Catalyst with improved durability, method for producing same, and method for dehydrogenating ammonia using same
Chemical coating of hexagonal boron nitride on transition metal particles supported on substrates addresses compatibility issues in hexagonal boron nitride-based catalysts, enhancing durability and activity for ammonia decomposition and dehydrogenation reactions.
Patent Information
- Application Number
- PCT/KR2024/005211
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-19
- Filing Date
- 2024-04-18
- Publication Date
- 2024-10-24
AI Technical Summary
Hexagonal boron nitride-based catalysts face challenges in compatibility due to the difficulty in pelletizing the powder form and low adhesion of physically coated layers, limiting their application in large-capacity ammonia decomposition systems.
A method involving chemical coating of hexagonal boron nitride on transition metal particles supported on various substrates, using an ammonia borane solution in a polar aprotic solvent, followed by heat treatment, to enhance catalyst durability and compatibility.
The approach results in a highly compatible catalyst with improved durability, maintaining high ammonia decomposition and dehydrogenation activity over long periods, even under external physical, chemical, or mechanical stress.
Smart Images

Figure KR2024005211_24102024_PF_FP_ABST
Abstract
Description
Catalyst with improved durability, method for producing the same, and method for dehydrogenating ammonia using the same
[0001] [Cross-reference to related applications]
[0002] This application claims priority to Republic of Korea Patent Application No. 10-2023-0051194, filed April 19, 2023, the entire contents of which are incorporated herein by reference.
[0003] [Description of Nationally Supported Research and Development]
[0004] This research was conducted at the Korea Institute of Science and Technology (KIST) under the management of the Korea Institute of Science and Technology (KIST) under the Ministry of Science and ICT. The research project name is KIST-Industry Bridge Program, supported by the Korea Institute of Science and Technology Research Operations Expenses Support (R&D) (Main Project Expenses). The research project name is KIST-Industry Bridge Program (Project Identification Number: 1711152092).
[0005] In addition, this study was conducted at the Korea Institute of Science and Technology (KIST) under the management of the Korea Institute of Science and Technology (KIST) under the Ministry of Science and ICT. The research project name is KIST Research Operation Expense Support (Main Project Expense), and the research project name is KIST-Industry Bridge Program (Project Unique Number: 1711173223).
[0006] The present disclosure discloses a catalyst with improved durability, a method for producing the same, and a method for dehydrogenating ammonia using the same.
[0007] Ammonia possesses a hydrogen storage capacity of 17.7% by weight and can be easily liquefied under relatively low pressures of 8 bar, making it a key material for solving hydrogen storage and transportation problems. High-temperature decomposition of ammonia produces hydrogen, which is used as fuel in energy-generating devices such as fuel cells and hydrogen turbines. Producing hydrogen from ammonia requires an ammonia decomposition reactor and, if necessary, an adsorption process to remove unreacted ammonia. The fields and scale of hydrogen demand are expanding, necessitating technologies capable of processing large quantities of hydrogen from ammonia. In particular, transition metals such as Ru, Ni, Fe, Co, and Rh can be used as catalysts in the ammonia decomposition reactor to lower the activation energy of the reaction.
[0008] In terms of catalyst shape, catalysts in the shape of beads, pellets, monoliths, honeycombs, etc., rather than powders that cause pressure drops, are more practical for ammonia decomposition or synthesis processes. Recently, a study reported that Ru / h-BN catalysts using hexagonal boron nitride as a support were effective in ammonia decomposition activity due to the heteroepitaxy effect (metal particles grow while maintaining continuity with the support lattice) and the effect of increasing electron density. However, because this hexagonal boron nitride support is a powder, it has the disadvantage of being difficult to apply to actual large-scale ammonia decomposition reaction systems. In particular, hexagonal boron nitride powder is difficult to pelletize, and the method of physically coating the hexagonal boron nitride powder exhibits low adhesion, which reduces the compatibility of hexagonal boron nitride-based catalysts. Therefore, technological development for hexagonal boron nitride-based catalysts to improve catalyst compatibility is necessary.
[0009] In one aspect, the present disclosure aims to provide a catalyst with improved durability.
[0010] In another aspect, the present disclosure aims to provide a method for preparing a catalyst having improved durability.
[0011] In another aspect, the present disclosure aims to provide a method for synthesizing hexagonal boron nitride on transition metal particles supported on a support.
[0012] In another aspect, the present disclosure aims to provide a method for dehydrogenating ammonia using the catalyst having improved durability.
[0013] In one aspect, the present disclosure provides a catalyst having improved durability, comprising: a support; a transition metal supported on the support; and hexagonal boron nitride synthesized on the transition metal.
[0014] In an exemplary embodiment, the support may be at least one selected from the group consisting of carbon, silica, silicon carbide, silicon nitride, alumina, magnesium oxide, magnesium aluminate, calcium oxide, calcium aluminate, zeolite, zirconia, titania, ceria, lanthania, yttria, and rare earth oxides.
[0015] In an exemplary embodiment, the transition metal may be at least one selected from the group consisting of Mo, Ni, Fe, Co, Cu, Pd, Pt, Ru, Rh, Au, and Ir.
[0016] In an exemplary embodiment, the hexagonal boron nitride may be synthesized from ammonia borane (AB).
[0017] In an exemplary embodiment, the hexagonal boron nitride may be synthesized by applying an ammonia borane solution on a transition metal supported on the support and then heat-treating it under an ammonia atmosphere.
