Adhesive sheet, method for producing adhesive sheet, and method for producing article

The adhesive sheet with a tacky adhesive layer of specific tack and hardness addresses slipperiness and blocking issues, enhancing handling and bonding efficiency by preventing cracking and peeling during storage and use.

WO2024219465A1PCT designated stage expired Publication Date: 2024-10-24DAI NIPPON PRINTING CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015421
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-18
Filing Date
2024-04-18
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Adhesive sheets with high tackiness have poor slipperiness, leading to insertion difficulties, and are prone to blocking, cracking, lifting, and peeling during storage and use, especially when rolled or bent, due to inadequate blocking resistance and adhesive layer stability.

Method used

An adhesive sheet with a base material and a first adhesive layer on one side, having a tack of less than 0.1N and Martens hardness between 20N/mm² and 130N/mm², which improves slipperiness and blocking resistance while preventing cracking, lifting, and peeling during winding and bending.

Benefits of technology

The adhesive sheet achieves balanced adhesive performance, easy handling, and reduced risk of adhesive layer failure during storage and use, allowing smooth insertion and effective bonding between members.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015421_24102024_PF_FP_ABST
    Figure JP2024015421_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure provides an adhesive sheet having: a substrate; and a first adhesive layer that is disposed on one surface side of the substrate and contains a first curable adhesive, wherein the tack of the first adhesive layer is less than 0.1 N, and the Martens hardness of the first adhesive layer is 20 N / mm2 to 130 N / mm2.
Need to check novelty before this filing date? Find Prior Art

Description

Adhesive sheet, method for manufacturing an adhesive sheet, and method for manufacturing an article

[0001] The present disclosure relates to an adhesive sheet and a method for producing the same, as well as a method for producing an article using the adhesive sheet.

[0002] Adhesives for bonding two components are used in a variety of fields. Liquid adhesives are the mainstream of adhesives. However, liquid adhesives can cause problems such as uneven application, spillage, and dripping, making the bonding process more complicated.

[0003] On the other hand, in recent years, the use of sheet-type adhesives, i.e., adhesive sheets, instead of liquid adhesives has been proposed, and adhesive sheets containing a foaming agent (foamable adhesive sheets) have also been proposed (see, for example, Patent Documents 1 and 2).

[0004] International Publication No. 2016 / 163514 Japanese Patent Application Laid-Open No. 2019-203062

[0005] One example of a method for bonding two components using an adhesive sheet is to place an adhesive sheet between the two components and then cure the adhesive sheet to bond the two components. In this method, for example, the adhesive sheet may be inserted into the gap between the two components, or one component and the adhesive sheet may be inserted into a hole or groove in the other component. In these cases, if the adhesive sheet has high tack, the adhesive sheet's slipperiness may be poor, making it difficult to insert the adhesive sheet.

[0006] Furthermore, adhesive sheets are desirably resistant to blocking, as blocking may occur during storage. Blocking is a phenomenon in which adhesive sheets stick together when they come into contact with each other.

[0007] Furthermore, adhesive sheets are sometimes stored in a rolled state. When placing an adhesive sheet between two components, the adhesive sheet may be folded to fit the shape of the components, for example. In these cases, the adhesive sheet may crack. Furthermore, when an adhesive sheet has an adhesive layer on one or both sides of a substrate, the adhesive layer may lift or peel off from the substrate when the sheet is wound up or folded. Therefore, it is also desirable for the adhesive sheet to be resistant to cracking, lifting, or peeling of the adhesive layer when the sheet is wound up or folded.

[0008] The present disclosure has been made in consideration of the above-mentioned circumstances, and has as its main object to provide an adhesive sheet in which the adhesive layer has good slip properties and blocking resistance, and which can suppress cracking, lifting, and peeling of the adhesive layer when wound up or folded.

[0009] One embodiment of the present disclosure is an adhesive sheet having a substrate and a first adhesive layer disposed on one side of the substrate and containing a first curable adhesive, wherein the tack of the first adhesive layer is less than 0.1 N and the Martens hardness of the first adhesive layer is 20 N / mm 2 130N / mm or more 2 An adhesive sheet is provided, which is:

[0010] Another embodiment of the present disclosure is a method for producing an adhesive sheet, including a first adhesive layer forming step of applying a first adhesive composition containing a first curable adhesive to one side of a substrate and drying the applied composition to form a first adhesive layer, wherein the tack of the first adhesive layer is less than 0.1 N, and in the first adhesive layer forming step, the Martens hardness of the first adhesive layer is 20 N / mm 2 130N / mm or more 2 The present invention provides a method for producing an adhesive sheet, which comprises drying the first adhesive composition as follows:

[0011] Another embodiment of the present disclosure provides a method for manufacturing an article, comprising: a placement step of placing the above-mentioned adhesive sheet between a first member and a second member; and a bonding step of curing the adhesive sheet to bond the first member and the second member.

[0012] The adhesive sheet of the present disclosure has an adhesive layer with good slip properties and blocking resistance, and exhibits the effect of being able to suppress cracking, lifting, and peeling of the adhesive layer when wound up or folded.

[0013] FIG. 1 is a schematic cross-sectional view showing an example of an adhesive sheet according to the present disclosure. FIG. 2 is a schematic perspective view showing another example of an adhesive sheet according to the present disclosure. FIG. 3 is a schematic cross-sectional view showing another example of an adhesive sheet according to the present disclosure. FIG. 4 is a schematic cross-sectional view showing another example of an adhesive sheet according to the present disclosure. FIG. 5 is a schematic cross-sectional view showing another example of an adhesive sheet according to the present disclosure. FIG. 6 is a schematic cross-sectional view showing another example of an adhesive sheet according to the present disclosure. FIG. 7 is a schematic cross-sectional view showing an example of a method for manufacturing an adhesive sheet according to the present disclosure. FIG. 8 is a schematic cross-sectional view showing an example of a method for manufacturing an article according to the present disclosure.

[0014] Embodiments of the present disclosure will be described below with reference to the drawings and the like. However, the present disclosure can be implemented in many different forms and should not be construed as being limited to the description of the embodiments exemplified below. Furthermore, to clarify the explanation, the drawings may show the width, thickness, shape, etc. of each part schematically compared to the actual form, but these are merely examples and do not limit the interpretation of the present disclosure. Furthermore, in this specification and each drawing, elements similar to those described above with reference to the previous drawings may be designated by the same reference numerals, and detailed descriptions may be omitted as appropriate.

[0015] In this specification, when describing a mode in which another component is placed on a certain component, the term "above" or "below" is used, unless otherwise specified, to include both a case in which another component is placed directly above or below a certain component so as to be in contact with the component, and a case in which another component is placed above or below a certain component with another component interposed therebetween. Also, in this specification, when describing a mode in which another component is placed on the surface of a certain component, the term "on the surface side" or "on the surface" is used, unless otherwise specified, to include both a case in which another component is placed directly above or below a certain component so as to be in contact with the component, and a case in which another component is placed above or below a certain component with another component interposed therebetween.

[0016] In this specification, the term "sheet" also includes a member called a "film." In addition, the term "film" also includes a member called a "sheet." In addition, the numerical ranges in this specification are ranges of average values.

[0017] The adhesive sheet, the method for producing the adhesive sheet, and the method for producing the article according to the present disclosure will be described in detail below.

[0018] A. Adhesive Sheet The inventors of the present disclosure conducted extensive research into adhesive sheets having adhesive layers on one or both sides of a substrate. First, to improve the slipperiness of the adhesive layer, for example, making the adhesive layer non-tacky (tack-free) is effective. However, a non-tacky adhesive layer tends to harden, making the adhesive layer more susceptible to cracking, lifting, and peeling when the adhesive sheet is wound up or folded. Next, when the adhesive layer is non-tacky and the adhesive sheet is wound into a roll, it is common to wind the adhesive sheet into a roll without placing a separator on the side of the non-tacky adhesive layer opposite the substrate, in consideration of cost reduction and preventing separator slippage. However, in this case, the non-tacky adhesive layer is not protected by a separator, which can lead to blocking. When the adhesive layer is non-tacky, to improve the blocking resistance of the adhesive layer, for example, making the adhesive layer hard is effective. However, as mentioned above, if the adhesive layer is too hard, the adhesive layer tends to crack, lift, or peel when the adhesive sheet is wound or bent. The inventors of the present disclosure have conducted extensive research and found that by setting the tack of the adhesive layer within a predetermined range and the Martens hardness of the adhesive layer within a predetermined range, it is possible to achieve a good balance between improving the slip properties and blocking resistance of the adhesive layer and suppressing cracking, lift, or peeling of the adhesive layer when the adhesive sheet is wound or bent. The present disclosure is based on this finding.

[0019] The adhesive sheet according to the present disclosure has a substrate and a first adhesive layer disposed on one side of the substrate and containing a first curable adhesive, wherein the tack of the first adhesive layer is less than 0.1 N and the Martens hardness of the first adhesive layer is 20 N / mm 2 130N / mm or more2 The following is the result.

[0020] In the present disclosure, by having the tack of the first adhesive layer be less than a predetermined value and the Martens hardness of the first adhesive layer be within a predetermined range, it is possible to achieve a good balance between improving the slipperiness and blocking resistance of the first adhesive layer and suppressing cracking, lifting, and peeling of the first adhesive layer when winding and bending.

[0021] Furthermore, in the present disclosure, the tackiness of the first adhesive layer is less than a predetermined value, and the first adhesive layer is substantially non-sticky (tack-free), thereby improving the handleability and workability of the adhesive sheet.

[0022] The "tack" is a value measured by a probe tack test. The method for measuring tack will be described later.

[0023] The adhesive sheet of the present disclosure has three preferred embodiments.

[0024] A first embodiment of the adhesive sheet of the present disclosure has a substrate and a first adhesive layer disposed on one side of the substrate and containing a first curable adhesive, wherein the tack of the first adhesive layer is less than 0.1 N and the Martens hardness of the first adhesive layer is 20 N / mm 2 130N / mm or more 2 The following is the result.

[0025] Figure 1 is a schematic cross-sectional view illustrating a first embodiment of an adhesive sheet according to the present disclosure. Adhesive sheet 10A in Figure 1 has a substrate 1 and a first adhesive layer 2 disposed on one side of substrate 1 and containing a first curable adhesive. Adhesive sheet 10A does not have another adhesive layer on the other side of substrate 1. The tack of first adhesive layer 2 is less than a predetermined value, and the Martens hardness of first adhesive layer 2 is within a predetermined range.

[0026] In adhesive sheet 10A shown in Fig. 1 , the tack of first adhesive layer 2 is less than a predetermined value, so first adhesive layer 2 is substantially non-tacky (tack-free). Therefore, when adhesive sheet 10A is wound into a roll, a separator is usually not placed on the side of first adhesive layer 2 opposite substrate 1, taking into consideration cost reduction and preventing separator slippage. In this case, as shown in Fig. 2 for example, in roll-shaped adhesive sheet 10A, first adhesive layer 2 and substrate 1 come into contact, raising concerns about blocking.

[0027] To improve the slipperiness and blocking resistance, for example, it is effective to harden the first adhesive layer. However, if the first adhesive layer is hardened, the first adhesive layer becomes more likely to crack or to lift or peel off from the substrate when the adhesive sheet is wound into a roll or folded. Furthermore, for example, if the first adhesive layer further contains a foaming agent, a hard first adhesive layer makes it difficult for the first adhesive layer to expand during foam curing, resulting in a lower foaming ratio. As a result, when an adhesive sheet is placed between two components and then foam cured to fill and bond the two components, the gap between the two components cannot be sufficiently filled, and the adhesiveness after foam curing is reduced.

[0028] In contrast, in the first embodiment, since the Martens hardness of the first adhesive layer is within a predetermined range, cracking, lifting, and peeling of the first adhesive layer when the adhesive sheet is wound up and folded can be suppressed, while the slipperiness of the first adhesive layer can be improved and blocking of the first adhesive layer can be suppressed. Furthermore, if the first adhesive layer contains a foaming agent, the adhesiveness after foaming and curing is also improved.

[0029] Furthermore, in the first embodiment, the tackiness of the first adhesive layer is less than a predetermined value, and the first adhesive layer is substantially non-tacky (tack-free), thereby improving the slipperiness of the first adhesive layer. Therefore, for example, when adhering two components by placing an adhesive sheet between them and then curing the adhesive sheet, the adhesive sheet can be smoothly inserted into the gap between the two components. Alternatively, one component and the adhesive sheet can be smoothly inserted into a hole or groove in the other component. Alternatively, after placing the adhesive sheet in a hole or groove in one component, the other component can be inserted into the gap. Furthermore, when aligning two components by moving one component relative to the other component, the other component can be smoothly moved relative to the first component while the other component is inserted into the hole or groove in the first component, facilitating alignment.

[0030] A second embodiment of the adhesive sheet of the present disclosure has a substrate, a first adhesive layer disposed on one side of the substrate and containing a first curable adhesive, and a second adhesive layer disposed on the other side of the substrate and containing a second curable adhesive, wherein the tack of the first adhesive layer and the second adhesive layer is less than 0.1 N, and the Martens hardness of the first adhesive layer and the second adhesive layer is 20 N / mm 2 130N / mm or more 2 The following is the result.

[0031] Figure 3 is a schematic cross-sectional view illustrating a second embodiment of an adhesive sheet according to the present disclosure. Adhesive sheet 10B in Figure 3 has a substrate 1, a first adhesive layer 2 disposed on one side of substrate 1 and containing a first curable adhesive, and a second adhesive layer 3 disposed on the other side of substrate 1 and containing a second curable adhesive. The tack of first adhesive layer 2 and second adhesive layer 3 is less than a predetermined value, and the Martens hardness of first adhesive layer 2 and second adhesive layer 3 is within a predetermined range.

[0032] 3 , the tackiness of the first adhesive layer 2 and the second adhesive layer 3 is less than a predetermined value, and therefore the first adhesive layer 2 and the second adhesive layer 3 are substantially non-tacky (tack-free). Therefore, when the adhesive sheet 10B is wound into a roll, in consideration of cost reduction and prevention of separator slippage, a separator is usually not placed on the surface of the first adhesive layer 2 opposite the substrate 1, and on the surface of the second adhesive layer 3 opposite the substrate 1. In this case, the first adhesive layer 2 and the second adhesive layer 3 come into contact, which raises concerns about blocking.

