Foamed rubber shoe material and preparation method therefor
By adding triterpene saponins, n-butanol and unsaturated fatty acids to the rubber compound, combined with pre-vulcanized rubber and modified glass fiber, the problem of bubbles breaking through the cell walls during the vulcanization process was solved, and the rubber compound was fully foamed and shoe-shaped. The material has good breathability and sweat-wicking effect.
Patent Information
- Application Number
- PCT/CN2023/128351
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-24
- Filing Date
- 2023-10-31
- Publication Date
- 2024-10-31
AI Technical Summary
During the vulcanization process of existing foamed rubber shoe materials, bubbles break through the cell walls, causing the cell walls to collapse, resulting in densification of the rubber material and affecting the full foaming effect.
Triterpene saponins, n-butanol and unsaturated fatty acids are added to the rubber compound, and dicumyl peroxide is used to promote the copolymerization reaction to enhance the strength of the cell walls. Combined with pre-vulcanized rubber and modified glass fiber, the vulcanization process parameters are optimized to reduce The possibility of bubbles breaking through the cell walls.
Significantly improves the strength of the air bubble wall, reduces the collapse of the cell wall, achieves full foaming of the rubber material, and improves the breathable and sweat-wicking effect of the shoe material.
Smart Images

Figure PCTCN2023128351-FTAPPB-I100001 
Figure PCTCN2023128351-FTAPPB-I100002 
Figure PCTCN2023128351-FTAPPB-I100003
Abstract
Description
Foamed rubber shoe material and preparation method thereof Technical Field
[0001] The present application relates to the technical field of foamed rubber shoe materials, and more specifically, to a foamed rubber shoe material and a preparation method thereof. Background Art
[0002] Foaming materials refer to materials containing a certain number of pores and are composed of a continuously distributed solid phase and a fluid phase (usually gas) distributed within the solid phase. Polymer foaming materials are an important type of foaming material, mainly including plastic foaming materials and rubber foaming materials. Rubber foaming materials are usually prepared by adding a foaming agent to the rubber matrix. During the vulcanization process of the rubber, the foaming agent undergoes physical or chemical changes to form gas. The gas is then trapped in the rubber compound under the action of vulcanization cross-linking, thereby forming a pore structure.
[0003] In the related art, a foamed rubber shoe material is obtained by vulcanizing and foaming a rubber shoe base. The rubber shoe base is composed of a rubber sheet and a fabric, with the fabric attached to the surface of the rubber sheet. Currently, to improve the foaming performance of rubber, multiple foaming agents are usually compounded, such as chemical foaming agents and physical foaming agents with different decomposition temperatures. This allows the different foaming agents to effectively foam during the heating process, thereby improving the foaming efficiency.
[0004] However, the related technologies also have the following problems: for example, when the foaming agent uses a low-boiling-point chemical foaming agent or a variety of physical foaming agents, a large number of bubbles will be generated during the foaming and vulcanization process. The released bubbles also have a softening effect on the rubber material. At the same time, the bubbles can easily break through the pore wall and cause the pore wall to collapse, resulting in the densification of the rubber material, which is not conducive to the full foaming of the rubber material.
[0005] Summary of the Invention
[0006] When implementing the technical solutions in the related art, bubbles easily break through the cell walls, causing the cell walls to collapse, which is not conducive to the full foaming of the rubber material. To improve this defect, the present application provides a foamed rubber shoe material and a preparation method thereof.
[0007] In a first aspect, the present application provides a foam rubber shoe material, which adopts the following technical solution:
[0008] A foamed rubber shoe material is obtained by foaming, vulcanizing and cutting a rubber shoe blank, the rubber shoe blank comprising a rubber sheet and a cloth attached to the surface of the rubber sheet. The rubber sheet is processed from a premixed rubber material in an open mill, the premixed rubber material comprising the following components in parts by weight: 44-48 parts of a rubber matrix, 24-28 parts of a filler, 5-7 parts of an oil, 4-5 parts of a vulcanizing aid, 1.8-2.2 parts of an antioxidant, 0.5-0.7 parts of an accelerator, 4-6 parts of a triterpenoid saponin, 8-12 parts of n-butanol, 3-5 parts of an unsaturated fatty acid, 7-9 parts of sulfur, 1.6-2.4 parts of dicumyl peroxide, and 10-14 parts of a foaming agent; the foaming agent comprises 4,4'-oxybisbenzenesulfonylhydrazine, petroleum ether, ethylene dichloride, and at least one bicarbonate. The rubber matrix comprises natural rubber.
