxylic acid and lactam that constitute structural unit B.

[0029] Examples of diamines other than pentamethylenediamine include ethylenediamine, trimethylenediamine, tetramethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, tridecanediamine, tetradecanediamine, pentadecanediamine, hexadecanediamine, heptadecanediamine, octadecanediamine, nonadecanediamine, eicosanediamine, 2-methyl-1,8-octanediamine, and 2,2,4 / 2,4,4-trimethylhexamethylenediamine. Aliphatic diamines; alicyclic diamines such as 1,3- / 1,4-cyclohexyldiamine, bis(4-aminocyclohexyl)methane, bis(4-aminocyclohexyl)propane, bis(3-methyl-4-aminocyclohexyl)methane, bis(3-methyl-4-aminocyclohexyl)propane, 1,3- / 1,4-bisaminomethylcyclohexane, 5-amino-2,2,4-trimethyl-1-cyclopentanemethylamine, 5-amino-1,3,3-trimethylcyclohexanemethylamine, bis(aminopropyl)piperazine, bis(aminoethyl)piperazine, and norbornanedimethylenediamine; and the like.

[0030] Examples of dicarboxylic acids other than adipic acid and sebacic acid include aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, pimelic acid, suberic acid, azelaic acid, undecanedioic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid, pentadecanedioic acid, hexadecanedioic acid, heptadecanedioic acid, octadecanedioic acid, nonadecanedioic acid, and eicosanedioic acid; and alicyclic dicarboxylic acids such as 1,3- / 1,4-cyclohexanedicarboxylic acid, dicyclohexanemethane-4,4'-dicarboxylic acid, and norbornanedicarboxylic acid.

[0031] Examples of aminocarboxylic acids other than the aminocarboxylic acids that constitute the structural unit B include 6-aminocaproic acid, 7-aminoheptanoic acid, 9-aminononanoic acid, etc. Examples of lactams other than the lactams that constitute the structural unit B include ε-caprolactam, enantholactam, α-pyrrolidone, α-piperidone, etc.

[0032] The amount of each structural unit of the copolymerized polyamide resin corresponds to the amount of each component charged during the production of the copolymerized polyamide resin, but can also be determined by measuring the obtained copolymerized polyamide resin as is or after hydrolysis using high performance liquid chromatography, gas chromatography, gas chromatograph / atomic emission detector (GC / AED), gel permeation chromatography, etc. The amount of each structural unit of the copolymerized polyamide resin described in this specification and claims is calculated from the charge ratio (mass ratio) of the raw materials, assuming that all of the raw materials for the copolymerized polyamide resin have reacted. In the examples, the amounts of each structural unit are calculated taking into consideration the elimination of condensation water by polymerization, with the following formula: contribution of 1,5-pentamethylenediamine to a molecular weight of 102.18 = 100.18 (= 102.18 - 2.00) g / mol; contribution of 1,6-hexamethylenediamine to a molecular weight of 116.20 = 114.20 (= 116.20 - 2.00) g / mol; contribution of adipic acid to a molecular weight of 146.14 = 112.14 (= The contribution of sebacic acid to a molecular weight of 202.25 = 168.25 (= 202.25 - 34.00) g / mol, the contribution of 12-aminododecanoic acid to a molecular weight of 215.34 = 197.34 (= 215.34 - 18.00) g / mol, and the contribution of 6-aminocaproic acid to a molecular weight of 131.17 = 113.17 (= 131.17 - 18.00) g / mol.

[0033] [Physical Properties of Copolymer Polyamide Resin] From the viewpoint of moldability, the melting point of the copolymer polyamide resin measured by differential scanning calorimetry (DSC) is preferably 100 to 250°C, more preferably 125 to 240°C. The melting point of the copolymer polyamide resin measured by DSC can be increased or decreased depending on the ratio of the structural units, the molecular weight of the copolymer polyamide resin, and the like. When the structural unit A is the structural unit A1, from the viewpoint of moldability, the melting point of the copolymer polyamide resin measured by differential scanning calorimetry (DSC) is preferably 130 to 250°C. The melting point of the copolymer polyamide resin can also be 125 to 240°C. When the structural unit A is the structural unit A2, from the viewpoint of moldability, the melting point of the copolymer polyamide resin measured by differential scanning calorimetry (DSC) is preferably 100 to 250°C, more preferably 125 to 240°C. From the viewpoint of the transparency of the molded article, the heat of fusion (enthalpy change accompanying melting) ΔH corresponding to the melting point is preferably 50 J / g or less, more preferably 2 to 50 J / g, and particularly preferably 5 to 50 J / g.

[0034] In this specification, the melting point measured by DSC is the top temperature of the endothermic peak in the DSC curve in the second heating process when a copolymer polyamide resin is heated to 300°C at a rate of 10°C / min in a nitrogen gas atmosphere, held at that temperature for 1 minute, cooled to 30°C at a rate of 10°C / min, and then heated again to 300°C at a rate of 10°C / min. The heat of fusion corresponding to the melting point is calculated from the endothermic peak in the DSC curve in the second heating process.

[0035] When the structural unit A is the structural unit A1, from the viewpoint of moldability, the crystallization temperature of the copolymerized polyamide resin measured by differential scanning calorimetry (DSC) is preferably 110 to 200°C. The crystallization temperature of the copolymerized polyamide resin measured by DSC can be increased or decreased depending on the ratio of the structural units, the molecular weight of the copolymerized polyamide resin, etc. In this specification, the crystallization temperature measured by DSC is the top temperature of the exothermic peak in the DSC curve during the cooling process when the copolymerized polyamide resin is heated to 300°C at a rate of 10°C / min in a nitrogen gas atmosphere, held at that temperature for 1 minute, and then cooled to 30°C at a rate of 10°C / min.

[0036] The copolyamide resin is preferably a random copolymer from the viewpoint of obtaining a preferable melting point and crystallization temperature. A random copolymer is a copolymer in which structural units A and B are arranged randomly. A copolyamide resin obtained by mixing and polymerizing each unit in the monomer state is usually a random copolymer. On the other hand, for example, a copolyamide resin obtained by mixing and further polymerizing polyamide resin A obtained by polymerizing a monomer that is the raw material for structural unit A and polyamide resin B obtained by polymerizing a monomer that is the raw material for structural unit B is usually not a random copolymer but a block copolymer. A block copolymer is a copolymer formed by polymerizing blocks in which a certain number of structural units A or structural units B are arranged consecutively. A random copolymer can be confirmed by a nuclear magnetic resonance spectrometer. 13 This can also be confirmed by examining the bonding probability of each structural unit from a C-NMR spectrum.

