Transparent insulating material

The integration of a water-repellent fluorinated alkyl group in cellulose nanofiber-based transparent heat insulating materials addresses the issue of maintaining transparency under high humidity, ensuring effective insulation and broad applicability in applications like laminated glass and double glazing.

WO2024219356A1PCT designated stage expired Publication Date: 2024-10-24FUJIFILM CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014975
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-20
Filing Date
2024-04-15
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Transparent heat insulating materials made from cellulose nanofibers struggle to maintain transparency under high humidity conditions due to water absorption, which affects their structural integrity and insulation properties.

Method used

A transparent heat insulating material comprising cellulose nanofibers with a water-repellent component, specifically a compound having a fluorinated alkyl group, is developed, with a fiber diameter of 3 to 40 nm and a maximum length of 1000 mm, ensuring minimal water absorption and maintaining transparency even in humid environments.

Benefits of technology

The material effectively maintains transparency and insulation properties under high humidity, with a water contact angle of 90 degrees or more, achieving transmittance of 30% or more, and can be applied in various applications such as laminated glass and double glazing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

The present invention addresses the problem of providing a transparent insulating material capable of maintaining transparency in high humidity. A transparent insulating material according to the present invention comprises a cellulose porous body, wherein the cellulose porous body contains cellulose nanofibers and a water-repellent component, and the fiber diameter of the cellulose porous body is 3-40 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Transparent insulation

[0001] The present invention relates to a transparent heat insulating material. More specifically, the present invention relates to a transparent heat insulating material made of a porous cellulose material.

[0002] Cellulose nanofibers (hereinafter also referred to as "CNF") are fibers produced from pulp and other cellulose-based raw materials through pulp milling and chemical processing. CNF is lightweight and strong, and is therefore expected to be used in a variety of applications. CNF is also a natural material derived from plants or living organisms, and is attracting attention for its low environmental impact upon disposal. Porous materials have also been used in a variety of applications due to their structure, specific surface area, and other factors. Here, porous cellulose materials containing CNF are expected to have the lightweight and high strength properties of CNF.

[0003] Generally, CNF is hydrophilic, and therefore the surface (internal surface) of the material constituting the CNF-containing porous cellulose body is also generally hydrophilic. Porous bodies have the property of adsorbing other substances to their internal surfaces, and porous cellulose bodies containing CNF with hydrophilic internal surfaces tend to adsorb water. Therefore, porous cellulose bodies containing CNF may not be able to withstand use under high humidity conditions. To address this problem, Patent Document 1 below discloses a porous cellulose body containing a water-repellent component, which is porous, and describes that such porous cellulose bodies have water repellency.

[0004] Patent No. 6212622

[0005] Because the porous cellulose material containing CNF is an aerogel, it has excellent heat insulating properties. Therefore, the porous cellulose material containing CNF can be used as a heat insulating material. Furthermore, such heat insulating materials may be required to have transparency depending on the application. Here, heat insulating materials may be used in high-humidity environments, and therefore may be required to maintain their transparency even in high-humidity environments. The present inventors have examined the porous cellulose material described in Patent Document 1 and found that it either does not have sufficient transparency or does not maintain sufficient transparency under high-humidity conditions, and that further improvement is necessary.

[0006] Therefore, an object of the present invention is to provide a transparent heat insulating material that can maintain its transparency under high humidity conditions.

[0007] The present inventors have conducted extensive research to solve the above problems and have completed the present invention. That is, they have found that the above problems can be solved by the following configuration.

[0008] [1] A transparent insulating material made of a porous cellulose body, wherein the porous cellulose body contains cellulose nanofibers and a water-repellent component, and the fiber diameter of the porous cellulose body is 3 to 40 nm. [2] The transparent insulating material according to [1], which has a maximum length of 1,000 mm or more. [3] The transparent insulating material according to [1] or [2], which has a water contact angle of 90 degrees or more. [4] The transparent insulating material according to any one of [1] to [3], wherein the water-repellent component is a compound having a fluorinated alkyl group. [5] The transparent insulating material according to [4], wherein the fluorinated alkyl group in the compound having a fluorinated alkyl group has 4 to 12 carbon atoms. [6] The transparent insulating material according to [4] or [5], wherein the compound having a fluorinated alkyl group is an alkoxysilane having a fluorinated alkyl group or a condensate of the alkoxysilane. [7] The transparent insulating material according to [6], wherein the alkoxysilane is a compound represented by formula (I) described below.

[0009] According to the present invention, a transparent heat insulating material capable of maintaining transparency under high humidity conditions can be provided.

[0010] The present invention will be described in detail below. The following description of the components may be based on representative embodiments of the present invention, but the present invention is not limited to such embodiments.

[0011] The meaning of each description in this specification is as follows: In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits.

[0012] <Transparent Insulation Material> The transparent insulation material of the present invention is a transparent insulation material made of a porous cellulose body, which contains cellulose nanofibers (CNF) and a water-repellent component, and the fiber diameter of the porous cellulose body is 3 to 40 nm. The mechanism by which the transparent insulation material of the present invention can maintain transparency under high humidity conditions is not entirely clear, but the inventors speculate as follows. The transparent insulation material of the present invention is made of a porous cellulose body, and since the porous cellulose body has a fiber diameter of 3 to 40 nm, it is thought that light scattering is easily reduced and transparency is excellent. Here, water adsorbed on the inner surface of the porous cellulose body can aggregate the fibers constituting the porous cellulose body due to its surface tension, so when water is adsorbed on the inner surface of the porous cellulose body, the fiber diameter of the porous cellulose body can increase. On the other hand, since the porous cellulose body that is the transparent insulation material of the present invention contains CNF and a water-repellent component, it is thought that the action of the water-repellent component makes it difficult for water to be adsorbed on the inner surface of the porous cellulose body, and therefore the porous cellulose body is unlikely to absorb water even under high humidity conditions. Therefore, it is thought that the transparent insulation material of the present invention maintains the above-mentioned fiber diameter, and as a result, transparency can be maintained under high humidity conditions.

