Synthesis method for and use of high-silicon mordenite molecular sieve having better reactive site accessibility
By introducing mother liquor concentrate and boron into the dimethyl ether carbonylation catalyst, and subjecting it to hydrothermal and acid treatment, a high-silica mordenite molecular sieve was prepared, which solved the problem of insufficient catalyst activity and stability and achieved low-temperature, high-efficiency catalysis and longevity. Prolonged effect.
Patent Information
- Application Number
- PCT/CN2023/090800
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-26
- Publication Date
- 2024-10-31
AI Technical Summary
The existing technology's catalyst for the carbonylation of dimethyl ether to prepare methyl acetate has insufficient reactivity and stability. Especially during long-term use, it is difficult to control the acidic site of the catalyst to achieve efficient catalysis, resulting in high reaction temperature and short catalyst life.
Through the introduction of mother liquor concentrate and boron, combined with hydrothermal and acid treatment, a high-silica mordenite molecular sieve was prepared to make its pores smoother and improve the accessibility of reaction active sites. As a dimethyl ether carbonylation catalyst, it significantly reduces Change the reaction temperature and increase the conversion rate.
The low-temperature activity of the catalyst is significantly improved, the conversion rate is improved, the single-pass life of the catalyst is greatly increased, solid waste is reduced during the production process, and the cost of sewage treatment is reduced.
Smart Images

Figure CN2023090800_31102024_PF_FP_ABST
Abstract
Description
A synthesis method and application of high-silicon mordenite molecular sieve with better accessibility of reactive active sites Technical Field
[0001] The present application relates to a synthesis method of a high-silicon mordenite molecular sieve with better accessibility of reactive active sites and its application, belonging to the field of molecular sieves. Background Art
[0002] Mordenite is a crystalline microporous aluminosilicate with a 12-membered ring and an 8-membered ring pore structure, suitable acidity, and good hydrothermal stability. It has become an important catalytic material in the fields of petrochemicals and coal chemical industry, especially in the recent application of dimethyl ether carbonylation reaction to produce methyl acetate.
[0003] Methyl acetate is an important chemical product and an environmentally friendly organic solvent, widely used in the production of resins and leather. Its downstream products, such as acetic acid, acetate esters, acetic anhydride, and ethanol, are all important chemical raw materials. Methyl acetate can be hydrogenated to produce ethanol, a key organic solvent and fuel additive. As a gasoline additive, it can increase octane rating, promote combustion, and reduce pollutant emissions. Large-scale industrial production of ethanol can effectively alleviate my country's long-standing high dependence on foreign crude oil.
[0004] The technical route of carbonylating dimethyl ether to produce methyl acetate, followed by further hydrogenation to produce ethanol, has opened up an efficient path from non-petroleum-based carbon resources to the production of clean energy ethanol. Therefore, studying the catalytic reaction of carbonylating dimethyl ether to produce methyl acetate is of great significance.
[0005] In 2006, the Iglesia group first reported the carbonylation of DME catalyzed by acidic molecular sieves under halogen-free and noble metal-free conditions (Angewandte Chemie, Int. Ed. 2006, 45(10), 1617-1620). They used infrared spectroscopy to characterize the acid distribution of the molecular sieves and used probe molecules with different kinetic diameters to determine the distribution of the acid in the octahedral pores. The amount of acid was correlated with the carbonyl activity, and it was found that the carbonylation activity was related to the number of The amount of acid centers is proportional to the amount of iodine (Acc. Chem. Res. 2008, 41, 4, 559-567).
[0006] The carbonylation catalytic reaction is a highly exothermic reaction, and the catalyst needs to have high activity and stability during long-term use. Therefore, the aluminum is controlled to fall within the eight-membered ring and form a strong Acidic sites are an effective means of improving the reactivity and stability of mordenite as a dimethyl ether carbonylation catalyst. CN 201611135717.2 discloses a method for synthesizing a mordenite (MOR) molecular sieve with adjustable Benzene acid center location and distribution. The resulting MOR zeolite has Benzene acid centers preferentially located in the "side pockets" of the 8-membered rings that connect to the 12-membered ring channels. The resulting catalyst exhibits excellent adsorption and catalytic performance.
