Resin sheet, laminated plate, metal-clad laminated plate, printed wiring board, and semiconductor package
The resin sheet composition addresses the challenge of maintaining low dielectric loss tangent and thermal expansion by using an elastomer and inorganic filler, ensuring compatibility with high-frequency signals and resistance to vacuum suction, thus enabling effective industrial-scale transportation and production of high-frequency compatible printed wiring boards.
Patent Information
- Application Number
- PCT/JP2024/015566
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-19
- Filing Date
- 2024-04-19
- Publication Date
- 2024-10-24
AI Technical Summary
Existing resin sheets for printed wiring boards face challenges in maintaining low dielectric loss tangent (Df) and thermal expansion while being compatible with high-frequency signals, and they tend to break during industrial-scale transportation using vacuum suction pads.
A resin sheet composition containing an elastomer with a number average molecular weight of 10,000 or more, an inorganic filler, and a thermosetting resin, with a specific content range of 25-70% by volume, which provides self-support, low thermal expansion, and resistance to vacuum suction, ensuring dielectric constants between 2.50 and 3.30 and dielectric loss tangents of 0.0020 or less in high-frequency bands.
The resin sheet achieves industrial conveyability, low thermal expansion, and optimal dielectric properties, enabling the production of laminates, printed wiring boards, and semiconductor packages suitable for high-frequency applications without breaking during transportation.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Resin sheets, laminates, metal-clad laminates, printed wiring boards and semiconductor packages
[0001] The present disclosure relates to a resin sheet, a laminate, a metal-clad laminate, a printed wiring board, and a semiconductor package.
[0002] Mobile communication devices, such as mobile phones, their base station equipment, servers, routers, and other network infrastructure equipment, and large-scale computers, are increasingly using faster and larger-capacity signals. This trend requires printed wiring boards (PCBs) for these electronic devices to support higher frequencies, necessitating the development of substrate materials with excellent dielectric properties in high-frequency bands, i.e., low dielectric constant (Dk) and dielectric loss tangent (Df), which enable reduced transmission loss. Meanwhile, as electronic devices become more compact, the density of electronic components used on PCBs is also increasing. To achieve this high density, PGA (pin grid array) packages have traditionally been used. PGA packages have a structure in which pins protrude vertically from the back surface of the substrate in a grid pattern at regular intervals. The size and spacing of these pins are often fixed, making design changes difficult. If the dielectric constant of the substrate material decreases, it becomes necessary to make the pins of the PGA package smaller and to narrow the spacing between the pins, but as mentioned above, it is difficult to make such design changes, so it is necessary to keep the dielectric constant of the substrate material at a desired value. In other words, in order to achieve high-density mounting and high-frequency compatibility, it is necessary to reduce the dielectric loss tangent while keeping the dielectric constant of the substrate material at a desired value, and material manufacturers are eagerly awaiting the development of such substrate materials.
[0003] To date, prepregs using thermosetting resin compositions with excellent dielectric properties in high frequency bands have been developed as substrate materials capable of achieving low transmission loss (see, for example, Patent Document 1). Prepregs are formed from aggregates and thermosetting resin compositions, and the presence of the aggregates makes it possible to handle the prepregs without a support.
[0004] Japanese Patent Application Laid-Open No. 2020-169276
[0005] However, glass cloth, which is one of the representative aggregates, is produced by bundling a plurality of glass filaments in the presence of a sizing agent and weaving the resulting twisted glass strands. 2 Impurities derived from glass components other than B 2 O 3 , CaO, MgO, Na 2 The present inventors have found that the impurities deteriorate the dielectric properties, limiting their ability to meet the recent demand for improved dielectric loss tangent (Df). Therefore, when they considered using a simple resin sheet without using glass cloth in conventional prepregs, they found that the absence of aggregates caused the resin sheet to tear or shatter unless a support such as a polyethylene terephthalate (PET) film was attached, and the low thermal expansion properties were also impaired.
[0006] Under these circumstances, the applicant has already filed an international patent application (PCT / JP2021 / 038025) for a resin sheet that can be handled without a support, has low thermal expansion, and has a dielectric constant (Dk) and dielectric dissipation factor (Df) within a predetermined range in a high frequency band of 10 GHz or higher. The application claims the following: "A resin sheet containing (A) a resin component and (B) an inorganic filler, wherein the component (A) contains (A1) an elastomer having a number average molecular weight of 10,000 or more, the content of the component (A1) being 30% by mass or more based on the component (A), and the content of the component (B) being 40 to 95% by volume based on the total amount of the resin sheet." However, after further investigations, the inventors found that while the resin sheet described in the above-mentioned international patent application (PCT / JP2021 / 038025) can indeed be handled without a support (it is self-supporting) and can be transported manually, when a method of transporting the resin sheet by adsorbing it with a vacuum suction pad is adopted for industrial scale implementation, the resin sheet tends to break easily.
[0007] In view of the above circumstances, the present disclosure aims to provide a resin sheet that can withstand suction and transport using a vacuum suction pad for transport, has low thermal expansion, and has a relative permittivity (Dk) of 2.50 to 3.30 in a high frequency band of 10 GHz or higher and a dielectric loss tangent (Df) of 0.0020 or less in a high frequency band of 10 GHz or higher. It also aims to provide a laminate, a printed wiring board, and a semiconductor package manufactured using the resin sheet.
[0008] The present inventors have conducted extensive research to achieve the above object, and have found that the object can be achieved by the present disclosure. The present disclosure includes the following embodiments [1] to
[13] . [1] A resin sheet containing (A) a resin component and (B) an inorganic filler, wherein the component (A) contains (A1) an elastomer with a number average molecular weight of 10,000 or more, the content of the component (B) is 25 to 70% by volume based on the total amount of the resin sheet, and the breaking energy is 0.1 mJ / mm 3[2] The resin sheet according to the above [1], wherein the component (A1) comprises one or more selected from the group consisting of styrene-based elastomers, maleimide-based elastomers, olefin-based elastomers, urethane-based elastomers, polyester-based elastomers, polyamide-based elastomers, acrylic elastomers, silicone-based elastomers, and derivatives thereof. [3] The resin sheet according to the above [1] or [2], further comprising (A2) an elastomer with a number average molecular weight of less than 10,000. [4] The resin sheet according to any one of the above [1] to [3], wherein the component (A) further comprises (A3) a thermosetting resin. [5] The resin sheet according to [4] above, wherein the component (A3) comprises one or more resins selected from the group consisting of epoxy resins, phenolic resins, unsaturated imide resins, cyanate resins, isocyanate resins, benzoxazine resins, oxetane resins, amino resins, unsaturated polyester resins, allyl resins, vinylbenzyl resins, dicyclopentadiene resins, silicone resins, triazine resins, modified polyphenylene ether resins, and melamine resins. [6] The resin sheet according to [4] or [5] above, wherein the total content of the components (A1) and (A2) is 40 to 95 mass% based on the component (A). [7] The resin sheet according to any of [1] to [6] above, wherein the resin sheet does not contain any organic solvent, or, if it contains any organic solvent, the content thereof is less than 1 mass% based on the total amount of the resin sheet. [8] The resin sheet according to any of [1] to [7] above, wherein the resin sheet does not contain any glass fiber, or, if it contains any glass fiber, the content thereof is 10 volume% or less based on the total amount of the resin sheet. [9] The resin sheet according to any one of [1] to [8] above, which breaks when adsorbed with a 20 mm diameter silicone vacuum adsorption pad at a vacuum level of -15 kPa or less.
