Tri-metallic catalyst for ammonia cracking, preparation method therefor, and production method for hydrogen using same
A tri-metal catalyst using ruthenium, potassium, and yttrium on a delta-alumina support enhances ammonia conversion at low temperatures, addressing the inefficiencies of conventional catalysts and enabling cost-effective hydrogen production for low-temperature applications.
Patent Information
- Application Number
- PCT/KR2024/004144
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-17
- Filing Date
- 2024-04-01
- Publication Date
- 2024-10-24
AI Technical Summary
Conventional ammonia cracking catalysts require high temperatures to achieve high ammonia conversion rates, leading to increased energy costs and reduced economic efficiency, and are not suitable for low-temperature applications such as marine and small-scale ammonia co-fired power generation.
A tri-metal catalyst composition is developed using a low content of ruthenium combined with potassium and yttrium as auxiliary metals, supported on a delta-alumina catalyst with specific crystalline phase, optimized to enhance ammonia conversion rates at low temperatures by maximizing the active sites and reducing impurities like chlorine and nitrogen compounds.
The tri-metal catalyst achieves high ammonia conversion rates and hydrogen production efficiency at temperatures between 300-550 degrees Celsius, improving durability and reducing energy costs, making it suitable for low-temperature applications.
Smart Images

Figure KR2024004144_24102024_PF_FP_ABST
Abstract
Description
A triple metal catalyst for ammonia cracking reaction, a method for producing the same, and a method for producing hydrogen using the same
[0001] The present invention relates to a high-yield triple metal catalyst composition capable of stably producing hydrogen at low temperatures as a catalyst for a cracking reaction that produces hydrogen from ammonia, a method for producing the same, and a method for producing hydrogen using the same.
[0002] Recent industrial development and population growth have led to a global increase in energy demand. However, fossil fuels, the primary energy source, are gradually depleting. Furthermore, to combat global warming caused by greenhouse gases, countries are continuously researching clean energy sources that can replace fossil fuels. Among these, hydrogen is the most actively researched environmentally friendly energy source.
[0003] Much research is being conducted on the ammonia cracking reaction process, which produces hydrogen from ammonia as an eco-friendly hydrogen production technology. The ammonia cracking reaction is an endothermic reaction that decomposes ammonia into hydrogen and nitrogen, requiring a heat supply. The ammonia cracking reaction has a relatively low energy cost because ammonia is completely converted to hydrogen at a relatively low temperature, with a temperature of approximately 450 to 500 degrees Celsius at equilibrium conversion. However, the endothermic reaction itself requires high temperatures (over 500 degrees Celsius). Further development is needed to bring this reaction to a milder temperature range. One approach is to develop a catalyst that can achieve high ammonia conversion rates at low temperatures.
[0004] Catalyst compositions developed so far have been reported to include precious metals such as platinum, palladium, rhodium, ruthenium, and iridium as active metals, or non-precious metals such as nickel, copper, chromium, cobalt, and iron. For supports, research has been reported on silica, alumina, activated carbon, graphite, mesoporous carbon, and carbon nanotubes (Muhammad Aziz et al., Energies 2020, 13, 3062). Although many catalyst studies have been conducted using the combination of the above active metals and supports, most catalysts require an operating temperature of over 600 degrees Celsius to achieve 100% conversion of ammonia to hydrogen. Therefore, a highly active catalyst at a lower temperature is required for application to actual commercial crackers. In particular, the ship and small-scale ammonia co-firing power generation sectors require catalysts that can operate at reaction temperatures of 300-500 degrees Celsius.
[0005] As such, most of the ammonia cracking catalysts known in the past require high reaction temperatures to increase the ammonia conversion rate and have problems in that the cost-effectiveness is significantly reduced due to the large amount of expensive metals supported on the catalyst, and thus, improvement is needed. In the present invention, this problem is solved by manufacturing a catalyst by combining a low content of ruthenium with a support and a specific catalyst support.
[0006] The main purpose of the present invention is to solve the above-mentioned problems, and to provide a method for producing a catalyst for an ammonia cracking reaction that can improve the ammonia conversion rate at low temperatures and exhibit long-term stability by producing a catalyst using a low content of ruthenium as an ammonia cracking reaction catalyst, potassium and yttrium as auxiliary fillers, and a specific support, and a method for producing hydrogen through an ammonia cracking reaction using the same.