[0033] To improve the slipperiness and blocking resistance, for example, it is effective to harden the first adhesive layer and the second adhesive layer. However, if the first adhesive layer and the second adhesive layer are hardened, the first adhesive layer and the second adhesive layer are likely to crack or to lift or peel off from the substrate when the adhesive sheet is wound into a roll or folded. Furthermore, for example, when at least one of the first adhesive layer and the second adhesive layer further contains a foaming agent, if the foaming agent-containing adhesive layer is hard, the adhesive layer will not expand easily when foaming and curing, resulting in a lower expansion ratio. Therefore, when an adhesive sheet is placed between two components and then the foaming agent-containing adhesive layer is foamed and cured to fill and bond the two components, the gap between the two components cannot be sufficiently filled, and the adhesion after foaming and curing is reduced.

[0034] In contrast, in a second embodiment, when the tack of the first adhesive layer and the second adhesive layer is less than a predetermined value, by having the Martens hardness of the first adhesive layer and the second adhesive layer be within a predetermined range, cracking, lifting, and peeling of the first adhesive layer and the second adhesive layer when the adhesive sheet is wound up and folded can be suppressed, while the slipperiness of the first adhesive layer and the second adhesive layer can be improved and blocking of the first adhesive layer and the second adhesive layer can be suppressed. Furthermore, when at least one of the first adhesive layer and the second adhesive layer contains a foaming agent, the adhesion after foaming and curing is also improved.

[0035] In the second embodiment, the tackiness of the first adhesive layer and the second adhesive layer is less than a predetermined value, and the first adhesive layer and the second adhesive layer are substantially non-tacky (tack-free), resulting in good slipperiness of the first adhesive layer and the second adhesive layer. Therefore, for example, when bonding two components by placing an adhesive sheet between them and then curing the adhesive sheet, the adhesive sheet can be smoothly inserted into the gap between the two components. Alternatively, one component and the adhesive sheet can be smoothly inserted into a hole or groove in the other component. Alternatively, after placing the adhesive sheet in a hole or groove in one component, the other component can be inserted into the gap. Furthermore, when aligning two components by moving one component relative to the other component, the other component can be smoothly moved relative to the first component while the other component is inserted into the hole or groove in the first component, facilitating alignment.

[0036] A third embodiment of an adhesive sheet according to the present disclosure comprises a substrate, a first adhesive layer disposed on one side of the substrate and containing a first curable adhesive, a second adhesive layer disposed on the other side of the substrate and containing a second curable adhesive, and a separator disposed on the side of the second adhesive layer opposite the substrate, wherein the tack of the first adhesive layer is less than 0.1 N, the tack of the second adhesive layer is 0.1 N or more, and the Martens hardness of the first adhesive layer is 20 N / mm 2 130N / mm or more 2 The following is the result.

[0037] Figure 4 is a schematic cross-sectional view illustrating a third embodiment of an adhesive sheet according to the present disclosure. Adhesive sheet 10C in Figure 4 has a substrate 1, a first adhesive layer 2 disposed on one side of substrate 1 and containing a first curable adhesive, a second adhesive layer 3 disposed on the other side of substrate 1 and containing a second curable adhesive, and a separator 4 disposed on the side of second adhesive layer 3 opposite substrate 1. The tack of first adhesive layer 2 is less than a predetermined value, the tack of second adhesive layer 3 is equal to or greater than a predetermined value, and the Martens hardness of first adhesive layer 2 is within a predetermined range.

[0038] In adhesive sheet 10C shown in Fig. 4, the tackiness of first adhesive layer 2 is less than a predetermined value, so first adhesive layer 2 is substantially non-tacky (tack-free). Therefore, when adhesive sheet 10C is wound into a roll, a separator is usually not placed on the side of first adhesive layer 2 opposite substrate 1, taking into consideration cost reduction and preventing separator slippage. On the other hand, because second adhesive layer 3 is adhesive, separator 4 is placed on the side of second adhesive layer 3 opposite substrate 1. In this case, first adhesive layer 2 and separator 4 come into contact, raising concerns about blocking.

[0039] To improve the slipperiness and blocking resistance, for example, it is effective to harden the first adhesive layer. However, if the first adhesive layer is hardened, the first adhesive layer becomes more likely to crack or to lift or peel off from the substrate when the adhesive sheet is wound into a roll or folded. Furthermore, for example, if the first adhesive layer further contains a foaming agent, a hard first adhesive layer makes it difficult for the first adhesive layer to expand during foam curing, resulting in a lower foaming ratio. As a result, when an adhesive sheet is placed between two components and then foam cured to fill and bond the two components, the gap between the two components cannot be sufficiently filled, and the adhesiveness after foam curing is reduced.

[0040] In contrast, in a third embodiment, when the tack of the first adhesive layer is less than a predetermined value, by having the Martens hardness of the first adhesive layer within a predetermined range, it is possible to suppress cracking of the first adhesive layer when the adhesive sheet is wound up or folded, improve the slipperiness of the first adhesive layer, and suppress blocking of the first adhesive layer. Furthermore, when the first adhesive layer contains a foaming agent, the adhesiveness after foaming and curing is also improved.

[0041] In a third embodiment, the tack of the first adhesive layer is less than a predetermined value, making the first adhesive layer substantially non-tacky (tack-free), thereby improving the slipperiness of the first adhesive layer. On the other hand, the tack of the second adhesive layer is equal to or greater than a predetermined value, thereby improving the adhesion of the second adhesive layer to the member. Therefore, for example, when bonding two members by placing an adhesive sheet between two members and then curing the adhesive sheet, after attaching the second adhesive layer surface of the adhesive sheet to one member, the member with the adhesive sheet attached can be smoothly inserted into a hole or groove in the other member. Furthermore, when inserting the member with the adhesive sheet attached into a hole or groove in the other member, peeling and misalignment of the adhesive sheet relative to the one member can be suppressed. Furthermore, when aligning two members by moving one member relative to the other member, the member with the adhesive sheet attached can be smoothly moved relative to the other member while inserted into the hole or groove in the other member, facilitating alignment.

[0042] Here, non-tacky is generally used mainly to mean low adhesive strength. In the present disclosure, "substantially non-tacky" means that the tack is less than 0.1 N.

[0043] "Adhesion" is a concept that is included in "adhesion." The two are sometimes distinguished in that "adhesion" is used to mean a temporary adhesive phenomenon, while "adhesion" is used to mean a substantially permanent adhesive phenomenon (Iwanami Shoten Physics and Chemistry Dictionary, 5th Edition). "Adhesion" and "adhesive strength" refer to the property of adhering by pressure and the adhesive strength at that time.

[0044] In this specification, unless otherwise specified, the terms "adhesion of the adhesive layer" and "adhesion strength of the adhesive layer" refer to the adhesion and adhesive strength of the adhesive layer before curing. In addition, in this specification, unless otherwise specified, the terms "adhesion of the adhesive layer" and "adhesion strength of the adhesive layer" refer to the adhesion and adhesive strength of the adhesive layer after curing.

[0045] Hereinafter, various embodiments of the adhesive sheet according to the present disclosure will be described.

[0046] I. First Embodiment of Adhesive Sheet A first embodiment of an adhesive sheet in the present disclosure includes a substrate and a first adhesive layer disposed on one side of the substrate and containing a first curable adhesive, wherein the tack of the first adhesive layer is less than 0.1 N and the Martens hardness of the first adhesive layer is 20 N / mm 2 130N / mm or more 2 The adhesive sheet of this embodiment does not have another adhesive layer on the other side of the substrate.

[0047] Each component of the adhesive sheet of this embodiment will be described below.

[0048] 1. First Adhesive Layer In this embodiment, the first adhesive layer is disposed on one side of the substrate and contains a first curable adhesive. Also, in this embodiment, the tack of the first adhesive layer is less than a predetermined value, and the Martens hardness of the first adhesive layer is within a predetermined range.

[0049] (1) Physical Properties of the First Adhesive Layer The tackiness of the first adhesive layer in this embodiment is less than 0.1 N, and may be 0.05 N or less, or may be 0.02 N or less. When the tackiness of the first adhesive layer is within the above range, the first adhesive layer can be made substantially non-sticky (tack-free). In addition, the slipperiness of the first adhesive layer is improved.

[0050] Here, the tackiness of the first adhesive layer is measured by a probe tack test. Specifically, a cylindrical stainless steel probe with a diameter of 5 mm is pressed against the surface of the first adhesive layer of the foamable adhesive sheet under conditions of a temperature of 23±5°C and a humidity of 50±30% RH at a load of 0.1 N and a speed of 30 mm / min, and after holding for 1.0 second, it is peeled off at a speed of 30 mm / min, and the load at the time of peeling is measured. This measurement is performed five times, and the average value is taken as the tackiness. As a probe tackiness tester, for example, a tackiness tester "TAC-II" manufactured by RHESCA can be used.

[0051] In this embodiment, an example of a method for controlling the tackiness of the first adhesive layer is to adjust the composition of the first adhesive layer. Specifically, the tackiness of the first adhesive layer can be reduced by using an epoxy resin that is solid at room temperature or a curing agent that is solid at room temperature in the first adhesive layer containing an epoxy resin and a curing agent. Furthermore, the tackiness of the first adhesive layer can be reduced by including an epoxy resin with a high softening temperature or an epoxy resin with a high weight-average molecular weight in the first adhesive layer containing an epoxy resin and a curing agent. For example, the tackiness of the first adhesive layer can be reduced by including multiple epoxy resins with different softening temperatures in the first adhesive layer, i.e., by including one epoxy resin and another epoxy resin with a softening temperature of 25°C or higher and 10°C or higher than the softening temperature of the first epoxy resin. Furthermore, for example, the tackiness of the first adhesive layer can be reduced by including multiple epoxy resins with different weight-average molecular weights in the first adhesive layer. That is, the first adhesive layer can include one epoxy resin and another epoxy resin with a weight-average molecular weight of 370 or more that is 300 or more greater than that of the first epoxy resin. More specifically, the tackiness of the first adhesive layer can be reduced by including a first epoxy resin with a low softening temperature and low molecular weight and a second epoxy resin with a high softening temperature and high molecular weight, as described below, in the first adhesive layer containing an epoxy resin and a curing agent. The tackiness of the first adhesive layer can also be reduced by including an acrylic resin that is compatible with the epoxy resin, as described below, in the first adhesive layer containing an epoxy resin and a curing agent.

[0052] The Martens hardness of the first adhesive layer in this embodiment is 20 N / mm 2 or more, and 2 It may be 40 N / mm or more. 2 When the Martens hardness of the first adhesive layer is in the above range, blocking resistance can be improved. In addition, the Martens hardness of the first adhesive layer may be 130 N / mm or more. 2 or less, 110 N / mm 2 It may be 90 N / mm or less2 If the Martens hardness of the first adhesive layer is in the above range, cracking, lifting, and peeling of the first adhesive layer can be suppressed when the adhesive sheet is wound up and folded. Specifically, the Martens hardness of the first adhesive layer may be 20 N / mm or less. 2 130N / mm or more 2 or less, 30 N / mm 2 110N / mm or more 2 It may be 40 N / mm or less 2 90N / mm or more 2 It may be the following:

[0053] Here, the Martens hardness of the first adhesive layer is measured by the indentation method in accordance with ISO 14577. The Martens hardness (HM) is calculated using the following formula: HM = F / As (In the above formula, F: indentation load, and As: surface area of ​​the indenter at the indentation depth.) As the ultra-microhardness tester, a "Picodentor HM500" manufactured by Fisher Instruments can be used. The following indenter is used. The measurement conditions are also shown below. Note that the indentation load is set small to eliminate dependence on thickness. Specifically, the indentation load is set so that the indentation depth is approximately 1 / 10 or less of the first adhesive layer.

[0054] (Indenter) Shape: regular square pyramid Material: diamond

[0055] (Measurement conditions) Indentation load: 25 mN Load time: 20 seconds Holding time: 5 seconds Temperature: 23±5°C Humidity: 50±30% RH

[0056] In this embodiment, methods for controlling the Martens hardness of the first adhesive layer include, for example, adjusting the composition of the first adhesive layer and adjusting the drying conditions when forming the first adhesive layer.

[0057] Specifically, in a method for adjusting the composition of the first adhesive layer, the Martens hardness of the first adhesive layer tends to increase when an epoxy resin that is solid at room temperature or a curing agent that is solid at room temperature is used in the first adhesive layer containing an epoxy resin and a curing agent. Furthermore, the Martens hardness of the first adhesive layer tends to increase when an epoxy resin with a high softening temperature or an epoxy resin with a high weight-average molecular weight is used in the first adhesive layer containing an epoxy resin and a curing agent. For example, the Martens hardness of the first adhesive layer tends to increase when the first adhesive layer contains multiple epoxy resins with different softening temperatures, i.e., when the first adhesive layer contains one epoxy resin and another epoxy resin whose softening temperature is 25°C or higher and 10°C or higher than the softening temperature of the first epoxy resin. Furthermore, for example, the Martens hardness of the first adhesive layer tends to be increased by including multiple epoxy resins with different weight-average molecular weights in the first adhesive layer, i.e., by including one epoxy resin and another epoxy resin with a weight-average molecular weight of 370 or more and 300 or more greater than that of the first epoxy resin. More specifically, in a first adhesive layer containing an epoxy resin and a curing agent, the Martens hardness of the first adhesive layer tends to be increased by including a first epoxy resin with a low softening temperature and a low molecular weight and a second epoxy resin with a high softening temperature and a high molecular weight, as described below. Furthermore, in a first adhesive layer containing an epoxy resin and a curing agent, the Martens hardness of the first adhesive layer tends to be increased by including an acrylic resin that is compatible with the epoxy resin, as described below.

[0058] Furthermore, in a method of adjusting the drying conditions during the formation of the first adhesive layer, for example, when the first adhesive layer is formed by applying a first adhesive composition to one side of a substrate and drying it, the Martens hardness of the first adhesive layer can be controlled by adjusting the drying conditions. Examples of drying conditions include the drying temperature, thermal history, and air speed. Examples of thermal history include the temperature rise rate and the total amount of heat. For example, as the drying temperature increases, the Martens hardness of the first adhesive layer tends to increase. On the other hand, as the drying temperature decreases, the Martens hardness of the first adhesive layer tends to decrease. For example, as the temperature rise rate increases, the total amount of heat increases for a constant drying time, and therefore the Martens hardness of the first adhesive layer tends to increase. On the other hand, as the temperature rise rate decreases, the total amount of heat decreases for a constant drying time, and therefore the Martens hardness of the first adhesive layer tends to decrease. For example, as the total amount of heat received by the first adhesive layer increases, the Martens hardness of the first adhesive layer tends to increase. On the other hand, when the total amount of heat received by the first adhesive layer is reduced, the Martens hardness of the first adhesive layer tends to decrease. Also, for example, when the wind speed is increased, the drying speed is increased, and the Martens hardness of the first adhesive layer tends to increase. On the other hand, when the wind speed is decreased, the drying speed is decreased, and the Martens hardness of the first adhesive layer tends to decrease.

