Stacked multi-channel structure and method for manufacturing same, and thin film transistor comprising same
The stacked multi-channel structure using PEALD for IGZO and Al2O3 layers in thin film transistors addresses the challenges of mobility and threshold voltage control, achieving high mobility and reliability by precisely managing channel thickness and composition, and maintaining stable threshold voltage.
Patent Information
- Application Number
- PCT/KR2024/004623
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2024-04-08
- Publication Date
- 2024-10-24
AI Technical Summary
Current stacked thin film transistors face challenges in controlling channel thickness and composition, mobility, and maintaining constant threshold voltage while achieving high mobility and low subthreshold swing, particularly due to limitations in sputter deposition methods and 2DEG structures which can lead to negative threshold voltage shifts.
A stacked multi-channel structure is developed using a plasma-enhanced atomic layer deposition (PEALD) process, where an oxide semiconductor (IGZO) and a metal oxide insulator (Al2O3) are alternately stacked to form multiple channels, allowing for precise control of thickness and composition, and maintaining a stable threshold voltage as the number of stacks increases.
This approach enables high mobility and controlled subthreshold swing, keeping the threshold voltage constant, thus enhancing the reliability and performance of thin film transistors suitable for display backplanes.
Smart Images

Figure KR2024004623_24102024_PF_FP_ABST
Abstract
Description
Stacked multi-channel structure and method for manufacturing the same, and thin film transistor including the same
[0001] The present invention relates to a laminated multi-channel structure in which an oxide semiconductor and a metal oxide insulator are laminated, a method for manufacturing the same, and a thin film transistor including the same.
[0002] TFTs form the backplane that controls the flow of current to drive display panels. The types of TFTs currently used in the display industry are determined by the semiconductor material used: amorphous silicon (a-Si) TFTs, low-temperature poly-silicon (LTPS) TFTs, and amorphous oxide TFTs. Among these, oxide semiconductor TFTs are considered promising candidates not only for use in display backplanes but also in memory / system semiconductor fields due to their relatively high mobility and extremely low leakage current characteristics.
[0003] However, in the display field, V is not only low leakage current characteristic but also reliability degradation. th TFTs with high SS in the shift state are attracting attention because they can maintain switching characteristics for longer due to minimal changes in drain current. Furthermore, higher mobility is required to replace LTPS. Therefore, research on various oxide semiconductors is underway to realize oxide semiconductor TFTs that possess both high mobility and SS control.
[0004] Existing research on stacked thin-film transistors (TFTs) using oxide semiconductors to achieve high mobility has relied on physical deposition techniques such as sputtering. This commercially used sputter deposition process presents challenges for studying TFTs due to its limitations in controlling nanoscale thickness due to physical deposition and in controlling cation composition due to its fixed target composition.
[0005] Conventional representative layered structures have been able to improve mobility by positioning high-mobility materials in the front-channel and relatively low-mobility, stable materials in the back-channel. Furthermore, to achieve high-mobility characteristics, two materials with large conduction band offsets are heterojunction-bonded to form a two-dimensional electron gas (2DEG) at the interface, thereby enhancing mobility.
[0006] However, while mobility enhancement is possible through conventional layered structures, controlling the SS value is challenging. In particular, the 2DEG structure is prone to a negative threshold voltage shift due to confined electrons.
[0007] The technical problem to be solved by the present invention is to provide a stacked multi-channel structure and a method for manufacturing the same, and a thin film transistor including the same.
[0008] Another technical problem to be solved by the present invention is to provide a multi-channel structure in which an oxide semiconductor and a metal oxide insulator are laminated, a method for manufacturing the same, and a thin film transistor including the same.
[0009] Another technical problem to be solved by the present invention is to provide a multi-channel structure and a manufacturing method thereof, in which the thickness and composition of the channel can be easily controlled, and a thin film transistor including the same.
[0010] Another technical problem to be solved by the present invention is to provide a multi-channel structure with easy mobility and subthreshold swing control, a method for manufacturing the same, and a thin film transistor including the same.
[0011] Another technical problem to be solved by the present invention is to provide a multi-channel structure and a method for manufacturing the same, in which the threshold voltage can be maintained substantially constant while mobility and subthreshold swing are controlled, and a thin film transistor including the same.
[0012] The technical problems to be solved by the present invention are not limited to those described above.
[0013] To solve the above-described technical problems, the present invention provides a thin film transistor.
[0014] According to one embodiment, a thin film transistor including a channel structure in which a first material layer including an oxide semiconductor and a second material layer including a metal oxide insulator are stacked, the channel structure may include a plurality of stacks in which the first material layer and the second material layer are stacked to form a multi-channel, and mobility and subthreshold swing increase as the number of stacks of the stacks increases.
[0015] According to one embodiment, the rate of increase in mobility as the number of layers of the stack increases may be higher than the rate of increase in the subthreshold swing.
[0016] According to one embodiment, even if the number of layers of the stack increases, the change in threshold voltage may be maintained at 10% or less.
[0017] According to one embodiment, even if the number of layers of the stack increases, the threshold voltage may be maintained in a range of 0.09 V to 0.19 V.
[0018] According to one embodiment, the number of layers of the stack may be 5 or more and 10 or less.
[0019] According to one embodiment, the second material layer may have a thickness of less than 4 nm.
[0020] According to one embodiment, the oxide semiconductor may include IGZO (Indium Gallium Zinc Oxide).
[0021] According to one embodiment, the metal oxide insulator may include aluminum oxide (Al2O3).
[0022] In one embodiment, the amount of movement of carriers within the first material layer disposed relatively close to the gate may be greater than the amount of movement of carriers within the first material layer disposed relatively far from the gate.
[0023]
[0024] To solve the above-described technical problems, the present invention provides a method for manufacturing a channel structure.