[0013] It is also preferable that the maximum length of the transparent insulating material is 1000 mm or more, as this expands the range of applications for the transparent insulating material. The maximum length refers to the maximum length of the continuously formed porous cellulose body. For example, if the transparent insulating material is plate-shaped and has a rectangular shape when viewed from a direction perpendicular to one surface of the plate, the maximum length of the transparent insulating material corresponds to the length of the long side of the rectangle. Furthermore, if the transparent insulating material is plate-shaped and has a circular shape when viewed from a direction perpendicular to one surface of the plate, the maximum length of the transparent insulating material corresponds to the diameter of the circle. A method for obtaining a transparent insulating material (porous cellulose body) having a maximum length of 1000 mm or more will be described in detail later.

[0014] It is also preferable that the transparent insulating material have a water contact angle of 90 degrees or more, since this allows the transparent insulating material to better maintain its transparency under high humidity conditions. "The transparent insulating material has a water contact angle of 90 degrees or more" means that the water contact angle on the surface of the transparent insulating material is 90 degrees or more. The method for measuring the contact angle of the transparent insulating material shall follow the method described in the examples.

[0015] The transmittance of the transparent heat insulating material is preferably 30% or more, more preferably 50% or more, even more preferably 70% or more, and particularly preferably 90% or more. The transmittance of the transparent heat insulating material is usually less than 100%. The transmittance of the transparent heat insulating material can be increased by reducing the fiber diameter of the cellulose porous body described below. The transmittance of the transparent heat insulating material is measured according to the method described in the examples.

[0016] The porous cellulose material constituting the transparent heat insulating material will be described in detail below.

[0017] <Porous cellulose body> The transparent heat insulating material of the present invention is made of a porous cellulose body. As described above, the porous cellulose body contains CNF and a water-repellent component, and the fiber diameter of the porous cellulose body is 3 to 40 nm.

[0018] In this specification, the fiber diameter of the porous cellulose body is measured by small angle X-ray scattering (SAXS). Specifically, X-rays are first incident on the porous cellulose body to obtain a pre-treatment scattering curve. The scattering intensity in this pre-treatment scattering curve is normalized based on the intensity of the incident X-rays transmitted through the beam stopper to obtain a normalized scattering curve for the porous cellulose body. A blank measurement is also performed, and a normalized scattering curve for the medium (air) is obtained in the same manner. The scattering curve I(q) for the fibers constituting the porous cellulose body is obtained by subtracting the normalized scattering curve for the medium from the normalized scattering curve for the porous cellulose body. Here, q is a scattering vector calculated from the following equation using the scattering angle 2θ. q = 4 * π * (sin(θ)) / λ (π: pi, 2θ: scattering angle [rad], λ: wavelength of X-rays [nm]) When the scattering curve I(q) of the obtained porous cellulose material is plotted on a double logarithmic graph, a region where the slope is linear appears. For this region, a Guinier plot for the cross section is created, and the scattering intensity average fiber diameter Dc is calculated using the following formula: q * I(q) ∝ exp(-(Dc 2 * q 2 ) / 16) The scattering intensity average fiber diameter Dc obtained by the above formula is the fiber diameter of the porous cellulose material.

[0019] As described above, in the present invention, the fiber diameter of the porous cellulose body is 3 to 40 nm, preferably 5 to 40 nm, and more preferably 10 to 40 nm. Furthermore, in terms of achieving superior transparency for the transparent heat insulating material, the fiber diameter of the porous cellulose body is preferably 3 to 30 nm, and more preferably 5 to 20 nm. On the other hand, in terms of enabling the transparent heat insulating material to better maintain its transparency under high humidity conditions, the fiber diameter of the porous cellulose body is preferably 10 to 40 nm, and more preferably 20 to 40 nm. The fiber diameter of the porous cellulose body can be adjusted, for example, by the fiber diameter and type of CNF used, the method for forming the porous cellulose body, etc.

[0020] The CNF and water-repellent component contained in the porous cellulose material, as well as other components that may be contained therein, will be described below.

[0021] [Cellulose Nanofibers] The cellulose nanofibers (CNFs) contained in the transparent heat insulating material of the present invention are not particularly limited, and known CNFs can be used. CNFs refer to cellulose molecular chains formed into bundles of two or more. "CNFs formed into bundles of two or more" refers to a state in which two or more cellulose molecular chains are aggregated to form an aggregate called a microfibril. CNFs are generally obtained by processing plant-derived fibers. The raw materials for CNFs are not particularly limited, and examples include plant-derived fibers contained in wood, bamboo, hemp, jute, kenaf, cotton, beet pulp, potato pulp, agricultural waste, cloth, and paper. These raw materials may be used alone or in combination.

