Multilayer film, display device, and packaging material
The multilayer film with a polyester resin and butenediol vinyl alcohol copolymer laminate structure addresses the peeling and processing issues of conventional films, achieving low oxygen permeability and improved mechanical properties, suitable for applications requiring oxygen blocking and mechanical strength.
Patent Information
- Application Number
- PCT/KR2024/095175
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-19
- Filing Date
- 2024-02-15
- Publication Date
- 2024-10-24
AI Technical Summary
Conventional multilayer films with polyester and ethylene vinyl alcohol copolymer (EVOH) layers face issues of peeling at the interface, complexity in processing, and uneven thickness, which complicates their application in fields requiring low oxygen permeability and mechanical strength.
A multilayer film is developed with a laminate structure comprising a polyester resin layer and a butenediol vinyl alcohol copolymer layer, where the polyester resin has a diol residue and a dicarboxylic acid residue, and the butenediol vinyl alcohol copolymer layer provides excellent adhesion and oxygen barrier properties, eliminating the need for an additional adhesive layer and simplifying the manufacturing process.
The multilayer film achieves low oxygen and moisture permeability, maintains mechanical strength, and improves processability, allowing for effective oxygen blocking and easy recycling, while ensuring the film's transparency and heat resistance.
Smart Images

Figure KR2024095175_24102024_PF_FP_ABST
Abstract
Description
Multilayer films, displays, and packaging materials
[0001] The embodiments relate to a multilayer film having low oxygen permeability, a display device including the same, and a packaging material including the same.
[0002]
[0003] Oxygen-barrier films are in demand across a wide range of industries. Examples include packaging materials for foods requiring freshness, and encapsulating materials for oxygen-sensitive electronic components. In particular, organic materials in organic light-emitting diodes and quantum dots in quantum dot layers are vulnerable to oxygen. To protect these materials, the need for films with adequate heat resistance, mechanical strength, and transparency, while also possessing low oxygen permeability, is growing.
[0004] Polyester possesses stable properties such as heat resistance, mechanical strength, and transparency. For this reason, polyester is widely used in various fields, including containers, packaging materials, films, and cables.
[0005] However, polyester's high oxygen permeability made it difficult to apply in areas requiring oxygen barrier protection. This problem was overcome by producing a multilayer film containing at least one layer containing a material with low oxygen permeability, such as ethylene vinyl alcohol copolymer (EVOH).
[0006] However, polyester and ethylene vinyl alcohol copolymer (EVOH) have a problem with delamination at the interface. This problem can be addressed by methods such as depositing an adhesive layer at the interface, but this complicates the process and increases the film thickness.
[0007] Additionally, differences in melting points and other properties between polyester and ethylene vinyl alcohol copolymer (EVOH) can cause numerous problems during laminate formation, leading to reduced processability.
[0008] The background technology described above is technical information that the inventor possessed for the purpose of deriving the present invention or acquired in the process of deriving the present invention, and cannot necessarily be considered as publicly known technology disclosed to the general public prior to the filing of this application.
[0009] Related prior art includes (Patent Document 1) Republic of Korea Registered Patent No. 10-0516550, (Patent Document 2) Republic of Korea Registered Patent No. 10-1890108, (Patent Document 3) Republic of Korea Registered Patent No. 10-1970168, etc.
[0010]
[0011] The purpose of the embodiment is to provide a multilayer film having low oxygen permeability, an interface that is not easily delaminated, and improved processability, and a display device and packaging material including the same.
[0012]
[0013] A multilayer film of one embodiment for achieving the above purpose comprises a laminate comprising a first layer and a second layer disposed on the first layer,
[0014] The first layer comprises a polyester resin containing a diol residue and a dicarboxylic acid residue,
[0015] The second layer comprises a butenediol vinyl alcohol copolymer,
[0016] The above laminate has a density of 0.1 cc / m at 23°C. 2 ·Has an oxygen permeability of less than day·atm.
[0017] In the above multilayer film, the diol residue may be any one selected from the group consisting of an ethylene glycol residue, a diethylene glycol residue, a neopentyl glycol residue, and a combination thereof.
[0018] The above diol residues may include 5 to 35 mol% of neopentyl glycol residues based on the total diol residues.
[0019] The melting point of the first layer may be lower than the thermal decomposition temperature of the second layer.
[0020] The glass transition temperature of the second layer may be 60°C or higher.
[0021] The above multilayer film may have a maximum thickness deviation of 3㎛ or less, as expressed by Equation 1 below.
[0022] [Formula 1]
[0023] MTD 50 = THK max - THK min
[0024] In the above equation 1, MTD 50 is the maximum thickness deviation, and THK max The maximum thickness, THK, was measured at 2 cm intervals on a specimen of a multilayer film with a width of 50 cm. min is the minimum thickness when the thickness of a multilayer film specimen with a width of 50 cm is measured at 2 cm intervals.
[0025] The laminate is formed by alternately laminating the first layer and the second layer in 3 to 225 layers, and the first layer may be located at the outermost layer of the laminate.
[0026] The above laminate is 50 g / m 2 ·Can have a moisture permeability of less than day.
[0027] A display device according to another embodiment comprises: a light-emitting portion; and an encapsulating layer disposed on the light-emitting portion; wherein the encapsulating layer may include the multilayer film described above in the claims.
[0028] Packaging material according to another embodiment may include the multilayer film described above.
[0029]
[0030] The multilayer film of the embodiment provides a multilayer film with low oxygen permeability, a non-peelable interface, and improved processability, as well as a display device and packaging material including the multilayer film. Through this, the embodiment can effectively block elements of the display device, packaged food, etc. from oxygen entering from the outside.
[0031] Furthermore, the multilayer film exhibits excellent processability, as its interfaces do not easily delaminate and its maximum thickness deviation is minimal. Furthermore, the resin applied to the multilayer film has controlled melting and decomposition temperatures, facilitating coextrusion. Furthermore, the multilayer film has high water-separability, making it easy to recycle.
[0032]
[0033] Figure 1 is a conceptual diagram illustrating a laminate included in a multilayer film according to an embodiment.
[0034] Figure 2 is a conceptual diagram illustrating a laminate included in a multilayer film according to another embodiment.