[0018] In an exemplary embodiment, the ammonia borane solution may contain ammonia borane in a polar aprotic solvent.
[0019] In an exemplary embodiment, the polar aprotic solvent may include at least one selected from tetrahydrofuran (THF), 1,2-dimethoxyethane (DME), dioxane (DXN), diethyleneglycoldimethylether (Diglyme), dimethylformamide (DMF), dimethylsulfoxide (DMSO), dimethylacetamide (DMA), and hexamethyl phosphoramide (HMPA).
[0020] In an exemplary embodiment, the polar aprotic solvent may have a boiling point of 100° C. or less.
[0021] In an exemplary embodiment, the molar concentration of the ammonia borane solution may be 0.2 mol / L or greater.
[0022] In an exemplary embodiment, the volume per mL of the polar aprotic solvent contained in the ammonia borane solution may be 0.5 times or less of the total weight per g of the support and transition metal.
[0023] In an exemplary embodiment, the hexagonal boron nitride may be included in an amount of less than 0.5 wt% based on the total weight of the support and transition metal.
[0024] In another aspect, the present disclosure provides a method for preparing a catalyst having improved durability, the method comprising the steps of: (1) preparing a catalyst comprising a support and a transition metal supported on the support; (2) preparing an ammonia borane solution by adding ammonia borane to a polar aprotic solvent; and (3) applying the ammonia borane solution onto the prepared catalyst.
[0025] In an exemplary embodiment, the method may further include a step of applying an ammonia borane solution in step (3) and then heat-treating the catalyst under an ammonia atmosphere.
[0026] In an exemplary embodiment, the heat treatment may be performed at 600 to 700°C.
[0027] In an exemplary embodiment, the step (1) may be a process of obtaining a catalyst by impregnating a support with a transition metal precursor solution and calcining the support impregnated with the transition metal precursor solution.
[0028] In another aspect, the present disclosure provides a method for dehydrogenating ammonia using the catalyst with improved durability, the method comprising the steps of: (1) charging the catalyst with improved durability into a reactor and then reducing it under a hydrogen atmosphere; and (2) injecting ammonia into the reactor and performing a heat treatment.
[0029] In one aspect, the technology disclosed in the present disclosure has the effect of providing a catalyst with improved durability.
[0030] In another aspect, the technology disclosed in the present disclosure has the effect of providing a method for producing a catalyst with improved durability.
[0031] In another aspect, the technology disclosed in the present disclosure provides a method for synthesizing hexagonal boron nitride on transition metal particles supported on a support. The method uses ammonia borane as a synthetic material for hexagonal boron nitride, coats polyborazylene on the transition metal particles supported on the support at room temperature, and then performs an additional ammonia heat treatment process to ultimately synthesize hexagonal boron nitride.
[0032] Hexagonal boron nitride powder is difficult to pelletize, and methods for physically coating hexagonal boron nitride powder exhibit low adhesion, resulting in low compatibility of existing catalysts based on hexagonal boron nitride. The present disclosure provides an effect that can significantly improve the compatibility of hexagonal boron nitride-based catalysts by chemically coating boron nitride onto the metal particles of the catalyst.
[0033] In another aspect, the technology disclosed in the present disclosure has the effect of providing a method for dehydrogenating ammonia using a catalyst with improved durability.
[0034] Figure 1 illustrates a flow chart for synthesizing hexagonal boron nitride on a catalyst according to one embodiment.
[0035] Figure 2 shows the results of room-temperature coating of polyborazylene on a catalyst according to one embodiment. The left photo shows catalyst No. 3, and the right photo shows catalyst No. 9.
[0036] FIG. 3 illustrates a room temperature coating process of polyborazylene on a catalyst in the preparation of catalyst No. 9 according to one embodiment.
[0037] Figure 4 shows the results of coating hexagonal boron nitride on a catalyst according to one embodiment. The left photo shows catalyst No. 1, and the right photo shows catalyst No. 9.
[0038] Figure 5 shows the results of coating hexagonal boron nitride on a catalyst according to one embodiment. The left photo shows catalyst No. 6, and the right photo shows catalyst No. 7.
[0039] Figure 6 shows the XPS analysis results of a catalyst surface according to one embodiment.
[0040] Fig. 7 shows the XPS analysis results of the catalyst surface of No. 7 according to one embodiment.
[0041] Fig. 8 shows the XPS analysis results of the catalyst surface of No. 9 according to one embodiment.
[0042] Figure 9 shows the results of an ammonia decomposition reaction using a catalyst according to one embodiment.
[0043] Figure 10 shows the results of an ammonia decomposition reaction using a catalyst according to one embodiment.
[0044] Figure 11 shows the results of scanning transmission electron microscopy (STEM) and energy dispersive spectroscopy (EDS) analysis of catalyst No. 2 according to a comparative example.
[0045] Fig. 12 shows the results of TEM-EDS mapping analysis for the catalyst of No. 9 according to one embodiment.
[0046] Figure 13 shows the XRD analysis results for a catalyst according to one embodiment.
[0047] Figure 14 shows the results of visually confirming the dispersion of an ammonia borane solution used in the preparation of a catalyst according to one embodiment.
[0048] Figure 15 shows the results of coating hexagonal boron nitride on a catalyst according to one embodiment.
[0049] Hereinafter, the present disclosure is described in detail.
[0050] In one aspect, the present disclosure provides a catalyst comprising: a support; a transition metal supported on the support; and hexagonal boron nitride synthesized on the transition metal.