[0022] CNF may be chemically modified, and chemically modified CNF is preferred because it is easier to increase the transmittance of the transparent heat insulating material. In chemically modified CNF, some or all of the groups in the cellulose molecular chain are changed by chemical treatment. For example, the cellulose molecular chain in chemically modified CNF may be oxidized to aldehyde groups, carboxyl groups, etc., some or all of the hydroxyl groups at the C6 position in the molecule, including hydroxyl groups at positions other than the C6 position, esterified CNF such as nitrate ester, acetate ester, phosphate ester, or etherified CNF such as methyl ether, hydroxypropyl ether, carboxymethyl ether, or substituted with other functional groups. More specifically, examples of groups that can be introduced by chemical modification include a carboxyl group, an acetyl group, a sulfate group, a sulfonate group, an acryloyl group, a methacryloyl group, a propionyl group, a propioloyl group, a butyryl group, a 2-butyryl group, a pentanoyl group, a hexanoyl group, a heptanoyl group, an octanoyl group, a nonanoyl group, a decanoyl group, an undecanoyl group, a dodecanoyl group, a myristoyl group, a palmitoyl group, a stearoyl group, a pivaloyl group, a benzoyl group, a naphthoyl group, a nicotinoyl group, an isopropyl ... Examples of such groups include acyl groups such as sonicotinoyl, furoyl, and cinnamoyl groups, isocyanate groups such as 2-methacryloyloxyethylisocyanoyl groups, alkyl groups such as methyl, ethyl, propyl, 2-propyl, butyl, 2-butyl, tert-butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, myristyl, palmityl, and stearyl groups, oxirane, oxetane, thiirane, and thietane groups. Of these, the group introduced by chemical modification preferably contains at least a carboxy group.

[0023] Chemical modification of CNF can be carried out using conventional methods. That is, cellulose can be chemically modified by reacting it with a chemical modifying agent. If necessary, solvents, catalysts, heating, reduced pressure, etc. may be used. Chemical modifying agents include acids, acid anhydrides, alcohols, halogenating agents, and cyclic ethers such as alcohols, isocyanates, alkoxysilanes, and oxiranes (epoxies). These may be used alone or in combination. Examples of acids include acetic acid, acrylic acid, methacrylic acid, propanoic acid, butanoic acid, 2-butanoic acid, and pentanoic acid. After chemical modification, it is preferable to thoroughly wash the cellulose with water to terminate the reaction. After thorough washing with water, it is also preferable to further replace the cellulose with an organic solvent such as alcohol. In this case, the cellulose is replaced by immersing it in an organic solvent such as alcohol.

[0024] The average fiber diameter of the CNF is not particularly limited, but is preferably 1 to 100 nm, more preferably 2 to 50 nm, and even more preferably 2 to 10 nm. Using CNF with an average fiber diameter of 1 to 100 nm makes it easier to obtain a porous cellulose body with a large specific surface area. When the average fiber diameter is 1 nm or more, the single fiber strength of the nanofiber increases, making it easier to maintain the structure of the porous cellulose body. Here, the average fiber diameter is calculated as follows: An electron microscope image of the CNF is obtained using a transmission electron microscope (TEM) or a scanning electron microscope (SEM). Two random axes are drawn vertically and horizontally on the obtained image, and the fiber diameters of the fibers intersecting the axes are visually read. This is done at a magnification of 5,000x, 10,000x, or 50,000x, depending on the size of the constituent fibers. The sample or magnification must be such that 20 or more fibers intersect the axis. At least three images of non-overlapping surface areas are then taken with an electron microscope, and the fiber diameter values ​​of the fibers intersecting each of the two axes are read. Therefore, a minimum of 20 x 2 x 3 = 120 pieces of fiber information are obtained. The number-average fiber diameter is calculated from the fiber diameter data thus obtained, and is used as the average fiber diameter of the CNF. For branched fibers, if the length of the branched portion is 50 nm or more, it is counted as a single fiber in the fiber diameter calculation.

[0025] The average fiber length of the CNF is not particularly limited, but is preferably 0.01 to 20 μm, and more preferably 0.05 to 10 μm. The average fiber length is calculated by casting a thin layer of CNF dispersion on a substrate, freeze-drying the resulting sample, and observing it with an SEM. From the obtained observation image, 10 independent fibers are randomly selected per image, and their fiber lengths are visually read. This is done at a magnification of either 5,000x or 10,000x, depending on the length of the constituent fibers. The sample or magnification is selected so that the starting and ending points of the fibers are within the same image. In this way, at least 12 non-overlapping surface portions are observed with the SEM, and the fiber lengths are read. Therefore, information on a minimum of 10 fibers x 12 images = 120 fibers is obtained. The number-average fiber length is calculated from the fiber diameter data obtained in this way, and is used as the average fiber length of the CNF. For branched fibers, the length of the longest part of the fiber is used as the fiber length.

[0026] The method for adjusting the average fiber diameter of CNF is not particularly limited, but for example, in the mechanical crushing method, it can be adjusted by the processing time and number of times of the ultra-high pressure homogenizer or grinder used. In addition, in the chemical crushing method, it can be adjusted by the type of oxidizing agent (e.g., sodium hypochlorite), the concentration of the catalyst (e.g., TEMPO (2,2,6,6-tetramethyl-1-piperidinyloxy) catalyst), the reaction time, etc.

[0027] The method for preparing CNF is not particularly limited, and a mechanical or chemical disintegration method is preferred. Examples of the mechanical disintegration method include a method in which an aqueous suspension or slurry of a cellulose fiber-containing material is mechanically ground or beaten using a refiner, a high-pressure homogenizer, a grinder, a single- or multi-screw kneader, a bead mill, or the like to disintegrate the material. Examples of mechanical processing methods include Japanese Patent No. 5500842, Japanese Patent No. 5283050, Japanese Patent No. 5207246, Japanese Patent No. 5170193, Japanese Patent No. 5170153, Japanese Patent No. 5099618, Japanese Patent No. 4845129, Japanese Patent No. 4766484, Japanese Patent No. 4724814, Japanese Patent No. 4721186, Japanese Patent No. 4428521, International Publication No. 11 / 068023, Japanese Patent No. 5477265, and Japanese Patent Laid-Open No. 2014-84434. On the other hand, examples of chemical disintegration methods include oxidizing a cellulosic raw material using an oxidizing agent in the presence of an N-oxyl compound and a bromide and / or iodide, and then subjecting the oxidized cellulose to wet atomization for defibration into nanofibers. Examples of chemical treatment methods include those described in Japanese Patent Nos. 5,381,338, 4,981,735, 5,404,131, 5,329,279, 5,285,197, 5,179,616, 5,178,931, 5,330,882, and 5,397,910.

