High-refractive-index UV printing ink, and preparation method therefor and use thereof

Through the application of high-refractive index UV printing ink, the problem of low light extraction efficiency of OLED light-emitting devices is solved, higher luminous efficiency and lower power consumption are achieved, the process is simplified and the cost is reduced.

WO2024221256A1PCT designated stage expired Publication Date: 2024-10-31WANHUA CHEM GRP CO LTD

Patent Information

Application Number
PCT/CN2023/090754
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-26
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The light extraction efficiency of existing OLED light-emitting devices is low, resulting in high power consumption. The preparation of existing light extraction layer materials is complex and costly.

Method used

Develop a high refractive index UV printing ink, through a combination of modified inorganic nanoparticle dispersion, acrylate resin and acrylate reactive monomer, and use a double bond-containing silane coupling agent and silane group to modify the inorganic nanoparticles , improve the refractive index and light extraction efficiency of the ink, and be used in light extraction films.

Benefits of technology

The luminous efficiency of the luminescent layer is improved, the power consumption of the OLED device is reduced, the service life is extended, the process is simple, the cost is low, and it is more energy-saving and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2023090754-FTAPPB-I100001
    Figure PCTCN2023090754-FTAPPB-I100001
  • Figure PCTCN2023090754-FTAPPB-I100002
    Figure PCTCN2023090754-FTAPPB-I100002
  • Figure PCTCN2023090754-FTAPPB-I100003
    Figure PCTCN2023090754-FTAPPB-I100003
Patent Text Reader

Abstract

The present application provides high-refractive-index UV printing ink, and a preparation method therefor and a use thereof. The UV printing ink is composed of certain parts of acrylate resin, a modified inorganic nanoparticle dispersion liquid, acrylate active monomers, and a photoinitiator. The modified inorganic nanoparticle dispersion liquid is obtained by modifying inorganic nanoparticles by means of a silane coupling agent containing a double bond and / or acrylate containing a silane group. Modifying inorganic nanoparticles by means of a silane coupling agent containing a double bond and / or acrylate containing a silane group can effectively relieve the problem of the reduction of the refractive index of inorganic nanoparticles due to modification, and two types of acrylate are compounded to effectively improve the refractive index and the light extraction efficiency of UV printing ink, so that when the UV printing ink is applied to light extraction films, the light-emitting efficiency of a light-emitting layer can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

A high-refractive-index UV printing ink and its preparation method and application Technical Field

[0001] The present application belongs to the field of ink technology, and specifically relates to a high-refractive-index UV printing ink, a preparation method thereof, and an application thereof. Background Art

[0002] OLED (Organic Light-Emitting Diode), also known as organic electric laser display, organic light-emitting semiconductor; it is a current-type organic light-emitting device, which emits light through the injection and recombination of carriers, and the luminous intensity is proportional to the injected current. Under the action of the electric field, the holes generated by the anode and the electrons generated by the cathode will move, and are injected into the hole transport layer and the electron transport layer respectively, and migrate to the light-emitting layer. When the two meet in the light-emitting layer, energy excitons are generated, thereby exciting the light-emitting molecules and ultimately generating visible light; OLED display screens, with their advantages of being lighter, brighter, lower power consumption, faster response, higher clarity, better flexibility, and higher luminous efficiency, have quickly gained new consumer demand for display technology, greatly promoting the industrialization process of OLED. However, due to the diversified development of terminal product application needs, higher requirements are placed on the ideal luminous efficiency of OLED.

[0003] Currently, only 20-30% of all photons generated by OLED light-emitting devices can be extracted, which greatly increases their power consumption requirements. Therefore, breakthroughs in effective light extraction layer materials are urgently needed.

[0004] CN103168373A discloses a light extraction film for an organic light-emitting device (OLED), which provides a flexible carrier film. The carrier film includes two layers of films with different refractive indices, and utilizes different reflectivity differences to refract and convert light, effectively improving the light extraction efficiency of the light-emitting layer. However, its preparation structure is complex and difficult to industrialize.

[0005] CN114747038A discloses an organic light-emitting diode light extraction layer with a gradient refractive index, and provides an OLED stacked layer. With the help of an axis perpendicular to the flat part, it has a refractive index gradient principle and is coated with UV-curable ink layers with different refractive indices for light extraction. This method effectively improves the light extraction efficiency of the light-emitting layer, but because it requires oil layers with different refractive index gradients, the operation process is too complicated and the cost investment is relatively high.

[0006] Therefore, it is expected to develop a UV printing ink with a high refractive index to solve the above technical problems.

[0007] Summary of the Invention

[0008] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.