[0007] In order to achieve the above technical purpose, the inventors of the present invention manufactured an alumina support having a specific crystal phase so that ammonia, which is a reactant, can diffuse within the catalyst and the product can move quickly outside the catalyst, and on the manufactured support, ruthenium as a main metal and yttrium and potassium as auxiliary metals that can increase the reaction rate of ruthenium were positioned in a tri-metallic form, thereby manufacturing a catalyst so that the unique characteristics of each metal are expressed.
[0008] In the catalyst manufactured according to the present invention, yttrium (Y) exists in the form of Al-YO-Al-O by combining with an alumina support, and not only plays a role in decomposing and dissociating and adsorbing H ions of ammonia, but also increases the mobility of H ions toward Ru, thereby accelerating the production rate of H2. It was confirmed that potassium (K) weakens the strength of N2 generated after the cracking reaction being adsorbed on the catalyst and induces rapid desorption from the catalyst, thereby increasing the catalytic reaction rate and durability. In addition, it was found that a separate process for removing chlorine and nitrogen compounds remaining in the catalyst during the catalyst manufacturing process is configured to maximize the active sites of ruthenium during the ammonia cracking reaction, thereby exhibiting a high conversion rate at low temperatures.
[0009] The composition of the present invention is non-limiting as follows.
[0010] (1) An ammonia cracking catalyst used for producing nitrogen and hydrogen through an ammonia cracking reaction, wherein the catalyst support is delta alumina thermally modified from alumina hydrate, a complex metal in the form of a triple metal of ruthenium-yttrium-potassium is supported as an active metal, and chlorine and nitrogen compounds in the catalyst are present in an amount of 10 ppm or less relative to the weight of the catalyst.
[0011] (2) The above support is characterized in that it uses alumina and alumina hydrate manufactured in a shape such as a sphere, tablet, or structure by thermally transforming them, and the phase-transformed delta-alumina support after the heat treatment has a volume density of 0.5 to 1.2 g / ml, a specific surface area of 100 to 200 m2 / g, a pore volume of 0.4 to 0.5 cm3 / g, and an average pore size distribution of 10 to 14 nm.
[0012] (3) An ammonia cracking catalyst characterized in that ruthenium, which is the main metal in the catalyst, is distributed within 30% of the length from the periphery to the center of the catalyst, and yttrium and potassium, which are auxiliary metals, are uniformly distributed within the catalyst.
[0013] (4) The ruthenium is 0.5 to 3.0 wt% based on the weight of the catalyst, and 0.005 to 0.028 wt% / m within 30% of the length from the outer edge of the catalyst to the center. 2 , and yttrium and potassium are present in the catalyst at a content of 0.01 to 0.05 wt% / m 2 An ammonia cracking catalyst characterized by having a uniform content per surface area.
[0014] (5) An ammonia cracking catalyst characterized in that the weight ratio of (yttrium + potassium) / ruthenium among the above active metals is in the range of 4 to 8, the weight ratio of yttrium / ruthenium is 1 to 2, and the weight ratio of potassium / ruthenium is 3 to 6.
[0015] (6) An ammonia cracking catalyst characterized in that residual chlorine compounds in the catalyst are removed to 10 ppm or less relative to the catalyst weight by an ion exchange method using a basic substance, and nitrogen compounds are removed to 10 ppm or less relative to the catalyst weight by a high-temperature heat treatment method.
[0016] (7) A method for manufacturing a catalyst used in an ammonia cracking reaction, comprising: a) a step of manufacturing an alumina support having a delta crystal phase by heat-treating spherical boehmite (AlOOH) in a range of 750 to 900 degrees; b) a step of loading a solution in which an yttrium precursor (Y(NO3)3) is mixed and dissolved in a solvent onto the manufactured delta-alumina (δ-Al2O3) support by a pressurized spray method at room temperature; c) a step of drying at 100 to 120 degrees and calcining at 500 to 600 degrees after the loading; d) a step of loading a solution in which a ruthenium precursor (RuCl3) is dissolved in a solvent onto the manufactured yttrium / delta-alumina material by a pressurized spray method at room temperature; e) a step of drying at 100 to 120 degrees and calcining at 500 to 600 degrees after the loading; and removing residual Cl through ion exchange. A method for producing an ammonia cracking catalyst, characterized by comprising the steps of: step f) applying a solution of potassium precursor (KNO3) dissolved in a solvent to the manufactured ruthenium / yttrium / delta alumina material at room temperature using a pressurized spray method; step g) removing residual NO3 through drying at 100 to 120 degrees and calcining at 500 to 600 degrees after applying the material; and step h) producing a final catalyst by subjecting the manufactured potassium / ruthenium / yttrium / delta alumina oxidation catalyst to a rapid reduction process at high temperature using hydrogen gas within a range of 400 to 500 degrees.