[0025] According to one embodiment, the method for manufacturing the channel structure includes the steps of preparing a substrate, forming a first material layer including an oxide semiconductor on the substrate by a plasma-enhanced atomic layer deposition (PEALD) process, and forming a second material layer including a metal oxide insulator on the first material layer by a PEALD process, wherein the step of forming the first material layer and the step of forming the second material layer may be alternately repeated to form multi-channels.
[0026] According to one embodiment, the step of forming the first material layer may include a step of reacting an indium (In) precursor, a gallium (Ga) precursor, a zinc (Zn) precursor, and oxygen plasma (O2plasma) on the substrate, and the step of forming the second material layer may include a step of reacting an aluminum (Al) precursor and oxygen plasma (O2plasma) on the first material layer.
[0027] According to one embodiment, the first material layer and the second material layer may be formed by an in-situ process.
[0028] A thin film transistor according to an embodiment of the present invention includes a channel structure in which a first material layer including an oxide semiconductor (e.g., IGZO) and a second material layer including a metal oxide insulator (e.g., Al2O3) are stacked, and the channel structure may form a multi-channel by stacking a plurality of stacks in which the first material layer and the second material layer are stacked.
[0029] In addition, since the channel structure is manufactured through a PEALD process, thickness and composition control can be easily achieved, and high mobility characteristics can be effectively expressed through thickness and composition control.
[0030] In addition, not only can the subthreshold swing (SS) be easily controlled, but also the mobility (μ FE ) and subthreshold swing (SS) are controlled, but the threshold voltage (V th ) can be maintained substantially constant. Accordingly, it can be easily applied to transistors of display backplanes that require high mobility and high reliability.
[0031] FIG. 1 is a flowchart illustrating a method for manufacturing a channel structure according to an embodiment of the present invention.
[0032] FIG. 2 is a drawing specifically explaining step S200 of a method for manufacturing a channel structure according to an embodiment of the present invention.
[0033] FIG. 3 is a drawing specifically explaining step S300 of a method for manufacturing a channel structure according to an embodiment of the present invention.
[0034] FIG. 4 is a drawing for explaining a channel structure according to an embodiment of the present invention.
[0035] FIG. 5 is a drawing for explaining a thin film transistor according to an embodiment of the present invention.
[0036] Figure 6 is a schematic cross-sectional view of TT' of Figure 5.
[0037] FIG. 7 is a drawing for explaining various forms of a channel structure included in a thin film transistor according to an embodiment of the present invention.
[0038] Figure 8 is a STEM image of a channel structure according to an experimental example of the present invention.
[0039] FIG. 9 and FIG. 10 are drawings for explaining the EDS analysis results of a channel structure according to an experimental example of the present invention.
[0040] FIG. 11 is a drawing for explaining the electrical characteristics of a thin film transistor according to Experimental Examples 1-1 to 1-4 of the present invention.
[0041] FIG. 12 is a diagram for comparing TCAD simulation results of thin film transistors according to experimental examples 1-1 to 1-9 of the present invention.
[0042] FIG. 13 is a drawing for explaining the electrical characteristics of a thin film transistor according to Experimental Examples 2-1 to 2-6 of the present invention.
[0043] FIG. 14 is a drawing for explaining the simulation results of a thin film transistor according to experimental examples 3-1 to 3-3 of the present invention.
[0044] FIG. 15 is a drawing for explaining the simulation results of a thin film transistor according to experimental examples 4-1 to 4-3 of the present invention.
[0045] FIG. 16 is a drawing for explaining the simulation results of a thin film transistor according to experimental examples 5-1 to 5-3 of the present invention.
[0046] Figure 17 is a graph comparing electrical characteristics of insulators according to their k values.
[0047] FIG. 18 and FIG. 19 are drawings for comparing the amount of carrier movement within the channel structure of the thin film transistor according to Experimental Examples 1-1 to 1-4 of the present invention.
[0048] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the attached drawings. However, the technical concept of the present invention is not limited to the embodiments described herein and may be embodied in other forms. Rather, the embodiments introduced herein are provided to ensure that the disclosed content is thorough and complete and to sufficiently convey the spirit of the present invention to those skilled in the art.
[0049] In this specification, when a component is referred to as being on another component, it means that it can be formed directly on the other component, or a third component may be interposed between them. In addition, in the drawings, the thicknesses of films and regions are exaggerated for the purpose of effectively explaining the technical contents.
[0050] Also, although terms such as first, second, and third have been used to describe various components in various embodiments of this specification, these components should not be limited by these terms. These terms are only used to distinguish one component from another. Thus, what is referred to as a first component in one embodiment may be referred to as a second component in another embodiment. Each embodiment described and illustrated herein also includes its complementary embodiments. Also, the term "and / or" has been used herein to mean including at least one of the components listed before and after.
[0051] In the specification, singular expressions include plural expressions unless the context clearly dictates otherwise. In addition, terms such as "comprise" or "have" are intended to specify the presence of a feature, number, step, component, or combination thereof described in the specification, and should not be construed as excluding the presence or addition of one or more other features, numbers, steps, components, or combinations thereof. In addition, the term "connection" is used in the present specification to mean both indirectly connecting multiple components and directly connecting them.
[0052] In addition, when describing the present invention below, if it is determined that a detailed description of a related known function or configuration may unnecessarily obscure the gist of the present invention, the detailed description will be omitted.
[0053]
[0054] FIG. 1 is a flowchart for explaining a method for manufacturing a channel structure according to an embodiment of the present invention, FIG. 2 is a drawing for specifically explaining step S200 of a method for manufacturing a channel structure according to an embodiment of the present invention, FIG. 3 is a drawing for specifically explaining step S300 of a method for manufacturing a channel structure according to an embodiment of the present invention, and FIG. 4 is a drawing for explaining a channel structure according to an embodiment of the present invention.
[0055] Referring to FIGS. 1 to 4, a substrate is prepared (S100). In one embodiment, the substrate may be a silicon semiconductor substrate. Alternatively, in another embodiment, the substrate may be any one of a compound semiconductor substrate, a glass substrate, or a plastic substrate. The type of the substrate is not limited.