[0037] The biomass ratio of the copolyamide resin measured in accordance with ASTM D6866 is preferably 3% or more, more preferably 10% or more, and even more preferably 20% or more. The biomass ratio is determined by the radioactive carbon ( 14 Specifically, if all of the carbon in the copolyamide resin is derived from fossil raw materials, the biomass degree is 0%, and if all of the carbon is derived from biomass, the biomass degree is 100%.

[0038] The proportion (by mass) of biomass raw material in the copolyamide resin is preferably 3% or more, more preferably 10% or more, and even more preferably 20% or more. The proportion of biomass raw material is the proportion (by mass) of the biomass-derived raw material charged out of 100% by mass of the total raw material charge, assuming that all of the raw materials for the copolyamide resin have reacted. The upper limit of the proportion of biomass raw material is 100%. When the structural unit A is the structural unit A1, the upper limit of the proportion of biomass raw material can be, for example, 45% or less. Furthermore, when the structural unit A is the structural unit A2, the upper limit of the proportion of biomass raw material can be, for example, 95% or less. When the biomass raw material consists only of 1,5-pentamethylenediamine and sebacic acid, the proportion of biomass raw material is the proportion of the amounts of 1,5-pentamethylenediamine and sebacic acid charged out of 100% by mass of the total raw material charge. In the examples, the proportions of biomass raw materials are determined taking into consideration that condensation water is removed by polymerization, and are as follows: contribution of 1,5-pentamethylenediamine to a molecular weight of 102.18 = 100.18 (= 102.18 - 2.00) g / mol; contribution of 1,6-hexamethylenediamine to a molecular weight of 116.20 = 114.20 (= 116.20 - 2.00) g / mol; contribution of adipic acid to a molecular weight of 146.14 = 112.14 (=146.14-34.00) g / mol, contribution of sebacic acid to a molecular weight of 202.25=168.25 (=202.25-34.00) g / mol, contribution of 12-aminododecanoic acid to a molecular weight of 215.34=197.34 (=215.34-18.00) g / mol, contribution of 6-aminocaproic acid to a molecular weight of 131.17=113.17 (=131.17-18.00) g / mol.

[0039] [Method for producing copolymerized polyamide resin] For the production of copolymerized polyamide resin, known polymerization methods such as melt polymerization, solution polymerization, interfacial polymerization, solid-state polymerization, and combinations thereof can be used. Usually, melt polymerization carried out at a temperature higher than the melting point of the copolymerized polyamide resin to be obtained is preferably used. For the production of copolymerized polyamide resin, known polymerization equipment can be used, and the copolymerized polyamide resin can be produced by appropriately combining operations such as normal pressure, reduced pressure, and increased pressure in a batch or continuous manner as needed. For example, the monomer that is the raw material for structural unit A and the monomer that is the raw material for structural unit B can be introduced at the same time.

[0040] Furthermore, although not particularly limited, since copolymerized polyamide resins have high viscosity, in some cases, in order to avoid difficulties in extracting the resin during polymerization, it is possible to synthesize a copolymerized polyamide resin having low viscosity by melt polymerization, and then obtain a copolymerized polyamide resin having increased viscosity by solid-state polymerization.

[0041] [Uses of Copolymer Polyamide Resins] Copolymer polyamide resins can increase the bio content, which can contribute to achieving Goal 12 of the SDGs (Sustainable Development Goals), and when formed into molded articles, they have low water absorption and excellent abrasion resistance. Copolymer polyamide resins can be used in polyamide resin compositions and molded articles such as films and monofilaments.

[0042] <Polyamide Resin Composition> One aspect of the present invention is a polyamide resin composition containing a copolymerized polyamide resin. The polyamide resin composition may contain other components in addition to the copolymerized polyamide resin, provided that the effects of the present invention are not impaired. Examples of other components include polyamide resins other than copolymerized polyamide resins; any resin other than polyamide resins, such as modified or unmodified polyolefin resins; and functionality-imparting agents such as plasticizers, heat resistance agents, foaming agents, antioxidants, UV absorbers, weathering agents, crystal nucleating agents, crystallization accelerators, mold release agents, lubricants, antistatic agents, antifogging agents, flame retardants, flame retardant assistants, pigments, and dyes. The polyamide resin composition containing these other components can be formed into molded articles such as pellets, films, and monofilaments.

[0043] The method for producing the polyamide resin composition is not particularly limited, and the polyamide resin composition can be produced, for example, by mixing the copolymer polyamide resin and other components using a known melt kneader such as a single-screw or twin-screw extruder, a Banbury mixer, a kneader, or a mixing roll.

[0044] <Molded Article> One aspect of the present invention is a molded article containing a copolymer polyamide resin or a polyamide resin composition. The method for producing the molded article is not particularly limited, and examples include injection molding, press molding, blow molding, extrusion molding, and rotational molding.