[0059] Furthermore, in this embodiment, when the first adhesive layer contains a foaming agent as described below, the first adhesive layer can be foamed at an expansion ratio of, for example, 1.5 times or more and 15 times or less. The expansion ratio may be, for example, 3.5 times or more, 4 times or more, or 4.5 times or more. The expansion ratio may be, for example, 9 times or less, 8.5 times or less, or 8 times or less. If the expansion ratio is too small, the gap between the two components may not be sufficiently filled, and the adhesiveness after foaming and curing may be reduced. If the expansion ratio is too large, the porosity of the first adhesive layer after foaming and curing may be increased, which may reduce the adhesiveness after foaming and curing.

[0060] Here, the expansion ratio is calculated by the following formula: Expansion ratio (times) = Thickness of the first adhesive layer after curing / Thickness of the first adhesive layer before curing

[0061] (2) Material of the First Adhesive Layer (a) First Curable Adhesive The first curable adhesive contained in the first adhesive layer in this embodiment can be a curable adhesive generally used in adhesive layers of adhesive sheets. Examples of the first curable adhesive include heat-curable adhesives and light-curable adhesives. Among these, heat-curable adhesives are preferred. Heat-curable adhesives can be applied even when the component does not have transparency, such as a metal component.

[0062] The first curable adhesive is preferably an epoxy resin adhesive. That is, the first curable adhesive preferably contains an epoxy resin and a curing agent. In general, epoxy resin adhesives produce hard and tough cured films, making them suitable for bonding hard material components such as metal and glass components. Furthermore, epoxy resin adhesives generally have excellent heat resistance, insulating properties, chemical resistance, etc., and exhibit little shrinkage upon curing, making them suitable for a wide range of applications.

[0063] Furthermore, when the first curable adhesive is an epoxy resin adhesive, the first curable adhesive preferably further contains an acrylic resin that is compatible with the epoxy resin. By using an acrylic resin that is compatible with the epoxy resin, the toughness of the first adhesive layer can be increased, thereby improving the adhesiveness after curing.

[0064] (i) Epoxy Resin The epoxy resin in this embodiment is a compound that has at least one epoxy group or glycidyl group and cures by crosslinking polymerization in combination with a curing agent. The epoxy resin also includes a monomer having at least one epoxy group or glycidyl group.

[0065] The epoxy resin can be any epoxy resin commonly used in adhesive layers of adhesive sheets. In particular, the curable adhesive preferably contains a first epoxy resin having a softening temperature of 50°C or higher and an epoxy equivalent of 5,000 g / eq or less, and a second epoxy resin having a softening temperature higher than that of the first epoxy resin and a weight-average molecular weight of 20,000 or more. By using a combination of the first epoxy resin and the second epoxy resin, an adhesive sheet with excellent blocking resistance and adhesive properties after curing can be obtained. Furthermore, the tackiness (tackiness) of the first adhesive layer can be reduced, resulting in an adhesive sheet with excellent slipperiness.

[0066] For example, when only improving adhesiveness after curing is desired, it is more effective to use a low molecular weight (low epoxy equivalent) epoxy resin than a high molecular weight (high epoxy equivalent) epoxy resin. However, when a low molecular weight (low epoxy equivalent) epoxy resin is used, for example, when the adhesive sheet is wound into a roll, the low molecular weight (low epoxy equivalent) epoxy resins tend to assimilate with each other, resulting in blocking.

[0067] In contrast, when a first epoxy resin having a relatively low softening temperature (relatively high crystallinity) and a low molecular weight (low epoxy equivalent weight) is used, the first epoxy resin rapidly melts and changes to a low-viscosity liquid when heated to a temperature above its softening temperature. This facilitates improved adhesiveness after curing. Meanwhile, the first epoxy resin has relatively high crystallinity, which can suppress blocking compared to epoxy resins with relatively low crystallinity or no crystallinity. However, using only the first epoxy resin may result in insufficient suppression of blocking, or excessive tackiness of the first adhesive layer. Therefore, by further using a second epoxy resin having a relatively high softening temperature (relatively low crystallinity) and a high molecular weight, the effect of suppressing blocking can be improved and the tackiness of the first adhesive layer can be suppressed.

[0068] (i-1) First Epoxy Resin The first epoxy resin has a softening temperature of 50°C or higher and an epoxy equivalent of 5000 g / eq or lower. The first epoxy resin has a relatively low softening temperature (relatively high crystallinity) compared to the second epoxy resin described below. The first epoxy resin has relatively high crystallinity and a low molecular weight, which makes it easy to improve adhesion and blocking resistance after curing. Furthermore, the first epoxy resin has a low molecular weight, which allows for a high crosslink density, resulting in a first adhesive layer with excellent mechanical strength, chemical resistance, and curing properties. Furthermore, the first epoxy resin is preferably an epoxy resin that is solid at room temperature (23°C).

[0069] The softening temperature of the first epoxy resin is usually 50° C. or higher, and may be 55° C. or higher, or 60° C. or higher. On the other hand, the softening temperature of the first epoxy resin is, for example, 150° C. or lower. The softening temperature is measured by the ring and ball method in accordance with JIS K7234:1986.

[0070] The epoxy equivalent of the first epoxy resin is, for example, 5000 g / eq or less, and may be 3000 g / eq or less, 1000 g / eq or less, or 600 g / eq or less. On the other hand, the epoxy equivalent of the first epoxy resin is, for example, 90 g / eq or more, 100 g / eq or more, or 110 g / eq or more. The epoxy equivalent is the number of grams of resin containing 1 gram equivalent of epoxy groups. The epoxy equivalent is measured by a method in accordance with JIS K7236:2009, which corresponds to ISO 3001 (Plastics - Epoxy compounds - Determination of epoxy equivalent).

[0071] The first epoxy resin may be a monofunctional epoxy resin, a difunctional epoxy resin, a trifunctional epoxy resin, or a tetrafunctional or higher functional epoxy resin.

[0072] The weight-average molecular weight (Mw) of the first epoxy resin is usually smaller than the weight-average molecular weight (Mw) of the second epoxy resin described below. The Mw of the first epoxy resin is, for example, 6,000 or less, and may be 4,000 or less, or 3,000 or less. On the other hand, the Mw of the first epoxy resin is, for example, 400 or more. Mw is a polystyrene-equivalent value measured by gel permeation chromatography (GPC).

[0073] The melt viscosity of the first epoxy resin at 150°C is, for example, 0.005 Pa·s or more, or may be 0.015 Pa·s or more, 0.03 Pa·s or more, 0.05 Pa·s or more, or 0.1 Pa·s or more. If the melt viscosity is too low, good foaming properties may not be obtained. Furthermore, if the melt viscosity of the first epoxy resin is too low (if the crystallinity of the first epoxy resin is too high), the resulting first adhesive layer may have high tackiness. This is presumably because if the melt viscosity of the first epoxy resin is too low (if the crystallinity of the first epoxy resin is too high), its crystallinity is significantly reduced when it is mixed with the second epoxy resin or the acrylic resin, thereby reducing the Tg of the entire adhesive composition. On the other hand, the melt viscosity of the first epoxy resin at 150°C is, for example, 10 Pa·s or less, or may be 5 Pa·s or less, or 2 Pa·s or less. If the melt viscosity is too high, the resulting first adhesive layer may have reduced uniformity. The melt viscosity is measured in accordance with JIS K6862:1984, which corresponds to ISO 2555 (Resins in the liquid state or as emulsions or dispersions—Determination of Brookfield RV viscosity), using a Brookfield-type single-cylinder rotational viscometer and a thermocell for heating the solution.

[0074] Next, the composition of the first epoxy resin will be described. Examples of the first epoxy resin include aromatic epoxy resins, aliphatic epoxy resins, alicyclic epoxy resins, and heterocyclic epoxy resins. Specific examples of the first epoxy resin include bisphenol-type epoxy resins, novolac-type epoxy resins, and modified epoxy resins. Examples of the bisphenol-type epoxy resin include bisphenol A-type epoxy resins and bisphenol F-type epoxy resins. Examples of the novolac-type epoxy resin include bisphenol A novolac-type epoxy resins and cresol novolac-type epoxy resins. Examples of the modified epoxy resin include urethane-modified epoxy resins and rubber-modified epoxy resins. Other specific examples include biphenyl-type epoxy resins, stilbene-type epoxy resins, triphenolmethane-type epoxy resins, alkyl-modified triphenolmethane-type epoxy resins, triazine-nucleus-containing epoxy resins, dicyclopentadiene-modified phenol-type epoxy resins, naphthalene-type epoxy resins, glycol-type epoxy resins, and pentaerythritol-type epoxy resins. The first epoxy resin may be one type or two or more types.

[0075] Bisphenol A epoxy resins can exist in a liquid state or a solid state at room temperature depending on the number of repeating units in the bisphenol skeleton. Bisphenol A epoxy resins having, for example, 2 to 10 bisphenol skeletons in the main chain are solid at room temperature. Bisphenol A epoxy resins are particularly preferred because they can improve heat resistance.

[0076] In particular, the first epoxy resin is preferably a bisphenol A novolac epoxy resin represented by the following general formula (1).

[0077]

[0078] In general formula (1), R 1 is C m H 2m (m is 1 or more and 3 or less), and R 2 and R 3 are each independently C p H2p+1 (p is 1 or more and 3 or less), and n is 0 or more and 10 or less.

[0079] In general formula (1), R 1 m in is 1, that is, R 1 Ha-CH 2 Similarly, R 2 and R 3 p in is 1, that is, R 2 and R 3 Ha-CH 3 Furthermore, the hydrogen bonded to the benzene ring in general formula (1) may be substituted with other elements or other groups.

[0080] The content of the first epoxy resin, relative to 100 parts by mass of the resin component contained in the first adhesive layer, may be, for example, 1 part by mass or more, 3 parts by mass or more, 5 parts by mass or more, 10 parts by mass or more, 15 parts by mass or more, or 25 parts by mass or more. If the content of the first epoxy resin is too low, the adhesiveness and blocking resistance after curing may be reduced. On the other hand, the content of the first epoxy resin, relative to 100 parts by mass of the resin component contained in the first adhesive layer, may be, for example, 90 parts by mass or less, 80 parts by mass or less, 70 parts by mass or less, 60 parts by mass or less, 50 parts by mass or less, or 40 parts by mass or less. If the content of the first epoxy resin is too high, the contents of the second epoxy resin and acrylic resin may be relatively low, which may make it difficult to balance blocking resistance, adhesion of the first adhesive layer to the substrate, and adhesiveness after curing.

[0081] (i-2) Second Epoxy Resin The second epoxy resin has a softening temperature higher than that of the first epoxy resin and a weight-average molecular weight of 20,000 or more. The second epoxy resin has a relatively high softening temperature (relatively low crystallinity) compared to the first epoxy resin described above. The second epoxy resin has relatively low crystallinity and a high molecular weight, which makes it easy to improve blocking resistance. Furthermore, the second epoxy resin has relatively low crystallinity and a high molecular weight, which can suppress an increase in adhesion (tackiness) caused by the first epoxy resin. In addition, the second epoxy resin is preferably an epoxy resin that is solid at room temperature (23°C).

[0082] The weight average molecular weight (Mw) of the second epoxy resin is usually larger than the weight average molecular weight (Mw) of the first epoxy resin. The Mw of the second epoxy resin is usually 20,000 or more, or may be 30,000 or more, or may be 35,000 or more. On the other hand, the Mw of the second epoxy resin is, for example, 100,000 or less.

[0083] The epoxy equivalent of the second epoxy resin may be greater than, less than, or the same as the epoxy equivalent of the first epoxy resin. The epoxy equivalent of the second epoxy resin is, for example, 4000 g / eq or more, 5000 g / eq or more, or 6000 g / eq or more. On the other hand, the epoxy equivalent of the second epoxy resin is, for example, 20000 g / eq or less.

[0084] The second epoxy resin may be a monofunctional epoxy resin, a difunctional epoxy resin, a trifunctional epoxy resin, or a tetrafunctional or higher functional epoxy resin.

[0085] The softening temperature of the second epoxy resin is usually higher than that of the first epoxy resin. The difference between the two temperatures is, for example, 10°C or higher, and may be 20°C or higher, or 30°C or higher. The softening temperature of the second epoxy resin is, for example, 80°C or higher, and may be 90°C or higher. On the other hand, the softening temperature of the second epoxy resin is, for example, 180°C or lower.

[0086] The constitution of the second epoxy resin is the same as that of the first epoxy resin described above, and therefore description thereof will be omitted here.

[0087] The content of the second epoxy resin, relative to 100 parts by mass of the resin component contained in the first adhesive layer, may be, for example, 10 parts by mass or more, 15 parts by mass or more, 20 parts by mass or more, 25 parts by mass or more, 30 parts by mass or more, 35 parts by mass or more, 40 parts by mass or more, or 45 parts by mass or more. If the content of the second epoxy resin is too low, blocking resistance may be reduced. On the other hand, the content of the second epoxy resin, relative to 100 parts by mass of the resin component contained in the first adhesive layer, may be, for example, 90 parts by mass or less, 85 parts by mass or less, 80 parts by mass or less, or 75 parts by mass or less. If the content of the second epoxy resin is too high, the contents of the first epoxy resin and acrylic resin may be relatively low, which may make it difficult to balance blocking resistance, adhesion of the first adhesive layer to the substrate, and adhesion after curing.

[0088] The proportion of the first epoxy resin relative to the total of the first epoxy resin and the second epoxy resin is, for example, 5% by mass or more, or alternatively 10% by mass or more, or 15% by mass or more, or alternatively 20% by mass or more, while the proportion of the first epoxy resin is, for example, 80% by mass or less, or alternatively 75% by mass or less, or alternatively 60% by mass or less.

[0089] Furthermore, the total proportion of the first epoxy resin and the second epoxy resin to all epoxy resins contained in the first adhesive layer is, for example, 50% by mass or more, or may be 70% by mass or more, or 90% by mass or more, or may be 100% by mass.