[0007] CN202011582829.9 discloses a preparation method and application of high silicon-aluminum ratio silk-denite. Through pre-crystallization, a high silicon-aluminum ratio precursor and the effect of structure-guided sol are obtained to obtain silk-denite with a silicon-aluminum ratio of 15 to 50. It has excellent performance in preparing methyl acetate by dimethyl ether carbonylation.
[0008] Patent CN108160100A uses pyridine and nitrate to modify the twelve-membered ring and eight-membered ring of HMOR, respectively, improving the stability of the catalyst. CN202111644362.0 discloses a method for synthesizing a mordenite molecular sieve with controlled aluminum placement, where the aluminum placement ratio of the eight-membered ring is greater than 50%. Patent CN201510117253.1 discloses a method for synthesizing a mordenite with both microporous and mesoporous structures.
[0009] Liu et al. obtained a mordenite zeolite with 32% of eight-membered ring acidic sites through selective ion exchange, achieving a DME conversion of 50% and a service life of over 210 hours (Catal. Sci. Technol., 2020, 10, 4663-4672). Liu et al. (Catalysis Communications, 2020, 147, 106161) introduced 1,3-dimethylimidazolium ions into MOR zeolite to selectively remove acid sites in the twelve-membered ring (12MR) channels, significantly improving stability and activity. However, this significantly increased the production cost of the catalyst.
[0010] Summary of the Invention
[0011] The present invention provides a method for synthesizing a high-silicon mordenite molecular sieve with improved accessibility to reactive active sites. This mordenite molecular sieve utilizes mother liquor concentrate and introduces boron into the synthesis system. Subsequent hydrothermal and / or acid treatment further enhances the pores of the zeolite and improves the accessibility of the reactive active sites. When used as a catalyst for the carbonylation of dimethyl ether to methyl acetate, the dimethyl ether conversion reaction temperature is significantly reduced and the conversion rate is improved, demonstrating improved active site accessibility. Its low-temperature activity is significantly superior to that of a mordenite molecular sieve synthesized in a one-step process under the same conditions.
[0012] According to a first aspect of the present application, a method for synthesizing high-silicon mordenite molecular sieve with better accessibility of reactive active sites is provided.
[0013] A method for synthesizing a high-silicon mordenite molecular sieve with better accessibility of reactive active sites comprises the following steps:
[0014] S1. Obtaining a silicon-boron precursor made from a mother liquor concentrate and a boron source;
[0015] S2, obtaining an alkaline solution containing aluminum;
[0016] S3, hydrothermally crystallizing the mixture containing the silicon boron precursor and the alkaline solution to obtain a product;
[0017] S4. The product is subjected to heat treatment and / or acid treatment under water vapor to obtain the high-silicon mordenite molecular sieve.
[0018] The atmosphere for heat treatment includes air and nitrogen.
[0019] Optionally, the silicon-boron precursor is prepared as follows:
[0020] The material I containing silicon source, boron source, template A, water and mother liquor concentrate is stirred and aged to prepare the silicon-boron precursor.
[0021] Optionally, the alkaline solution is prepared as follows:
[0022] The material II containing an aluminum source, an alkali source, a template B and water is stirred and aged to prepare the alkaline solution.
[0023] Optionally, in step S3, the mother liquor containing the product is separated and distilled to obtain the mother liquor concentrate.
[0024] The mother liquor concentrate is prepared as follows:
[0025] 1) filtering and separating the molecular sieve solid product synthesized for the first time, and then recovering the mother liquor;
[0026] 2) Analyze the content of each component in the recovered mother liquor;
[0027] 3) The mother liquor is placed in a sealed container and heated to distill off a certain amount of water to obtain a concentrated solution;
[0028] 4) Analyze the content of each component in the mother liquor concentrate.