[10] A laminate comprising a cured product of the resin sheet according to any one of [1] to [9] above.
[11] A metal-clad laminate comprising a metal foil and a cured product of the resin sheet according to any one of [1] to [9] above.
[12] A printed wiring board comprising the laminate according to
[10] above or the metal-clad laminate according to
[11] above.
[13] A semiconductor package comprising the printed wiring board according to
[12] above and a semiconductor element.
[0009] According to the present disclosure, it is possible to provide a resin sheet that can withstand suction and transportation using a vacuum suction pad for transportation, has low thermal expansion, and has a relative permittivity (Dk) of 2.50 to 3.30 in a high frequency band of 10 GHz or more and a dielectric loss tangent (Df) of 0.0020 or less in a high frequency band of 10 GHz or more. Furthermore, it is possible to provide a laminate, a printed wiring board, and a semiconductor package manufactured using the resin sheet.
[0010] 10 is a photograph showing the state of a resin sheet when a break occurs in an adsorption portion of the resin sheet during measurement of a breaking vacuum degree.
[0011] In the numerical ranges described herein, the upper or lower limit of the numerical range may be replaced with a value shown in the examples. Furthermore, the lower and upper limits of a numerical range can be arbitrarily combined with the lower or upper limit of another numerical range. In the expression "AA to BB," the two extreme values AA and BB are included as the lower and upper limits, respectively, of the numerical range. In this specification, for example, "10 or more" means 10 and a value greater than 10, and this also applies when the numerical values differ. Furthermore, for example, "10 or less" means 10 and a value less than 10, and this also applies when the numerical values differ. Furthermore, unless otherwise specified, each component and material exemplified herein may be used alone or in combination of two or more types. In this specification, when multiple substances corresponding to each component are present in the composition, the content of each component in the composition refers to the total amount of the multiple substances present in the composition, unless otherwise specified.
[0012] In this specification, "solid content" refers to non-volatile content excluding water and the diluent described below contained in the photosensitive resin composition, and includes liquid, syrup-like, and wax-like substances at room temperature around 25°C. In this specification, "relative permittivity" and "dielectric loss tangent" refer to "relative permittivity" and "dielectric loss tangent" in the 10 GHz band unless otherwise specified. In this specification, the relative permittivity and dielectric loss tangent may be collectively referred to as "dielectric properties." Any combination of the items described in this specification is also included in the present disclosure and the present embodiment.
[0013] [Resin Sheet] One aspect of this embodiment is the following resin sheet: A resin sheet containing (A) a resin component and (B) an inorganic filler, wherein the component (A) contains (A1) an elastomer with a number average molecular weight of 10,000 or more, the content of the component (B) is 25 to 70% by volume based on the total amount of the resin sheet, and the breaking energy is 0.1 mJ / mm 3 Here, the expression "a resin sheet containing ..." includes both a resin sheet that contains the component described in ... as it is, and a resin sheet obtained by reacting at least a part of the component described in ....
[0014] The breaking energy of the resin sheet of this embodiment is 0.1 mJ / mm 3 By satisfying the above, the resin sheet can withstand suction by a vacuum suction pad for transportation and transportation (hereinafter, this property may be referred to as "industrial transportability"). From the same viewpoint, the breaking energy of the resin sheet is preferably 0.5 mJ / mm 3 More preferably, 1.0 mJ / mm 3 More preferably, 1.5 mJ / mm 3 The breaking energy of the resin sheet is 1.0 mJ / mm 3 When the breaking energy is 4.0 mJ / mm or more, the work of peeling the resin sheet from the support such as PET tends to be performed by machine (automation), which is preferable from the viewpoint of industrial implementation. 3 It may be 3.5 mJ / mm or less. 3 or less, 3.0 mJ / mm 3 or less, and may be 2.8 mJ / mm 3 That is, the breaking energy of the resin sheet of this embodiment may be 0.1 to 4.0 mJ / mm 3There are no particular limitations on the method for adjusting the breaking energy of the resin sheet of the present embodiment to fall within the above range, and examples thereof include (i) a method of adjusting the content of the (A1) component within the range described below, (ii) a method of adjusting the content of the (B) component within the range described below, and a combination of the above (i) and (ii).
[0015] Although the resin sheet of this embodiment is not particularly limited, from the viewpoint of facilitating suction and transport with a vacuum suction pad for transport, the degree of vacuum at which the resin sheet breaks when adsorbed with a 20 mm diameter silicone vacuum suction pad (adsorption portion shape: circular) (hereinafter, sometimes referred to as the breaking vacuum degree) is preferably −15 kPa or less, more preferably −20 kPa or less, even more preferably −30 kPa or less, and particularly preferably −40 kPa or less, and although not particularly limited, the degree of vacuum may be −150 kPa or more, −120 kPa or more, or −100 kPa or more. A more detailed method for measuring the breaking vacuum degree is as described in the examples.
[0016] The resin sheet of this embodiment can withstand suction and transport using a vacuum suction pad, has low thermal expansion, and has a relative dielectric constant (Dk) of 2.50 to 3.30 in the high frequency band of 10 GHz or higher and a dielectric dissipation factor (Df) of 0.0020 or less in the high frequency band of 10 GHz or higher. The relative dielectric constant (Dk) is preferably 2.65 to 3.30, more preferably 2.70 to 3.20, even more preferably 2.75 to 3.10, and particularly preferably 2.80 to 3.10. The dielectric dissipation factor (Df) is preferably 0.0018 or less, more preferably 0.0015 or less, even more preferably 0.0010 or less, particularly preferably 0.0009 or less, and most preferably 0.0008 or less. The lower limit of the dielectric dissipation factor (Df) is not particularly limited, and may be 0.0003 or more, 0.0004 or more, or 0.0005 or more. The relative permittivity (Dk) and the dielectric loss tangent (Df) are values measured using a split post dielectric resonator (SPDR), more specifically, by the method described in the examples.
[0017] Furthermore, a preferred embodiment of the resin sheet of this embodiment does not contain an organic solvent, or if it contains an organic solvent, the content of the organic solvent is less than 1 mass% based on the total amount of the resin sheet, but nevertheless has sufficient flexibility, so that cracks and the like are unlikely to occur and handling is excellent. In a preferred embodiment of the resin sheet of this embodiment, the content of the organic solvent is low, which has the advantage that there is little risk of voids occurring during reflow, etc.
[0018] Another preferred aspect of the resin sheet of this embodiment is that, from the viewpoint of dielectric loss tangent (Df), the resin sheet does not contain glass fibers, or if it contains glass fibers, the content is 10 volume % or less based on the total amount of the resin sheet (hereinafter, this may be referred to as "Feature A"). Nevertheless, the resin sheet has excellent industrial transportability. When the resin sheet contains glass fibers, the content is preferably 7 volume % or less, more preferably 5 volume % or less, and even more preferably 3 volume % or less based on the total amount of the resin sheet, from the viewpoint of dielectric loss tangent (Df). Note that in the description of Feature A in the above aspect, the term "glass fiber" can be replaced with "glass cloth" or "fiber substrate." In other words, another preferred aspect of the resin sheet of this embodiment is that, from the viewpoint of dielectric loss tangent (Df), the resin sheet does not contain glass cloth, or if it contains glass cloth, the content is 10 volume % or less based on the total amount of the resin sheet. In addition, in another preferred embodiment of the resin sheet of this embodiment, from the viewpoint of dielectric loss tangent (Df), the resin sheet does not contain a fiber substrate, or if it contains a fiber substrate, the content thereof is 10 volume % or less based on the total amount of the resin sheet. When the resin sheet of this embodiment contains a glass cloth or a fiber substrate, the preferred content thereof is the same as that of the glass fiber described above.