[0090] (ii) Acrylic Resin The acrylic resin in this embodiment is a resin compatible with epoxy resin. Because acrylic resin is compatible with epoxy resin, it is easy to improve the toughness of the first adhesive layer. As a result, the adhesion of the first adhesive layer to the substrate can be improved. Furthermore, improved toughness of the adhesive layer can improve adhesion after curing. Furthermore, it is thought that the acrylic resin acts as a compatibilizer for the foaming agent (for example, a foaming agent whose shell portion is an acrylonitrile copolymer resin), uniformly dispersing and foaming, thereby improving adhesion after curing. Furthermore, the compatibility of the acrylic resin with the epoxy resin can maintain high hardness of the surface of the first adhesive layer. On the other hand, if the acrylic resin is incompatible with the epoxy resin, a flexible portion is formed on the surface of the first adhesive layer, making the interface with the adherend less slippery and reducing workability.

[0091] In this embodiment, the acrylic resin is compatible with the epoxy resin. The compatibility of the acrylic resin with the epoxy resin can be confirmed by observing the cross section of the first adhesive layer of the adhesive sheet with a scanning electron microscope (SEM) or a transmission electron microscope (TEM) to see if micron-sized islands are present. More specifically, the average particle size of the islands is preferably 1 μm or less. In particular, the average particle size of the islands may be 0.5 μm or less, or even 0.3 μm or less. A large number of samples is preferably used, for example, 100 or more. The area to be observed is within a range of 100 μm × 100 μm, or, if the average thickness of the first adhesive layer is 100 μm or less, within a range of the average thickness × 100 μm.

[0092] The weight-average molecular weight (Mw) of the acrylic resin is, for example, 50,000 or more, or may be 70,000 or more, or even 100,000 or more. The first epoxy resin has relatively high crystallinity, which can result in a low melt viscosity (or dynamic viscoelasticity) when heated, potentially causing shrinkage during curing after foaming (between the end of foaming of the foaming agent and the curing of the adhesive composition). However, by using an acrylic resin with a certain molecular weight, it is possible to prevent the melt viscosity from becoming too low, making it less likely for shrinkage to occur during curing after foaming. Meanwhile, the Mw of the acrylic resin is, for example, 1,500,000 or less. The weight-average molecular weight of the acrylic resin is measured by GPC (eluent: THF, standard: PS, sample: 20 μL, flow rate: 1 mL / min, column temperature: 40°C).

[0093] The glass transition temperature (Tg) of the acrylic resin is, for example, 90° C. or higher, and may be 100° C. or higher. On the other hand, the Tg of the acrylic resin is, for example, 180° C. or lower. Tg is measured by a differential scanning calorimeter (DSC) in accordance with JIS K7121:2012, which corresponds to ISO 3146.

[0094] The acrylic resin has a storage modulus (E') of 1 x 10 at the foaming initiation temperature. 6 A low E' at the foaming initiation temperature can improve fluidity and provide good foaming properties. On the other hand, E' at the foaming initiation temperature can be, for example, 1 x 10 5 The foaming initiation temperature is a temperature that varies depending on the type of foaming agent. When two or more foaming agents are used, the foaming initiation temperature is the temperature at which the main foaming reaction begins.

[0095] The acrylic resin has a storage modulus (E') of 1 x 10 at the curing initiation temperature. 5Pa or more. As described above, shrinkage may occur during curing after foaming (from the time when foaming of the foaming agent is completed until the adhesive composition is cured). However, if E' at the curing initiation temperature is large, shrinkage can be suppressed and good shape retention can be obtained. The curing initiation temperature varies depending on the type of curing agent. When two or more curing agents are used as the curing agent, the initiation temperature of the main curing reaction is taken as the curing initiation temperature.

[0096] The acrylic resin has an average storage modulus (E') of 1 x 10 at temperatures between 0°C and 100°C. 6 The average value of E' before foaming may be high, which allows for good blocking resistance. On the other hand, the average value of the storage modulus (E') at temperatures of 0°C or higher and 100°C or lower may be, for example, 1 x 10 8 Pa or less.

[0097] The storage modulus (E') of the acrylic resin is measured by a dynamic viscoelasticity measurement method in accordance with JIS K7244-1:1998. The measurement conditions are as follows: attachment mode: compression mode, frequency: 1 Hz, temperature: -30°C to 200°C, and temperature rise rate: 10°C / min. The device that can be used is a solid viscoelasticity analyzer "RSA-III" manufactured by TA Instruments.

[0098] The acrylic resin may have a polar group, such as an epoxy group, a hydroxyl group, a carboxyl group, a nitrile group, or an amide group.

[0099] The acrylic resin may be a homopolymer of an acrylic acid ester monomer, a mixed component containing two or more of the above homopolymers, or a copolymer of two or more acrylic acid ester monomers, a component containing one or more copolymers. The acrylic resin may also be a mixed component of the above homopolymer and the above copolymer. The "acrylic acid" acrylic acid ester monomer also includes the concept of methacrylic acid. Specifically, the acrylic resin may be a mixture of a methacrylate polymer and an acrylate polymer, or an acrylic acid ester polymer such as acrylate-acrylate, methacrylate-methacrylate, or methacrylate-acrylate. Of these, it is preferable that the acrylic resin contain a copolymer of two or more acrylic acid ester monomers (a (meth)acrylic acid ester copolymer).

[0100] Examples of the monomer component constituting the (meth)acrylic acid ester copolymer include the monomer components described in JP 2014-065889 A. The monomer component may have the polar group described above. Examples of the (meth)acrylic acid ester copolymer include an ethyl acrylate-butyl acrylate-acrylonitrile copolymer, an ethyl acrylate-acrylonitrile copolymer, and a butyl acrylate-acrylonitrile copolymer. Note that "acrylic acid" such as methyl acrylate and ethyl acrylate also includes "methacrylic acid" such as methyl methacrylate and ethyl methacrylate.

[0101] The (meth)acrylic acid ester copolymer is preferably a block copolymer, and more preferably an acrylic block copolymer such as a methacrylate-acrylate copolymer. Examples of (meth)acrylates constituting the acrylic block copolymer include methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, cyclohexyl acrylate, and benzidyl acrylate. In these examples, "acrylic acid" also includes "methacrylic acid."

[0102] Specific examples of methacrylate-acrylate copolymers include acrylic copolymers such as methyl methacrylate-butyl acrylate-methyl methacrylate (MMA-BA-MMA) copolymer, which also includes block copolymers of polymethyl methacrylate-polybutyl acrylate-polymethyl methacrylate (PMMA-PBA-PMMA).

[0103] The acrylic copolymer may have no polar groups, or may be a modified product in which the above-mentioned polar groups have been partially introduced. Such modified products are more compatible with epoxy resins, thereby further improving adhesiveness.

[0104] Among these, the acrylic resin is preferably a (meth)acrylic acid ester copolymer having a first polymer portion having a glass transition temperature (Tg) of 10° C. or lower and a second polymer portion having a glass transition temperature (Tg) of 20° C. or higher. Such a (meth)acrylic acid ester copolymer has the first polymer portion that becomes a soft segment and the second polymer portion that becomes a hard segment.

[0105] The manifestation of the above-mentioned effect can be presumed as follows: By using an acrylic resin having both a soft segment and a hard segment, such as the above-mentioned (meth)acrylic acid ester copolymer, the hard segment contributes to heat resistance, and the soft segment contributes to toughness or flexibility, so that a first adhesive layer having good heat resistance, toughness, and flexibility can be obtained.

[0106] At least one of the first polymer portion and the second polymer portion contained in the (meth)acrylic acid ester copolymer has compatibility with epoxy resins. When the first polymer portion has compatibility with epoxy resins, flexibility can be increased. Furthermore, when the second polymer portion has compatibility with epoxy resins, cohesion and toughness can be increased.

[0107] When either the first polymer portion or the second polymer portion is incompatible with the epoxy resin, the (meth)acrylic acid ester copolymer has a compatible portion, which is a polymer portion that is compatible with the epoxy resin, and an incompatible portion, which is a polymer portion that is incompatible with the epoxy resin. In this case, when the (meth)acrylic acid ester copolymer is added to an adhesive composition, the compatible portion is compatible with the epoxy resin, and the incompatible portion is incompatible with the epoxy resin, causing fine phase separation. As a result, a fine sea-island structure is formed. The sea-island structure varies depending on the type of (meth)acrylic acid ester copolymer, the compatibility of the first polymer portion and the second polymer portion contained in the (meth)acrylic acid ester copolymer, and whether or not modification by introduction of polar groups has been performed, and examples include a sea-island structure in which the compatible portions of the cured epoxy resin and the (meth)acrylic acid ester copolymer are the sea and the incompatible portions of the (meth)acrylic acid ester copolymer are the islands, a sea-island structure in which the incompatible portions of the (meth)acrylic acid ester copolymer are the sea and the compatible portions of the cured epoxy resin and the (meth)acrylic acid ester copolymer are the islands, and a sea-island structure in which the (meth)acrylic acid ester copolymer is the sea and the cured epoxy resin is the islands. Having such a sea-island structure makes it easier to disperse stress, thereby preventing interfacial failure and achieving excellent adhesion after curing.

[0108] The (meth)acrylic acid ester copolymer is preferably a block copolymer, and particularly preferably an A-B-A block copolymer in which a compatible portion is polymer block A and an incompatible portion is polymer block B. Furthermore, an A-B-A block copolymer in which a first polymer portion is an incompatible portion and a second polymer portion is a compatible portion, with the first polymer portion being polymer block B and the second polymer portion being polymer block A, is preferred. By using such an A-B-A block copolymer as the acrylic resin, in a case where a sea-island structure is formed in which the compatible portion of the cured epoxy resin and the (meth)acrylic acid ester copolymer is a sea and the incompatible portion of the (meth)acrylic acid ester copolymer is an island, the island portions can be made smaller. Furthermore, in a case where a sea-island structure is formed in which the incompatible portion of the (meth)acrylic acid ester copolymer is a sea and the compatible portion of the cured epoxy resin and the (meth)acrylic acid ester copolymer is an island, or in a case where the (meth)acrylic acid ester copolymer is a sea and the cured epoxy resin is an island, the sea portions can be made smaller.

[0109] The (meth)acrylic acid ester copolymer may be a modified product in which the above-mentioned polar group is introduced into a part of the first polymer segment or the second polymer segment.

[0110] The Tg of the first polymer portion contained in the (meth)acrylic acid ester copolymer is 10°C or lower, and may be in the range of -150°C or higher and 10°C or lower, -130°C or higher and 0°C or lower, or -110°C or higher and -10°C or lower.

[0111] The Tg of the first polymer portion is calculated using the following formula based on the Tg(K) of each homopolymer described in "POLYMER HANDBOOK, Third Edition" (published by John Wiley & Sons, Inc.): 1 / Tg(K)=W 1 / Tg 1 +W 2 / Tg 2 +...+W n / Tg n W n : mass fraction of each monomer Tg n: Tg (K) of the homopolymer of each monomer, and publicly available values ​​such as those in the Polymer Handbook (3rd Ed., J. Brandrup and E. H. Immergut, Wiley Interscience) may be used. The same applies to the Tg of the second polymer portion described below.

[0112] The first polymer portion contained in the (meth)acrylic acid ester copolymer may be either a homopolymer or a copolymer, but is preferably a homopolymer. The monomer component and polymer component constituting the first polymer portion may be any monomer component and polymer component that can give a first polymer portion having a Tg within a predetermined range, and examples thereof include acrylate monomers such as butyl acrylate, 2-ethylhexyl acrylate, isononyl acrylate, and methyl acrylate, other monomers such as vinyl acetate, acetal, and urethane, polar group-containing monomers containing the above-mentioned polar groups, and copolymers such as EVA.

[0113] The Tg of the second polymer portion contained in the (meth)acrylic acid ester copolymer is 20°C or higher, and may be in the range of 20°C or higher and 150°C or lower, 30°C or higher and 150°C or lower, or 40°C or higher and 150°C or lower.

[0114] The second polymer portion contained in the (meth)acrylic acid ester copolymer may be either a homopolymer or a copolymer, but is preferably a homopolymer. The monomer component constituting the second polymer portion may be any monomer component capable of obtaining a second polymer portion having a Tg within a predetermined range, and examples thereof include acrylic acid ester monomers such as methyl methacrylate, other monomers such as acrylamide, styrene, vinyl chloride, amide, acrylonitrile, cellulose acetate, phenol, urethane, vinylidene chloride, methylene chloride, and methacrylonitrile, and polar group-containing monomers containing the above-mentioned polar groups.

[0115] A specific example of the (meth)acrylic acid ester copolymer having the first polymer portion and the second polymer portion is the above-mentioned MMA-BA-MMA copolymer.

[0116] The content of the acrylic resin, relative to 100 parts by mass of the resin component contained in the first adhesive layer, may be, for example, 1 part by mass or more, 3 parts by mass or more, 5 parts by mass or more, 7 parts by mass or more, or 10 parts by mass or more. If the content of the acrylic resin is too low, the adhesion of the first adhesive layer to the substrate and the adhesiveness after curing may be reduced. On the other hand, the content of the acrylic resin, relative to 100 parts by mass of the resin component contained in the first adhesive layer, may be, for example, 60 parts by mass or less, 50 parts by mass or less, 40 parts by mass or less, 35 parts by mass or less, or 30 parts by mass or less. If the content of the acrylic resin is too high, the contents of the first epoxy resin and the second epoxy resin may be relatively low, which may make it difficult to balance blocking resistance, adhesion of the first adhesive layer to the substrate, and adhesiveness after curing.

[0117] (iii) Curing Agent The curing agent in this embodiment is appropriately selected depending on the type of the first curing adhesive. When the first curing adhesive is, for example, an epoxy resin adhesive, a curing agent generally used in epoxy resin adhesives can be used as the curing agent. The curing agent is preferably solid at 23°C. A curing agent that is solid at 23°C can extend storage stability (pot life) compared to a curing agent that is liquid at 23°C. The curing agent may also be a latent curing agent. The curing agent may also be a curing agent that undergoes a curing reaction due to heat or a curing agent that undergoes a curing reaction due to light. The curing agents may be used alone or in combination of two or more types.

