Method for producing a hydrogel

The method of using alkaline earth metal ions in fibrinogen solutions to create thermoresponsive hydrogels addresses the limitations of existing fibrinogen material production, achieving cost-effective and enzyme-free fibrinogen hydrogels with tunable properties for diverse applications.

WO2024221027A1PCT designated stage expired Publication Date: 2024-10-31UNIVERSITY OF INNSBRUCK
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
PCT/AT2024/060167
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-24
Filing Date
2024-04-24
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Current methods for producing fibrinogen-based materials are limited in defining desired properties and require expensive enzymes like thrombin, posing risks of allergic reactions and unwanted thrombus formation, while existing salt-induced processes are only suitable for producing direct reaction products with unalterable properties.

Method used

A method involving an aqueous fibrinogen solution with specific pH and temperature conditions, combined with alkaline earth metal ions (Ca²⁺, Mg²⁺, Sr²⁺) to create thermoresponsive fibrinogen hydrogels, allowing for controlled gelation and reversible properties, enabling defined material properties and enzyme-free production.

Benefits of technology

The method produces fibrinogen hydrogels with tunable properties, reducing production costs and risks, and enabling applications in drug delivery, cell culture, and medical diagnostics, with reversible and irreversible gelation options depending on ion types and conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure AT2024060167_31102024_PF_FP_ABST
    Figure AT2024060167_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The invention relates to a method for producing a thermoresponsive fibrinogen hydrogel, comprising the steps of: (a) preparing an aqueous solution of fibrinogen, wherein the concentration of fibrinogen is at least 20 g / L, wherein the temperature of the solution is between 35 °C and 40 °C, wherein the solution has a pH of 7.0 to 8.0, wherein a buffer is present in a concentration of 15 mmol / L to 25 mmol / L, (b) adding an alkaline earth metal ion from the group consisting of Ca2+, Mg2+ and Sr2+, wherein the alkaline earth metal ion is added in the form of a water-soluble alkaline earth metal salt at an amount of 15 to 30 mmol / L, (c) incubating the solution obtained in step (b) at a temperature of 35 °C to 40 °C, (d) gelling the solution obtained in step (c) to form a thermoresponsive fibrinogen hydrogel by reducing the temperature of the solution.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] METHOD FOR PRODUCING A HYDROGEL

[0002] The present invention relates to a method for producing a thermoresponsive fibrinogen hydrogel from fibrinogen. Furthermore, the invention relates to a thermoresponsive fibrinogen hydrogel.

[0003] BACKGROUND OF THE INVENTION

[0004] Due to its versatile properties, fibrinogen is widely used in materials and medical research. Its natural role as a wound-healing protein already gives it excellent biocompatibility combined with exceptional cell adhesion. This is demonstrated, among other things, by the successful application of fibrinogen-based materials in tissue engineering and drug encapsulation. In natural wound healing, fibrinogen is polymerized into a fibrous hydrogel – fibrin – to optimally close wounds.

[0005] The biggest disadvantage of fibrin production on an industrial scale is the necessary use of the expensive enzyme thrombin. In addition to high costs, there are also risks of allergic reactions or unwanted thrombus formation.

[0006] DE 10 2020 130 778 Al has already shown that fibrin-like, fibrous materials can be obtained even without enzymes. This process is based on a simple salt-induced process based on fibrinogen or smaller fibrinogen aggregates in solution. However, the process according to DE 10 2020 130 778 Al is only suitable for the production of fibrin-like materials as a direct reaction product. This process cannot be used to produce a material that can be specifically used elsewhere, for example, and the properties of the fibrin-like material produced according to DE 10 2020 130 778 Al are hardly influenceable.

[0007] BRIEF DESCRIPTION OF THE INVENTION

[0008] Given that the state of the art only allows for limited specification of desired properties in the production of fibrinogen-based fibers prior to synthesis, the inventors set themselves the task of converting fibrinogen into a material with defined properties.

