Low thermal expansion steel casting product and method for manufacturing same

The described method for low thermal expansion cast steel products, involving a specific chemical composition and thermal treatment, addresses the issue of poor plating properties and etch pit formation by achieving a low thermal expansion coefficient and enhanced plating performance.

WO2024219358A1PCT designated stage expired Publication Date: 2024-10-24SHINHOKOKU STEEL CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014980
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-19
Filing Date
2024-04-15
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Low thermal expansion cast steel products often suffer from poor plating properties and etch pit formation during pretreatment, leading to deteriorated plating performance and potential pinholes due to impurities like sulfur and oxygen.

Method used

A cast steel product with a specific chemical composition (C: 0.040% or less, Si: 0.30% or less, Mn: 0.50% or less, S: 0.010% or less, Ni: 31.00 to 34.00%, Co: 4.90 to 6.00%, O: 0.0100% or less, Al: 0.010 to 0.100%, and the remainder being Fe and unavoidable impurities) is treated with cryo treatment below the Ms point, followed by heating and rapid cooling, and subsequent recrystallization to achieve an austenitic structure with a thermal expansion coefficient of 0.4×10^-6 /°C or less, thereby suppressing etch pit formation and enhancing plating properties.

Benefits of technology

The method results in a low thermal expansion cast steel product with improved plating properties and reduced etch pit occurrence, maintaining a low thermal expansion coefficient while ensuring effective plating performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014980_24102024_PF_FP_ABST
    Figure JP2024014980_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing a low thermal expansion steel casting product having excellent plating properties. A low thermal expansion steel casting product according to the present invention has a chemical composition containing, in mass%, 0.040% or less of C, 0.30% or less of Si, 0.50% or less of Mn, 0.010% or less of S, 31.00-34.00% of Ni, 4.90-6.00% of Co, 0.0100% or less of O, and 0.010-0.100% of Al, the remaining portion being Fe and unavoidable impurities, has an austenite structure having an average grain size of 200 µm or less, and has an average thermal expansion coefficient of 0.4×10-6 / °C or less at 25-100°C.
Need to check novelty before this filing date? Find Prior Art

Description

Low thermal expansion cast steel products and their manufacturing method

[0001] The present invention relates to a low thermal expansion cast steel product having a low thermal expansion coefficient and a method for producing the same.

[0002] Thermally stable invar alloys are widely used as materials for components in electronics and semiconductor-related equipment, laser processing machines, and ultra-precision processing equipment.

[0003] Patent Document 1 describes a steel sheet containing 29.5 to 35% Ni, 2.0 to 7.0% Co, and 0.001 to 2.0% Cr, with a thermal expansion coefficient of 0.5 × 10 -6 / ℃ ~ 2.0 × 10 -6 This alloy is obtained by homogeneous solution treatment, followed by quenching or annealing by cooling at a rate of 1°C / sec or less, and then cold rolling by 10% or more.

[0004] Patent Document 2 discloses a low thermal expansion wire containing 65% or less Co, 30% or less Ni, and 10% or less Cr, with the total content of Co and Ni being 25 to 65%. Patent Document 2 also discloses a method of transforming the low thermal expansion wire into a strain-induced martensite phase by cold working a part of the austenite phase.

[0005] Patent Document 3 discloses a low thermal expansion alloy containing 0.03 to 1.5% Ni, 53 to 55% Ni and Co combined, and 9 to 10% Cr. Patent Document 3 discloses a method of annealing the alloy at 650 to 900°C and then cooling it in a furnace at a rate of less than 20°C / min.

[0006] Patent No. 2796966 Japanese Patent Publication No. 6-279945 Patent No. 5534150

[0007] When plating low-thermal expansion cast steel products, they are pre-treated. This involves etching, which can sometimes cause etch pits on the surface of the cast steel. If etch pits occur, plating performance will be reduced and pinholes may appear when plating is applied.

[0008] An object of the present invention is to solve the above problems and to provide a low-thermal expansion cast steel product with good platability in which the occurrence of etch pits during pretreatment for plating is suppressed.

[0009] The present inventors have conducted extensive research into methods for suppressing etch pits in low thermal expansion cast steel products, and have developed the present invention. The present invention includes the following aspects.