[0118] The reaction initiation temperature of the curing agent is, for example, 110°C or higher, and may be 130°C or higher. If the reaction initiation temperature is too low, the reaction will start early, and curing will occur with low flexibility and fluidity of the resin component, making it difficult to achieve uniform curing. On the other hand, the reaction initiation temperature of the curing agent is, for example, 200°C or lower. If the reaction initiation temperature is too high, the resin component may deteriorate. Note that when a highly heat-resistant resin such as a phenolic resin is used in addition to the epoxy resin, the resin component will deteriorate less, and the reaction initiation temperature of the curing agent may be, for example, 300°C or lower. The reaction initiation temperature of the curing agent is determined by differential scanning calorimetry (DSC).

[0119] Specific examples of the curing agent include imidazole-based curing agents, phenol-based curing agents, amine-based curing agents, acid anhydride-based curing agents, isocyanate-based curing agents, and thiol-based curing agents.

[0120] Examples of imidazole-based curing agents include imidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-isopropylimidazole, 2-phenylimidazole, carboxylic acid salts of imidazole compounds, and adducts with epoxy compounds. Furthermore, it is preferable that the imidazole-based curing agent has a hydroxyl group. Crystallization occurs due to hydrogen bonding between the hydroxy groups, so the reaction initiation temperature tends to be high.

[0121] Examples of phenolic curing agents include phenolic resins. Further, examples of phenolic resins include resol-type phenolic resins and novolac-type phenolic resins. From the viewpoint of adhesion of the first adhesive layer to the substrate, phenolic-type novolac resins having a Tg of 110°C or less are particularly preferred. Furthermore, phenolic curing agents and imidazole-type curing agents may be used in combination. In this case, it is preferable to use an imidazole-type curing agent as a curing catalyst.

[0122] In addition, although the heat resistance of the first adhesive layer can be improved by including a phenolic resin, there is a concern that the toughness may be reduced. Therefore, when the first adhesive layer includes a phenolic resin, it is preferable that an intermediate layer is disposed between the substrate and the first adhesive layer, as described below.

[0123] The phenolic resin is preferably a biphenyl type from the viewpoint of heat resistance. The phenolic resin may also be a resin in which the phenol nucleus is modified. By modifying the phenol nucleus, for example, it is possible to further improve heat resistance.

[0124] Examples of amine-based curing agents include aliphatic amines, aromatic amines, alicyclic amines, and polyamidoamines. Examples of aliphatic amines include diethylenetriamine (DETA), triethylenetetramine (TETA), and metaxylylenediamine (MXDA). Examples of aromatic amines include diaminodiphenylmethane (DDM), m-phenylenediamine (MPDA), and diaminodiphenylsulfone (DDS). In addition, examples of amine-based curing agents that can be used include dicyandiamide-based curing agents such as dicyandiamide (DICY), organic acid dihydrazide-based curing agents, amine adduct-based curing agents, and ketimine-based curing agents.

[0125] Examples of acid anhydride curing agents include alicyclic acid anhydrides (liquid acid anhydrides) and aromatic acid anhydrides. Examples of alicyclic acid anhydrides (liquid acid anhydrides) include hexahydrophthalic anhydride (HHPA) and methyltetrahydrophthalic anhydride (MTHPA). Examples of aromatic acid anhydrides include trimellitic anhydride (TMA), pyromellitic anhydride (PMDA), and benzophenonetetracarboxylic dianhydride (BTDA).

[0126] The isocyanate curing agent may, for example, be a blocked isocyanate.

[0127] Examples of thiol-based curing agents include ester-bonded thiol compounds, aliphatic ether-bonded thiol compounds, and aromatic ether-bonded thiol compounds.

[0128] The content of the curing agent is, for example, 1 part by mass or more and 40 parts by mass or less, based on 100 parts by mass of the resin component contained in the first adhesive layer. For example, when an imidazole-based curing agent is used as the main component of the curing agent, the content of the curing agent is preferably, for example, 1 part by mass or more and 15 parts by mass or less, based on 100 parts by mass of the resin component contained in the first adhesive layer. On the other hand, when a phenol-based curing agent is used as the main component of the curing agent, the content of the curing agent is preferably, for example, 5 parts by mass or more and 40 parts by mass or less, based on 100 parts by mass of the resin component contained in the first adhesive layer. Note that using an imidazole-based curing agent or a phenol-based curing agent as the main component of the curing agent means that the mass proportion of the imidazole-based curing agent or the phenol-based curing agent is the highest in the curing agent.

[0129] (b) Foaming Agent The first adhesive layer in this embodiment preferably contains a foaming agent. After the adhesive sheet is placed between two components, the first adhesive layer of the adhesive sheet is foamed and cured, thereby filling the gap between the two components and bonding them together.

[0130] The foaming agent in this embodiment may be a foaming agent generally used in the adhesive layer of an adhesive sheet. The foaming agent may be a foaming agent that undergoes a foaming reaction when exposed to heat or light.

[0131] The foaming initiation temperature of the foaming agent is preferably equal to or higher than the softening temperature of the base of the curable adhesive, such as an epoxy resin, and equal to or lower than the activation temperature of the curing reaction of the base of the curable adhesive, such as an epoxy resin. The foaming initiation temperature of the foaming agent is, for example, 70°C or higher, and may be 100°C or higher. If the foaming initiation temperature is too low, the reaction may start early, causing foaming to occur in a state where the flexibility and fluidity of the resin component are low, making it difficult to achieve uniform foaming. On the other hand, the foaming initiation temperature of the foaming agent is, for example, 210°C or lower. If the foaming initiation temperature is too high, the resin component may deteriorate.

[0132] The softening temperature of the base resin of the curable adhesive such as epoxy resin is measured by the ring and ball method specified in JIS K7234:1986.

[0133] Examples of the blowing agent include organic blowing agents and inorganic blowing agents. Examples of the organic blowing agent include azo blowing agents such as azodicarbonamide (ADCA), azobisformamide, and azobisisobutyronitrile, fluorinated alkane blowing agents such as trichloromonofluoromethane, hydrazine blowing agents such as paratoluenesulfonylhydrazide, semicarbazide blowing agents such as p-toluenesulfonylsemicarbazide, triazole blowing agents such as 5-morpholyl-1,2,3,4-thiatriazole, and N-nitroso blowing agents such as N,N-dinitrosoterephthalamide. On the other hand, examples of the inorganic blowing agent include ammonium carbonate, ammonium bicarbonate, ammonium nitrite, ammonium borohydride, and azides.

[0134] Alternatively, a microcapsule type foaming agent may be used as the foaming agent. The microcapsule type foaming agent preferably has a core made of a thermal expansion agent such as hydrocarbon and a shell made of a resin such as acrylonitrile copolymer.

[0135] The average particle size of the foaming agent may be, for example, 7 μm or more, 10 μm or more, 13 μm or more, or 17 μm or more. On the other hand, the average particle size of the foaming agent is preferably equal to or less than the average thickness of the first adhesive layer, and may be, for example, 24 μm or less.

[0136] The average particle size of the foaming agent is the particle size at 50% of the cumulative value in the particle size distribution determined by laser diffraction scattering. To measure the average particle size of the foaming agent, the first adhesive layer is dissolved in a solvent to separate the foaming agent. The solvent is not particularly limited as long as it can dissolve components other than the foaming agent contained in the first adhesive layer. It is appropriately selected depending on the type of curable adhesive contained in the first adhesive layer. For example, a solvent used in the adhesive composition used to form the first adhesive layer can be used. Specifically, methyl ethyl ketone, ethyl acetate, toluene, etc. can be used.

[0137] The content of the foaming agent is, for example, 0.5 parts by mass or more, 2 parts by mass or more, 3 parts by mass or more, 4 parts by mass or more, or 5 parts by mass or more, relative to 100 parts by mass of the resin component contained in the first adhesive layer. On the other hand, the content of the foaming agent is, for example, 25 parts by mass or less, 20 parts by mass or less, or 15 parts by mass or less, relative to 100 parts by mass of the resin component contained in the first adhesive layer. If the content of the foaming agent is too low, the expansion ratio of the first adhesive layer may be small, and the adhesiveness may be reduced. On the other hand, if the content of the foaming agent is too high, the content of the curable adhesive may be relatively small, which may result in a decrease in cohesive strength and a decrease in adhesiveness.

[0138] (c) Other Components In the present embodiment, when the first curable adhesive is an epoxy resin adhesive, the first adhesive layer may contain only an epoxy resin and an acrylic resin as resin components, or may further contain other resins, such as urethane resins.

[0139] The total ratio of the first epoxy resin, the second epoxy resin and the acrylic resin to the resin components contained in the first adhesive layer is, for example, 70% by mass or more, or may be 80% by mass or more, or 90% by mass or more, or may be 100% by mass.

[0140] The content of the resin component contained in the first adhesive layer is, for example, 60% by mass or more, or may be 70% by mass or more, or 80% by mass or more, or may be 90% by mass or more.

[0141] The first adhesive layer may contain, as needed, for example, a silane coupling agent, a filler, an antioxidant, a light stabilizer, an ultraviolet absorber, a lubricant, a plasticizer, an antistatic agent, a crosslinking agent, and a colorant. Examples of the silane coupling agent include epoxy-based silane coupling agents. Examples of the filler include inorganic fillers such as calcium carbonate, aluminum hydroxide, magnesium hydroxide, antimony trioxide, zinc borate, molybdenum compounds, and titanium dioxide. Examples of the antioxidant include phenol-based antioxidants and sulfur-based antioxidants.

[0142] (3) Configuration of the First Adhesive Layer The thickness of the first adhesive layer is not particularly limited. In particular, when the first adhesive layer contains a foaming agent, the thickness of the first adhesive layer is preferably equal to or greater than the average particle size of the foaming agent. The average thickness of the first adhesive layer is, for example, 10 μm or more, or may be 15 μm or more, or may be 20 μm or more. If the first adhesive layer is too thin, it may be difficult to obtain sufficient adhesion to the substrate and adhesion after curing. On the other hand, the average thickness of the first adhesive layer is, for example, 200 μm or less, or may be 150 μm or less, or may be 100 μm or less. If the first adhesive layer is too thick, the surface quality may be deteriorated.

[0143] Here, the average thickness of the first adhesive layer is a value measured from a cross section of the adhesive sheet in the thickness direction observed with a transmission electron microscope (TEM), a scanning electron microscope (SEM), or a scanning transmission electron microscope (STEM), and is the average value of thicknesses at 10 randomly selected locations. The same applies to the method for measuring the average thickness of other layers of the adhesive sheet.

[0144] The first adhesive layer may be a continuous layer or a discontinuous layer. Examples of discontinuous layers include stripes and dots. The surface of the first adhesive layer may have an uneven shape such as an embossed shape.

[0145] The method for forming the first adhesive layer will be described later in "B. Method for manufacturing adhesive sheet," and therefore, description thereof will be omitted here.

[0146] 2. Substrate The substrate in this embodiment is, for example, a member that supports the first adhesive layer.

[0147] The substrate in this embodiment preferably has insulating properties. The substrate is preferably in the form of a sheet. The substrate may have a single-layer structure or a multi-layer structure. The substrate may or may not have a porous structure inside.

[0148] Examples of the substrate include a resin substrate and a nonwoven fabric.

[0149] Examples of resins contained in the resin substrate include polyester resin, polycarbonate, polyarylate, polyurethane, polyamide resin, polyimide resin, polysulfone resin, polyether ketone resin, polyphenylene sulfide (PPS), modified polyphenylene oxide, etc. Examples of polyester resins include polyethylene terephthalate (PET), polybutylene terephthalate, polyethylene naphthalate (PEN), and aromatic polyester. Examples of polyamide resins include polyamide and polyether amide. Examples of polyimide resins include polyimide, polyether imide, and polyamide imide. Examples of polysulfonic acid resins include polysulfone and polyether sulfone. Examples of polyether ketone resins include polyether ketone and polyether ether ketone. Furthermore, liquid crystal polymers (LCPs) may also be used as the resin.

[0150] The glass transition temperature of the resin is, for example, 80° C. or higher, or may be 140° C. or higher, or may be 200° C. or higher.

[0151] Examples of nonwoven fabrics include nonwoven fabrics containing fibers such as cellulose fibers, polyester fibers, nylon fibers, aramid fibers, polyphenylene sulfide fibers, liquid crystal polymer fibers, glass fibers, metal fibers, and carbon fibers.

[0152] The substrate may be subjected to a surface treatment on the surface on which the first adhesive layer is to be disposed in order to enhance adhesion to the first adhesive layer.

[0153] The average thickness of the substrate is not particularly limited, but may be, for example, 2 μm or more, 5 μm or more, or 9 μm or more, and may be, for example, 200 μm or less, 100 μm or less, or 50 μm or less.

[0154] 3. First Intermediate Layer The adhesive sheet in this embodiment may have a first intermediate layer between the substrate and the first adhesive layer. The presence of the first intermediate layer can improve the adhesion of the first adhesive layer to the substrate. Furthermore, the presence of the first intermediate layer can, for example, alleviate stress at the bent portion when the adhesive sheet is folded, or at the cut portion when the adhesive sheet is cut. As a result, lifting or peeling of the first adhesive layer from the substrate can be suppressed when the adhesive sheet is bent or cut.

[0155] For example, in an adhesive sheet 10A shown in FIG. 5, a substrate 1, a first intermediate layer 5, and a first adhesive layer 2 are arranged in this order in the thickness direction.

[0156] The material contained in the first intermediate layer is not particularly limited as long as it can increase the adhesion between the substrate and the first adhesive layer and relieve stress, and is appropriately selected depending on the materials of the substrate and the adhesive layer, etc. Examples include polyester, polyvinyl chloride, polyvinyl acetate, polyurethane, polymers obtained by copolymerizing at least two or more of these, crosslinked products thereof, and mixtures thereof.

[0157] The crosslinked product is a crosslinked product obtained by crosslinking the above-mentioned resin with a curing agent. Examples of the curing agent include an isocyanate-based curing agent. Furthermore, for example, when the reactive group / NCO equivalent is 1, it is preferable to add the isocyanate-based curing agent in a ratio of 0.5 mass % to 20 mass % relative to the resin.

[0158] In particular, the first intermediate layer preferably contains a crosslinked resin. A crosslinked resin refers to a resin that does not melt even at high temperatures. This improves adhesive strength at high temperatures, i.e., heat resistance. Furthermore, if the crosslinked resin is crosslinked with, for example, an isocyanate-based curing agent, the flexibility of the first intermediate layer is improved, and cracking of the first adhesive layer and lifting and peeling of the adhesive layer from the substrate when the adhesive sheet is bent can be suppressed.