[0009] This object is achieved by a method for producing a thermoresponsive fibrinogen hydrogel, comprising the steps

[0010] (a) providing an aqueous solution of fibrinogen, wherein the concentration of fibrinogen is at least 20 g / L, wherein the temperature of the solution is between 35 °C to 40 °C, wherein the solution has a pH of 7.0 to 8.0, wherein a buffer is present in a concentration of 15 mmol / L to 25 mmol / L,

[0011] (b) Addition of an alkaline earth metal ion from the group consisting of Ca 2+ , Mg 2+ and Sr 2*, wherein the alkaline earth metal ion is added in the form of a water-soluble alkaline earth metal salt in an amount of 15 to 30 mmol / L,

[0012] (c) incubating the solution obtained in step (b) at a temperature of 35 °C to 40 °C,

[0013] (d) gelling the solution obtained in step (c) to form the thermoresponsive fibrinogen hydrogel by lowering the temperature of the solution.

[0014] Surprisingly, the method according to the invention resulted in the discovery of a thermoresponsive hydrogel based on the protein fibrinogen. Until now, it was unknown that such a fibrinogen-based material was even possible, regardless of whether an enzyme was used to polymerize fibrinogen or whether fibrinogen was treated in another way. These novel thermoresponsive fibrinogen hydrogels therefore open up numerous new possibilities and application potentials in addition to those already known. First and foremost, these include drug delivery, reusable substrates for cell culture growth, and the broad field of non-invasive medical diagnostics.

[0015] The production of thermoresponsive fibrinogen hydrogels is straightforward and even cheaper than that of non-thermoresponsive fibrin. The key is that defined concentrations of alkaline earth metal ions (Ca 2+ , Mg 2+ , South+ ) and buffers as well as high concentrations of fibrinogen are used, whereby different properties are achieved depending on the alkaline earth metal ion and, if applicable, temperature:

[0016] Ca 2+ -induced gelation

[0017] With Ca 2+ Irreversible gelation to fibrinogen hydrogels can be achieved "on demand" by cooling within, for example, 15 minutes. This requires a defined temperature program and a narrow range of ion concentrations.

[0018] • Dissolve at least 20 mg / mL fibrinogen in a buffer at 37 °C (buffer concentration: 20 mmol / L, pH 7.0 - 8.0 possible, preferably 7.5).

[0019] • 15 - 30 mmol / L Ca 2+ admit.

[0020] • Incubation takes place at 35°C to 40°C, preferably at approximately 37°C. The incubation time should be at least 6 hours. The solution will not change visually during this time. However, subsequent gelation is only ideal if this time is observed. Gelation after 4 hours is incomplete. If necessary, the incubation time should be approximately 8 hours.

[0021] • Once the fibrinogen hydrogel is desired, gelation is induced by cooling the sample. Cooling is preferably to a maximum of 33°C. The time until irreversible gelation depends on the final temperature. At 33°C, this takes overnight, at 30°C only 1.5 hours, and at 25°C approximately 10 minutes.

[0022] A variation is gelation at 5 °C. Here, the prepared precursor solution (after 6 h at 35 °C to 40 °C, preferably around 37 °C) can also be gelled at 5 °C. This gelation is initially reversible (for about 2 h) but then transforms into the usual thermally irreversible gels.

[0023] Mg 2+ -induced gelation

[0024] The addition of Mg 2+ As an alkaline earth metal ion, fibrinogen hydrogels can be formed, which gel upon slow cooling and then completely dissolved again at elevated temperatures within a few minutes. This process can be repeated as often as required.

[0025] With Mg 2+ -ions, completely thermoreversible, fibrous fibrinogen hydrogels are accessible. This gelation is independent of the incubation time of the Mg 2+ , as is the case with Ca 2+This is the case. The gels can always be thermally dissolved again. Tests have shown that thermal redissolution is possible after a gelation time of 2 weeks. A typical test procedure is as follows:

[0026] • Dissolve at least 20 mg / mL fibrinogen in a buffer at 37 °C (buffer concentration: 20 mmol / L, pH 7.0 - 8.0, ideally 7.5).

[0027] • 15 - 30 mmol / L Mg 2+ add (should be between 15 and less than 30 mmol / Mg 2+ added, NaCl can also be added in an amount that the total concentration of Mg 2+ and NaCl together is around 30 mmol / L. For example, it is also possible to add 15 mmol / L of Mg 2+ and 15 mmol / L NaCl. The total ion concentration of the salts should be max. 30 mmol / L. It is advantageous not to add complexing anions (such as oxalate, etc.) at this point, as this can delay gelation or increase the free Mg 2+Concentration reduced due to complex formation. At more than 30 mmol / L Mg 2+ the gelation becomes increasingly incomplete and the material no longer becomes solid.