[0009] In response to the shortcomings of the existing technology, the purpose of this application is to provide a high-refractive index UV printing ink and its preparation method and application. The UV printing ink has a high refractive index and light extraction rate, and when applied to the light extraction film, it can effectively improve the luminous efficiency of the light-emitting layer, reduce the power consumption of the OLED device, extend its service life, and be more energy-saving and environmentally friendly.

[0010] To achieve this goal, this application adopts the following technical solutions:

[0011] In a first aspect, the present application provides a high refractive index UV printing ink, wherein the UV printing ink comprises the following components in parts by weight:

[0012] The modified inorganic nanoparticle dispersion is obtained by modifying inorganic nanoparticles with a silane coupling agent containing a double bond and / or an acrylate containing a silane group.

[0013] The amount of the acrylic resin may be 5 parts by weight, 10 parts by weight, 15 parts by weight, 20 parts by weight, 25 parts by weight, 30 parts by weight, or 35 parts by weight.

[0014] The modified inorganic nanoparticle dispersion can be 35 parts by weight, 40 parts by weight, 45 parts by weight, 50 parts by weight, 55 parts by weight, 60 parts by weight, 65 parts by weight, 70 parts by weight, or 75 parts by weight.

[0015] The amount of the acrylate reactive monomer may be 15 parts by weight, 20 parts by weight, 30 parts by weight, 40 parts by weight, 50 parts by weight, or 55 parts by weight.

[0016] The photoinitiator can be 1 part by weight, 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight, 3 parts by weight, 3.5 parts by weight, 4 parts by weight or 4.5 parts by weight, etc.

[0017] The high-refractive-index UV printing ink provided in the present application includes a combination of a specific number of acrylate resins, a modified inorganic nanoparticle dispersion, an acrylate reactive monomer, and a photoinitiator, and the modified inorganic nanoparticle dispersion is obtained by modifying inorganic nanoparticles with a double-bond silane coupling agent and / or a silane-containing acrylate. By modifying the inorganic nanoparticles with the aid of a double-bond silane coupling agent and / or a silane-containing acrylate, the problem of a decrease in the refractive index of the inorganic nanoparticles due to the modification is effectively reduced, thereby improving the refractive index of the overall formula and enhancing the light extraction efficiency. At the same time, the present application uses an acrylate resin and an acrylate reactive monomer for compounding, effectively improving the stability of the system, so that the obtained UV printing ink can be applied to the light extraction layer to effectively improve the luminous efficiency of the light-emitting layer, thereby reducing the power consumption of the terminal device, extending the service life, and being more energy-saving and environmentally friendly.

[0018] The high refractive index UV printing ink provided in this application refers to a UV printing ink with a liquid refractive index of not less than 1.55.

[0019] Optionally, the solid content of the modified inorganic nanoparticle dispersion is not less than 50%, for example, 52%, 54%, 56%, 58% or 60%.

[0020] Optionally, the particle size of the inorganic nanoparticles is not greater than 50 nm, for example, 45 nm, 40 nm, 35 nm, 30 nm, 25 nm, 15 nm, 10 nm, 9 nm, 8 nm, 7 nm, 6 nm, 5 nm, 4 nm or 3 nm, and can be further selected to be not greater than 10 nm, and further selected to be 5 to 7 nm.

[0021] Optionally, the inorganic nanoparticles have a crystal form of tetragonal phase and / or monoclinic phase.

[0022] Optionally, the mass percentage of tetragonal inorganic nanoparticles in the inorganic nanoparticles is not less than 70%, for example, 72%, 74%, 76%, 78%, 80%, 82%, 84%, 86% or 88%.

[0023] Optionally, the inorganic nanoparticles include any one or a combination of at least two of ZrO, ZrOC, AlO, AlOC, TiO, TiOC, ZnO or ZnOC.

[0024] Optionally, the silane coupling agent containing a double bond includes any one of γ-methacryloxypropyltrimethoxysilane, vinyltriethoxysilane, vinyltrimethoxysilane, vinyltri(2-methoxyethoxy)silane, vinyltriisopropoxysilane, vinyltriisopropoxysilane, methylvinyldiethoxysilane, methylvinyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropylmethyldimethoxysilane or 3-methacryloxypropyltris(trimethylsiloxy)silane, or a combination of at least two thereof.

[0025] Optionally, the acrylate containing a silane group is obtained by reacting component A and component B; the component A is a siloxane containing a double bond, which can be any one of methacryloxypropyltrimethoxysilane, vinyltriethoxysilane, vinyltrimethoxysilane, vinyltri(2-methoxyethoxy)silane, vinyltriisopropoxysilane, vinyltriisopropoxysilane, methylvinyldiethoxysilane, methylvinyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropylmethyldimethoxysilane or 3-methacryloxypropyltris(trimethylsiloxy)silane, or a combination of at least two thereof;

[0026] The component B is a fluorene compound having a hydroxyl group, which can be any one of 9,9-bis[(4-hydroxyethoxy)phenyl]fluorene, bisphenol fluorene or 9,9-bis(3-methyl-4-hydroxyphenyl)fluorene, or a combination of at least two thereof.