[0019] Each component contained in the resin sheet of this embodiment is described in detail below. ((A) Resin Component, (A1) Elastomer with Number-Average Molecular Weight of 10,000 or More) The resin sheet of this embodiment contains a resin component as component (A), which includes "(A1) an elastomer with a number-average molecular weight of 10,000 or more." By including component (A1), the resin sheet of this embodiment can stand on its own even without a support and exhibit high flexibility. Furthermore, by including component (A1), the resin sheet of this embodiment can have the predetermined relative dielectric constant (Dk) and dielectric loss tangent (Df). From the viewpoint of enabling the resin sheet to stand on its own even without a support, the number-average molecular weight (Mn) of component (A1) is preferably 15,000 or more, more preferably 18,000 or more, even more preferably 25,000 or more, particularly preferably 35,000 or more, and most preferably 50,000 or more. Although there is no particular upper limit to the number average molecular weight of component (A1), from the viewpoint of circuit embedding properties, it is preferably 300,000 or less, more preferably 250,000 or less, even more preferably 200,000 or less, particularly preferably 120,000 or less, and most preferably 90,000 or less. In other words, the number average molecular weight (Mn) of component (A1) is preferably 10,000 or more and 300,000 or less. In this specification, the number average molecular weight is a value determined in terms of standard polystyrene by gel permeation chromatography (GPC) using tetrahydrofuran as a solvent.
[0020] The content of the component (A1) is preferably 20% by mass or more, i.e., 20 to 100% by mass, more preferably 25 to 90% by mass, even more preferably 25 to 80% by mass, particularly preferably 30 to 70% by mass, and most preferably 35 to 65% by mass, based on the component (A). When the content of the component (A1) is equal to or more than the lower limit, it becomes easier to control the breaking energy of the resin sheet to the predetermined value, improving the industrial transportability of the resin sheet and enabling it to have the predetermined relative dielectric constant (Dk) and dielectric loss tangent (Df).
[0021] Component (A1) preferably contains at least one selected from the group consisting of styrene-based elastomers, maleimide-based elastomers, olefin-based elastomers, urethane-based elastomers, polyester-based elastomers, polyamide-based elastomers, acrylic elastomers, silicone-based elastomers, and derivatives thereof. While not particularly limited, styrene-based elastomers and maleimide-based elastomers are preferred, and styrene-based elastomers are more preferred, from the viewpoint of achieving the desired dielectric constant (Dk) and dielectric loss tangent (Df). Commercially available elastomers can be used for any of these elastomers. Examples of the elastomer derivatives include those having reactive functional groups at the molecular end or in the molecular chain of the elastomers. Examples of such reactive functional groups include acid anhydride groups, epoxy groups, hydroxyl groups, carboxyl groups, amino groups, amide groups, isocyanato groups, acrylic groups, methacrylic groups, and vinyl groups. The elastomer derivatives may have one or more reactive functional groups. The reactive functional group may be of one type or of two or more types.
[0022] (Styrene-Based Elastomer; Component (A1)) The styrene-based elastomer is not particularly limited, but examples thereof include styrene-butadiene copolymers such as styrene-butadiene diblock copolymers and styrene-butadiene-styrene triblock copolymers; styrene-isoprene copolymers such as styrene-isoprene diblock copolymers and styrene-isoprene-styrene triblock copolymers; hydrogenated products of the styrene-butadiene copolymers; and hydrogenated products of the styrene-isoprene copolymers. These copolymers may or may not contain structural units derived from vinyl group-containing aromatic compounds such as divinylbenzene. One type of styrene-based elastomer may be used alone, or two or more types may be used in combination. The number average molecular weight (Mn) of the styrene-based elastomer is the same as the number average molecular weight (Mn) of the component (A1). The styrene content of the styrene-based elastomer is not particularly limited, but is preferably 10 to 70% by mass, more preferably 10 to 50% by mass, even more preferably 10 to 40% by mass, and particularly preferably 15 to 35% by mass. Here, the styrene content refers to the content of styrene structural units relative to all structural units. If the styrene content is equal to or greater than the lower limit, heat resistance tends to be good, while if it is equal to or less than the upper limit, rubber elasticity tends to be excellent and industrial transportability and flexibility tend to be good. The styrene elastomer may be unhydrogenated or may be a hydrogenated product. If it is a hydrogenated product, the hydrogenation rate of the styrene elastomer is not particularly limited, but is preferably 80 to 100 mol%, more preferably 85 to 100 mol%, even more preferably 90 to 100 mol%, or may be 95 to 100 mol%.
[0023] As the styrene-based elastomer, commercially available products may be used, such as the Tuftec (registered trademark) H series, P series, and M series manufactured by Asahi Kasei Corporation, the Septon (registered trademark) series manufactured by Kuraray Co., Ltd., and the Kraton (registered trademark) G Polymer series and D Polymer series manufactured by Kraton Polymer Japan Co., Ltd.
[0024] (Maleimide-Based Elastomer; Component (A1)) The maleimide-based elastomer is not particularly limited as long as it is an elastomer having a maleimide skeleton, and examples thereof include maleimide compounds having a structure in which a saturated or unsaturated aliphatic hydrocarbon group is bonded to a maleimide group. The maleimide compound having a structure in which a saturated or unsaturated aliphatic hydrocarbon group is bonded to a maleimide group is preferably a maleimide compound having a structure in which the saturated or unsaturated aliphatic hydrocarbon group is bonded to a nitrogen atom of the maleimide group. The maleimide compound having a structure in which a saturated or unsaturated aliphatic hydrocarbon group is bonded to a maleimide group preferably has at least two maleimide groups, more preferably a maleimide compound having one or more structures represented by the following general formula (1), and even more preferably a maleimide compound represented by the following general formula (2). The saturated or unsaturated aliphatic hydrocarbon group preferably has 1 to 100 carbon atoms, more preferably 2 to 50, and even more preferably 4 to 40 carbon atoms. The saturated or unsaturated aliphatic hydrocarbon group may have 8 to 100 carbon atoms, 8 to 50 carbon atoms, 15 to 50 carbon atoms, 25 to 50 carbon atoms, or 30 to 45 carbon atoms. The saturated or unsaturated aliphatic hydrocarbon group may be a linear group, a branched group, a cyclic group, or a combination thereof. The cyclic group is preferably an alicyclic hydrocarbon group. The saturated or unsaturated aliphatic hydrocarbon group is preferably a combination of a linear group and a cyclic group, and more preferably a combination of a linear group and an alicyclic hydrocarbon group.
[0025]
[0026]
[0027] In the above general formulas (1) and (2), x represents an integer of 10 to 50, and preferably an integer of 20 to 40. In addition, in the above general formula (2), n represents the number of structural units enclosed in brackets, and is preferably an integer of 0 to 50, more preferably an integer of 1 to 30, even more preferably an integer of 1 to 20, and particularly preferably an integer of 1 to 10.
[0028] Specific examples of the maleimide compound represented by the general formula (2) include compounds represented by the following formula (3): In the following formula (3), n represents the number of structural units enclosed in parentheses and is an integer of 1 to 10.
[0029]
[0030] The number average molecular weight (Mn) of the maleimide elastomer is the same as the number average molecular weight (Mn) of the component (A1), but is preferably 10,000 or more and less than 100,000, and may be 10,000 to 50,000, 15,000 to 35,000, or 17,000 to 30,000.