[0028] • The sample can be stored at 5 °C for gelation. Further storage at 37 °C does not alter the process.

[0029] • Stable gels ideally require about 2 h at 5 °C, longer gelation times at 5 °C (24 h) lead to a significantly increased fiber yield.

[0030] • Gelling at 25 °C is not possible.

[0031] • The gels can be completely dissolved again by incubating them at 37 °C for approximately 15 minutes. A temperature of 25 °C is not sufficient and only results in a cloudy suspension. The completely dissolved samples can be regelled and dissolved as desired. 2+ -induced gelation

[0032] The addition of Sr 2* as alkaline earth metal ion enables the formation of fibrinogen hydrogels with combined properties of Mg 2+ and Ca 2+ : This also makes thermally switchable fibrinogen hydrogels accessible, which can be subsequently converted into thermally irreversible fibrinogen hydrogels as needed. To enable this "post-curing," the fibrinogen hydrogel must be stored at room temperature for several hours after it has been removed from the refrigerator.

[0033] With Sr 2+ can be analogous to Mg 2+ reversible gels can be produced. The experimental procedure is basically identical to the Mg 2+ -process. However, it is also possible to produce irreversible gels. For this purpose, the gel is stored for (at least) 4 h at 5 °C and then "post-cured" for 2 h at room temperature (with Mg 2+This results in a cloudy, liquid "suspension", while the Sr^ gels initially appear optically unchanged. However, if gelation is only carried out for 2 h at 5 °C, post-curing at room temperature only results in the suspension described.

[0034] An alternative is storage for 2 weeks at 5 °C, which also produces irreversible gels.

[0035] Optionally, a step (c') can be provided between step (c) and step (d), in which the solution is formed into a desired shape. This allows the thermoresponsive fibrinogen hydrogel to be given a specific three-dimensional shape.

[0036] The findings described above result in various embodiments with different alkaline earth metal ions. In a first embodiment, the alkaline earth metal ion is Ca 2+ , wherein in step (e) the temperature is then cooled to 25 to 33 °C for a period of 10 minutes to 12 hours.

[0037] In a further embodiment, the alkaline earth metal ion is Mg 2+ or Sr 2+ , wherein in step (d) the temperature is then cooled to 0 to 10 °C, preferably about 5 °C, for a period of 2 hours.

[0038] In the embodiment with Mg 2+ or Sr 2+ , it can be provided that the thermoresponsive fibrinogen hydrogel is heated to 35 °C to 40 °C for 15 min after step (d) and dissolved, and then processed again at a desired location by gelling by lowering the temperature of the solution to form the thermoresponsive fibrinogen hydrogel. In this embodiment, a reversible hydrogel is obtained. Alternatively, if the alkaline earth metal Srf +In step (d), the temperature can be cooled to 2 °C to 10 °C, preferably approximately 5 °C, for a period of at least 4 hours. If the gel is subsequently cured for at least 2 hours at approximately 20 °C to 25 °C, an irreversible fibrinogen hydrogel is obtained.

[0039] "Irreversible" in this context means that the fibrinogen hydrogels no longer dissolve. Tests were conducted for one week at 37°C or with subsequent addition of salt (NaCl and oxalate).

[0040] 2-(4-(2-hydroxyethyl)-l-piperazinyl)-ethanesulfonic acid (“HEPES”) has proven to be advantageous as a buffer.

[0041] In biological systems, NaCl is often added to improve the solubility of fibrinogen and to mimic physiological conditions. For the purposes of the invention, the NaCl concentration should be kept low, otherwise gelation will not proceed completely. Therefore, it is preferred that the NaCl concentration in the solution be a maximum of 15 mmol / L.

[0042] At the Mg 2+ -induced gels, a pH of max. 7.5 is advantageous, since otherwise the solubility limit of Mg(OH)2 is potentially exceeded.