[0027] Optionally, the mass ratio of component A to component B is 1:(2-3), such as 1:2.2, 1:2.4, 1:2.6 or 1:2.8.

[0028] The present application does not impose any special restrictions on the preparation method of the provided silane group-containing acrylate. For example, component A and component B can be reacted under the condition of a catalyst to obtain the silane group-containing acrylate; wherein the catalyst can be tetrabutyl titanate, the reaction temperature is 50-80°C, and the reaction time is 3-4 hours.

[0029] Optionally, the mass ratio of the inorganic nanoparticles to the silane coupling agent containing double bonds is (0.5-1.5):1, for example, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 1.1:1, 1.2:1, 1.3:1 or 1.4:1.

[0030] Optionally, the mass ratio of the inorganic nanoparticles to the acrylate containing silane groups is (0.5-1.5):1, for example, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 1.1:1, 1.2:1, 1.3:1 or 1.4:1, etc.

[0031] Optionally, the modified inorganic nanoparticle dispersion is obtained by modifying inorganic nanoparticles with a silane coupling agent containing a double bond and / or an acrylate containing a silane group at 50-80°C (e.g., 55°C, 60°C, 65°C, 70°C or 75°C, etc.) for 3-4h (e.g., 3.2h, 3.4h, 3.6h or 3.8h, etc.).

[0032] Optionally, the number average molecular weight of the acrylic resin is 500 to 5000, for example, 1000, 1500, 2000, 2500, 3000, 3500, 4000 or 4500.

[0033] Optionally, the acrylic resin includes an acrylic acid ester compound having a structure represented by Formula I and / or an acrylic acid ester compound having a structure represented by Formula II;

[0034] Wherein, R1 to R4 are each independently selected from an alkylene group or an alkyleneoxy group, and n1 to n4 are each independently selected from an integer between 1 and 20 (for example, 2, 4, 6, 8, 10, 12, 14, 16 or 18, etc.).

[0035] Optionally, R1 to R4 are each independently selected from C1 to C20 methylene (e.g., C, C2, C4, C6, C8, C10, C12, C14, C16 or C18 methylene) or C1 to C20 ethyleneoxy (e.g., C, C2, C4, C6, C8, C10, C12, C14, C16 or C18 ethyleneoxy).

[0036] Optionally, the acrylic resin includes an acrylic ester compound having a structure represented by Formula II.

[0037] Optionally, the acrylate resin includes tri(ethoxy)bisphenol A diacrylate and / or deca(ethoxy)bisphenol fluorene diacrylate.

[0038] Optionally, the acrylate reactive monomer includes any one or a combination of at least two of an acrylate compound having a structure shown in Formula III, an acrylate compound having a structure shown in Formula IV, or an acrylate compound having a structure shown in Formula V:

[0039] Wherein, X, Y, and Z are each independently selected from H or an alkyl group; and R5 to R7 are each independently selected from an alkylene group, an ether group, or an alkyleneoxy group.

[0040] Optionally, X, Y, and Z are each independently selected from C1 to C5 alkyl groups (eg, C2, C3, or C4 alkyl groups).

[0041] Optionally, R5 to R7 are each independently selected from C1 to C10 alkylene (e.g., C2, C4, C6 or C8 alkylene), C1 to C10 alkyleneoxy (e.g., C2, C4, C6 or C8 alkyleneoxy) or C1 to C10 ether (e.g., C2, C4, C6 or C8 ether).

[0042] Optionally, R5 to R7 are each independently selected from a methylene group, an ether group or a methyleneoxy group.

[0043] Optionally, the acrylate reactive monomer includes any one or a combination of at least two of benzyl methacrylate, o-phenylphenoxyethyl acrylate or 3-phenoxybenzyl acrylate.

[0044] Optionally, the photoinitiator includes any one of benzoin diethyl ether, diphenylacetone, α-hydroxyalkyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-2-(4-morpholinyl)-1-[4-(methylthio)phenyl]-1-propanone, 2-dimethylamino-2-benzyl-1-[4-(4-morpholinyl)phenyl]-1-butanone, bis(2,4,6)-trimethylbenzoylphenylphosphine oxide or 2,4,6-trimethylbenzoyl-ethoxy-phenylphosphine oxide, or a combination of at least two thereof.

[0045] Optionally, the UV printing ink further includes an auxiliary agent.

[0046] Optionally, the content of the additive in the UV printing ink is 0.1 to 5 parts by weight, for example, 1 part by weight, 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight, 3 parts by weight, 3.5 parts by weight, 4 parts by weight or 4.5 parts by weight.

