Metal separator and method for manufacturing same

The metal separator plate, with a porous body and selective surface modification, addresses the cost and performance challenges in fuel cell applications by ensuring excellent corrosion resistance and electrical conductivity at a lower cost.

WO2024219558A1PCT designated stage expired Publication Date: 2024-10-24HYUNDAE STEEL CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2023/012824
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-17
Filing Date
2023-08-29
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

The manufacturing of metal separator plates for fuel cells faces challenges in achieving excellent corrosion resistance and electrical conductivity at a low cost, particularly during the surface modification process.

Method used

A metal separator plate is manufactured using a first base material with a porous body laminated on its surface, where the porous body contains specific compositions and has a surface modification layer only on its upper surface, not on the inner surface of the holes, enhancing corrosion resistance and electrical conductivity.

Benefits of technology

The solution secures excellent corrosion resistance and electrical conductivity while reducing manufacturing costs, as demonstrated by the contact resistance and current density measurements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2023012824_24102024_PF_FP_ABST
    Figure KR2023012824_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to a metal separator and a method for manufacturing same. The metal separator and the method for manufacturing same, according to the present application, make it possible to ensure, at a low cost, excellent corrosion resistance and electrical conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Metal separator and manufacturing method thereof

[0001] This application relates to a metal separator and a method for manufacturing the same.

[0002] Recently, to combat global warming, powertrains are shifting from internal combustion engines (ICEs) to electric vehicles (EVs) and hydrogen fuel cell vehicles (FCEVs). Fuel cells used in FCEVs not only power industrial, household, and vehicular applications, but also power small electronic devices such as portable devices. Their applications are expanding as a highly efficient, clean energy source, contributing to both energy conservation and environmental protection.

[0003] A fuel cell is a type of power generation device that converts the chemical energy of fuel into electrical energy through an electrochemical reaction within a stack. It generates power by utilizing the energy generated by the combination reaction of hydrogen and oxygen. Specifically, a fuel cell can use hydrogen gas or a substance capable of producing hydrogen as fuel, and the oxidation reaction of the fuel produces hydrogen ions (protons) and electrons. These hydrogen ions and electrons then undergo an electrochemical reaction with oxygen in the air, producing water and generating electrical energy from the electron flow.

[0004] These hydrogen fuel cells are composed of a membrane electrode assembly, a gas diffusion layer (GDL), and a metal separator.

[0005] Among these components, the metal separator must separate hydrogen, oxygen, and coolant, and distribute and supply them evenly across the entire membrane electrode assembly to ensure smooth electrochemical reactions. Therefore, the required properties of the metal separator material include, in addition to low cost, excellent processability, excellent mechanical strength, high electrical conductivity, low gas permeability, thermal conductivity, and chemical stability.

[0006] The shape of the metal separator can be broadly divided into two parts: a reaction section formed in the center and a manifold section formed on each side of the reaction section.

[0007] Since the reaction section of the metal separator is in contact with the membrane electrode assembly or gas diffusion layer, flow channels can be formed to guide the flow of hydrogen, oxygen, and coolant. To enhance the function of these flow channels, a porous body with multiple holes can be attached to manufacture the metal separator with a two-layer structure.

[0008] Meanwhile, metal separators are undergoing surface modification to improve corrosion resistance and conductivity. However, the process of surface modification has raised manufacturing costs.

[0009] Therefore, to solve these problems, a metal separator and a method for manufacturing the same that can secure excellent corrosion resistance and electrical conductivity at low cost are required.

[0010] The object of this application is to provide a metal separator and a method for manufacturing the same that can secure excellent corrosion resistance and electrical conductivity at low cost.

[0011] In order to solve the above problem, the metal separator of the present application includes a first base material; and a porous body laminated on the upper surface of the first base material, wherein the porous body has a plurality of holes and a surface portion existing between the plurality of holes, a surface modification layer is formed on the upper surface of the surface portion, and the surface modification layer is not formed on the inner surface of the hole.

[0012] The above porous body may contain 18.00 to 23.00 wt% of chromium, 0.10 wt% or less of carbon, 1.00 wt% or less of silicon, 2.00 wt% or less of manganese, 0.50 wt% or less of titanium, 1.00 wt% or less of copper, the remainder being iron and other unavoidable impurities.

[0013] Additionally, the surface modification layer may include 5 at% to 14 at% of chromium in a region extending from the externally exposed surface to a depth of 1.0 nm.

[0014] Additionally, the surface modification layer may contain 25 at% to 35 at% of iron in a region extending from the externally exposed surface to a depth of 1.0 nm.

[0015] Additionally, each of the above holes may have a passive film formed on the inside.

[0016] In addition, the porous body has a contact resistance of 17 mΩ·cm under a contact pressure of 1.0 MPa. 2 It could be as follows:

[0017] In addition, the porous body has a voltage of 0.6 V vs SCE At a potential of , the current density is 15 ㎂ / cm 2 It could be as follows:

[0018] Additionally, the first parent material may include a first manifold section, a second manifold section, and a reaction section provided between the first manifold section and the second manifold section.

[0019] Additionally, the fuel cell of the present application includes the metal separator.

