Method and system for producing refined hydrocarbon from waste plastic

The method and system for refining hydrocarbons from waste plastic address impurity issues by preprocessing, pyrolysis, dehydration, and hydrogenation, achieving high-quality, high-yield light hydrocarbons suitable for blending with petroleum products and maintaining catalyst activity.

WO2024219933A1PCT designated stage expired Publication Date: 2024-10-24SK INNOVATION CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/095691
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-03-08
Filing Date
2024-04-05
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

The pyrolysis oil from waste plastic contains high levels of impurities like chlorine, nitrogen, and metals, leading to issues such as device corrosion, reduced catalyst durability, and decreased process efficiency, as well as limitations in blending with high-value fuels due to the formation of ammonium salts during hydrogenation.

Method used

A method and system that includes a pretreatment step to preprocess waste plastic, followed by pyrolysis, dehydration, and hydrogenation treatments, utilizing a high-temperature filter with beads and a temperature gradient, and reintroducing condensed liquid into the pyrolysis reactor to enhance the yield and quality of refined hydrocarbons, while minimizing impurity content and preventing ammonium salt formation.

Benefits of technology

This approach produces high-value-added pyrolysis oil with a high proportion of light hydrocarbons, improves yield, and reduces impurities, enabling the use of refined hydrocarbons as a raw material for blending with petroleum products, while maintaining catalyst activity and preventing reactor clogging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024095691_24102024_PF_FP_ABST
    Figure KR2024095691_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure relates to a method and a system for producing refined hydrocarbon from waste plastic, comprising: a preprocessing step for preprocessing waste plastic; a pyrolysis step for producing a pyrolysis gas by loading, into a pyrolysis reactor, the waste plastic which has been preprocessed in the preprocessing step; an upgrading step for producing a pyrolysis oil by loading the pyrolysis gas into a hot filter; a dehydration step for dehydrating a first mixed solution by applying a voltage thereto, the first mixed solution being formed by mixing the produced pyrolysis oil with washing water and a demulsifier; a hydrogenation step for producing a refined pyrolysis oil having impurities removed therefrom, by hydrogenating a second mixed solution formed by mixing the dehydrated first mixed solution with a sulfur source; and a second hydrogenation step for secondarily hydrogenating the refined pyrolysis oil, wherein a liquid condensed in the hot filter is reloaded into the pyrolysis reactor.
Need to check novelty before this filing date? Find Prior Art

Description

Method and system for producing purified hydrocarbons from waste plastics

[0001] The present disclosure relates to a method and a system for producing purified hydrocarbons from waste plastic.

[0002] Pyrolysis oil, which is produced through cracking and pyrolysis of waste materials such as waste plastic pyrolysis oil, contains a large amount of impurities originating from the waste materials. Therefore, when used as fuel, there are concerns about the emission of air pollutants such as SOx and NOx. In particular, there is a problem that the chlorine component is converted to hydrogen chloride during the high-temperature processing process, which can cause equipment corrosion and is emitted. Furthermore, waste plastic pyrolysis oil has a higher content of impurities such as chlorine, nitrogen, and metals than the oil produced from crude oil using conventional methods. Therefore, only a limited amount can be blended into high-value-added fuels such as gasoline and diesel, and it must go through a refining process to be used in large quantities.

[0003] As in the prior art, when reacting oil and hydrogen under a hydrogenation catalyst, chlorine compounds such as hydrogen chloride and nitrogen compounds produced along with the refined oil react to produce ammonium salts (NH4Cl), which cause various process problems. Specifically, the ammonium salts produced inside the reactor when oil and hydrogen react not only cause corrosion of the reactor, reducing its durability, but also cause numerous process problems such as differential pressure generation and consequently reduced process efficiency. Furthermore, if the process is operated for a long period of time, impurity particles in the waste plastic pyrolysis oil become stuck inside the reactor, similarly causing various process problems.

[0004] Therefore, in the purification process of waste plastic pyrolysis oil containing impurities such as chlorine and nitrogen, a technology is required that can prevent the generation of ammonium salt (NH4Cl) or minimize its generation, and prevent the phenomenon of impurity particles from sticking within the reactor.

[0005] In addition to removing impurities, it is necessary to increase the yield of waste plastic pyrolysis oil and to increase the added value of waste plastic pyrolysis oil through hardening to secure economic feasibility.

[0006] In addition, there is a need for the development of a technology capable of obtaining refined hydrocarbons with a high proportion of light hydrocarbons from the waste plastic pyrolysis oil.

[0007] According to one aspect of the present disclosure, a high value-added pyrolysis oil having a high proportion of light hydrocarbons can be produced from waste plastic containing a large amount of impurities, and a refined hydrocarbon having a high proportion of light hydrocarbons can be obtained therefrom.

[0008] According to another aspect of the present disclosure, the yield of pyrolysis oil obtained from waste plastic can be improved.

[0009] According to another aspect of the present disclosure, a high value-added pyrolysis oil with reduced impurities can be produced from waste plastic containing a large amount of impurities, and a refined hydrocarbon with reduced impurities can be obtained therefrom.

[0010] According to another aspect of the present disclosure, a method and device for producing purified hydrocarbons from waste plastics can be provided with a simplified process.

[0011] According to one aspect of the present disclosure, it is possible to produce high value-added pyrolysis oil having excellent quality and usable as a raw material for blending with existing petroleum products or in a refining process, and to obtain refined hydrocarbons therefrom.

[0012] According to another aspect of the present disclosure, a method and system for producing purified hydrocarbons from waste plastics can be provided, which minimize the production of ammonium salts (NH4Cl) from waste plastic pyrolysis oil containing impurities including chlorine and nitrogen.

[0013] According to one aspect of the present disclosure, a method and system for producing purified hydrocarbons from waste plastics can be provided, in which the activity of the catalyst is maintained for a long time, the purification efficiency is excellent, and long-term operation is possible.

[0014] According to another aspect of the present disclosure, a method and system for producing purified hydrocarbon from waste plastics can be provided, which can prevent the phenomenon of fixation of impurity particles.

[0015] According to another aspect of the present disclosure, a method and system for producing refined hydrocarbons from waste plastics can be provided, which have very low content of impurities such as chlorine, nitrogen, oxygen, metals, etc. and olefin content, and are of excellent quality, so that they can be used as raw materials for blending with existing petroleum products or for refining and petrochemical processes.

[0016] The present disclosure provides a method for producing refined hydrocarbons from waste plastic, comprising: a pretreatment step of pretreating waste plastic; a pyrolysis step of introducing the pretreated waste plastic into a pyrolysis reactor to produce pyrolysis gas; a hardening step of introducing the pyrolysis gas into a hot filter to produce pyrolysis oil; a dehydration step of dehydrating a first mixture obtained by mixing the produced pyrolysis oil with washing water and a demulsifier by applying voltage; a hydrogenation step of hydrogenating a second mixture obtained by mixing the dehydrated first mixture with a sulfur source to produce refined pyrolysis oil from which impurities have been removed; and a second hydrogenation step of hydrogenating the refined pyrolysis oil, wherein a liquid condensed in the hot filter is reintroduced into the pyrolysis reactor.

[0017] In one embodiment according to the present disclosure, the high temperature filter may be filled with beads.

[0018] In one embodiment according to the present disclosure, the bead may include at least one selected from the group consisting of silica (SiO2) and aluminum oxide (Al2O3).

[0019] In one embodiment according to the present disclosure, the method for producing purified hydrocarbon from waste plastic may be such that a temperature gradient is formed in the high-temperature filter.

[0020] In one embodiment according to the present disclosure, the temperature gradient may be formed by providing at least two heaters on the outside of the high temperature filter.

[0021] In one embodiment according to the present disclosure, the pyrolysis reactor may comprise at least two batch reactors.

[0022] In one embodiment according to the present disclosure, the thermal decomposition step can be performed by switching operation of at least two batch reactors.

[0023] In one embodiment according to the present disclosure, the refined pyrolysis oil may be mixed with petroleum hydrocarbons and subjected to secondary hydrogenation treatment to form a mixed oil.

[0024] In one embodiment according to the present disclosure, the refined pyrolysis oil may be included in an amount of 90 wt% or less relative to the total weight of the mixed oil.

[0025] In one embodiment according to the present disclosure, the waste plastic may include at least one selected from the group consisting of polyethylene (PE), polypropylene (PP), polyethylene terephthalate (PET), polyvinyl chloride (PVC), and polystyrene (PS).

[0026] In one embodiment according to the present disclosure, the method for producing purified hydrocarbon from waste plastic may be such that, in the dehydration step, the pyrolysis oil may be mixed in a larger volume than the wash water.

[0027] In one embodiment according to the present disclosure, the method for producing purified hydrocarbon from waste plastic may be such that, in the dehydration step, the first mixture is mixed with the pyrolysis oil and the washing water in a volume ratio of 1:0.001 to 0.5.

[0028] In one embodiment according to the present disclosure, the method for producing purified hydrocarbon from waste plastic may be such that, in the dehydration step, the first mixture is mixed with the pyrolysis oil and the demulsifier in a volume ratio of 1:0.000001 to 0.001.

[0029] In one embodiment according to the present disclosure, the demulsifier may be one or a mixture of two or more selected from the group consisting of polyethylene glycol, tert-butanol, acetone, alkylnaphthalenesulfonate, alkylbenzenesulfonate, nonionic alkoxylated alkyl phenol resin, polyalkyleneoxide, and polyoxyethylene sorbitan ester.

[0030] In addition, the present disclosure can provide a system for producing refined hydrocarbons from waste plastic, including: a pretreatment device for pretreating waste plastic; a pyrolysis reactor for producing pyrolysis gas by introducing waste plastic pretreated in the pretreatment device; a hot filter for producing pyrolysis oil by introducing the pyrolysis gas; a connecting pipe for connecting the hot filter and the pyrolysis reactor so that a liquid condensed in the hot filter is reintroduced into the pyrolysis reactor; a dehydration device for dehydrating a first mixture obtained by mixing the produced pyrolysis oil with washing water and a demulsifier by applying voltage; a hydrogenation device for hydrogenating a second mixture obtained by mixing the dehydrated first mixture with a sulfur source to produce refined pyrolysis oil from which impurities are removed; and a second hydrogenation device for hydrogenating the refined pyrolysis oil.

[0031] In one embodiment according to the present disclosure, the high temperature filter may be filled with beads.

[0032] In one embodiment according to the present disclosure, the bead may include at least one selected from the group consisting of silica (SiO2) and aluminum oxide (Al2O3).

[0033] In one embodiment according to the present disclosure, the manufacturing system may have at least two heaters external to the high temperature filter.

[0034] In one embodiment according to the present disclosure, the method for producing refined hydrocarbon from waste plastic may further include a distillation step of distilling the refined pyrolysis oil after the hydrogenation treatment step.

[0035] In one embodiment according to the present disclosure, the method for producing refined hydrocarbons from the waste plastic may be such that hydrocarbons derived from the refined pyrolysis oil separated in the distillation step and petroleum hydrocarbons are mixed and subjected to a second hydrogenation process to form a mixed oil.

[0036] A method and system for producing refined hydrocarbons from waste plastics according to one embodiment of the present disclosure can produce high value-added pyrolysis oil having a high proportion of light hydrocarbons from waste plastics containing a large amount of impurities, and can obtain refined hydrocarbons having a high proportion of light hydrocarbons therefrom.

[0037] A method and system for producing purified hydrocarbons from waste plastics according to one embodiment of the present disclosure can improve the yield of pyrolysis oil obtained from waste plastics.

[0038] A method and system for producing purified hydrocarbon from waste plastic according to one embodiment of the present disclosure can produce high value-added pyrolysis oil with reduced impurities from waste plastic containing a large amount of impurities, and can obtain purified hydrocarbon with reduced impurities therefrom.

[0039] A method and system for producing purified hydrocarbons from waste plastics according to another embodiment of the present disclosure can simplify the process for producing purified hydrocarbons from waste plastics.

[0040] The method and system for producing refined hydrocarbons from waste plastic according to one embodiment of the present disclosure can produce high value-added pyrolysis oil having a high proportion of light hydrocarbons that is excellent in quality and can be used as a raw material for blending with existing petroleum products or in an oil refining process, and can obtain refined hydrocarbons having a high proportion of light hydrocarbons therefrom.