[0029] Optionally, in step S3, the conditions for hydrothermal crystallization are as follows:
[0030] The temperature is 120-200°C;
[0031] The time is 12 to 120 hours.
[0032] Optionally, the hydrothermal crystallization conditions include: a crystallization temperature of 60 to 150° C., and a crystallization time of 2 to 15 hours.
[0033] Optionally, in step S4, the heat treatment conditions are as follows:
[0034] Temperature is 80-200℃;
[0035] The time is 0.5 to 2.0 hours.
[0036] Optionally, the acid treatment comprises placing the product in an acid solution of a certain concentration.
[0037] Optionally, the mass ratio of the product to the volume of the acid is 3 to 10:1.
[0038] Optionally, the acid is selected from at least one of sulfuric acid, nitric acid, hydrochloric acid, citric acid, acetic acid, and the like.
[0039] Optionally, the conditions for the acid treatment are as follows:
[0040] Temperature is 55-85℃;
[0041] The time is 0.5 to 2.5 hours.
[0042] Optionally, the silicon source is selected from at least one of sol, water glass, white carbon black, and diatomaceous earth.
[0043] Optionally, the boron source is selected from boric acid.
[0044] Optionally, the template A is selected from at least one of hexadecyltrimethylammonium bromide, dodecyltrimethylammonium bromide, tetrapropylammonium bromide, tetraethylammonium bromide, tetramethylammonium bromide, hexadecyltrimethylammonium chloride, dodecyltrimethylammonium chloride, tetrapropylammonium chloride, tetraethylammonium chloride, tetramethylammonium chloride, hexadecyltrimethylammonium hydroxide, dodecyltrimethylammonium hydroxide, tetrapropylammonium hydroxide, tetraethylammonium hydroxide, tetramethylammonium hydroxide, triethylamine, isopropylamine, diisopropylamine, triisopropylamine, n-butylamine, cyclohexylamine, caprolactam, hexamethyleneimine, heptamethyleneimine, cycloheptaneamine, and cyclopentaneamine.
[0045] Optionally, the molar ratio of the raw materials in the material I is:
[0046] M2O:SiO2:B2O3:Template A:H2O=(0.06~0.50):1:(0.01~0.15):(0.01~0.12):(10~150).
[0047] Optionally, the aluminum source is selected from at least one of sodium aluminate, aluminum isopropoxide, aluminum hydroxide, and aluminum sulfate.
[0048] Optionally, the alkali source is selected from at least one of alkali metal hydroxides and oxides.
[0049] Optionally, the alkali source is selected from at least one of potassium hydroxide and sodium hydroxide.
[0050] Optionally, the template B is selected from at least one of hexadecyltrimethylammonium bromide, dodecyltrimethylammonium bromide, tetrapropylammonium bromide, tetraethylammonium bromide, tetramethylammonium bromide, hexadecyltrimethylammonium chloride, dodecyltrimethylammonium chloride, tetrapropylammonium chloride, tetraethylammonium chloride, tetramethylammonium chloride, hexadecyltrimethylammonium hydroxide, dodecyltrimethylammonium hydroxide, tetrapropylammonium hydroxide, tetraethylammonium hydroxide, tetramethylammonium hydroxide, triethylamine, isopropylamine, diisopropylamine, triisopropylamine, n-butylamine, cyclohexylamine, caprolactam, hexamethyleneimine, heptamethyleneimine, cycloheptaneamine, and cyclopentaneamine.
[0051] Optionally, the gel molar ratio after adding material II is:
[0052] SiO2: Al2O3: B2O3: M2O: H2O: T=1: (0.01~0.1): (0.02~0.45): (0.05~0.3): (10~50): (0.01~0.30).
[0053] Optionally, the aging conditions are as follows:
[0054] Temperature is 40-120℃;
[0055] The time is 4 to 12 hours.