[0159] The average thickness of the first intermediate layer is not particularly limited and may be, for example, 0.1 μm or more, 0.5 μm or more, or even 1 μm or more. If the first intermediate layer is too thin, the effect of suppressing peeling of the first adhesive layer from the substrate when the adhesive sheet is bent or cut may not be sufficiently obtained. On the other hand, the average thickness of the first intermediate layer may be, for example, 4 μm or less, or 3.5 μm or less. Since the first intermediate layer itself usually does not have high heat resistance, if the first intermediate layer is too thick, heat resistance (adhesive strength at high temperatures) may be reduced.

[0160] The first intermediate layer can be formed, for example, by applying a resin composition and removing the solvent. Examples of the application method include roll coating, reverse roll coating, transfer roll coating, gravure coating, gravure reverse coating, comma coating, rod coating, blade coating, bar coating, wire bar coating, die coating, lip coating, and dip coating.

[0161] 4. Adhesive Sheet The adhesive sheet of this embodiment does not have another adhesive layer on the other side of the substrate. In the adhesive sheet of this embodiment, it is preferable that a first adhesive layer is disposed on one outermost surface and a substrate is disposed on the other outermost surface. When the adhesive sheet is wound into a roll, blocking caused by contact between the first adhesive layer and the substrate can be suppressed.

[0162] The adhesive sheet in this embodiment has an average thickness of, for example, 10 μm or more, and may have an average thickness of 20 μm or more, while the adhesive sheet has an average thickness of, for example, 1000 μm or less, and may have an average thickness of 200 μm or less.

[0163] The adhesive sheet in this embodiment preferably has good shape retention. The bending moment based on JIS P8125-2:2017, which corresponds to ISO 2493-2, is, for example, 3 gf·cm or more, and may be 5 gf·cm or more. On the other hand, the bending moment may be, for example, less than 40 gf·cm, and may be less than 30 gf·cm. Conventionally, adhesive sheets generally have a high bending moment to improve their shape retention and ease of insertion into narrow gaps. In contrast, the inventors of the present disclosure have discovered that shape retention can be ensured by modifying the shape, and that a high bending moment has other drawbacks, so that in consideration of other characteristics, it is preferable that the bending moment be within the above range. If the bending moment is smaller than the above range, it may be difficult to maintain the shape even with measures such as folding. Furthermore, if the bending moment is larger than the above range, the shape will return to its original state after folding, making it necessary to heat the sheet or create a crease in the fold during folding. Heating reduces the sheet life, and striations can reduce the insulation properties of that area.

[0164] The adhesive sheet in this embodiment preferably has high adhesiveness after curing. The shear adhesive strength based on JIS K6850:1999, which corresponds to ISO 4587, may be, for example, 2.10 MPa or more, 2.40 MPa or more, or 3.0 MPa or more at 23°C. Furthermore, the shear adhesive strength may be, for example, 0.27 MPa or more, 0.55 MPa or more, or 0.58 MPa or more at 200°C. For example, a high-strength acrylic foam adhesive tape that does not require heating has a shear adhesive strength of approximately 1 MPa or more and 2 MPa or less at room temperature, and does not have heat resistance at 200°C. Therefore, if the shear adhesive strength is within the above range at 23°C, it has advantages in terms of strength. Furthermore, if the shear adhesive strength is within the above range at 200°C, it can be used in applications requiring heat resistance around automobile engines or similar.

[0165] The adhesive sheet of this embodiment preferably has high electrical insulation after curing. The breakdown voltage based on JIS C2107:2011, which corresponds to IEC 60454-2, is preferably, for example, 3 kV or higher, more preferably 5 kV or higher. Having the breakdown voltage within the above range enables application for rust prevention and around copper wires. Furthermore, the adhesive sheet after curing preferably has a thermal conductivity of, for example, 0.1 W / mK or higher, more preferably 0.15 W / mK or higher. Having the thermal conductivity within the above range allows for miniaturization of components and promotes the curing reaction during heating.

[0166] The use of the adhesive sheet in this embodiment is not particularly limited. For example, the adhesive sheet in this embodiment can be used when two members are bonded together by placing the adhesive sheet between them and then curing the adhesive sheet.

[0167] The method for producing the adhesive sheet in this embodiment is not particularly limited, and will be described in the section "B. Method for producing adhesive sheet" below.

[0168] II. Second Embodiment of Adhesive Sheet A second embodiment of an adhesive sheet in the present disclosure includes a substrate, a first adhesive layer disposed on one side of the substrate and containing a first curable adhesive, and a second adhesive layer disposed on the other side of the substrate and containing a second curable adhesive, wherein the tack of the first adhesive layer and the second adhesive layer is less than 0.1 N, and the Martens hardness of the first adhesive layer and the second adhesive layer is 20 N / mm 2 130N / mm or more 2 The following is the result.

[0169] Each component of the adhesive sheet of this embodiment will be described below.

[0170] 1. First Adhesive Layer and Second Adhesive Layer The physical properties, material, thickness, and formation method of the first adhesive layer in this embodiment are the same as those of the first adhesive layer in the first embodiment described above. Furthermore, the physical properties, material, thickness, and formation method of the second adhesive layer in this embodiment are the same as those of the first adhesive layer in the first embodiment described above.

[0171] When measuring the Martens hardness of the first adhesive layer, the second adhesive layer is removed from the adhesive sheet, and then the Martens hardness of the first adhesive layer is measured. On the other hand, when measuring the Martens hardness of the second adhesive layer, the first adhesive layer is removed from the adhesive sheet, and then the Martens hardness of the second adhesive layer is measured. Methods for removing the first adhesive layer or the second adhesive layer include, for example, wiping with a solvent and scraping. When wiping with a solvent, the solvent is not particularly limited as long as it dissolves the first adhesive layer or the second adhesive layer but does not dissolve the substrate. For example, a solvent contained in the adhesive composition used to form the adhesive layer can be used.

[0172] In this embodiment, it is preferable that at least one of the first adhesive layer and the second adhesive layer contains a foaming agent. After placing the adhesive sheet between two components, the first adhesive layer of the adhesive sheet is foamed and cured to fill and bond the space between the two components. In this case, only the first adhesive layer may contain a foaming agent, only the second adhesive layer may contain a foaming agent, or both the first adhesive layer and the second adhesive layer may contain a foaming agent. In particular, it is preferable that both the first adhesive layer and the second adhesive layer contain a foaming agent. This can improve adhesion after foaming and curing.

[0173] 2. Substrate The substrate in this embodiment is a member that supports the first adhesive layer and the second adhesive layer. The substrate is the same as the substrate in the first embodiment.

[0174] 3. First Intermediate Layer and Second Intermediate Layer The adhesive sheet in this embodiment may have a first intermediate layer between the substrate and the first adhesive layer. Also, the adhesive sheet in this embodiment may have a second intermediate layer between the substrate and the second adhesive layer.

[0175] For example, in adhesive sheet 10B shown in Fig. 6, a first adhesive layer 2 is disposed on one side of substrate 1, a second adhesive layer 3 is disposed on the other side of substrate 1, a first intermediate layer 5 is disposed between substrate 1 and first adhesive layer 2, and a second intermediate layer 6 is disposed between substrate 1 and second adhesive layer 3. Although adhesive sheet 10B in Fig. 6 has both first intermediate layer 5 and second intermediate layer 6, it may have only one of them.

[0176] It is sufficient that an intermediate layer is disposed between the substrate and at least one of the adhesive layers, and for example, an intermediate layer may be disposed between only the substrate and one of the adhesive layers, or an intermediate layer may be disposed between the substrate and both of the adhesive layers, and it is particularly preferable that an intermediate layer is disposed between the substrate and both of the adhesive layers.

[0177] The material, thickness and forming method of the first intermediate layer and the second intermediate layer are the same as the material, thickness and forming method of the first intermediate layer in the first embodiment described above.

[0178] 4. Adhesive Sheet In the adhesive sheet of this embodiment, it is preferable that a first adhesive layer is disposed on one outermost surface and a second adhesive layer is disposed on the other outermost surface, which can prevent blocking caused by contact between the first adhesive layer and the second adhesive layer when the adhesive sheet is wound into a roll.

[0179] The thickness, physical properties, uses, and manufacturing method of the adhesive sheet are the same as those of the adhesive sheet of the first embodiment described above.

[0180] III. Third Embodiment of Adhesive Sheet A third embodiment of an adhesive sheet in the present disclosure includes a substrate, a first adhesive layer disposed on one side of the substrate and containing a first curable adhesive, a second adhesive layer disposed on the other side of the substrate and containing a second curable adhesive, and a separator disposed on the side of the second adhesive layer opposite the substrate, wherein the tack of the first adhesive layer is less than 0.1 N, the tack of the second adhesive layer is 0.1 N or more, and the Martens hardness of the first adhesive layer is 20 N / mm 2 130N / mm or more 2 The following is the result.

[0181] Each component of the adhesive sheet of this embodiment will be described below.

[0182] 1. First Adhesive Layer The physical properties, material, thickness, and formation method of the first adhesive layer in this embodiment are the same as those of the first adhesive layer in the first embodiment described above.

[0183] When measuring the Martens hardness of the first adhesive layer, the Martens hardness of the first adhesive layer is measured after removing the second adhesive layer from the adhesive sheet. The method for removing the second adhesive layer is the same as that described in the second embodiment above.

[0184] 2. Second Adhesive Layer The second adhesive layer in this embodiment is disposed on the other surface side of the substrate, and the tackiness of the second adhesive layer is equal to or greater than a predetermined value.

[0185] (1) Physical Properties of the Second Adhesive Layer In this embodiment, the tackiness of the second adhesive layer is 0.1 N or more, or may be 0.3 N or more, or may be 0.5 N or more. By having the tackiness of the second adhesive layer in the above range, the adhesion of the second adhesive layer to the member can be improved. Furthermore, the tackiness of the second adhesive layer is, for example, 10 N or less, or may be 5 N or less, or may be 3 N or less. If the tackiness of the second adhesive layer is too high, reworkability may be reduced, and it may be difficult to correct misalignment of the adhesive sheet when attaching the second adhesive layer surface of the adhesive sheet to one of the members.

[0186] Here, the method for measuring the tackiness of the second adhesive layer is the same as the method for measuring the tackiness of the first adhesive layer.

[0187] In this embodiment, an example of a method for controlling the tackiness of the second adhesive layer is to adjust the composition of the second adhesive layer. Specifically, when an epoxy resin that is liquid at room temperature or a curing agent that is liquid at room temperature is used in a second adhesive layer containing an epoxy resin and a curing agent, the tackiness of the second adhesive layer tends to be high. Furthermore, when an epoxy resin with a low softening temperature or an epoxy resin with a low weight-average molecular weight is used in a second adhesive layer containing an epoxy resin and a curing agent, the tackiness of the second adhesive layer tends to be high. Furthermore, adding a tackifier to the second adhesive layer tends to increase the tackiness of the second adhesive layer. Note that using a curing agent that is liquid at room temperature tends to increase the tackiness, but may result in reduced storage stability. Therefore, it is preferable to adjust the tackiness of the second adhesive layer by adjusting the properties and type of components other than the curing agent, such as the epoxy resin.

[0188] (2) Material for the Second Adhesive Layer The second adhesive layer in this embodiment contains a second curable adhesive.

[0189] (a) Second Curable Adhesive The second curable adhesive contained in the second adhesive layer in this embodiment is the same as the first curable adhesive used in the first adhesive layer in the first embodiment described above. In particular, the second curable adhesive is preferably an epoxy resin adhesive.

[0190] Hereinafter, an example in which the second curable adhesive is an epoxy resin adhesive will be described.

[0191] (i) Epoxy Resin The epoxy resin in this embodiment is the same as the epoxy resin used in the first adhesive layer in the first embodiment described above.

[0192] As the epoxy resin, an epoxy resin generally used for the adhesive layer of an adhesive sheet can be used.

[0193] Examples of the epoxy resin include aromatic epoxy resins, aliphatic epoxy resins, alicyclic epoxy resins, and heterocyclic epoxy resins. Specific examples of the epoxy resin are the same as the specific examples of the first epoxy resin used in the first adhesive layer in the first embodiment described above.

[0194] The epoxy resin may be a monofunctional epoxy resin, a difunctional epoxy resin, a trifunctional epoxy resin, or a tetrafunctional or higher functional epoxy resin.

[0195] Among these, it is preferable to use, as the epoxy resin, an epoxy resin that is liquid at room temperature, such as a bisphenol A type epoxy resin or a bisphenol F type epoxy resin, or an epoxy resin with a low softening point, because by using these epoxy resins, it is easy to adjust the tackiness of the second adhesive layer within a predetermined range.

[0196] (ii) Acrylic Resin When the second curable adhesive is an epoxy resin adhesive, the second adhesive layer may further contain an acrylic resin that is compatible with the epoxy resin. This can improve film-forming properties.

[0197] The acrylic resin is the same as the acrylic resin used in the first adhesive layer in the first embodiment described above.

[0198] (iii) Curing agent The curing agent is the same as the curing agent used in the first adhesive layer in the first embodiment described above. Furthermore, as the curing agent, a curing agent that is solid at room temperature or a curing agent that is liquid at room temperature can be used. Among these, a curing agent that is solid at room temperature is preferred from the viewpoint of storage stability.

[0199] (b) Foaming Agent In this embodiment, it is preferable that at least one of the first adhesive layer and the second adhesive layer contains a foaming agent. After placing the adhesive sheet between two components, the first adhesive layer of the adhesive sheet is foamed and cured to fill and bond the space between the two components. In this case, only the first adhesive layer may contain a foaming agent, only the second adhesive layer may contain a foaming agent, or both the first adhesive layer and the second adhesive layer may contain a foaming agent. In particular, it is preferable that both the first adhesive layer and the second adhesive layer contain a foaming agent. This can improve adhesion after foaming and curing.

[0200] The foaming agent is the same as the foaming agent used in the first adhesive layer in the first embodiment described above.

[0201] (c) Other Components In the present embodiment, when the second curable adhesive is an epoxy resin adhesive, the second adhesive layer may contain only an epoxy resin and an acrylic resin as resin components, or may further contain other resins, such as urethane resins.

[0202] The total ratio of epoxy resin and acrylic resin to the resin components contained in the second adhesive layer is, for example, 70% by mass or more, or may be 80% by mass or more, or 90% by mass or more, or may be 100% by mass.