[0043] In one aspect of the invention, a thermoresponsive fibrinogen hydrogel is provided, obtainable by the aforementioned method. "Thermoresponsive" is generally understood to mean that the material can be specifically modified when the temperature is increased or decreased. Generally, all materials react to a decrease in temperature by gelling. By subsequently increasing the temperature, the Mg 2+ - and partly Sr 2+ -induced gels can be dissolved again or even “post-cured”.

[0044] Furthermore, a fibrinogen hydrogel is provided, which contains fibers with fibrinogen, Ca 2+ or Mg 2+ or Sr 2+ wherein the fibers have a length of > 5 pm, preferably > 10 pm.

[0045] DETAILED DESCRIPTION OF THE INVENTION

[0046] Further details and advantages of the invention are explained with reference to figures and a description of the figures. For explanation, reference is also made in particular to the prior art according to DE 10 2020 130 778 A1.

[0047] Fig. 1 shows a scheme of the Mg 2+ induced fibrinogen hydrogel formation. Fig. 2 shows a scheme of the Sr 2 * induced fibrinogen hydrogel formation.

[0048] Fig. 3 shows according to the invention with Mg 2+ or Sr 2+ induced fibrinogen hydrogels compared to the fibrin-like material according to DE 10 2020 130 778 Al.

[0049] Fig. 4 shows according to the invention with Ca 2+ induced fibrinogen hydrogel compared to the fibrin-like material according to DE 10 2020 130 778 Al.

[0050] Fig. 5 shows SEM images at two different magnifications of fibrin-like material according to DE 10 2020 130 778 Al.

[0051] Fig. 6 shows SEM images (top) in two different magnifications of fibrinogen hydrogel according to the invention on Ca 2+ Base and photographic representations (below) of this fibrinogen hydrogel as a function of time.

[0052] In Fig. 1 the Mg 2+ -induced hydrogel formation from fibrinogen is schematically explained using an example embodiment. Mg 2+ enables fibrinogen hydrogels that gel upon slow cooling and then dissolve completely again at elevated temperatures within a few minutes. This process can be repeated as often as required.

[0053] At a HEPES buffer concentration of 20 mmol / L at pH 7.5, at least 20 mg / mL fibrinogen is dissolved in a buffer at 37 °C. Subsequently, 15 - 30 mmol / L Mg 2+ added (it is also possible to add 15 mmol / L Mg 2+and 15 mmol / L NaCl). The sample can be stored at 5 °C for gelation. Further storage at 37 °C does not alter the process. Stable gels should be stored at 5 °C for at least 2 h. Longer gelation times of up to 24 h at 5 °C lead to an increased fiber yield. At 25 °C, gelation does not yet occur, so longer-term storage at this temperature is possible. If partial precipitation occurs during storage, a solution can be achieved by heating at 37 °C for approximately 15 min, followed by gelation. Completely dissolved samples can be regelled and dissolved as required.

[0054] Fig. 2 shows the SrM-induced formation of hydrogels. Srf + combines the properties of Mg 2+ and Ca 2+ : Also with Sr 2+As an alkaline earth metal ion, thermally switchable fibrinogen hydrogels are accessible, which can subsequently be converted into thermally irreversible fibrinogen hydrogels as needed. To enable this "post-curing," the fibrinogen hydrogel is stored at room temperature for several hours after it is removed from the refrigerator.

[0055] With Sr 2+ can be analogous to Mg 2+ reversible gels can be produced. The experimental procedure corresponds to the Mg 2+ -process. Alternatively, it is possible to produce irreversible gels. For this, the hydrogel is stored for (at least) 4 hours at 5 °C and then "post-cured" for 2 hours at room temperature. However, if gelation is only carried out for 2 hours at 5 °C, "post-curing" at room temperature only results in the described "suspension."

[0056] If the process described in DE 10 2020 130 778 Al is carried out with MgCh or SrCh, no gels are formed and at most slightly fibrous structures are formed. This is illustrated in Fig. 3. Examples for Mg 2+ Photos of the corresponding samples are shown, which show that gels are actually only possible with the method according to the invention.

[0057] As shown in Fig. 4, Ca 2+ According to DE 10 2020 130 778 A1, fibrous hydrogels are accessible, but no "on-demand" gelation. Improved material properties can be characterized in this case by rheology measurements. A comparison of the SEM images is shown in Fig. 4.