[0041] A method and system for producing purified hydrocarbons from waste plastics according to one embodiment of the present disclosure can prevent or minimize the generation of ammonium salts (NH4Cl) during the purification of waste plastic pyrolysis oil containing impurities including chlorine and nitrogen, and can prevent the phenomenon of fixation of impurity particles.

[0042] The method and system for producing purified hydrocarbons from waste plastic according to one embodiment of the present disclosure have excellent purification efficiency and enable long-term operation of the process by preventing catalyst deactivation due to moisture.

[0043] The method and system for producing refined hydrocarbons from waste plastic according to one embodiment of the present disclosure can provide waste plastic pyrolysis oil having a very low content of impurities such as chlorine, nitrogen, oxygen, and metals and an olefin content, and having excellent quality, so that it can be used for blending with existing petroleum products or as a raw material for oil refining and petrochemical processes.

[0044] The method and system for producing purified hydrocarbons from waste plastic according to one embodiment of the present disclosure can be used in the production of eco-friendly petrochemical products using waste plastic as a raw material.

[0045] FIG. 1 is a flow chart showing a method for producing purified hydrocarbons from waste plastic according to one embodiment of the present disclosure.

[0046] Figure 2 is a process diagram for manufacturing waste plastic pyrolysis oil according to one embodiment of the present disclosure.

[0047] FIG. 3 is a drawing of a high temperature filter according to one embodiment of the present disclosure.

[0048] FIG. 4 is a process diagram of a dehydration step, a hydrogenation step, and a second hydrogenation step according to one embodiment of the present disclosure.

[0049] The advantages and features of the present disclosure, and methods for achieving them, will become clearer with reference to the embodiments described in detail below. However, the present disclosure is not limited to the embodiments disclosed below and may be implemented in various different forms. These embodiments are provided solely to ensure the completeness of the present disclosure and to fully inform those skilled in the art of the scope of the invention. The present disclosure is defined solely by the scope of the claims.

[0050] Unless otherwise defined, all terms (including technical and scientific terms) used in this specification may be used in a meaning that can be commonly understood by a person of ordinary skill in the art to which this disclosure belongs.

[0051] As used herein, the singular forms of terms may be construed to include the plural forms as well, unless otherwise specified.

[0052] The numerical ranges used herein include lower and upper limits and all values ​​within that range, increments logically derived from the shape and width of the defined range, all doubly defined values, and all possible combinations of upper and lower limits of numerical ranges defined in different shapes. Unless otherwise specified in the specification of the present disclosure, values ​​outside the defined range that may arise due to experimental error or rounding of values ​​are also included in the defined numerical range.

[0053] The term "includes" as used herein is an open-ended description having the equivalent meaning of expressions such as "comprises," "contains," "has," and "characterizes," and does not exclude additional elements, materials, or processes not listed.

[0054] The unit of % used in this specification without special mention means weight % unless otherwise defined.

[0055] In this specification, “A to B” means “A or more and B or less” unless otherwise specifically defined.

[0056] In this specification, “pyrolysis oil yield” means the weight ratio of oil to the total weight of oil, aqueous by-products, pyrolysis residue (char), and by-product gas among the products of the pyrolysis step.

[0057] As used herein, the term 'vertical electrode' may mean an electrode erected vertically with respect to the ground, and the term 'horizontal electrode' may mean an electrode laid horizontally with respect to the ground.

[0058] Below, the method and system for producing purified hydrocarbons from waste plastics of the present disclosure will be described in detail. However, these are merely exemplary, and the present disclosure is not limited to the specific embodiments described as examples.

[0059] Referring to FIG. 1, the present disclosure comprises a pretreatment step (P-101) of pretreating waste plastic; a pyrolysis step (P-102) of introducing the waste plastic pretreated in the pretreatment step into a pyrolysis reactor to produce pyrolysis gas; a hardening step (P-103) of introducing the pyrolysis gas into a hot filter to produce pyrolysis oil; a dehydration step (P-104) of applying voltage to a first mixture solution of the produced pyrolysis oil mixed with washing water and a demulsifier to dehydrate it; a hydrogenation step (P-105) of hydrogenating a second mixture solution of the dehydrated first mixture solution and a sulfur source to produce refined pyrolysis oil from which impurities are removed; And a second hydrogenation treatment step (P-106) of second hydrogenation treatment of the refined pyrolysis oil; and a liquid condensed in the high-temperature filter is reintroduced into the pyrolysis reactor, thereby providing a method for producing refined hydrocarbon from waste plastic.

[0060] Accordingly, a method for producing refined hydrocarbons from waste plastics according to one embodiment of the present disclosure can produce high value-added pyrolysis oil having a high proportion of light hydrocarbons from waste plastics containing a large amount of impurities, and can obtain refined hydrocarbons having a high proportion of light hydrocarbons therefrom. In addition, the yield of the obtained pyrolysis oil can be significantly improved.

[0061] In addition, a method for producing refined hydrocarbon from waste plastic according to one embodiment of the present disclosure can produce high value-added pyrolysis oil with reduced impurities from waste plastic containing a large amount of impurities, and can obtain refined hydrocarbon with reduced impurities therefrom.

[0062] A method for producing refined hydrocarbons from waste plastics according to one embodiment of the present disclosure can improve cracking of heavy hydrocarbons in pyrolysis oil by reintroducing the liquid condensed in the high-temperature filter (15) into the pyrolysis reactor (14). Accordingly, pyrolysis oil having a high proportion of light hydrocarbons can be produced, and refined hydrocarbons having a high proportion of light hydrocarbons can be obtained therefrom.

[0063] According to another embodiment of the present disclosure, the high-temperature filter may be filled with beads. When the high-temperature filter is filled with beads, the inertness and heat transfer effects within the high-temperature filter are maximized, thereby producing pyrolysis oil with a high proportion of light hydrocarbons. Furthermore, the yield of the pyrolysis oil may be improved.

[0064] According to one embodiment of the present disclosure, the beads may be filled in the high temperature filter at 50 vol% or more, 60 vol% or more, 70 vol% or more, 80 vol% or more, 85 vol% or more, 90 vol% or more, 95 vol% or less, 93 vol% or less, 91 vol% or less, 90 vol% or less, 89 vol% or less, 87 vol% or less, 85 vol% or less, 80 vol% or less, or a value between the above values ​​relative to the internal volume of the high temperature filter. Specifically, the beads may be filled in the high temperature filter at 70 to 95 vol%, 80 to 90 vol%, or 85 to 90 vol% relative to the internal volume of the high temperature filter, but is not limited thereto.

[0065] According to one embodiment of the present disclosure, a temperature gradient can be formed in the high-temperature filter. When a temperature gradient is formed in the high-temperature filter, the pyrolysis gas moving to the upper part of the high-temperature filter and the liquid condensing to the lower part can be efficiently circulated, thereby producing pyrolysis oil with a high proportion of light hydrocarbons. Furthermore, refined hydrocarbons with a high proportion of light hydrocarbons can be produced from this. Furthermore, the yield of the pyrolysis oil can be improved.

[0066] According to one embodiment of the present disclosure, the temperature gradient may be such that the temperature at the bottom of the high-temperature filter is higher than the temperature at the top of the high-temperature filter. According to another embodiment of the present disclosure, the temperature gradient may be such that the temperature at the bottom of the high-temperature filter is higher than the temperature at the middle of the high-temperature filter, and the temperature at the middle of the high-temperature filter is higher than the temperature at the top of the high-temperature filter. Accordingly, the circulation efficiency and heat transfer efficiency within the high-temperature filter may be improved.

[0067] Referring to FIG. 3, according to one embodiment of the present disclosure, the temperature gradient may be formed by providing at least two heaters (17) on the outside of the high-temperature filter (15). According to another embodiment of the present disclosure, the temperature gradient may be formed by providing at least three heaters on the outside of the high-temperature filter. When at least two heaters are provided on the outside of the high-temperature filter, it is easy to form a temperature gradient of the high-temperature filter, and the temperatures of the upper, middle, and lower parts can be flexibly controlled depending on the operating conditions of the high-temperature filter, thereby enabling flexible process operation. For example, the temperature gradient of the high-temperature filter may be formed by independently controlling the temperatures of the upper, middle, and lower parts by providing heaters at the upper, middle, and lower parts of the high-temperature filter, respectively.

[0068] According to one embodiment of the present disclosure, the temperature at the bottom of the high temperature filter may be 400°C or higher, 420°C or higher, 440°C or higher, 460°C or higher, 480°C or higher, 500°C or higher, 550°C or higher, 600°C or higher, 700°C or lower, 600°C or lower, 550°C or lower, 530°C or lower, 510°C or lower, or a value between the above values.

[0069] According to one embodiment of the present disclosure, the temperature at the top of the high temperature filter may be 400°C or higher, 420°C or higher, 440°C or higher, 460°C or higher, 480°C or higher, 500°C or higher, 600°C or lower, 550°C or lower, 500°C or lower, 480°C or lower, 460°C or lower, 440°C or lower, 420°C or lower, or 400°C or lower.

[0070] According to one embodiment of the present disclosure, the temperature of the stop of the high temperature filter may be 300°C or more and 600°C or less, 400°C or more and 600°C or less, 400°C or more and 500°C or less, 420°C or more and 480°C or less, or 440°C or more and 460°C or less.

[0071] According to one embodiment of the present disclosure, the pretreatment step may include: a) reacting waste plastic with a neutralizing agent; and b) reacting the product of step a) with a copper compound. Accordingly, the pretreatment step can treat the waste plastic raw material to reduce the Cl content to a level suitable for introduction into a refining process.

[0072] According to one embodiment of the present disclosure, in step b), additives or neutralizing agents such as metal oxides and zeolites other than copper compounds may be used. The metal oxide may be in the form of an oxide of a divalent metal, but is not limited thereto.

[0073] The above waste plastic may include at least one selected from the group consisting of polyethylene (PE), polypropylene (PP), polyethylene terephthalate (PET), polyvinyl chloride (PVC), and polystyrene (PS). The waste plastic may include organic chlorine (Cl), inorganic chlorine (Inorganic Cl), and aromatic chlorine (Aromatic Cl), and the chlorine content of the waste plastic may be 10 ppm or more, 50 ppm or more, 100 ppm or more, or 100 to 1,000 ppm, but the present disclosure is not limited thereto. The pyrolysis oil produced through cracking or pyrolysis reaction of waste plastic, such as waste plastic pyrolysis oil, contains a large amount of impurities originating from the waste plastic. In particular, it is necessary to pretreat the pyrolysis oil to remove chlorine components such as organic / inorganic chlorine. The waste plastic may be classified into household waste plastic and industrial waste plastic. Household waste plastics are plastics mixed with PVC, PS, PET, PBT, etc. other than PE and PP. In the present disclosure, it may refer to mixed waste plastics containing 3 wt% or more of PVC along with PE and PP. Since the chlorine derived from PVC has a high ratio of organic Cl and inorganic Cl, the Cl in household waste plastics can be removed with high efficiency even with inexpensive neutralizing agents (Ca series, Zn series, Al series). Most industrial waste plastics are made up of PE / PP, but there is a problem that it is difficult to remove them with the general inexpensive neutralizing agents mentioned above because the organic Cl content derived from adhesive or dye components is high, and in particular, the ratio of Cl (aromatic chlorine) contained in the aromatic ring is high.

[0074] The present disclosure is characterized in that it removes chlorine of at least 95 wt%, at least 97 wt%, at least 98 wt%, or at least 99 wt%, based on the total weight of chlorine contained in waste plastic derived from waste plastic. For this purpose, it is preferable to remove chlorine contained in the aromatic ring.

[0075] The above step a) is a step of reacting waste plastic with a neutralizing agent, and a large amount of hydrogen chloride generated during the melting and thermal decomposition process of PVC, etc. can be removed in the form of a neutralized salt.

[0076] The neutralizing agent may include a metal oxide, hydroxide, carbonate, or a combination thereof, and the metal may be calcium, aluminum, magnesium, zinc, copper, iron, or a combination thereof. Specifically, the neutralizing agent may be copper oxide, aluminum oxide, calcium oxide, magnesium oxide, zinc oxide, or iron oxide. The neutralizing agent may include a zeolite component. Specifically, the neutralizing agent may include a spent FCC catalyst (E-cat) including a zeolite component, and may further include a spent FCC catalyst in the metal oxide. Specifically, the neutralizing agent may be calcium oxide, a spent FCC catalyst, copper metal, or copper oxide, or may be calcium oxide.