[0047] Optionally, the auxiliary agent includes any one of a defoaming agent, an inhibitor, a coupling agent or a leveling agent, or a combination of at least two thereof.

[0048] Optionally, the liquid refractive index of the UV printing ink is not less than 1.55, for example, 1.6, 1.65, 1.7, 1.75, 1.8, 1.85, 1.9 or 1.95.

[0049] Optionally, the refractive index of the UV printing ink after being completely cured into a film is not less than 1.62, for example, 1.63, 1.64, 1.65, 1.66, 1.67, 1.68 or 1.69.

[0050] Optionally, the viscosity of the UV printing ink is not greater than 30 cps, for example, 28 cps, 26 cps, 24 cps, 22 cps, 20 cps, 18 cps, 16 cps, 14 cps, 12 cps or 10 cps.

[0051] In a second aspect, the present application provides a method for preparing the UV printing ink as described in the first aspect, the preparation method comprising: mixing an acrylate resin, a modified inorganic nanoparticle dispersion, an acrylate active monomer, a photoinitiator and optionally an auxiliary agent to obtain the UV printing ink.

[0052] Optionally, the mixing time is not less than 2 min, for example, 2.5 min, 3 min, 3.5 min, 4 min, 4.5 min, 5 min or 5.5 min.

[0053] Optionally, the mixing is performed under stirring conditions.

[0054] Optionally, the stirring speed is not less than 1500 rpm, for example, 1550 rpm, 1600 rpm, 1650 rpm, 1700 rpm, 1750 rpm, 1800 rpm or 1850 rpm.

[0055] In a third aspect, the present application provides a light extraction film, which includes a base film and a UV printing ink layer, wherein the raw material of the UV printing ink layer includes the UV printing ink described in the first aspect.

[0056] Optionally, the UV printing ink layer is obtained by coating UV printing ink on the base film in a printing mode using a printer and drying the coating.

[0057] Optionally, the thickness of the UV printing ink layer is not greater than 50 μm, such as 45 μm, 40 μm, 35 μm, 30 μm, 25 μm or 20 μm, and can further be 10 to 30 μm.

[0058] In a fourth aspect, the present application provides an organic light emitting diode, comprising the light extraction film according to the third aspect.

[0059] Compared with the prior art, this application has the following beneficial effects:

[0060] The high-refractive-index UV printing ink provided in the present application includes a combination of a specific number of acrylate resins, a modified inorganic nanoparticle dispersion, an acrylate reactive monomer, and a photoinitiator. The modified inorganic nanoparticle dispersion is obtained by modifying inorganic nanoparticles with a double-bond silane coupling agent and / or a silane-containing acrylate. The inorganic nanoparticles are modified with the help of a double-bond silane coupling agent and / or a silane-containing acrylate, thereby effectively reducing the problem of a decrease in the refractive index of the inorganic nanoparticles caused by the modification, thereby improving the refractive index and light extraction efficiency of the ink. At the same time, the acrylate resin and the acrylate reactive monomer are compounded to effectively improve the stability of the system, further improve the refractive index and light extraction efficiency of the ink, so that the obtained UV printing ink has a high light extraction efficiency when applied to a light extraction film, thereby effectively improving the luminous efficiency of the light-emitting layer, reducing the power consumption of the OLED light-emitting device, extending its service life, and being more energy-saving and environmentally friendly.

[0061] Still other aspects will become apparent upon reading and understanding the detailed description. DETAILED DESCRIPTION

[0062] The technical solution of the present application is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present application and should not be regarded as specific limitations of the present application.

[0063] (1) The raw material information involved in the specific implementation of this application is as follows:

[0064] Benzyl methacrylate: Aladdin, reagent grade;

[0065] 9,9-Bis[(4-hydroxyethoxy)phenyl]fluorene: Osaka Gas Chemical Co., Ltd., industrial product;

[0066] 9,9-Bis(3-methyl-4-hydroxyphenyl)fluorene: Osaka Gas Chemical Co., Ltd., industrial product;

[0067] Zirconium dioxide particles: national porcelain, industrial products;

[0068] Tri(ethoxy)bisphenol A diacrylate: Meiyuan, industrial product;

[0069] Deca(ethoxy)bisphenol fluorene diacrylate: Zhide Chemical, industrial product;

[0070] 3-Acryloxypropyltrimethoxysilane: Evonik, industrial product;

[0071] o-Phenylphenoxyethyl acrylate: Korean KPX, industrial product;

[0072] 3-Phenoxybenzyl acrylate: Korean KPX, industrial product;

[0073] Phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide: Tianjin Jiuri, industrial product;

[0074] 2,4,6-Trimethylbenzoyl-ethoxy-phenylphosphine oxide: Tianjin Jiuri, industrial product;

[0075] Leveling agent: BYK333, industrial product;

[0076] Tetrabutyl titanate: Aladdin, reagent grade.