[0045] (Uses of Molded Articles) Molded articles containing copolymerized polyamide resins or polyamide resin compositions take advantage of their excellent properties and are used in a variety of applications, including films, monofilaments, electronic components, electrical components, household goods, office supplies, automobile and vehicle-related parts, building materials, sporting goods, etc. Preferred electronic component applications include, for example, connectors, coils, sensors, LED lamps, sockets, resistors, relay cases, small switches, coil bobbins, capacitors, variable capacitor cases, optical pickup chassis, oscillators, various terminal boards, transformers, plugs, printed circuit boards, tuners, speakers, microphones, headphones, small motors, magnetic head bases, power modules, semiconductors, liquid crystal displays, FDD carriages, FDD chassis, motor brush holders, transformer components, parabolic antennas, and computer-related parts. Preferred applications for electrical components include generators, motors, transformers, current transformers, voltage regulators, rectifiers, inverters, relays, power contacts, switches, circuit breakers, knife switches, opposite-pole rods, electrical components, motor cases, notebook computer housings and internal components, CRT display housings and internal components, printer housings and internal components; portable terminal housings and internal components for mobile phones, mobile personal computers, handheld mobile devices, etc.; various gears, various cases, cabinets, etc. Preferred applications for household and office supplies include VTR parts, television parts, irons, hair dryers, rice cooker parts, microwave oven parts; audio and video equipment parts such as acoustic components, audio equipment, laser discs (registered trademark), compact discs, and DVDs; lighting parts, refrigerator parts, air conditioner parts, typewriter parts, word processor parts, electronic device housings for personal computers and notebook computers, etc., office computer-related parts, telephone-related parts, facsimile-related parts, copier-related parts, cleaning jigs, motor parts, lighters, typewriters, microscopes, binoculars, cameras, clocks, etc.Automotive and vehicle-related part applications include, for example, alternator terminals, alternator connectors, IC regulators, light dimmer potentiometer bases, various valves such as exhaust gas valves, various pipes, hoses, and tubes for fuel, cooling, brake, wiper, exhaust, and intake systems, air intake nozzle snorkels, intake manifolds, fuel pumps, engine coolant joints, carburetor main bodies, carburetor spacers, exhaust gas sensors, coolant sensors, oil temperature sensors, brake pad wear sensors, throttle position sensors, crankshaft position sensors, air flow meters, brake pad wear sensors, battery peripherals, air conditioner thermostat bases, heating hot air flow control valves, radiator motor brush holders, water pump impellers, turbine vanes, wiper motor-related parts, distributors, starter switches, starter relays, transmission wire harnesses, transmission oil pans, windshield washer nozzles, air conditioners, etc. Preferred uses include engine panel switch boards, coils for fuel-related electromagnetic valves; various connectors such as wire harness connectors, SMJ connectors, PCB connectors, door grommet connectors, and fuse connectors; horn terminals, insulating plates for electrical components, step motor rotors, lamp sockets, lamp reflectors, lamp housings, brake pistons, solenoid bobbins, engine oil pans, engine oil filters, ignition device cases, torque control levers, safety belt parts, register blades, washer levers, window regulator handles, window regulator handle knobs, passing light levers, sun visor brackets, instrument panels, airbag peripheral parts, door pads, pillars, console boxes, various motor housings, roof rails, fenders, garnishes, roof panels, hood panels, trunk lids, door mirror stays, spoilers, hood louvers, wheel covers, wheel caps, grill apron cover frames, lamp bezels, door handles, door moldings, rear finishers, and wipers.Preferred applications for building materials include, for example, wall, roof, and ceiling-related parts for civil engineering buildings; window-related parts, heat-insulating parts, flooring-related parts, seismic isolation and vibration-damping member-related parts, lifeline-related parts, etc. Preferred applications for sporting goods include, for example, golf-related goods such as golf clubs and shafts; personal protective equipment for sports such as masks, helmets, breast pads, elbow pads, and knee pads for American football, baseball, softball, etc.; shoe-related goods such as soles for sports shoes; fishing tackle-related goods such as fishing rods and fishing lines; summer sports-related goods for surfing, etc.; winter sports-related goods for skiing and snowboarding, etc.; and other indoor and outdoor sports-related goods.

[0046] <Film> Another aspect of the present invention is a film containing a copolymer polyamide resin or a polyamide resin composition. The film may be a monolayer film consisting of only a copolymer polyamide resin layer, or a laminate film of two or more layers including a copolymer polyamide resin layer and another layer. Examples of the other layer include a layer containing a resin other than the copolymer polyamide resin, such as a thermoplastic resin or a thermosetting resin, or a layer made of a metal such as aluminum. Examples of resins other than the copolymer polyamide resin include ethylene-based resins such as low-density polyethylene, linear low-density polyethylene, ionomers, ethylene-vinyl alcohol copolymer (EVOH), ethylene-acrylic acid copolymer, ethylene-vinyl acetate copolymer, ethylene-acrylic acid ester copolymer, and ethylene-methacrylic acid copolymer; polyolefins such as polypropylene, modified polyolefins, polyesters, polyvinyl alcohol, polyamides other than copolymer polyamide resins, polyamide elastomers; and biomass plastics such as polylactic acid (PLA) and polyhydroxyalkanoates (PHA).

[0047] The thickness of the film can be appropriately selected depending on the application. For example, in the case of a monolayer film, the thickness is preferably 5 to 200 μm, more preferably 10 to 50 μm. In the case of a laminated film, the total thickness is preferably 10 to 1000 μm, more preferably 20 to 500 μm; and the thickness of the layer containing the copolymerized polyamide resin or polyamide resin composition is preferably 5 to 100 μm, more preferably 10 to 50 μm.

[0048] The film may be an unstretched film or a stretched film obtained by stretching the unstretched film. The stretching method is not particularly limited, and examples thereof include uniaxial stretching using heated rolls, simultaneous biaxial stretching using a tubular method, and sequential biaxial stretching using heated rolls or a tenter.

[0049] (Film Manufacturing Method) The method for manufacturing the film is not particularly limited, and for example, known manufacturing methods can be applied. For example, a copolymerized polyamide resin or a polyamide resin composition can be melt-kneaded using an extruder, and a monolayer film can be produced by a molding method such as a T-die molding method, an air-cooled inflation molding method, a water-cooled inflation molding method, or a triple bubble molding method. The laminated film can be directly laminated by coextrusion, lamination, or the like, or can be laminated via an adhesive or adhesive resin layer. Coextrusion is preferred because of its excellent productivity. When a laminated film is produced by a coextrusion method, for example, a coextrusion T-die molding method in which a copolymerized polyamide resin or a composition thereof, a thermoplastic resin or a composition thereof, etc. are melted in separate extruders and continuously extruded through a T-die and cooled with a casting roll to form a film; a coextrusion air-cooled inflation molding method in which the resins are continuously extruded through a circular die and cooled by air; or a coextrusion water-cooled inflation molding method in which the resins are continuously extruded through a circular die and cooled by contact with water, etc., can be used to produce a substantially unoriented unstretched film.

[0050] Of these, air-cooled inflation molding and water-cooled inflation molding (also simply referred to as "inflation molding" or "inflation molding") require simple equipment and allow the film width to be easily changed simply by adjusting the blow-up ratio, resulting in good workability and high productivity in film production. When used in air-cooled or water-cooled inflation molding or co-extrusion air-cooled or water-cooled inflation molding, copolymerized polyamide resins can suppress film curling. In particular, when a multilayer film containing a layer containing a copolymerized polyamide resin and a low-melting-point thermoplastic resin layer is produced by co-extrusion air-cooled or water-cooled inflation molding, thermal degradation and curling of the film can be suppressed, making this method preferred.

[0051] The conditions for forming an inflation-molded film are not particularly limited, but the resin temperature is preferably above the melting point of the raw resin used and below 300°C. In the present invention, the resin temperature can be, for example, 160°C to 250°C, preferably 160°C to 220°C. The blow-up ratio (also referred to as the blow ratio) refers to the ratio of the maximum bubble diameter to the die diameter. The blow-up ratio is preferably 1.1 to 3.0, more preferably 1.2 to 2.5. The take-up speed is determined by the thickness and width of the film and the extrusion rate, and can be adjusted within a range that maintains film formation stability. Generally, the take-up speed is preferably 1 to 150 m / min, more preferably 5 to 100 m / min.