[0009] By adopting the above technical solution, compared with the related art, the present application further adds triterpenoid saponins, n-butanol, unsaturated fatty acids and diisopropylbenzene peroxide into the rubber material. The main structure of the sapogenin in the triterpenoid saponins is similar to that of natural rubber, so the triterpenoid saponins have a good binding force with natural rubber; the triterpenoid saponins are soluble in n-butanol, which can improve the migration performance of the triterpenoid saponins in the rubber material system, and the n-butanol itself can be foamed by vaporization, playing the role of a foaming agent; the triterpenoid saponins and unsaturated fatty acids migrate to the interface between the cell wall and the continuous phase of the rubber, and The hydrophobic ends are arranged within the continuous rubber phase, while the hydrophilic ends form hydrogen bonds on the inner side of the pore walls. Simultaneously, during the foaming and vulcanization process, triterpenoid saponins, under the action of dicumyl peroxide, copolymerize with unsaturated fatty acids and natural rubber on the outer side of the pore walls. The copolymerization reaction on the outer side of the pore walls synergizes with the hydrogen bonds on the inner side of the pores, significantly increasing the strength of the bubble pore walls and helping to reduce the possibility of bubbles breaking through the pore walls and causing pore wall collapse. This overcomes the problem of the rubber compound being prone to densification due to pore wall collapse and facilitates full foaming of the rubber compound. Due to the improved foaming effect, the air pores created in the shoe material have greater permeability, resulting in better ventilation and perspiration wicking properties.
[0010] Preferably, the unsaturated fatty acid molecule contains 2-4 carbon-carbon double bonds.
[0011] By adopting the above technical solution, the number of carbon-carbon double bonds in the unsaturated fatty acid molecules is preferably 2-4. Unsaturated fatty acids containing multiple carbon-carbon double bonds have more copolymerization sites than monoolefinic acids, which helps promote the copolymerization reaction during the foaming and vulcanization stage, thereby reducing the possibility of bubbles breaking through the pore wall and promoting the full foaming of the rubber compound.
[0012] Preferably, the unsaturated fatty acid is farnesic acid.
[0013] By adopting the above technical solution, the alkyl group of farnesic acid is mainly composed of isoprene units, which has good compatibility with triterpenoid saponins and natural rubber, helps to improve the strength of the pore wall, and fully promotes the foaming of the rubber compound.
[0014] Preferably, the rubber matrix further comprises pre-vulcanized rubber, the weight ratio of the natural rubber to the pre-vulcanized rubber is 10:(1-2), and the pre-vulcanized rubber is prepared according to the following method:
[0015] (1) mixing zinc oxide, stearic acid, an accelerator, an antioxidant and sulfur with styrene-butadiene rubber to obtain a styrene-butadiene rubber mixture;
[0016] (2) taking a portion of the styrene-butadiene rubber mixture, selecting vulcanization process parameters and performing vulcanization processing, and measuring the theoretical positive vulcanization time of the styrene-butadiene rubber mixture under the selected vulcanization process parameters;
[0017] (3) vulcanizing the remaining styrene-butadiene rubber mixture according to the vulcanization process parameters selected in step (2), wherein the vulcanization time is set at 20-70% of the theoretical positive vulcanization time measured in step (2), and pre-vulcanized rubber is obtained after the vulcanization process is completed.
[0018] By adopting the above technical solution, the present application uses styrene-butadiene rubber as raw material, and on the basis of the theoretical vulcanization time measured in step (2), the vulcanization time is selected as 20-70% of the theoretical vulcanization time in step (3), thereby obtaining a pre-vulcanized rubber with a certain degree of crosslinking. The vulcanization of the pre-vulcanized rubber is not thorough, but still has processability and can continue to vulcanize under suitable conditions. In the preparation process of the premixed rubber, the remaining sulfur in the pre-vulcanized rubber can cause the natural rubber to also undergo a certain degree of vulcanization. In addition, the pre-vulcanized rubber itself has formed a certain crosslinking structure. Therefore, the rubber matrix in the rubber material has a certain degree of crosslinking at the beginning of foaming vulcanization, thereby improving the barrier effect of the rubber material on gas, reducing the possibility of bubbles breaking through the pore wall and causing the pore wall to collapse, and is conducive to the full foaming of the rubber material.
[0019] Preferably, in step (3) of preparing the pre-vulcanized rubber, the vulcanization processing time is set according to 28-52% of the theoretical positive vulcanization time measured in step (2).