[0020] In addition, the method for manufacturing a metal separator of the present application includes a preparation step of preparing first and second base materials, respectively; a surface modification layer forming step of modifying an externally exposed surface of the second base material to form a surface modification layer on the exposed surface of the second base material; a porous body piercing step of forming a porous body having a plurality of holes and a surface portion existing between the plurality of holes by punching the second base material on which the surface modification layer has been formed; and a laminate forming step of laminating the porous body on the center of the first base material and bonding it to form a laminate, wherein the surface modification layer may be formed on an upper surface of the surface portion, and the surface modification layer may not be formed on an inner surface of the hole.

[0021] In addition, the second parent material may contain 18.00 to 23.00 wt% of chromium, 0.10 wt% or less of carbon, 1.00 wt% or less of silicon, 2.00 wt% or less of manganese, 0.50 wt% or less of titanium, 1.00 wt% or less of copper, the remainder of iron, and other unavoidable impurities.

[0022] In addition, the surface modification layer forming step may include a first modification step of preparing a solution in which at least one selected from fluorine, hydrochloric acid, and phosphoric acid is added to a sulfuric acid solution, and immersing the surface of the second base material in the solution; and a second modification step of immersing the second base material that has undergone the first modification step in a solution containing hydrogen peroxide and fluorine.

[0023] In addition, the method for manufacturing the metal separator may further include a slitting step of slitting the width of each of the prepared first base material and the second base material on which the surface modification layer is formed.

[0024] Additionally, the porous body that has undergone the porous body piercing step may have a passive film formed on the inner surface of the hole.

[0025] In addition, the method for manufacturing the metal separator may further include a manifold piercing step of forming a first manifold part and a second manifold part, each including a plurality of openings, by piercing both sides of one side of the first base material prepared above.

[0026] According to the metal separator of the present application and its manufacturing method, excellent corrosion resistance and electrical conductivity can be secured at low cost.

[0027] FIG. 1 is a top view illustrating an example of a metal separator according to one embodiment of the present application.

[0028] Fig. 2 is a side view illustrating an example of a metal separator according to one embodiment of the present application.

[0029] Hereinafter, the metal separator of the present application will be described with reference to the attached drawings. The attached drawings are exemplary, and the metal separator of the present application is not limited to the attached drawings.

[0030] Fig. 1 is a top view illustrating a metal separator according to one embodiment of the present application. As shown in Fig. 1, the metal separator of the present application includes a first base material (110) and a porous body (120). According to the metal separator of the present application, excellent corrosion resistance and electrical conductivity can be secured at low cost.

[0031] The above first parent material (110) is a material used for a metal separator for a fuel cell, and may include a first manifold part (111), a second manifold part (112), and a reaction part (113) provided between the first manifold part (111) and the second manifold part (112).

[0032] The first manifold part (111) and the second manifold part (112) are parts that supply hydrogen and air to the first base material (110) so that an electrochemical reaction can occur in the separator, respectively, and may each have a plurality of openings and a surface part existing between the plurality of openings. Specifically, the first manifold part (111) and the second manifold part (112) are formed with hydrogen and air inlets and outlets for supplying and discharging hydrogen and air, respectively, and are formed with cooling water inlets and outlets for controlling the operating temperature, and each surface part may exist between each inlet and outlet. In one embodiment, the first manifold part (111) is formed at one end with respect to the longitudinal direction of the first base material (110), and a hydrogen inlet, a cooling water outlet, and an air outlet may be formed along a width direction perpendicular to the longitudinal direction of the first base material (110), and a surface part may exist between the hydrogen inlet, the cooling water outlet, and the air outlet, respectively. In addition, the second manifold part (112) is formed at the other end with respect to the longitudinal direction of the first base material (110), and an air inlet, a cooling water inlet, and a hydrogen outlet may be formed along a width direction perpendicular to the longitudinal direction of the first base material (110), and a surface part may exist between the air inlet, the cooling water inlet, and the hydrogen outlet, respectively. At this time, the number of the openings is not particularly limited as long as it is two or more, and thus the upper limit is not particularly limited. In this specification, the term "manifold section" is used to refer to both the first manifold section and the second manifold section. Furthermore, the longitudinal direction refers to the direction from one end to the other end of the first parent material (110). Furthermore, the width direction refers to a direction perpendicular to the longitudinal direction.

[0033] In one example, the first manifold part (111) and the second manifold part (112) may have a surface modification layer or a passive film formed on the upper surface of the surface part and the inner surface of the opening part, respectively. When a surface modification layer is formed on the upper surface of the surface part and / or the inner surface of the opening part provided in each of the first manifold part (111) and the second manifold part (112), excellent corrosion resistance and electrical conductivity of the manifold part can be secured. In addition, when a passive film is formed on the upper surface of the surface part and / or the inner surface of the opening part provided in each of the first manifold part (111) and the second manifold part (112), oxygen can be blocked from penetrating into the interior of the first base material (110), thereby preventing rust from occurring.