[0203] The content of the resin component contained in the second adhesive layer is, for example, 60% by mass or more, or may be 70% by mass or more, or 80% by mass or more, or may be 90% by mass or more.

[0204] The second adhesive layer may contain additives as needed, which may be the same as the additives used in the first adhesive layer in the first embodiment.

[0205] (3) Configuration of the Second Adhesive Layer When the second adhesive layer further contains a foaming agent, the expansion ratio is the same as the expansion ratio of the first adhesive layer in the first embodiment described above.

[0206] The average thickness of the second adhesive layer is the same as the average thickness of the first adhesive layer in the first embodiment described above.

[0207] The second adhesive layer may be a continuous layer or a discontinuous layer. The surface of the second adhesive layer may have an uneven shape such as an embossed shape.

[0208] The method for forming the second adhesive layer is the same as the method for forming the first adhesive layer in the first embodiment described above.

[0209] 3. Substrate The substrate in this embodiment is a member that supports the first adhesive layer and the second adhesive layer. The substrate is the same as the substrate in the first embodiment.

[0210] 4. Separator The separator in this embodiment is disposed on the surface of the second adhesive layer opposite to the substrate.

[0211] The separator is not particularly limited as long as it can be peeled from the second adhesive layer, and it can have a strength sufficient to protect the second adhesive layer. Examples of such separators include release films and release papers. The separator may have a single-layer structure or a multi-layer structure.

[0212] An example of a separator having a single layer structure is a fluororesin film.

[0213] Further, examples of multilayer separators include laminates having a release layer on one or both sides of a substrate layer. Examples of substrate layers include resin films such as polypropylene, polyethylene, and polyethylene terephthalate, as well as paper such as fine paper, coated paper, and impregnated paper. The material for the release layer is not particularly limited as long as it has releasability, and examples include silicone compounds, organic compound-modified silicone compounds, fluorine compounds, aminoalkyd compounds, melamine compounds, acrylic compounds, polyester compounds, and long-chain alkyl compounds. These compounds can be emulsion-type, solvent-type, or solventless.

[0214] 5. First Intermediate Layer and Second Intermediate Layer The adhesive sheet in this embodiment may have a first intermediate layer between the substrate and the first adhesive layer. Also, the adhesive sheet in this embodiment may have a second intermediate layer between the substrate and the second adhesive layer.

[0215] For example, in adhesive sheet 10C shown in Fig. 7, a first intermediate layer 5 is disposed between substrate 1 and first adhesive layer 2, and a second intermediate layer 6 is disposed between substrate 1 and second adhesive layer 3. Note that, although adhesive sheet 10B in Fig. 7 has both first intermediate layer 5 and second intermediate layer 6, it may have only one of them.

[0216] It is sufficient that an intermediate layer is disposed between the substrate and at least one of the adhesive layers, and for example, an intermediate layer may be disposed between only the substrate and one of the adhesive layers, or an intermediate layer may be disposed between the substrate and both of the adhesive layers, and it is particularly preferable that an intermediate layer is disposed between the substrate and both of the adhesive layers.

[0217] The material, thickness and forming method of the first intermediate layer and the second intermediate layer are the same as the material, thickness and forming method of the first intermediate layer in the first embodiment described above.

[0218] 6. Adhesive Sheet In the adhesive sheet of this embodiment, it is preferable that a first adhesive layer is disposed on one outermost surface and a separator is disposed on the other outermost surface, which can prevent blocking caused by contact between the first adhesive layer and the separator when the adhesive sheet is wound into a roll.

[0219] The thickness, physical properties, uses, and manufacturing method of the adhesive sheet are the same as those of the adhesive sheet of the first embodiment described above.

[0220] B. Manufacturing Method of Adhesive Sheet The inventors of the present disclosure conducted extensive research into a manufacturing method of an adhesive sheet having an adhesive layer on one or both sides of a substrate. First, as described in the above section "A. Adhesive Sheet," for example, hardening the adhesive layer is effective in improving the slipperiness and blocking resistance of the adhesive layer. However, if the adhesive layer is too hard, it tends to crack, lift, or peel when the adhesive sheet is wound or folded. Next, in the adhesive sheet, the adhesive layer can be formed, for example, by applying an adhesive composition to a substrate and drying it. In this case, if the drying temperature is low, blocking of the adhesive layer may not be suppressed. Furthermore, the drying temperature must be lower than the curing temperature of the adhesive layer. Furthermore, if the adhesive layer contains a foaming agent, the drying temperature must be lower than the foaming initiation temperature or decomposition temperature of the foaming agent. Therefore, the drying temperature cannot be too high. Therefore, it is important to optimize the drying temperature. However, it was found that even when the drying temperature and drying time are set to a predetermined temperature and time, blocking of the adhesive layer may or may not occur depending on the coating and drying device used. The inventors of the present disclosure conducted extensive research and found that blocking of the adhesive layer can be suppressed by setting the drying conditions using the hardness of the adhesive layer as an indicator. They also found that by setting the tack of the adhesive layer within a predetermined range and drying the adhesive composition so that the Martens hardness of the adhesive layer falls within a predetermined range during formation of the adhesive layer, it is possible to achieve a good balance between improving the slip properties and blocking resistance of the adhesive layer and suppressing cracking, lifting, and peeling of the adhesive layer during winding and bending. The present disclosure is based on this finding.

[0221] A method for producing an adhesive sheet according to the present disclosure includes a first adhesive layer forming step of applying a first adhesive composition containing a first curable adhesive to one side of a substrate and drying the applied composition to form a first adhesive layer, wherein the tack of the first adhesive layer is less than 0.1 N, and in the first adhesive layer forming step, the Martens hardness of the first adhesive layer is 20 N / mm 2 130N / mm or more 2 The first adhesive composition is dried as follows:

[0222] 8(a) and 8(b) are process diagrams illustrating an example method for producing an adhesive sheet according to the present disclosure. First, as shown in FIG. 8(a), a first adhesive composition 2a containing a first curable adhesive is applied to one side of a substrate 1 and then dried. This forms a first adhesive layer 2 as shown in FIG. 8(b).

[0223] In the present disclosure, by drying the first adhesive composition in the first adhesive layer formation process so that the tack of the first adhesive layer is less than a predetermined value and the Martens hardness of the first adhesive layer is within a predetermined range, it is possible to achieve a good balance between improving the slip properties and blocking resistance of the first adhesive layer and suppressing cracking, lifting, and peeling of the first adhesive layer when it is wound up and folded.

[0224] In this manner, in the present disclosure, by using the Martens hardness of the first adhesive layer as an indicator of drying conditions and optimizing the drying conditions, it is possible to simultaneously improve blocking resistance and suppress cracking, lifting, and peeling of the first adhesive layer during winding and bending, thereby improving blocking resistance regardless of the coating and drying device used.

[0225] Furthermore, an adhesive sheet produced by the adhesive sheet production method according to the present disclosure exhibits the same effects as the adhesive sheet described above.

[0226] Each step in the method for producing an adhesive sheet according to the present disclosure will be described below.

[0227] 1. First adhesive layer forming step In the first adhesive layer forming step of the present disclosure, a first adhesive composition containing a first curable adhesive is applied to one side of a substrate and dried to form a first adhesive layer. In the first adhesive layer forming step, a first adhesive layer having a Martens hardness of 20 N / mm 2 130N / mm or more 2 The first adhesive composition is dried as follows:

[0228] The first adhesive composition contains a first curable adhesive. The first adhesive composition may also contain a foaming agent. The components contained in the first adhesive composition are the same as the components contained in the first adhesive layer of the adhesive sheet described above.

[0229] The first adhesive composition may or may not contain a solvent. In this specification, the term "solvent" is used in a broad sense to include not only a strict solvent (a solvent that dissolves a solute) but also a dispersion medium. The solvent contained in the first adhesive composition is volatilized and removed when the first adhesive composition is dried.

[0230] The first adhesive composition can be obtained by mixing the components and, if necessary, kneading and dispersing them. As a mixing and dispersing method, a general kneading disperser, such as a two-roll mill, a three-roll mill, a pebble mill, a tron ​​mill, a Szegvari attritor, a high-speed impeller disperser, a high-speed stone mill, a high-speed impact mill, a desper, a high-speed mixer, a ribbon blender, a co-kneader, an intensive mixer, a tumbler, a blender, a desperzer, a homogenizer, or an ultrasonic disperser, can be used.

[0231] Examples of methods for applying the first adhesive composition include roll coating, reverse roll coating, transfer roll coating, gravure coating, gravure reverse coating, comma coating, rod coating, blade coating, bar coating, wire bar coating, die coating, lip coating, and dip coating.

[0232] The method for drying the applied first adhesive composition is not particularly limited as long as it is a method that can dry the first adhesive composition so that the Martens hardness of the first adhesive layer falls within a predetermined range, and examples thereof include heat drying.

[0233] In this step, the Martens hardness of the first adhesive layer is 20 N / mm 2 130N / mm or more 2 The first adhesive composition is dried so that the Martens hardness of the first adhesive layer is the same as the Martens hardness of the first adhesive layer in the adhesive sheet described above.

[0234] Drying conditions that affect the Martens hardness of the first adhesive layer include, for example, the drying temperature, thermal history, and air velocity. Examples of thermal history include the heating rate and the total amount of heat. For example, as the drying temperature increases, the Martens hardness of the first adhesive layer tends to increase. On the other hand, as the drying temperature decreases, the Martens hardness of the first adhesive layer tends to decrease. For example, as the heating rate increases, the total amount of heat increases for a constant drying time, and the Martens hardness of the first adhesive layer tends to increase. On the other hand, as the heating rate decreases, the total amount of heat decreases for a constant drying time, and the Martens hardness of the first adhesive layer tends to decrease. For example, as the total amount of heat received by the first adhesive layer increases, the Martens hardness of the first adhesive layer tends to increase. On the other hand, as the total amount of heat received by the first adhesive layer decreases, the Martens hardness of the first adhesive layer tends to decrease. For example, as the air velocity increases, the drying rate increases, and the Martens hardness of the first adhesive layer tends to increase. On the other hand, when the wind speed is slow, the drying speed is slowed, and the Martens hardness of the first adhesive layer tends to be small.

[0235] The drying conditions are appropriately set so that the Martens hardness of the first adhesive layer falls within a predetermined range. The drying temperature is, for example, 80°C or higher, or may be 85°C or higher, or 90°C or higher. The drying temperature is, for example, 130°C or lower, or may be 120°C or lower, or may be 110°C or lower. Specifically, the drying temperature is 80°C or higher and 130°C or lower, or may be 85°C or higher and 120°C or lower, or may be 90°C or higher and 110°C or lower. The drying time is, for example, 1 minute or longer, or may be 1 minute 30 seconds or longer, or may be 2 minutes or longer. The drying time is, for example, 15 minutes or shorter, or may be 10 minutes or shorter, or may be 8 minutes or shorter. Specifically, the drying time is 1 minute or longer and 15 minutes or shorter, or may be 1 minute 30 seconds or longer and 10 minutes or shorter, or may be 2 minutes or longer and 8 minutes or shorter. The temperature rise rate is, for example, 0.2°C / second or higher, or may be 0.5°C / second or higher, or may be 0.8°C / second or higher. The temperature rise rate is, for example, 5.0°C / sec or less, or may be 4.0°C / sec or less, or may be 3.0°C / sec or less. Specifically, the temperature rise rate is 0.2°C / sec or more and 5.0°C / sec or less, or 0.5°C / sec or more and 4.0°C / sec or less, or may be 0.8°C / sec or more and 3.0°C / sec or less. The wind speed is, for example, 1 m / sec or more, or may be 3 m / sec or more, or may be 5 m / sec or more. The wind speed is, for example, 20 m / sec or less, or may be 18 m / sec or less, or may be 15 m / sec or less. Specifically, the wind speed is 1 m / sec or more and 20 m / sec or less, or may be 3 m / sec or more and 18 m / sec or less, or may be 5 m / sec or more and 15 m / sec or less.

[0236] The tackiness of the first adhesive layer is less than a predetermined value, which is the same as the tackiness of the first adhesive layer in the adhesive sheet described above.

[0237] 2. Second Adhesive Layer Forming Step The method for producing an adhesive sheet according to the present disclosure may include a second adhesive layer forming step of applying a second adhesive composition containing a second curable adhesive to the other surface of the substrate or one surface of the separator, and drying the composition to form a second adhesive layer.

[0238] When producing the adhesive sheet of the second embodiment described above, in the second adhesive layer forming step, the Martens hardness of the second adhesive layer is 20 N / mm 2 130N / mm or more 2 The second adhesive composition is dried as follows: In this case, the second adhesive layer forming step is the same as the first adhesive layer forming step described above.

[0239] In the above case, the first adhesive layer forming step and the second adhesive layer forming step may be performed simultaneously or sequentially. Among these, the first adhesive layer forming step and the second adhesive layer forming step are preferably performed simultaneously. If the first adhesive layer forming step and the second adhesive layer forming step are performed sequentially, the first adhesive layer or the second adhesive layer will be dried more, which may result in the drying conditions being different from the preferred conditions. When the first adhesive layer forming step and the second adhesive layer forming step are performed sequentially, the drying conditions may be set so that the Martens hardness of the first adhesive layer and the second adhesive layer after the first adhesive layer forming step and the second adhesive layer forming step is within a predetermined range.

[0240] On the other hand, when producing the adhesive sheet of the third embodiment described above, the drying conditions in the second adhesive layer forming step are not particularly limited.

[0241] In the above case, the first adhesive layer forming process and the second adhesive layer forming process may be performed simultaneously or sequentially. Simultaneous execution of the first adhesive layer forming process and the second adhesive layer forming process is preferred. Alternatively, the first adhesive layer and the second adhesive layer are preferably formed by applying the first adhesive composition to one side of the substrate, applying the second adhesive composition to one side of the separator, laminating a coating of the separator-attached second adhesive composition to the other side of the substrate, and drying the first adhesive composition and the second adhesive composition. These procedures require only one drying step, making it easy to adjust the drying conditions for the first adhesive composition to optimal conditions. Furthermore, if the first adhesive layer forming process and the second adhesive layer forming process are performed sequentially, the first adhesive layer may be dried more than the optimal drying conditions. However, if the first adhesive layer forming process and the second adhesive layer forming process are performed sequentially, the drying conditions may be set so that the Martens hardness of the first adhesive layer after the first adhesive layer forming process and the second adhesive layer forming process is within a predetermined range.