[0017] (8) Used in ammonia cracking reaction, ammonia gas is produced at a reaction temperature of 300 to 550 degrees at a gas space velocity of 2,000 to 20,000 h -1 An ammonia cracking catalyst exhibiting a high hydrogen conversion rate, characterized by reacting under conditions.
[0018] The present invention relates to a ruthenium-based ammonia cracking catalyst, and more particularly, to an ammonia cracking catalyst prepared by selecting active metals, namely ruthenium as a main metal, yttrium as an auxiliary metal, and potassium, on a delta-alumina support, and a method for preparing the same. The ammonia cracking catalyst according to the present invention can achieve a very high ammonia conversion rate and hydrogen production efficiency even at low temperatures compared to a catalyst having the same ruthenium metal content by controlling the weight ratio of ruthenium / yttrium / potassium together with a thermally modified alumina support of a specific phase, minimizing the content of chlorine and nitrogen compounds, which are impurities in the catalyst, and designating the position of the active metal in the catalyst, even when using a low content of ruthenium metal.
[0019] Figure 1 is a flowchart illustrating the manufacturing method steps of Example 1 of the present invention.
[0020] Figure 2 is an electron microscope (video microscopy) and electron probe X-ray microanalyzer (EPMA) photograph of the catalyst manufactured in Example 1 of the present invention.
[0021] definition
[0022] In the present invention, the active metal is a term including a main metal and a supporting metal, and the support is also referred to as a carrier as an oxide for supporting the active metal.
[0023] The present invention relates to an ammonia cracking catalyst and a manufacturing method for hydrogen production, and more particularly, to a catalyst and a manufacturing method manufactured through a process of manufacturing a delta-alumina support having controlled acid sites and pore sizes, selecting active metals such as ruthenium as a main metal and yttrium and potassium as auxiliary metals, and removing chlorine and nitrogen compounds derived from metal precursors and remaining in the catalyst.
[0024] According to the present invention, hydrogen ions dissociated through the combination of yttrium and a support can rapidly generate hydrogen by ruthenium, and if this reaction continues, the ruthenium gradually increases in particle size due to sintering, which reduces the cracking conversion rate. In order to prevent this sintering phenomenon, it was found that potassium can be strongly combined with ruthenium to suppress the particle growth phenomenon of ruthenium during the reaction and play a role in increasing the durability of the catalyst.
[0025] In addition, when the main metal among the active metals is generally distributed throughout the support, the contact frequency between the reactant and the support / active metal decreases, resulting in a loss of the amount of hydrogen produced per unit time (ammonia conversion rate). To solve this problem, ruthenium was positioned on the surface of the support, and the hydrogen production was designed to increase due to the ruthenium concentrated on the catalyst surface even when the reactant is introduced into the reactor at a high space velocity. In the case of yttrium and potassium, the catalyst was manufactured by uniformly distributing them within the support to maximize their interaction with the alumina support.
[0026] Hereinafter, preferred embodiments of the present invention will be described in detail.
[0027] A composite metal catalyst in the form of a ruthenium-auxiliary metal supported on a heat-modified alumina support with controlled crystal phase and pore characteristics of the present invention can be manufactured through the following steps.
[0028] a) A step of producing a support of alumina having a delta crystal phase by heat-treating spherical boehmite (AlOOH) in the range of 750 to 900 degrees,
[0029] b) A step of loading a solution in which yttrium precursor (Y(NO3)3) is mixed in a solvent and dissolved on the manufactured delta-alumina (δ-Al2O3) support using a pressurized spray method at room temperature;
[0030] c) A step of drying at 100 to 120 degrees and calcining at 500 to 600 degrees after yttrium is loaded;
[0031] d) A step of loading a solution of ruthenium precursor (RuCl3) dissolved in a solvent onto the manufactured yttrium / delta alumina material by pressurized spraying at room temperature;
[0032] e) A step of drying at 100 to 120 degrees and calcining at 500 to 600 degrees after ruthenium is loaded, and a step of removing residual Cl through ion exchange.
[0033] f) A step of applying a solution of potassium precursor (KNO3) dissolved in a solvent to the manufactured ruthenium / yttrium / delta alumina material by pressurized spraying at room temperature.
[0034] g) a step of removing residual NO3 by drying at 100 to 120 degrees and calcining at 500 to 600 degrees after potassium is loaded, and
[0035] h) A step of completing the final catalyst by subjecting the manufactured potassium / ruthenium / yttrium / delta alumina oxidation catalyst to a rapid reduction process at high temperatures using hydrogen gas within the range of 400 to 500 degrees.