[0056] According to one embodiment of the present application, a method for synthesizing a high-silicon mordenite molecular sieve with better accessibility of reactive sites is provided, the method comprising at least the following steps:
[0057] (1) Preparation of silicon-boron precursor: a silicon source, a boron source, a template agent A, water and a mother liquor concentrate are stirred and aged in a certain proportion under certain temperature conditions to prepare a silicon-boron precursor; preparation of alkaline solution: an aluminum source, an alkali source, a template agent B and water are stirred and aged in a certain proportion under certain temperature conditions to prepare an alkaline solution;
[0058] (2) The alkaline solution is added to the silicon boron precursor in a certain proportion, and a hydrothermal crystallization reaction is carried out in a stainless steel autoclave. The product is washed and dried, and then subjected to acid hydrothermal treatment to obtain a high-silicon mordenite molecular sieve with better reaction accessibility; the mother liquor after the product is separated is distilled to obtain a mother liquor concentrate, which can be used for the preparation of the above-mentioned silicon boron precursor after component analysis;
[0059] The preparation conditions of the silicon-boron precursor and the alkaline solution in step (1) of synthesizing the mordenite according to the method are: temperature of 40 to 120° C. and time of 4 to 12 hours;
[0060] In step (2), the hydrothermal and acid treatment refers to heat-treating the molecular sieve powder in the presence of water vapor and then performing acid treatment.
[0061] According to a second aspect of the present application, a high-silicon mordenite molecular sieve is provided.
[0062] The high-silicon mordenite molecular sieve obtained by the above-mentioned synthesis method has a silicon-aluminum ratio of 15-85.
[0063] Optionally, the total acid content of the high-silica mordenite molecular sieve is 550-700 μmol / g.
[0064] Optionally, the specific surface area of the high-silicon mordenite molecular sieve is 350 to 450 m 2 / g.
[0065] According to a third aspect of the present application, an application of a high-silicon mordenite molecular sieve is provided.
[0066] The high-silica mordenite molecular sieve obtained by the above-mentioned synthesis method and / or the application of the high-silica mordenite molecular sieve as a catalyst in the carbonylation of dimethyl ether.
[0067] The beneficial effects of this application include:
[0068] 1) The present application provides a method for synthesizing a high-silica mordenite molecular sieve with better accessibility to reactive sites, which improves the acid strength and the ratio of 8-membered cyclic acids while also improving the low-temperature activity of the reaction. The method also significantly reduces solid waste from molecular sieve synthesis, reduces wastewater treatment costs for scaled-up molecular sieve production, significantly reduces the initial reaction temperature compared to current conditions, and significantly increases the catalyst's single-pass life.
[0069] 2) The application of a high-silica mordenite molecular sieve provided in this application as a catalyst for the carbonylation of dimethyl ether to methyl acetate significantly reduces the conversion reaction temperature of dimethyl ether and improves the conversion rate, indicating that its active site accessibility is better. Its low-temperature activity is significantly better than that of a mordenite molecular sieve synthesized in a one-step process under the same conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0070] FIG1 is the XRD of Examples 2, 4, 6 and Comparative Example 1 of the present application. DETAILED DESCRIPTION
[0071] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.
[0072] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.
[0073] Dimethyl ether adsorption experiments were conducted on a Mettler-Toledo thermogravimetric analyzer (TGA / DSC 3+). Samples (approximately 30 mg) were dehydrated under high vacuum at 350°C for 6 hours prior to testing. The samples were then transferred to the thermogravimetric analyzer and stabilized at 50°C. Dimethyl ether (5.0 v% DME, balanced in Ar) was then introduced into the system for adsorption.
[0074] Fourier transform infrared spectroscopy
[0075] IR fitting,IR spectra were performed using a Bruke Tensor II spectrometer equipped with a vacuum in-situ cell. First, 5 mg of powdered sample was pressed into The self-supporting disc was then placed in an in-situ infrared cell and pretreated at 400°C (heating rate of 5°C / min) under vacuum for 1 hour to remove water from the sample. After pretreatment, the sample was cooled to room temperature and infrared spectroscopy was performed in the scanning range of 4000-600cm -1 , the number of scans is 32, and the resolution is 4cm -1 .