[0052] Furthermore, in order to improve printability, lamination ability, or adhesive applicability, the film may be subjected to surface treatment such as corona discharge treatment, plasma treatment, flame treatment, acid treatment, etc. After such treatment, if necessary, the film may be subjected to secondary processing steps such as printing, lamination, adhesive application, and heat sealing, and then used for the respective intended applications.

[0053] (Applications of the film) The film has low water absorption and excellent abrasion resistance, so it can be used as a food packaging film. The film is also suitable for use as an inflation-molded film. Furthermore, the film can be used for various applications, such as electronic components, electrical components, household goods, office supplies, automobile and vehicle-related parts, building materials, and sporting goods, which are examples of applications of molded products.

[0054] <Monofilament> Yet another aspect of the present invention is a monofilament comprising a copolymer polyamide resin or a polyamide resin composition. The diameter of the monofilament is not particularly limited, but is preferably 0.5 to 20 mm, more preferably 1 to 5 mm. The monofilament may be a continuous fiber or a staple fiber.

[0055] (Monofilament Manufacturing Method) Monofilaments can be obtained by known manufacturing methods using copolymerized polyamide resins or polyamide resin compositions. Examples of methods for manufacturing monofilaments include melting polyamide resin pellets in an extruder or the like, extruding them through a spinning nozzle, and cooling them in a refrigerant bath such as water or trichloroethylene to produce undrawn yarns. In this case, the distance between the filament outlet of the spinning nozzle and the refrigerant liquid level is preferably maintained at approximately 10 to 300 mm.

[0056] The undrawn yarn may be further drawn and heat-set. Here, two-stage drawing, in which drawing is performed in two stages, is preferred. In the first stage of the two-stage drawing, the undrawn yarn is preferably drawn 2 to 5 times, more preferably 3 to 4 times, in steam or hot water. If the draw ratio is within this range, the knot strength tends to be further improved.

[0057] When stretching is performed in water vapor, the temperature range is preferably 95 to 120° C., more preferably 100 to 110° C. When the temperature of the water vapor is within this temperature range, the knot strength and transparency of the obtained monofilament tend to be further improved.

[0058] When stretching is performed in hot water, the temperature of the hot water is preferably 50 to 95° C., more preferably 60 to 90° C. When the temperature of the hot water is within this range, the knot strength and transparency of the obtained monofilament tend to be further improved.

[0059] In the second-stage drawing, the monofilament is preferably drawn 1.1 to 2.5 times, more preferably 1.2 to 2.5 times, in a gas atmosphere. The gas is not particularly limited, and examples thereof include inert gases such as helium, nitrogen, and argon, and air. The temperature of the gas atmosphere in the second-stage drawing is preferably 100 to 300°C, more preferably 120 to 300°C, even more preferably 150 to 250°C, and particularly preferably 180 to 250°C. When the second-stage drawing is performed within the above-mentioned temperature range and draw ratio, the knot strength and transparency of the resulting monofilament tend to be further improved.

[0060] The two-stage drawn monofilament is preferably heat-set. The two-stage drawn monofilament can be heat-set in a gas atmosphere of preferably 120 to 350°C, more preferably 160 to 350°C, and even more preferably 160 to 320°C while undergoing a 0 to 10% relaxation treatment. The temperature of the gas atmosphere during heat-setting can also be 150 to 320°C. When the temperature is within this range, the knot strength tends to be further improved.

[0061] In the above two-stage drawing and heat setting, the total draw ratio is preferably in the range of 4.0 to 7.0 times, more preferably 4.5 to 6.5 times, and even more preferably 5.5 to 6.0 times.

[0062] (Uses of Monofilaments) Monofilaments have low water absorption and excellent abrasion resistance, and therefore can be used as filaments, multifilaments, nets, and other structures for applications in fishing, industry, clothing, medicine, etc. Furthermore, monofilaments can be used in a variety of applications, including electronic components, electrical components, household goods, office supplies, automobile and vehicle-related parts, building materials, and sporting goods, which are exemplified as uses of molded products.

[0063] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0064] [Measurement of physical properties] (1) Melting point (Tm) and heat of fusion (ΔH) Using a DSC7020 model manufactured by Hitachi High-Tech Science Corporation, the polyamide resins of the Examples and Comparative Examples were heated to 300°C at a rate of 10°C / min under a nitrogen gas atmosphere, held at that temperature for 1 minute, cooled to 30°C at a rate of 10°C / min, and then heated again to 300°C at a rate of 10°C / min. The top temperature of the endothermic peak in the DSC curve during the second heating process was taken as the melting point (Tm), and the corresponding heat of fusion was taken as ΔH (unit: J / g).

[0065] (2) Crystallization Temperature (Tc) Using a Hitachi High-Tech Science DSC7020 model, the polyamide resins of the Examples and Comparative Examples were heated to 300°C at a rate of 10°C / min under a nitrogen gas atmosphere, held at that temperature for 1 minute, and then cooled to 30°C at a rate of 10°C / min. The top temperature of the exothermic peak in the DSC curve during the cooling process was recorded as the crystallization temperature (Tc). In measuring the crystallization temperature (Tc), if no exothermic peak was present during the cooling process, the result of the crystallization temperature (Tc) was recorded as "n.d."

[0066] (3) Calculation of the Proportion of Each Structural Unit and Biomass Raw Material The proportion of each structural unit and biomass raw material in the polyamide resins of the Examples and Comparative Examples was calculated from the amount of raw material charged, assuming that all of the raw materials for the polyamide resin had reacted. The proportion of biomass raw material is the proportion of the amount (mass) of raw material derived from biomass charged in 100% by mass of the total amount of raw materials charged, assuming that all of the raw materials for the polyamide resin had reacted. Specifically, the proportions of each structural unit and biomass raw material were as follows: contribution of 1,5-pentamethylenediamine to a molecular weight of 102.18 = 100.18 (= 102.18 - 2.00) g / mol; contribution of 1,6-hexamethylenediamine to a molecular weight of 116.20 = 114.20 (= 116.20 - 2.00) g / mol; contribution of adipic acid to a molecular weight of 146.14 = 112.14 (= 146.14 The contribution of sebacic acid to a molecular weight of 202.25 = 168.25 (= 202.25 - 34.00) g / mol, the contribution of 12-aminododecanoic acid to a molecular weight of 215.34 = 197.34 (= 215.34 - 18.00) g / mol, and the contribution of 6-aminocaproic acid to a molecular weight of 131.17 = 113.17 (= 131.17 - 18.00) g / mol.