[0077] In one embodiment according to the present disclosure, the neutralizing agent may be added during the thermal decomposition step.

[0078] The neutralizing agent may be mixed in an amount of 0.5 to 20 wt%, 1 to 10 wt%, or 1 to 5 wt% based on the total weight of the waste plastic. In addition, the ... M / N Cl )1 to 25, specifically 0.7 to 15, more specifically 0.5 to 5.

[0079] Meanwhile, the total mole number of chlorine element (Cl) in the waste plastic may refer to the total mole number of chlorine element in the solid raw material of the waste plastic before pretreatment and pyrolysis.

[0080] In the above a) chlorine removal step, the chlorine weight ratio (C1 / C) of the product of step a) to the chlorine content of 100 wt% (C) of the waste plastic may be 50% or less, 40% or less, or 20 to 30%. Chlorine remaining in the waste plastic after step a) can be effectively removed in step b).

[0081] Step b) is a step of reacting the product of step a) with a copper compound, and a small amount of organic chlorine and aromatic chlorine not removed in step a) can be removed with a copper compound (catalyst). When a copper compound is used together with the neutralizing agent of step a) or as a substitute for the neutralizing agent, the copper compound may react first with chlorine at the end of the hydrocarbon chain among organic chlorine and inorganic chlorine (hydrogen chloride), making it difficult for it to come into contact with aromatic chlorine, which is difficult to remove with a neutralizing agent. In addition, the initial pyrolysis time when the temperature inside the reactor is raised for pretreatment or pyrolysis is relatively low (250-300℃), and hydrogen chloride begins to be generated, so it is preferable to remove chlorine with a neutralizing agent first. After that, when the full-scale pyrolysis step proceeds, the temperature is relatively high, and the removal reaction of aromatic chlorine is activated. Therefore, it is effective to first remove organic Cl and inorganic Cl with hydrogen chloride using a neutralizing agent, and then to remove aromatic chlorine with a copper compound.

[0082] The copper compound may include at least one selected from the group consisting of copper metal (Cu), copper oxide (CuO), copper hydroxide (Cu(OH)2) and copper carbonate (CuCO3), and specifically may include copper metal (Cu) and / or copper oxide (CuO).

[0083] The copper compound may be mixed in an amount of 0.1 to 20 wt%, 0.5 to 10 wt%, or 1 to 5 wt% based on the total weight of the product of step a). In addition, the ... Cu / N Cl )1 to 10, specifically 0.7 to 5, more specifically 0.5 to 3.

[0084] Meanwhile, the total mole number of chlorine element (Cl) in the waste plastic may refer to the total mole number of chlorine element in the solid raw material of the waste plastic before pretreatment and pyrolysis.

[0085] In the above b) chlorine removal step, the chlorine content ratio (C2 / C) of the product of step b) to the chlorine content of 100 wt% (C) of the waste plastic may be 10% or less, 5% or less, or 0.5 to 3%.

[0086] According to one embodiment of the present disclosure, step a) may be performed at a temperature of 200 to 320°C, and step b) may be performed at a temperature of 400 to 550°C. When steps a) and b) are performed at each of the above temperature ranges, chlorine in waste plastic can be effectively removed.

[0087] According to one embodiment of the present disclosure, the thermal decomposition step may further include: a) a step of reacting waste plastic with a neutralizing agent; and b) a step of reacting the product of step a) with a copper compound.

[0088] In the present disclosure, the pretreatment step may additionally include a crushing step of feeding waste plastic into a screw reactor and crushing it. The crushing of the waste plastic may be performed using a crushing process known in the art. For example, the waste plastic may be fed into the pretreatment reactor (13) and heated to approximately 300°C to produce a pellet-shaped hydrocarbon flow precursor. However, the present disclosure is not limited thereto.

[0089] According to one embodiment of the present disclosure, the crushing step may be performed at room temperature.

[0090] For example, the crushing step may involve mixing the waste plastic and a neutralizing agent and introducing them into a pretreatment reactor. When the waste plastic and the neutralizing agent, such as calcium oxide, are mixed and crushed at room temperature, a mechanochemical reaction occurs, generating hydrocarbons and CaOHCl. This has the effect of stably fixing chlorine in the waste plastic raw material into CaOHCl.

[0091] Next, the pretreatment step may be to heat the crushed waste plastic by putting it into a pretreatment reactor, and to physically and chemically treat the solid waste plastic raw material to remove chlorine and produce a hydrocarbon flow precursor (pyrolysis raw material). The hydrocarbon flow precursor may mean a waste plastic melt, and the waste plastic melt may mean all or part of the crushed or uncrushed solid waste plastic converted into liquid waste plastic.

[0092] For example, the pretreatment step may be to introduce the crushed or uncrushed waste plastic and the neutralizing agent into a pretreatment reactor and heat them, respectively. Furthermore, the pretreatment step may be to introduce the crushed or uncrushed waste plastic and the neutralizing agent into a pretreatment reactor to perform a first pretreatment (heating), and then introduce a copper compound into the pretreatment reactor to perform a second pretreatment (heating).

[0093] The above heating may be performed at a temperature of 200 to 320°C and atmospheric pressure. Specifically, the heating may be performed at a temperature of 250 to 320°C or 280 to 300°C. Generally, the pretreatment temperature for waste plastic is at least 250°C, but the pretreatment can be easily performed at a lower temperature of 200°C to generate hydrogen or methane gas from the hydrocarbons after the above dechlorination.

[0094] The above pretreatment reactor may be an extruder, an autoclave reactor, a batch reactor, etc., and may be, for example, an auger reactor, but the present disclosure is not limited thereto.

[0095] The above pyrolysis step may be a step of introducing pyrolysis raw materials classified into three material phases, namely gaseous, liquid (oil + wax + water), and solid, into a pyrolysis reactor, and specifically, may be a step of introducing and heating the non-pretreated or pretreated waste plastic into the pyrolysis reactor.

[0096] For example, the pyrolysis step may be to mix pretreated waste plastic and a divalent metal compound, specifically a copper compound, and introduce the mixture into a pyrolysis reactor and heat the mixture. In addition, the pyrolysis step may be to perform a first pyrolysis by mixing waste plastic and a neutralizing agent, introduce the mixture into a pyrolysis reactor and heat the mixture, and then perform a second pyrolysis by introducing a divalent metal compound, specifically a copper compound, into the pyrolysis reactor and heating the mixture. The pyrolysis may be performed at least twice continuously or discontinuously.

[0097] The above heating can be performed at a temperature of 320 to 900°C, specifically 350 to 700°C, more specifically 400 to 550°C, in a non-oxidizing atmosphere. In addition, the heating can be performed at normal pressure. The non-oxidizing atmosphere is an atmosphere in which waste plastic does not oxidize (burn), and may be, for example, an atmosphere in which the oxygen concentration is adjusted to 1% by volume or less, an atmosphere of an inert gas such as nitrogen, water vapor, carbon dioxide, and argon.

[0098] If the heating temperature is 400℃ or higher, the fusion of chlorine-containing plastics can be prevented, and conversely, if the heating temperature is 550℃ or lower, the chlorine in the waste plastic can remain in the pyrolysis residue (Char) in the form of XCl2, where X is a divalent metal cation, specifically, CaCl2, CuCl2, etc.

[0099] The above pyrolysis reactor can be carried out in a high-temperature, high-pressure reactor (autoclave reactor), a batch stirred reactor, a fluidized-bed reactor, a packed-bed reactor, etc., and specifically, can be applied to all reactors capable of stirring and temperature control, and according to one embodiment according to the present disclosure, can be carried out in a batch reactor.

[0100] According to one embodiment of the present disclosure, the pyrolysis reactor may comprise at least two batch reactors.

[0101] According to one embodiment of the present disclosure, the thermal decomposition step may be performed by switching the operation of at least two batch reactors. Accordingly, the thermal decomposition step can ensure process continuity even at high temperatures.

[0102] In a method for producing refined hydrocarbons from waste plastic according to one embodiment of the present disclosure, the pyrolysis step or the hardening step may further include at least one step selected from the group consisting of a pyrolysis gas recovery step for recovering a pyrolysis gas phase and a pyrolysis liquid phase as gas, and a separation step for separating a pyrolysis solid phase (solid content) into fine particles and coarse particles.

[0103] In the above gas recovery step, pyrolysis gas containing low-boiling-point hydrocarbon compounds such as methane, ethane, and propane, which is generated in the pyrolysis step or the hardening step, is recovered. The pyrolysis gas may generally contain combustible substances such as hydrogen, carbon monoxide, and low-molecular-weight hydrocarbon compounds. Examples of hydrocarbon compounds include methane, ethane, ethylene, propane, propene, butane, and butene. Since such pyrolysis gas contains combustible substances, it can be used as fuel.

[0104] In the above separation step, the solid phase generated in the pyrolysis step or the hardening step, such as the solid matter, for example, carbide, neutralizer, and / or copper compound, can be separated into fine particles and coarse particles. Specifically, the solid matter generated by the pyrolysis reaction can be separated into fine particles and coarse particles by classifying using a sieve having a smaller average particle diameter than the chlorine-containing plastic and a larger average particle diameter than the neutralizer and copper compound. In the above separation step, it is preferable to separate the solid matter into fine particles containing a relatively large amount of the chlorine-containing neutralizer and copper compound, and coarse particles containing a relatively large amount of carbide. The fine particles and carbide can be reprocessed as needed, and can be reused in the pyrolysis step, used as fuel, or discarded, but the present disclosure is not limited thereto.

[0105] According to one embodiment of the present disclosure, the high-temperature filter may be filled with at least one selected from the group consisting of beads and neutralizing agents.

[0106] According to another embodiment of the present disclosure, the high-temperature filter may be filled with beads. When the high-temperature filter is filled with beads, the inert effect and heat exchange effect within the high-temperature filter are maximized, thereby producing pyrolysis oil with a high proportion of light hydrocarbons.

[0107] According to one embodiment of the present disclosure, the beads may include at least one selected from the group consisting of silica (SiO2) and aluminum oxide (Al2O3). Specifically, when the beads include silica (SiO2), the inert effect and heat exchange effect within the high-temperature filter are maximized, and stable process operation is possible without wear even during long-term high-temperature operation.

[0108] According to one embodiment of the present disclosure, the bead may be, but is not limited to, a glass bead.

[0109] According to one embodiment of the present disclosure, the diameter of the beads may be 0.1 mm or more, 1 mm or more, 1.5 mm or more, 2 mm or more, 2.5 mm or more, 3 mm or more, 10 mm or less, 8 mm or less, 6 mm or less, 4 mm or less, 3.5 mm or less, 3 mm or less, 2.5 mm or less, 2 mm or less, or a value between the above values, and specifically, may be 1 mm to 5 mm, 2 mm to 4 mm, 2.5 mm to 3.5 mm, but is not limited thereto. By filling the beads having the above particle size into the high-temperature filter in the hardening step of the present disclosure, not only can the residence time (GHSV) of the pyrolysis gas be controlled to achieve hardening of the oil, but also the generation of differential pressure in the high-temperature filter can be suppressed, thereby improving the efficiency of process operation.

[0110] According to one embodiment of the present disclosure, in the hardening step, the pyrolysis gas may be introduced into a hot filter filled with the neutralizing agent to produce pyrolysis oil.

[0111] The above-mentioned hardening step may be carried out at a temperature of 400 to 550°C and a pressure of atmospheric pressure to 0.5 bar in an oxygen-free atmosphere, and the oxygen-free atmosphere may be an inert gas atmosphere or a closed system atmosphere without oxygen. In the temperature range of the above-mentioned hardening step, the hardening of the pyrolysis gas may be carried out well, thereby improving the clogging phenomenon caused by wax and the occurrence of differential pressure.

[0112] Meanwhile, the hardening step may have a gas volumetric flow rate (GHSV) of 0.3 to 1.2 / hr or 0.5 to 0.8 / hr. Accordingly, the hardening and impurities (Cl, etc.) of the waste plastic pyrolysis product can be reduced without performing a separate post-treatment process, and by controlling the residence time (GHSV) of the pyrolysis gas, a pyrolysis oil with a high proportion of light hydrocarbons intended in the present disclosure and a refined hydrocarbon with a high proportion of light hydrocarbons can be produced.