[0051] In another aspect, the present disclosure provides a catalyst having improved durability, comprising: a support; a transition metal supported on the support; and hexagonal boron nitride synthesized on the transition metal.
[0052] In an exemplary embodiment, the catalyst may be a hexagonal boron nitride grown directly on transition metal particles of a pre-synthesized catalyst.
[0053] In an exemplary embodiment, the catalyst and / or the synthesized catalyst may have a bead, pellet, monolith, or honeycomb form. This has the effect of providing a highly compatible catalyst.
[0054] In the catalyst according to the present disclosure, hexagonal boron nitride causes particle deformation of the metal, which provides an effect of offsetting deactivation due to agglomeration of the metal, thereby improving the durability of the catalyst.
[0055] In an exemplary embodiment, the catalyst may be a catalyst for an ammonia decomposition reaction.
[0056] In an exemplary embodiment, the catalyst may be a catalyst for the dehydrogenation reaction of ammonia.
[0057] In an exemplary embodiment, the catalyst may have improved durability against ammonia decomposition and / or ammonia dehydrogenation. For example, durability refers to the property of the catalyst to withstand external physical, chemical, or mechanical actions over a long period of time without deterioration or deformation from its original state.
[0058] The catalyst according to the present disclosure has the effect of not only providing high ammonia decomposition reaction activity and / or ammonia dehydrogenation reaction activity, but also providing high ammonia decomposition reaction activity and / or ammonia dehydrogenation reaction activity without degradation of catalyst performance even over a long period of time.
[0059] In an exemplary embodiment, the support may be at least one selected from the group consisting of carbon, silica, silicon carbide, silicon nitride, alumina, magnesium oxide, magnesium aluminate, calcium oxide, calcium aluminate, zeolite, zirconia, titania, and rare earth oxides.
[0060] In an exemplary embodiment, the rare earth element may be at least one selected from the group consisting of Sc, Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu.
[0061] In an exemplary embodiment, the rare earth oxide may be one or more of ceria, lanthanum, yttria, and gadolium oxide.
[0062] In an exemplary embodiment, the transition metal may be at least one selected from the group consisting of Mo, Ni, Fe, Co, Cu, Pd, Pt, Ru, Rh, Au, and Ir.
[0063] In an exemplary embodiment, the support may be alumina and the transition metal may be Ru or Ni.
[0064] In an exemplary embodiment, the transition metal may be supported in an amount of 10 wt% or less based on the total weight of the support and the transition metal.
[0065] In an exemplary embodiment, the hexagonal boron nitride may be synthesized from ammonia borane (H3NBH3).
[0066] In an exemplary embodiment, the hexagonal boron nitride may be synthesized by applying an ammonia borane solution onto a transition metal supported on the support and then heat treating the solution under an ammonia atmosphere. The ammonia borane solution is applied at room temperature and pressure.
[0067] In an exemplary embodiment, the ammonia borane solution may contain ammonia borane in a polar aprotic solvent to induce a dehydrogenation reaction of ammonia borane.
[0068] In an exemplary embodiment, the ammonia borane solution may be ammonia borane dispersed by ultrasonic treatment. The high dispersion process resulting from ultrasonic treatment has the effect of further improving the uniformity of the hexagonal boron nitride coating film.
[0069] In an exemplary embodiment, the polar aprotic solvent may include at least one selected from tetrahydrofuran (THF), 1,2-dimethoxyethane (DME), dioxane (DXN), diethyleneglycoldimethylether (Diglyme), dimethylformamide (DMF), dimethylsulfoxide (DMSO), dimethylacetamide (DMA), and hexamethyl phosphoramide (HMPA).
[0070] In the catalyst according to the present disclosure, the evaporation time of the solvent may vary during the room temperature coating process of a nitrogen-boron compound, such as polyborazylene, depending on the boiling point and vapor pressure characteristics of the polar aprotic solvent itself, and therefore it may be preferable to use a polar aprotic solvent with a relatively low boiling point. For example, the boiling point of Diglyme is 162°C, which is higher than the boiling point (53°C) of borazine, a substance that can change into hexagonal boron nitride among the products, and thus it may take a relatively long time to evaporate the solvent. Therefore, the polar aprotic solvent may preferably be, for example, tetrahydrofuran (THF).
[0071] In one exemplary embodiment, the polar aprotic solvent may have a boiling point of 100° C. or less, 90° C. or less, 80° C. or less, 70° C. or less, 60° C. or less, or 50° C. or less. In another exemplary embodiment, the polar aprotic solvent may preferably have a boiling point of 40 to 80° C., or 45 to 75° C., or 50 to 70° C.
[0072] In one exemplary embodiment, the molar concentration of the ammonia borane solution may be at least 0.2 mol / L. In another exemplary embodiment, the molar concentration of the ammonia borane solution may be at least 0.2 mol / L, at least 0.3 mol / L, at least 0.4 mol / L, or at least 0.5 mol / L, and at most 2.0 mol / L, at most 1.9 mol / L, at most 1.8 mol / L, at most 1.7 mol / L, at most 1.6 mol / L, at most 1.5 mol / L, at most 1.4 mol / L, at most 1.3 mol / L, at most 1.2 mol / L, at most 1.1 mol / L, at most 1.0 mol / L, at most 0.9 mol / L, at most 0.8 mol / L, at most 0.7 mol / L, or at most 0.6 mol / L. For example, in forming a uniform coating film without an additional solvent evaporation or removal process, the molar concentration of the ammonia borane solution may preferably be 0.3 to 0.7 mol / L or 0.4 to 0.6 mol / L.