[0076] Nitrogen physical adsorption and desorption
[0077] Nitrogen physical adsorption experiments were conducted on a Quantachrome Autosorb-iQ instrument. First, 0.05 g of a molecular sieve sample (20-40 mesh) was weighed into a physical adsorption tube. Prior to testing, the sample was pretreated at 350°C under vacuum for 6 hours to remove adsorbed water and other surface substances. Subsequently, nitrogen physical adsorption and desorption tests were performed at a liquid nitrogen temperature of 77 K. The specific surface area of the sample was calculated using the BET equation, and the total pore volume of the molecular sieve was calculated using the nitrogen adsorption at the highest relative pressure point. The micropore specific surface area and micropore volume of the sample were calculated using the t-plot method. The pore size distribution of the sample was calculated using the BJH method. The pore width and total pore distribution were calculated using the DFT method.
[0078] X-ray diffractometer (XRD)
[0079] The sample test conditions of the SmartLab SE X-ray diffractometer of Rigaku Corporation are as follows: Cu target, Kα radiation (λ=0.1542 nm), tube voltage 40 kV, tube current 30 mA, scanning rate 20° / min, and range 3° to 55°.
[0080] X-ray fluorescence spectroscopy (XRF)
[0081] The elemental composition and content of the samples were analyzed using a ZSX Primus III+ fluorescence spectrometer from Rigaku Corporation. Before testing, the molecular sieve samples were fully ground into fine powder, pressed into pellets at 30 MPa, and then placed in a test cell for analysis.
[0082] Ammonia temperature-programmed desorption (NH3-TPD)
[0083] Chemical adsorption analysis was performed using an AMI300 chemical adsorption instrument from AMI (USA). A 0.1g sample of molecular sieve was placed in a U-shaped quartz tube and pretreated in a He atmosphere at 600°C for 1 hour. The sample was then cooled to 150°C and introduced into an NH3 / He mixture for 0.5 hour. Physically adsorbed NH3 was then removed by purging under a He atmosphere for 0.5 hour. After the baseline stabilized, the sample was heated to 700°C at a rate of 10°C / min. The desorbed NH3 was recorded using a thermal conductivity detector (TCD).
[0084] Reaction performance evaluation:
[0085] Catalyst evaluation was performed in a high-pressure fixed-bed reactor. The reactor tube was constructed of 316L stainless steel with an inner diameter of 9 mm. The catalyst loading was 1.0 g and the size was 20-40 mesh. The feed gas was (DME:CO:H2=5:35:60), the reaction pressure was 2.0 MPa, and the hourly space velocity was 1800 mL / g. cat The reaction temperature was 180°C, and the gas products after the reaction were analyzed online on a Pano A60 or 1949 gas chromatograph with an HP-PLOT / Q capillary column and an FID detector.
[0086] The conversion rate and selectivity in the examples of this application are calculated as follows:
[0087] Dimethyl ether conversion rate = [(moles of dimethyl ether carbon in the feed gas) - (moles of dimethyl ether carbon in the product)] ÷ (moles of dimethyl ether carbon in the feed gas) × (100%);
[0088] Methyl acetate selectivity = (2 / 3) × (mole number of carbon atoms of methyl acetate in the product) ÷ [(mole number of carbon atoms of dimethyl ether in the feed gas) - (mole number of carbon atoms of dimethyl ether in the product)] × (100%).