[0067] (4) Equilibrium Water Absorption Using polyamide resin flakes or pellets from the Examples and Comparative Examples, a heat press manufactured by Shinto Metal Industries Co., Ltd. was used to preheat the polyamide resin flakes or pellets at a temperature of melting point + 30°C for 3 minutes, then heat-pressed at 5 MPa for 1 minute, and then cooled and pressed at 30°C and 5 MPa for 3 minutes to produce an unstretched polyamide sheet measuring 20 mm x 80 mm x 2 mm. The resulting sheet was vacuum-dried at 80°C for 48 hours, and its mass was measured. The sheet was then immersed in water at 23°C for 800 hours, and the surface moisture of the removed sheet was lightly absorbed with a cloth, after which its mass was measured. The equilibrium water absorption was calculated from the masses of the sheet before and after immersion in water using the following formula: Equilibrium Water Absorption = [(Sheet Mass After Immersion in Water - Sheet Mass Before Immersion in Water) / Sheet Mass Before Immersion in Water] x 100

[0068] (5) Abrasion Volume Using polyamide resin chips or pellets from the Examples and Comparative Examples, a heat press manufactured by Shinto Metal Industries Co., Ltd. was used. The polyamide resin chips or pellets were preheated at a temperature of melting point +30°C for 3 minutes, then heat-pressed at 5 MPa for 1 minute, and then cooled and pressed at 30°C and 5 MPa for 3 minutes to produce two 45 mm x 45 mm x 1 mm unstretched polyamide sheets. The resulting sheets were vacuum-dried at 80°C for 48 hours and sealed in an aluminum bag. One of the two sheets was used as a sample for the abrasion test, and the other was used as a sample for measuring water absorption to correct for the water absorption of the sample (dried sheet) during the abrasion test. First, the aluminum bag was opened, and the masses of the two samples were measured. G (garnet)-50 abrasive paper cut to a length of 157 mm and a width of 12 mm was attached to the abrasion wheel of a reciprocating flat abrasion tester manufactured by Suga Test Instruments Co., Ltd., and abrasion tests were performed on the samples for the abrasion test under conditions of a load of 3000 g, a stroke of 30 mm, and 120 reciprocations. After the test, resin powder generated on the sample due to abrasion was brushed off, and the mass of the sample was measured. At approximately the same time, the mass of the sample for measuring water absorption was measured. The mass obtained by adding the mass increase (apparent water absorption) of the sample for measuring water absorption to the difference in mass of the sample for abrasion test before and after the abrasion test was taken as the abrasion amount. Abrasion amounts of less than 11.5 mg were considered to be excellent in abrasion resistance.

[0069] (6) Notched Charpy Impact Strength Using the polyamide resin chips or pellets of the Examples and Comparative Examples, polyamide test pieces for Charpy impact tests were prepared using an injection molding machine SE100D manufactured by Sumitomo Heavy Industries, Ltd. at a cylinder temperature of 250 ° C and a mold temperature of 30 ° C., and immediately sealed in an aluminum bag for storage. The test pieces were immediately removed from the aluminum bag and their Charpy impact strength was measured at test temperatures of 23 ° C and -40 ° C in accordance with ISO 179 / 1eA using a Charpy impact tester No. 141-PC manufactured by Yasuda Seiki Seisakusho Co., Ltd. (all test pieces were in a dry state). Regarding the notation of the measurement results in Table 4, if the test piece was completely destroyed by the test, "C" was added to the measured value, and if it was not completely destroyed, "NB" was added to the measured value.

[0070] (7) Tensile Modulus Using the polyamide resin flakes or pellets of the Examples and Comparative Examples, a heat press manufactured by Shinto Metal Industries Co., Ltd. was used. The polyamide resin flakes or pellets were preheated at a temperature of melting point +30°C for 3 minutes, then heat-pressed at 5 MPa for 1 minute, and then cold-pressed at 30°C and 5 MPa for 3 minutes to produce unstretched polyamide sheets measuring 100 mm x 100 mm x 0.1 mm. The resulting sheets were cut into 90 mm long x 10 mm wide strips to prepare samples for tensile testing. The tensile modulus of the tensile test samples was measured in accordance with ISO 527-1 and 2 under conditions of an atmosphere of 23°C and 50% RH, a chuck distance of 50 mm, and a crosshead speed of 300 mm / min. A tensile modulus of 500 to 1,000 MPa was considered to have an excellent balance of strength and flexibility.

[0071] [Raw materials used] (1) Nylon salt Equimolar salt of 1,6-hexamethylenediamine and adipic acid (nylon 66 salt): manufactured by Asahi Kasei Corporation (derived from fossil raw materials, 48% by mass aqueous solution) (2) Diamine 1,5-pentamethylenediamine: manufactured by CJ Research (derived from biomass, purity: 99.90% by mass) 1,6-hexamethylenediamine: manufactured by Tokyo Chemical Industry Co., Ltd. (derived from fossil raw materials, purity: 99% by mass) (3) Dicarboxylic acid Adipic acid: manufactured by Asahi Kasei Corporation (derived from fossil raw materials, purity: 99.8% by mass) Sebacic acid: manufactured by Casda Biomaterials (derived from biomass, purity: 99.5% by mass) (4) Aminocarboxylic acid 12-aminododecanoic acid: manufactured by UBE Corporation (derived from fossil raw materials, purity: 99.7% by mass) 6-Aminocaproic acid: manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. (derived from fossil raw materials, purity: 97.0% by mass) (5) Organic solvents 2-propanol: manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. (purity: 99.7% by mass) Ethanol: manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. (purity: 99.5% by mass)

[0072] Example A Synthesis of Nylon 56 Salt 32.42 kg of adipic acid and 273 kg of 2-propanol were placed in a 700 L reaction vessel and heated to 40°C to dissolve the adipic acid. 22.67 kg of 1,5-pentamethylenediamine was then slowly added over 71 minutes. Heat of neutralization and heat of crystallization were generated, but the solution temperature was adjusted to fall within the range of 40°C to 50°C during the addition. After the addition of 1,5-pentamethylenediamine was completed, the solution was stirred for 30 minutes while maintaining the temperature at 35°C to 40°C, and then cooled and stirred for 2 hours while maintaining the temperature at 0°C to 5°C. The precipitated nylon 56 salt was collected as a cake and then dried under reduced pressure at 60°C for 48 hours to obtain 54.8 kg of nylon 56 salt.