[0010] (1) The chemical composition contains, in mass%, C: 0.040% or less, Si: 0.30% or less, Mn: 0.50% or less, S: 0.010% or less, Ni: 31.00 to 34.00%, Co: 4.90 to 6.00%, O: 0.0100% or less, and Al: 0.010 to 0.100%, with the balance being Fe and unavoidable impurities, the average grain size of the austenitic structure is 200 μm or less, and the average thermal expansion coefficient at 25 to 100 ° C is 0.4 × 10 -6 / °C or less.

[0011] (2) A method for producing the low thermal expansion cast steel product of (1), which comprises the following steps in order: a cryo-treatment step in which a cast steel product having a chemical composition, in mass%, of C: 0.040% or less, Si: 0.30% or less, Mn: 0.50% or less, S: 0.010% or less, Ni: 31.00 to 34.00%, Co: 4.90 to 6.00%, O: 0.0100% or less, and Al: 0.010 to 0.100%, with the balance being Fe and unavoidable impurities, is cooled to the Ms point or below, held at a temperature below the Ms point for 0.5 to 3 hours, and then heated to room temperature; and a recrystallization step in which the cryo-treated cast steel product is heated to 800 to 1100 ° C, held for 0.5 to 5 hours, and then rapidly cooled.

[0012] According to the present invention, it is possible to obtain a low thermal expansion cast steel product that has good plating properties.

[0013] 1 shows an example of the structure of a cast steel product after cryo-treatment. 2 shows an example of the structure of a cast steel product after recrystallization treatment.

[0014] The present invention will be described in detail below.

[0015] <Chemical Composition> First, the chemical composition of the cast steel product of the present invention will be described. Hereinafter, "%" regarding the chemical composition represents "mass %" unless otherwise specified.

[0016] (C: 0.040% or less) C dissolves in austenite and contributes to increasing strength. However, C dissolves in the matrix during the recrystallization process and precipitates during cooling, increasing the thermal expansion coefficient. The average thermal expansion coefficient at 25 to 100°C is 0.4 x 10 -6 / °C or less, it is necessary to reduce the amount of C precipitated. Therefore, the C content is set to 0.040% or less. The C content may be 0.035% or less, 0.030% or less, 0.025% or less, or 0.020% or less. The C content may be 0.001% or more, 0.002% or more, 0.003% or more, 0.004% or more, or 0.005% or more.

[0017] (Si: 0.30% or less, Mn: 0.50% or less) Si and Mn are added as deoxidizers. In the present invention, in order to produce a sound cast steel product without blowing, it is sufficient to add each of them in the minimum amount necessary for deoxidation. The final cast steel product does not need to contain Si or Mn, and the Si content and Mn content may be 0%, but they may be contained within the ranges of Si: 0.30% or less and Mn: 0.50% or less, respectively. Since deoxidation can also be performed with Al, Si and Mn do not need to be added. The Si content may be 0.25% or less, 0.20% or less, 0.15% or less, or 0.10% or less. The Si content may be 0.01% or more, 0.02% or more, 0.03% or more, 0.04% or more, or 0.05% or more. The Mn content may be 0.40% or less, 0.30% or less, or 0.20% or less. The Mn content may be 0.01% or more, 0.05% or more, 0.08% or more, 0.10% or more, 0.12% or more, or 0.15% or more.

[0018] (S: 0.010% or less) S is contained as an impurity. S generates sulfides, and the generated sulfides cause etch pits during pretreatment for plating. To suppress the generation of sulfides, the S content is set to 0.010% or less. The S content may be 0.009% or less, 0.008% or less, 0.007% or less, 0.006% or less, or 0.005% or less. The lower the S content, the better, and the S content may be 0%. However, since setting the S content to 0% increases costs, the S content may be 0.001% or more, or 0.002% or more.

[0019] (Ni: 31.00 to 34.00%) Ni is an element that lowers the thermal expansion coefficient. If the Ni content is too high or too low, the thermal expansion coefficient will not be sufficiently low. Also, if the Ni content is too high, it becomes difficult to cause martensitic transformation by cooling. The average thermal expansion coefficient at 25 to 100°C is 0.4 × 10 -6 / °C or less, it is necessary to control the Ni content within a narrow range. Specifically, the Ni content is set to a range of 31.00 to 34.00%. The Ni content may be 31.20% or more, 31.30% or more, or 31.50% or more. The Ni content may be 33.50% or less, 33.00% or less, or 32.50% or less.