[0113] The neutralizing agent filled in the above high-temperature filter may have a particle size of 400 to 900 μm, or may have a particle size of 500 to 800 μm. Under the operating conditions of the hardening step of the present disclosure, by filling the high-temperature filter with the neutralizing agent having the above particle size, not only can the residence time (GHSV) of the pyrolysis gas be controlled to achieve hardening of the oil, but also the generation of differential pressure in the high-temperature filter can be suppressed, thereby improving the process operation efficiency.

[0114] Meanwhile, the size of the above particles may refer to D50, and D50 refers to the particle diameter when the cumulative volume from the smallest particle size is 50% in particle size distribution measurement using the laser scattering method. Here, D50 can be measured by collecting a sample according to the KS A ISO 13320-1 standard for the manufactured carbonaceous material and using Malvern's Mastersizer3000 to measure the particle size distribution. Specifically, the bulk density can be measured after dispersion using ethanol as a solvent and, if necessary, an ultrasonic disperser.

[0115] According to one embodiment of the present disclosure, the high temperature filter may be filled with the beads and the neutralizing agent.

[0116] In the relevant technical field, it is common for a high-temperature filter to separate gas and char from the products of the pyrolysis step, but in the present disclosure, a high-temperature filter filled with at least one selected from the group consisting of beads and neutralizing agents was applied to remove impurities such as chlorine while hardening, and as described above, the operating conditions such as the temperature of the high-temperature filter and the particle size of the neutralizing agent were adjusted to a specific range.

[0117] The above hardening step may satisfy the following equations 1 and 2.

[0118] [Relationship 1]

[0119] 50 < (A2-A1) / A1(%)<100

[0120] [Relationship 2]

[0121] -80 < (B2-B1 / B1)(%)<-50

[0122] In the above relational expression 1, A1 is the total amount (weight %) of naphtha (boiling point ~150°C) and kerosene (boiling point 150 to 265°C) of the pyrolysis gas, A2 is the total amount (weight %) of naphtha (bp ~150°C) and kerosene (bp 150 to 265°C) of the pyrolysis oil, and in the above relational expression 2, B1 is the content (ppm) of chlorine of the pyrolysis gas, and B2 is the content (ppm) of chlorine of the pyrolysis oil.

[0123] The above relationship 1 and 2 may specifically be 60 < (A2-A1) / A1(%)<90, 65<(A2-A1) / A1(%)<85 or 70 < (A2-A1) / A1(%)<80, and -75 < (B2-B1 / B1)(%)<-55, -70<(B2-B1 / B1)(%)<-55 or -65 < (B2-B1 / B1)(%)<-55.

[0124] The above equations 1 and 2 numerically represent the degree of hardening and heavyening of waste plastic pyrolysis product by using a high-temperature filter filled with at least one selected from the group consisting of beads and neutralizing agents of the present disclosure. The present disclosure has a technical feature of producing pyrolysis oil having a high proportion of light hydrocarbons by controlling the oil composition and chlorine content of pyrolysis gas fed into the high-temperature filter and the organic / inorganic substances containing the chlorine.

[0125] The pyrolysis oil manufactured in the above hardening step may include 30 to 50 wt% of naphtha (bp ~150℃), 30 to 50 wt% of kerosene (bp 150 to 265℃), 10 to 30 wt% of LGO (Light gas oil, bp 265 to 380℃), and 0 to 10 wt% of UCO-2 / AR (bp 380℃~) based on the total weight, and specifically, 35 to 50 wt% of naphtha (bp ~150℃), 35 to 50 wt% of kerosene (bp 150 to 265℃), 10 to 30 wt% of LGO (Light gas oil, bp 265 to 380℃), and 0 to 8 wt% of UCO-2 / AR (bp 380℃~) or 35 to 45 wt% of naphtha (bp ~150℃), kerosene (bp The pyrolysis gas may contain 35 to 45 wt% of LGO (Light gas oil, bp 265 to 380°C), 10 to 20 wt% of LGO (Light gas oil, bp 265 to 380°C), and 0 to 6 wt% of UCO-2 / AR (bp 380°C~). In addition, the weight ratio of the light fraction (sum of naphtha and kerosene) to the heavy fraction (sum of LGO and UCO-2 / AR) may be 2.5 to 5, 2.5 to 4, or 3 to 3.8.

[0126] The pyrolysis oil produced in the above hardening step may have a total chlorine content of less than 100 ppm, 80 ppm or less, 60 ppm or less, 5 to 50 ppm, or 10 to 50 ppm, and an organic chlorine content of less than 90 ppm, 70 ppm or less, 50 ppm or less, 5 to 50 ppm, or 5 to 40 ppm, based on the total weight.

[0127] According to one embodiment of the present disclosure, the thermal decomposition step and the hardening step can satisfy the following relationship 3.

[0128] [Relationship 3]

[0129] 0.7 < T2 / T1<1.3

[0130] In the above relational expression 3, T1 and T2 are the temperatures at which the thermal decomposition step and the hardening step proceed, respectively.

[0131] When the pyrolysis step and the hardening step are carried out so that the above T2 / T1 value satisfies 0.7 or less, the temperature of the pyrolysis step may be relatively high, or the temperature of the hardening step may be relatively low. In this case, the ratio of condensation in the high-temperature filter and circulation to the pyrolysis reactor may increase, which may excessively lower the final boiling point of the pyrolysis oil. On the other hand, when the above steps are carried out so that the above T2 / T1 value satisfies 1.3 or more, the loss ratio in the gas phase may excessively increase, which may lower the yield of the pyrolysis oil.

[0132] Specifically, the T2 / T1 may be 0.7 to 1.2, 0.8 to 1.2, 0.8 to 1.1, 0.9 to 1.1, or, for example, 1. Accordingly, the above-described effect can be further improved.

[0133] The dehydration step according to one embodiment of the present disclosure may be a step of dehydrating by applying voltage to a first mixture containing pyrolysis oil, washing water, and a demulsifier.

[0134] The above pyrolysis oil contains moisture, which can cause problems such as deactivation of the hydrogenation catalyst and corrosion of the reactor due to moisture in the pyrolysis oil. Furthermore, since the moisture contains water-soluble impurities, it is necessary to remove the moisture. By performing the dehydration step, the moisture present in the form of an emulsion in the waste plastic pyrolysis oil can be easily removed.

[0135] The pyrolysis oil according to one embodiment of the present disclosure may be a hydrocarbon oil mixture produced by pyrolyzing waste plastic, wherein the waste plastic may include solid or liquid waste related to synthetic polymer compounds such as waste synthetic resin, waste synthetic fiber, waste synthetic rubber, and waste vinyl.

[0136] The hydrocarbon oil mixture according to one embodiment of the present disclosure may include impurities such as chlorine compounds, nitrogen compounds, oxygen compounds, metal compounds, char-derived particles, etc., in addition to hydrocarbon oil, and may include impurities in the form of compounds in which chlorine, nitrogen, oxygen, or metals are combined within the hydrocarbon, and may include hydrocarbons in the form of paraffins, olefins, naphthenes, or aromatics.

[0137] According to one embodiment of the present disclosure, the washing water may serve to increase the probability of contact between the water and the emulsion present in the pyrolysis oil. Furthermore, a basic compound may be added to the washing water to remove water-soluble acidic substances contained in the water. The basic compound may be sodium hydroxide (NaOH), but is not particularly limited thereto.

[0138] According to one embodiment of the present disclosure, the pyrolysis oil may be mixed in a larger volume than the washing water, and specifically, the first mixture may be a mixture of waste plastic pyrolysis oil and washing water in a volume ratio of 1:0.001 to 0.5, more specifically in a volume ratio of 1:0.005 to 0.4, and most specifically in a volume ratio of 1:0.01 to 0.3. When the above range is satisfied, washing can be sufficiently performed so that impurities in the pyrolysis oil can be significantly reduced, and the cost required for removing the mixed washing water can be minimized.

[0139] According to one embodiment of the present disclosure, the demulsifier may be one or a mixture of two or more selected from the group consisting of polyethylene glycol, tert-butanol, acetone, alkylnaphthalenesulfonate, alkylbenzenesulfonate, nonionic alkoxylated alkyl phenol resin, polyalkylene oxide, and polyoxyethylene sorbitan ester, but is not limited thereto.

[0140] According to one embodiment of the present disclosure, the first mixture may be a mixture of the pyrolysis oil and the demulsifier in a volume ratio of 1:0.000001 to 0.001, specifically in a volume ratio of 1:0.000002 to 0.0005, and more specifically in a volume ratio of 1:0.000003 to 0.0001. When the above range is satisfied, the emulsion can be decomposed while minimizing the impact on the quality of the pyrolysis oil.

[0141] The demulsifier according to one embodiment of the present disclosure may have a weight average molecular weight in the range of 200 to 2,000, specifically a weight average molecular weight in the range of 300 to 1,000, and more specifically a weight average molecular weight in the range of 400 to 800. When the above range is satisfied, mixing with the pyrolysis oil and washing water under conditions in which the dehydration process is performed is facilitated, thereby increasing the decomposition efficiency of the water emulsion.

[0142] The emulsion-type moisture contained in the first mixture comprising the above-mentioned pyrolysis oil, washing water, and demulsifier is still difficult to remove because it is stable. Therefore, the removal of moisture can be facilitated by applying voltage to the first mixture.

[0143] According to one embodiment of the present disclosure, the voltage may be applied as an alternating current or a combination of an alternating current and a direct current. Some impurity particles contained in the pyrolysis oil exhibit polarity, and when a direct current voltage is applied, polarized impurity particles may accumulate on a specific electrode, and when the process is performed for a long period of time, a phenomenon in which impurities are fixed on the electrode may occur. However, when an alternating current voltage is applied, the polarity of the electrode changes periodically, so the fixation of impurity particles can be prevented. In addition, according to one embodiment of the present disclosure, the frequency of the alternating current may be a single frequency or a combination of two or more frequencies. As a specific example, in the case of a single frequency, an alternating current having a frequency of 60 Hz may be applied, and in the case of a combination of two or more frequencies, an alternating current having frequencies of 50 Hz and 60 Hz may be applied alternately, but is not limited thereto.

[0144] According to one embodiment of the present disclosure, the voltage may be applied via a vertical electrode. If impurity particles accumulate on the electrode during the process of preparing the mixture or applying the voltage, the impurity particles may become fixed to the electrode after a long period of time if they are not artificially cleaned. However, by using a vertical electrode, the impurity particles fall to the bottom of the reactor by gravity without accumulating on the electrode without performing a separate cleaning process, so the fixation of the impurity particles can be prevented in advance.

[0145] The magnitude of the voltage according to one embodiment of the present disclosure may be, but is not limited to, 0.1 to 50 kV, specifically 1 to 30 kV, and more specifically 5 to 20 kV.

[0146] The dehydration according to one embodiment of the present disclosure can be performed by any method known in the art. As a non-limiting example, water can be removed by sieving the separated water layer after applying voltage. Water can also be removed in a gas-liquid separator.

[0147] Metal impurities in the pyrolysis oil stabilize the emulsion, hindering oil-water separation and facilitating the formation of a stable emulsion layer, commonly referred to as a rag layer. This rag layer can form between the demineralized oil layer above the first mixture and the water layer below, and can gradually thicken during the continuous dehydration process. An excessively thick rag layer can be discharged to the hydrotreating stage equipment along with the demineralized oil. This reduces the demineralization effect of the demineralized oil, thereby reducing the efficiency of the process. Furthermore, the rag layer can be discharged together with the water, causing problems in the wastewater treatment process. Therefore, it is desirable to remove the rag layer formed between the demineralized oil layer and the water layer.

[0148] Thus, the method for producing purified hydrocarbons from waste plastic according to one embodiment of the present disclosure may further include a step of removing a rag layer from the first mixture after applying voltage in the dehydration step. The removal of the rag layer may be performed by measuring a change in the density of the mixture through a density meter in the dehydrator (22) to determine the formation location and thickness of the rag layer, and then through a pipe that penetrates the wall of the dehydrator and is connected to the outside, but is not necessarily limited thereto.

[0149] According to one embodiment of the present disclosure, the dehydration step may be to dehydrate the first mixture, and then further dehydrate the dehydrated first mixture by coagulating moisture.

[0150] According to one embodiment of the present disclosure, the additional dehydration may be performed by supplying the dehydrated first mixture to a coalescer. Specifically, the residual moisture contained in the dehydrated first mixture may be removed by being coagulated by a collection filter within the coalescer, but this is merely a specific example and is not necessarily limited thereto. Through the additional dehydration, the moisture content in the waste plastic pyrolysis oil is further reduced, thereby preventing the deactivation of the catalyst due to moisture, and improving the stability of the process and the quality of the refined pyrolysis oil.