[0020] By adopting the above technical solution, as the vulcanization time of the pre-vulcanized rubber is extended, the cross-linking degree of the pre-vulcanized rubber also increases. The vulcanization time is closely related to the degree of exchange. The pre-vulcanized rubber of this application needs to have an appropriate degree of cross-linking, which can effectively play a role in isolating air and improve the problem of bubbles easily breaking during the exchange vulcanization process; at the same time, the degree of cross-linking should not be too large, because the pre-vulcanized rubber with too large a cross-linking degree is not easy to disperse evenly in the natural rubber. Therefore, the vulcanization time is set between 28-52% of the theoretical positive vulcanization time.
[0021] Preferably, the filler comprises modified glass fiber, and the modified glass fiber is a glass fiber with amino groups grafted on the surface.
[0022] By adopting the above technical solution, the present application adds modified glass fiber to the rubber compound. The amino groups on the surface of the modified glass fiber promote the vulcanization and cross-linking of the rubber, helping to overcome the delayed effect of 4,4'-oxybisbenzenesulfonylhydrazine on rubber vulcanization. This improves the matching degree between the vulcanization process and the foaming process, reduces the possibility of bubbles breaking through the pore walls and causing pore wall collapse, and promotes sufficient foaming of the rubber compound.
[0023] Preferably, the modified glass fiber is prepared as follows:
[0024] (1) adding a silane coupling agent to water to obtain a silane-modified liquid, which is set aside; heating and degreasing the glass fiber, which is set aside; the silane coupling agent includes γ-aminopropyltriethoxysilane, and the mass fraction of the γ-aminopropyltriethoxysilane in the silane-modified liquid is 2.5-4.5%;
[0025] (2) Adding glass fiber to the silane modification liquid, stirring under nitrogen protection, and heating to 70-75°C, then keeping warm for 2-3 hours. After the insulation is completed, filter out the glass fiber, wash and dry the taken out glass fiber to obtain modified glass fiber.
[0026] By adopting the above technical solution, the present application obtains modified glass fiber by grafting amino groups onto the surface of glass fiber through treatment with γ-aminopropyltriethoxysilane and utilizing the coupling effect between the silane coupling agent and the glass fiber.
[0027] Preferably, in the method for preparing the modified glass fiber, the silane coupling agent used further includes vinyltriethoxysilane, and the mass fraction of the vinyltriethoxysilane in the silane modification solution is 3.8-5.4%.
[0028] By adopting the above technical solution, vinyl triethoxysilane can introduce vinyl groups onto the surface of modified glass fibers. This introduced vinyl group, under the action of dicumyl peroxide, copolymerizes with the unsaturated bonds in the rubber matrix, achieving a bond between the fiber and the rubber matrix. This helps limit the softening effect of bubbles on the rubber compound, and within an appropriate dosage range, helps improve the foaming effect of the rubber compound. Due to this improved foaming effect, the air pores created in the shoe material have greater permeability, resulting in better ventilation and perspiration wicking properties.
[0029] Preferably, the amount of the modified glass fiber is 0.8-1.2% of the weight of the rubber matrix.
[0030] By adopting the above technical solution, the amount of modified glass fiber is optimized, which helps to limit the softening effect of bubbles on the rubber compound and improve the foaming effect of the rubber compound.
[0031] In a second aspect, the present application provides a method for preparing a foamed rubber shoe material, which adopts the following technical solution.
[0032] A method for preparing a foamed rubber shoe material comprises the following steps:
[0033] (1) putting a rubber matrix, a filler, an oil, an antioxidant, a vulcanizing agent, n-butanol, a triterpenoid saponin, and an unsaturated fatty acid into an internal mixer and mixing them, and then draining the rubber to obtain a masterbatch; mixing 4,4'-oxybisbenzenesulfonylhydrazine, petroleum ether, dichloroethane, and bicarbonate, and then stirring, and then homogenizing to obtain a foaming agent for standby use;
[0034] (2) mixing a masterbatch, an accelerator, sulfur, dicumyl peroxide, and a foaming agent to obtain a premixed rubber material, and performing thin-pass plasticizing on the premixed rubber material in an open mill to obtain a rubber sheet;
[0035] (3) attaching cloth to the surface of the rubber sheet to obtain a rubber shoe blank, transferring the rubber shoe blank to a vulcanization device for foaming and vulcanization, and then cutting to obtain a foamed rubber shoe material.