[0028] In the porous cellulose material, the CNF content is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, based on the total mass of the porous cellulose material.

[0029] [Water-Repellent Component] The water-repellent component contained in the transparent heat insulating material of the present invention is not particularly limited as long as it can impart water-repellent properties, and known water-repellent components can be used. Examples of water-repellent components include fluorine-based water repellents, silicone-based water repellents, wax-based water repellents, alkyl ketene dimers, and hydrolysis condensates of alkoxysilanes. Furthermore, surfactants are also preferred as the generating component. Here, surfactants refer to compounds having a hydrophobic group and a hydrophilic group in the molecule. In addition, in the transparent heat insulating material of the present invention, a portion of the water-repellent component may react to form a component derived from the water-repellent component. Examples of components derived from the water-repellent component include hydrolysis condensates of alkoxysilanes.

[0030] Among these, compounds having a fluorinated alkyl group are preferred as the water-repellent component. The fluorinated alkyl group may be a partially fluorinated alkyl group or a perfluoroalkyl group. The number of carbon atoms in the fluorinated alkyl group is preferably 1 to 20, more preferably 2 to 16, and even more preferably 4 to 12. The number of carbon atoms in the fluorinated alkyl group refers to the number of carbon atoms to which fluorine atoms are bonded, and carbon atoms to which no fluorine atoms are bonded are not included in the number of carbon atoms in the fluorinated alkyl group.

[0031] More specifically, preferred examples of the water-repellent component include an alkoxysilane having a fluorinated alkyl group, a hydrolysis condensate of an alkoxysilane having a fluorinated alkyl group, and a surfactant having a fluorinated alkyl group. The surfactant having a fluorinated alkyl group is preferably an anionic surfactant or a cationic surfactant. In terms of being able to better maintain transparency under high humidity conditions, it is also preferred that the water-repellent component contain a surfactant having a fluorinated alkyl group.

[0032] The alkoxysilane having a fluorinated alkyl group is preferably a compound represented by the following formula (I):

[0033]

[0034] In formula (I), R a represents an alkyl group having 1 to 4 carbon atoms. aWhen there are a plurality of R, they may be the same or different from each other. a preferably represents a methyl group or an ethyl group. a represents an alkyl group having 1 to 4 carbon atoms. a When there are a plurality of R, they may be the same or different from each other. b preferably represents a methyl group or an ethyl group. p represents an integer of 1 to 3. p is preferably 2 or 3, and more preferably 3. q represents an integer of 0 to 10. q is preferably 0 to 4, and more preferably 0 to 2. r represents an integer of 0 to 19. r is preferably 1 to 15, and more preferably 3 to 11. X represents a hydrogen atom or a fluorine atom. X preferably represents a fluorine atom.

[0035] In the porous cellulose body, the content of the water-repellent component is preferably 0.001 to 10% by mass, more preferably 0.01 to 5% by mass, relative to the total mass of the porous cellulose body. One type of water-repellent component may be used alone, or two or more types may be used simultaneously. When two or more types of water-repellent components are used simultaneously, it is preferable that the total content thereof is within the above-mentioned preferred range.

[0036] [Additives] The porous cellulose body may contain additives other than CNF and the water-repellent component. Examples of additives include freeze stabilizers and strength modifiers. Examples of freeze stabilizers include sucrose, trehalose, L-arginine, and L-histidine. Examples of strength modifiers include various latex emulsions such as acrylic latex, NBR latex, vinyl acetate latex, and olefin latex, as well as water-soluble polymers such as polyacrylamide, polyamide epichlorohydrin, polyvinyl alcohol, and starch. The content of the additive is preferably 5% by mass or less, more preferably 1% by mass or less, based on the total mass of the porous cellulose body. The porous cellulose body does not necessarily contain additives.

[0037] [Method for producing porous cellulose body] The method for producing a porous cellulose body is not particularly limited as long as it can produce a porous cellulose body that can be used as a transparent thermal insulation material, but it is preferable to adopt the first method for producing a porous cellulose body or the second method for producing a porous cellulose body described below, as these methods make it easier to obtain a transparent thermal insulation material with excellent transmittance. Furthermore, by adopting the first method for producing a porous cellulose body or the second method for producing a porous cellulose body described below, it is possible to obtain a porous cellulose body with a large area, and a transparent thermal insulation material with a maximum length of 1,000 mm or more can be obtained.

[0038] (Method for producing a first porous cellulose body) The method for producing a first porous cellulose body includes, in this order, a step of preparing a CNF dispersion liquid in which CNFs are dispersed, a step of gelling the CNF dispersion liquid to obtain a CNF wet gel, a step of substituting the solvent component in the CNF wet gel, a step of freeze-drying the CNF wet gel to obtain a CNF aerogel, and a step of subjecting the CNF aerogel to a water-repellent treatment. Each step is described below.