[0036] Each step is explained in detail.
[0037] In the above step a), the alumina support can be made using boehmite or gamma alumina as a starting material, and can be manufactured by heat-treating the support at a temperature of 750 to 900 degrees for 1 to 5 hours in a heat treatment furnace to remove acid sites and control pore size, thereby changing it into a crystal phase having more than 90% delta alumina. The heat treatment temperature is closely related to the crystal phase and pore structure of the support. Boehmite exists in four alumina phases (gamma, delta, theta, alpha) depending on the heat treatment temperature, and delta alumina is produced by a phase transformation between about 750 and 900 degrees. Table 1 shows the changes in the alumina crystal phase, specific surface area, pore volume, and pore size that appear when boehmite is heat-treated at different temperatures.
[0038] Table 1 (Pore characteristics by support sintering temperature)
[0039] Starting material, processing temperature (℃), alumina state after heat treatment (crystal phase), specific surface area (m 2 / g) pore volume (cm) 3 / g)Pore size (nm)Boehmite (AlOOH) 450Gamma alumina (γ-Al2O3) 2060.499.5850Delta alumina (δ-Al2O3) 1580.4712.1900Delta alumina (δ-Al2O3) 1530.4712.61000Theta alumina (θ-Al2O3) 930.3314.11200Alpha alumina (α-Al2O3) 30.0498
[0040] Delta alumina has a similar specific surface area to gamma alumina, but its pore size is increased, which allows more space for the active metal to be located inside the alumina. In addition, it has the characteristic of weakening the Lewis acid sites and Brønsted acid sites of gamma alumina, allowing the reactant ammonia to react only with the active metal. The high specific surface area improves the dispersibility of the metal when supporting the active metal, and the increased pore size has the advantage of improving the permeability between the reactant and the catalyst when applied to a cracking reaction, which can increase the reaction rate of the catalyst.
[0041] On the other hand, theta or alpha alumina heat-treated at a higher temperature, especially above 900 degrees, has a larger pore size, but has a disadvantage in that the specific surface area decreases rapidly, causing agglomeration of metal particles in the process of supporting the active metal, thereby lowering the dispersion, and is therefore not suitable as a support to be used in the manufacturing method of the present invention. The manufactured alumina support may have a bulk density of 0.5 to 1.2 g / ml, a specific surface area of 100 to 200 m2 / g, a pore volume of 0.4 to 0.5 cm3 / g, an average pore size distribution of 10 to 14 nm, and a delta-alumina / gamma-alumina ratio of 9 or more. The support may be in the form of a sphere, a cylinder, a pellet, or a tube, and these forms may be manufactured by a method of oil-drop, tableting, or extrusion.
[0042] In the step b), as the yttrium precursor, one of yttrium nitrate hydrate, yttrium chloride hydrate, yttrium acetate hydrate, and yttrium sulfate hydrate may be used, and preferably, yttrium nitrate, which can increase the dispersion of ruthenium, may be used for production. The yttrium precursor may be dissolved in a solvent such as ionized water or dihydric alcohol (ethanol, ethylene glycol, etc.) in an amount equivalent to the pore volume of the support and supported on the support using a pressurized spray method. Meanwhile, the yttrium precursor may be supported in an amount of 1 to 4 wt% based on the final catalyst. If it is loaded at less than 1 wt%, it is difficult to realize catalytic performance, and if it is loaded at more than 4 wt%, the yttrium precursor cannot be introduced into the support and may accumulate on some of the support surface, resulting in low ruthenium activity, which in turn reduces durability. The yttrium precursor can be loaded at a level of 1-2 based on the yttrium / lutetium weight ratio, and preferably can be manufactured at a level of 1 based on the yttrium / lutetium weight ratio.
[0043] In the above step c), the yttrium / delta alumina manufactured in step b) may be manufactured by including a step of drying at 100 to 120 degrees and then heat treating at 500 to 600 degrees to remove moisture and precursor material derived from the metal precursor.
[0044] In the step d), as the ruthenium precursor, one of ruthenium nitrate hydrate, ruthenium chloride hydrate, ruthenium acetate hydrate, ruthenium hydroxide hydrate, and ruthenium nitrosyl nitrate hydrate may be used, and preferably, ruthenium chloride, which can increase ruthenium dispersibility, may be used for the preparation. The active metal precursor may be dissolved in a solvent such as ionized water or dihydric alcohol (ethanol, ethylene glycol, etc.) in an amount equivalent to the pore volume of the support and supported on the support using a pressurized spray method. The ruthenium precursor may be supported at a level of 0.5 to 3 based on the weight ratio of the final catalyst, and may preferably be prepared at a level of 1 to 2 for commercial applications.