[0089] Example 1
[0090] Preparation of silicon-boron precursor:
[0091] With NaOH as the alkali source, boric acid as the boron source, sodium silicate as the silicon source, aluminum isopropoxide as the aluminum source, and hexadecyltrimethylammonium chloride as the template A, a certain amount of the mother liquor concentrate was taken, mixed, and transferred to a reactor. After aging at 100°C for 8 hours, a silicon-boron precursor was prepared, whose molar composition was SiO2:B2O3:Na2O:H2O:A=1:0.028:0.08:40:0.02;
[0092] Preparation of alkaline solution:
[0093] Aluminum isopropoxide, tetraethylammonium hydroxide and water are mixed in a molar composition of Al2O3:Na2O:H2O:B=1:9.64:535:3.2, stirred evenly, aged at 60°C for 2 hours and then cooled to room temperature to prepare an alkaline solution;
[0094] Synthesis of high-silica mordenite molecular sieve with better accessibility of reactive sites:
[0095] A certain amount of silicon boron precursor and alkaline solution are mixed, stirred for a period of time after addition, heated to 170°C and maintained for 72 hours to obtain a product. The mother liquor after product separation is distilled to obtain a mother liquor concentrate, which can be used for the preparation of the above-mentioned silicon boron precursor after component analysis, and then acid treatment is performed to obtain the high-silicon mordenite molecular sieve.
[0096] Comparative Example 1
[0097] The experimental steps were the same as those in Example 1, except that no boron source was added when preparing the silicon-boron precursor.
[0098] Examples 2-6
[0099] The preparation process of Examples 2-6 is the same as that of Example 1. The silicon boron precursor, raw material types and ratios in the alkaline solution, pre-crystallization temperature and time, and crystallization temperature and time of the prepared samples are shown in Table 1. The subsequent treatment materials and methods are detailed in Table 2.
[0100] Table 1
[0101] Table 2
[0102] Analysis example 1
[0103] The molecular sieve catalysts obtained in Examples 1-6 and Comparative Example 1 were subjected to measurements of silicon-aluminum ratio, total TPD acid content, and physical adsorption. The results are shown in Table 3.
[0104] Table 3
[0105] The molecular sieve catalysts obtained in Examples 1-6 and Comparative Example 1 were subjected to dimethyl ether gravimetric adsorption experiments. The results are shown in Table 4.
[0106] Table 4
[0107] It can be seen from the above characterization results that after the synthesis and treatment method of the present application, the total acid content of the catalyst TPD increases, and the equilibrium time of the catalyst adsorption time for dimethyl ether becomes shorter, which makes the reaction accessibility of the catalyst better. For the carbonylation reaction, at the same reaction temperature, the dimethyl ether conversion rate increases.
[0108] The above descriptions are merely a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application discloses the preferred embodiments as above, they are not intended to limit the present application. Any technical personnel familiar with the present profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A method for synthesizing a high-silicon mordenite molecular sieve with better accessibility of reactive active sites, characterized in that: The following steps are involved: S1, obtaining a silicon-boron precursor made from a mother liquor concentrate and a boron source; S2, obtaining an alkaline solution containing aluminum; S3, hydrothermally crystallizing a mixture containing the silicon-boron precursor and the alkaline solution to obtain a product; S4, subjecting the above product to heat treatment and / or acid treatment under water vapor to obtain the high-silicon mordenite molecular sieve.
2. The synthesis method according to claim 1, characterized in that The preparation of the silicon-boron precursor is as follows: The material I containing silicon source, boron source, template A, water and mother liquor concentrate is stirred and aged to prepare the silicon-boron precursor.
3. The synthesis method according to claim 1, characterized in that The preparation of the alkaline solution is as follows: The material II containing an aluminum source, an alkali source, a template agent B and water is stirred and aged to prepare the alkaline solution.
4. The synthesis method according to claim 1, characterized in that In step S3, the mother liquor containing the product is separated and distilled to obtain the mother liquor concentrate; In step S3, the conditions for hydrothermal crystallization are as follows: The temperature is 120-200°C; The time is 12 to 120 hours.
5. The synthesis method according to claim 1, characterized in that In step S4, the conditions for heat treatment are as follows: The temperature is 80-200°C; Time is 0.5~2.0h; The acid treatment comprises placing the product in an acid: The mass ratio of the product to the volume of the acid is 3 to 10:1; The acid is selected from at least one of sulfuric acid, nitric acid, hydrochloric acid, citric acid, acetic acid, etc.; The conditions for the acid treatment are as follows: Temperature is 55-85℃; The time is 0.5 to 2.5 hours.