[0039] First, a CNF dispersion in which CNFs are dispersed is prepared. The CNF dispersion in which CNFs are dispersed can be obtained, for example, by the method described in the CNF preparation method above. The dispersion medium in the CNF dispersion preferably contains water, and the dispersion medium preferably contains 70 mass% or more of water, more preferably 90 mass% or more, and even more preferably 99 mass% or more of water, relative to the total mass of the dispersion medium. The dispersion medium in the CNF dispersion may be water. The CNF content in the CNF dispersion is preferably 0.001 to 5 mass%, more preferably 0.01 to 2 mass%, and even more preferably 0.1 to 1 mass%. The CNF dispersion may contain the additives described above.

[0040] Next, the CNF dispersion is gelled to obtain a CNF wet gel. The method for gelling the CNF dispersion is not particularly limited, but examples include adding an acidic or alkaline component, with the addition of an acidic component being preferred. The addition of the above component weakens the electrostatic repulsion that contributes to the dispersion of CNFs in the CNF dispersion, forming a CNF network and thus obtaining a CNF wet gel. The acidic component to be added is not particularly limited, but examples include inorganic acids (e.g., hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid), organic acids (e.g., methanesulfonic acid, tosylic acid), and metal halides (e.g., aluminum chloride). The acidic component is preferably added to the CNF dispersion in the form of a solution. The amount of the acidic component added can be adjusted as appropriate, but it is preferable to add it so that the total volume of the CNF dispersion after the addition of the acidic component is 0.01 to 5 mol / L. It is also preferable to add the acidic component without forcible stirring and then allow it to stand.

[0041] Next, the solvent components in the CNF wet gel are replaced. The solvent components in the CNF wet gel are preferably replaced with a solvent that precipitates fine crystals during the subsequent freezing step. Examples of solvents that precipitate fine crystals include mixed solvents, with a mixed solvent of water and alcohol being particularly preferred. The mixed solvent is preferably prepared in a ratio that allows the components contained in the mixed solvent to precipitate as a eutectic when the temperature is lowered. Examples of alcohols include alcohols that are miscible with water at any ratio, with t-butyl alcohol being preferred. Mixed solvents of water and t-butyl alcohol preferably contain 3 to 20% by mass of water, more preferably 5 to 15% by mass, based on the total mass of the mixed solvent. In the mixed solvent, the component other than water is preferably t-butyl alcohol. The solvent components in the CNF wet gel can be replaced by known methods, for example, by immersing the CNF wet gel in the mixed solvent. Shaking may be performed to promote the replacement.

[0042] Next, the CNF wet gel with the solvent components replaced is freeze-dried to obtain a CNF aerogel. Freezing can be performed by known methods, but rapid cooling is preferred to reduce the size of crystals precipitated from the solvent contained in the CNF wet gel and obtain a transparent insulation material with higher transmittance. A rapid cooling method includes, for example, contacting the CNF wet gel with a member cooled with liquid nitrogen. After freezing the CNF wet gel, the solvent components in the frozen CNF wet gel are sublimated. The solvent components can be sublimated by placing the frozen CNF wet gel in an environment below the freezing point of the solvent components. During the sublimation of the solvent components, the sublimation rate can be increased by reducing the pressure.

[0043] Next, the freeze-dried CNF aerogel is subjected to a water-repellent treatment. Examples of water-repellent treatment include a method of supplying the above-mentioned water-repellent component to the CNF aerogel. When supplying the water-repellent component to the CNF aerogel, it is preferable to supply it in the gas phase. For example, a method of storing the above-mentioned water-repellent component and the CNF aerogel in a chamber and heating the water-repellent component may be used. Alternatively, a gas containing the above-mentioned water-repellent component may be supplied to the chamber storing the CNF aerogel.

[0044] Through the above steps, the transparent heat insulating material (porous cellulose material) of the present invention is obtained.

[0045] (Second Method for Producing a Porous Cellulose Body) The second method for producing a porous cellulose body comprises, in this order: preparing a CNF dispersion containing dispersed CNFs and a water-repellent component; gelling the CNF dispersion to obtain a CNF wet gel; substituting the solvent component in the CNF wet gel; and freeze-drying the CNF wet gel to obtain a CNF aerogel. The second method for producing a porous cellulose body differs from the first method for producing a porous cellulose body in that a CNF dispersion containing dispersed CNFs and a water-repellent component is used. The water-repellent component is preferably a surfactant as described above. The content of the water-repellent component in the CNF dispersion may be adjusted as needed so that the content of the water-repellent component in the porous cellulose body falls within the preferred range described above. Other than the above, the second method for producing a porous cellulose body can be carried out in the same manner as the first method for producing a porous cellulose body, and therefore, further explanation is omitted. The second method for producing a porous cellulose body produces a porous cellulose body containing a more uniform water-repellent component, allowing the resulting porous cellulose body to better maintain transparency under high humidity conditions.

[0046] In another embodiment of the method for producing a porous cellulose body, the freeze-drying performed in the first method for producing a porous cellulose body and the second method for producing a porous cellulose body may be replaced with a process in which the solvent component in the CNF wet gel is replaced with a supercritical fluid and then dried.

[0047] <Uses> The transparent heat insulating material of the present invention has high transparency and can be applied to a variety of uses. For example, it can be suitably applied to uses where it is necessary to transmit light while exhibiting a heat insulating effect. Specifically, the transparent heat insulating material of the present invention can be suitably applied to windows or components thereof. Specific examples of applying the transparent heat insulating material of the present invention to windows will be described below, but the transparent heat insulating material of the present invention is not limited to the specific examples below.