[0056] A first material layer (410) including an oxide semiconductor can be formed on the substrate using a PEALD (Plasma Enhanced Atomic Layer Deposition) process (S200). According to one embodiment, the first material layer (410) can be formed by a reaction of an indium (In) precursor, a gallium (Ga) precursor, a zinc (Zn) precursor, and oxygen plasma (O2plasma). Accordingly, the first material layer (410) can include IGZO (Indium Gallium Zinc Oxide). That is, the oxide semiconductor included in the first material layer (410) can be IGZO.
[0057] More specifically, as illustrated in FIG. 2, the first material layer (410) can be formed by sequentially performing an indium precursor (In precursor) providing step, a purge step, an oxygen plasma (O2plasma) providing step, a purge step, a gallium precursor (Ga precursor) providing step, a purge step, an oxygen plasma (O2plasma) providing step, a purge step, a zinc precursor (Zn precursor) providing step, a purge step, an oxygen plasma (O2plasma) providing step, and a purge step.
[0058] For example, the indium precursor may include DADI ((3-Dimethylaminopropyl)dimethylindium).다른 예를 들어, 상기 인듐 전구체는 TMI(Trimethyl indium), TEI(Triethyl indium), InCA-1(Bis(trimethysilyl)amidodiethyl Indium), CpIn(Cyclopentadienylindium), In(tmhd)3((Tris(2,2,6,6-tetramethyl-3,5-heptanedionato) indium (III)), In(acac)3((Indium (III) acetylacetonate), DATI((dimethylbutylamino) trimethylindium), Me2In(EDPA)(dimethyl(Nethoxy-2,2-dimethylpropanamido)indium), InEtCp(ethylcyclopentadienyl indium), TMION(Trimethyl[N-(2-methoxyethyl)-2-methylpropan-2-amine]indium), DMION(Dimethyl[N-(tert-butyl)-2-methoxy-2-methylpropan-1-amine]indium), DMITN(Dimethyl[N1-(tert-butyl)-N2,N2-dimethylethane-1,2-diamine]indium), [In[(i Pr)2CNEt2]3](tris-(N,N'-diisopropyl-2diethylamido-guanidinato)-indium(III)), [In[(i Pr)2CNMe2]3](tris-(N,N'-diisopropyl-2-dimethylamidoguanidinato)-indium(III)), Et2InN(SiMe3)2(diethyl[bis(trimethylsilyl)amido]indium), In(dmamp)3(tris(1-dimethylamino-2-methyl-2-propoxy)indium), 및 tris((N,N'-diisopropylacetamidinato) indium(III)) 중 어느 하나를 포함할 수 있다.
[0059] For example, the gallium precursor may include TMGa (trimethylgallium). For another example, the gallium precursor is TEGa(Triethyl gallium), Ga(acac)3(Gallium acetylacetonate), [(CH3)2GaNH2]3(dimethylgallium amide), Ga2(NMe2)6(hexakis(dimethylamido)digallium), Me2GaOiPr(dimethylgallium isopropoxide), Ga(OiPr)3(gallium) tri-isopropoxide), [Ga(TMHD)3]([tris (2,2,6,6-tetramethyl-3,5-heptanedionato) gallium(III)]), GaCp (pentamethylcyclopentadienyl gallium), [Ga(thd)3](gallium 2,2,6,6-tetramethyl-3,5-heptanedionate), TMGON (Trimethyl[N-(2-methoxyethyl)-2-methylpropan-2-amine]gallium), It may include either DMGON (Dimethyl[N-(tert-butyl)-2-methoxy-2-methylpropan-1-amine]gallium), or DMGTN (Dimethyl[N1-(tert-butyl)-N2,N2-dimethylethane-1,2-diamine]gallium).
[0060] For example, the zinc precursor may include DEZ (diethylzinc). For another example, the zinc precursor may include any one of DMZ (dimethylzinc), ZnCl2 (zinc chloride), Zn(CH3COO)2 (zinc acetate), Zn(eeki)2 (bis[4-((2-ethoxyethyl)imino)-pent-2-en-2-olate]zinc), and BDMPZ (bis-3-(N,N-dimethylamino)propyl zinc).
[0061] According to one embodiment, the indium precursor (In precursor) providing step, the purge step, the oxygen plasma (O2plasma) providing step, and the purge step are included in the first unit process (1 st can be defined as a unit process. In contrast, the gallium precursor (Ga precursor) providing step, the purge step, the oxygen plasma (O2plasma) providing step, and the purge step are defined as a second unit process (2 nd can be defined as a third unit process (3). In contrast, the zinc precursor (Zn precursor) providing step, the purge step, the oxygen plasma (O2plasma) providing step, and the purge step are defined as a third unit process (3 rd unit process). In addition, the first to third unit processes are the first overall process (1 st can be defined as total process.
[0062] The first to third unit processes may each be repeated multiple times. The first overall process may also be repeated multiple times. As the number of repetitions of the first to third unit processes and the number of repetitions of the first overall process are controlled, the thickness of the first material layer (410) may be controlled.
[0063] As described above, since the thickness of the first material layer (410) can be controlled by controlling the number of repetitions of the first overall process, the thickness of the first material layer (410) can be easily controlled. In addition, since the number of repetitions of the first to third unit processes can each be controlled, the composition of indium (In), gallium (Ga), and zinc (Zn) in the first material layer (410) can be easily controlled.
[0064] A second material layer (420) including a metal oxide insulator can be formed on the first material layer (410) using a PEALD (Plasma Enhanced Atomic Layer Deposition) process (S300).
[0065] According to one embodiment, the second material layer (420) may be formed by a reaction between an aluminum (Al) precursor and oxygen plasma (O2plasma). Accordingly, the second material layer (420) may include aluminum oxide (Al2O3). That is, the metal oxide insulator included in the second material layer (420) may be aluminum oxide (Al2O3).