[0058] Compared to DE 10 2020 130 778 Al, there are significant differences in the concentrations and temperatures in the process. This allows for "on-demand" gelation if the pH value is maintained by buffers and the appropriate temperature profile is maintained.

[0059] In Fig. 6, the thermoresponsive fibrinogen hydrogel on Ca 2+ -Gel "on demand" is visualized in the form of SEM images and sample photos. The SEM images show the gelled sample (after 10 min at room temperature). In comparison, Fig. 5 shows the fibrin-like materials according to DE 102020 130 778 A1 (5 g / L fibrinogen with 15 mmol / L CaCh after a) 4 h at 5 °C and b) 24 h at 5 °C). Based on the SEM images, longer fiber structures are visible in the fibrinogen hydrogel according to the invention, and the fiber yield is higher.

[0060] For the Mg 2+ - and Sr 2+-induced process, the differences are more clearly visible in the SEM. With the process according to the invention, defined fibers are achieved with high yield, while the prior art process produces more spherical aggregates that may be slightly interconnected. In contrast to the prior art material, the material produced by the process according to the invention with the Mg 2+ - and Sr 2+ -induced process solid and no longer liquid.

Claims

CLAIMS 1. A method for producing a thermoresponsive fibrinogen hydrogel, comprising the steps (a) providing an aqueous solution of fibrinogen, wherein the concentration of fibrinogen is at least 20 g / L, wherein the temperature of the solution is between 35 °C to 40 °C, wherein the solution has a pH of 7.0 to 8.0, wherein a buffer is present in a concentration of 15 mmol / L to 25 mmol / L, (b) Addition of an alkaline earth metal ion from the group consisting of Ca 2+ , Mg 2+ and Sü + , wherein the alkaline earth metal ion is added in the form of a water-soluble alkaline earth metal salt in an amount of 15 to 30 mmol / L, (c) Incubation of the solution obtained in step (b) at a temperature of 35 °C to 40 °C (d) gelling the solution obtained in step (c) to form the thermoresponsive fibrinogen hydrogel by lowering the temperature of the solution.

2. Process according to claim 1, characterized in that between step (c) and step (d) the solution is introduced into a desired shape.

3. A process according to claim 1 or claim 2, characterized in that the alkaline earth metal ion is Ca 2+ wherein the incubation in step (c) is carried out for a period of at least 6 hours, wherein in step (d) the temperature is cooled to 25 to 33 °C for a period of 10 minutes to 12 hours.

4. A process according to claim 1 or claim 2, characterized in that the alkaline earth metal ion is Mg 2+ or SÜ + and in step (d) the temperature is cooled to < 5 °C for a period of 2 hours.

5. A process according to claim 1 or claim 2, characterized in that the alkaline earth metal ion is Sr 2+ and in step (d) the temperature is cooled to 2 °C to 10 °C for a period of at least 4 hours.

6. The method according to claim 4 or claim 5, characterized in that the thermoresponsive fibrinogen hydrogel is subsequently heated to 35 °C to 40 °C for 15 minutes and dissolved and is then processed again at a desired location by gelling by lowering the temperature of the solution to form the thermoresponsive fibrinogen hydrogel.

7. The method according to claim 5 or claim 6, characterized in that after step (d), a step (e) is provided in which the temperature is brought to 20°C to 30°C, preferably about 25°C, for a period of at least 2 hours.

8. A thermoresponsive fibrinogen hydrogel, in particular a fibrous thermoresponsive fibrinogen hydrogel, obtainable by a method according to any one of claims 1 to 7.

9. Fibrinogen hydrogel comprising fibers with fibrinogen, Ca 2+ or Mg 2+ or Sr 2 *, wherein the fibers have a length of > 5 pm, preferably > 10 pm.

10. Fibrinogen hydrogel comprising Fibers with fibrinogen, Ca 2+ or Mg 2+ or Sr 2 *, wherein the fibers have a length of > 5 pm, preferably > 10 pm, wherein the fibrinogen hydrogel is thermoresponsive.

Citation Information

Patent Citations

  • Methods for the production of fibrinogen networks

    DE102020130778A1