[0045] In the above step e), the ruthenium / yttrium / delta-alumina material manufactured in step d) may be manufactured by including a step of drying at 100 to 120 degrees and then heat-treating at 500 to 600 degrees in an air atmosphere to remove moisture and precursor material derived from the metal precursor. In addition, when ruthenium chloride is used among the metal precursor materials, a process of removing chloride ions by an ion exchange method using a base material may be added since chloride ions may remain even after the heat treatment. The base material may be one of ammonium hydroxide, ammonium nitrate, sodium hydroxide, and sodium nitrate, and preferably, ammonium hydroxide, which is easy to clean, may be used.
[0046] In the step f), the potassium precursor may be one of potassium nitrate hydrate, potassium chloride hydrate, potassium acetate hydrate, and potassium hydroxide hydrate, and preferably, potassium nitrate, which can increase ruthenium dispersibility, may be used. The potassium precursor may be prepared by dissolving it in a solvent of ionized water or dihydric alcohol (ethanol, ethylene glycol, etc.) in an amount equivalent to the pore volume of the support and supporting it on the support using a pressurized spray method. Meanwhile, the potassium precursor may be supported in an amount of 4 to 10 wt% based on the final catalyst. If supported in an amount of less than 4 wt%, it is difficult to realize catalytic performance, and if supported in an amount of more than 10 wt%, the potassium precursor may not be introduced into the support and may accumulate on the surface of some of the support, resulting in low ruthenium activity, which may result in reduced durability. The potassium precursor can be supported at a level of 3 to 6 based on the potassium / lutetium weight ratio, and preferably can be manufactured at a level of 3 to 4 based on the potassium / lutetium weight ratio.
[0047] In the above step g), the potassium / ruthenium / yttrium / delta-alumina material manufactured in step f) may be manufactured by including a step of drying at 100 to 120 degrees and then heat-treating at 500 to 600 degrees in an air atmosphere to remove moisture and precursor material derived from the metal precursor. The heat-treating temperature can be performed within an appropriate range as is common knowledge, and thus will not be described in detail further.
[0048] In the above step h), in order to develop catalytic activity in the potassium / ruthenium / yttrium / delta-alumina oxides manufactured in step g), a rapid reduction process is performed using hydrogen gas within the range of 400-600 degrees, preferably within the range of 400 to 500 degrees, to obtain the final catalyst. If the reduction temperature is lower than 400 degrees during the reduction process, the metal oxide species may not be completely reduced, and if the reduction temperature is higher than 600 degrees, agglomeration and sintering of the metal particles may occur, which may result in a decrease in active sites. In the reduction process, the catalyst was manufactured by heating in a nitrogen atmosphere to the target temperature in a stepwise manner and then flowing hydrogen gas. If two or more active metal species are contained in the catalyst, if it is directly exposed to hydrogen gas at a high temperature as in the above reduction method, the active metal species can be instantaneously manufactured into an alloy form. However, if the temperature is gradually increased from room temperature in a hydrogen atmosphere for reduction, each metal is reduced according to its own oxygen desorption temperature, making it difficult to form an alloy.
[0049] The catalyst manufactured in the present invention can be used in the cracking reaction of ammonia gas after being introduced into a reactor, and ammonia gas can be cracked at a reaction temperature of 300 to 550 degrees with a gas hourly space velocity (GHSV) of 2,000 to 20,000 h -1Hydrogen can be produced by a gas phase reaction under these conditions. As the gas space velocity increases, the amount of hydrogen produced increases proportionally, so the optimal value can be arbitrarily adjusted according to the reactor volume and catalyst amount, and is not limited to a specific value within the range. The reactor that produces hydrogen through the reforming reaction is not particularly limited, but a fixed-bed catalytic reactor in which a catalyst is filled inside the reactor can be used. In addition, since the cracking reaction is an endothermic reaction, it is important for the catalytic reactor to always be maintained in an adiabatic state. It is important for the cracking reaction process of the present invention to proceed while maintaining the reaction conditions, such as reaction temperature, pressure, and gas space velocity, within an appropriate range. If the reaction temperature is below 300°C, the cracking reaction does not proceed sufficiently, resulting in a very low amount of hydrogen. If the reaction temperature is above 550°C, the energy cost increases for commercial applications, which reduces efficiency.