[0035] Figure 3 is a conceptual diagram illustrating a laminate included in a multilayer film according to another embodiment.
[0036]
[0037] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings so that those skilled in the art can easily implement the present invention. However, the present invention may be implemented in various different forms and is not limited to the embodiments described herein. Like reference numerals designate similar parts throughout the specification.
[0038] Throughout this specification, the term "combination thereof" included in the expressions in the Makushi format means one or more mixtures or combinations selected from the group consisting of the components described in the expressions in the Makushi format, and means including one or more selected from the group consisting of said components.
[0039] Throughout this specification, references to “A and / or B” mean “A, B, or A and B.”
[0040] Throughout this specification, terms such as "first" and "second" are used to distinguish between identical terms. Furthermore, singular expressions include plural expressions unless the context clearly indicates otherwise.
[0041] Throughout this specification, whenever a part is said to "include" a component, this means that it may include other components, but not to the exclusion of other components, unless specifically stated otherwise.
[0042] Throughout this specification, the meaning of B being placed on A means that B is positioned directly on A or that B is positioned on A with another layer positioned in between, and is not limited to being positioned in contact with the surface of A.
[0043] In this specification, the drawings may be presented with exaggerated or omitted configurations for the purpose of explanation, and the scope of the implementation examples shall not be construed as being limited thereby.
[0044]
[0045] Multilayer films are applied, which insert an oxygen-barrier layer into a layer containing polyester resin. These multilayer films have been used as materials that possess superior mechanical and optical properties while simultaneously blocking external oxygen. However, conventional polyester resin layers and oxygen barrier layers tend to delaminate at the interface. Consequently, a separate adhesive layer is required between each layer. This complicates the process, increases the thickness of the multilayer film, and makes film recycling difficult.
[0046] The inventors of the embodiment studied to solve the above-mentioned problem and invented a multilayer film in which the interface between the first layer including a polyester resin and the second layer performing an oxygen barrier function does not separate from each other.
[0047] According to one aspect of the invention of the embodiment, the invention of the embodiment can provide a multilayer film having excellent mechanical and optical properties, excellent oxygen and moisture barrier properties, improved processability, and recyclability of polyester resin.
[0048] In addition, a display device including a sealing layer having the above-described characteristics can be provided.
[0049] In addition, a packaging material having the above-described characteristics can be provided.
[0050]
[0051] FIG. 1 is a conceptual diagram illustrating a laminate included in a multilayer film according to an embodiment, FIG. 2 is a conceptual diagram illustrating a laminate included in a multilayer film according to another embodiment, and FIG. 3 is a conceptual diagram illustrating a laminate included in a multilayer film according to another embodiment. The embodiments will be described in detail below with reference to the drawings.
[0052]
[0053] laminate
[0054] The laminate (10) according to the above embodiment is a laminate (10) in which a first layer (11) and a second layer (12) containing different polymer resins are alternately laminated.
[0055] The first layer (11) according to the above embodiment includes a copolymerized polyester resin.
[0056] The above first layer (11) can prevent the second layer (12) from being directly exposed to the external environment, thereby preventing the properties of the laminate or multilayer film from deteriorating.
[0057] The above-mentioned copolymerized polyester resin may be a polymerization of a diol and a dicarboxylic acid comprising two or more diol residues and one or more dicarboxylic acid residues. Specifically, the above-mentioned copolymerized polyester resin may be a polymerization of a diol and a dicarboxylic acid comprising three or more diol residues and one or more dicarboxylic acid residues.
[0058] The above diol residue may include an aliphatic diol residue, an alicyclic diol residue, an aromatic diol residue, or a derivative thereof. The aliphatic diol residue may be, for example, an aliphatic diol residue having 2 to 10 carbon atoms and may have a linear or branched structure.
[0059] Specific examples of aliphatic diols containing the above aliphatic diol residue include ethylene glycol, diethylene glycol, neopentyl glycol, 1,3-propanediol, 1,2-octanediol, 1,3-octanediol, 2,3-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 2-butyl-2-ethyl-1,3-propanediol, 2,2-diethyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,1-dimethyl-1,5-pentanediol, 1,6-hexanediol, 2-ethyl-3-methyl-1,5-hexanediol, 2-ethyl-3-ethyl-1,5-hexanediol, 1,7-heptanediol, 2-ethyl-3-methyl-1,5-heptanediol, 2-ethyl-3-ethyl-1,6-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, derivatives thereof, or any combination thereof.
[0060] The above dicarboxylic acid residue may include an aromatic dicarboxylic acid residue, an aliphatic dicarboxylic acid residue, an alicyclic dicarboxylic acid residue, or an ester residue thereof.
[0061] Specific examples of the dicarboxylic acid containing the above dicarboxylic acid residue include terephthalic acid, dimethylterephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, orthophthalic acid, adipic acid, azelaic acid, sebacic acid, decanedicarboxylic acid, and esters thereof; or combinations thereof. Specifically, the dicarboxylic acid may include at least one selected from the group consisting of terephthalic acid, dimethylterephthalate, naphthalenedicarboxylic acid, and orthophthalic acid.
[0062] According to one embodiment, the copolymerized polyester resin may be a polymerization of a diol and an aromatic dicarboxylic acid comprising two or more diol residues and one or more aromatic dicarboxylic acid residues. According to another embodiment, the copolymerized polyester resin may be a polymerization of a diol comprising ethylene glycol and one or more comonomers and one or more aromatic dicarboxylic acids. According to yet another embodiment, the copolymerized polyester resin may be a polymerization of a diol comprising ethylene glycol and two or more comonomers and an aromatic dicarboxylic acid.
[0063] The above diol residue may include an ethylene glycol residue. The diol may include 50 to 90 mol% of ethylene glycol based on the entire diol. Specifically, the diol may include 60 to 90 mol%, 63 to 85 mol%, or 65 to 83 mol% of ethylene glycol based on the entire diol. When the above range is satisfied, the polyester resin may have improved heat shrinkage and reduced clumping fraction.