[0151] According to one embodiment of the present disclosure, the ratio of the moisture content of the pyrolysis oil to the moisture content of the dehydrated first mixture may be 1:0.0001 to 0.9, specifically 1:0.0005 to 0.5, and more specifically 1:0.001 to 0.1. When the above range is satisfied, the risk of trouble occurring in subsequent processes including hydrogenation treatment is significantly reduced, and high-quality refined pyrolysis oil satisfying the specifications as a raw material for blending or refining and petrochemical processes can be produced, but is not necessarily limited thereto.

[0152] The dehydration step according to one embodiment of the present disclosure may be performed at a pressure of 50 bar or less. When performed at a pressure of 50 bar or less, moisture within the pyrolysis oil can be easily removed, and process stability can be ensured. Specifically, the dehydration step may be performed at a pressure of 30 bar or less, more specifically, at a pressure of 20 bar or less, and, without limitation, at a pressure of 5 bar or more.

[0153] The dehydration step according to one embodiment of the present disclosure may be performed at a temperature of 20°C to 300°C. When the above range is satisfied, emulsion decomposition and moisture coagulation may occur smoothly, thereby improving dehydration efficiency. Specifically, the dehydration step may be performed at a temperature of 50°C to 250°C, and more specifically, 80°C to 200°C.

[0154] To improve the dehydration efficiency in the dehydration step according to one embodiment of the present disclosure, one or more additional processes selected from the group consisting of centrifugation and distillation may be performed before and / or after dehydration. The aforementioned additional processes may be performed using methods known in the art and are not particularly limited.

[0155] The hydrogenation treatment step according to one embodiment of the present disclosure may be a step of hydrogenating a first mixture dehydrated in the dehydration step and a second mixture mixed with a sulfur source to produce refined pyrolysis oil from which impurities have been removed.

[0156] The second mixture according to one embodiment of the present disclosure may have a chlorine (Cl) concentration of 10 ppm or more, specifically 100 ppm or more, more specifically 200 ppm or more, and an upper limit may be, but is not limited to, 3000 ppm or less.

[0157] The second mixture according to one embodiment of the present disclosure may have a weight ratio of nitrogen to chlorine of 1:0.1 to 10, specifically 1:0.5 to 5, and more specifically 1:1 to 2; however, the weight ratio is only a specific example of what may be included in the pyrolysis oil, and the composition of the pyrolysis oil is not limited thereto.

[0158] Hydrogenation treatment according to one embodiment of the present disclosure is performed in which the ratio of hydrogen to the second mixture is 100 Nm 3 / Sm 3 Up to 5000 Nm 3 / Sm 3 , specifically 500 Nm 3 / Sm 3 Up to 3000 Nm 3 / Sm 3 , more specifically 1000 Nm 3 / Sm 3 Up to 1500 Nm 3 / Sm 3This can be performed under these conditions. If this is satisfied, impurities can be effectively removed, the activity of the hydrogenation catalyst can be maintained at a high level for a long period of time, and process efficiency can be improved.

[0159] The above sulfur source refers to a sulfur source that can continuously supply sulfur components during the refining process.

[0160] The above hydrogenation treatment step can suppress deactivation of a molybdenum-based hydrogenation catalyst due to lack of sulfur source and high-temperature operation during the purification process and maintain catalytic activity by producing a second mixture containing the sulfur source.

[0161] According to one embodiment of the present disclosure, the sulfur source may include a sulfur-containing oil fraction. The sulfur-containing oil fraction refers to an oil fraction composed of sulfur-containing hydrocarbons obtained from crude oil as a raw material. There is no particular limitation on the sulfur-containing oil fraction, and examples thereof include light gas oil, straight-run naphtha, vacuum naphtha, pyrolysis naphtha, straight-run kerosene, vacuum kerosene, pyrolysis kerosene, straight-run gas oil, vacuum gas oil, pyrolysis gas oil, sulfur-containing waste tire oil, and the like, or any mixture thereof.

[0162] According to one embodiment of the present disclosure, by including waste tire oil as the sulfur-containing oil, the high sulfur content contained in waste tires is converted into oil together with hydrocarbons, thereby advantageously functioning as a sulfur source for waste plastic pyrolysis oil. Furthermore, by utilizing waste tire oil as a sulfur source for waste plastic pyrolysis oil, it is advantageous in terms of reducing the environmental burden resulting from recycling of waste tires and maintaining catalytic activity for a long period of time.

[0163] Specifically, the sulfur-containing oil fraction may be light gas oil (LGO) having a specific gravity of 0.7 to 1. When this is used, it can be uniformly mixed with the dehydrated first mixture, and has the advantage of high hydrogenation efficiency. Specifically, the specific gravity may be 0.75 to 0.95, and more specifically, may be 0.8 to 0.9. The sulfur-containing oil fraction may contain sulfur in an amount of 100 ppm or more. If the sulfur component is contained in an amount of 100 ppm or less, the content of the supplied sulfur component may be small, and thus the effect of preventing the deactivation of the molybdenum-based hydrogenation catalyst may be minimal. Specifically, the sulfur component may be contained in an amount of 800 ppm or more, more specifically, 8,000 ppm or more, and, without limitation, 200,000 ppm or less.

[0164] The second mixture according to one embodiment of the present disclosure may contain sulfur in an amount of 100 ppm or more. As in the case of the sulfur-containing oil, if the sulfur component in the second mixture is contained in an amount of 100 ppm or less, the content of the supplied sulfur component may be small, and thus the effect of preventing the deactivation of the molybdenum-based hydrogenation catalyst may be minimal. Specifically, the sulfur component may be contained in an amount of 800 ppm or more, more specifically, 8,000 ppm or more, and, without limitation, 200,000 ppm or less.

[0165] According to one embodiment of the present disclosure, the sulfur-containing oil may be included in an amount of less than 0.5 parts by weight based on 100 parts by weight of the first mixture dehydrated in the dehydration step. Specifically, the sulfur-containing oil may be included in an amount of less than 0.1 parts by weight, more specifically, less than 0.05 parts by weight, and, without limitation, more than 0.01 parts by weight. Since the sulfur-containing oil is included in an amount of less than 0.5 parts by weight, the concentration of chlorine (Cl) or nitrogen (N) included in the waste plastic pyrolysis oil is diluted, thereby controlling the rate of ammonium salt (NH4Cl) production and improving process stability.

[0166] According to one embodiment of the present disclosure, the sulfur source may include one or more sulfur-containing organic compounds selected from disulfide compounds, sulfide compounds, sulfonate compounds, and sulfate compounds. Specifically, it may include one or a mixture of two or more selected from dimethyldisulfide, dimethylsulfide, polysulfide, dimethyl sulfoxide (DMSO), methyl methanesulfonate, ethyl methanesulfonate, propyl methanesulfonate, propenyl propenesulfonate, propenyl cyanoethansulfonate, ethylene sulfate, bicyclo glyoxal sulfate, and methyl sulfate, which are presented as examples only and the present disclosure is not limited thereto.

[0167] According to one embodiment of the present disclosure, the sulfur-containing organic compound may be included in an amount of 0.01 to 0.1 parts by weight based on 100 parts by weight of the first mixture dehydrated in the dehydration step. Specifically, it may be included in an amount of 0.02 to 0.08 parts by weight, and more specifically, it may be included in an amount of 0.03 to 0.06 parts by weight. If it is included in an amount of less than 0.01 parts by weight, the content of the supplied sulfur component may be low, and thus the effect of preventing deactivation of the molybdenum-based hydrogenation catalyst may be minimal.

[0168] The above hydrogenation treatment refers to a hydrogenation reaction that occurs in the presence of a molybdenum-based hydrogenation catalyst by adding a reaction gas containing hydrogen gas (H2) to a first mixture dehydrated in the dehydration step and a second mixture containing a sulfur source. Specifically, the hydrogenation treatment may refer to a conventionally known hydrogenation treatment including a hydrodesulfurization reaction, a hydrocracking reaction, a hydrodechlorination reaction, a hydrodenitrogenation reaction, a hydrodeoxygenation reaction, and a hydrodemetallation reaction. Through the hydrogenation treatment, impurities including chlorine (Cl), nitrogen (N), and oxygen (O) and a portion of olefins are removed, and other metal impurities can also be removed, and by-products containing the above impurities are generated.

[0169] The above by-product is generated by the reaction of hydrogen gas (H2) with impurities such as chlorine (Cl), nitrogen (N), sulfur (S) or oxygen (O) contained in waste plastic pyrolysis oil, and specifically may include hydrogen sulfide gas (H2S), hydrogen chloride (HCl), ammonia (NH3) or water vapor (H2O), and in addition, unreacted hydrogen gas (H2), trace amounts of methane (CH4), ethane (C2H6), propane (C3H8) or butane (C4H 10 ) may be included.

[0170] The molybdenum-based hydrogenation catalyst according to one embodiment of the present disclosure may be a catalyst in which a molybdenum-based metal or a metal including one or more selected from nickel, cobalt, and tungsten and the molybdenum-based metal are supported on a support. The molybdenum-based hydrogenation catalyst has high catalytic activity during hydrogenation treatment, and may be used alone or, if necessary, in the form of a binary system catalyst combined with a metal such as nickel, cobalt, or tungsten.

[0171] According to one embodiment of the present disclosure, the support may be, but is not limited to, alumina, silica, silica-alumina, titanium oxide, molecular sieve, zirconia, aluminum phosphate, carbon, niobia, or a mixture thereof.

[0172] The molybdenum-based hydrogenation catalyst according to one embodiment of the present disclosure may include a molybdenum-based sulfide hydrogenation catalyst. For example, the catalyst may include molybdenum sulfide (MoS) or molybdenum disulfide (MoS2), but is not limited thereto, and may include any known molybdenum-based sulfide hydrogenation catalyst.

[0173] According to one embodiment of the present disclosure, the reaction gas may further include hydrogen sulfide gas (H2S). The hydrogen sulfide gas (H2S) contained in the reaction gas may act as a sulfur source and regenerate the activity of a molybdenum-based hydrogenation catalyst that has been deactivated during the purification process, such as a sulfur source mixed with waste plastic pyrolysis oil.

[0174] The hydrogenation process according to one embodiment of the present disclosure may be performed at a pressure of 150 bar or less. Specifically, it may be performed at a pressure of 120 bar or less, more specifically, 100 bar or less, and, but not limited to, a pressure of 50 bar or more. When the hydrogenation process is performed under a pressure condition exceeding 150 bar, since an excessive amount of ammonia and hydrogen chloride are generated during the hydrogenation process, the ammonium salt formation temperature may rise, which may easily cause a differential pressure within the process, such as a reactor, and may significantly deteriorate the process stability. Although the increase in the ammonium salt formation temperature may be partially suppressed even under a pressure condition exceeding 150 bar by controlling the nitrogen and chlorine contents in the waste plastic pyrolysis oil, in this case, the waste plastic pyrolysis oil that is the target of the purification process according to the present disclosure may be extremely limited, making it unsuitable.

[0175] The hydrogenation process according to one embodiment of the present disclosure may be performed at a temperature of 150°C to 500°C. When the above range is satisfied, the hydrogenation process efficiency may be improved. Specifically, the process may be performed at a temperature of 200°C to 400°C.

[0176] The hydrogenation treatment according to one embodiment of the present disclosure may be performed in multiple stages, and as a specific example, may be performed in two stages. When the hydrogenation treatment is performed in two stages, the first stage may be performed at a lower temperature than the second stage. In this case, the first stage may be performed at a temperature of 150°C to 300°C, specifically 200°C to 250°C, and the second stage may be performed at a temperature of 300°C to 500°C, specifically 350°C to 400°C, but is not limited thereto.

[0177] The hydrogenation treatment according to one embodiment of the present disclosure is performed for 0.1 to 5 h -1It can be performed at the fluid space velocity (LHSV). When the LHSV satisfies the above range, it has the effect of more stably obtaining refined pyrolysis oil with impurities such as chlorine, nitrogen, or metals removed. Specifically, it is 0.3 to 3 h -1 , more specifically 0.5 to 1.5h -1 can be performed in the LHSV.