[0073] In an exemplary embodiment, the mL unit volume of the polar aprotic solvent contained in the ammonia borane solution may be 0.5 times or less, 0.01 to 0.5 times, 0.05 to 0.5 times, 0.05 to 0.3 times, or 0.1 to 0.3 times the total g unit weight of the support and the transition metal. Accordingly, it provides the effect of forming a uniform coating film without an additional solvent evaporation or removal process.
[0074] In an exemplary embodiment, the hexagonal boron nitride may be included in an amount of less than 0.5 wt% based on the total weight of the support and the transition metal. In the catalyst according to the present disclosure, if the content of hexagonal boron nitride increases, the catalytic activity may decrease or an uneven coating film may be formed. Therefore, the hexagonal boron nitride may be included in an amount of less than 0.5 wt%, 0.4 wt% or less, or 0.3 wt% or less, and preferably 0.01 wt% or more, 0.05 wt% or more, 0.1 wt% or more, 0.15 wt% or more, 0.2 wt% or more, 0.25 wt% or more, or 0.3 wt% or more based on the total weight of the support and the transition metal.
[0075] In an exemplary embodiment, the catalyst with improved durability can be used in an ammonia dehydrogenation reaction and / or an ammonia synthesis reaction. In the case of a catalyst using hexagonal boron nitride as a support (e.g., Ru / h-BN), there is a disadvantage that the hexagonal boron nitride support is in the form of powder, making it difficult to apply to a large-scale ammonia decomposition reaction system, and in the case of a catalyst in which a metal is loaded on a support physically coated with boron nitride (e.g., Ru / BN-paint / θ-Al2O3), there is no durability enhancing effect, whereas a catalyst in which hexagonal boron nitride is formed on a transition metal supported on a support according to the present disclosure (e.g., BN-K-Ru / θ-Al2O3) provides not only excellent ammonia decomposition reaction activity but also an durability enhancing effect.
[0076] In another aspect, the present disclosure provides a method for preparing a catalyst having improved durability, the method comprising the steps of: (1) preparing a catalyst comprising a support and a transition metal supported on the support; (2) preparing an ammonia borane solution by adding ammonia borane to a polar aprotic solvent; and (3) applying the ammonia borane solution onto the prepared catalyst.
[0077] In an exemplary embodiment, the method for preparing the catalyst with improved durability may be a method for synthesizing hexagonal boron nitride on a catalyst. In this respect, the present disclosure provides a method for synthesizing hexagonal boron nitride on a catalyst, the method comprising the steps of: (1) preparing a catalyst comprising a support and a transition metal supported on the support; (2) preparing an ammonia borane solution by adding ammonia borane to a polar aprotic solvent; and (3) applying the ammonia borane solution on the prepared catalyst. The method can directly grow hexagonal boron nitride on transition metal particles of the catalyst.
[0078] The low-temperature synthesis method of hexagonal boron nitride according to the present disclosure comprises using ammonia borane as a synthesis material to coat polyborazylene on metal particles at room temperature through a selective dehydrogenation reaction, and then further heat treatment under an ammonia atmosphere to finally synthesize hexagonal boron nitride.
[0079] In an exemplary embodiment, the step (3) may be to coat a nitrogen-boron compound, such as borazine or polyborazylene, on the catalyst by applying an ammonia borane solution at room temperature.
[0080] In an exemplary embodiment, the method may further include a step of applying an ammonia borane solution in step (3) and then heat-treating the catalyst under an ammonia atmosphere. For example, the method may include applying an ammonia borane solution in step (3) and then heat-treating the catalyst from which the solvent has been evaporated under an ammonia atmosphere to produce a catalyst with improved durability or synthesizing hexagonal boron nitride on the catalyst.
[0081] The method for preparing a catalyst according to the present disclosure is such that when an ammonia borane solution comes into contact with the transition metal particles of the catalyst, a dehydrogenation reaction occurs to produce polyborazylene, and the heat generated evaporates the solvent, eliminating the need for an additional solvent removal process. Accordingly, the method may not include a process for evaporating or removing the solvent of the ammonia borane solution, since the ammonia borane solution is immediately evaporated within about 1 second when dropped onto the catalyst.
[0082] In an exemplary embodiment, the step of heat treatment under an ammonia atmosphere may be performed during a dehydrogenation reaction of ammonia. That is, the step of heat treatment under an ammonia atmosphere may be performed simultaneously with the dehydrogenation reaction of ammonia. In the dehydrogenation reaction of ammonia, hexagonal boron nitride may be synthesized on the catalyst through the heat treatment process, and the catalyst formed with the hexagonal boron nitride may increase the efficiency of the dehydrogenation reaction of ammonia.
[0083] In an exemplary embodiment, the heat treatment is performed at a gas hour space velocity (GHSV) of 60,000 mL / g cat / h or less. In another exemplary embodiment, the heat treatment may be performed by injecting ammonia gas at a rate of 200 mL / min or less. In another exemplary embodiment, the heat treatment may be performed by injecting ammonia gas at a rate of 200 mL / min or less based on 0.2 g of catalyst.
[0084] In an exemplary embodiment, the heat treatment may be performed at 600°C or higher, or at a temperature between 600 and 700°C. The method can induce transformation of metal particles in a reducing atmosphere (including ammonia decomposition or synthesis process) at 600°C or higher, thereby enhancing the activity and / or durability of the catalyst.
[0085] In an exemplary embodiment, the heat treatment may be performed for one hour or more.