[0066] More specifically, as illustrated in FIG. 3, the second material layer (420) may be formed by sequentially performing an aluminum precursor (Al precursor) providing step, a purge step, an oxygen plasma (O2 plasma) providing step, and a purge step. For example, the aluminum precursor may include trimethyl aluminum (TMA).
[0067] According to one embodiment, the aluminum precursor (Al precursor) providing step, the purge step, the oxygen plasma (O2plasma) providing step, and the purge step comprise a second overall process (2 nd The second total process can be defined as a total process. The second total process can be repeated multiple times. As the number of repetitions of the second total process is controlled, the thickness of the second material layer (420) can be controlled.
[0068] According to one embodiment, the multi-channel characteristics of the channel structure (400) described later can be controlled depending on the thickness of the second material layer (420). Specifically, when the thickness of the second material layer (420) is controlled to be less than 4 nm, the multi-channel characteristics of the channel structure (400) described later can be expressed. Conversely, when the thickness of the second material layer (420) is controlled to be 4 nm or more, a problem may arise in which the multi-channel characteristics of the channel structure (400) described later are not expressed.
[0069] The step (S200) of forming the first material layer (410) and the step (S300) of forming the second material layer (420) can be alternately repeated to manufacture a channel structure (400). That is, the channel structure (400) can have a structure in which the first material layer (410) and the second material layer (420) are alternately and repeatedly laminated.
[0070] According to one embodiment, a structure in which the first material layer (410) and the second material layer (420) are stacked may be defined as a stack. Accordingly, the channel structure (400) may have a structure in which a plurality of stacks are stacked.
[0071] As the above stacks are stacked in multiples, the channel structure (400) can form multiple channels. Specifically, the channel structure (400) in which the multiple stacks are stacked can allow movement of carriers through each of the multiple first material layers (410). The second material layer (420) can act as an insulating layer between the adjacent first material layers (410).
[0072] The transistor to which the above channel structure (400) is applied has a threshold voltage (V) depending on the number of stacks of the above stacks.th ), mobility (μ FE ), and subthreshold swing (SS) characteristics can be controlled.
[0073] In one embodiment, as the number of layers of the stack increases, the threshold voltage (V th ) can be kept practically constant, while the mobility (μ FE ) and subthreshold swing (SS) can increase. In addition, the mobility (μ) according to the increase in the number of stacks of the stack FE ) may be higher than the increase rate of the subthreshold swing (SS).
[0074] According to one embodiment, in order to secure high mobility and high reliability of a transistor to which the channel structure (400) is applied, the number of stacks may be controlled. Specifically, the number of stacks may be controlled to be 5 or more and 10 or less.
[0075] The transistor to which the channel structure (400) is applied, in which the stacks of the above-described range (5 or more and 10 or less) are stacked, has a threshold voltage (V) according to an increase in the number of stacks of the above-described stacks. th ) can be maintained at less than 10%. Specifically, despite the increase in the number of stacks of the above stacks, the threshold voltage (V th ) can be maintained in the range of 0.09 V to 0.19 V. On the other hand, as the number of layers of the stack increases, the mobility (μ FE ) and subthreshold swing (SS) can be improved.
[0076] That is, since the channel structure according to the embodiment of the present invention is manufactured through the PEALD process, thickness and composition control can be easily achieved, and high mobility characteristics can be effectively expressed through thickness and composition control. In addition, not only can the subthreshold swing (SS) be easily controlled, but also the mobility (μ FE) and subthreshold swing (SS) are controlled, but the threshold voltage (V th ) can be maintained substantially constant. Accordingly, it can be easily applied to transistors of display backplanes that require high mobility and high reliability.
[0077]
[0078] Above, a channel structure and a manufacturing method thereof according to an embodiment of the present invention have been described. Below, a thin film transistor to which a channel structure according to an embodiment of the present invention is applied is described.
[0079] FIG. 5 is a drawing for explaining a thin film transistor according to an embodiment of the present invention, FIG. 6 is a schematic cross-sectional view taken along line TT' of FIG. 5, and FIG. 7 is a drawing for explaining various forms of a channel structure included in a thin film transistor according to an embodiment of the present invention.
[0080] Referring to FIGS. 5 and 6, the thin film transistor according to the embodiment may include a substrate (100), a gate (300) disposed on the substrate (100), a gate insulating layer (200) disposed on the substrate (100) and covering the gate (300), a channel structure (400) disposed on the gate insulating layer (200), a source (S) disposed on the gate insulating layer (200) and in contact with one side of the channel structure (400), and a drain (D) disposed on the gate insulating layer (200) and in contact with the other side of the channel structure (400).
[0081] According to one embodiment, the channel structure (400) may be the same as the channel structure (400) described with reference to FIGS. 1 to 4. That is, the thin film transistor according to the embodiment may have a structure in which the channel structure (400) is applied to a thin film transistor having a bottom gate structure. Alternatively, according to another embodiment, the channel structure (400) may also be applied to a thin film transistor having a top gate structure. As illustrated in FIG. 7, the channel structure (400) may have various thicknesses depending on the number of layers of the stack.
[0082] In the above thin film transistor, the channel structure (400) can form a multi-channel. Specifically, in the thin film transistor, carriers can move through each of the plurality of first material layers (410) included in the channel structure (400).
[0083] However, the amount of movement of carriers within the plurality of first material layers (410) may be different from each other. Specifically, the amount of movement of carriers within the first material layer (410) disposed relatively close to the gate (300) may be greater than the amount of movement of carriers within the first material layer (420) disposed relatively far from the gate (300). That is, the first material layer (410) disposed relatively close to the gate (300) may be formed as a main channel, and the first material layer (420) disposed relatively far from the gate (300) may be formed as a sub channel.
[0084] As described above, by controlling the number of stacks forming the channel structure (400), the characteristics (mobility, subthreshold swing) of the thin film transistor can be easily controlled, so that the thin film transistor can be easily applied to the back-plane of a display.