[0064] The above diol may include, as a comonomer, any of the diols exemplified above, except for ethylene glycol. For example, the above diol may include, as a comonomer, diethylene glycol, 1,4-cyclohexanedimethanol, 1,3-propanediol, 1,2-octanediol, 1,3-octanediol, 2,3-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, neopentylglycol, 2-butyl-2-ethyl-1,3-propanediol, 2,2-diethyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,1-dimethyl-1,5-pentanediol, or a combination thereof. Specifically, the diol may include at least one selected from the group consisting of neopentyl glycol, cyclohexanedimethanol, and diethyl glycol as a comonomer.
[0065] Specifically, the diol may include diethylene glycol as a comonomer. The content of diethylene glycol in the diol may include 1 to 15 mol% based on the entire diol. Specifically, the diol may include 1 to 10 mol%, 1 to 5 mol%, 5 to 10 mol%, or 3 to 7 mol% based on the entire diol. When the above range is satisfied, the polyester resin may have improved heat shrinkage and reduced clumping fraction.
[0066] In addition, the diol may include at least one of neopentyl glycol and cyclohexanedimethanol as a comonomer. Among the diols, neopentyl glycol and / or cyclohexanedimethanol may be included in an amount of 1 to 50 mol% based on the total amount of the diol. Specifically, it may include 10 to 40 mol%, 10 to 30 mol%, 20 to 40 mol%, 20 to 30 mol%, 20 to 25 mol%, or 25 to 30 mol%. When the above range is satisfied, the copolyester resin can appropriately maintain a heat shrinkage rate in a direction perpendicular to the main shrinkage direction during stretching even at high temperatures. When the content of the neopentyl glycol and / or cyclohexanedimethanol exceeds the above range, the copolyester resin may expand excessively in a direction perpendicular to the main shrinkage direction during stretching, thereby causing wrinkles or deformation. In addition, when the content of the neopentyl glycol and / or cyclohexanedimethanol is less than the above range, the amorphous region of the copolymerized polyester resin may expand, so that the shrinkage characteristics in the main shrinkage direction may improve, but the shrinkage characteristics in the direction perpendicular to the main shrinkage direction may decrease, so that the expansion coefficient may increase.
[0067] Specifically, the diol may include at least one selected from neopentyl glycol and cyclohexanedimethanol as comonomers; and diethylene glycol. For example, the diol may include 20 to 30 mol% of at least one selected from neopentyl glycol and cyclohexanedimethanol as comonomers; and 1 to 15 mol% of diethylene glycol.
[0068] The dicarboxylic acid may contain terephthalic acid or dimethyl terephthalate in an amount of 80 mol% or more, 90 mol% or more, or 95 mol% or more, based on the total amount of the dicarboxylic acid. However, the dicarboxylic acid may contain little or no isophthalic acid. For example, the content of isophthalic acid in the dicarboxylic acid may be 5 mol% or less, 3 mol% or less, or 1 mol% or less. Specifically, the diol may contain 20 to 40 mol% of at least one selected from the group consisting of neopentyl glycol, cyclohexanedimethanol, diethylene glycol, and combinations thereof as a comonomer, and the content of isophthalic acid in the aromatic dicarboxylic acid may be less than 1 mol%. As a specific embodiment, the copolymerized polyester resin may be glycol-modified polyethylene terephthalate (PETG).
[0069] The above-mentioned copolymerized polyester resin may further contain an alcohol other than the diol, for example, a monohydric alcohol. For example, the monohydric alcohol may be methanol, ethanol, isopropanol, allyl alcohol, or benzyl alcohol. Specifically, the above-mentioned copolymerized polyester resin may contain 10 to 40 parts by weight, or 15 to 30 parts by weight, of the monohydric alcohol based on 100 parts by weight of the diol.
[0070] According to one embodiment, the melting point of the first layer (11) may be 170 to 230°C. Specifically, the melting point of the first layer (11) may be 180 to 220°C, and may be 190 to 210°C. When the above range is satisfied, the melting point of the first layer (11) may be lower than the thermal decomposition temperature of the second layer (12). Therefore, the first layer (11) and the second layer (12) of the embodiment may be easily subjected to a co-extrusion process.
[0071] The second layer (12) according to the above embodiment includes a butenediol vinyl alcohol copolymer (BVOH).
[0072] The above butenediol vinyl alcohol copolymer (BVOH) can be produced by copolymerization of butenediol and vinyl acetate followed by hydrolysis of vinyl acetate.
[0073] Alternatively, the butenediol vinyl alcohol copolymer (BVOH) may be BVOH sold as NICHIGO G-POLYMER™ by Mistubishi Chemical. Specifically, the pellet type product of NICHIGO G-POLYMER™ may be any one selected from the group consisting of AVE8077P, BVE8049P, OKS-8074P, OKS-8211P, and combinations thereof.
[0074] The second layer (12) is a water-soluble layer that dissolves in water. In particular, the second layer (12) dissolves not only in high-temperature water but also in relatively low-temperature water. Specifically, the second layer (12) can be substantially completely dissolved in 90°C water within 1 hour, in 70°C water within 1 hour, and in 20°C water within 2 hours. The second layer (12) dissolves well in water and can improve the water separation property of the laminate (10) as described below. In addition, the second layer (12) dissolves well in water and can substantially leave no residual composition on the first layer (11) when the laminate (10) is recycled.
[0075] The second layer (12) may have a melt flow rate (MFR) of 10 g / 10 min or more at 210°C. Specifically, the second layer (12) may have a melt mass index (MFR) of 15 g / 10 min or more, 20 g / 10 min or more, 25 g / 10 min or more, or 30 g / 10 min or more. The second layer (12) may have a melt mass index (MFR) of 100 g / 10 min or less. When the above range is satisfied, the manufacturing processability of the second layer (12) may be improved. For example, the second layer (12) may be easily formed through a coextrusion process.
[0076] The viscosity of the second layer (12) may be 30,000 poise or less at 230°C. Specifically, the viscosity of the second layer (12) may be 20,000 poise or less, 10,000 poise or less, or 9,000 poise or less at 230°C. The viscosity of the second layer (12) may be 100 poise or more at 230°C. Specifically, the viscosity of the second layer (12) may be 300 poise or more, 500 poise or more, or 1,000 poise or more at 230°C. When the above range is satisfied, the second layer (12) can be easily formed through a co-extrusion process because fluidity is secured during extrusion.