[0086] The catalyst manufacturing method according to the present disclosure has the advantage of enabling the mass production of a hexagonal boron nitride-based catalyst with enhanced durability. Compared to the conventional coating method, chemical vapor deposition, hexagonal boron nitride is synthesized at a temperature approximately 400°C lower, and since no vacuum equipment is required, large-scale synthesis is relatively easy.
[0087] In an exemplary embodiment, the step (1) may be a process of obtaining a catalyst by impregnating a support with a transition metal precursor solution and calcining the support impregnated with the transition metal precursor solution.
[0088] In an exemplary embodiment, the transition metal precursor may be at least one selected from the group consisting of metal chlorides, metal chlorides, metal acetate compounds, metal halide compounds, metal nitrate compounds, metal hydroxide compounds, metal carbonyl compounds, metal sulfate compounds, and metal fatty acid salt compounds.
[0089] In an exemplary embodiment, the transition metal precursor may be a metal nitrate compound or a metal carbonyl chlorate.
[0090] In an exemplary embodiment, the firing in step (1) may be performed at 400 to 500°C.
[0091] In an exemplary embodiment, the firing in step (1) may be performed in an air atmosphere, an inert gas atmosphere such as nitrogen or argon, a hydrogen atmosphere, or a vacuum atmosphere.
[0092] In an exemplary embodiment, in step (3), the ammonia borane solution may be applied onto the catalyst at room temperature and pressure.
[0093] In an exemplary embodiment, the mL unit volume of the polar aprotic solvent contained in the ammonia borane solution applied on the catalyst in step (3) may be 0.5 times or less, 0.01 to 0.5 times, 0.05 to 0.5 times, 0.05 to 0.3 times, or 0.1 to 0.3 times the total g unit weight of the support and the transition metal.
[0094] In another aspect, the present disclosure provides a method for dehydrogenating ammonia using the catalyst with improved durability, the method comprising the steps of: (1) charging the catalyst with improved durability into a reactor and then reducing it under a hydrogen atmosphere; and (2) injecting ammonia into the reactor and performing a heat treatment.
[0095] In an exemplary embodiment, the reduction in step (1) may be performed at 400°C or higher, 420°C or higher, 440°C or higher, 460°C or higher, 480°C or higher, 500°C or higher, 520°C or higher, 540°C or higher, or 550°C or higher. In another exemplary embodiment, the reduction in step (1) may be performed at 400 to 700°C, 450 to 700°C, 500 to 700°C, 550 to 700°C, or 600 to 700°C.
[0096] In an exemplary embodiment, the heat treatment in step (2) may be performed at 450°C or higher, 500°C or higher, or 550°C or higher. In another exemplary embodiment, the heat treatment in step (2) may be performed at 450 to 600°C or 500 to 600°C.
[0097] Hereinafter, the present disclosure will be described in more detail through examples. These examples are intended solely to illustrate the present disclosure, and it will be apparent to those skilled in the art that the scope of the present disclosure is not limited by these examples.
[0098] Comparative example.
[0099] Ru3(CO), a ruthenium precursor 12 A bead-shaped θ-Al2O3 support was impregnated in a methanol solvent containing potassium hydroxide and then the solvent was evaporated at a temperature of 45°C using a vacuum rotary evaporator to prepare a catalyst loaded with 6 wt% ruthenium based on the total weight of the catalyst. The catalyst was calcined at 450°C under a hydrogen atmosphere for 3 hours to prepare a K-Ru / θ-Al2O3 catalyst.
[0100] In addition, according to Table 1 below, hexagonal boron nitride (h-BN) powder was dispersed in a methanol solvent, and then the K-Ru / θ-Al2O3 catalyst manufactured above was impregnated, and the hexagonal boron nitride was physically coated using a vacuum rotary evaporator to manufacture the catalyst No. 1 (BN-K-Ru / θ-Al2O3 catalyst).
[0101] In addition, paint containing hexagonal boron nitride was diluted in water according to Table 1 below, and then hexagonal boron nitride was physically coated on a bead-shaped θ-Al2O3 support. Thereafter, the paint was calcined in air at a temperature of approximately 100°C for 2 hours to produce a catalyst No. 2 (Ru / BN-paint / θ-Al2O3 catalyst) supporting ruthenium as a transition metal.
[0102] No.Coating methodMaterialCatalyst weight (g)Metal content in catalyst phase (wt%)h-BN powder weight (g)Solvent volume (mL, name)BN content in catalyst phase (wt%)1Physical methodh-BN powder5.060.539(mL,Methanol)102Physical methodh-BN paint1.060.12917.5 (mL, BN Paint 2.5 + DI water 15)12.9
[0103] In the above Table 1, the catalyst weight refers to the total weight of the support and transition metal, and the catalyst phase content refers to the amount calculated based on the total weight of the support and transition metal.
[0104] Example.
[0105] Using the K-Ru / θ-Al2O3 catalyst manufactured in the comparative example above, catalysts Nos. 3-13 (BN-K-Ru / θ-Al2O3 catalysts) were manufactured by chemically coating hexagonal boron nitride on transition metal particles according to Tables 2 and 3 below. Catalysts Nos. 6-7 were manufactured and used using a Ruthenium(III) nitrosyl nitrate solution as a ruthenium precursor, and catalysts loaded with 2 wt% ruthenium were manufactured and used.