[0031] ((A2) Elastomer with a number-average molecular weight of less than 10,000) Component (A) may or may not contain an elastomer other than the aforementioned "(A1) elastomer with a number-average molecular weight of 10,000 or more," i.e., "(A2) elastomer with a number-average molecular weight of less than 10,000," but it is preferable that it contains such an elastomer. Component (A2) has the effect of improving the compatibility between the aforementioned component (A1) and the "(A3) thermosetting resin" described below. From the viewpoint of improving compatibility between the aforementioned component (A1) and the "(A3) thermosetting resin" described below, the number average molecular weight (Mn) of the component (A2) is preferably at least 300 and less than 10,000, and more preferably 400 to 9,000, and may be 500 to 6,000, 1,000 to 5,500, 1,500 to 5,000, 2,000 to 5,000, or 2,500 to 4,000.
[0032] Examples of the component (A2) include the same materials as the component (A1). Among these, from the viewpoint of improving the compatibility between the aforementioned component (A1) and the "(A3) thermosetting resin" described below, and from the viewpoint of the relative dielectric constant (Dk) and the dielectric loss tangent (Df), one or more types selected from the group consisting of polybutadiene-based elastomers and styrene-based elastomers are preferred, and the component (A2) may be either a polybutadiene-based elastomer or a styrene-based elastomer.
[0033] (Polybutadiene-based elastomer; component (A2)) Examples of polybutadiene-based elastomers include polybutadiene diol, polybutadiene dicarboxylic acid, maleated polybutadiene, butadiene homopolymer, copolymers copolymerizable with butadiene, compounds obtained by reacting polybutadiene diol with a compound having an isocyanate group, compounds obtained by reacting polybutadiene diol with a compound having a carboxyl group, compounds obtained by reacting polybutadiene dicarboxylic acid with a compound having a hydroxyl group, and compounds obtained by reacting polybutadiene dicarboxylic acid with a compound having an epoxy group. Among these, butadiene homopolymer is preferred as the polybutadiene-based elastomer.
[0034] The number average molecular weight (Mn) of the polybutadiene elastomer used as component (A2) is the same as the number average molecular weight (Mn) of component (A2) described above.
[0035] Commercially available polybutadiene elastomers may be used. Commercially available polybutadiene dicarboxylic acids include C-1000 (content of 1,2-structural units: 85% or more, product name: Nippon Soda Co., Ltd.). Commercially available butadiene homopolymers include B-1000 (content of 1,2-structural units: 85%), B-2000 (content of 1,2-structural units: 85%), and B-3000 (content of 1,2-structural units: 90%) (all of which are product names, ...
[0036] (Styrene-based elastomer; component (A2)) Examples of the styrene-based elastomer include the same styrene-based elastomer as the component (A1). However, the number average molecular weight (Mn) of the styrene-based elastomer used as component (A2) is the same as the number average molecular weight (Mn) of component (A2) described above. Commercially available styrene-based elastomers may be used.
[0037] (Total Content of Component (A1) and Component (A2)) The total content of the component (A1) and the component (A2) is preferably 40 to 95% by mass, more preferably 45 to 95% by mass, and even more preferably 50 to 90% by mass, based on the component (A). It may be 55 to 90% by mass or 65 to 85% by mass. When the total content of the component (A1) and the component (A2) is equal to or greater than the lower limit, the resin sheet tends to be mainly composed of an elastomer, the dielectric loss tangent (Df) is low, and the resin sheet tends to have high flexibility. When the total content of the component (A1) and the component (A2) is equal to or less than the upper limit, the resin sheet can contain a sufficient amount of the thermosetting resin (A3), which will be described later, and therefore tends to be able to impart various properties to the resin sheet, such as low thermal expansion, heat resistance, and adhesion to conductors.
[0038] ((A3) Thermosetting Resin) The component (A) may further contain a thermosetting resin as the component (A3). The inclusion of a thermosetting resin can improve the heat resistance of the resin sheet. The component (A3) may be used alone or in combination of two or more. Examples of thermosetting resins include epoxy resins, phenolic resins, unsaturated imide resins, cyanate resins, isocyanate resins, benzoxazine resins, oxetane resins, amino resins, unsaturated polyester resins, allyl resins, vinylbenzyl resins, dicyclopentadiene resins, silicone resins, triazine resins, modified polyphenylene ether resins, and melamine resins. It is preferable to contain one or more selected from the group consisting of these. Furthermore, the thermosetting resin is not particularly limited to these, and any known thermosetting resin can be used. Among these, unsaturated imide resins and vinylbenzyl resins are preferred from the viewpoints of low thermal expansion and heat resistance, as well as adhesion to conductors. The modified polyphenylene ether resin is a polyphenylene ether resin having a reactive group such as a vinyl group or a (meth)acrylic group. As the unsaturated imide resin, a maleimide compound is preferred from the viewpoints of low thermal expansion, heat resistance, and adhesion to conductors. Examples of the maleimide compound include one or more maleimide compounds having one or more N-substituted maleimide groups and their derivatives. The maleimide compound referred to here does not include the maleimide elastomer. The maleimide compound having one or more N-substituted maleimide groups is preferably a maleimide compound having two or more N-substituted maleimide groups. In the maleimide compound having two or more N-substituted maleimide groups, the nitrogen atoms of the two or more maleimide groups are preferably bonded to each other via an organic group. Examples of the "derivative of a maleimide compound having one or more N-substituted maleimide groups" include an addition reaction product of the maleimide compound having one or more N-substituted maleimide groups and an amine compound such as a diamine compound.
[0039] As the maleimide compound, from the viewpoints of low thermal expansion and heat resistance, and adhesion to a conductor, it is preferable to use at least one type selected from the group consisting of: a maleimide compound having one or more N-substituted maleimide groups; and an aminomaleimide compound having a structural unit derived from a maleimide compound and a structural unit derived from a diamine compound.
[0040] The vinylbenzyl resin is not particularly limited as long as it is a compound having a vinylbenzyl group, but preferably contains at least one selected from the group consisting of compounds having three or more vinylbenzyl groups bonded to oxygen atoms and compounds having one or more vinylbenzyl groups bonded to carbon atoms. Furthermore, from the viewpoint of dielectric properties, the vinylbenzyl resin is preferably a vinylbenzyl resin containing at least one ring selected from the group consisting of a fluorene ring and an indene ring. The vinylbenzyl group may be any of an o-vinylbenzyl group, an m-vinylbenzyl group, and a p-vinylbenzyl group.
[0041] When the component (A) further contains a thermosetting resin (A3), the content of the component (A3) is not particularly limited, but is preferably 5 to 60 mass%, more preferably 5 to 55 mass%, and even more preferably 10 to 50 mass%, or may be 10 to 45 mass%, or may be 15 to 35 mass%, based on the component (A). When the content of the component (A3) is equal to or greater than the lower limit, the resin sheet tends to be easily endowed with various properties such as low thermal expansion, heat resistance, and adhesion to conductors. When the content is equal to or less than the upper limit, the resin sheet tends to be mainly composed of an elastomer, which reduces the dielectric loss tangent (Df) and provides high flexibility.
[0042] The total amount of the components (A1), (A2), and (A3) in the component (A) is preferably 50 to 100 mass%, more preferably 80 to 100 mass%, even more preferably 90 to 100 mass%, particularly preferably 95 to 100 mass%, and may even be 100 mass%.