[0085] Specifically, the thin film transistor can be applied to a switching TFT and a driving TFT of a display backplane. However, the switching TFT and the driving TFT may have different stacking numbers of the channel structure (400). For example, a channel structure (400) having one stack may be used for the switching TFT. In contrast, a channel structure (400) having ten stacks may be used for the driving TFT.
[0086] For switching TFTs, fast on / off characteristics are important, and therefore, a lower subthreshold swing (SS) is advantageous. Therefore, by using a channel structure (400) having a single stack, the fast on / off characteristics of the switching TFT can be improved.
[0087] In contrast, for driving TFTs, it is important to read the current value, so the mobility (μ FE ) is higher, the higher the advantage. Therefore, by using a channel structure (400) having 10 stacks, the characteristics of the driving TFT can be improved. In addition, in the case of a channel structure (400) having 10 stacks, since the subthreshold swing (SS) is high, the value of the current can be read in detail at a microvoltage, which has the advantage of low power consumption.
[0088]
[0089] Above, a thin film transistor according to an embodiment of the present invention has been described. Below, specific experimental examples of a channel structure and a thin film transistor according to an embodiment of the present invention are described.
[0090] Manufacturing of channel structures according to experimental examples
[0091] An IGZO material layer was formed on the substrate using a PEALD (Plasma Enhanced Atomic Layer Deposition) process, and an Al2O3 material layer was formed on the IGZO material layer using a PEALD process.
[0092] Specifically, DADI ((3-Dimethylaminopropyl)dimethylindium) was used as an indium precursor, TMGa (trimethylgallium) was used as a gallium precursor, DEZ (diethylzinc) was used as a zinc precursor, TMA (trimethyl aluminum) was used as an aluminum precursor, and oxygen plasma (O2plasma) was used as a reactant. The oxygen plasma (O2plasma) was provided with a power of 100 W, and the PEALD process was performed at a temperature of 200°C.
[0093] In addition, a structure in which an IGZO material layer and an Al2O3 material layer are laminated is made into 1 stack, and a total of 10 stacks are laminated to manufacture a channel structure according to the experimental example above.
[0094]
[0095] Figure 8 is a STEM image of a channel structure according to an experimental example of the present invention.
[0096] Referring to Fig. 8, a STEM (Scanning Transmission Electron Microscope) image of the channel structure according to the experimental example is shown. As can be seen in Fig. 8, it was confirmed that the IGZO material layer and the Al2O3 material layer had a structure in which they were alternately and repeatedly laminated. In addition, it was confirmed that the IGZO material layer had a thickness of 2.22 nm, and the Al2O3 material layer had a thickness of 3.45 nm.
[0097] FIG. 9 and FIG. 10 are drawings for explaining the EDS analysis results of a channel structure according to an experimental example of the present invention.
[0098] Referring to Fig. 9, the EDS (Energy Dispersive X-ray Spectroscopy) analysis results of the channel structure according to the above experimental example are shown, and referencing Fig. 10, the EDS line scan results are shown.
[0099] Through Fig. 9, the composition distribution of the IGZO material layer and the Al2O3 material layer can be confirmed, and through Fig. 10, it can be confirmed that the IGZO material layer and the Al2O3 material layer are laminated in a 1D distribution.
[0100]
[0101] Preparation of thin film transistor according to Experimental Example 1-1
[0102] A thin film transistor having a bottom gate structure to which a channel structure according to the above experimental example is applied is prepared, and a channel structure having 1 stack is prepared.
[0103]
[0104] Preparation of thin film transistor according to Experimental Example 1-2
[0105] A thin film transistor having a bottom gate structure to which a channel structure according to the above experimental example is applied was prepared, and a channel structure having 3 stacks was prepared.
[0106]
[0107] Preparation of thin film transistors according to Experimental Example 1-3
[0108] A thin film transistor having a bottom gate structure to which a channel structure according to the above experimental example is applied was prepared, and a channel structure having 5 stacks was prepared.
[0109]
[0110] Preparation of thin film transistors according to Experimental Example 1-4
[0111] A thin film transistor having a bottom gate structure to which a channel structure according to the above experimental example is applied is prepared, and a channel structure having 10 stacks is prepared.
[0112]
[0113] Preparation of thin film transistors according to Experimental Example 1-5
[0114] A thin film transistor having a bottom gate structure to which a channel structure according to the above experimental example is applied is prepared, and a channel structure having 12 stacks is prepared.
[0115]
[0116] Preparation of thin film transistors according to Experimental Example 1-6
[0117] A thin film transistor having a bottom gate structure to which a channel structure according to the above experimental example is applied was prepared, and a channel structure having 14 stacks was prepared.
[0118]
[0119] Preparation of thin film transistors according to Experimental Example 1-7
[0120] A thin film transistor having a bottom gate structure to which a channel structure according to the above experimental example is applied was prepared, and a channel structure having 16 stacks was prepared.
[0121]
[0122] Preparation of thin film transistors according to Experimental Example 1-8
[0123] A thin film transistor having a bottom gate structure to which a channel structure according to the above experimental example is applied was prepared, and a channel structure having 18 stacks was prepared.
[0124]
[0125] Preparation of thin film transistors according to Experimental Example 1-9
[0126] A thin film transistor having a bottom gate structure to which a channel structure according to the above experimental example is applied was prepared, and a channel structure having 20 stacks was prepared.
[0127]
[0128] Number of stacks Experimental example 1-11 Experimental example 1-23 Experimental example 1-35 Experimental example 1-410 Experimental example 1-512 Experimental example 1-614 Experimental example 1-716 Experimental example 1-818 Experimental example 1-920
[0129] FIG. 11 is a drawing for explaining the electrical characteristics of a thin film transistor according to Experimental Examples 1-1 to 1-4 of the present invention.
[0130] Referring to Fig. 11, for each of the thin film transistors according to the experimental examples 1-1 to 1-4, the threshold voltage (V th , V), mobility (cm 2 / Vs), and subthreshold swing (SS, V / decade).