[0050] The technical configuration of the present invention will be described in detail with reference to the following drawings, examples, and comparative examples.
[0051] Example 1
[0052] As a support, 1.8 mm spherical boehmite (manufacturer: BASF, Germany, specific surface area: 250 m 2 / g) was calcined at 900 degrees for 5 hours to undergo phase transfer and then used. The phase-transferred support had a delta-alumina crystal phase and a specific surface area of 153 m 2 / g, pore volume 0.47cm 3 / g, and has physical properties of a pore size of 12.6 nm. In order to first support the metal, yttrium was used as a precursor, yttrium nitrate (Y(NO3)3.6H2O), and the yttrium precursor was dissolved in water and impregnated into the phase-transferred delta-alumina support using a spray impregnation method. After impregnation, an aging process was performed for about 1 hour to ensure that the metal solution was sufficiently distributed into the support, and then dried at 120 degrees for 12 hours to completely remove moisture in the catalyst, followed by a heat treatment process at 600 degrees for 6 hours in an air atmosphere to immobilize the metal. Next, in order to support lutetium, which was selected as the main metal among the active metals, ruthenium chloride (RuCl3.xH2O) was used as a precursor, and this was dissolved in water and impregnated into yttrium / delta-alumina using a spray impregnation method. The manufactured ruthenium / yttrium / delta-alumina was dried at 120°C for 12 hours to completely remove moisture within the catalyst, and then heat-treated at 600°C for 6 hours in an air atmosphere to immobilize the metal. Subsequently, the heat-treated ruthenium / yttrium / delta-alumina oxide was further treated with ammonia water to ion-exchange the chloride component remaining within the oxide with ammonium chloride, and then washed / removed.
[0053] Next, potassium nitrate (KNO3) was also supported on the ruthenium / yttrium / delta-alumina oxide by a spray support method, and finally, the metal-supported potassium / ruthenium / yttrium / delta-alumina composition was heat-treated at 550 degrees in an air atmosphere for 4 hours to produce a metal-supported catalyst oxide. Finally, the heat-treated oxide was heated to 500 degrees in an air atmosphere, purged with nitrogen for 5 minutes, and then rapidly reduced while flowing hydrogen gas to produce a catalyst. The overall manufacturing sequence and method are shown in Fig. 1.
[0054] The catalyst manufactured in Example 1 was confirmed to contain 1.93 wt% yttrium, 1.7 wt% lutetium, 6.8 wt% potassium, 4 ppm chloride ions, and 0 ppm nitrate ions. In addition, yttrium and potassium were uniformly distributed within the support, and ruthenium was manufactured to be distributed to a depth of approximately 30% from the periphery of the catalyst. The metal distribution within the catalyst manufactured in Example 1 is shown in Fig. 2.
[0055] Example 2
[0056] Example 2 was performed in the same manner as Example 1 to manufacture a catalyst, except that the metal content of the final catalyst was 3.86 wt% of yttrium, 1.7 wt% of lutetium, and 6.8 wt% of potassium.
[0057] Example 3
[0058] Example 3 was performed in the same manner as Example 1 to manufacture a catalyst, except that the metal content of the final catalyst was such that it contained 0.57 wt% of yttrium, 0.5 wt% of lutetium, and 2.0 wt% of potassium.
[0059] Comparative Example 1
[0060] Comparative Example 1 was prepared by the same method as Example 1, except that the catalyst was prepared without containing yttrium.
[0061] Comparative Example 2
[0062] Comparative Example 2 was prepared by the same method as Example 1, except that it was prepared without containing potassium.
[0063] Comparative Example 3
[0064] Comparative Example 3 was prepared by the same method as Example 1, except that the catalyst was prepared without containing yttrium and potassium.
[0065] Comparative Example 4
[0066] Comparative Example 4 was prepared by manufacturing a catalyst in the same manner as Comparative Example 3, except that it was manufactured by loading 2 wt% of ruthenium.
[0067] Comparative Example 5
[0068] Comparative Example 5 was prepared by manufacturing a catalyst in the same manner as Comparative Example 3, except that it was manufactured by loading 3 wt% of ruthenium.
[0069] Comparative Example 6
[0070] Comparative Example 6 was performed in the same manner as Example 1, except that the heat treatment temperature was 1000 degrees when manufacturing the support used in Example 1, and a catalyst was manufactured. The support crystal phase of the catalyst was theta phase, and the specific surface area was 93 m 2 / g, the pore size was 14.1 nm.