[0034] In addition, the first base material (110) may include 18.00 wt% to 23.00 wt% of chromium, 0.10 wt% or less of carbon, 1.00 wt% or less of silicon, 2.00 wt% or less of manganese, 0.50 wt% or less of titanium, 1.00 wt% or less of copper, the remainder iron, and other unavoidable impurities. In one embodiment, the first base material (110) may include about 18.00 wt% to about 23.00 wt% of chromium, about 0.10 wt% or less of carbon, about 1.00 wt% or less of silicon, about 2.00 wt% or less of manganese, about 0.50 wt% or less of titanium, about 1.00 wt% or less of copper, the remainder iron, and other unavoidable impurities. Specifically, the first base material (110) may have an upper limit of a chromium content of about 22.00 wt% or less or about 21.00 wt% or less, and a lower limit of a chromium content of about 19.00 wt% or more or about 20.00 wt% or more. In addition, the first base material (110) may have a lower limit of a carbon content of about 0.01 wt% or more, a lower limit of a silicon content of about 0.30 wt% or more, a lower limit of a manganese content of about 0.30 wt% or more, a lower limit of a titanium content of about 0.20 wt% or more, and a lower limit of a copper content of about 0.30 wt% or more. Since the first base material (110) is made of stainless steel containing chromium having the aforementioned content, when the surface is exposed to the outside, a very thin Cr2O3 passive film having a thickness of 1 nm to 5 nm, in one embodiment, about 1 nm to about 5 nm, can be naturally formed on the surface, and when the passive film is modified, a surface modification layer can be formed. At this time, since the physical properties of each component included in the first base material (110) are known in the art, they will be omitted.

[0035] In one example, the first base material (110) may further include at least one selected from among 0.04 wt% or less of phosphorus, 0.03 wt% or less of sulfur, and 0.30 wt% or less of niobium. In one embodiment, the first base material (110) may further include at least one selected from about 0.04 wt% or less of phosphorus, about 0.03 wt% or less of sulfur, and about 0.30 wt% or less of niobium. The lower limits of phosphorus, sulfur, and niobium are not particularly limited, and for example, each may be about 0 wt% or more.

[0036] In another example, the thickness of the first base material (110) may be from 0.05 mm to 1 mm, and in one embodiment, from about 0.05 mm to about 1 mm. By having a thickness within the aforementioned range, the first base material (110) can achieve excellent mechanical strength and gas permeability.

[0037] The above reaction section (113) is a section where an electrochemical reaction occurs by hydrogen and air supplied and discharged through the first manifold section (111) and the second manifold section (112), respectively, and the porous body (120) is laminated on the upper surface. The shape of the reaction section (113) is not particularly limited, and as an example, it may be in the form of a flat plate. By laminating the porous body (120) on the reaction section (113) in the form of a flat plate, a separate flow path forming process may not be required. A separator having the shape of the reaction section (113) can be applied and used to both the hydrogen electrode and the air electrode.

[0038] The porous body (120) is a channel having a microporous structure in a porous shape, in which the aforementioned electrochemical reaction occurs, and is laminated on the upper surface of the first base material (110), specifically, on the upper surface of the reaction section (113). At this time, the porous body (120) may have an area corresponding to the reaction section (113) of the first base material (110). In this specification, the term "corresponding area" means the same area. The porous body (120) may be laminated on the upper surface of the reaction section (113) of the first base material (110), thereby improving the function of a hydrogen or air channel.

[0039] In addition, the porous body (120) includes 18.00 wt% to 23.00 wt% of chromium, 0.10 wt% or less of carbon, 1.00 wt% or less of silicon, 2.00 wt% or less of manganese, 0.50 wt% or less of titanium, 1.00 wt% or less of copper, the remainder iron, and other unavoidable impurities. In one embodiment, the porous body (120) may include about 18.00 wt% to about 23.00 wt% of chromium, about 0.10 wt% or less of carbon, about 1.00 wt% or less of silicon, about 2.00 wt% or less of manganese, about 0.50 wt% or less of titanium, about 1.00 wt% or less of copper, the remainder iron, and other unavoidable impurities. Specifically, the porous body (120) may have an upper limit of a chromium content of about 22.00 wt% or less or about 21.00 wt% or less, and a lower limit of a chromium content of about 19.00 wt% or more or about 20.00 wt% or more. In addition, the porous body (120) may have a lower limit of a carbon content of about 0.01 wt% or more, a lower limit of a silicon content of about 0.30 wt% or more, a lower limit of a manganese content of about 0.30 wt% or more, a lower limit of a titanium content of about 0.20 wt% or more, and a lower limit of a copper content of about 0.30 wt% or more. The porous body (120) includes the above-described components, and in particular, by lowering a chromium content while increasing an iron content, excellent corrosion resistance and electrical conductivity can be secured at a low cost. At this time, since the properties of each component included in the porous body (120) are known in the art, they will be omitted.

[0040] In one example, the porous body (120) may further include at least one selected from 0.04 wt% or less of phosphorus, 0.03 wt% or less of sulfur, and 0.30 wt% or less of niobium. In one embodiment, the porous body (120) may further include at least one selected from about 0.04 wt% or less of phosphorus, about 0.03 wt% or less of sulfur, and about 0.30 wt% or less of niobium. The lower limits of phosphorus, sulfur, and niobium are not particularly limited, and for example, each may be about 0 wt% or more.

[0041] FIG. 2 is a side view exemplarily showing a metal separator according to one embodiment of the present application. As shown in FIG. 2, the porous body (120) has a plurality of holes (121) and a surface portion (122) respectively existing between the plurality of holes (121), and a surface modification layer (123) is formed on the upper surface of each surface portion (122) provided in the porous body (120), and no surface modification layer is formed on the inner surface of the hole (121) provided in the porous body (120). At this time, the number of holes provided in the porous body (120) is not particularly limited as long as it is two or more, and thus the upper limit is not particularly limited. Even if the surface modification layer (123) described above is formed only on the upper surface of the surface portion (122), the porous body (120) can secure excellent corrosion resistance and electrical conductivity.