[0020] (Co: 4.90 to 6.00%) Co contributes to lowering the thermal expansion coefficient in combination with Ni. The average thermal expansion coefficient at 25 to 100°C is 0.4 × 10 -6 / °C or less, the Co content needs to be controlled within a narrow range. Specifically, the Co content is 4.90 to 6.00%. The Co content may be 5.80% or less, 5.70% or less, 5.60% or less, 5.50% or less, or 5.40% or less. The Co content may be 4.95% or more, 5.00% or more, 5.05% or more, 5.10% or more, or 5.15% or more.

[0021] (O: 0.0100% or less) O ​​is contained as an impurity. O generates oxides, and the generated oxides cause etch pits during pretreatment for plating. In order to suppress the generation of oxides, the O content is set to 0.0100% or less. The O content may be 0.0090% or less, 0.0080% or less, 0.0070% or less, 0.0060% or less, or 0.0050% or less. The lower the O content, the better, and the O content may be 0%. However, since setting the O content to 0% increases costs, the O content may be 0.0001% or more, 0.0005% or more, 0.0010% or more, 0.0015% or more, or 0.0020% or more.

[0022] (Al: 0.010 to 0.100%) Al is added as a deoxidizer. In the low thermal expansion casting of the present invention, sufficient Al is contained to make the O content 0.0100% or less. Therefore, the Al content in the finally manufactured cast steel product is set to 0.010 to 0.100%. The Al content may be 0.015% or more, 0.020% or more, 0.025% or more, 0.030% or more, 0.035% or more, or 0.040% or more. The Al content may be 0.090% or less, 0.085% or less, 0.080% or less, 0.075% or less, or 0.070% or less.

[0023] The remainder of the chemical composition is Fe and inevitable impurities. The inevitable impurities are those elements that are not intentionally added to steel but are inevitably mixed in due to raw materials, the manufacturing environment, etc., when industrially manufacturing a steel having the chemical composition specified in the present invention. Examples of inevitable impurities include P and Cu, which are elements that are not intentionally added in the manufacturing process. The content of the impurities is not limited as long as it is within a range that does not affect the effects of the present invention. The total content of the impurities, in mass %, may be 0.50% or less, 0.40% or less, 0.30% or less, 0.20% or less, 0.15% or less, 0.10% or less, 0.05% or less, or 0%.

[0024] <Structure of Cast Steel Product> The structure of the cast steel product of the present invention is an austenite structure with an average grain size of 200 μm or less. The structure is mainly composed of fine equiaxed crystals. Although it is not necessary for all of the structure to be equiaxed crystals, it is preferable that the proportion of equiaxed crystals is 60% or more in terms of area ratio. It is more preferable that the proportion of equiaxed crystals is 90% or more in terms of area ratio, and even more preferable that it is 95% or more.

[0025] The average grain size of austenite was determined as the average value of the circle-equivalent diameters of crystal grains obtained by cutting out a sample for microstructure observation from near the center of the cast steel product, mirror-polishing the observation surface, and then etching with Marble reagent and observing it with an optical microscope.

[0026] <Coefficient of thermal expansion> The cast steel product of the present invention has an average coefficient of thermal expansion of 0.4 × 10 at 25 to 100°C. -6 / °C or less. The thermal expansion coefficient is measured by taking a thermal expansion measurement specimen from near the center of the cast steel product and heating it from 0°C to 130°C at a temperature increase rate of 3°C / min using a thermal expansion measuring instrument, and measuring the average thermal expansion coefficient from 25 to 100°C. A DIL 402C manufactured by NETZSCH can be used as the thermal expansion measuring instrument. The average thermal expansion coefficient from 25 to 100°C is 0.40 x 10 -6 / °C or less, 0.35 x 10 -6 / ℃ or less, 0.30 × 10 -6 / °C or less, or 0.25 x 10 -6 / °C or less.

[0027] <<Manufacturing Method>> Next, a method for manufacturing the low thermal expansion cast steel product of the present invention will be described.

[0028] (Casting) First, molten steel is produced so that the cast steel product has the aforementioned chemical composition. The method for producing the molten steel is not particularly limited, and known devices and methods may be used. Next, the molten steel is poured into a mold and solidified to obtain the cast steel product. The mold, the device for pouring the molten steel into the mold, and the method for pouring are not particularly limited, and known devices and methods may be used. The structure of the cast steel product produced in the mold will be a structure centered on columnar crystals. The obtained cast steel product is subjected to the following heat treatment.