[0178] A method for producing refined hydrocarbons from waste plastics according to one embodiment of the present disclosure may further include, after the hydrogenation step, a step of separating a stream containing refined pyrolysis oil from which the impurities have been removed and then washing the stream.

[0179] The stream containing the purified pyrolysis oil from which the impurities have been removed according to one embodiment of the present disclosure may include hydrogen chloride, ammonia, and unreacted hydrogen gas, as well as the purified pyrolysis oil from which the impurities have been removed discharged from the rear end of the reactor where the hydrogenation treatment step is performed.

[0180] According to one embodiment of the present disclosure, ammonia and hydrogen chloride generated by hydrogenation can be removed from a stream containing purified pyrolysis oil from which impurities have been removed through the gas-liquid separation, and unreacted hydrogen gas can be recovered.

[0181] The gas-liquid separation according to one embodiment of the present disclosure can be performed using a separator by a method known in the art, and is not particularly limited.

[0182] According to one embodiment of the present disclosure, the gas-liquid separation may be performed 2 to 4 times, specifically 3 to 4 times, and more specifically 4 times. When the above range is satisfied, since the refined pyrolysis oil contains trace amounts of NH3 and hydrogen chloride, the production of ammonium salts can be minimized even under low-temperature conditions for oil-water separation. In addition, oil refining and petrochemical processes using the refined pyrolysis oil as a raw material can be stably performed without adding a separate salt remover to the refined pyrolysis oil in the future.

[0183] The gas stream generated as a result of the gas-liquid separation according to one embodiment of the present disclosure may include off-gas containing light hydrocarbons, hydrogen sulfide, ammonia, or hydrogen chloride, and unreacted hydrogen gas. The off-gas and unreacted hydrogen gas are separated according to a method known in the art, and the unreacted hydrogen gas is recycled within the process, and the off-gas is processed through the steps described below and can be used as fuel or discharged into the atmosphere.

[0184] According to one embodiment of the present disclosure, the washing process can dissolve and remove salts contained in the gas stream, or can dissolve gases capable of forming salts to inhibit salt formation. The washing process can be performed using methods known in the art, and is not particularly limited.

[0185] According to one embodiment of the present disclosure, the washing process may be performed two to four times, specifically two to three times. When the above range is satisfied, the salt removal and salt formation inhibition effects are sufficiently exerted, thereby obtaining high-quality refined pyrolysis oil and ensuring process stability.

[0186] A method for producing refined hydrocarbons from waste plastics according to one embodiment of the present disclosure may further include, after the step of separating a stream containing refined pyrolysis oil from which impurities have been removed and then washing it, a step of combusting the separated off-gas; and a step of treating uncombusted off-gas.

[0187] According to one embodiment of the present disclosure, the waste gas may include C1-C4 light hydrocarbons, hydrogen sulfide (H2S), ammonia (NH3), etc. Therefore, in order to use the waste gas as fuel, it is necessary to remove hydrogen sulfide (H2S), ammonia (NH3), etc. by burning the waste gas. The exhaust gas containing sulfur dioxide (SO2), nitrogen dioxide (NO2), etc. generated by combustion of the waste gas may be discharged into the atmosphere after performing caustic scrubbing to meet emission standards.

[0188] Additionally, after the step of burning the waste gas, the unburned waste gas can be discharged as waste water after being treated by sour water stripping, adsorption, biological treatment, oxidation, amine scrubbing, or caustic scrubbing.

[0189] According to one embodiment of the present disclosure, the method for producing purified hydrocarbons from waste plastics of the present disclosure may include a second hydrogenation treatment step. By performing the second hydrogenation treatment step, the content of impurities contained in the purified pyrolysis oil can be significantly reduced.

[0190] The contents described in the above hydrogenation treatment can be equally applied to the second hydrogenation treatment to the overlapping extent.

[0191] The second hydrogenation treatment according to one embodiment of the present disclosure means a hydrogenation reaction that occurs by adding a reaction gas containing hydrogen gas (H2) to the refined pyrolysis oil under a molybdenum-based hydrogenation catalyst.

[0192] The molybdenum-based hydrogenation catalyst according to one embodiment of the present disclosure may be a catalyst in which a molybdenum-based metal or a metal including one or more selected from nickel, cobalt, and tungsten and the molybdenum-based metal are supported on a support. The molybdenum-based hydrogenation catalyst has high catalytic activity during the second hydrogenation treatment, and may be used alone or, if necessary, in the form of a binary system catalyst combined with a metal such as nickel, cobalt, or tungsten.

[0193] According to one embodiment of the present disclosure, the support may be, but is not limited to, alumina, silica, silica-alumina, titanium oxide, molecular sieve, zirconia, aluminum phosphate, carbon, niobia, or a mixture thereof.

[0194] The molybdenum-based hydrogenation catalyst according to one embodiment of the present disclosure may include a molybdenum-based sulfide hydrogenation catalyst. For example, the catalyst may include molybdenum sulfide (MoS) or molybdenum disulfide (MoS2), but is not limited thereto, and may include any known molybdenum-based sulfide hydrogenation catalyst.

[0195] According to one embodiment of the present disclosure, the reaction gas may further include hydrogen sulfide gas (H2S). The hydrogen sulfide gas (H2S) contained in the reaction gas may act as a sulfur source and regenerate the activity of a molybdenum-based hydrogenation catalyst that has been deactivated during the purification process, such as a sulfur source mixed with waste plastic pyrolysis oil.

[0196] The second hydrogenation treatment according to one embodiment of the present disclosure may be performed at a pressure of 200 bar or less. Specifically, it may be performed at a pressure of 150 bar or less, more specifically, 120 bar or less, and, without limitation, it may be performed at a pressure of 10 bar or more, but is not limited thereto.

[0197] The second hydrogenation treatment according to one embodiment of the present disclosure may be performed at a temperature of 150°C to 500°C. Specifically, it may be performed at a temperature of 200°C to 400°C, but is not limited thereto.

[0198] The second hydrogenation treatment according to one embodiment of the present disclosure is performed for 0.1 to 5 h -1 can be performed at a fluid space velocity (LHSV) of 0.3 to 3 h specifically. -1 , more specifically 0.5 to 1.5 h -1 It can be performed in LHSV, but is not necessarily limited thereto.

[0199] In one embodiment of the present disclosure, the refined pyrolysis oil may be mixed with petroleum hydrocarbons and subjected to secondary hydrogenation treatment to form a mixed oil.

[0200] The second hydrogenation treatment step according to one embodiment of the present disclosure may be hydrogenating a refined oil fraction separated by distillation from refined pyrolysis oil from which impurities have been removed. The refined oil fraction according to one embodiment of the present disclosure may be at least one selected from the group consisting of naphtha, kerosene, light gas oil, heavy gas oil (HGO), vacuum gas oil (VGO), atmospheric residue, and vacuum residue, but is not limited thereto.

[0201] The second hydrogenation treatment step according to one embodiment of the present disclosure may be a second hydrogenation treatment of a mixed oil mixture comprising the refined pyrolysis oil from which impurities have been removed and a petroleum hydrocarbon. Furthermore, it goes without saying that a mixed oil mixture comprising the refined pyrolysis oil and a petroleum hydrocarbon may also be subjected to a second hydrogenation treatment.

[0202] The above petroleum hydrocarbon is a general term for a mixture of naturally occurring hydrocarbons or a compound separated from the mixture, and may be at least one selected from the group consisting of crude oil and hydrocarbons derived from crude oil, but is not limited thereto.

[0203] According to one embodiment of the present disclosure, the mixed oil may contain the refined pyrolysis oil in an amount of 5 wt% or more, 10 wt% or more, 20 wt% or more, 40 wt% or more, or 50 wt% or more, based on the total weight of the mixed oil, and may include, but is not limited to, an upper limit of 95 wt% or less or 90 wt% or less. Although the present disclosure is not necessarily limited to the above range, generally, the lower the impurity content in the pyrolysis oil, the higher the proportion of pyrolysis oil that can be included in the mixed oil.

[0204] The method for producing refined hydrocarbon from waste plastic according to one embodiment of the present disclosure may further include a distillation step of distilling the refined pyrolysis oil after the hydrogenation treatment step.

[0205] According to one embodiment of the present disclosure, the method for producing refined hydrocarbons from waste plastics may be such that hydrocarbons derived from the refined pyrolysis oil separated in the distillation step and petroleum hydrocarbons are mixed and subjected to secondary hydrogenation treatment to form a mixed oil.

[0206] According to one embodiment of the present disclosure, in the distillation step, the refined pyrolysis oil may be distilled to obtain refined hydrocarbons such as naphtha when the boiling point is in the range of 150°C or lower, kerosene when the boiling point is in the range of 150 to 265°C, LGO (Light gas oil) when the boiling point is in the range of 265 to 340°C, and VGO (Vacuum gas oil) when the boiling point is in the range of 340°C or higher. In addition, in the distillation step, the refined pyrolysis oil may be distilled to obtain light oil having a boiling point of 230°C to 380°C.

[0207] According to one embodiment of the present disclosure, the method for producing purified hydrocarbons from waste plastics of the present disclosure may further include, but is not limited to, a distillation step, and may include, but is not limited to, steps applicable in an oil refining process or a petrochemical process.

[0208] According to one embodiment of the present disclosure, the distillation may be performed in at least one process selected from the group consisting of a crude distillation unit (CDU) and a vacuum distillation unit (VDU).

[0209] Additionally, the present disclosure provides a system for producing purified hydrocarbons from waste plastic.

[0210] The description of the method for producing purified hydrocarbons from waste plastics can be equally applied to the description of the system for producing purified hydrocarbons from waste plastics, to the extent that there is overlap.

[0211] The present disclosure provides a system for producing refined hydrocarbons from waste plastic, comprising: a pretreatment device for pretreating waste plastic; a pyrolysis reactor for producing pyrolysis gas by introducing waste plastic pretreated in the pretreatment device; a hot filter for producing pyrolysis oil by introducing the pyrolysis gas; a connecting pipe for connecting the hot filter and the pyrolysis reactor so that liquid condensed in the hot filter is reintroduced into the pyrolysis reactor; a dehydration device for dehydrating a first mixture obtained by mixing the produced pyrolysis oil with washing water and a demulsifier by applying voltage; a hydrogenation device for hydrogenating a second mixture obtained by mixing the dehydrated first mixture with a sulfur source to produce refined pyrolysis oil from which impurities have been removed; and a second hydrogenation device for hydrogenating the refined pyrolysis oil.

[0212] The manufacturing system of the present disclosure can produce high value-added pyrolysis oil with a high proportion of light hydrocarbons from waste plastic containing a large amount of impurities, and can produce refined hydrocarbons with a high proportion of light hydrocarbons from the same. Furthermore, the manufacturing system of the present disclosure can improve the yield of pyrolysis oil obtained from waste plastic.

[0213] Referring to Fig. 2, the feedstock (11) may be injected into the feedstock injection unit (12) and screw mixing may be performed. After the crushed waste plastic and additives are injected into the pretreatment reactor (13), pretreatment may be performed. The pretreated waste plastic may be injected into the pyrolysis reactor (14) and pyrolysis may be performed to generate pyrolysis gas. The generated pyrolysis gas may be injected into the high-temperature filter (15) and then hardened. Thereafter, the hardened pyrolysis gas may be introduced into the condenser (16), and pyrolysis oil may be obtained from the pyrolysis oil recovery unit (18). The liquid condensed in the high-temperature filter (15) may be reintroduced into the pyrolysis reactor (14) through the connecting pipe (19).

[0214] Referring to Fig. 4, the pyrolysis oil obtained from the feed tank (21) can be fed into a dehydrator (22) and stirred to produce a first mixture. The first mixture can be separated into oil and water by applying an alternating voltage through a vertical electrode. Thereafter, the separated water layer can be removed to perform dehydration. The first mixture dehydrated in the dehydrator (22) can be mixed with dimethyl disulfide to produce a second mixture, and then the second mixture can be hydrogenated in a hydrogenation treatment device (23). Thereafter, the hydrogenated pyrolysis oil can be introduced into a first separator (24-1) to separate liquid and gas from the hydrogenated pyrolysis oil. The liquid separated in the first separator (24-1) can be introduced into a third separator (24-3) and then introduced into a fractionator (25). The gas separated in the first separator (24-1) can be introduced into the second separator (24-2). Impurities including NH3 and HCl contained in the gas separated in the first separator (24-1) can be removed together with water in the second separator (24-2). After performing additional separation in the fourth separator (24-4), the oil fraction recovered from the gas can be introduced into the fractionator (25) to produce refined pyrolysis oil from which impurities have been removed. The refined pyrolysis oil fraction separated by distillation in the fractionator (25) and the mixed oil obtained by mixing at least one selected from the group consisting of naphtha, kerosene, LGO, and residual oil can be introduced into the second hydrogenation treatment device to perform the second hydrogenation treatment. The above second hydrogenation treatment device may be, but is not limited to, a naphtha hydrogenation treatment device (26-1), a kerosene / gas oil hydrogenation treatment device (26-2), or a residual oil hydrogenation treatment device (26-3).