[0043] The content of the component (A) is not particularly limited, but is preferably 80 to 100 mass%, more preferably 85 to 100 mass%, even more preferably 90 to 100 mass%, and particularly preferably 95 to 100 mass%, based on the total amount of resin components in the resin sheet.
[0044] ((B) Inorganic Filler) The resin sheet of this embodiment contains an inorganic filler as component (B), and the content of component (B) is 25 to 70% by volume based on the total amount of the resin sheet. By containing 25% by volume or more of component (B), low thermal expansion is improved and the tackiness of the resin sheet is reduced, making it easier to peel the resin sheet from the support. By containing component (B) in an amount of 70% by volume or less, it becomes easier to control the breaking energy of the resin sheet to the predetermined value. One type of component (B) may be used alone, or two or more types may be used in combination.
[0045] The inorganic filler is not particularly limited, but may include silica, alumina, titanium oxide, mica, beryllia, barium titanate, potassium titanate, strontium titanate, calcium titanate, aluminum carbonate, magnesium hydroxide, aluminum hydroxide, aluminum silicate, calcium carbonate, calcium silicate, magnesium silicate, silicon nitride, boron nitride, clay (calcined clay, etc.), molybdenum compounds such as zinc molybdate, talc, aluminum borate, silicon carbide, etc. These may be used alone or in combination of two or more. Among these, from the viewpoints of thermal expansion coefficient, elastic modulus, heat resistance and flame retardancy, silica, alumina, mica, molybdenum compounds, and talc are preferred, silica and alumina are more preferred, and silica is even more preferred. Examples of silica include precipitated silica produced by wet method, which has a high water content, and dry method silica produced by dry method, which contains almost no bound water.Dry method silica can further include crushed silica, fumed silica, fused silica (fused spherical silica), etc., depending on the manufacturing method.There is no particular limitation on the shape of the inorganic filler, and it can be spherical, needle-like, scaly, plate-like, etc., but from the viewpoint of easily loading the inorganic filler with a high amount, spherical is preferred.However, in this embodiment, (B) inorganic filler does not include fiber substrate such as glass cloth, and further does not include glass fiber. Therefore, when the resin sheet of this embodiment contains a fiber base material such as glass cloth or glass fiber, it is contained as another component rather than as component (B), and the content of the fiber base material or glass fiber is preferably within the above-mentioned range (i.e., 10 volume % or less, preferably 7 volume % or less, more preferably 5 volume % or less, and even more preferably 3 volume % or less, based on the total amount of the resin sheet), and the total content of the fiber base material and glass fiber is preferably 10 volume % or less, more preferably 7 volume % or less, even more preferably 5 volume % or less, and particularly preferably 3 volume % or less, based on the total amount of the resin sheet.
[0046] The inorganic filler may not be surface-treated with a coupling agent, but from the viewpoint of improving dispersibility in the resin sheet, it may be surface-treated with a coupling agent such as a silane coupling agent, or it is preferable that it is surface-treated with a coupling agent such as a silane coupling agent. Examples of silane coupling agents include aminosilane coupling agents, epoxysilane coupling agents, phenylsilane coupling agents, alkylsilane coupling agents, alkenylsilane coupling agents, alkynylsilane coupling agents, haloalkylsilane coupling agents, siloxane coupling agents, hydrosilane coupling agents, silazane coupling agents, alkoxysilane coupling agents, chlorosilane coupling agents, (meth)acrylic silane coupling agents, isocyanurate silane coupling agents, ureidosilane coupling agents, mercaptosilane coupling agents, sulfide silane coupling agents, isocyanate silane coupling agents, etc. Among these, aminosilane coupling agents, alkenylsilane coupling agents, and (meth)acrylic silane coupling agents are preferred.
[0047] The average particle size of the inorganic filler is not particularly limited, but is preferably 0.01 to 20 μm, more preferably 0.1 to 10 μm, even more preferably 0.2 to 8 μm, and particularly preferably 0.3 to 5 μm. It may be 0.5 to 5 μm, 0.5 to 3 μm, or 0.5 to 1.5 μm. Several types of inorganic fillers with different average particle sizes may be used in combination. Using several types of inorganic fillers with different average particle sizes tends to facilitate high loading of the inorganic filler into the resin sheet. Herein, the average particle size refers to the particle size at the point corresponding to 50% volume when a cumulative frequency distribution curve of particle size is calculated, assuming the total volume of the particles to be 100%. The particle size of the inorganic filler can be measured using a particle size distribution analyzer using a laser diffraction scattering method, and the same applies hereinafter.
[0048] As described above, the content of the (B) component is 25 to 70 vol%, preferably 30 to 70 vol%, more preferably 35 to 70 vol%, even more preferably 45 to 70 vol%, particularly preferably 50 to 70 vol%, and may be 50 to 65 vol%, based on the total amount of the resin sheet. When the content of the (B) component is equal to or greater than the lower limit, the resin sheet exhibits excellent low thermal expansion properties and sufficiently reduces tackiness. When the content of the (B) component is equal to or less than the upper limit, the resin sheet exhibits excellent industrial transportability. Thus, since this embodiment can have Feature A, it is also possible to highly fill the resin sheet with the (B) component. Note that in the case of a prepreg, rather than a resin sheet as in this embodiment, Feature A is not possessed, and therefore the upper limit of the inorganic filler content is 55 vol%, based on the total amount of the resin composition in the prepreg. If the inorganic filler content in the prepreg exceeds 55% by volume, the inorganic filler will overflow due to the presence of the fiber base material, making it difficult to melt the resin composition, and as a result, it tends to become impossible to produce the prepreg at all.
[0049] ((C) Organic Filler) The resin sheet of this embodiment may or may not further contain an organic filler as component (C). When the resin sheet of this embodiment contains an organic filler, the dielectric loss tangent (Df) tends to be further reduced, and the relative dielectric constant (Dk) tends to be easily adjusted to the predetermined range. The organic filler is not particularly limited, but examples thereof include single-structure resin particles made of polyethylene, polypropylene, polystyrene, polyphenylene ether resin, silicone resin, tetrafluoroethylene resin, etc.; core-shell structured resin particles having a rubber-like core layer made of an acrylate resin, a methacrylate resin, a conjugated diene resin, etc., and a glassy shell layer made of an acrylate resin, a methacrylate resin, an aromatic vinyl resin, a vinyl cyanide resin, etc.; and the like. The average particle size of the organic filler is preferably 0.1 to 10 μm, more preferably 0.2 to 5 μm, even more preferably 0.5 to 4.0 μm, and particularly preferably 1.5 to 4.0 μm.
[0050] When the resin sheet of the present embodiment contains the organic filler (C), the content thereof is not particularly limited, but is preferably 1 to 30% by volume, more preferably 3 to 25% by volume, and even more preferably 5 to 20% by volume, based on the total amount of the resin sheet.
[0051] ((D) Thermal Polymerization Initiator) The resin sheet of the present embodiment may further contain a thermal polymerization initiator as component (D). The thermal polymerization initiator is not particularly limited, and examples thereof include hydroperoxide compounds such as diisopropylbenzene hydroperoxide "Percumyl P" (trade name, manufactured by NOF Corporation (the same applies hereinafter)), cumene hydroperoxide "Percumyl H", and t-butyl hydroperoxide "Perbutyl H"; α,α-bis(t-butylperoxy-m-isopropyl)benzene "Perbutyl P", dicumyl peroxide "Percumyl D", 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane "Perhexa 25B", t-butylcumyl peroxide "Perbutyl C", di-t-butyl peroxide "Perbutyl ... Examples of suitable peroxides include dialkyl peroxide compounds such as n-butyl-2,5-bis(t-butylperoxy)hexyne-3 "Perhexyne 25B" and t-butylperoxy-2-ethylhexanoate "Perbutyl O"; ketone peroxide compounds; peroxyketal compounds such as n-butyl 4,4-di-(t-butylperoxy)valerate "Perhexa V"; diacyl peroxide compounds; peroxydicarbonate compounds; organic peroxides such as peroxyester compounds; and azo compounds such as 2,2'-azobisisobutylnitrile, 2,2'-azobis(2-cyclopropylpropionitrile), and 2,2'-azobis(2,4-dimethylvaleronitrile). Among these, α,α-bis(t-butylperoxy-m-isopropyl)benzene "Perbutyl P" is preferred.