[0106] The above chemical coating method is divided into 1) a room-temperature polyborazylene coating step on a transition metal and 2) an ammonia heat treatment step (see Fig. 1). Nitrogen-boron compounds such as borazine and polyborazylene can be formed on the metal through a dehydrogenation reaction of ammonia borane, and can be converted into boron nitride materials through an additional ammonia heat treatment process. Specifically, a mixture of ammonia borane (AB) dispersed in a solvent was applied onto the catalyst to coat the nitrogen-boron compound at room temperature. Thereafter, a catalyst chemically coated with hexagonal boron nitride was manufactured by supplying ammonia at about 100 mL / min for 0.5 g of the catalyst and heat-treating at 600°C for 1 hour.
[0107] No.Coating methodMaterialCatalyst weight (g)Metal content in catalyst phase (wt%)ABWeight (mg)Solvent volume (mL, name)Molar concentration of ammonia borane solution (mol / L)BN content in catalyst phase (wt%)3Chemical methodAmmonia borane (AB)0.56644(mL, Diglyme)0.529.34Chemical methodAmmonia borane (AB)0.56321(mL, THF)1.044.95Chemical methodAmmonia borane (AB)0.563.20.1(mL, THF)1.040.56Chemical methodAmmonia borane (AB)0.522.560.08(mL, Diglyme)1.040.47Chemical methodAmmonia borane (AB)0.521.920.06(mL, Diglyme)1.040.38Chemical formulaAmmonia borane (AB)0.562.560.08(mL, THF)1.040.49Chemical formulaAmmonia borane (AB)0.561.920.06(mL, THF)1.040.3
[0108] In Table 2 above, the catalyst weight refers to the total weight of the support and transition metal, and the catalyst phase content refers to the amount calculated based on the total weight of the support and transition metal.
[0109] No.Coating methodMaterialCatalyst weight (g)Metal content in catalyst phase (wt%)ABWeight (mg)Solvent volume (mL, name)Molar concentration of ammonia borane solution (mol / L)BN content in catalyst phase (wt%)10Chemical methodAmmonia borane (AB)0.260.770.192(mL, THF)0.130.311Chemical methodAmmonia borane (AB)0.260.770.048(mL, THF)0.520.312Chemical methodAmmonia borane (AB)0.260.770.024(mL, THF)1.040.313Chemical methodAmmonia borane (AB)0.260.770.016(mL, THF)1.560.3
[0110] In Table 3 above, the catalyst weight refers to the total weight of the support and transition metal, and the catalyst phase content refers to the amount calculated based on the total weight of the support and transition metal.
[0111] The catalyst of No. 3 was coated with hexagonal boron nitride so that the BN content in the catalyst phase was 9.3 wt% in an ammonia borane solution having a molar concentration of 0.52 mol / L. The catalysts of Nos. 4-9 were coated with hexagonal boron nitride so that the BN content in the catalyst phase was varied from 0.3 to 4.9 wt% in an ammonia borane solution having a molar concentration of 1.04 mol / L. The catalysts of Nos. 10-13 were coated with hexagonal boron nitride so that the BN content in the catalyst phase was 0.3 wt% in an ammonia borane solution having a molar concentration of 0.13 to 1.56 mol / L.
[0112] Figure 2 shows the results of room temperature coating of polyborazylene on a catalyst. The left photo shows catalyst No. 3, and the right photo shows catalyst No. 9.
[0113] For catalyst No. 3, it was observed that the nitrogen-boron compound (white), which is the product of the ammonia borane dehydrogenation reaction, and the catalyst (black) existed as layers separated in the diglyme solvent phase. For catalysts Nos. 4-5, it was also confirmed that the nitrogen-boron compound, which is the product, and the catalyst existed as layers separated in the THF solvent phase.
[0114] In the case of catalyst No. 9, the boiling point of the solvent is about 66 ℃, which is a high vapor pressure characteristic, so when the solution was dropped, the dehydrogenation reaction of ammonia borane proceeded and the solvent vaporized and evaporated simultaneously, and it was observed that only the product was uniformly coated on the catalyst. Figure 3 shows that when a portion of the solution containing 1.92 mg of ammonia borane and 0.06 mL of THF was dropped on 0.5 g of catalyst, the dehydrogenation reaction of ammonia borane proceeded after about 1 second and the THF evaporated simultaneously, resulting in the coating of polyborazylene on the catalyst surface over time. It is important to drop the ammonia borane solution so that it is evenly distributed so as to come into contact with the catalyst surface.
[0115] Figure 4 shows the results of coating hexagonal boron nitride on a catalyst. The left photo shows the physically coated catalyst No. 1, and the right photo shows the chemically coated catalyst No. 9. When hexagonal boron nitride powder was dispersed in a methanol solvent and physically coated on a bead-shaped catalyst, an uneven coating film and low adhesion properties were observed. On the other hand, the catalyst No. 9 formed a uniform and highly adhesive coating film, confirming that hexagonal boron nitride was synthesized on the bead-shaped catalyst. The catalysts Nos. 6-8 also showed uniform coating films, confirming that hexagonal boron nitride was formed on the bead-shaped catalyst.
[0116] Figure 5 shows catalysts Nos. 6-7 coated with hexagonal boron nitride using diglyme as a solvent. It was confirmed that a uniform, highly adhesive coating film was formed, and that the solvent evaporated quickly, eliminating the need for an additional drying process. Furthermore, catalyst No. 7, which had a lower BN content on the catalyst layer, was found to form a more uniform coating film.