[0073] Example A1: A 1-L polymerization vessel was charged with 237.5 g of nylon 56 salt, 12.5 g of 12-aminododecanoic acid, and 50.0 g of degassed ion-exchanged water. The atmosphere inside the polymerization vessel was replaced with nitrogen, then sealed and heated to 200°C. The pressure inside the polymerization vessel was then adjusted to 1.3 MPa with stirring, and polymerization was carried out for 3 hours. The pressure inside the polymerization vessel was released to atmospheric pressure over 40 minutes while the temperature inside the polymerization vessel was raised to 280°C. After pressure release, polymerization was carried out for 2 hours under a nitrogen stream of 200 mL / min. The stirrer was then stopped, and nitrogen was introduced to pressurize the vessel to 1.0 MPa. After pressurization, the vessel was extracted as strands and pelletized. The polyamide pellets were dried under reduced pressure at 90°C for 48 hours to obtain the copolymerized polyamide resin of Example A1. The raw material charge amounts, composition ratios in the polymer, and physical properties of the copolymerized polyamide resin of Example A1 are shown in Table 1. The randomness of the copolymerized polyamide resin of Example A1 was also measured. 13 The C-NMR spectrum confirmed that the copolymer was a random copolymer.

[0074] Examples A2 to A4 Copolyamide resins of Examples A2 to A4 were obtained in the same manner as in Example A1, except that the amounts of nylon 56 salt and 12-aminododecanoic acid used as raw materials were changed as shown in Table 1.

[0075] Example A5: A 1-L polymerization vessel was charged with 150.0 g of nylon 56 salt, 100.0 g of 12-aminododecanoic acid, and 50.0 g of degassed ion-exchanged water. The atmosphere inside the polymerization vessel was replaced with nitrogen, then sealed and heated to 200°C. The pressure inside the polymerization vessel was then adjusted to 1.3 MPa with stirring, and polymerization was carried out for 3 hours. The pressure inside the polymerization vessel was released to atmospheric pressure over 40 minutes while the temperature inside the polymerization vessel was raised to 250°C. After pressure release, polymerization was carried out for 2 hours under a nitrogen stream of 200 mL / min. The stirrer was then stopped, and nitrogen was introduced to pressurize the vessel to 1.0 MPa. After pressurization, the vessel was extracted as strands and pelletized. The polyamide pellets were dried under reduced pressure at 90°C for 48 hours to obtain the copolymerized polyamide resin of Example A5. The raw material charge amounts, component ratios in the polymer, and physical properties of the copolymerized polyamide resin of Example A5 are shown in Table 1. The randomness of the copolymerized polyamide resin of Example A5 was also measured. 13 The C-NMR spectrum confirmed that the copolymer was a random copolymer.

[0076] Examples A6 to A10 Copolyamide resins of Examples A6 to A10 were obtained in the same manner as in Example A5, except that the amounts of nylon 56 salt and 12-aminododecanoic acid used as raw materials were changed as shown in Table 1.

[0077] A 1 L polymerization vessel was charged with 205.0 g of 6-aminocaproic acid and 93.75 g of a nylon 66 salt aqueous solution (48 mass % aqueous solution), and polymerization was carried out in the same manner as in Example A5, followed by pelletization to obtain a copolymerized polyamide resin of Comparative Example A1. The amounts of raw materials charged, the composition ratios in the polymer, and physical properties of the copolymerized polyamide resin of Comparative Example A1 are shown in Table 1.

[0078] A 1-L polymerization vessel was charged with 100.0 g of 6-aminocaproic acid, 150.0 g of nylon 56 salt, and 50.0 g of degassed ion-exchanged water, and polymerization was carried out in the same manner as in Example A5, followed by pelletization to obtain a copolymerized polyamide resin of Comparative Example A2. The amounts of raw materials charged, the composition ratios in the polymer, and physical properties of the copolymerized polyamide resin of Comparative Example A2 are shown in Table 1.

[0079] A 1-L polymerization vessel was charged with 250.0 g of nylon 56 salt and 50.0 g of degassed ion-exchanged water, and polymerization was carried out in the same manner as in Example A1. The resulting mixture was pelletized to obtain a homopolyamide resin of Comparative Example A3. The amounts of raw materials charged, the composition ratios in the polymer, and the physical properties of the homopolyamide resin of Comparative Example A3 are shown in Table 1.

[0080] A 1-L polymerization vessel was charged with 250.0 g of 12-aminododecanoic acid and 50.0 g of degassed ion-exchanged water, and polymerization was carried out in the same manner as in Example A5, followed by pelletization to obtain a homopolyamide resin of Comparative Example A4. The amounts of raw materials charged, the composition ratios in the polymer, and the physical properties of the homopolyamide resin of Comparative Example A4 are shown in Table 1.

[0081] Comparative Example A5 60 parts by mass of the homopolyamide resin of Comparative Example A3 and 40 parts by mass of the homopolyamide resin of Comparative Example A4 were mixed to obtain a pellet mixture of Comparative Example A5. The constituent ratios and physical properties of the polymer of Comparative Example A5 are shown in Table 1. Note that, since Comparative Example A5 is a pellet mixture, the column for the amount of raw material charged in Table 1 was omitted.

[0082] Table 1 shows the composition ratios of each structural unit in the polymer (calculated on a mass basis from the amounts of raw materials charged), DSC measurement data for the obtained copolyamide resins, and the proportions of biomass raw materials for Examples A1 to A10 and Comparative Examples A1 to A5. In Table 1, n.d. indicates that no crystallization temperature peak was detected.

[0083]

[0084] The equilibrium water absorption and abrasion data for the polyamide resins of Example A2 and Comparative Examples A1 and A3 are shown in Table 2. Similarly, the equilibrium water absorption and abrasion data for the polyamide resins of Examples A5 and A8 and Comparative Examples A2, A4 and A5 are shown in Table 3.

[0085]

[0086]

[0087] Table 2 shows that Example A2, which contains structural units A1 derived from the equimolar reaction product of pentamethylenediamine and adipic acid and structural units B derived from 12-aminododecanoic acid, has a lower equilibrium water absorption than Comparative Examples A1 and A3. Similarly, Table 3 shows that Examples A5 and A8 have a lower equilibrium water absorption than Comparative Examples A2 and A5. Furthermore, Tables 2 and 3 show that Examples A2, A5, and A8 all have a wear amount of less than 11.5 mg, demonstrating superior wear resistance compared to Comparative Examples A1 to A5. In particular, a comparison of Example A5 and Comparative Example A5 shows that the copolymerized polyamide resin of Example A5, which contains structural units A1 and B, has significantly superior equilibrium water absorption and wear resistance compared to Comparative Example A5, which contains a homopolyamide resin composed of structural units A1 and a homopolyamide resin composed of structural units B mixed to have the same composition.

[0088] Table 4 shows the data on the equilibrium water absorption, abrasion loss and Charpy impact strength for the copolyamide resins of Example A5 and Comparative Example A1.