[0029] (Cryo-treatment step) Next, the cast steel product is rapidly cooled to below the Ms point, held at a temperature below the Ms point for 0.5 to 3 hours, and then heated to room temperature (cryo-treatment step). The cooling method is not particularly limited. Generally, the Ms point can be estimated using the composition of the steel using the following formula:

[0030] Ms (°C) = 521 - 353C - 22Si - 24.3Mn - 7.7Cu - 17.3Ni - 17.7Cr - 25.8Mo where C, Si, Mn, Cu, Ni, Cr, and Mo are the contents (mass%) of each element. Elements that are not contained are set to 0.

[0031] In the case of the chemical composition of the low-thermal-expansion cast steel product of the present invention, the Ms point calculated by the above formula will be approximately -10°C to -70°C, depending particularly on the Ni content. Therefore, methods such as immersion in dry ice and methyl alcohol or ethyl alcohol, liquid nitrogen, or spraying with liquid nitrogen can be used as cooling media. This results in the formation of a structure containing fine martensite. Furthermore, the temperature can be raised by lifting the material into room-temperature air. Figure 1 shows an example of the structure after the cryo-treatment process. The black areas in the structure photograph are martensite. The formation of a large amount of martensite refines the austenite grain size in the subsequent recrystallization process.

[0032] (Recrystallization Treatment Step) Next, the cast steel product is reheated to 800-1100°C, held at 800-1100°C for 0.5-5 hours, and then rapidly cooled. This causes the martensite-formed structure to revert to an austenite structure. While the grain size of a structure formed by normal solidification is approximately 1-10 mm, the austenite structure becomes a fine structure with an average grain size of 200 μm or less, centered on equiaxed crystals, through the above-mentioned cryo-treatment step and the subsequent recrystallization treatment step. The cooling rate of the rapid cooling is preferably 10°C / min or more, more preferably 30°C / min or more, and even more preferably 100°C / min or more, as the average cooling rate from the holding temperature to room temperature. Figure 2 shows an example of the structure after the recrystallization treatment step. It can be seen that the structure after the recrystallization treatment step has become a fine structure with an average grain size of 200 μm or less.

[0033] (Solution Treatment Step) Before cryo-treatment, a solution treatment step may be performed in which the cast steel product is heated to 800 to 1100°C, held for 0.5 to 5 hours, and then rapidly cooled. The solution treatment step is not an essential step and may be performed as needed. By solution treatment, precipitates that precipitated during casting are dissolved, improving ductility and toughness.

[0034] (Diffusion Treatment Step) A diffusion treatment step may be further provided before the cryo-treatment step (or before the solution treatment step if a solution treatment step is provided), in which the cast steel product is held at 1100 to 1300°C for 5 to 50 hours. The diffusion treatment step is not an essential step and may be performed as needed. This eliminates the segregation of Ni and impurities in the steel, and allows for the more stable production of cast steel products with a low thermal expansion coefficient, even for large-sized cast steel products.

[0035] (Tempering Treatment Step) Between the cryo-treatment step and the recrystallization treatment step, the cast steel product may be subjected to martensite tempering treatment in which the cast steel product is heated to 300 to 400°C, just below the AC3 point, and held at 300 to 400°C for 1 to 10 hours, in order to further refine the recrystallized austenite grains. The tempering treatment step is not an essential step and may be performed as needed.

[0036] Example 1 Using a high-frequency melting furnace, a molten metal was poured into a mold to produce a Y-type test material having the composition shown in No. 1 in Table 1. The produced Y-type test material was cooled to -80°C and subjected to cryo-treatment by holding the temperature for 1.5 hours, subsequently subjected to thermal refining treatment by heating to 350°C and holding the temperature for 4 hours, and further subjected to recrystallization treatment by reheating to 1100°C, holding the temperature for 2.0 hours, and quenching at 2000°C / min, to obtain a low-thermal-expansion cast steel product.