[0071] Comparative Example 7
[0072] Comparative Example 7 was performed in the same manner as Example 1, except that the heat treatment temperature was 1200 degrees when manufacturing the support used in Example 1, and a catalyst was manufactured. The support crystal phase of the catalyst was alpha phase, and the specific surface area was 3 m 2 / g, the pore size was 98 nm.
[0073] The material composition and active metal composition of the catalysts in the above examples and comparative examples are summarized in Table 2.
[0074] Table 2 (Manufacturing methods for examples and comparative examples)
[0075] Active metal in the support catalyst Composition Ru (wt%) K (wt%) Y (wt%) (Y+K) / Ru (weight ratio) Example-1 δ-Al2O 1.7 6.8 1.9 3 5.1 Example-2 δ-Al2O 1.7 6.8 3.8 6 6.3 Example-3 δ-Al2O 0.5 2.0 0.5 7 5.1 Comparative Example-1 δ-Al2O 1.7 6.8 4 Comparative Example-2 δ-Al2O 1.7 1.9 3 1.1 Comparative Example-3 δ-Al2O 1.7 --- Comparative Example-4 δ-Al2O 2 --- Comparative Example-5 δ-Al2O 3 --- Comparative Example-6θ-Al2O 1.7 6.8 1.9 3 5.1 Comparative Example-7 α-Al2O 1.7 6.8 1.9 3 5.1
[0076] Example reaction
[0077] The performance of the catalysts manufactured in the above examples was evaluated as follows. To measure the catalytic activity, a cracking reaction was performed using ammonia gas, and the reactor was evaluated using a fixed-bed reaction system. 3 ml of the catalyst was charged into a tubular reactor, and before performing the reaction, hydrogen gas was constantly flowed at 10 cc / min to remove oxygen species on the catalyst surface, thereby reducing the catalyst at 400°C for 1 hour. Then, the temperature of the reactor was constantly maintained at 300°C, 400°C, and 500°C, and ammonia gas, which was the raw material for the reaction, was continuously supplied to the reactor at a constant rate of 100 cc / min, and the gas space velocity was 2,000 h -1 was fixed at a constant value. The reaction pressure was evaluated under atmospheric pressure conditions. The substance produced after the reaction was transferred to GC (Gas chromatography) through the injection line and quantitatively analyzed using TCD (thermal conductivity detector).
[0078] The conversion rate of ammonia for the reactants was calculated based on the following criteria, and the activities of the catalysts were compared. The results are shown in Table 3.
[0079] Conversion rate of ammonia (%) = [number of moles of ammonia before reaction - number of moles of ammonia after reaction] / [number of moles of ammonia before reaction] × 100
[0080] Table 3 (Ammonia cracking reaction evaluation results for examples and comparative examples)
[0081] Classification Ammonia Conversion Rate (%) 300 degrees 400 degrees 500 degrees Example - 19.0 45.0 100 Example - 26.0 37.0 100 Example - 30.7 2168.0 Comparative Example - 16.3 24.18 0.3 Comparative Example - 20.5 10.0 49.0 Comparative Example - 30.5 13.76 8.7 Comparative Example - 41.6 25.87 2.0 Comparative Example - 52.0 38.39 8.0 Comparative Example - 64.5 25.18 5.2 Comparative Example - 70.8 11.0 48.0
[0082] - These catalysts have in common that the main active metal ruthenium was positioned at about 30% from the periphery of the catalyst to increase the hydrogen production rate from the reactants, and the auxiliary metals yttrium and potassium were manufactured to be uniformly distributed within the catalyst to maximize the interaction with the alumina support. In addition, the catalysts were manufactured to remove all impurities such as chlorine and nitrogen compounds. - Example 1 and Comparative Examples 1 to 3 are the contents of catalysts manufactured depending on the presence or absence of the auxiliary metals potassium and yttrium, and the activity evaluation results showed that Example 1 showed the highest low-temperature activity, and ultimately, ammonia was converted 100% at 500 degrees. In particular, yttrium had an effect on increasing the ammonia conversion rate at low temperatures, and potassium shows that it is a factor that can increase the overall conversion rate.
[0083] - Comparative Examples 3 to 5 are catalysts manufactured by changing the amount of ruthenium, the main active metal, to 1.7 wt%, 2 wt%, and 3 wt%, and the results showed that the ammonia conversion rate increased depending on the amount of ruthenium loaded, but the conversion rate at 500 degrees was less than 100%. However, the catalyst of Example 1, which additionally loaded yttrium and potassium at the same 1.7 wt% ruthenium content as Comparative Example 3, showed a higher ammonia conversion rate than the 3 wt% ruthenium-loaded catalyst of Comparative Example 5, indicating that the combination of ruthenium and a supporting metal can contribute to greatly increasing the reaction activity.