[0077] (2) The main instruments and equipment information involved in the specific implementation of this application is as follows:

[0078] Temperature control device: heat collecting constant temperature heating magnetic stirrer, Gongyi Yuhua Instrument;

[0079] Stirring device: stirring motor, IKA;

[0080] Condensation device: Qiuxing condenser tube, Gongyi Yuhua Instrument;

[0081] Alcohol removal device: vacuum pump, Baoling Instruments and Equipment;

[0082] Mixing equipment: FlackTek DAC600, FlackTek Inc;

[0083] Hardness and Young's modulus testing instruments: Nanoindenter, Agilent, USA;

[0084] Infrared tester: Mettler-Toledo infrared spectrometer, METTLER TOLEDO;

[0085] Refractive index tester: Abbe refractometer, Shanghai Wuguang;

[0086] Surface tension testing instrument: QBZY series fully automatic surface tension meter, Shanghai Fangrui Instrument Co., Ltd.;

[0087] Viscosity testing instrument: lamina viscometer, Brookfield, USA;

[0088] High temperature and high humidity aging chamber: Suzhou Zhihe and high temperature and high humidity aging chamber, espec;

[0089] Thermal shock test chamber: Suzhou Zhihe;

[0090] High temperature oven: Suzhou Zhihe;

[0091] Liquid optical particle counter: Shimadzu, Japan;

[0092] Calfisch moisture titrator: Metrohm, Switzerland;

[0093] Spectrophotometer: HunterLab Shanghai Xinlian.

[0094] Preparation Example 1

[0095] A modified inorganic nanoparticle dispersion, the preparation method of which comprises the following steps:

[0096] (1) 109.625 g of 9,9-bis[(4-hydroxyethoxy)phenyl]fluorene and 248.35 g of 3-methacryloyloxypropyltrimethoxysilane were added to a reaction flask equipped with a stirring device, a temperature control device, and a condensing device, and inert protective gas nitrogen was introduced. 0.05 g of tetrabutyl titanate was added, and the mixture was vacuum-treated at 50° C. to remove alcohol for 3 h. The hydroxyl group content was analyzed by infrared spectrometer. After the hydroxyl peak disappeared, an acrylate containing a silane group was obtained.

[0097] (2) Add 537 g of zirconium dioxide particles to the reaction bottle obtained in step (1), and continue to react at 50° C. and 1500 rpm for 3 hours to obtain the modified inorganic nanoparticle dispersion.

[0098] Preparation Example 2

[0099] A modified inorganic nanoparticle dispersion, the preparation method of which comprises the following steps:

[0100] (1) 95 g of 9,9-bis(3-methyl-4-hydroxyphenyl)fluorene and 248.35 g of 3-methacryloyloxypropyltrimethoxysilane were added to a reaction flask equipped with a stirring device, a temperature control device, and a condensing device, and inert protective gas nitrogen was introduced. 0.05 g of tetrabutyl titanate was added, and the mixture was vacuum-extracted at 80° C. to remove alcohol for 4 h. The hydroxyl group content was analyzed by infrared spectrometer. After the hydroxyl peak disappeared, the silane group-containing acrylate was obtained;

[0101] (2) Add 515 g of zirconium dioxide particles to the reaction bottle of step (1), and continue to react at 80° C. and 1500 rpm for 3 h to obtain the modified inorganic nanoparticle dispersion.

[0102] Preparation Example 3

[0103] A modified inorganic nanoparticle dispersion liquid is prepared by reacting 300 g of zirconium dioxide particles and 300 g of 3-methacryloxypropyltrimethoxysilane at 80° C. and 1500 rpm for 3 hours to obtain the modified inorganic nanoparticle dispersion liquid.

[0104] Comparative Preparation Example 1

[0105] An inorganic nanoparticle dispersion liquid is prepared by reacting 300 g of zirconium dioxide particles and 300 g of γ-glycidyloxypropyltrimethoxysilane at 80° C. and 1500 rpm for 3 hours to obtain the modified inorganic nanoparticle dispersion liquid.