[0131] As can be seen in Fig. 11, as the number of stacks constituting the channel structure increases (1->10), the mobility and subthreshold swing increase. On the other hand, the threshold voltage was confirmed to remain substantially constant despite the increase in the number of stacks. In addition, the rate of increase in mobility due to the increase in the number of stacks was confirmed to be higher than the rate of increase in the subthreshold swing. The specific measured values are summarized in below.
[0132] FIG. 12 is a diagram for comparing TCAD simulation results of thin film transistors according to experimental examples 1-1 to 1-9 of the present invention.
[0133] Referring to Fig. 12, TCAD simulation was performed for each thin film transistor according to the experimental examples 1-1 to 1-9 to determine the threshold voltage (V th , V), mobility (cm 2 / Vs), and subthreshold swing (SS, V / decade) were measured. The specific measured values are summarized in below. That is, in , the actually measured values are shown for Experimental Examples 1-1 to 1-4, and the values measured through TCAD simulation are shown for Experimental Examples 1-5 to 1-9.
[0134] Threshold voltage (V) th , V) mobility (μ) FE , cm 2 / Vs)Subthreshold swing (SS, V / decade)Experimental example 1-1 (1 stack) 0.22 ± 0.02 1.34 ± 0.2 10.31 ± 0.01Experimental example 1-2 (3 stack) 0.19 ± 0.05 2.40 ± 0.19 0.31 ± 0.02Experimental example 1-3 (5 stack) 0.13 ± 0.04 2.94 ± 0.10 0.36 ± 0.02Experimental example 1-4 (10 stack) 0.16 ± 0.03 4.33 ± 0.08 0.45 ± 0.02Experimental example 1-5 (12 stack) 0.41 3.57 0.47Experimental example 1-6 (14 stack) 0.44 3.41 0.46Experimental example 1-7 (16 stack)0.473.380.46Experimental Example 1-8(18 stack)0.633.370.47Experimental Example 1-9(20 stack)1.273.100.46
[0135] As can be seen in , when the number of stacks increases from 1 to 10, the mobility also increases (1.34 -> 4.33 cm). 2 / Vs), when it exceeds 10, the mobility decreases (4.33 -> 3.10 cm) 2 / Vs) was observed. In addition, it was confirmed that the subthreshold swing increased (0.31 -> 0.45 V / decade) when the number of stacks increased from 1 to 10, but became practically constant (0.45~0.47 V / decade) when the number of stacks exceeded 10. In addition, it was confirmed that the threshold voltage remained practically constant (0.13~0.22 V) when the number of stacks increased from 1 to 10, but increased (0.16 -> 1.27 V) when the number of stacks exceeded 10.
[0136] Therefore, it can be seen that in order to increase the mobility and subthreshold swing through stack increase while keeping the threshold voltage practically constant, the number of stacks should be controlled to 10 or less.
[0137] In addition, it can be seen that in order to have high mobility while maintaining the threshold voltage substantially constant and to easily control the subthreshold swing, the number of stacks must be controlled to be 5 or more and 10 or less.
[0138] Specifically, when the number of stacks is controlled to be 5 or more and 10 or less, the threshold voltage is maintained in the range of a minimum of 0.09 V to a maximum of 0.19 V despite the increase in stacks, with a variation of less than 10%, while the mobility can have a value of a maximum of 4.41 cm2 / Vs, indicating high mobility, and the subthreshold swing can be controlled from a minimum of 0.34 V / decade to a maximum of 0.47 V / decade.
[0139]
[0140] Preparation of thin film transistor according to Experimental Example 2-1
[0141] A thin film transistor having a bottom gate structure to which a channel structure according to the above experimental example is applied was prepared, and a channel structure having 3 stacks was prepared.
[0142] Additionally, the IGZO material layer was prepared to have a thickness of 1 nm, and the Al2O3 material layer was prepared to have a thickness of 3 nm.
[0143]
[0144] Preparation of thin film transistor according to Experimental Example 2-2
[0145] A thin film transistor having a bottom gate structure to which a channel structure according to the above experimental example is applied was prepared, and a channel structure having 3 stacks was prepared.
[0146] Additionally, the IGZO material layer was prepared to have a thickness of 2 nm, and the Al2O3 material layer was prepared to have a thickness of 3 nm.
[0147]
[0148] Preparation of thin film transistor according to Experimental Example 2-3
[0149] A thin film transistor having a bottom gate structure to which a channel structure according to the above experimental example is applied was prepared, and a channel structure having 3 stacks was prepared.
[0150] Additionally, the IGZO material layer was prepared to have a thickness of 3 nm, and the Al2O3 material layer was prepared to have a thickness of 3 nm.
[0151]
[0152] Preparation of thin film transistor according to Experimental Example 2-4
[0153] A thin film transistor having a bottom gate structure to which a channel structure according to the above experimental example is applied was prepared, and a channel structure having 3 stacks was prepared.
[0154] Additionally, the IGZO material layer was prepared to have a thickness of 2 nm, and the Al2O3 material layer was prepared to have a thickness of 1 nm.
[0155]
[0156] Preparation of thin film transistor according to Experimental Example 2-5
[0157] A thin film transistor having a bottom gate structure to which a channel structure according to the above experimental example is applied was prepared, and a channel structure having 3 stacks was prepared.
[0158] Additionally, the IGZO material layer was prepared to have a thickness of 2 nm, and the Al2O3 material layer was prepared to have a thickness of 3 nm.
[0159]
[0160] Preparation of thin film transistor according to Experimental Example 2-6
[0161] A thin film transistor having a bottom gate structure to which a channel structure according to the above experimental example is applied was prepared, and a channel structure having 3 stacks was prepared.
[0162] Additionally, the IGZO material layer was prepared to have a thickness of 2 nm, and the Al2O3 material layer was prepared to have a thickness of 5 nm.
[0163]
[0164] Number of stacks IGZO material layer thickness Al2O3 material layer thickness Experimental example 2-1 313 Experimental example 2-2 323 Experimental example 2-3 333 Experimental example 2-4 321 Experimental example 2-5 323 Experimental example 2-6 325
[0165] FIG. 13 is a drawing for explaining the electrical characteristics of a thin film transistor according to Experimental Examples 2-1 to 2-6 of the present invention.