[0084] - Example 1 and Comparative Examples 6 and 7 are the contents of manufacturing a catalyst by changing the crystal phase of alumina, which is a catalyst support, and the results of the activity evaluation show lower ammonia cracking reaction activity compared to Example 1, and in particular, Comparative Example 7 shows a reactivity of 11% at 400 degrees and 48% at 500 degrees compared to Example 1, indicating that the crystal phase of the support has a significant effect on the ammonia cracking reaction.
[0085] - Thus, as in Example 1, the catalyst can be manufactured by manufacturing a catalyst in which the crystal phase of the support is delta alumina, the metal is 1.7 wt% lutetium, 6.8 wt% potassium, and 1.93 wt% yttrium, and the [yttrium + potassium] / ruthenium weight ratio is approximately 5.1, thereby manufacturing a catalyst that exhibits a high ammonia cracking conversion rate at a relatively low temperature of 300-500 degrees.
Claims
1. An ammonia cracking catalyst as a catalyst for an ammonia cracking reaction, characterized in that the catalyst support is delta alumina thermally modified from alumina hydrate, a complex metal in the form of a triple metal of ruthenium-yttrium-potassium is supported as an active metal, and chlorine and nitrogen compounds in the catalyst are present in an amount of 10 ppm or less relative to the weight of the catalyst.
2. In the first paragraph, the thermally modified delta alumina support has a volume density of 0.5 to 1.2 g / ml and a specific surface area of 100 to 200 m 2 / g, pore volume is 0.4 to 0.5 cm 3 / g, an ammonia cracking catalyst characterized by an average pore size distribution in the range of 10 to 14 nm.
3. An ammonia cracking catalyst according to claim 1, wherein the ruthenium is distributed within 30% of the length from the periphery of the catalyst to the center, and the yttrium and potassium are uniformly distributed within the catalyst.
4. In the first paragraph, the ruthenium is 0.5 to 3.0 wt% based on the weight of the catalyst, and 0.005 to 0.028 wt% / m within 30% of the length from the outer edge of the catalyst to the center. 2 An ammonia cracking catalyst characterized by the presence of a content of .
5. In the first paragraph, the yttrium and potassium are contained in the catalyst at 0.01 to 0.05 wt% / m 2 An ammonia cracking catalyst characterized by the presence of a uniform content of .
6. An ammonia cracking catalyst characterized in that in the first paragraph, the weight ratio of (yttrium + potassium) / ruthenium is in the range of 4 to 8, the weight ratio of yttrium / ruthenium is 1 to 2, and the weight ratio of potassium / ruthenium is 3 to 6.
7. A method for manufacturing a catalyst used in an ammonia cracking reaction, comprising: a) a step of manufacturing an alumina support having a delta crystal phase by heat-treating spherical boehmite (AlOOH) in a range of 750 to 900 degrees; b) a step of loading a solution in which an yttrium precursor (Y(NO3)3) is mixed and dissolved in a solvent onto the manufactured delta-alumina (δ-Al2O3) support by a pressurized spray method at room temperature; c) a step of drying at 100 to 120 degrees and calcining at 500 to 600 degrees after the loading; d) a step of loading a solution in which a ruthenium precursor (RuCl3) is dissolved in a solvent onto the manufactured yttrium / delta-alumina material by a pressurized spray method at room temperature; e) a step of drying at 100 to 120 degrees and calcining at 500 to 600 degrees after the loading; and removing residual Cl through ion exchange. A method for producing an ammonia cracking catalyst, characterized by comprising the steps of: step f) applying a solution of potassium precursor (KNO3) dissolved in a solvent to the manufactured ruthenium / yttrium / delta alumina material at room temperature using a pressurized spray method; step g) removing residual NO3 through drying at 100 to 120 degrees and calcining at 500 to 600 degrees after applying the material; and step h) producing a final catalyst by subjecting the manufactured potassium / ruthenium / yttrium / delta alumina oxidation catalyst to a rapid reduction process at high temperature using hydrogen gas within a range of 400 to 500 degrees.
Citation Information
Patent Citations
Preparation and application of rare earth modified catalyst for hydrogen production through ammonia decomposition
CN114471553A
Ammonia decomposition catalyst, method for producing ammonia decomposition catalyst, method for producing hydrogen and apparatus for producing hydrogen
JP2016198720A
Ammonia Decomposition Catalyst Systems
US20200062590A1
Systems and methods for processing ammonia
US20220395810A1