[0077] The thermal decomposition temperature of the second layer (12) may be 210°C to 230°C. Specifically, the thermal decomposition temperature of the second layer (12) may be 215°C to 225°C, or 217°C to 223°C. As a general polyester, the melting point of polyethylene terephthalate (PET) is higher than the thermal decomposition temperature of polyvinyl alcohol (PVOH), making it difficult to apply a co-extrusion process. In the case of an embodiment, the melting point of the first layer (11) may be lower than the thermal decomposition temperature of the second layer (12). Therefore, the first layer (11) and the second layer (12) of the embodiment may be easily applied with a co-extrusion process.
[0078] The glass transition temperature of the second layer (12) may be 60°C or higher. Specifically, the glass transition temperature of the second layer (12) may be 65°C or higher, 70°C or higher, or 75°C or higher. The glass transition temperature of the second layer (12) may be 200°C or lower, 150°C or lower, or 100°C or lower. Since a general display device may have a high-temperature environment created inside, a heat-resistant material may be required. When the above range is satisfied, the heat resistance of the second layer (12) may be enhanced.
[0079] The laminate (10) according to the above embodiment may include an adhesive layer between the first layer (11) and the second layer (12), and may be in direct contact with each other. Even when the first layer (11) and the second layer (12) are in direct contact with each other, the first layer (11) and the second layer (12) have high adhesion that is substantially not peeled off even in a high temperature and high humidity environment. It was confirmed that the laminate (10) did not exhibit peeling between the first layer (11) and the second layer (12) even when exposed for 500 hours or more at a temperature of 85°C and a relative humidity of 85% using a constant temperature and humidity chamber (QM200M from QMESYS). Therefore, the multilayer film can omit the interlayer adhesive layer, simplifying the process and making it easy to control the thickness of the film.
[0080] The laminate (10) may contain 1 to 50 parts by weight of the second layer (12) based on 100 parts by weight of the laminate. Specifically, the laminate (10) may contain 3 to 40 parts by weight of the second layer (12), or 5 to 30 parts by weight of the second layer (12), based on 100 parts by weight of the laminate.
[0081] The above laminate (10) has excellent water separability and is easy to recycle. Specifically, when 10 laminate samples measuring 1 cm in width and 1 cm in length are placed in water at 60±5°C and stirred at a rotation speed of 300 rpm for 120 minutes using a stirrer, the second layer (12) dissolves in the water. In addition, when 10 laminate samples measuring 0.5 cm in width and 0.25 cm in length are placed in a 1 wt% sodium hydroxide (NaOH) aqueous solution at 85±5°C and stirred at a rotation speed of 300 rpm for 15 minutes, the second layer (12) dissolves in the 1 wt% sodium hydroxide aqueous solution. In this case, the first layer (11) does not dissolve and is thus recyclable.
[0082] The above laminate (10) is 0.1 cc / m 2 ·day·atm or less oxygen permeability. Specifically, the laminate (10) has an oxygen permeability of 0.07 cc / m 2 ·It can have an oxygen permeability of less than day·atm and 0.05 cc / m 2 ·It can have an oxygen permeability of less than day·atm and 0.03 cc / m 2 ·May have an oxygen permeability of less than day·atm, or 0.01 cc / m 2 ·day·atm or less. The laminate (10) may have an oxygen permeability of 0.0001 cc / m 2 ·day·atm or higher oxygen permeability. When the above range is satisfied, the multilayer film can effectively block oxygen from entering from the outside.
[0083] The above laminate (10) has a density of 1,000 g / m at a temperature of 37.8±0.5℃. 2 ·day or less moisture permeability. Specifically, the laminate (10) has a moisture permeability of 100 g / m 2 ·It can have a moisture permeability of less than 50 g / m2 2 ·It can have a moisture permeability of less than 45 g / m 2 ·It can have a moisture permeability of less than 40 g / m2 2 ·It can have a moisture permeability of less than 36 g / m 2 ·It can have a moisture permeability of less than 25 g / m 2 ·It can have a moisture permeability of less than 24 g / m 2 ·May have a moisture permeability of less than 23 g / m2 or less 2 ·day or less moisture permeability. The laminate (10) may have a moisture permeability of 0.0001 g / m 2 · It can have a moisture permeability of more than a day. When the above range is satisfied, the multilayer film can effectively block moisture from entering from the outside. The above moisture permeability is based on the results measured under temperature and humidity conditions of 37.8 ± 0.5 ℃ and 100 RH% in accordance with ASTM F1249-20 using a PERMATRAN-W700 tester from MOCON, USA, at any thickness selected from 0.3 to 0.15 mm.
[0084] The total number of layers of the laminate (10) may be 4 or more, 6 or more, 10 or more, 31 or more, 35 or more, or 37 or more. The laminate (10) may be 425 or less, 325 or less, or 225 or less. The total number of layers of the laminate (10) is based on the number of layers determined by assuming that the first layer (11) of the laminate (10) exists when it is difficult to distinguish between the first layer (11) of the laminate (10) and the adjacent skin layers by applying the same resin as the first layer (11) resin to the skin layer described later.
[0085] The above laminate (10) can provide a multilayer film that maintains mechanical strength of the polyester film at an appropriate level or higher by alternately laminating the first layer (11) and the second layer (12) in a multilayer structure.
[0086] The above laminate (10) may be formed by alternately laminating the first layer (11) and the second layer (12) in three or more layers, and may be formed by alternately laminating 3 to 255 layers. In this case, even if a relatively large amount of the second layer composition is applied, the manufacturing process can be further improved.
[0087]
[0088] skin layer
[0089] The multilayer film of the embodiment may further include a skin layer.
[0090] The skin layer can be placed on one side or the other side of the laminate (10).
[0091] The skin layer may be disposed on one or the other surface of the laminate (10). In this case, the laminate (10) can be prevented from being directly exposed to the external environment, thereby preventing deterioration of its physical properties.
[0092] The skin layer may be applied with the resin of the first layer (11). In this case, the mechanical and optical properties and processability of the multilayer film can be further improved.
[0093] The thickness of the skin layer can be applied at a thickness ratio of 5 to 30 based on the thickness of 100 of the laminate (10). Specifically, the thickness of the skin layer can be applied at a thickness ratio of 10 to 25, or 15 to 20 based on the thickness of 100 of the laminate (10).