[0052] When the resin sheet of this embodiment contains a thermal polymerization initiator (D), its content is not particularly limited, but is preferably 0.01 to 5 mass%, more preferably 0.1 to 4 mass%, and even more preferably 0.5 to 3 mass%, based on the component (A). When the content of the thermal polymerization initiator (D) is equal to or greater than the lower limit, a sufficiently heat-cured resin sheet tends to be easily obtained, and when it is equal to or less than the upper limit, heat resistance tends to be good.
[0053] (Other Components) The resin sheet of this embodiment may further contain other components. Examples of other components include, but are not limited to, curing accelerators, flame retardants, flame retardant aids, peroxides, antioxidants, fluorescent brighteners, adhesion improvers, heat stabilizers, antistatic agents, UV absorbers, pigments, colorants, and lubricants. When the resin sheet of this embodiment contains other components, the content of each component is preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 1% by mass or less, based on the total amount of the resin sheet. It may be 0.1% by mass or more, or 0.5% by mass or more.
[0054] (Thickness of Resin Sheet) The thickness of the resin sheet of this embodiment is preferably the same as that of one sheet of prepreg conventionally used for printed wiring board applications, preferably 10 to 120 μm, more preferably 20 to 110 μm, and even more preferably 20 to 100 μm, and may be 40 to 100 μm or 60 to 100 μm. However, the thickness of the resin sheet of this embodiment is not limited to the above range.
[0055] (Method for Producing Resin Sheet) The resin sheet of this embodiment can be produced, for example, by applying a resin composition obtained by mixing the above-mentioned components and, if necessary, an organic solvent to a support, heating and drying the resin to bring it to a B-stage, and then peeling off the support. Herein, B-staging refers to bringing the resin to a B-stage state as defined in JIS K6900 (1994), and is also referred to as semi-curing. Examples of supports include polyolefin films such as polyethylene, polypropylene, and polyvinyl chloride; polyester films such as polyethylene terephthalate (hereinafter also referred to as "PET") and polyethylene naphthalate; various plastic films such as polycarbonate films and polyimide films; metal foils such as copper foil and aluminum foil; and release paper. The support may be subjected to a surface treatment such as a matte finish or a corona treatment. The support may also be subjected to a release treatment using a silicone resin-based release agent, an alkyd resin-based release agent, a fluororesin-based release agent, or the like. The thickness of the support is not particularly limited, but is preferably 10 to 150 μm, more preferably 25 to 80 μm.
[0056] There are no particular limitations on the method for applying the resin composition to the support, and application can be performed using a coating device known to those skilled in the art, such as a comma coater, bar coater, kiss coater, roll coater, gravure coater, or die coater. These coating devices may be selected appropriately depending on the thickness of the resin sheet to be produced. There are no particular limitations on the drying temperature or drying time after application of the resin composition, but examples include a method in which the resin composition is dried at 50 to 140°C for approximately 3 to 15 minutes. The drying temperature is preferably 70 to 135°C, more preferably 80 to 130°C. The drying time is preferably 3 to 12 minutes.
[0057] The resin sheet of this embodiment may have a protective film on one or both sides. By providing a protective film, it is possible to prevent scratches during transportation. Alternatively, the resin sheet of this embodiment may not have a protective film.
[0058] [Laminate, Metal-Clad Laminate] The laminate of this embodiment is a laminate including a cured resin sheet of this embodiment. A laminate including a metal foil is sometimes referred to as a metal-clad laminate. In other words, the metal-clad laminate of this embodiment is a metal-clad laminate including a metal foil and a cured resin sheet of this embodiment. The metal-clad laminate of this embodiment can be produced, for example, by placing metal foil on one or both sides of a single resin sheet of this embodiment, or by placing metal foil on one or both sides of a laminate sheet obtained by stacking two or more resin sheets of this embodiment (preferably 2 to 20 sheets, more preferably 2 to 10 sheets), and then hot-pressing and molding. Another method for producing a metal-clad laminate of this embodiment includes placing one or more resin films other than this embodiment on one or both sides of a single resin sheet of this embodiment, then placing metal foil, and then hot-pressing and pressing. In this case, when two or more resin films other than this embodiment are used, they may be the same resin film, or different resin films may be combined. The same resin film refers to a resin film having the same components, and a different resin film refers to a resin film having different components, and the same applies hereinafter. Here, as the resin film other than that of this embodiment, a known support-attached resin film used for multilayering of printed wiring boards can be used, and the same applies hereinafter. Another method for producing a metal-clad laminate of this embodiment includes a method in which one or more resin films other than that of this embodiment are placed on one or both sides of a laminate sheet obtained by stacking two or more resin sheets of this embodiment (preferably 2 to 20 sheets, more preferably 2 to 10 sheets), and then a metal foil is placed and heated and pressed. In this case, when two or more resin films other than that of this embodiment are used, they may be the same resin film, or different resin films may be combined.
[0059] The metal of the metal foil is not particularly limited as long as it is used in electrical insulating material applications, but from the viewpoint of electrical conductivity, it may be copper, gold, silver, nickel, platinum, molybdenum, ruthenium, aluminum, tungsten, iron, titanium, chromium, or an alloy containing one or more of these metal elements, with copper and aluminum being preferred, and copper being more preferred. The conditions for hot-press molding are not particularly limited, but can be, for example, a temperature of preferably 100 to 300°C, more preferably 150 to 250°C, even more preferably 180 to 240°C, a pressure of preferably 0.2 to 10 MPa, more preferably 1.5 to 6 MPa, and a time of preferably 0.1 to 5 hours, more preferably 1 to 3 hours. Furthermore, hot-press molding can be performed using a vacuum press or the like, preferably maintaining a vacuum state for 0.5 to 5 hours.
[0060] In the laminate and metal-clad laminate of this embodiment, the resin sheet is C-staged and cured. In other words, the laminate of this embodiment includes a C-staged resin sheet, and the metal-clad laminate of this embodiment can also be said to include a C-staged resin sheet and a metal foil. Here, C-staging in this specification refers to bringing the material into a C-stage state as defined in JIS K6900 (1994).
[0061] [Printed Wiring Board] The printed wiring board of this embodiment includes the laminate or metal-clad laminate of this embodiment. Here, the expression "including a laminate or metal-clad laminate" includes cases where the laminate or metal-clad laminate is itself, and cases where the laminate or metal-clad laminate has been subjected to circuit formation processing, such as drilling, metal plating, or metal foil etching. The printed wiring board of this embodiment can be manufactured by using the laminate of this embodiment, i.e., the metal-clad laminate, which has metal foil on one or both sides, and performing circuit formation processing, such as drilling, metal plating, or metal foil etching, by a known method, and further performing multi-layer processing as necessary.