[0106] Examples 1 to 9 and Comparative Examples 1 to 6

[0107] A high-refractive-index UV printing ink, comprising a preparation method comprising: sequentially adding an acrylate resin, a modified inorganic nanoparticle dispersion, an acrylate active monomer, a photoinitiator, and a leveling agent into a high-cleanliness storage tank; placing the storage tank in a chamber of a FlackTek DAC600 high-speed stirring device; controlling the temperature at 25° C. and the vacuum condition at a gauge pressure of -0.1 MPa; setting a segmented mode; stirring at a speed of 1500 rpm for 2 minutes, at a speed of 2000 rpm for 5 minutes, and at a speed of 1500 rpm for 2 minutes, until uniformly stirred; and removing the mixture after depressurization to obtain the high-refractive-index UV printing ink;

[0108] The raw material selection and dosage of each component in the above Examples 1 to 9 and Comparative Examples 1 to 6 are shown in Table 1, where the dosage range is "g":

[0109] Table 1

[0110] Performance testing:

[0111] (1) Surface tension: tested using the QBZY series fully automatic surface tension meter from Shanghai Fangrui Instrument Co., Ltd., and the average value was obtained by three tests;

[0112] (2) Viscosity test: Use a lamella viscometer, use a 52# rotor at 150 rpm, and test three times to obtain the average value;

[0113] (3) Cleanliness: Use a liquid particle counter and test three times to obtain the average value;

[0114] (4) Moisture content: Use a Calfisch tester and test three times to obtain the average value;

[0115] (5) Refractive index: Abbe refractometer tests the refractive index of liquid;

[0116] (6) Surface drying time: by 365nm wavelength LED ultraviolet light (2500mJ / cm 2 ) solidification, the time when the finger touches the surface and no string is drawn is the surface dry time;

[0117] (7) Surface dryness (touch test): by 365nm wavelength LED ultraviolet light (2500mJ / cm 2) Curing, finger touch method to judge the surface dry, requiring the finger to touch the surface of the spray film lightly, without sticky, sticky, or drawing phenomenon;

[0118] (8) Transmittance: Through 365nm wavelength LED ultraviolet light (2500mJ / cm 2 ) was cured to a film thickness of 30 μm, and the film transmittance was tested using a spectrophotometer;

[0119] (9) Yellowing index: 365nm wavelength LED ultraviolet light (2500mJ / cm 2 ) was cured to a film thickness of 30 μm, and the yellowing index of the film was tested by a spectrophotometer;

[0120] (10) Haze: by 365nm wavelength LED ultraviolet light (2500mJ / cm 2 ) was cured to a film thickness of 30 μm, and the haze of the film was tested using a spectrophotometer;

[0121] (11) Hardness and Young's modulus: The hardness and Young's modulus of the cured film were tested by nanoindentation instrument, and the film thickness was less than 1 μm;

[0122] (12) Double 85 high temperature and high humidity aging test: Use a spin coater to evenly coat a glass sheet with a certain amount of liquid product at a speed of 5000 rpm and expose it to a 365 nm wavelength LED ultraviolet light (2500 mJ / cm 2 ) Curing, after curing, the film is placed at 85 ° C, 85% humidity for 240 hours. If there is no wrinkle, bubble or separation on the film, it is qualified, otherwise it is unqualified;

[0123] (13) 110℃ high temperature and high humidity aging test: Use a spin coater to evenly coat a glass sheet with a certain amount of liquid product at a speed of 5000rpm and place it under a 365nm wavelength LED ultraviolet light (2500mJ / cm 2 ) After curing, the film is placed at 110℃ and 85% humidity for 32 hours. If there is no wrinkle, bubble or separation on the film, it is qualified, otherwise it is unqualified;

[0124] (14) Thermal shock test: Use a spin coater to evenly coat a glass sheet with a certain amount of liquid product at a speed of 5000 rpm and expose it to a 365 nm wavelength LED ultraviolet light (2500 mJ / cm 2 ) After curing, the diaphragm is cycled for 200 cycles at -40℃ / 30min and 80℃ / 30min. If there is no wrinkle, bubble or separation on the diaphragm, it is qualified, otherwise it is unqualified;

[0125] (15) High temperature resistance test: Use a spin coater to evenly coat a glass sheet with a certain amount of liquid product at a speed of 5000 rpm and place it under a 365 nm wavelength LED ultraviolet light (2500 mJ / cm 2 ) After curing, the film is placed at 120℃ for 240h. If there is no wrinkle, bubble or separation on the film, it is qualified, otherwise it is unqualified;

[0126] (16) Ethanol resistance test: Use a spin coater to evenly coat a glass sheet with a certain amount of liquid product at a speed of 5000 rpm and place it under a 365 nm wavelength LED ultraviolet light (2500 mJ / cm 2 ) solidification, and after solidification, the membrane was immersed in ethanol with a concentration of ≥95%, and its volume shrinkage was tested after 5 minutes.

[0127] The UV printing inks provided in Examples 1 to 9 and Comparative Examples 1 to 6 were tested according to the above test method. The test results are shown in Table 2:

[0128] Table 2

[0129] According to the data in Table 2, we can see that:

[0130] The high-refractive-index UV printing ink provided in Examples 1 to 9 has low viscosity, easy leveling, and excellent printing construction matching; and can be rapidly UV-cured within 1 to 3 seconds, and the cured coating has a high refractive index, good optical properties, mechanical properties, and high-temperature resistance; combined with the different structures and refractive indices of the device layers, it can effectively extract light from the luminescent layer, greatly reducing the power consumption of the terminal device, effectively improving product life and energy conservation.