[0048] [Laminated Glass] The transparent insulating material of the present invention can be used as an interlayer film for laminated glass. The configuration of the laminated glass is not particularly limited, and known configurations can be used. For example, the number of glass plates used in the laminated glass may be two or more, or may be three or more, or may be four or more. When the transparent insulating material of the present invention is used as an interlayer film for laminated glass, it is disposed between two or more glass plates used in the laminated glass. When the number of glass plates is three or more, the transparent insulating material of the present invention may be disposed between each glass plate, or the transparent insulating material of the present invention may be disposed only between one pair of glass plates.

[0049] When the transparent insulating material of the present invention is used as an interlayer film in laminated glass, a configuration other than the transparent insulating material of the present invention (another layer) may be present between a pair of glass sheets. That is, the transparent insulating material of the present invention provided between the glass sheets may be in direct contact with the glass sheets or may be in contact with the glass sheets via another layer. Preferred examples of the other layer include one or more resin layers selected from the group consisting of polyvinyl butyral, polycarbonate, ethylene-vinyl acetate copolymer, polyethylene terephthalate, etc. Preferred examples of the other layer include an adhesive layer or a pressure-sensitive adhesive layer. In addition, the other layers described below in connection with double-glazing may be applied to the laminated glass.

[0050] The glass plates used in the laminated glass can be any known glass depending on the purpose, and examples thereof include transparent glass plates, patterned glass plates, wired glass plates, lined glass plates, tempered glass plates, heat-reflecting glass plates, heat-absorbing glass plates, Low-E glass plates, and various other glass plates. Furthermore, one or more of the glass plates used in the laminated glass may be made of a glass-substitute resin such as polycarbonate. The thickness of the glass plates can be appropriately selected depending on the purpose. The shape of the glass plates is not particularly limited and can be appropriately adjusted depending on the application. Furthermore, the glass plates may have curved surfaces.

[0051] The laminated glass may have a known sealing structure, for example, a structure in which the outer edge of the laminated glass is sealed with a sealing material such as a resin.

[0052] [Double Glazing] The transparent insulating material of the present invention can be applied to double glazing. Double glazing refers to glass containing a gas layer between two or more glass panes. The gas layer is a layer made of gas, and the gas contained in the gas layer may be air or an inert gas such as nitrogen gas or argon gas. The gas layer may be at a pressure lower than atmospheric pressure. The number of glass panes contained in the double glazing may be two or more, three or more, or four or more. When the transparent insulating material of the present invention is applied to double glazing, the transparent insulating material of the present invention is disposed between a pair of glass panes. However, when the number of glass panes is three or more, the transparent insulating material of the present invention may be disposed between each glass pane, or the transparent insulating material of the present invention may be disposed only between a pair of glass panes.

[0053] When the transparent heat insulating material of the present invention is applied to double-glazed glass, it may have one or more components (other layers) other than the transparent heat insulating material of the present invention. Examples of other layers include the other layers described above, as well as a light-shielding layer and a heat-shielding layer. The light-shielding layer may be a layer with low transmittance for at least a portion of visible light, or may be a layer with low transmittance for at least a portion of ultraviolet light. Examples of light-shielding layers include metal vapor deposition films and colored layers such as a dye layer containing a dye. Examples of heat-shielding layers include layers that reflect or absorb infrared rays, such as metal vapor deposition films, polymer layers containing metal particles or metal oxide particles, and dielectric multilayer films. Examples of other layers include flame-retardant layers. Examples of the flame-retardant layer include layers containing a flame retardant, and known flame retardants can be used as the flame retardant. Examples of flame retardants include aromatic phosphate esters, phosphorus compounds such as red phosphorus, halogen compounds such as chlorinated paraffins containing at least one of chlorine and bromine, antimony compounds such as antimony trioxide, metal hydroxides such as aluminum hydroxide and magnesium hydroxide, and nitrogen compounds such as melamine cyanurate.

[0054] The glass sheet may be a glass sheet used in the above-mentioned laminated glass. The glass sheet included in the double glazing may be a laminated glass. The laminated glass may include the above-mentioned transparent heat insulating material of the present invention.

[0055] The double-glazed glass may have a known sealing structure. For example, the sealing structure may include a spacer disposed on the outer edge of a pair of glass sheets and a sealing material disposed between the spacer and the opposing glass sheet. The sealing structure allows the space formed by the pair of glass sheets and the spacer to become the gas layer. The spacer may contain a desiccant for the purpose of absorbing moisture from the gas layer. The glass sheets may be sealed with another sealing material further toward the outer edge than the spacer. Examples of other sealing materials include curable resins such as polysulfide resins and silicone resins. The sealing structure may also be formed by a frame that holds the double-glazed glass.

[0056] When applying the transparent insulating material of the present invention to the above-mentioned laminated glass and double glazing, an integrally molded transparent insulating material may be applied, or multiple transparent insulating materials may be applied by arranging them in the planar direction of the glass sheets. Furthermore, multiple transparent insulating materials may be applied by stacking them in the lamination direction of the glass sheets. When applying the transparent insulating material of the present invention to the above-mentioned laminated glass and double glazing, the above-mentioned flame retardant may be added to the transparent insulating material.

[0057] The above-described laminated glass and double-glazed glass can be suitably used, for example, as windows for houses and windows for vehicles such as passenger cars. Furthermore, the above-described laminated glass and double-glazed glass can transmit radio waves because the transparent heat insulating material of the present invention is not electrically conductive. When radio wave transmission is desired, it is preferable to select a layer that is not electrically conductive as the other layer.

[0058] The present invention will be described in more detail below with reference to examples. The materials, amounts used, ratios, treatment details, treatment procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be construed as being limited by the examples shown below.