[0166] Figure 13 (a) shows the electrical characteristics of the thin film transistor according to the above experimental examples 2-1 to 2-3, and Figure 13 (b) shows the electrical characteristics of the thin film transistor according to the above experimental examples 2-4 to 2-6.
[0167] As can be seen in (a) of Fig. 13, when the thickness of the Al2O3 material layer is fixed at 3 nm and the thickness of the IGZO material layer is changed from 1 nm to 3 nm, it was confirmed that the electrical characteristics of the thin film transistor (Experimental Example 2-2) having the IGZO material layer with a thickness of 2 nm were the highest.
[0168] As can be seen in (b) of Fig. 13, when the thickness of the IGZO material layer is fixed at 2 nm and the thickness of the Al2O3 material layer is changed from 1 nm to 5 nm, it can be confirmed that the electrical characteristics decrease as the thickness of the Al2O3 material layer increases. The electrical characteristic measurement results of the thin film transistors according to the experimental examples 2-4 to 2-6 are summarized in below.
[0169] Classification Experiment Example 2-4 Experiment Example 2-5 Experiment Example 2-6V th [V]-1.21 ± 0.080.19 ± 0.051.01 ± 0.12μ FE [cm 2 / Vs]2.53 ± 0.312.40 ± 0.190.11 ± 0.01SS [V / decade]0.60 ± 0.030.31 ± 0.020.86 ± 0.03
[0170] Preparation of thin film transistor according to Experimental Example 3-1
[0171] A thin film transistor having a bottom gate structure to which a channel structure according to the above experimental example is applied was prepared, and a channel structure having 3 stacks was prepared.
[0172] Additionally, the IGZO material layer was prepared to have a thickness of 1 nm, and the Al2O3 material layer was prepared to have a thickness of 3 nm.
[0173]
[0174] Preparation of thin film transistor according to Experimental Example 3-2
[0175] A thin film transistor having a bottom gate structure to which a channel structure according to the above experimental example is applied was prepared, and a channel structure having 3 stacks was prepared.
[0176] Additionally, the IGZO material layer was prepared to have a thickness of 4 nm, and the Al2O3 material layer was prepared to have a thickness of 3 nm.
[0177]
[0178] Preparation of thin film transistor according to Experimental Example 3-3
[0179] A thin film transistor having a bottom gate structure to which a channel structure according to the above experimental example is applied was prepared, and a channel structure having 3 stacks was prepared.
[0180] Additionally, the IGZO material layer was prepared to have a thickness of 8 nm, and the Al2O3 material layer was prepared to have a thickness of 3 nm.
[0181]
[0182] Number of stacks IGZO material layer thickness Al2O3 material layer thickness Experimental example 3-1313 Experimental example 3-2343 Experimental example 3-3383
[0183] FIG. 14 is a drawing for explaining the simulation results of a thin film transistor according to experimental examples 3-1 to 3-3 of the present invention.
[0184] Referring to Fig. 14, the current density mapping simulation results are shown for each thin film transistor according to Experimental Examples 3-1 to 3-3. Specifically, V GS 20V, V DS Shows the results at 20.1 V.
[0185] As can be seen in Fig. 14, when the thickness of the Al2O3 material layer is fixed at 3 nm, it was confirmed that multi-channel formation was easily achieved even when the thickness of the IGZO material layer was changed from 1 nm to 8 nm.
[0186]
[0187] Preparation of thin film transistor according to Experimental Example 4-1
[0188] A thin film transistor having a bottom gate structure to which a channel structure according to the above experimental example is applied was prepared, and a channel structure having 3 stacks was prepared.
[0189] Additionally, the IGZO material layer was prepared to have a thickness of 2 nm, and the Al2O3 material layer was prepared to have a thickness of 1 nm.
[0190]
[0191] Preparation of thin film transistor according to Experimental Example 4-2
[0192] A thin film transistor having a bottom gate structure to which a channel structure according to the above experimental example is applied was prepared, and a channel structure having 3 stacks was prepared.
[0193] Additionally, the IGZO material layer was prepared to have a thickness of 2 nm, and the Al2O3 material layer was prepared to have a thickness of 4 nm.
[0194]
[0195] Preparation of thin film transistor according to Experimental Example 4-3
[0196] A thin film transistor having a bottom gate structure to which a channel structure according to the above experimental example is applied was prepared, and a channel structure having 3 stacks was prepared.
[0197] Additionally, the IGZO material layer was prepared to have a thickness of 2 nm, and the Al2O3 material layer was prepared to have a thickness of 8 nm.
[0198]
[0199] Number of stacks IGZO material layer thickness Al2O3 material layer thickness Experimental example 4-1321 Experimental example 4-2324 Experimental example 4-3328
[0200] FIG. 15 is a drawing for explaining the simulation results of a thin film transistor according to experimental examples 4-1 to 4-3 of the present invention.
[0201] Referring to Fig. 15, the current density mapping simulation results are shown for each thin film transistor according to the experimental examples 4-1 to 4-3. Specifically, V GS 20V, V DS Shows the results at 20.1 V.
[0202] As can be seen in Fig. 15, multi-channels were formed in the thin film transistor according to Experimental Example 4-1, but multi-channels were not formed in the thin film transistors according to Experimental Examples 4-2 and 4-3. Accordingly, it can be seen that the thickness of the Al2O3 material film must be controlled to less than 4 nm to form multi-channels.
[0203]
[0204] Preparation of thin film transistor according to Experimental Example 5-1
[0205] A thin film transistor having a bottom gate structure to which a channel structure according to the above experimental example is applied was prepared, and a channel structure having 3 stacks was prepared.
[0206] Additionally, the IGZO material layer was prepared to have a thickness of 1 nm, and the Al2O3 material layer was prepared to have a thickness of 1 nm.