[0131] By comparing Example 1 and Comparative Examples 1 to 4, it can be found that if the amount of the modified inorganic nanoparticle dispersion added is too low (Comparative Example 1), the hardness and Young's modulus of the UV printing ink will be low, and the high temperature resistance test will show failure; if the amount of the modified inorganic nanoparticle dispersion added is too high (Comparative Example 2), the surface tension of the UV printing ink will be too high, and the high temperature resistance test will also show failure; and if the modified inorganic nanoparticle dispersion is not added directly (Comparative Example 3), the high temperature resistance, high temperature aging performance and impact resistance of the UV printing ink will all be unqualified; and adding the modified inorganic nanoparticle dispersion obtained in Comparative Preparation Example 1 (Comparative Example 4) will also result in the obtained UV printing ink having unqualified impact resistance.

[0132] Comparing Example 1 with Comparative Examples 5-6, it can be found that not adding acrylate resin (Comparative Example 5) or not adding acrylate reactive monomer (Comparative Example 6) will affect the high temperature resistance and impact resistance of the final UV printing ink.

[0133] The applicant declares that this application, through the above-mentioned embodiments, illustrates a high-refractive-index UV printing ink, its preparation method, and application. However, this application is not limited to the above-mentioned embodiments, which does not necessarily mean that this application must rely on the above-mentioned embodiments in order to be implemented. Persons skilled in the art should understand that any improvements to this application, equivalent replacements for various raw materials in the product of this application, addition of auxiliary ingredients, and selection of specific methods, etc., fall within the scope of protection and disclosure of this application.

Claims

1. A high refractive index UV printing ink, the UV printing ink comprising the following components in parts by weight: The modified inorganic nanoparticle dispersion is obtained by modifying inorganic nanoparticles with a silane coupling agent containing a double bond and / or an acrylate containing a silane group.

2. The UV printing ink according to claim 1, wherein The solid content of the modified inorganic nanoparticle dispersion is not less than 50%; Optionally, the particle size of the inorganic nanoparticles is not greater than 50 nm, further preferably not greater than 10 nm, and further preferably 5 to 7 nm; Optionally, the crystalline form of the inorganic nanoparticles is tetragonal and / or monoclinic; Optionally, the mass percentage of tetragonal inorganic nanoparticles in the inorganic nanoparticles is not less than 70%; Optionally, the inorganic nanoparticles include any one of ZrO2, ZrOC, AlO, AlOC, TiO2, Ti2O3, TiOC, ZnO or ZnOC, or a combination of at least two thereof.

3. The UV printing ink according to claim 1 or 2, wherein: The silane coupling agent containing double bonds includes any one of γ-methacryloxypropyl trimethoxysilane, vinyl triethoxysilane, vinyl trimethoxysilane, vinyl tri(2-methoxyethoxy)silane, vinyl triisopropoxysilane, vinyl triisopropenoxysilane, methyl vinyl diethoxysilane, methyl vinyl dimethoxysilane, 3-methacryloxypropyl trimethoxysilane, 3-methacryloxypropyl triethoxysilane, 3-methacryloxypropyl methyl diethoxysilane, 3-methacryloxypropyl methyl dimethoxysilane or 3-methacryloxypropyl tri(trimethylsiloxy)silane, or a combination of at least two thereof; Optionally, the acrylate containing a silane group is obtained by reacting component A and component B; The component A is a siloxane containing double bonds; The B component is a fluorene compound having a hydroxyl group; Optionally, the mass ratio of component A to component B is 1:(2-3); Optionally, the mass ratio of the inorganic nanoparticles to the silane coupling agent containing double bonds is (0.5-1.5):1; Optionally, the mass ratio of the inorganic nanoparticles to the acrylate containing silane groups is (0.5-1.5):1; Optionally, the modified inorganic nanoparticle dispersion is obtained by modifying inorganic nanoparticles with a silane coupling agent containing a double bond and / or an acrylate containing a silane group at 50 to 80° C. for 3 to 4 hours.

4. The UV printing ink according to claim 3, wherein: Component A is any one of methacryloxypropyl trimethoxysilane, vinyl triethoxysilane, vinyl trimethoxysilane, vinyl tri(2-methoxyethoxy)silane, vinyl triisopropoxysilane, vinyl triisopropenoxysilane, methyl vinyl diethoxysilane, methyl vinyl dimethoxysilane, 3-methacryloxypropyl trimethoxysilane, 3-methacryloxypropyl triethoxysilane, 3-methacryloxypropyl methyl diethoxysilane, 3-methacryloxypropyl methyl dimethoxysilane or 3-methacryloxypropyl tri(trimethylsiloxy)silane, or a combination of at least two thereof; Optionally, component B is any one of 9,9-bis[(4-hydroxyethoxy)phenyl]fluorene, bisphenol fluorene or 9,9-bis(3-methyl-4-hydroxyphenyl)fluorene, or a combination of at least two thereof.