[0062] [Semiconductor Package] The semiconductor package of this embodiment is a semiconductor package including the printed wiring board of this embodiment and a semiconductor element. The semiconductor package of this embodiment can be manufactured by mounting a semiconductor element such as a semiconductor chip or memory at a predetermined position on the printed wiring board of this embodiment and sealing the semiconductor element with a sealing resin or the like.
[0063] The resin sheet, laminate, printed wiring board, and semiconductor package of the present embodiment can be suitably used in electronic devices that handle high-frequency signals of 10 GHz or more. In particular, the printed wiring board is useful as a printed wiring board for millimeter-wave radar.
[0064] Although preferred embodiments have been described above, these are merely examples for explaining the present disclosure, and the scope of the present disclosure is not intended to be limited to these embodiments. The present disclosure also includes implementations in various forms different from the above-described embodiments, provided that they do not deviate from the gist of the disclosure.
[0065] The present embodiment will be specifically described below with reference to examples, although the present embodiment is not limited to the following examples.
[0066] Production Example 1: Production of vinylbenzyl resin A 500 mL reaction vessel equipped with a stirrer, thermometer, reflux condenser, and nitrogen inlet was charged with 35.6 parts by mass of indene, 101.2 parts by mass of chloromethylstyrene (a mixture of 50% by mass of m-isomer and 50% by mass of p-isomer), 7.1 parts by mass of tetra-n-butylammonium bromide (phase transfer catalyst), 0.1 parts by mass of phenothiazine (polymerization inhibitor), and 77.6 parts by mass of toluene (solvent), and heated and stirred at 40 ° C. while blowing in nitrogen at a flow rate of 50 ml / min. Next, 46.5 parts by mass of a 48% by mass aqueous sodium hydroxide solution was added dropwise over 20 minutes, and the mixture was further stirred at 60 ° C. for 9 hours. Note that blowing in nitrogen was continued during the reaction. The mixture was cooled to room temperature (25°C), neutralized with a 10% aqueous hydrochloric acid solution, washed twice with pure water, and the toluene was removed by distillation under reduced pressure. The resulting viscous liquid was washed with methanol and then vacuum dried to obtain vinylbenzyl resin A3-1. 1H-NMR analysis confirmed that the vinylbenzyl resin A3-1 had a structure in which substantially all of the two hydrogen atoms directly bonded to the carbon atom at position 1 of indene represented by the following formula (A3-1) had been substituted with vinylbenzyl groups. GPC analysis also revealed that the vinylbenzyl resin A3-1 was a mixture of one into which two vinylbenzyl groups had been introduced and one into which three vinylbenzyl groups had been introduced.
[0067]
[0068] Examples 1 to 10, Comparative Examples 1 to 4 (Preparation of Resin Sheets) A resin composition with a solids concentration of 60% by mass was prepared by stirring and mixing the components listed in Table 1 or Table 2 with toluene at room temperature (25°C) according to the blending amounts listed in Table 1 or Table 2. The prepared resin composition was applied to a 50 μm thick PET film (manufactured by Toyobo Co., Ltd., product name: Purex (registered trademark) A5300) and then heated and dried at 110°C for 5 minutes to B-stage the resin composition. As a result, a resin sheet (width 500 mm x length 500 mm, thickness 80 μm) with a PET film was obtained. For the resin sheet with the PET film, a corner of the PET film was grasped with tweezers and the PET film was slowly peeled from the resin sheet toward the other corner diagonally to obtain a bare resin sheet. (Preparation of Copper-Clad Laminates) Four or ten resin sheets obtained by the above method were stacked to form a laminate sheet. On top and bottom of the laminate sheet, 18 μm thick low-profile copper foil (manufactured by Mitsui Mining & Smelting Co., Ltd., product name: SI VSP AM 3R) was placed with its M side (matte side) in contact with the laminate sheet, and the resin sheet was heated and press-molded at a temperature of 230°C, a pressure of 2 MPa, and a time of 120 minutes to C-stage the resin sheet, thereby producing a double-sided copper-clad laminate (the double-sided copper-clad laminate using four resin sheets is referred to as "double-sided copper-clad laminate A," and the double-sided copper-clad laminate using ten resin sheets is referred to as "double-sided copper-clad laminate B").
[0069] [Evaluation and Measurement Methods] The resin sheets and copper-clad laminates obtained in the above Examples and Comparative Examples were subjected to measurements and evaluations according to the following methods. The results are shown in Table 1 or Table 2.
[0070] (1. Evaluation of Industrial Transportability) In each example, the resin sheet peeled from the PET film was adsorbed by a vacuum adsorption pad (diameter 20 mm, made of silicone) using an adsorption machine equipped with the vacuum adsorption pad, and then transported 500 mm in the horizontal direction. The degree of vacuum during adsorption during transport was -27 kPa. The state at that time was evaluated according to the following evaluation criteria and used as an index of industrial transportability. Evaluation A indicates excellent industrial transportability, Evaluation B indicates that the resin sheet can stand on its own even without a support, but the industrial transportability is insufficient, and Evaluation C indicates that the resin sheet cannot even stand on its own. A: The resin sheet was not destroyed even after being transported by the vacuum adsorption pad. B: The resin sheet was destroyed when the resin sheet was adsorbed by the vacuum adsorption pad or during transport. C: The resin sheet was destroyed when the PET film was peeled off.
[0071] (2. Measurement of Breaking Energy) Five evaluation resin sheets (10 mm wide x 40 mm long) were prepared from the resin sheet peeled from the PET film in each example, and a tensile test was performed in the length direction using an autograph (AG-X, manufactured by Shimadzu Corporation). Measurements were performed on each evaluation resin sheet under conditions of a measurement temperature of 25°C, a chuck distance of 20 mm, and a tensile speed of 10 mm / min. The breaking energy was calculated by integrating the stress from the origin of elongation (initial chuck distance) to the breaking point of each test piece (the amount of displacement when the test piece broke) with the displacement. The obtained breaking energy was divided by the volume of the test piece to obtain the breaking energy per unit volume (mJ / mm 3 The average value of five measurements was taken as the breaking energy of the resin sheet.
[0072] (3. Measurement of Breaking Vacuum Degree) For the resin sheet peeled from the PET film in each example, an arbitrary vacuum degree was set using an adsorption machine equipped with a vacuum adsorption pad (diameter 20 mm, made of silicone), and the sheet was then adsorbed by the vacuum adsorption pad for 3 seconds, after which the pressure was released to normal pressure, and the presence or absence of breakage in the sheet was confirmed visually. If no breakage in the sheet was observed, the vacuum degree was reset to a higher value and the same operation was performed at a different location from the previous time. The vacuum degree at which a break occurred in the adsorbed portion of the resin sheet (see Figure 1) was taken as the breaking vacuum degree. A breaking vacuum degree of -15 kPa or less (preferably -20 kPa or less, more preferably -30 kPa or less, and even more preferably -40 kPa or less) is preferable because it facilitates adsorption and transport using a vacuum adsorption pad for transport.
[0073] (4. Dielectric Properties: Measurement of Relative Permittivity and Dielectric Loss Tangent) The double-sided copper-clad laminate A obtained in each example was immersed in a 10% by mass solution of ammonium persulfate (manufactured by Mitsubishi Gas Chemical Company, Inc.), which is a copper etching solution, to remove the copper foil, and a 40 mm x 50 mm evaluation board was produced from the evaluation board. The relative permittivity and dielectric loss tangent were measured at 25°C in the 10 GHz band using a "PNA Network Analyzer N5227A" (manufactured by Agilent Technologies) equipped with a split post dielectric resonator (SPDR).