[0094] If the skin layer is applied to both the upper and lower parts of the laminate (10), the thickness of the skin layer described above means the thickness of one skin layer.
[0095]
[0096] multilayer film
[0097] The above multilayer film (100) has a density of 0.1 cc / m measured at a temperature of 23.0±0.5℃. 2 ·day·atm or less. Specifically, the multilayer film (100) may have an oxygen permeability of 0.07 cc / m 2 ·It can have an oxygen permeability of less than day·atm and 0.05 cc / m 2 ·It can have an oxygen permeability of less than day·atm and 0.03 cc / m 2 ·May have an oxygen permeability of less than day·atm, or 0.01 cc / m 2 ·day·atm or less can have an oxygen permeability. When the above range is satisfied, the multilayer film (100) can effectively block oxygen flowing in from the outside.
[0098] The above multilayer film (100) has a density of 1,000 g / m when measured at a temperature of 37.8±0.5℃ and a humidity of 100 RH% according to ASTM F1249-20. 2 ·day or less moisture permeability. Specifically, the multilayer film may have a moisture permeability of 100 g / m 2 ·It can have a moisture permeability of less than 50 g / m2 2 ·It can have a moisture permeability of less than 45 g / m 2·It can have a moisture permeability of less than 40 g / m2 2 ·It can have a moisture permeability of less than 36 g / m 2 ·It can have a moisture permeability of less than 25 g / m 2 ·It can have a moisture permeability of less than 24 g / m 2 ·May have a moisture permeability of less than 23 g / m2 or less 2 ·day or less moisture permeability. The multilayer film (100) may have a moisture permeability of 0.0001 g / m 2 · It can have a moisture permeability of more than a day. When the above range is satisfied, the multilayer film can effectively block moisture from entering from the outside.
[0099] The total thickness of the multilayer film may be 10 to 1,000 μm. Specifically, the total thickness of the multilayer film may be 20 to 500 μm, 30 to 250 μm, 40 to 200 μm, or 60 to 100 μm. The multilayer film may omit the adhesive layer between the first layer (11) and the second layer (12), so that the total thickness can be easily controlled.
[0100] The above multilayer film has a maximum thickness deviation (MTD) expressed by Equation 1 below. 50 ) may be 3 ㎛ or less. Specifically, the multilayer film has a maximum thickness deviation (MTD) expressed by Equation 1 below. 50 ) may be 2.7 ㎛ or less, 2.5 ㎛ or less, or 2.0 ㎛ or less. When the above range is satisfied, the multilayer film can easily maintain flatness, thereby improving processability.
[0101] [Formula 1]
[0102] MTD 50 = THK max - THK min
[0103] In the above equation 1, THK max The maximum thickness, THK, was measured at 2 cm intervals on a specimen of a multilayer film with a width of 50 cm. min is the minimum thickness when the thickness of a multilayer film specimen with a width of 50 cm is measured at 2 cm intervals.
[0104] The above multilayer film has a maximum thickness deviation (MTD) expressed by Equation 2 below. 200 ) may be 3 ㎛ or less. Specifically, the multilayer film has a maximum thickness deviation (MTD) expressed by Equation 1 below. 200 ) may be 2.7 ㎛ or less, 2.5 ㎛ or less, or 2.0 ㎛ or less. When the above range is satisfied, the multilayer film can easily maintain flatness, thereby improving processability.
[0105] [Formula 2]
[0106] MTD 200 = THK max - THK min
[0107] In the above equation 1, THK max The maximum thickness, THK, was measured at 2 cm intervals on a specimen of a multilayer film with a width of 200 cm. min is the minimum thickness when the thickness of a multilayer film specimen with a width of 200 cm is measured at 2 cm intervals.
[0108] The multilayer film may have a light transmittance of 80% or more in a visible light region of a wavelength of 380 nm to 780 nm. Specifically, the light transmittance in a visible light region of a wavelength of 380 nm to 780 nm may be 85% or more, the light transmittance in a visible light region of a wavelength of 380 nm to 780 nm may be 90% or more, or the light transmittance in a visible light region of a wavelength of 380 nm to 780 nm may be 95% or more. The multilayer film may have a light transmittance in a visible light region of a wavelength of 380 nm to 780 nm of less than 100%. When the above range is satisfied, the multilayer film has excellent light transmittance, and thus can be applied to a display device described below to implement excellent optical characteristics.
[0109] The multilayer film may have a haze of 30% or less. Specifically, the multilayer film may have a haze of 15% or less, 10% or less, 9% or less, or 5% or less. The multilayer film may have a haze of 0.001% or more. When the above range is satisfied, transparency is secured, and the film may be used for various purposes requiring light transmission.
[0110]
[0111] Method for manufacturing multilayer films
[0112] A method for manufacturing a multilayer film according to another embodiment includes a step of preparing a composition, a step of obtaining an unstretched sheet, and a step of obtaining a multilayer film.
[0113] The composition preparation step is a step of preparing a first layer composition including a diol residue and a dicarboxylic acid residue and a second layer composition including a butenediol vinyl alcohol copolymer (BVOH).
[0114] Specific descriptions of the first layer composition and the second layer composition overlap with the description given above, so detailed descriptions are omitted.
[0115] The first layer composition and the second layer composition can each be prepared in chip form. Preparing each composition in chip form facilitates storage and application to the melting stage.
[0116] The above preparation step may further include a drying process for drying the first layer composition and the second layer composition in the form of chips, respectively. The second layer composition may be applied to the dried packaging as is.
[0117] The drying may be performed at 40°C to 100°C, or at 50°C to 80°C. The drying may be performed for 2 to 24 hours, or for 6 to 18 hours. For example, hot air drying may be applied for the drying. The moisture content in the dried chips may be 300 ppm or less, or 200 ppm or less. The moisture content may be 30 ppm or more. When chips dried in this manner are used, bubble generation due to moisture can be substantially suppressed, and the appearance of the manufactured product can be improved. In addition, smooth processability can also be provided.
[0118] The step of obtaining an unstretched sheet is a step of obtaining an unstretched sheet including a laminate in which a first layer (11) including the first layer composition and a second layer (12) including the second layer composition are alternately laminated by melt-extruding the first layer composition and the second layer composition, respectively.