[0117] Figure 6 shows the XPS analysis results of the catalyst surfaces of Nos. 4, 5, 8, and 9. The surface XPS results for the catalysts that were subjected to the dehydrogenation reaction of ammonia borane and then heat-treated (600°C, 1 hour) in the same ammonia atmosphere were analyzed. In the N 1s XPS spectra of the catalysts of Nos. 8 and 9, a peak corresponding to B-N bonds was observed, confirming the formation of boron nitride. Considering that the B-N bond energy value approaches 398.4 to 398.0 eV as the crystal size of hexagonal boron nitride increases among boron nitrides, it was found that the catalyst of No. 9 showed the best result in synthesizing hexagonal boron nitride.
[0118] Figure 7 shows the XPS analysis results of the catalyst surface of No. 7. It was confirmed that a catalyst in which boron nitride was formed was obtained using diglyme as a polar aprotic solvent. The peak indicating BN bonds (BN bond energy value 398.96 eV) was observed, confirming that hexagonal boron nitride was successfully synthesized.
[0119] Figure 8 shows the XPS analysis results of the catalyst surface of No. 9. After ammonia heat treatment (or 168 hours after ammonia decomposition reaction), BN bonds were observed in the XPS spectra corresponding to B 1s and N 1s, confirming the formation of hexagonal boron nitride.
[0120] Figure 9 compares the results of ammonia decomposition reaction using K-Ru / θ-Al2O3 bead-type catalyst and catalysts of Nos. 2 and 9. After filling a quartz reactor with a volume of 0.27 mL with a diameter of 1 / 2", the catalyst was heated for 21,000 h. -1 Ammonia decomposition reaction was carried out at a reaction temperature of 500 ℃ for up to 170 hours under Gas Hourly Space Velocity (GHSV) conditions. The slope of the equation after linear fitting the change in ammonia conversion rate with respect to time was utilized as a criterion for judging the performance deterioration of the catalyst. As a result, in the case of the catalyst without BN coating, a performance degradation of approximately -1.68% was observed for approximately 40 hours. On the other hand, the catalyst coated with BN according to the present disclosure showed a positive slope value despite the long-term experiment, confirming that it had improved durability. The catalyst in which BN was physically coated on Al2O3 and then Ru was loaded showed a negative slope value with a decrease in performance as the evaluation time progressed, similar to the catalyst without BN coating.
[0121] Fig. 10 compares the results of the ammonia decomposition reaction using a K-Ru / θ-Al2O3 bead-type catalyst and a catalyst coated with BN. Here, the BN-coated catalyst was prepared in the same manner as the catalyst of No. 9, but using a Ruthenium(III) nitrosyl nitrate solution as a ruthenium precursor. After charging a quartz reactor with a diameter of 1 / 2" with a volume of 0.27 mL, reduction was performed at a temperature of 550°C for 1 hour at a flow rate of H2100 mL / min, and ammonia was injected at a flow rate of 93.33 mL / min for 21,000 h. -1 Ammonia decomposition reaction was carried out at a reaction temperature of 500 ℃ for up to 100 hours under GHSV conditions. As a result, a performance decrease of about -1.96% was observed for the catalyst without BN coating for about 100 hours. On the other hand, it was confirmed that the catalyst coated with BN according to the present disclosure not only increased the ammonia conversion rate by 2.49% after 100 hours of evaluation, but also increased the catalytic activity by about 6%. Accordingly, it was found that low-temperature chemical BN coating is effective in enhancing the catalytic activity and / or durability for a transition metal, such as Ru-based catalyst. In addition, it was confirmed that the effect of enhancing the catalytic activity and / or durability by BN coating can be implemented regardless of the type of metal precursor.
[0122] Figure 11 shows the results of scanning transmission electron microscopy (STEM) and energy dispersive spectroscopy (EDS) analysis for catalyst No. 2. As a result, considering the hydrophobic nature of BN, Ru3(CO) 12Although (triruthenium dodecacarbonyl) was used as a Ru precursor, it was observed that Ru nanoparticles were concentrated on the Al2O3 support rather than on BN. Meanwhile, some rod-shaped Ru particles with a thickness of about 20 nm and a length of about 70 nm or triangular Ru particles with a size of about 20 nm were observed at the edge of BN. From the above results, it was found that the BN-coated Al2O3 composite support is difficult to utilize as a support for Ru nanoparticles because Ru is not uniformly loaded on BN.
[0123] Figure 12 shows the results of TEM-EDS mapping analysis for catalyst No. 9. From the analysis results showing that B and N are simultaneously distributed in the area where Ru particles are distributed, it was confirmed that hexagonal boron nitride was successfully formed on the catalyst through the low-temperature synthesis method according to the present disclosure.
[0124] Figure 13 shows the XRD analysis results for the K-Ru / θ-Al2O3 bead-type catalyst and catalyst No. 9. In catalyst No. 9, a peak corresponding to h-BN(002) was observed, indicating that hexagonal boron nitride was formed through a low-temperature synthesis method using ammonia borane. In addition, the ICDD card no. for the observed Ru particle peak was confirmed to be 04-018-8034 and 04-015-6086, respectively, and from the above results, the density of the Ru particles was 11.854 g / cm. 3 12.361 g / cm 3 It was found that it increased.