[0215] According to one embodiment of the present disclosure, the high-temperature filter may be filled with beads. When the high-temperature filter is filled with beads, the inertness and heat transfer effects within the high-temperature filter are maximized, allowing for the production of pyrolysis oil with a high proportion of light hydrocarbons. Furthermore, the yield of the pyrolysis oil may be improved.

[0216] According to one embodiment of the present disclosure, the bead may include at least one selected from the group consisting of silica (SiO2) and aluminum oxide (Al2O3).

[0217] According to one embodiment of the present disclosure, the manufacturing system may be provided with at least two heaters on the outside of the high-temperature filter. In addition, the manufacturing system may be provided with at least three heaters on the outside of the high-temperature filter. When at least two heaters are provided on the outside of the high-temperature filter, it is easy to form a temperature gradient in the high-temperature filter, and the temperatures at the top, middle, and bottom can be flexibly adjusted depending on the operating conditions of the high-temperature filter, thereby enabling flexible process operation.

[0218] The dehydration device according to one embodiment of the present disclosure may be equipped with vertical electrodes. The number of vertical electrodes equipped in the dehydration device according to one embodiment of the present disclosure may be at least 2 or more, specifically 4 or more, and more specifically 6 or more, and may be up to 20, but is not necessarily limited thereto.

[0219] The dehydration device according to one embodiment of the present disclosure may include a coalescer. The coalescer is a device that collects fine droplets to form large droplets, and any device commonly used in industry may be used, without any particular limitations.

[0220] According to one embodiment of the present disclosure, the first mixture dehydrated in the dehydration device may be introduced into the coagulator to produce a further dehydrated first mixture. When using a dehydration device including the coagulator, the further dehydrated first mixture is of course introduced into the hydrogenation reactor together with hydrogen gas.

[0221] The system for producing refined hydrocarbons from waste plastic according to one embodiment of the present disclosure may further include a separator for gas-liquid separation of refined pyrolysis oil from which impurities have been removed, generated from the hydrogenation treatment device.

[0222] According to one embodiment of the present disclosure, the number of separators may be 2 to 4, specifically 3 to 4, and more specifically 4. When the above range is satisfied, since the refined pyrolysis oil contains trace amounts of NH3 and hydrogen chloride, the generation of ammonium salts can be minimized even under low-temperature conditions for oil-water separation. In addition, oil refining and petrochemical processes using the refined pyrolysis oil as a raw material can be stably performed without adding a separate salt remover to the refined pyrolysis oil in the future.

[0223] A system for producing purified hydrocarbons from waste plastic according to one embodiment of the present disclosure may further include a recycle gas compressor for recovering unreacted hydrogen gas from a gas stream separated from the separator and feeding it into a hydrogenation treatment device.

[0224]

[0225] Hereinafter, embodiments of the present disclosure will be further described with reference to specific experimental examples. The examples and comparative examples included in the experimental examples are merely illustrative of the present disclosure and do not limit the scope of the appended claims. It will be apparent to those skilled in the art that various changes and modifications to the examples are possible within the scope and technical idea of ​​the present disclosure, and it is also natural that such changes and modifications fall within the scope of the appended claims.

[0226] In this specification, “pyrolysis oil yield” means the weight ratio of oil to the total weight of oil, aqueous by-products, pyrolysis residue (char), and by-product gas among the products of the pyrolysis step.

[0227] [Example 1]

[0228] The waste plastics from daily life for use as feed contained 78.8 wt% PE, 11.6 wt% PP, 3.1 wt% PVC, 2.4 wt% PET, 2.1 wt% nylon, and 2.0 wt% PU.

[0229] The above-mentioned 1020g of waste plastic feed from the living world was fed into the feed inlet and screw mixed. 200g / hr of crushed waste plastic and 10g / hr of CaO were fed into the auger reactor, and pretreatment was performed under the conditions of a screw speed of 10 rpm, a nitrogen flow rate of 3cc / min, a temperature of 300°C, and a residence time of 1 hr.

[0230] Pretreated waste plastic was fed into a rotary kiln batch pyrolysis reactor, and pyrolysis was performed under the conditions of a rotary kiln rotation speed of 4 rpm and 430°C to produce pyrolysis gas.

[0231] The produced pyrolysis gas was fed into a 1.3 L hot filter not filled with glass beads, hardened, and then pyrolysis oil was obtained from the recovery unit. The liquid condensed in the hot filter was reintroduced into the pyrolysis reactor. The pyrolysis oil yield is shown in Table 1.

[0232] Under conditions of 150°C and 10 bar, the obtained pyrolysis oil, washing water, and polyethylene glycol having a weight average molecular weight of 500 were introduced into a dehydrator in a volume ratio of 1:0.25:0.0001 and stirred to prepare a first mixture. The first mixture was subjected to oil-water separation by applying an AC voltage of 15 kV through a vertical electrode, and then the water layer was removed to perform dehydration.

[0233] At this time, the dehydrator can process high concentration impurities such as moisture content of about 5,000 ppm or more, nitrogen (N) of 500 ppm or more, chlorine (Cl) of 200 ppm or more, and olefin of 20% by volume or more.

[0234] A second mixture was prepared by mixing 0.04 parts by weight of dimethyl disulfide with 100 parts by weight of the first mixture dehydrated in the above dehydrator, and then hydrogenation was performed under conditions of 300°C and 70 bar to produce refined pyrolysis oil from which impurities were removed.

[0235] The results of GC-Simdis analysis (HT 750) performed to confirm the molecular weight distribution of the above refined pyrolysis oil are shown in Table 2, and the results of measurement related to the content of impurities in the refined pyrolysis oil are shown in Tables 3 and 4.

[0236] The above refined pyrolysis oil and crude oil derived from crude oil with a boiling point of 230°C to 380°C were mixed in a weight ratio of 9:1 and subjected to secondary hydrogenation treatment under the conditions of 350°C and 60 bar using a molybdenum disulfide (MoS2) catalyst to obtain refined hydrocarbons.

[0237] [Example 2]

[0238] The same procedure as Example 1 was followed, except that 3 mm diameter glass beads were filled into a 1.3 L high-temperature filter at 88 vol% of the internal volume of the high-temperature filter, and the upper temperature, middle temperature, and lower temperature of the high-temperature filter were maintained at 430°C.

[0239] [Example 3]

[0240] The same procedure as Example 1 was followed, except that 3 mm diameter glass beads were filled into a 1.3 L high-temperature filter at 88 vol% of the internal volume of the high-temperature filter, and the upper temperature of the high-temperature filter was maintained at 430°C, and the middle and lower temperatures were maintained at 500°C.

[0241] [Example 4]

[0242] The same procedure as Example 1 was performed, except that 3 mm diameter glass beads were filled in a 1.3 L high temperature filter at 88 vol% of the internal volume of the high temperature filter, and the upper temperature of the high temperature filter was maintained at 430°C, the middle temperature at 450°C, and the lower temperature at 500°C.

[0243] [Examples 5 and 6]

[0244] In Example 1, waste plastic pyrolysis oil, washing water, and polyethylene glycol were introduced into a dehydrator in the volume ratios shown in Table 1 below, and the same conditions as in Example 1 were performed to produce purified pyrolysis oil from which impurities were removed.

[0245] [Example 7]

[0246] In Example 1, except that a direct current voltage was applied through a horizontal electrode, the same conditions as in Example 1 were performed to produce purified pyrolysis oil from which impurities were removed.

[0247] [Example 8]

[0248] In Example 1, dehydration of the first mixture was performed under the same conditions as in Example 1, except that it was performed at a temperature of 120°C, thereby producing purified pyrolysis oil from which impurities were removed.

[0249] [Example 9]

[0250] In Example 8, waste plastic pyrolysis oil and polyethylene glycol were introduced in a volume ratio of 1:0.00001, and the same conditions as Example 1 were performed except that hydrogenation treatment was performed under a pressure of 180 bar, thereby producing purified pyrolysis oil from which impurities were removed.

[0251] [Example 10]

[0252] In Example 1, the same conditions as in Example 1 were performed except that the first mixture was dehydrated and then further dehydrated through a coagulant to produce purified pyrolysis oil from which impurities were removed.

[0253] [Example 11]

[0254] The same procedure as Example 1 was followed, except that a mixed oil was used in which the refined pyrolysis oil having a boiling point of 230°C to 380°C derived from the refined pyrolysis oil separated by distillation and the crude oil having a boiling point of 230°C to 380°C derived from the crude oil were mixed in a weight ratio of 9:1.

[0255] [Comparative Example 1]

[0256] The same procedure as Example 1 was followed, except that the liquid condensed in the high-temperature filter was not reintroduced into the thermal decomposition reactor.

[0257] [Comparative Example 2]

[0258] A purified pyrolysis oil with impurities removed was produced under the same conditions as Example 1, except that washing water was not added.

[0259] [Comparative Example 3]

[0260] A purified pyrolysis oil with impurities removed was produced under the same conditions as Example 1, except that polyethylene glycol was not added.

[0261] [Comparative Example 4]

[0262] A purified pyrolysis oil with impurities removed was produced under the same conditions as Example 1, except that no voltage was applied in Example 1.

[0263] [Comparative Example 5]

[0264] In Example 1, except that dimethyl disulfide was not mixed into the dehydrated first mixture, the same conditions as in Example 1 were performed to produce purified pyrolysis oil from which impurities were removed.

[0265] Evaluation example

[0266] [measurement method]

[0267] The composition of waste plastic feed was analyzed using a Flake analyzer from RTT, Germany, among NIR analyzers.

[0268] To confirm the composition of pyrolysis products related to the measurement of pyrolysis oil yield, GC-Simdis analysis (HT 750) was performed.

[0269] To analyze the moisture and impurity Cl, S, N, O contents in the mixture obtained after the dehydration process and the impurity Cl, S, N, O contents in the finally obtained refined pyrolysis oil, ICP, TNS, EA-O, and XRF analyses were performed. The total Cl content was measured according to ASTM D5808, the N content was measured according to ASTM D4629, and the S content was measured according to ASTM D5453.

[0270] The catalytic activity retention time was measured in hours based on the point at which the nitrogen content in the refined pyrolysis oil exceeded 10 ppm through Total Nitrogen & Sulfur (TNS element) analysis on refined pyrolysis oil.

[0271] In addition, the process of the above examples and comparative examples was operated for 3 months, and the particle fixation rate was measured according to the following equation 1.

[0272] [Formula 1]

[0273] Particle sticking rate (%) = (Amount of impurity particles stuck to the electrode / Amount of impurity particles in the pyrolysis oil)*100

[0274] Comparative Example 1 Example 1 Example 2 Example 3 Example 4 Pyrolysis oil yield (weight%) 52.155.157.060.862.4

[0275] Refined pyrolysis oil composition ratio (weight %) Comparative example 1 Example 1 Example 2 Example 3 Example 4 Naphtha (boiling point 150 ℃ or less) 26.9 3 2.5 4 0.5 4 5.5 4 5.7 Kerosene (boiling point 150 to 265 ℃) 32.5 35.5 3.6 39.4 4 1.8 LGO (boiling point 265 to 340 ℃) 21.0 17.8 13.07.8 8.1 VGO (boiling point 340 ℃ or higher) 19.6 14.2 12.9 7.3 4.4 Sum of naphtha and kerosene 59.4 6 8.0 7 4.1 8 4.9 8 7.5

[0276] Comparative Example 1, in which the high-temperature filter was not filled with beads and the liquid condensed from the high-temperature filter was not reintroduced into the pyrolysis reactor, confirmed that the pyrolysis oil yield and the proportion of light fractions including naphtha and kerosene were the lowest.

[0277] Example 1, in which the liquid condensed in the high-temperature filter is reintroduced into the pyrolysis reactor, was confirmed to achieve a superior pyrolysis oil yield and a proportion of light hydrocarbons including naphtha and kerosene compared to Comparative Example 1.