[0059] Example 1 Preparation of Cellulose Nanofiber Aqueous Dispersion 2.00 g (dry mass equivalent) of NBKP (kraft pulp obtained by bleaching softwood raw materials, mainly consisting of fibers with a fiber diameter exceeding 1000 nm), 0.025 g of TEMPO (2,2,6,6-tetramethylpiperidine-1-oxy radical), and 0.25 g of sodium bromide were dispersed in 150 ml of water, and then a 13% aqueous solution of sodium hypochlorite was added to 1.00 g of NBKP so that the amount of sodium hypochlorite was 5.00 mmol. The reaction was initiated by adding sodium hypochlorite. During the reaction, a 0.50 mol / L aqueous solution of sodium hydroxide was added dropwise to maintain the pH at 10. After the reaction for 2 hours, the reaction product was filtered and thoroughly washed with water to obtain an oxidized cellulose slurry. A 0.15% by mass oxidized cellulose slurry was defibrated for 5 minutes at 15,000 rpm using a biomixer (BM-2, manufactured by Nippon Seiki Seisakusho Co., Ltd.), and then further defibrated for 20 minutes using an ultrasonic disperser (model US-300E, manufactured by Nippon Seiki Seisakusho Co., Ltd.). Subsequently, coarse fibers were removed by centrifugation to obtain a transparent aqueous dispersion of cellulose nanofibers. The obtained aqueous dispersion of cellulose nanofibers was concentrated using a rotary evaporator to a solids concentration of 0.40% and used in subsequent steps. Hereinafter, the aqueous dispersion of cellulose nanofibers with a solids concentration of 0.40% will also be referred to as "aqueous dispersion of cellulose nanofibers A."

[0060] [Gelling step] 500 g of cellulose nanofiber aqueous dispersion A was poured into a 100 cm square Petri dish, and 100 g of 1.0 M hydrochloric acid was gently poured down the side of the dish, followed by standing for 1 hour. The dispersion physically gelled, and the thickness was 5 mm.

[0061] [Solvent substitution step] Solvent substitution was carried out using a mixed solvent in which the mixing ratio of t-butyl alcohol and water was 90:10 by mass. The solvent substitution was carried out by immersing the physical gel in a sufficient amount of the substitution solvent and shaking it slowly. Each substitution step was carried out over 4 hours, and substitution was carried out four or more times.

[0062] The physical gel obtained in the solvent substitution step was frozen by sandwiching it between iron plates sufficiently cooled with liquid nitrogen (-196°C). The frozen gel was then dried in a vacuum dryer (manufactured by Tokyo Rikakikai Co., Ltd.) to sublimate the solvent component and obtain an aerogel.

[0063] [Vapor Phase Deposition Process] The aerogel obtained in the freeze-drying process was placed in a sealed chamber, and 100 mg of trimethoxyheptadecafluorodecylsilane was added as a water-repellent component. The chamber was kept at 60°C for 1 hour, and triethoxyheptadecafluorodecylsilane was supplied to the aerogel to obtain a porous cellulose body.

[0064] Example 2 A porous cellulose material was obtained in the same manner as in Example 1, except that trimethoxytrifluoropropylsilane was used as the water-repellent component in the vapor phase deposition step.

[0065] Example 3 A porous cellulose material was obtained in the same manner as in Example 1, except that a 0.1 M aqueous aluminum chloride solution was used instead of hydrochloric acid in the gelation step.

[0066] Example 4 A porous cellulose material was obtained in the same manner as in Example 1, except that trimethoxytrifluoropropylsilane was added as a water-repellent component.

[0067] Example 5 A porous cellulose body was obtained in the same manner as in Example 1, except that potassium nonafluorobutanesulfonate was added to the cellulose nanofiber dispersion A and the vapor phase deposition step was omitted. The potassium nonafluorobutanesulfonate was added so as to be 0.08 mass % relative to the total mass of the potassium nonafluorobutanesulfonate and the cellulose nanofiber aqueous dispersion A.

[0068] Example 6 A porous cellulose body was obtained in the same manner as in Example 1, except that potassium bis(nonafluorobutanesulfonyl)imide was added to cellulose nanofiber dispersion A and the vapor phase deposition step was omitted. Potassium bis(nonafluorobutanesulfonyl)imide was added so as to be 0.08 mass % relative to the total mass of potassium bis(nonafluorobutanesulfonyl)imide and the cellulose nanofiber aqueous dispersion A.

[0069] Example 7 A porous cellulose body was obtained in the same manner as in Example 1, except that ethanol was used instead of the mixed solvent in the solvent substitution step, and an aerogel was obtained by drying in the supercritical drying step described below.

[0070] [Supercritical Drying Process] The solvent-substituted physical gel was placed in a sealed reactor, and then liquefied carbon dioxide was introduced into the sealed reactor. The sealed reactor was then heated and the pressure inside the sealed reactor was increased using a high-pressure pump, bringing the carbon dioxide inside the sealed reactor to a supercritical state. The liquefied carbon dioxide was then introduced into the sealed reactor, and the supercritical carbon dioxide was then discharged from the sealed reactor, thereby allowing the supercritical carbon dioxide to flow through the physical gel inside the sealed reactor. When the supercritical carbon dioxide flows through the solvent-substituted physical gel, the solvent dissolves in the supercritical carbon dioxide, and the solvent is removed along with the supercritical carbon dioxide flowing out of the sealed reactor. The temperature and pressure inside the sealed reactor were set to those that would bring the carbon dioxide to a supercritical state. The critical point of carbon dioxide is 31.1°C / 7.38 MPa, and the temperature and pressure were, for example, 50 to 200°C / 10 to 30 MPa.

[0071] Comparative Example 1 A porous cellulose material was obtained in the same manner as in Example 1, except that the vapor phase deposition step was omitted.