[0125] Figure 14 shows the results of visual inspection of the dispersion of the ammonia borane solution used in the preparation of catalysts Nos. 10-13. (a) The photo shows the appearance immediately after mixing ammonia borane and THF, and (b) The photo shows the appearance 1 minute after mixing. Mixing was performed by placing ammonia borane and THF in a glass vial, dispersing them using an ultrasonic cleaner (AJC-5030, OMAX. Co., Ltd., Korea) for 10 minutes, and then mixing them using a vortex mixer (VM-10, DAIHAN Scientific, Korea) for 1 minute. After mixing, the glass vial was left to stand for 1 minute, and the dispersion stability according to the molar concentration of the ammonia borane solution was visually inspected to compare and observe. It was confirmed that the ammonia borane solution exhibited excellent dispersion stability when the molar concentration was 0.3 to 0.7 mol / L, and more specifically, 0.52 mol / L.
[0126] Figure 15 shows a comparative observation of the hexagonal boron nitride coating results for catalysts Nos. 10-13. The catalyst No. 10 exhibited insufficient heat generation from the dehydrogenation reaction during the room-temperature polyborazylene coating process, which prevented proper evaporation of the ammonia borane solution. This required an additional drying process, which resulted in an uneven coating layer. Even when hexagonal boron nitride was coated so that the BN content in the catalyst was less than 0.5 wt%, it was found that it was difficult to form a uniform coating film with excellent adhesion properties when the molar concentration of the ammonia borane solution was lower than 0.2 mol / L. On the other hand, the catalysts Nos. 11-13 formed a uniform coating film without an additional drying process. In addition, it was confirmed that the uniformity of the coating film could be further improved by using an ammonia borane solution with a high molar concentration and high dispersion stability for the catalyst No. 11.
[0127] While specific aspects of the present disclosure have been described in detail, it will be apparent to those skilled in the art that these specific descriptions are merely preferred embodiments and do not limit the scope of the present disclosure. Accordingly, the substantial scope of the present disclosure is defined by the appended claims and their equivalents.
Claims
1. Support; A transition metal supported on the support; and A catalyst with improved durability comprising hexagonal boron nitride synthesized on the above transition metal.
2. In paragraph 1, A catalyst having improved durability, wherein the support is at least one selected from the group consisting of carbon, silica, silicon carbide, silicon nitride, alumina, magnesium oxide, magnesium aluminate, calcium oxide, calcium aluminate, zeolite, zirconia, titania, ceria, lanthania, yttria, and rare earth oxides.
3. In paragraph 1, A catalyst having improved durability, wherein the above transition metal is at least one selected from the group consisting of Mo, Ni, Fe, Co, Cu, Pd, Pt, Ru, Rh, Au and Ir.
4. In paragraph 1, The above hexagonal boron nitride is a catalyst with improved durability, synthesized from ammonia borane.
5. In paragraph 4, The above hexagonal boron nitride is a catalyst with improved durability, which is synthesized by applying an ammonia borane solution on a transition metal supported on the support and then heat-treating it in an ammonia atmosphere.
6. In paragraph 5, The above ammonia borane solution is a catalyst with improved durability, wherein ammonia borane is contained in a polar aprotic solvent.
7. In paragraph 6, A catalyst having improved durability, wherein the polar aprotic solvent comprises at least one selected from tetrahydrofuran (THF), 1,2-dimethoxyethane (DME), dioxane (DXN), diethyleneglycoldimethylether (Diglyme), dimethylformamide (DMF), dimethylsulfoxide (DMSO), dimethylacetamide (DMA), and hexamethyl phosphoramide (HMPA).
8. In paragraph 6, The above polar aprotic solvent is a catalyst with improved durability having a boiling point of 100°C or less.
9. In paragraph 5, A catalyst with improved durability, wherein the molar concentration of the ammonia borane solution is 0.2 mol / L or more.
10. In paragraph 6, A catalyst with improved durability, wherein the volume in mL of the polar aprotic solvent contained in the ammonia borane solution is 0.5 times or less of the total weight in g of the support and transition metal.
11. In paragraph 1, A catalyst with improved durability, wherein the hexagonal boron nitride is contained in an amount of less than 0.5 wt% based on the total weight of the support and the transition metal.
12. A method for producing a catalyst with improved durability according to any one of claims 1 to 11, wherein the method comprises: (1) A step of preparing a catalyst including a support and a transition metal supported on the support; (2) a step of preparing an ammonia borane solution by adding ammonia borane to a polar aprotic solvent; and (3) A method for producing a catalyst with improved durability, comprising a step of applying an ammonia borane solution on the prepared catalyst.
13. In paragraph 12, A method for producing a catalyst with improved durability, wherein the method further comprises a step of applying an ammonia borane solution in the step (3) and then heat-treating the catalyst under an ammonia atmosphere.
14. In paragraph 13, A method for producing a catalyst with improved durability, wherein the above heat treatment is performed at 600 to 700°C.
15. A method for dehydrogenating ammonia using a catalyst with improved durability according to any one of claims 1 to 11, wherein the method (1) A step of charging a catalyst with improved durability according to any one of claims 1 to 11 into a reactor and then reducing it under a hydrogen atmosphere; and (2) A method for dehydrogenating ammonia using a catalyst with improved durability, comprising a step of injecting ammonia into the reactor and performing heat treatment.
Citation Information
Patent Citations
Preparation method of ammonia borane-metal catalyst composite hydrogen storage material
CN103011074A
Metal@BN core-shell structure nanometer catalyst for synthesis gas methanation reaction, and preparation method thereof
CN106179438A
Preparation method of high-defect boron nitride supported atomic-scale dispersed metal catalyst
CN114653371A
Ink marker automatic ink filling machine
KR1020210158082A
An air sterilizer that uses an ultraviolet lamp covered with a diamond-shaped aluminum cylindrical mesh net coated with Tio2
KR1020230053159A