[0119] The melt extrusion temperature of the first layer composition may be 220°C or higher. Specifically, the melt extrusion temperature of the first layer composition may be 230°C or higher, or may be 240°C or higher.
[0120] The melt extrusion temperature of the second layer composition may be 180°C or higher. Specifically, the melt extrusion temperature of the second layer composition may be 190°C or higher, or may be 200°C or higher.
[0121] The melt extrusion temperature of the first layer composition and the melt extrusion temperature of the second layer composition may be the same or different. For example, the difference between the melt extrusion temperature of the first layer composition and the melt extrusion temperature of the second layer composition may be 20° C. or less, or 15° C. or less. The difference may be 0° C. or more. The melting temperatures of the first layer composition and the second layer composition may be different for the purpose of controlling the melt viscosity. Specifically, when the extruder is configured in the order of a melting conduit (a conduit through which the molten resin moves) - a laminating means (e.g., a multilayer block) - a die, the temperatures of the melting conduits of the first layer composition and the second layer composition may be different. When the melt extrusion process is performed in the manner described above, it may be easier to control the thickness of each layer in the film.
[0122] The above laminate may have three or more alternately laminated first and second layers. Specifically, the above laminate may have three to 255 alternately laminated first and second layers.
[0123] The alternate lamination means may be any lamination means used in film manufacturing, and examples thereof include feed blocks and multi-manifolds.
[0124] The step of obtaining the above-mentioned unstretched sheet may include a step of forming the laminate into a sheet by a process such as pressing the laminate against a cooling roll.
[0125] The step of obtaining a multilayer film is a step of stretching and heat-setting the laminated sheet to obtain a multilayer film.
[0126] The stretching may be biaxial stretching or axial biaxial stretching. Specifically, the stretching may be stretching 2 to 4 times in the machine direction (MD) at 40°C to 130°C and stretching 3 to 6 times in the transverse direction (TD) at 50°C to 150°C.
[0127] The heat fixation step can be performed at 50°C to 300°C, 100°C to 200°C, 125°C to 175°C, or 140°C to 160°C.
[0128] Through the above stretching and heat fixing, the multilayer film can have improved mechanical strength and dimensional stability while having a thin thickness.
[0129] A detailed description of the multilayer film and the laminate is omitted as it overlaps with what was described above.
[0130] The thickness ratio, number of layers, etc. are as described above, and the thickness of each layer can be controlled and applied by taking into account the stretching process described later.
[0131] This method allows for the production of high-quality multilayer films in a relatively simple and efficient manner. The characteristics of the multilayer films produced in this manner are described below.
[0132]
[0133] display device
[0134] A display device according to another embodiment includes the multilayer film described above. A detailed description of the multilayer film is omitted as it overlaps with the description provided above.
[0135] The display device may include a light-emitting portion. The light-emitting portion may include a layer that directly or indirectly outputs light. Specifically, the light-emitting portion may further include a light source that directly outputs light and an insulating layer, a color filter layer, a wavelength conversion layer, and the like, in addition to the light source that directly outputs light.
[0136] The light source may be a backlight unit that outputs white light, or a backlight unit that outputs blue light. The light source may be an organic light-emitting element further including a hole injection layer, a hole transport layer, an electron transport layer, and an organic material layer.
[0137] The display device may include an encapsulating layer disposed on the light-emitting portion. When the organic layer is exposed to an external environment such as oxygen or moisture, oxidation of the constituent material may be accelerated, thereby reducing the light-emitting characteristics. The wavelength conversion layer may include a plurality of quantum dots. When the quantum dots are exposed to an external environment such as oxygen or moisture, the light-emitting characteristics may be reduced. The encapsulating layer comprising the multilayer film described above on the light-emitting portion can effectively prevent the organic layer or the wavelength conversion layer included in the light-emitting portion from being exposed to external oxygen due to the low oxygen permeability of the multilayer film.
[0138]
[0139] packaging materials
[0140] Packaging material according to another embodiment includes the multilayer film described above. Since a detailed description of the multilayer film is identical to that described above, a detailed description thereof will be omitted.
[0141] Packaging materials can be applied, for example, disposable packaging materials, food packaging materials, etc., and the multilayer film can be applied as is, or can be applied by further including aluminum foil, color layers, etc.
[0142] The above packaging material can effectively prevent the packaging material from being exposed to external oxygen due to the low oxygen permeability of the multilayer film.
[0143]
[0144] Hereinafter, a more detailed explanation will be given through specific examples. The following examples are merely illustrative examples to aid understanding of the present invention and are not intended to limit the scope of the present invention.
[0145]
[0146] [Example 1]
[0147] <Preparation of the first layer composition>
[0148] The first layer composition was prepared by mixing the diol component and the dicarboxylic acid component in an autoclave equipped with a stirrer and a distillation column.
[0149] Specifically, in the first layer composition, the diol component used was 80 mol% of ethylene glycol (EG), 15 mol% of neopentyl glycol (NPG), and 5 mol% of diethylene glycol (DEG), and the dicarboxylic acid component used was 100 mol% of dimethyl terephthalate (DMT).
[0150] The first layer composition was subjected to an ester exchange reaction with an ester exchange catalyst. Specifically, the catalyst for the ester exchange reaction was manganese acetate, applied in an amount of 0.07 parts by weight relative to the weight of the dicarboxylic acid. Subsequently, the ester exchange reaction was conducted at a temperature of 220°C while removing methanol, a byproduct.
[0151] When the above ester exchange reaction was completed, 0.07 parts by weight of silica having an average particle size of 0.28 ㎛ per 100 parts by weight of dicarboxylic acid and 0.4 parts by weight of trimethyl phosphate as a stabilizer per 100 parts by weight of dicarboxylic acid were added to the first layer composition.
[0152] After 5 minutes, 0.035 parts by weight of antimony trioxide and 0.005 parts by weight of tetrabutylene titanate as polymerization catalysts were added to the first layer composition, and stirred for 10 minutes.
[0153] Next, the first layer composition was transferred to a second reactor equipped with a vacuum facility, and the temperature was increased to 285°C, the pressure was gradually reduced, and polymerization was performed for about 210 minutes to obtain the first layer composition.