[0207]
[0208] Preparation of thin film transistor according to Experimental Example 5-2
[0209] A thin film transistor having a bottom gate structure to which a channel structure according to the above experimental example is applied was prepared, and a channel structure having 3 stacks was prepared.
[0210] Additionally, the IGZO material layer was prepared to have a thickness of 2 nm, and the Al2O3 material layer was prepared to have a thickness of 1 nm.
[0211]
[0212] Preparation of thin film transistor according to Experimental Example 5-3
[0213] A thin film transistor having a bottom gate structure to which a channel structure according to the above experimental example is applied was prepared, and a channel structure having 3 stacks was prepared.
[0214] Additionally, the IGZO material layer was prepared to have a thickness of 5 nm, and the Al2O3 material layer was prepared to have a thickness of 1 nm.
[0215]
[0216] Number of stacks IGZO material layer thickness Al2O3 material layer thickness Experimental example 5-1311 Experimental example 5-2321 Experimental example 5-3351
[0217] FIG. 16 is a drawing for explaining the simulation results of a thin film transistor according to experimental examples 5-1 to 5-3 of the present invention.
[0218] Referring to Fig. 16, the current density mapping simulation results are shown for each thin film transistor according to Experimental Examples 5-1 to 5-3. Specifically, V GS 20V, V DS Shows the results at 20.1 V.
[0219] As can be seen in Fig. 16, when the thickness of the Al2O3 material layer is fixed at 1 nm, it was confirmed that multi-channel formation was not easily achieved as the thickness of the IGZO material layer increased.
[0220] Figure 17 is a graph comparing electrical characteristics of insulators according to their k values.
[0221] Referring to Figure 17, the electrical characteristic changes according to the k value change of the insulator in a channel structure having a stacked structure of an oxide semiconductor and an insulator are shown through the results of TCAD simulation. As can be confirmed in Figure 17, it was confirmed that the lower the k value of the insulator, the higher the mobility tends to be.
[0222] FIG. 18 and FIG. 19 are drawings for comparing the amount of carrier movement within the channel structure of the thin film transistor according to Experimental Examples 1-1 to 1-4 of the present invention.
[0223] Referring to FIGS. 18 and 19, simulation results for carrier movement within each channel structure are shown after preparing thin film transistors according to Experimental Examples 1-1 to 1-4. Specifically, (a) of FIG. 18 shows the result of Experimental Example 1-1, (b) of FIG. 18 shows the result of Experimental Example 1-2, (c) of FIG. 18 shows the result of Experimental Example 1-3, and (d) of FIG. 18 shows the result of Experimental Example 1-4.
[0224] As can be seen in FIGS. 18 and 19, it was confirmed that a relatively large amount of carriers were moved in the IGZO material layer placed at a relatively close distance from the gate, and a relatively small amount of carriers were moved in the IGZO material layer placed at a relatively far distance from the gate.
[0225]
[0226] While the present invention has been described in detail using preferred embodiments, the scope of the present invention is not limited to the specific embodiments described above, and should be interpreted in accordance with the appended claims. Furthermore, those skilled in the art will appreciate that numerous modifications and variations are possible without departing from the scope of the present invention.
[0227] The present invention can be used in the semiconductor industry.
Claims
1. In a thin film transistor including a channel structure in which a first material layer including an oxide semiconductor and a second material layer including a metal oxide insulator are stacked, The above channel structure is formed by stacking a plurality of stacks of the first material layer and the second material layer to form a multi-channel, A thin film transistor including an increase in mobility and subthreshold swing as the number of layers of the stack increases.
2. In paragraph 1, A thin film transistor including a rate of increase in mobility according to an increase in the number of layers of the above stack is higher than a rate of increase in subthreshold voltage swing.
3. In paragraph 1, A thin film transistor, wherein even if the number of layers of the above stack increases, the change in threshold voltage is maintained at 10% or less.
4. In paragraph 3, A thin film transistor including a threshold voltage maintained in a range of 0.09 V to 0.19 V even when the number of layers of the stack increases.
5. In paragraph 1, A thin film transistor comprising a stack having a number of layers of 5 or more and 10 or less.
6. In paragraph 1, A thin film transistor comprising a second material layer having a thickness of less than 4 nm.
7. In paragraph 1, The above oxide semiconductor is a thin film transistor including IGZO (Indium Gallium Zinc Oxide).
8. In paragraph 1, The above metal oxide insulator is a thin film transistor including aluminum oxide (Al2O3).
9. In paragraph 1, A thin film transistor, wherein the amount of movement of carriers within the first material layer arranged relatively close to the gate is greater than the amount of movement of carriers within the first material layer arranged relatively far from the gate.
10. Step for preparing the substrate; A step of forming a first material layer including an oxide semiconductor on the substrate by a PEALD (plasma-enhanced atomic layer deposition) process; and A step of forming a second material layer including a metal oxide insulator on the first material layer by a PEALD process, A method for manufacturing a channel structure, comprising forming a multi-channel by alternately repeating the step of forming the first material layer and the step of forming the second material layer.
11. In paragraph 10, The step of forming the first material layer is: On the above substrate, a step of reacting an indium (In) precursor, a gallium (Ga) precursor, a zinc (Zn) precursor, and oxygen plasma (O2plasma) is included, The step of forming the second material layer is: A method for manufacturing a channel structure, comprising a step of reacting an aluminum (Al) precursor and oxygen plasma (O2plasma) on the first material layer.
12. In paragraph 10, A method for manufacturing a channel structure, comprising forming the first material layer and the second material layer through an in-situ process.
Citation Information
Patent Citations
Semiconductor device and method of manufacturing same
KR1020140086911A
Semiconductor device
KR1020180087473A
Method and apparatus of user equipment for handling short-time switching gap configuration information in mobile communication system
KR1020220134365A
Positive current collector for lithium secondary battery, method of manufacturing the same and lithium secondary battery including the same
KR1020240061401A
Ultrasonic inspection device and ultrasonic inspection method using the same