[0074] (5. Measurement of Thermal Expansion Coefficient) The double-sided copper-clad laminate B obtained in each example was immersed in a copper etching solution to remove the copper foil, thereby preparing a 5 mm square evaluation substrate. Thermomechanical analysis was performed using a thermomechanical measuring apparatus (TMA) [manufactured by TA Instruments Japan Co., Ltd., model number Q400] by compression. After the evaluation substrate was mounted in the apparatus in the X direction, measurements were performed twice consecutively under the measurement conditions of a load of 5 g and a heating rate of 10 ° C. / min. The average thermal expansion coefficient (average of the linear thermal expansion coefficient in the plane direction) from 50 ° C. to 120 ° C. in the second measurement was calculated, and this was used as the thermal expansion coefficient (linear thermal expansion coefficient). The results of the second measurement were used to improve accuracy.
[0075] (6. Measurement of Glass Transition Temperature (Tg)) The double-sided copper-clad laminate B obtained in each example was immersed in a copper etching solution to remove the copper foil, and a 5 mm square test piece was used to measure the glass transition temperature in accordance with the IPC (The Institute for Interconnecting and Packaging Electronic Circuits) standard using a thermomechanical analyzer (TMA) [manufactured by TA Instruments Japan, Ltd., model number Q400]. The higher the glass transition temperature, the better the heat resistance.
[0076]
[0077] The components listed in Table 1 or Table 2 are as follows: [Component (A)] (Component (A1)) Elastomer 1: styrene-ethylene-butylene-styrene copolymer (SEBS), styrene content 20% by mass, hydrogenation rate 100% by mole, Mn=70,000
[0078] (Component (A2)) Elastomer 2: 1,2-polybutadiene homopolymer, Mn=1,200 Elastomer 3: 1,2-polybutadiene homopolymer, Mn=3,200
[0079] (Component (A3)) Vinylbenzyl resin: Vinylbenzyl resin A3-1 obtained by Production Example 1
[0080] Unsaturated imide resin: an aromatic bismaleimide compound containing an indane ring and having the following structure: (In the above formula, n3 is a number from 0.95 to 10.0.)
[0081] [Component (B)] Silica: Silica having an average particle size of 1.0 μm treated with an aminosilane coupling agent [Component (D)] Thermal polymerization initiator 1: α,α-bis(t-butylperoxy-m-isopropyl)benzene (see structure below)
[0082] [Other ingredients] Flame retardant 1: 1,3-phenylenebis(di-2,6-xylenyl phosphate), phosphorus content 9% by mass
[0083] The number average molecular weight of the component (A) was measured according to the following method. (Method for measuring number average molecular weight (Mn)) The number average molecular weight was calculated by gel permeation chromatography (GPC) from a calibration curve using standard polystyrene. The calibration curve was approximated by a cubic equation using standard polystyrene: TSKstandard POLYSTYRENE (Types: A-2500, A-5000, F-1, F-2, F-4, F-10, F-20, F-40) [product name, manufactured by Tosoh Corporation]. The GPC measurement conditions are shown below. [GPC measurement conditions] Apparatus: High-speed GPC apparatus HLC-8320GPC Detector: Ultraviolet absorption detector UV-8320 [manufactured by Tosoh Corporation] Column: Guard column; TSK Guard column SuperHZ-L + column; TSKgel SuperHZM-N + TSKgel SuperHZM-M + TSKgel SuperH-RC (all product names manufactured by Tosoh Corporation) Column size: 4.6 x 20 mm (guard column), 4.6 x 150 mm (column), 6.0 x 150 mm (reference column) Eluent: Tetrahydrofuran Sample concentration: 10 mg / 5 mL Injection volume: 25 μL Flow rate: 1.00 mL / min Measurement temperature: 25°C
[0084] As is clear from the results shown in Tables 1 and 2, the resin sheets produced in the examples satisfy the following: (1) they can withstand suction and transport by a vacuum suction pad for transport, (2) they have low thermal expansion, (3) their relative dielectric constant (Dk) is within the range of 2.50 to 3.30 in the high frequency band of 10 GHz or higher, and (4) their dielectric loss tangent (Df) is 0.0020 or less in the high frequency band of 10 GHz or higher. Furthermore, it can be seen that the resin sheets produced in the examples have a breaking vacuum of -15 kPa or less, making them easy to suction and transport by a vacuum suction pad for transport, and also have good heat resistance. On the other hand, the breaking energy is 0.1 mJ / mm 3 The resin sheets of Comparative Examples 1 to 3, in which the content of component (A1) was increased to make the resin sheet more self-supporting, had very poor industrial transportability. Also, in Comparative Example 4, in which the content of component (A1) was increased to 72% by mass, the silica content was high, resulting in a small breaking energy and insufficient industrial transportability.
Claims
1. A resin sheet containing (A) a resin component and (B) an inorganic filler, wherein the (A) component contains (A1) an elastomer with a number average molecular weight of 10,000 or more, the content of the (B) component is 25 to 70 volume % based on the total amount of the resin sheet, and the breaking energy is 0.1 mJ / mm 3 This is the resin sheet.
2. The resin sheet according to claim 1, wherein the component (A1) comprises at least one member selected from the group consisting of styrene-based elastomers, maleimide-based elastomers, olefin-based elastomers, urethane-based elastomers, polyester-based elastomers, polyamide-based elastomers, acrylic-based elastomers, silicone-based elastomers, and derivatives thereof.
3. The resin sheet according to claim 1, further comprising (A2) an elastomer having a number average molecular weight of less than 10,000.
4. The resin sheet according to claim 1, wherein the component (A) further comprises (A3) a thermosetting resin.
5. The resin sheet according to claim 4, wherein the component (A3) comprises one or more resins selected from the group consisting of epoxy resins, phenolic resins, unsaturated imide resins, cyanate resins, isocyanate resins, benzoxazine resins, oxetane resins, amino resins, unsaturated polyester resins, allyl resins, vinylbenzyl resins, dicyclopentadiene resins, silicone resins, triazine resins, modified polyphenylene ether resins and melamine resins.
6. The resin sheet according to claim 4, wherein the total content of the (A1) component and the (A2) component is 40 to 95 mass % based on the (A) component.
7. The resin sheet according to claim 1, which does not contain an organic solvent, or if it contains an organic solvent, the content thereof is less than 1 mass % based on the total amount of the resin sheet.
8. The resin sheet according to claim 1, which does not contain glass fibers, or if it contains glass fibers, the content of glass fibers is 10 volume % or less based on the total amount of the resin sheet.
9. The resin sheet according to claim 1, which breaks when adsorbed by a silicone vacuum adsorption pad having a diameter of 20 mm at a vacuum level of -15 kPa or less.
10. A laminate comprising the cured resin sheet according to claim 1.
11. A metal-clad laminate comprising a metal foil and the cured resin sheet according to claim 1.
12. A printed wiring board comprising the laminate according to claim 10 or the metal-clad laminate according to claim 11.
13. A semiconductor package comprising the printed wiring board according to claim 12 and a semiconductor element.
Citation Information
Patent Citations
Thermoplastic elastomer composition
JP2004204180A
Organic-inorganic composite material, optical component and material composition
JP2009040819A
Resin composition, prepreg, laminate, resin film, multilayer printed wiring board and semiconductor package
JP2021176926A
Maleimide resin composition, prepreg, resin film, laminate, multilayer printed wiring board, and semiconductor package
JP2022122542A
Substrate, printed wiring board and semiconductor package
JP2023179316A