[0154]
[0155] <2nd layer composition>
[0156] As a second layer composition, a butenediol vinyl alcohol copolymer (BVOH) produced by hydrolysis of vinyl acetate after copolymerization of butenediol and vinyl acetate can be applied.
[0157] Alternatively, the butenediol vinyl alcohol copolymer (BVOH) may be BVOH sold as NICHIGO GPOLYMER™ by Mitsubishi Chemical. Specifically, BVE8049P of NICHIGO GPOLYMER™ was applied.
[0158]
[0159] <Manufacturing of multilayer barrier films>
[0160] The first layer composition was first dried in a dehumidifying dryer at 100°C for more than 4 hours, and then secondarily dried at 160°C for more than 6 hours to remove moisture. The second layer composition was applied as is to the dried packaging.
[0161] Using two extruders and a feed block capable of stacking in three layers in advance, the first layer composition was melt-extruded using an extruder with a temperature of 240°C, and the second layer composition was melt-extruded using an extruder with a temperature of 200°C. The ratio (volume ratio) of the discharge amounts of the first layer composition and the second layer composition was applied as 90:10.
[0162] Within the three-layer feed block, the first-layer composition was branched into two skin layers, the second-layer composition was branched into an intermediate layer, and then laminated. Afterwards, the laminate was passed through a 400 mm die and pressed against a cooling roll cooled to 20°C to obtain a total of three-layer unstretched sheets.
[0163] The above three-layer unstretched sheet was stretched 3.0 times in the longitudinal direction at 85°C and 4.0 times in the transverse direction at 110°C, and then heat-set was performed at 150°C with a relaxation rate of 1% to produce a 20 μm biaxially stretched three-layer film (Example 1).
[0164]
[0165] [Examples 2 to 4]
[0166] Example 2 was manufactured in the same manner as Example 1, but was manufactured to have a thickness of 45 μm after stretching and heat setting.
[0167] Example 3 was manufactured in the same manner as Example 1, but was manufactured to have a thickness of 60 μm after stretching and heat setting.
[0168] Example 4 was manufactured in the same manner as Example 1, but the discharge ratio (volume ratio) of the first resin and the second resin was applied as 95:5.
[0169]
[0170] [Examples 5 to 8]
[0171] Example 5 was manufactured in the same manner as Example 1, but the first layer composition was alternately laminated into 36 layers and the second layer composition into 36 layers within a multilayer feed block, and each of the first layer (11) and the second layer (12) was laminated into 73 layers, and a skin layer was positioned on the outermost layer of the upper and lower surfaces, and the first layer composition was applied to the skin layer to have the same composition as the first layer (11).
[0172] Example 6 was manufactured in the same manner as Example 5, but the discharge ratio (volume ratio) of the first layer composition and the second layer composition was applied as 70:30.
[0173] Example 7 was manufactured in the same manner as Example 1, but the first layer composition was alternately laminated into 72 layers and the second layer composition into 72 layers within a multilayer feed block, and each of the first layer (11) and the second layer (12) was laminated into 145 layers, and a skin layer was positioned on the outermost layers of the upper and lower surfaces, and the first layer composition was applied to the skin layer to have the same composition as the first layer (11).
[0174] Example 8 was manufactured in the same manner as Example 7, but the discharge ratio (volume ratio) of the first layer composition and the second layer composition was applied as 70:30.
[0175]
[0176] [Comparative Examples 1 to 4]
[0177] Comparative Example 1 used the first layer composition described in Example 1. The first layer composition was first dried at 100°C for 4 hours or more in a dehumidifying dryer, and secondarily dried at 160°C for 6 hours or more to remove moisture. The first layer composition was melt-extruded with an extruder having a temperature of 240°C. Thereafter, the first layer composition was passed through a 400 mm die and then pressed against a cooling roll cooled to 20°C to obtain a single-layer unstretched sheet. The single-layer unstretched sheet thus obtained was stretched 3.0 times in the longitudinal direction at 85°C and 4.0 times in the transverse direction at 100°C, and then heat-set at a temperature of 150°C and a relaxation rate of 1% to produce a 45 μm biaxially oriented single-layer film (Comparative Example 1).
[0178] Comparative Example 2 was manufactured in the same manner as Example 2, but the second layer composition used ethylene vinyl alcohol copolymer (EVOH) instead of butenediol vinyl alcohol copolymer (BVOH).
[0179] Comparative Example 3 was manufactured in the same manner as Comparative Example 2, but the first layer composition was alternately laminated into 36 layers and the second layer composition into 36 layers within the multilayer feed block, and each of the first layer (11) and the second layer (12) was laminated into 73 layers, and a skin layer was positioned on the outermost layer of the upper and lower surfaces, and the first layer composition was applied to the skin layer to have the same composition as the first layer (11).
[0180]
[0181] [Evaluation Example 1: Oxygen Permeability Evaluation]
[0182] The multilayer barrier film manufactured above was tested using OX-TRAN 702 from MOCON, USA, in accordance with ASTM D3985-17, with a test area of 50 cm. 2 Oxygen permeability was measured under the conditions of 1 atm, temperature 23.0 ± 0.5℃, and relative humidity 0%. [Unit: cc / m 2 ·day]
[0183]
[0184] [Evaluation Example 2: Film Interface Peeling]
[0185] The multilayer barrier film manufactured above was crumpled by hand for 5 seconds, and then the presence or absence of peeling between the first and second resin layers was determined. If no interfacial peeling occurred, the film was judged as good, and if interfacial peeling occurred, the film was judged as weak.
[0186]
[0187] [Evaluation Example 3: Film Water Separation]
[0188] Ten specimens of the multilayer film manufactured above were prepared, each measuring 1 cm in width and 1 cm in length. The film specimens were placed in a 500 ml beaker, and stirred for 30 minutes using a stirrer (300 rpm) while maintaining the water temperature at 60°C. Afterwards, the thickness of the specimens was checked to determine the water separation. If water separation occurred, it was judged as good.
[0189]
[0190] [Evaluation Example 4: Film Fairness]
[0191] The multilayer barrier film manufactured above was measured at 2 cm intervals on a 200 cm wide film to determine the maximum thickness (THK max ) and minimum thickness (THK min ) difference (MTD) 200 ) is measured. If the difference between the maximum and minimum thicknesses is less than 3㎛, it is judged to be good.