5. The UV printing ink according to any one of claims 1 to 4, wherein: The number average molecular weight of the acrylic resin is 500 to 5000; Optionally, the acrylic resin includes an acrylic acid ester compound having a structure shown in Formula I and / or Or an acrylate compound having a structure shown in formula II; wherein R1 to R4 are each independently selected from C1 to C20 alkylene or C1 to C20 alkyleneoxy, and n1 to n4 are each independently selected from an integer between 1 and 20; Optionally, the R1 to R4 are each independently selected from methylene or ethyleneoxy; Optionally, the acrylic resin is selected from acrylic compounds having a structure shown in Formula II; Optionally, the acrylate resin includes tri(ethoxy)bisphenol A diacrylate and / or deca(ethoxy)bisphenol fluorene diacrylate.

6. The UV printing ink according to any one of claims 1 to 5, wherein: The acrylate reactive monomer includes any one or a combination of at least two of an acrylate compound having a structure shown in Formula III, an acrylate compound having a structure shown in Formula IV, or an acrylate compound having a structure shown in Formula V: Wherein, X, Y, and Z are each independently selected from H or an alkyl group, and R5 to R7 are each independently selected from an alkylene group, an ether group, or an alkyleneoxy group; Optionally, X, Y, and Z are each independently selected from H or C1-C5 alkyl; Optionally, the R5 to R7 are each independently selected from C1 to C10 alkylene, C1 to C10 alkyleneoxy or C1 to C10 ether, and more preferably methylene, ether or methyleneoxy; Optionally, the acrylate reactive monomer includes any one of benzyl methacrylate, o-phenylphenoxyethyl acrylate or 3-phenoxybenzyl acrylate, or a combination of at least two thereof.

7. The UV printing ink according to any one of claims 1 to 6, wherein: The photoinitiator includes any one of benzoin diethyl ether, diphenylacetone, α-hydroxyalkyl phenone, 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexylphenylketone, 2-methyl-2-(4-morpholinyl)-1-[4-(methylthio)phenyl]-1-propanone, 2-dimethylamino-2-benzyl-1-[4-(4-morpholinyl)phenyl]-1-butanone, bis(2,4,6)-trimethylbenzoylphenylphosphine oxide or 2,4,6-trimethylbenzoyl-ethoxy-phenylphosphine oxide, or a combination of at least two thereof; Optionally, the UV printing ink further includes an additive; Optionally, the content of the auxiliary agent in the UV printing ink is 0.1 to 5 parts by weight; Optionally, the auxiliary agent includes any one or a combination of at least two of a defoamer, an inhibitor, a coupling agent or a leveling agent; Optionally, the liquid refractive index of the UV printing ink is not less than 1.55; Optionally, the refractive index of the UV printing ink after it is completely cured into a film is not less than 1.62; Optionally, the viscosity of the UV printing ink is no more than 30 cps.

8. A method for preparing the UV printing ink according to any one of claims 1 to 7, the method comprising: The UV printing ink is obtained by mixing acrylate resin, modified inorganic nanoparticle dispersion, acrylate active monomer, photoinitiator and optional auxiliary agent.

9. The preparation method according to claim 8, wherein: The mixing time is not less than 2 minutes; Optionally, the mixing is performed under stirring; Optionally, the stirring rotation speed is not less than 1500 rpm.

10. A light extraction film, comprising a base film and a UV printing ink layer, wherein a raw material of the UV printing ink layer comprises the UV printing ink according to any one of claims 1 to 7; Optionally, the UV printing ink layer is obtained by coating the UV printing ink on the base film in a printing mode using a printer and drying it; Optionally, the thickness of the UV printing ink layer is not greater than 50 μm, and more preferably 10 to 30 μm. 11 . An organic light emitting diode comprising the light extraction film according to claim 10 .

Citation Information

Patent Citations

  • Ink composition and organic electroluminescent element using same

    CN110024483A

  • High-refractive-index photosensitive resin and preparation method thereof

    CN111944077A

  • Surface-modified metal oxide nanoparticle dispersion liquid composition, method for preparing same, thin film composition, and optical thin film

    CN114249956A

  • Inorganic nanoparticle ink, light-emitting film, and display device

    CN114907724A

  • High-refractive-index ink for pure organic ink-jet printing and preparation method of high-refractive-index ink

    CN115785735A

Cited By

  • Metal medium UV printing method

    CN119898130A