[0037] <Inventive Examples 2 to 8, Comparative Examples 1 to 6> Low thermal expansion cast steel products were obtained in the same manner as in Example 1, except that the composition, cryo-treatment, and recrystallization temperatures were as shown in Tables 1 and 2. For each treatment temperature in Table 2, a "-" indicates that the corresponding step was not performed. Inventive Example 6 and Comparative Example 5, the aforementioned diffusion treatment step was performed before the cryo-treatment step. Inventive Examples 7 and 8 and Comparative Example 6, the aforementioned solution treatment step was performed before the cryo-treatment step, and in Inventive Example 8, an additional diffusion treatment step was performed before the solution treatment step. Furthermore, in Inventive Examples 1, 2, 6, and 8 and Comparative Examples 1, 2, and 4, the aforementioned tempering treatment step was performed between the cryo-treatment step and the recrystallization treatment step. The holding temperatures for the diffusion treatment step, solution treatment step, and tempering treatment step were as shown in Table 2, and the holding times were 20 hours, 2 hours, and 5 hours, respectively. The MS points listed in Table 2 are values ​​calculated using the above-mentioned estimation formula.

[0038] (Average Austenite Grain Size and Average Thermal Expansion Coefficient from 25 to 100° C.) The average austenite grain size and average thermal expansion coefficient from 25 to 100° C. were determined for the obtained low thermal expansion cast steel products by the above-mentioned method.

[0039] (Platability) The platability was evaluated by the following method: A sample of 50 mm × 50 mm × 10 mm thick was taken from the obtained low thermal expansion cast steel product, and the surface was pickled with hydrochloric acid, and then further pickled with a mixed solution of hydrochloric acid and sulfuric acid, and then immersed for 8 hours so that the Ni plating thickness became approximately 100 μm.

[0040] After plating, a 50 mm × 50 mm surface of the sample was observed with an optical microscope, and the presence or absence of plating defects (pinholes) with a diameter of 200 μm or more was evaluated. When no pinholes were observed, the plating property was judged to be good.

[0041] The results are shown in Table 2.

[0042]

[0043]

[0044] As shown in Table 2, it was confirmed that the low thermal expansion cast steel products of the present invention had a low thermal expansion coefficient at 25 to 100°C and also had good platability.

[0045] Comparative Example 1 had a low Co content and a high thermal expansion coefficient.

[0046] Comparative Example 2 had a high content of Co, S, and O, resulting in a large thermal expansion coefficient and poor plating properties.

[0047] Comparative Example 3 is an example in which the Ni content was high, the Al and O contents were low, and further, cryo-treatment and recrystallization treatment were not performed. As a result, the crystal grain size was not refined, the thermal expansion coefficient was large, and the plating property was poor.

[0048] Comparative Example 4 had a large Si and Mn content and a small Ni and Co content, resulting in a large thermal expansion coefficient.

[0049] Comparative Example 5 had a low Co content and a large thermal expansion coefficient.

[0050] Comparative Example 6 had a high content of Co, S, and O, resulting in a large thermal expansion coefficient and poor plating properties.

Claims

1. The chemical composition, by mass%, is C: 0.040% or less, Si: 0.30% or less, Mn: 0.50% or less, S: 0.010% or less, Ni: 31.00 to 34.00%, Co: 4.90 to 6.00%, O: 0.0100% or less, and Al: 0.010 to 0.100%, with the balance being Fe and unavoidable impurities; the average grain size of the austenitic structure is 200 μm or less; and the average thermal expansion coefficient at 25 to 100 °C is 0.4 × 10 -6 / °C or less.

2. A method for producing a low thermal expansion cast steel product according to claim 1, comprising the steps of: a cryo-treatment step of cooling a cast steel product having a chemical composition, by mass%, of C: 0.040% or less, Si: 0.30% or less, Mn: 0.50% or less, S: 0.010% or less, Ni: 31.00-34.00%, Co: 4.90-6.00%, O: 0.0100% or less, and Al: 0.010-0.100%, with the balance being Fe and unavoidable impurities, to the Ms point or below, holding the temperature at the Ms point or below for 0.5-3 hours, and then raising the temperature to room temperature; and a recrystallization step of heating the cryo-treated cast steel product to 800-1100°C, holding the temperature for 0.5-5 hours, and then quenching.

Citation Information

Patent Citations

  • Fe-ni-co alloy for electron gun parts, electron gun press punched work piece and electron gun electrode

    JP1999269616A

  • iron-nickel-cobalt alloy

    JP2009525400A

  • High-rigidity low-thermal expansion casting and method for producing the same

    JP2016027187A

  • Low-thermal expansion cast steel product and method for producing the same

    JP2016027188A

  • Low thermal expansion alloy

    JP2018145491A