[0192]
[0193] The results of each measurement are summarized in Tables 1 and 2 below.
[0194] Example #Example 1Example 2Example 3Example 4Example 5Example 6Example 7Example 8Film thickness (㎛)2045602020202020Number of skin layers22222222Number of 1st layer / 2nd layer set layers----36367272Total number of laminates33337373145145Composition1st layer composition90909095907090702nd layer composition (BVOH)1010105103010302nd layer composition (EVOH)--------Film propertiesOxygen permeability (cc / (㎡·atm·day) )<0.01<0.01<0.01<0.01<0.01<0.01<0.01<0.01Interfacial delaminationGoodGoodGoodGoodGoodGoodGoodGoodGoodWater separationGoodGoodGoodGoodGoodGoodGoodGoodMTD 200 (㎛)2.62.41.92.72.53.02.72.9Haze(%)6.510255.44.75.04.14.5Moisture permeability(g / m) 2 ·day)4024234238433945Light transmittance90.7690.2390.0290.8390.8890.8690.9590.90
[0195] Comparative Example #Comparative Example 1Comparative Example 2Comparative Example 3Film Thickness (㎛) 454520Number of Skin Layers-22Number of 1st Layer / 2nd Layer Set Layers--36Total Number of Layers 1373Composition1st Layer Composition 10090902nd Layer Composition (BVOH)---2nd Layer Composition (EVOH)-1010Film PropertiesOxygen Permeability (cc / (㎡·atm·day) 72.46.14.3Interfacial Delamination-BrokeBrokeWater SeparabilityInsoluble in waterInsoluble in waterInsoluble in waterMTD 200 (㎛)1.911.18.4Haze(%)3.934.83.2Moisture permeability(g / m) 2 ·day)242622 Light transmittance 9190.8991.2
[0196] Comparative Example 1 is a film that uses the first layer (11) alone. It was confirmed that the film according to Comparative Example 1 has a high oxygen permeability and thus cannot function as a barrier film to block oxygen. Comparative Example 2 is a three-layer coextruded film manufactured by applying ethylene vinyl alcohol copolymer (EVOH) instead of butenediol vinyl alcohol copolymer (BVOH) to the second layer composition, unlike other examples. It was confirmed that the multilayer film according to Comparative Example 2 has a high oxygen permeability and thus cannot function as a barrier film to oxygen.
[0197] Comparative Example 3 was manufactured in the same manner as Comparative Example 2, but the first layer composition was alternately laminated into 36 layers and the second resin composition into 36 layers within a multilayer feed block, and each of the first layer (11) and the second layer (12) was laminated into 73 layers, and a skin layer was positioned on the outermost layers of the upper and lower surfaces, and the first layer composition was applied to the skin layer, resulting in a film having the same composition as the first layer (11). It was confirmed that the film according to Comparative Example 3 did not have a lower oxygen permeability to a desirable level.
[0198] On the other hand, the film manufactured by the embodiment of the embodiment has an oxygen permeability of 0.01 cc / (㎡·atm·day) or less. In addition, the film manufactured by the embodiment of the embodiment has good interfacial peeling characteristics evaluated by the evaluation example. In addition, the film manufactured by the embodiment of the embodiment has good water separation properties evaluated by the evaluation example. In addition, the film manufactured by the embodiment of the embodiment has a maximum thickness deviation (MTD) evaluated by the evaluation example. 200 ) was evaluated to be 3㎛ or less.
[0199]
[0200] Although the preferred embodiments of the implementation examples have been described in detail above, the scope of the implementation examples is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concepts of the implementation examples defined in the following claims also fall within the scope of the implementation examples.
[0201]
[0202] (Explanation of symbols)
[0203] 100: multilayer film 10: laminate
[0204] 11: 1st floor 12: 2nd floor
Claims
1. A laminate comprising a first layer and a second layer disposed on the first layer, The first layer comprises a polyester resin containing a diol residue and a dicarboxylic acid residue, The second layer comprises a butenediol vinyl alcohol copolymer, The above laminate has a density of 0.1 cc / m at 23°C. 2 A multilayer film having an oxygen permeability of less than day·atm.
2. In paragraph 1, A multilayer film, wherein the above diol residue is any one selected from the group consisting of an ethylene glycol residue, a diethylene glycol residue, a neopentyl glycol residue, and a combination thereof.
3. In paragraph 1, A multilayer film, wherein the diol residues comprise 5 to 35 mol% of neopentyl glycol residues based on the total diol residues.
4. In paragraph 1, A multilayer film, wherein the melting point of the first layer is lower than or equal to the thermal decomposition temperature of the second layer.
5. In paragraph 1, A multilayer film having a glass transition temperature of the second layer of 60°C or higher.
6. In paragraph 1, A multilayer film having a maximum thickness deviation of 3㎛ or less, as expressed by Equation 1 below; [Formula 1] MTD 50 = THK max - THK min In the above equation 1, MTD 50 is the maximum thickness deviation, and THK max The maximum thickness, THK, was measured at 2 cm intervals on a specimen of a multilayer film with a width of 50 cm. min is the minimum thickness when the thickness of a multilayer film specimen with a width of 50 cm is measured at 2 cm intervals.
7. In paragraph 1, The above laminate is formed by alternately laminating the first layer and the second layer in 3 to 225 layers, A multilayer film, wherein the first layer is located at the outermost layer of the laminate.
8. In paragraph 1, The above laminate is 50 g / m 2 ·A multilayer film having a moisture permeability of less than day.
9. Light-emitting part; and A sealing layer disposed on the above light-emitting portion; A display device, wherein the sealing layer comprises a multilayer film according to claim 1.
10. Packaging material comprising a multilayer film according to paragraph 1.
Citation Information
Patent Citations
Multilayered thermoplastic container or bottler for storage of a comestible product having improved resistance to oxygen permeation and processes for production thereof
KR100516550B1
Ethylene-vinyl alcohol copolymer and resin composition, and molded product obtained using the same
KR101890108B1
Wavelength conversion member and backlight unit and liquid crystal display device having the same
KR101970168B1
Heat-sealable film having barrier functionality
JP2008221811A
Gas barrier laminate film