[0042] In one example, the surface modification layer (123) may contain chromium in an amount of 5 at% to 14 at% in a region from the externally exposed surface to a depth of 1.0 nm, and in one embodiment, may contain about 5 at% to about 14 at%, specifically, may contain about 7 at% to about 13 at% or about 9 at% to about 11 at%. By containing chromium in the aforementioned amount in a region from the externally exposed surface to a depth of 1.0 nm in the surface modification layer (123), excellent corrosion resistance and electrical conductivity can be secured at a low cost. At this time, the chromium content of the surface modification layer (123) can be measured using an EDAX device.

[0043] In another example, the surface modification layer (123) may include iron in an amount of 25 at% to 35 at% in a region from the externally exposed surface to a depth of 1.0 nm, and in one embodiment, may include iron in an amount of about 25 at% to about 35 at%, specifically, may include iron in an amount of about 27 at% to about 33 at% or about 29 at% to about 31 at%. By including iron in the aforementioned amount in a region from the externally exposed surface to a depth of 1.0 nm, the surface modification layer (123) may secure excellent corrosion resistance and electrical conductivity of the porous body at a low cost. At this time, the iron content of the surface modification layer (123) may be measured using an EDAX device.

[0044] The plurality of holes (121) may have a short axis length formed in a direction parallel to the air flow direction and a long axis length formed in a direction perpendicular to the air flow direction. For example, the short axis length may have a length of 0.3 mm to 1.0 mm, and in one embodiment, about 0.3 mm to about 1.0 mm. In addition, the long axis length may have a length of 1.0 mm to 2.0 mm, and in one embodiment, about 1.0 mm to 2.0 mm. Since the plurality of holes (121) each have the aforementioned length, the role of a hydrogen or air flow path may be improved.

[0045] In one example, each hole (121) provided in the porous body (120) may have a passive film (124) formed on the inner surface thereof. Specifically, each surface portion (122) provided in the porous body (120) may have a passive film (124) formed on a surface adjacent to a plurality of holes (121). That is, even if the metal separator of the present application forms the surface modification layer (123) described above only on the upper surface of the surface portion (122) provided in the porous body (120), it can secure excellent corrosion resistance and electrical conductivity due to the low chromium content and the high iron content. At this time, the passive film (124) may be formed by natural oxidation of the surface of the porous body (120) on which the surface modification layer (123) is not formed. Specifically, when the base material is made of stainless steel containing 12 wt% or more of chromium, and in one embodiment, about 12 wt% or more, a very thin Cr2O3 passive film having a thickness of 1 nm to 5 nm, and in one embodiment, about 1 nm to about 5 nm, can be naturally formed on the surface of the base material. As a result, the porous body (120) can have the aforementioned passive film formed on the inner surface of the hole (121). By forming the passive film on the inner surface of the hole (121) provided in the porous body (120), oxygen can be blocked from penetrating into the porous body (120) on which the passive film is formed, thereby preventing rust from occurring.

[0046] The surface modification layer (123) provided on the porous body (120) may have a thickness of 5 nm or less. In one embodiment, the surface modification layer (123) provided on the porous body (120) may have a thickness of about 5 nm or less. Specifically, the thickness of the surface modification layer (123) provided on the porous body (120) may be about 4 nm or less or about 3 nm or less. In addition, the lower limit of the thickness of the surface modification layer (123) provided on the porous body (120) may be about 1 nm or more. Since the surface modification layer (123) provided on the porous body (120) has the aforementioned thickness, excellent corrosion resistance and electrical conductivity can be secured at a low cost.

[0047] In one example, the porous body (120) has a contact resistance of 17 mΩ·cm under a contact pressure of 1.0 MPa. 2 It may be as follows. In one embodiment, the porous body (120) has a contact resistance of about 17 mΩ·cm under a contact pressure of 1.0 MPa. 2 It may be below. The porous body (120) may have excellent electrical conductivity since the contact resistance measured under the aforementioned contact pressure has the aforementioned range. In addition, the lower the contact resistance of the porous body (120) measured under the aforementioned contact pressure, the better the electrical conductivity, and therefore, the lower limit is not particularly limited, but, for example, about 1 mΩ cm. 2 It can be ideal, specifically, about 3 mΩ·cm 2 Above, about 5 mΩ·cm 2 Above, about 10 mΩ·cm 2 Ideal or about 15 mΩ·cm 2 It could be strange.

[0048] In another example, the porous body (120) is 0.6 V vs SCE At a potential of , the current density is 15 ㎂ / cm 2 may be less than or equal to 0.6 V. In one embodiment, the porous body (120) is vs SCE At a potential of , the current density is approximately 15 ㎂ / cm2 It may be below. The porous body (120) may have excellent corrosion resistance since the current density measured at the above-mentioned potential has the above-mentioned range. In addition, the lower limit of the current density of the porous body (120) measured at the above-mentioned potential is not particularly limited in that the lower the current density, the better the corrosion resistance. For example, it may be about 1 ㎂ / cm. 2 It can be ideal, specifically, about 3 ㎂ / cm 2 Ideally, about 5 ㎂ / cm 2 Ideal, about 10 ㎂ / cm 2 or more than about 14 ㎂ / cm 2 It could be strange.