[0278] Example 2, in which the liquid condensed in the high-temperature filter was reintroduced into the pyrolysis reactor and the high-temperature filter was filled with beads, showed a pyrolysis oil yield and a ratio of light hydrocarbons including naphtha and kerosene that were better than those of Example 1.

[0279] Examples 3 and 4, in which the liquid condensed in the high-temperature filter was reintroduced into the pyrolysis reactor, the high-temperature filter was filled with beads, and a temperature gradient was formed in the high-temperature filter, showed a better pyrolysis oil yield and a ratio of light hydrocarbons including naphtha and kerosene compared to Examples 1 and 2.

[0280] In particular, it was confirmed that Example 4, in which the upper temperature of the high-temperature filter was maintained at 430°C, the middle temperature at 450°C, and the lower temperature at 500°C, exhibited the best pyrolysis oil yield and the ratio of light hydrocarbons including naphtha and kerosene.

[0281] In addition, the measurement results related to the content of impurities in the refined pyrolysis oil according to the above examples and comparative examples are shown in Tables 3 and 4.

[0282] Example 1 Example 5 Example 6 Example 7 Example 8 Example 9 Example 10 Dehydration Washing Water (Volume) 0.25 0.50 0.25 0.25 0.25 0.25 0.25 De-emulsifier (Volume) 0.000 10.000 10.000 10.000 10.000 10.000 10.000 10.000 10.000 1 Temperature (℃) 150 150 150 150 120 120 150 Pressure (bar) 10 10 10 10 10 10 10 Voltage Type AC AC AC DC AC AC AC Electrode Vertical Vertical Vertical Horizontal Vertical Vertical Vertical Coagulator Whether or not XXXXXXO Hydrogenation Treatment Sulfur Source Mixing WhetherOOOOOOOTemperature (℃)300300300300300300300Pressure (bar)707070707018070Moisture content after dehydration (ppm)592783672595721895510Cl content after dehydration (ppm)126123137125144165108N content after dehydration (ppm)836814858839866947770Catalytic activity retention time (hr)>720>720>720>720>720>720>720Cl content in refined pyrolysis oil (ppm)<1<1<1<1<1<1<1N content in refined pyrolysis oil (ppm)<1<1<1<1<1<1Particles Sticking rate (%) 0.200.180.203.50.210.200.18

[0283] Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Dehydration Washing water (volume ratio) -0.25 0.25 0.25 De-emulsifier (volume ratio) 0.0001 - 0.0001 0.0001 Temperature (℃) 150 150 150 150 Pressure (bar) 10 10 10 10 Voltage type Alternating current Alternating current Electrode Vertical Vertical Vertical Coagulator XXXX Hydrogenation treatment Sulfur source mixed OOOX Temperature (℃) 300 300 300 300 Pressure (bar) 70 70 70 70 Moisture content after dehydration (ppm) 248 544 1638 406 10 Cl content after dehydration (ppm) 229 250 247 126 N content after dehydration (ppm) 10 49 1100 109 0 847 Catalytic activity Retention time (hr) <576 <576 <576 <336 Cl content in refined pyrolysis oil (ppm) 4.4 5.9 4.7 3.2 N content in refined pyrolysis oil (ppm) 11.4 14.5 12.4 11 Particle sticking rate (%) 0.2 4 0.21-0.20

[0284] As shown in Tables 3 and 4 above, Comparative Examples 2 to 4 showed poor moisture and Cl removal results as a result of changing the presence or absence of washing water, the presence or absence of demulsifier, and the presence or absence of voltage application from the examples, respectively. Accordingly, the catalyst was adversely affected in the hydrogenation treatment step, and the Cl content in the finally obtained refined pyrolysis oil was high. Although in Comparative Example 5, moisture and some impurities in the pyrolysis oil were sufficiently removed in the dehydration step, the hydrogenation catalyst was deactivated in a short period of time due to the insufficient sulfur content, and when the refining process was maintained for a long period of time, the Cl content in the refined pyrolysis oil was high, as in the other comparative examples.

[0285] However, in Examples 1 and 5 to 10 of the present disclosure, a significant amount of moisture contained in the pyrolysis oil was removed through the dehydration step, and a sulfur source was added, thereby significantly extending the activity of the hydrogenation catalyst. Furthermore, since some water-soluble impurities were preemptively removed during the dehydration step and the excellent activity of the catalyst was maintained for a long period of time, high-quality refined pyrolysis oil with a very low impurity content could be obtained.

[0286] Meanwhile, when applying an AC voltage using vertical electrodes, we confirmed that the rate of adhesion of impurity particles derived from char in the pyrolysis oil to the electrode surface was very low even after the process was conducted for more than three months. This indicates that applying an AC voltage or using vertical electrodes can eliminate the need for process shutdowns for internal reactor cleaning, thereby achieving superior process efficiency.

[0287] In addition, in Example 9, the dehydration results were poor compared to other examples, but the Cl content of impurities in the refined pyrolysis oil was very low as the hydrogenation treatment was conducted under high pressure conditions. However, it was confirmed that a relatively large amount of ammonium salts were generated even at the temperature at which the hydrogenation treatment was performed, as the high pressure resulted in excessive generation of ammonia and hydrogen chloride.

[0288] In Example 10, as additional dehydration was performed using a coagulant, the moisture and chlorine contents after dehydration were lower than in other examples, and it was confirmed that the activation time of the catalyst, process stability, and quality of refined pyrolysis oil were relatively better than in other examples.

[0289] The above description is merely an example of applying the principles of the present disclosure, and other configurations may be further included without departing from the scope of the present disclosure.

[0290] Description of the symbol

[0291] P-101 pretreatment stage

[0292] P-102 pyrolysis stage

[0293] P-103 hardening stage

[0294] P-104 Dehydration Stage

[0295] P-105 hydrogenation process

[0296] P-106 Second hydrogenation treatment stage

[0297] 11 Feedstock

[0298] 12 Feedstock injection section

[0299] 13 Pretreatment reactor

[0300] 14 Pyrolysis reactor

[0301] 15 High Temperature Filters

[0302] 16 Condenser

[0303] 17 Heater

[0304] 18 Pyrolysis oil recovery unit

[0305] 19 connecting pipes

[0306] 21 feed tanks

[0307] 22 Dehydrator

[0308] 23 Hydrogenation Unit

[0309] 24-1 First Separator

[0310] 24-2 Second Separator

[0311] 24-3 Third Separator

[0312] 24-4 4th Separator

[0313] 25 Fractionator

[0314] 26-1 Naphtha Hydrotreating Unit

[0315] 26-2 Kerosene / Gas Oil Hydrogenation Unit

[0316] 26-3 Residue Hydrogenation Unit

Claims

1. Pretreatment step for preprocessing waste plastic; A pyrolysis step of producing pyrolysis gas by putting pretreated waste plastic in the above pretreatment step into a pyrolysis reactor; A hardening step of producing pyrolysis oil by introducing the above pyrolysis gas into a hot filter; A dehydration step of applying voltage to a first mixture of the above-mentioned pyrolysis oil, washing water, and a demulsifier to dehydrate it; A hydrogenation step for producing refined pyrolysis oil from which impurities have been removed by hydrogenating a second mixture obtained by mixing the dehydrated first mixture and a sulfur source; and A second hydrogenation treatment step of second hydrogenation treatment of the above refined pyrolysis oil; Including, The liquid condensed in the above high temperature filter is reintroduced into the pyrolysis reactor. Method for producing purified hydrocarbons from waste plastic.

2. In paragraph 1, A method for producing purified hydrocarbons from waste plastic, wherein the high-temperature filter is filled with beads.

3. In paragraph 2, A method for producing purified hydrocarbon from waste plastic, wherein the above beads include at least one selected from the group consisting of silica (SiO2) and aluminum oxide (Al2O3).

4. In paragraph 1, A method for producing purified hydrocarbons from waste plastic, wherein a temperature gradient is formed in the above high-temperature filter.

5. In paragraph 4, A method for producing purified hydrocarbons from waste plastic, wherein the above temperature gradient is formed by providing at least two heaters on the outside of the high-temperature filter.

6. In paragraph 1, A method for producing purified hydrocarbons from waste plastic, wherein the pyrolysis reactor comprises at least two batch reactors.

7. In paragraph 6, A method for producing purified hydrocarbons from waste plastic, wherein the thermal decomposition step is performed by switching operation of at least two batch reactors.

8. In paragraph 1, A method for producing refined hydrocarbons from waste plastic, wherein the refined pyrolysis oil is mixed with petroleum hydrocarbons and subjected to secondary hydrogenation treatment to form a mixed oil.

9. In paragraph 8, A method for producing refined hydrocarbons from waste plastic, wherein the refined pyrolysis oil is included in an amount of 90 wt% or less of the total weight of the mixed oil.

10. In paragraph 1, A method for producing purified hydrocarbon from waste plastic, wherein the waste plastic comprises at least one selected from the group consisting of polyethylene (PE), polypropylene (PP), polyethylene terephthalate (PET), polyvinyl chloride (PVC), and polystyrene (PS).

11. In paragraph 1, In the above dehydration step, A method for producing purified hydrocarbons from waste plastic, wherein the pyrolysis oil is mixed in a larger volume than the washing water.

12. In paragraph 1, In the above dehydration step, A method for producing purified hydrocarbon from waste plastic, wherein the first mixture is a mixture of the pyrolysis oil and the washing water in a volume ratio of 1:0.001 to 0.

5.

13. In paragraph 1, In the above dehydration step, A method for producing refined hydrocarbons from waste plastic, wherein the first mixture is a mixture of the pyrolysis oil and the demulsifier in a volume ratio of 1:0.000001 to 0.

001.

14. In paragraph 1, A method for producing purified hydrocarbon from waste plastic, wherein the above-mentioned demulsifier is one or a mixture of two or more selected from the group consisting of polyethylene glycol, tert-butanol, acetone, alkylnaphthalenesulfonate, alkylbenzenesulfonate, nonionic alkoxylated alkyl phenol resin, polyalkylene oxide, and polyoxyethylene sorbitan ester.

15. Pretreatment device for pretreatment of waste plastic; A pyrolysis reactor that produces pyrolysis gas by injecting pretreated waste plastic from the above pretreatment device; A hot filter that produces pyrolysis oil by injecting the above pyrolysis gas; A connecting pipe connecting the high-temperature filter and the pyrolysis reactor so that the liquid condensed in the high-temperature filter is reintroduced into the pyrolysis reactor; A dehydration device that dehydrates the first mixture of the above-mentioned pyrolysis oil, washing water, and a demulsifier by applying voltage; A hydrogenation treatment device that hydrogenates a second mixture obtained by mixing the dehydrated first mixture and a sulfur source to produce refined pyrolysis oil from which impurities have been removed; and A second hydrogenation treatment device for second hydrogenation treatment of the above refined pyrolysis oil; A system for producing purified hydrocarbons from waste plastics, comprising:

16. In paragraph 15, A system for producing purified hydrocarbons from waste plastic, wherein the above high-temperature filter is filled with beads.

17. In paragraph 16, A system for producing purified hydrocarbons from waste plastic, wherein the above beads include at least one selected from the group consisting of silica (SiO2) and aluminum oxide (Al2O3).

18. In paragraph 15, A system for producing purified hydrocarbons from waste plastic, wherein the above manufacturing system comprises at least two heaters on the outside of the high-temperature filter.

19. In paragraph 1, A method for producing refined hydrocarbon from waste plastic, wherein the method further comprises a distillation step of distilling the refined pyrolysis oil after the hydrogenation treatment step.

20. In paragraph 19, A method for producing refined hydrocarbons from the above waste plastic, wherein hydrocarbons derived from the refined pyrolysis oil separated in the above distillation step and petroleum hydrocarbons are mixed and subjected to secondary hydrogenation treatment to form a mixed oil.

Citation Information

Patent Citations

  • Heavy and inferior crude oil pretreatment process

    CN114479913A

  • Process for cooling hot pyrolysis gas

    EP0297424B1

  • Method for generating sound stimulation to control breathing rhythm and device therefor

    KR1020240118233A

  • Sealed type waste press and storage apparatus

    KR102160451B1

  • Circular economy for plastic waste to polypropylene via oil refinery with filtering and metal oxide treatment of pyrolysis oil

    US20210332300A1