[0089] Table 4 shows that Example A5, which contains structural units A1 derived from equimolar reactants of pentamethylenediamine and adipic acid and structural units B derived from 12-aminododecanoic acid, has a lower water absorption rate, is superior in abrasion resistance and impact strength, and has a higher bio content than Comparative Example A1.

[0090] Example B Synthesis of Nylon 510 Salt 24.27 kg of sebacic acid and 184 kg of 2-propanol were placed in a 700 L reaction vessel and heated to 40°C to dissolve the sebacic acid. 12.27 kg of 1,5-pentamethylenediamine was then slowly added over 65 minutes. Heat of neutralization and heat of crystallization were generated, but the solution temperature was adjusted to fall within the range of 40°C to 50°C during the addition. After the addition of 1,5-pentamethylenediamine was completed, the solution was stirred for 30 minutes while maintaining the temperature at 35°C to 40°C, and then cooled and stirred for 2 hours while maintaining the temperature at 0°C to 5°C. The precipitated nylon 510 salt was collected as a filter cake and then dried under reduced pressure at 60°C for 48 hours to obtain 36.3 kg of nylon 510 salt.

[0091] Synthesis of Nylon 66 Salt: 250.0 g of adipic acid and 1900 ml of ethanol were placed in a 3 L separable flask and heated to 40°C to dissolve the adipic acid. 198.8 g of 1,6-hexamethylenediamine and 200 ml of ethanol were placed in a 500 mL beaker and stirred to obtain a homogeneous solution. The 1,6-hexamethylenediamine solution in the beaker was slowly added to the adipic acid solution in the separable flask over 90 minutes. Heat of neutralization and crystallization was generated, but the solution temperature was adjusted to fall within the range of 40°C to 50°C during the addition. After the addition of the 1,6-hexamethylenediamine solution was completed, the solution was stirred for 30 minutes while maintaining the temperature at 35°C to 40°C, and then cooled and stirred for 2 hours while maintaining the temperature at 0°C to 5°C. The precipitated nylon 66 salt was collected as a filter cake and then dried under reduced pressure at 60°C for 15 hours to obtain 442.3 g of nylon 66 salt.

[0092] Example B1 A 50 cc autoclave was charged with 6.65 g of nylon 510 salt, 0.35 g of 12-aminododecanoic acid, and 1.4 g of degassed ion-exchanged water. The autoclave was then purged with nitrogen, sealed, and immersed in a 200°C oil bath. A prepolymer was obtained by pressure polymerization for 200 minutes at a pressure of 0.5 MPa without stirring. The resulting prepolymer was transferred to a glass test tube, and the glass test tube was immersed in a 250°C oil bath and polymerized for 190 minutes under a 50 mL / min nitrogen stream while stirring to obtain a polyamide resin. The resulting resin was shredded into 3-5 mm square pieces and dried under reduced pressure at 90°C for 48 hours to obtain fine pieces of the copolymerized polyamide resin of Example B1. Table 5 shows the raw material charge amounts, composition ratios in the polymer, and physical properties of the copolymerized polyamide resin of Example B1. The randomness of the copolymerized polyamide resin of Example B1 was also measured. 13 The C-NMR spectrum confirmed that the copolymer was a random copolymer.

[0093] Example B2: A 1-L polymerization vessel was charged with 225.0 g of nylon 510 salt, 25.0 g of 12-aminododecanoic acid, and 50.0 g of degassed ion-exchanged water. The atmosphere inside the polymerization vessel was replaced with nitrogen, then sealed and heated to 200°C. The pressure inside the polymerization vessel was then adjusted to 1.3 MPa with stirring, and polymerization was carried out for 3 hours. The pressure inside the polymerization vessel was released to atmospheric pressure over 40 minutes while raising the temperature to 250°C. After pressure release, polymerization was carried out for 100 minutes under a nitrogen stream of 200 mL / min. The stirrer was then stopped, and nitrogen was introduced to pressurize the mixture to 1.0 MPa. After pressurization, the mixture was withdrawn as strands and pelletized. The polyamide pellets were dried under reduced pressure at 90°C for 48 hours to obtain the copolymerized polyamide resin of Example B2. The raw material charge amounts, component ratios in the polymer, and physical properties of the copolymerized polyamide resin of Example B2 are shown in Table 5. The randomness of the copolymerized polyamide resin of Example B2 was also measured. 13 The C-NMR spectrum confirmed that the copolymer was a random copolymer.

[0094] Examples B3, B4, B6, B7 and B8 Copolymerized polyamide resins of Examples B3, B4, B6, B7 and B8 were obtained in the same manner as in Example B1, except that the amounts of raw materials nylon 510 salt and 12-aminododecanoic acid charged were changed as shown in Table 5.

[0095] Examples B5, B9 and B10 Copolyamide resins of Examples B5, B9 and B10 were obtained in the same manner as in Example B2, except that the amounts of nylon 510 salt and 12-aminododecanoic acid used as raw materials were changed as shown in Table 5.

[0096] A 1-L polymerization vessel was charged with 150.0 g of nylon 510 salt, 100.0 g of 6-aminocaproic acid, and 50.0 g of degassed ion-exchanged water, and polymerization was carried out in the same manner as in Example B2. The mixture was pelletized to obtain a copolymerized polyamide resin of Comparative Example B1. The amounts of raw materials charged, the composition ratios in the polymer, and the physical properties of the copolymerized polyamide resin of Comparative Example B1 are shown in Table 5.

[0097] Comparative Example B2: A 1 L polymerization vessel was charged with 225.0 g of nylon 66 salt, 25.0 g of 12-aminododecanoic acid, and 50.0 g of degassed ion-exchanged water. The atmosphere inside the polymerization vessel was replaced with nitrogen, then sealed and heated to 200°C. The pressure inside the polymerization vessel was then adjusted to 1.3 MPa with stirring, and polymerization was carried out for 3 hours. The pressure inside the polymerization vessel was released to atmospheric pressure over 40 minutes while raising the temperature to 280°C. After pressure release, polymerization was carried out for 100 minutes under a nitrogen stream of 200 mL / min, after which the stirrer was stopped and nitrogen was introduced to pressurize to 1.0 MPa. After pressurization, the mixture was withdrawn as strands and pelletized. The polyamide pellets were dried under reduced pressure at 90°C for 48 hours to obtain the copolymerized polyamide resin of Comparative Example B2. Table 5 shows the raw material charge amounts, component ratios in the polymer, and physical properties of the copolymerized polyamide resin of Comparative Example B2.

[0098] Reference Example B3: A 1-L polymerization vessel was charged with 150.0 g of nylon 66 salt, 100.0 g of 12-aminododecanoic acid, and 50.0 g of degassed ion-exchanged water, and polymerization was carried out in the same manner as in Example B2. The mixture was pelletized to obtain a copolymerized polyamide resin of Reference Example B3. The amounts of raw materials charged, the composition ratios in the polymer, and the physical properties of the copolymerized polyamide resin of Reference Example B3 are shown in Table 5.