[0049] The present application also relates to a fuel cell. The fuel cell relates to a fuel cell including the aforementioned metal separator. Since the specific details of the metal separator described below are equally applicable to the description of the metal separator, they will be omitted.

[0050] The fuel cell cell includes the aforementioned metal separator. By including the aforementioned metal separator, the fuel cell can perform a smooth electrochemical reaction of the membrane electrode assembly and can smoothly function as an electrical path.

[0051] The fuel cell may include two of the aforementioned metal separators, and a first gas diffusion layer, a membrane electrode assembly, and a second gas diffusion layer may be provided between the two metal separators. At this time, the first gas diffusion layer, the membrane electrode assembly, and the second gas diffusion layer may be any type known in the art without limitation, and are not particularly limited.

[0052] The present application also relates to a method for manufacturing a metal separator. The method for manufacturing the metal separator relates to a method for manufacturing the aforementioned metal separator. Since the specific details of the metal separator described below are equally applicable to the metal separator described above, they will be omitted.

[0053] The method for manufacturing a metal separator of the present application comprises a preparation step, a surface modification layer formation step, a porous body piercing step, and a laminate formation step. According to the method for manufacturing a metal separator of the present application, a metal separator with improved corrosion resistance and electrical conductivity of a porous body can be manufactured at low cost.

[0054] The above preparation step is a step of preparing the first and second base materials, respectively.

[0055] For example, the second base material may include 18.00 wt% to 23.00 wt% chromium, 0.10 wt% or less carbon, 1.00 wt% or less silicon, 2.00 wt% or less manganese, 0.50 wt% or less titanium, 1.00 wt% or less copper, the remainder iron, and other unavoidable impurities. In one embodiment, the second base material may include about 18.00 wt% to about 23.00 wt% chromium, about 0.10 wt% or less carbon, about 1.00 wt% or less silicon, about 2.00 wt% or less manganese, about 0.50 wt% or less titanium, about 1.00 wt% or less copper, the remainder iron, and other unavoidable impurities. Specifically, the second base material may have an upper limit of a chromium content of about 22.00 wt% or less or about 21.00 wt% or less, and a lower limit of a chromium content of about 19.00 wt% or more or about 20.00 wt% or more. In addition, the second base material may have a lower limit of a carbon content of about 0.01 wt% or more, a lower limit of a silicon content of about 0.30 wt% or more, a lower limit of a manganese content of about 0.30 wt% or more, a lower limit of a titanium content of about 0.20 wt% or more, and a lower limit of a copper content of about 0.30 wt% or more. By including the above-described components, a naturally very thin Cr2O3 passive film having a thickness of about 1 nm to about 5 nm, in one embodiment, about 1 nm to about 5 nm, may be formed on the surface.

[0056] In addition, the second base material may further include at least one selected from among 0.04 wt% or less of phosphorus, 0.03 wt% or less of sulfur, and 0.30 wt% or less of niobium. In one embodiment, the second base material may further include at least one selected from about 0.04 wt% or less of phosphorus, about 0.03 wt% or less of sulfur, and about 0.30 wt% or less of niobium. The lower limits of phosphorus, sulfur, and niobium are not particularly limited, and for example, each may be about 0 wt% or more.

[0057] In one example, the first base material may comprise the same components as the second base material. By comprising the same components as the second base material, a naturally very thin Cr2O3 passive film may be formed on the surface, with a thickness of 1 nm to 5 nm, in one embodiment, about 1 nm to about 5 nm.

[0058] In one example, the method for manufacturing the metal separator may further include a cold rolling step. Specifically, the cold rolling step may be a step of forming the first and second base materials by passing them between two rolls that rotate below a recrystallization temperature, and may be performed in the preparation step. By further including the cold rolling step, the method for manufacturing the metal separator may improve the dimensional accuracy and mechanical properties of the first and second base materials. At this time, when performing each step in the method for manufacturing the metal separator, if the first and / or second base materials are exposed to the outside, a passive film may be formed on the surface of each of the first and / or second base materials by natural oxidation. Specifically, since each of the first and second base materials is made of stainless steel containing chromium having the aforementioned content, a naturally very thin Cr2O3 passive film having a thickness of 1 nm to 5 nm, in one embodiment, about 1 nm to about 5 nm, can be formed.

[0059] The above-described surface modification layer forming step is a step of forming a surface modification layer on the exposed surface of the second base material prepared in the above-described preparation step, and is performed by modifying the externally exposed surface of the second base material, specifically, the passive film formed on the surface of the second base material. The method for manufacturing a metal separator includes the above-described surface modification layer forming step, thereby enabling the manufacture of a metal separator with improved corrosion resistance and electrical conductivity of a porous body at low cost.

[0060] In one example, the surface modification layer forming step may include a first modification step and a second modification step.