6. The synthesis method according to claim 2, characterized in that The silicon source is selected from at least one of silica sol, water glass, white carbon black and diatomaceous earth; The boron source is selected from boric acid; The template agent A is selected from at least one of hexadecyltrimethylammonium bromide, dodecyltrimethylammonium bromide, tetrapropylammonium bromide, tetraethylammonium bromide, tetramethylammonium bromide, hexadecyltrimethylammonium chloride, dodecyltrimethylammonium chloride, tetrapropylammonium chloride, tetraethylammonium chloride, tetramethylammonium chloride, hexadecyltrimethylammonium hydroxide, dodecyltrimethylammonium hydroxide, tetrapropylammonium hydroxide, tetraethylammonium hydroxide, tetramethylammonium hydroxide, triethylamine, isopropylamine, diisopropylamine, triisopropylamine, n-butylamine, cyclohexylamine, caprolactam, hexamethyleneimine, heptamethyleneimine, cycloheptylamine, and cyclopentylamine; The molar ratio of the raw materials in the material I is: M2O:SiO2:B2O3:Template A:H2O=(0.06~0.50):1:(0.01~0.15):(0.01~0.12):(10~150).
7. The synthesis method according to claim 3, characterized in that The aluminum source is selected from at least one of sodium aluminate, aluminum isopropoxide, aluminum hydroxide, aluminum sulfate, etc.; The alkali source is selected from at least one of alkali metal hydroxides and oxides; The template agent B is selected from hexadecyltrimethylammonium bromide, dodecyltrimethylammonium bromide, tetrapropylammonium bromide, tetraethylammonium bromide, tetramethylammonium bromide, hexadecyltrimethylammonium chloride, dodecyltrimethylammonium chloride, tetrapropylammonium chloride, tetraethylammonium chloride, At least one of tetramethylammonium chloride, hexadecyltrimethylammonium hydroxide, dodecyltrimethylammonium hydroxide, tetrapropylammonium hydroxide, tetraethylammonium hydroxide, tetramethylammonium hydroxide, triethylamine, isopropylamine, diisopropylamine, triisopropylamine, n-butylamine, cyclohexylamine, caprolactam, hexamethyleneimine, heptamethyleneimine, cycloheptylamine, and cyclopentylamine; After adding material II, the gel molar ratio is: SiO2: Al2O3: B2O3: M2O: H2O: T=1: (0.01~0.1): (0.02~0.45): (0.05~0.3): (10~50): (0.01~0.30).
8. The synthesis method according to claim 2 or 3, characterized in that: The aging conditions are as follows: The temperature is 40-120°C; The time is 4 to 12 hours.
9. The high-silicon mordenite molecular sieve obtained by the synthesis method according to any one of claims 1 to 8, characterized in that: The silicon-aluminum ratio of the high-silicon mordenite molecular sieve is 15 to 85; The total acid content of the high-silica mordenite molecular sieve is 550-700 μmol / g; The specific surface area of the high-silicon mordenite molecular sieve is 400-450 m 2 / g.
10. Use of the high-silicon mordenite molecular sieve obtained by the synthesis method according to any one of claims 1 to 8 or the high-silicon mordenite molecular sieve according to claim 9 as a catalyst in the carbonylation of dimethyl ether.
Citation Information
Patent Citations
Preparation method of MCM-49 zeolite molecular sieve
CN104402021A
Preparation method for mordenite molecular sieve
CN111977665A
Synthetic method of lamellar mordenite molecular sieve
CN114229864A
Preparation method of mordenite molecular sieve
CN114291823A
Mordenite molecular sieve as well as preparation method and application thereof
CN114572997A
Cited By
Preparation method and application of high-silicon mordenite molecular sieve
CN116588949A
Preparation method and application of high-silicon mordenite molecular sieve
CN116588949B
Purification method of photoinitiator FMT crude product
CN119462780A
Process for preparing Ti-Beta zeolite based on gas-phase transport method and recyclable organic base
CN120229734A
Molecular sieve and preparation method thereof
CN120793958A