[0242] 3. Intermediate Layer Formation Step The adhesive sheet manufacturing method of the present disclosure may include a first intermediate layer formation step of forming a first intermediate layer on one side of the substrate before the first adhesive layer formation step. The adhesive sheet manufacturing method of the present disclosure may also include a second intermediate layer formation step of forming a second intermediate layer on the other side of the substrate before the second adhesive layer formation step. The materials and methods for forming the first and second intermediate layers are the same as those described above in the section "A. Adhesive Sheet."

[0243] C. Article Manufacturing Method The article manufacturing method according to the present disclosure includes a disposing step of disposing the adhesive sheet described above between a first member and a second member, and a bonding step of curing the adhesive sheet to bond the first member and the second member together.

[0244] 9(a) and 9(b) are process diagrams showing an example of a method for manufacturing an article according to the present disclosure. First, as shown in FIG. 9(a), an adhesive sheet 10 is placed between a first member 20a and a second member 20b. Next, as shown in FIG. 9(b), the adhesive sheet 10 is cured, for example, by heating. The cured adhesive sheet 11 adheres (bonds) the first member 20a and the second member 20b. This results in an article 100 in which the adhesive sheet 11 is placed between the first member 20a and the second member 20b.

[0245] In the method for manufacturing an article according to the present disclosure, the adhesive sheet described above is used, which improves ease of insertion when inserting an adhesive sheet into a gap between two components, when inserting one component into the gap after placing the adhesive sheet in a hole or groove in the other component, or when inserting the other component with the adhesive sheet attached into a hole or groove in the other component. Furthermore, even if the adhesive sheet is folded in advance when placing it between the first and second components, cracking, lifting, and peeling of the adhesive layer can be suppressed. Therefore, an article can be obtained in which the first and second components have good adhesion.

[0246] The method for manufacturing the article according to the present disclosure will now be described.

[0247] 1. Adhesive Sheet The adhesive sheet used in the method for producing an article according to the present disclosure is the same as the adhesive sheet described above.

[0248] 2. Placement Step In the placement step of the present disclosure, the method for placing the adhesive sheet between the first member and the second member is not particularly limited. When using the adhesive sheet of the first embodiment and the adhesive sheet of the second embodiment, examples include a method of inserting the adhesive sheet into the gap between the first member and the second member, a method of placing the adhesive sheet in a hole or groove in the first member and then inserting the second member into the gap after placing the adhesive sheet in the hole or groove in the first member, and a method of inserting the second member with the adhesive sheet placed in the hole or groove in the first member. Furthermore, when using the adhesive sheet of the third embodiment, examples include a method of inserting the second member with the adhesive sheet attached into the hole or groove in the first member.

[0249] The material and shape of the first member and the second member are not particularly limited and may be appropriately selected depending on the application.

[0250] 3. Bonding Step In the bonding step of the present disclosure, examples of methods for curing the adhesive sheet include heating and light irradiation. Among these, it is preferable to cure the adhesive sheet by heating. Heating methods are applicable even when the first and second members are not transparent, such as when the first and second members are made of metal.

[0251] The heating conditions are appropriately set depending on the types of curable adhesive and foaming agent contained in the adhesive layer, the type of base material, etc. The heating temperature is, for example, 130° C. or higher and 200° C. or lower. The heating time is, for example, 3 minutes or higher and 3 hours or lower.

[0252] The present disclosure is not limited to the above-described embodiments. The above-described embodiments are merely examples, and any configuration that is substantially identical to the technical idea described in the claims of the present disclosure and that provides similar effects is included within the technical scope of the present disclosure.

[0253] First, an adhesive composition having the composition (parts by mass) shown in Table 1 below was prepared. Details of each material listed in Table 1 are also shown in Table 2. A highly insulating polyethylene naphthalate film (PEN film, manufactured by Toyobo Co., Ltd., Teonex Q5100, thicknesses of 25 μm, 75 μm, and 100 μm) was prepared as a substrate. The adhesive composition was applied to one surface of this substrate using a coating device so that the thickness after coating would be a predetermined thickness. The coating was then dried in a coating and drying device at a predetermined temperature for a predetermined time to form a first adhesive layer.

[0254] [Evaluation] (1) Tack For the tack of the first adhesive layer, a tack tester "TAC-II" manufactured by RHESCA was used to measure the load of the first adhesive layer of the adhesive sheet, by pressing a cylindrical stainless steel probe having a diameter of 5 mm against the surface of the first adhesive layer at a load of 0.1 N and a speed of 30 mm / min under conditions of a temperature of 23±5°C and a humidity of 50±30% RH, holding the probe for 1.0 second, and then peeling it off at a speed of 30 mm / min. This measurement was performed five times, and the average value was taken as the tack.

[0255] (2) Martens Hardness Using a Fisher Instruments Picodentor HM500, a diamond square pyramidal indenter was pressed against the surface of the first adhesive layer of the adhesive sheet at a temperature of 23±5°C and a humidity of 50±30% RH with a load of 25 mN and a load time of 20 seconds, and then held for 5 seconds. After that, the load was reduced to 0 mN for the same time as the load time, and the Martens hardness was measured. This measurement was performed 8 times, and the average value was taken as the measured value. During the measurement, the surface opposite the first adhesive layer of the adhesive sheet was cured with adhesive on a glass slide, eliminating the dependency on the contact surface.

[0256] (3) Blocking Resistance The adhesive sheet was cut into a piece of 5 cm x 5 cm, and two adhesive sheets were stacked together with the first adhesive layers facing each other. 2 The tapes were stored for 10 days under conditions of 23°C and 50% RH, and the blocking resistance was evaluated. The blocking resistance was evaluated according to the following criteria. A: There was no transfer or peeling of the first adhesive layer, and the adhesive sheets peeled off naturally. B: There was no transfer or peeling of the first adhesive layer, and the adhesive sheets did not peel off naturally, but they peeled off with very little force. C: There was transfer or peeling of the first adhesive layer, or the adhesive sheets did not peel off naturally, and they were so tightly attached that they made a peeling sound.

[0257] (5) Cross-bending test The adhesive sheet was cut into a piece of 3 cm x 3 cm, and this adhesive sheet was folded in half by 180° so that the surface on the first adhesive layer side was facing inward, resulting in a size of 3 cm x 1.5 cm. Next, the adhesive sheet in this state was folded again by 180° so that the size was 1.5 cm x 1.5 cm. It was then confirmed whether the first adhesive layer was lifted from the substrate. The adhesion in the cross-bending test was evaluated according to the following criteria: A: No lifting at the bent portion. B: Lifting at the bent portion.

[0258] (6) Cutter Cutting Test The surface of the adhesive sheet on the side of the first adhesive layer was cut with a cutter (Cutter Knife A Plus, manufactured by Olfa Co., Ltd.) at a speed of 20 mm / s to 100 mm / s inclusive, over a length of 100 mm. Then, it was confirmed whether or not the first adhesive layer was lifted from the substrate at the cut surface. The adhesion in the cutter cutting test was evaluated according to the following criteria: A: No lifting at all at the cut surface. B: Some lifting at the cut surface. C: Complete lifting at the cut surface.

[0259]

[0260]

[0261] The adhesive composition contains methyl ethyl ketone as a solvent, and in Table 1, the solid content (%) is the solid content concentration of the adhesive composition.

[0262]

[0263]

[0264]

[0265]

[0266] Tables 3 and 4 show the evaluation results when adhesive composition A was used and the thickness of the substrate, the thickness of the first adhesive layer, the drying temperature, or the type of coater / dryer was changed. Table 4 is a summary of Table 3. Table 3 shows that the Martens hardness of the first adhesive layer changes depending on the thickness of the substrate, the thickness of the first adhesive layer, the drying temperature, or the type of coater / dryer.

[0267] Table 5 shows the evaluation results when the drying temperature or drying time was changed when adhesive composition A or adhesive composition B was used. Table 6 shows the evaluation results when the drying temperature or drying time was changed when adhesive composition C or adhesive composition D was used.

[0268] It was confirmed that when the tack and Martens hardness of the first adhesive layer are within the specified ranges, the blocking resistance is good and cracking, lifting, and peeling of the adhesive layer during winding and bending can be suppressed.

[0269] The present disclosure provides the following inventions: [1] An adhesive sheet having a substrate and a first adhesive layer disposed on one side of the substrate and containing a first curable adhesive, wherein the tack of the first adhesive layer is less than 0.1 N, and the Martens hardness of the first adhesive layer is 20 N / mm 2 130N / mm or more 2 [2] An adhesive sheet having a second adhesive layer containing a second curable adhesive on the side of the substrate opposite to the first adhesive layer, wherein the tack of the second adhesive layer is less than 0.1 N, and the Martens hardness of the second adhesive layer is 20 N / mm or less. 2 130N / mm or more 2 [3] The adhesive sheet according to [1], wherein the adhesive sheet has a second adhesive layer containing a second curable adhesive and a separator, in this order, on the surface of the substrate opposite to the first adhesive layer, and wherein the tack of the second adhesive layer is 0.1 N or more. [4] The adhesive sheet according to [1], wherein the first adhesive layer contains a foaming agent. [5] The adhesive sheet according to [2] or [3], wherein at least one of the first adhesive layer and the second adhesive layer contains a foaming agent. [6] The adhesive sheet according to [1], wherein the first adhesive layer contains an epoxy resin. [7] The adhesive sheet according to [2] or [3], wherein the first adhesive layer and the second adhesive layer contain an epoxy resin. [8] A method for producing an adhesive sheet, comprising a first adhesive layer-forming step of applying a first adhesive composition containing a first curable adhesive to one surface of a substrate and drying it to form a first adhesive layer, wherein the tack of the first adhesive layer is less than 0.1 N, and wherein in the first adhesive layer-forming step, the first adhesive layer has a Martens hardness of 20 N / mm 2 130N / mm or more 2 [9] A method for manufacturing an adhesive sheet, comprising: a second adhesive layer forming step of applying a second adhesive composition containing a second curable adhesive to the other surface side of the substrate and drying the applied second adhesive composition to form a second adhesive layer, wherein the tack of the second adhesive layer is less than 0.1 N, and in the second adhesive layer forming step, the Martens hardness of the first adhesive layer is 20 N / mm 2 130N / mm or more2 [6] A method for producing an adhesive sheet according to [6], wherein the second adhesive composition is dried so that the following occurs:

[10] A method for producing an adhesive sheet according to [8], wherein the first adhesive composition contains a foaming agent;

[11] A method for producing an adhesive sheet according to [9], wherein at least one of the first adhesive composition and the second adhesive composition contains a foaming agent;

[12] A method for producing an adhesive sheet according to [8], wherein the first adhesive composition contains an epoxy resin;

[13] A method for producing an adhesive sheet according to [9], wherein the first adhesive composition and the second adhesive composition contain epoxy resins;

[14] A method for producing an article, comprising: a positioning step of positioning the adhesive sheet according to any one of [1] to [7] between a first member and a second member; and a bonding step of curing the adhesive sheet and bonding the first member and the second member together.

[0270] DESCRIPTION OF SYMBOLS 1... Substrate 2... First adhesive layer 3... Second adhesive layer 4... Separator 5... First intermediate layer 6... Second intermediate layer 10, 10A, 10B, 10C... Adhesive sheet 11... Cured adhesive sheet 20a... First member 20b... Second member 100... Article

Claims

1. An adhesive sheet having a substrate and a first adhesive layer disposed on one side of the substrate and containing a first curable adhesive, wherein the tack of the first adhesive layer is less than 0.1 N, and the Martens hardness of the first adhesive layer is 20 N / mm 2 130N / mm or more 2 Below is the adhesive sheet.

2. The substrate has a second adhesive layer containing a second curable adhesive on the side opposite to the first adhesive layer, the tack of the second adhesive layer is less than 0.1 N, and the Martens hardness of the second adhesive layer is 20 N / mm 2 130N / mm or more 2 The adhesive sheet according to claim 1 , wherein:

3. The adhesive sheet according to claim 1, having a second adhesive layer containing a second curable adhesive and a separator, in that order, on the side of the substrate opposite the first adhesive layer, and the tack of the second adhesive layer is 0.1 N or more.

4. The adhesive sheet according to claim 1, wherein the first adhesive layer contains a foaming agent.

5. The adhesive sheet according to claim 2 or 3, wherein at least one of the first adhesive layer and the second adhesive layer contains a foaming agent.

6. The adhesive sheet according to claim 1, wherein the first adhesive layer contains an epoxy resin.

7. The adhesive sheet according to claim 2 or 3, wherein the first adhesive layer and the second adhesive layer contain an epoxy resin.

8. A method for producing an adhesive sheet, comprising a first adhesive layer forming step of applying a first adhesive composition containing a first curable adhesive to one side of a substrate and drying the applied composition to form a first adhesive layer, wherein the tack of the first adhesive layer is less than 0.1 N, and in the first adhesive layer forming step, the Martens hardness of the first adhesive layer is 20 N / mm 2 130N / mm or more 2 The method for producing an adhesive sheet comprises drying the first adhesive composition so as to obtain the following:

9. A second adhesive layer forming step is provided in which a second adhesive composition containing a second curable adhesive is applied to the other surface side of the substrate and dried to form a second adhesive layer, wherein the tack of the second adhesive layer is less than 0.1 N, and in the second adhesive layer forming step, the Martens hardness of the first adhesive layer is 20 N / mm 2 130N / mm or more 2 The method for producing an adhesive sheet according to claim 8 , wherein the second adhesive composition is dried so that:

10. The method for producing an adhesive sheet according to claim 8, wherein the first adhesive composition contains a foaming agent.

11. The method for producing an adhesive sheet according to claim 9, wherein at least one of the first adhesive composition and the second adhesive composition contains a foaming agent.

12. The method for producing an adhesive sheet according to claim 8, wherein the first adhesive composition contains an epoxy resin.

13. The method for producing an adhesive sheet according to claim 9, wherein the first adhesive composition and the second adhesive composition contain an epoxy resin.

14. A method for manufacturing an article, comprising: a step of placing an adhesive sheet according to any one of claims 1 to 3 between a first member and a second member; and a step of curing the adhesive sheet to bond the first member and the second member.

Citation Information

Patent Citations

  • Adhesive sheet

    JP2018021203A

  • Adhesive sheet

    JP2019214729A

  • Adhesive composition and foamable adhesive sheet

    JP2020076059A

  • Adhesive sheet