[0061] The above first modification step is a step of removing a passive film formed on the surface of the second base material and reconstituting chemical components, and can be performed by preparing a solution in which at least one selected from fluorine, hydrochloric acid, and phosphoric acid is added to a sulfuric acid solution, and immersing the surface of the second base material in the solution. Specifically, the above first modification step can be performed by preparing a solution in which at least one selected from 1.0 mol to 5.0 mol of fluorine, 0.3 mol to 1.0 mol of hydrochloric acid, and 0.3 mol to 1.0 mol of phosphoric acid is added to a sulfuric acid solution having a concentration of 350 g / L or more, and immersing the surface of the second base material, specifically, the passive film formed on the surface of the second base material, in the solution at 40°C to 80°C for 10 seconds to 180 seconds. In one embodiment, the first modification step may be performed by preparing a solution in which at least one selected from among about 1.0 mol to about 5.0 mol of fluorine, about 0.3 mol to about 1.0 mol of hydrochloric acid, and about 0.3 mol to about 1.0 mol of phosphoric acid is added to a sulfuric acid solution having a concentration of about 350 g / L or more, and immersing the surface of the second base material, specifically, the passive film formed on the surface of the second base material, in the solution at about 40° C. to about 80° C. for about 10 seconds to about 180 seconds. The method for manufacturing the metal separator may include the first modification step, thereby improving the amount of iron hydroxide produced in the surface modification layer, thereby improving the corrosion resistance and electrical conductivity of the porous body. At this time, the ratio of the components included in the surface modification layer may be adjusted depending on the ratio of the components of the solution used in the first modification step and the immersion conditions.

[0062] The second modification step is a step for removing SMUT, which is a by-product that may be generated through the first modification step, and may be performed continuously after the first modification step, and may be performed by immersing the second base material that has undergone the first modification step in a solution containing hydrogen peroxide and fluorine. Specifically, the second modification step may be performed by immersing the second base material that has undergone the first modification step in a solution containing 1.0 mol to 5.0 mol of hydrogen peroxide and 1.0 mol to 5.0 mol of fluorine at 40°C to 80°C for 10 seconds to 180 seconds. In one embodiment, the second modification step may be performed by immersing the second base material subjected to the first modification step in a solution containing about 1.0 mol to about 5.0 mol of hydrogen peroxide and about 1.0 mol to about 5.0 mol of fluorine at about 40° C. to about 80° C. for about 10 seconds to about 180 seconds. The surface modification layer forming step may include the second modification step, thereby ensuring the cleanliness of the surface of the surface modification layer.

[0063] In one example, the method for manufacturing the metal separator may further include a slitting step. Specifically, the slitting step is a step of slitting each of the first base material prepared in the preparation step and the second base material on which the surface modification layer is formed through the surface modification layer forming step into a width suitable for application to the metal separator. For example, the width of each of the prepared first base material and the second base material on which the surface modification layer is formed may be divided into 1 / 4 through the slitting step. The method for manufacturing the metal separator of the present application may improve productivity by performing the surface modification layer forming step on the second base material before performing the slitting step, compared to a case where the surface modification layer forming step is performed after the slitting step.

[0064] The above porous body piercing step is a step of forming the second base material on which the surface modification layer is formed into a porous body having a plurality of holes and a surface portion existing between the plurality of holes, and is performed by punching the second base material on which the surface modification layer is formed, and the surface modification layer is formed on the upper surface of the surface portion provided in the porous body, and the surface modification layer is not formed on the inner surface of the hole provided in the porous body. At this time, a passive film may be formed by natural oxidation on the surface of the second base material exposed to the outside through the porous body piercing step. Specifically, the passive film may be formed on the inner surface of the hole of the porous body.

[0065] The method for manufacturing the above metal separator not only increases the production efficiency of the metal separator, but also allows for manufacturing a metal separator with improved corrosion resistance and electrical conductivity of the porous body at a low cost, even if the porous body piercing step is performed after the surface modification layer forming step, since the second base material includes the above-described component.

[0066] In one example, the method for manufacturing the metal separator may further include a three-dimensional molding step. The three-dimensional molding step is a step for forming air channels in the porous body, and may be performed by molding the porous body using a press. By further including the three-dimensional molding step, the method for manufacturing the metal separator may secure a three-dimensional air channel structure in the porous body that has undergone the three-dimensional molding step.

[0067] In another example, the method for manufacturing the metal separator may further include a manifold piercing step. The manifold piercing step is a step of forming a first manifold part and a second manifold part on the first base material prepared in the preparation step, and may be performed by perforating both side surfaces of one surface of the first base material on which the surface modification layer is formed through the surface modification layer forming step. The manifold piercing step may be performed after the slitting step or the porous body piercing step.

[0068] In one example, the surface modification layer forming step may further include modifying the exposed surface of the first base material to form a surface modification layer on the first base material. Specifically, the surface modification layer forming step for the first base material may be performed on the first base material prepared in the preparation step before the manifold piercing step, or may be performed on the first base material that has undergone the manifold piercing step. Since the method for forming the surface modification layer on the exposed surface of the first base material is identically applied to the method for forming the surface modification layer on the exposed surface of the second base material, it will be omitted. If the surface modification layer forming step for the first base material is performed before the manifold piercing step, after the manifold piercing step, a surface modification layer may be formed on the upper surface of the surface portion provided in each of the first manifold part and the second manifold part, and a passive film may be formed on the inner surface of the opening. In addition, when the step of forming a surface modification layer for the first base material is performed after the step of piercing the manifold, a surface modification layer can be formed on each of the upper surface of the surface portion and the inner surface of the opening provided in each of the first manifold and the second manifold.