[0072] Comparative Example 2 To cellulose nanofiber aqueous dispersion A, t-butyl alcohol was added so that the mixing ratio of t-butyl alcohol to water was 20:80 by mass, and a predetermined amount of potassium nonafluorobutanesulfonate was added to obtain cellulose nanofiber aqueous dispersion B. The potassium nonafluorobutanesulfonate was added so that the amount was 0.08% by mass relative to the total mass of cellulose nanofiber aqueous dispersion B. A porous cellulose body was obtained in the same manner as in Example 1, except that the cellulose nanofiber aqueous dispersion B was used and the gelation step and the vapor phase deposition step were omitted.

[0073] Comparative Example 3 A porous cellulose material was obtained in the same manner as in Example 7, except that the vapor phase deposition step was omitted.

[0074] <Measurement and Evaluation> [Measurement of Fiber Diameter] The fiber diameters of the porous cellulose bodies of the Examples and Comparative Examples were measured by the method described above.

[0075] [Transmittance evaluation] The transmittance of the porous cellulose bodies of the Examples and Comparative Examples was measured using an ultraviolet-visible-near-infrared spectrophotometer V-660 equipped with an automatic absolute reflectance measurement unit ARMN-735 manufactured by JASCO Corporation. During the measurement, the sample was placed close to an integrating sphere to measure the total light transmittance, and the transmittance was evaluated as the transmittance at 550 nm. The thickness of the porous cellulose bodies of the Examples and Comparative Examples was 5 mm.

[0076] [Evaluation of Moisture Resistance] The porous cellulose bodies of the Examples and Comparative Examples were left standing in a thermostatic chamber at a temperature of 20°C and a relative humidity of 50% for 14 days. After standing, the transmittance was evaluated in the same manner as above. The table below shows the value obtained by subtracting the transmittance before standing from the transmittance after standing. In other words, if the transmittance after standing is reduced compared to before standing, the value is negative, and a smaller negative value indicates that transparency can be maintained under high humidity conditions.

[0077] [Contact Angle Evaluation] The water contact angles of the porous cellulose bodies of the Examples and Comparative Examples were measured using a water contact angle meter FAMAS (manufactured by Kyowa Interface Science Co., Ltd.) to measure the contact angle when water was dropped.

[0078] <Results> The production procedures, fiber diameter, transmittance, and moisture resistance evaluation of the porous cellulose bodies (transparent heat insulating materials) of the Examples and Comparative Examples are shown in Table 1. In Table 1, the size column indicates the size of the porous cellulose bodies (transparent heat insulating materials) that were successfully produced.

[0079]

[0080] The results shown in Table 1 indicate that the porous cellulose bodies of Comparative Examples 1 and 3, which did not contain a water-repellent component, were unable to maintain transparency under high humidity conditions compared to the other Examples. Furthermore, the results of Comparative Example 2 indicated that when the fiber diameter was 40 nm or greater, the transmittance was low, and the porous cellulose bodies could not be used as transparent heat insulating materials. Comparison of Example 4 with Examples 1 to 3, 5, and 6 confirmed that when a compound having a fluorinated alkyl group was included as the water-repellent component and the fluorinated alkyl group had 4 to 12 carbon atoms, transparency could be better maintained under high humidity conditions. Comparison of Examples 5 and 6 with other Examples confirmed that when a surfactant having a fluorinated alkyl group was included as the water-repellent component, transparency could be better maintained under high humidity conditions. Comparison of Example 7 with other Examples confirmed that when the fiber diameter was 20 to 40 nm, transparency could be better maintained under high humidity conditions. Comparison of Example 7 with other Examples confirmed that by employing the first or second porous cellulose body manufacturing method described above, a porous cellulose body with a large area could be obtained, and a transparent heat insulating material with a maximum length of 1,000 mm or more could be obtained. A comparison of Example 4 with Examples 1 to 3 confirmed that the contact angle was larger when the water-repellent component was a compound having a fluorinated alkyl group and the number of carbon atoms in the fluorinated alkyl group in the compound having a fluorinated alkyl group was 4 to 12.

Claims

1. A transparent insulation material made of a porous cellulose body, the porous cellulose body containing cellulose nanofibers and a water-repellent component, and the fiber diameter of the porous cellulose body being 3 to 40 nm.

2. The transparent insulation material according to claim 1, having a maximum length of 1000 mm or more.

3. The transparent heat insulating material according to claim 1 or 2, which has a contact angle with water of 90 degrees or more.

4. The transparent heat insulating material according to claim 1 or 2, wherein the water-repellent component is a compound having a fluorinated alkyl group.

5. The transparent heat insulating material according to claim 4, wherein the fluoroalkyl group in the compound having the fluoroalkyl group has 4 to 12 carbon atoms.

6. The transparent heat insulating material according to claim 4, wherein the compound having a fluorinated alkyl group is an alkoxysilane having a fluorinated alkyl group or a condensate of the alkoxysilane.

7. The transparent heat insulating material according to claim 6, wherein the alkoxysilane is a compound represented by the following formula (I): In formula (I), R a represents an alkyl group having 1 to 4 carbon atoms. a When there are a plurality of R, they may be the same or different. b represents an alkyl group having 1 to 4 carbon atoms. b When there are a plurality of, they may be the same or different. p represents an integer of 1 to 3. q represents an integer of 0 to 10. r represents an integer of 0 to 19. X represents a hydrogen atom or a fluorine atom.

Citation Information

Patent Citations

  • Cellulose porous body and manufacturing method therefor

    JP2015105366A

  • Cellulose porous body and manufacturing method therefor

    JP2015105453A

  • Method for producing cellulose porous body

    JP2023115733A