[0099] Comparative Example B4: A 1 L polymerization vessel was charged with 205.0 g of 6-aminocaproic acid, 45.0 g of 12-aminododecanoic acid, and 50.0 g of degassed ion-exchanged water, and polymerization was carried out in the same manner as in Example B2. The mixture was pelletized to obtain a copolymerized polyamide resin of Comparative Example B4. The raw material charging amounts, component ratios in the polymer, and physical properties of the copolymerized polyamide resin of Comparative Example B4 are shown in Table 5.

[0100] A 1-L polymerization vessel was charged with 250.0 g of 12-aminododecanoic acid and 50.0 g of degassed ion-exchanged water, and polymerization was carried out in the same manner as in Example B2. The resulting mixture was pelletized to obtain a homopolyamide resin of Comparative Example B5. The amounts of raw materials charged, the composition ratios in the polymer, and the physical properties of the homopolyamide resin of Comparative Example B5 are shown in Table 5.

[0101] A 1-L polymerization vessel was charged with 250.0 g of nylon 510 salt and 50.0 g of degassed ion-exchanged water, and polymerization was carried out in the same manner as in Example B2, followed by pelletization to obtain a homopolyamide resin of Comparative Example B6. The amounts of raw materials charged, the composition ratios in the polymer, and the physical properties of the homopolyamide resin of Comparative Example B6 are shown in Table 5.

[0102] Table 5 shows the composition ratios (calculated by mass from the amounts of raw materials charged) of each structural unit in the polymer of Examples B1 to B10, Comparative Examples B1, B2, and B4 to B6, and Reference Example B3, as well as the DSC measurement data and the proportion of biomass raw material of the resulting polyamide resin. In Table 5, n.d. indicates that no peak at the crystallization temperature was detected.

[0103]

[0104] Table 6 shows data on equilibrium water absorption, abrasion loss and tensile modulus for the polyamide resins of Examples B2, B5, B9 and B10, Comparative Examples B1, B2 and B4 to B6 and Reference Example B3.

[0105]

[0106] Tables 5 and 6 show that the copolymerized polyamide resins of Examples B2, B5, B9, and B10, which contain structural unit A2 derived from the reaction product of equimolar amounts of pentamethylenediamine and sebacic acid and structural unit B derived from 12-aminododecanoic acid, have low equilibrium water absorption, excellent abrasion resistance and tensile modulus, and a high bio content.

[0107] Comparative Example B1, which contained the structural unit A2 and a structural unit derived from 6-aminocaproic acid, had a high equilibrium water absorption rate, poor abrasion resistance, and a tensile modulus outside the acceptable range. Comparative Example B2, which contained a structural unit derived from a nylon 66 salt different from structural unit A and a structural unit derived from 12-aminododecanoic acid, had a high equilibrium water absorption rate, poor abrasion resistance, and a tensile modulus outside the acceptable range. Furthermore, Reference Example B3, which was composed of structural units similar to those of Comparative Example B2 but had a different composition ratio of the structural units, had abrasion resistance and tensile modulus within the acceptable range, but had a higher equilibrium water absorption rate than Examples B2, B5, B9, and B10. Comparative Example B4, which contained a structural unit derived from 6-aminocaproic acid and a structural unit derived from 12-aminododecanoic acid, had a high equilibrium water absorption rate and poor abrasion resistance. Comparative Example B5, which contained only structural unit B, had excellent equilibrium water absorption rate but poor abrasion resistance, and the tensile modulus significantly exceeded the upper limit of the acceptable range, resulting in poor flexibility. Furthermore, the polyamide resins of Comparative Examples B2, B4, and B5 and Reference Example B3 did not use biomass raw materials and could not contribute to the creation of a sustainable society. Comparative Example B6, which contained only structural unit A, had poor abrasion resistance and a tensile modulus outside the acceptable range.

[0108] The copolyamide resin of the present invention can be suitably used for applications such as molded articles produced by various molding methods, food packaging films, etc. The copolyamide resin can contribute to the achievement of Goal 12 of the SDGs (Sustainable Development Goals), etc.

Claims

1. A structural unit A1 derived from a reaction product of equimolar amounts of pentamethylenediamine and adipic acid represented by the following formula (A1): and a structural unit A2 derived from a reaction product of equimolar amounts of pentamethylenediamine and sebacic acid, represented by the following formula (A2): and a structural unit B derived from at least one aminocarboxylic acid selected from 10-aminodecanoic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid, and / or at least one lactam selected from decalactam, undecalactam, and dodecalactam.

2. The copolymer polyamide resin according to claim 1, wherein the structural unit B is a unit derived from 12-aminododecanoic acid and / or dodecalactam.

3. A copolyamide resin according to claim 1 or 2, in which the proportion of biomass raw material in the copolyamide resin is 3% or more by mass.

4. The copolyamide resin according to claim 1 or 2, wherein the structural unit A is structural unit A1, and the mass ratio of structural unit A1 / structural unit B is 95 / 5 to 9 / 91.

5. A copolyamide resin according to claim 1 or 2, in which the structural unit A is structural unit A2, and the mass ratio of structural unit A2 / structural unit B is 97 / 3 to 7 / 93.

6. The copolyamide resin according to claim 1 or 2, wherein the structural unit A is structural unit A1, and the melting point of the copolyamide resin as measured by DSC is 130 to 250°C.

7. The copolyamide resin according to claim 1 or 2, wherein the structural unit A is structural unit A2, and the melting point of the copolyamide resin as measured by DSC is 100 to 250°C.

8. The copolyamide resin according to claim 1 or 2, wherein the structural unit A is a structural unit A1, and the crystallization temperature of the copolyamide resin as measured by DSC is 110 to 200°C.

9. A polyamide resin composition comprising the copolymer polyamide resin according to claim 1 or 2.

10. A molded article comprising the copolymer polyamide resin according to claim 1 or 2.

11. A film comprising the copolymer polyamide resin according to claim 1 or 2.

12. A monofilament comprising the copolymer polyamide resin according to claim 1 or 2.

Citation Information

Patent Citations

  • PA6-56 copolymerized material and preparation method thereof

    CN108250433A

  • Polyamide resin and polyamide resin composition

    JP2010121113A

  • Polyamide resin composition excellent in low temperature impact property, and molded article thereof

    JP2011207979A

  • Storage method of polyamide pellet

    JP2016069557A

  • Polyamide molded article

    JP2018012761A