[0069] The above laminate forming step is a step of forming a laminate composed of the first base material and a porous body having the upper surface of the surface portion and the inner surface of the hole as described above, and is performed by laminating and bonding the porous body to the center of the first base material. For example, the bonding method may use a laser welding or micro spot welding bonding method. The method for manufacturing the metal separator includes the above laminate forming step, thereby manufacturing a two-layer metal separator in which the porous body having the upper surface of the surface portion and the inner surface of the hole as described above is laminated on the first base material.

[0070]

[0071] Hereinafter, the present application will be described in more detail through examples according to the present application and comparative examples not according to the present application, but the scope of the present application is not limited by the examples presented below.

[0072]

[0073] Example 1

[0074] Manufacturing of metal separators

[0075] A first base material having a thickness of 0.1 mm and a second base material having a thickness of 0.08 mm, each composed of 21,000 wt% chromium, 0.010 wt% carbon, 0.130 wt% silicon, 0.170 wt% manganese, 0.024 wt% phosphorus, 0.024 wt% sulfur, 0.270 wt% titanium, 0.340 wt% copper, the remainder iron, and other unavoidable impurities, were prepared, and cold rolling was performed by passing each of the first base material and the second base material between two rotating rolls. At this time, the surfaces of each of the first base material and the second base material were naturally formed with a very thin Cr2O3 passive film having a thickness of 1 nm to 5 nm by natural oxidation.

[0076] Afterwards, a solution containing 3.0 mol of fluorine in a sulfuric acid solution having a concentration of 400 g / L was prepared, and the surfaces of each of the first and second base materials were immersed in the solution at a temperature of 60°C for 30 seconds for a first modification treatment, and then a second modification treatment was performed successively by immersing the surfaces in a solution containing 3.5 mol of hydrogen peroxide and 2.5 mol of fluorine at a temperature of 60°C for 60 seconds to form a surface modification layer having a thickness of 2 nm on the surfaces of each of the first and second base materials.

[0077] Afterwards, the widths of the first and second base materials, each having a surface modified layer formed thereon, were slit from 500 mm to 1 / 4 to divide them into 120 mm widths.

[0078] Thereafter, the second base material on which the surface modification layer was formed was pierced, and then three-dimensionally molded using a press to have a plurality of holes and a surface portion existing between the plurality of holes, and a surface modification layer was formed on the upper surface of the surface portion, and a porous body was formed in which a very thin Cr2O3 passive film having a thickness of 1 nm to 5 nm was naturally formed without forming a surface modification layer on the inner surface of the hole. At this time, during the three-dimensional molding, an unnecessary outer portion of the porous body was removed.

[0079] Thereafter, in the first base material on which the surface modification layer was formed, both sides of one side of the first base material were perforated to form a first manifold part and a second manifold part, each including a plurality of openings and a surface part existing between the plurality of openings.

[0080] Afterwards, the porous body was laminated on the center of the first base material, and joining was performed by laser welding to manufacture a metal separator in which the porous body was laminated on the first base material.

[0081]

[0082] Comparative Example 1

[0083] Manufacturing of metal separators

[0084] A metal separator was manufactured in the same manner as in Example 1, except that the first and second base materials were made of 30,000 wt% chromium, 0.006 wt% carbon, 0.144 wt% silicon, 0.200 wt% manganese, 0.016 wt% phosphorus, 0.001 wt% sulfur, 0.200 wt% titanium, 0.200 wt% niobium, and the remainder iron and other unavoidable impurities.

[0085]

[0086] Comparative Example 2

[0087] Manufacturing of metal separators

[0088] A metal separator was manufactured in the same manner as in Example 1, except that the first modification treatment and the second modification treatment were not performed. At this time, the manufactured metal separator had a naturally very thin Cr2O3 passive film with a thickness of 1 nm to 5 nm formed on the upper surface of the surface of the porous body and the inner surface of the hole, respectively.

[0089]

[0090] Experimental Example 1. Evaluation of the components of the surface modification layer and passive film.

[0091] Using energy dispersive spectroscopy (EDS), the components in the region up to a depth of 1.0 nm from the externally exposed surface of the surface modification layer or passive film formed on the upper surface of the surface of the porous body of the metal separator manufactured in the above examples and comparative examples were analyzed with an EDAX device, and the results are shown in Table 1 below.

[0092]

[0093] Experimental Example 2. Contact Resistance Evaluation

[0094] The contact resistance of the porous body of the metal separator manufactured in the examples and comparative examples was measured using a method of measuring current under a contact pressure of 1.0 MPa after inserting the metal separator manufactured in the examples and comparative examples between gas diffusion layers (Carbon paper type, SGL). The results are shown in Table 1 below.

[0095]

[0096] Experimental Example 3. Current Density Evaluation

[0097] The current density for the porous body of the metal separator manufactured in the examples and comparative examples was evaluated using the Tafel Slop of a potentiostat, and the dynamic potential was evaluated in a mixture of 0.1 N sulfuric acid and 2 ppm hydrofluoric acid heated to 80°C, and 0.6 V SCE The voltage was measured when applied, and the results are shown in Table 1 below.

[0098] Analysis of the components of the surface modification layer or passive film formed on the upper surface of the surface part of the porous body. Contact resistance (mΩ·cm) with or without the surface modification layer. 2 )Current density (㎂ / cm 2 ) Chrome (at%) Iron (at%) Surface of the porous body The inner surface of the hole provided in the porous body Example 11030OX1614 Comparative example 11520OX2010 Comparative example 2215XX3008

[0099] As shown in Table 1 above, the metal separator manufactured in Example 1 has a porous body with the desired current density and has lower contact resistance than the metal separators manufactured in Comparative Examples 1 and 2, so it was confirmed that it has excellent electrical conductivity and corrosion resistance.

[0100] In particular, since the metal separator manufactured in Example 1 has a lower chromium content in the porous body than the metal separator manufactured in Comparative Example 1, the manufacturing cost can also be reduced.

[0101] <Explanation of symbols>

[0102] 110: First Mother Material

[0103] 111: 1st manifold section

[0104] 112: Second manifold section

[0105] 113: Reaction section

[0106] 120: Porous body

[0107] 121: Hall

[0108] 122: Surface

[0109] 123: Surface modification layer

[0110] 124: Passive film

Claims

1. A first base material; and a porous body laminated on the upper surface of the first base material, The above porous body has a plurality of holes and a surface layer existing between the plurality of holes, A metal separator having a surface modification layer formed on the upper surface of the surface portion and having no surface modification layer formed on the inner surface of the hole.

2. In paragraph 1, The above porous body is a metal separator containing 18.00 to 23.00 wt% of chromium, 0.10 wt% or less of carbon, 1.00 wt% or less of silicon, 2.00 wt% or less of manganese, 0.50 wt% or less of titanium, 1.00 wt% or less of copper, the remainder being iron and other unavoidable impurities.

3. In paragraph 1, A metal separator having a surface modification layer comprising 5 at% to 14 at% of chromium in a region extending from the externally exposed surface to a depth of 1.0 nm.

4. In paragraph 1, A metal separator having a surface modification layer comprising 25 at% to 35 at% of iron in a region extending from the surface exposed to the outside to a depth of 1.0 nm.

5. In paragraph 1, Each of the above holes is a metal separator with a passive film formed on the inside.

6. In paragraph 1, The above porous body has a contact resistance of 17 mΩ·cm under a contact pressure of 1.0 MPa. 2 Below is the metal separator.

7. In paragraph 1, The above porous body is 0.6 V vs SCE At a potential of , the current density is 15 ㎂ / cm 2 Below is the metal separator.

8. In paragraph 1, The above first parent material is a metal separator including a first manifold section, a second manifold section, and a reaction section provided between the first manifold section and the second manifold section.

9. A fuel cell cell comprising a metal separator according to any one of claims 1 to 8.

10. Preparatory step of preparing the first and second parent materials respectively; A surface modification layer forming step of modifying the externally exposed surface of the second parent material to form a surface modification layer on the exposed surface of the second parent material; A porous body piercing step of forming a porous body having a plurality of holes and a surface layer existing between the plurality of holes by punching the second base material on which the surface modification layer is formed; and A laminate forming step is included, which comprises laminating the porous body at the center of the first parent material and bonding the porous body to form a laminate. A method for manufacturing a metal separator in which a surface modification layer is formed on the upper surface of the surface portion and no surface modification layer is formed on the inner surface of the hole.

11. In paragraph 10, A method for manufacturing a metal separator, wherein the second base material comprises 18.00 to 23.00 wt% of chromium, 0.10 wt% or less of carbon, 1.00 wt% or less of silicon, 2.00 wt% or less of manganese, 0.50 wt% or less of titanium, 1.00 wt% or less of copper, and the remainder being iron and other unavoidable impurities.

12. In paragraph 10, The above surface modification layer forming step comprises a first modification step of preparing a solution in which at least one selected from fluorine, hydrochloric acid, and phosphoric acid is added to a sulfuric acid solution, and immersing the surface of the second base material in the solution; and A method for manufacturing a metal separator, comprising a second modification step of immersing a second base material that has undergone the first modification step in a solution containing hydrogen peroxide and fluorine.

13. In paragraph 10, A method for manufacturing a metal separator, further comprising a slitting step of slitting the width of each of the prepared first base material and the second base material on which the surface modification layer is formed.

14. In paragraph 10, A method for manufacturing a metal separator in which a porous body having undergone the above porous body piercing step has a passive film formed on the inner surface of the hole.

15. In paragraph 10, A method for manufacturing a metal separator further comprising a manifold piercing step of forming a first manifold portion and a second manifold portion, each including a plurality of openings, by piercing both sides of one surface of the first base material prepared above.

Citation Information

Patent Citations

  • Stainless steel separator for polymer electrolyte fuel cell and polymer electrolyte fuel cell

    JP2006302731A

  • Gas- distributing plate for compact polymer electrolyte membrane fuel cell and separator plate using the said gas-distributing plate

    KR100429685B1

  • Bipolar plate for direct methanol fuel cell and method of manufacturing the same

    KR1020120072824A

  • Metal bipolar plate for pemfc and manufacturing method thereof

    KR1020160082632A

  • Paste For Solar Cell's Electrode And Solar Cell using the same

    KR102539382B1