[0036] By adopting the above technical solution, in the preparation method of the present application, a masterbatch and a foaming agent are first prepared separately, and then the masterbatch and the foaming agent are mixed to obtain a premixed rubber material. After further milling, a rubber sheet is obtained. Subsequently, a fabric is attached to the surface of the rubber sheet and foamed and vulcanized to obtain a foamed rubber shoe material. In the preparation method of the present application, the hydrophilic groups of the triterpenoid saponins and unsaturated fatty acids form hydrogen bonds on the inner side of the pore walls and copolymerize with the rubber matrix on the outer side of the pore walls, thereby reducing the possibility of bubbles breaking through the pore walls and causing pore wall collapse. This overcomes the defect of the rubber material being easily densified due to pore wall collapse and promotes sufficient foaming of the rubber material.
[0037] In summary, this application has the following beneficial effects:
[0038] 1. While the rubber compound is being foamed and vulcanized, the copolymerization reaction occurring on the outside of the pore wall and the hydrogen bonding occurring on the inside of the pore wall jointly improve the strength of the pore wall, thereby reducing the possibility of bubbles breaking through the pore wall and causing the pore wall to collapse, overcoming the defect that the rubber compound is easily densified due to the collapse of the pore wall, and facilitating the full foaming of the rubber compound.
[0039] 2. In this application, farnesic acid is preferably used as the unsaturated fatty acid. The alkyl group of farnesic acid is mainly composed of isoprene units, which has good compatibility with triterpenoid saponins and natural rubber. By using farnesic acid, the copolymerization effect between the unsaturated fatty acid, triterpenoid saponins, and natural rubber can be further improved, which helps to increase the cell wall strength and fully promote the foaming of the rubber compound.
[0040] 3. The method of the present application first prepares a masterbatch and a foaming agent, then mixes the masterbatch and the foaming agent to obtain a premixed rubber material. The premixed rubber material is then milled to obtain a rubber sheet. Subsequently, a fabric is attached to the surface of the rubber sheet and subjected to foaming and vulcanization to obtain a foamed rubber shoe material. DETAILED DESCRIPTION
[0041] The present application is further described in detail below with reference to the Examples, Preparation Examples and Comparative Examples. The raw materials involved in the present application can all be obtained commercially.
[0042] Preparation example of pre-vulcanized rubber
[0043] The following is an explanation using Preparation Example 1.
[0044] Preparation Example 1
[0045] In this preparation example, the pre-vulcanized rubber was prepared according to the following method:
[0046] (1) 100 kg of styrene-butadiene rubber (SBR) was mixed with additives to obtain a SBR mixture; the additives included 5 kg of zinc oxide, 5 kg of stearic acid, 1.2 kg of accelerator, 1 kg of antioxidant, and 2 kg of sulfur;
[0047] (2) taking out a portion accounting for 5% of the total weight of the styrene-butadiene rubber mixture, performing a vulcanization process at a temperature of 150° C., and measuring the theoretical positive vulcanization time of the styrene-butadiene rubber mixture;
[0048] (3) vulcanizing the remaining styrene-butadiene rubber mixture according to the vulcanization process parameters selected in step (2), and setting the vulcanization time according to 20% of the theoretical positive vulcanization time measured in step (2). After the vulcanization process is completed, pre-vulcanized rubber is obtained.
[0049] As shown in Table 1, the difference between Preparation Examples 1-5 is that the percentage of the vulcanization processing time of the styrene-butadiene rubber mixture to the theoretical positive vulcanization time (hereinafter referred to as the vulcanization time percentage) is different.
[0050] Table 1 Vulcanization time ratio
[0051] Example
[0052] Examples 1-5
[0053] The following description will be given using Example 1 as an example.
[0054] Example 1
[0055] This embodiment provides a foamed rubber shoe material obtained by foaming, vulcanizing, and cutting a rubber shoe base. The rubber shoe base includes a rubber sheet and a fabric attached to the surface of the rubber sheet. The rubber sheet is processed in an open mill from a premixed rubber material. The premixed rubber material includes the following components: 44 kg of natural rubber, 24 kg of filler, 5 kg of oil, 4 kg of vulcanizing agent, 1.8 kg of antioxidant, 0.5 kg of accelerator, 4 kg of triterpenoid saponin, 8 kg of n-butanol, 3 kg of unsaturated fatty acid, 7 kg of sulfur, 1.6 kg of dicumyl peroxide, and 10 kg of foaming agent.
[0056] The rubber matrix is natural rubber (3L standard rubber), the filler is a mixture of 800 heavy calcium powder and 300 mesh white carbon black in a weight ratio of 14:9, the oil is 10# white mineral oil, the vulcanizing agent is a mixture of petroleum resin, PEG-4000, paraffin and zinc oxide in a weight ratio of 0.8:1.4:0.25:1.9, the antioxidant is a mixture of antioxidant SP-C and antioxidant SP-P in a weight ratio of 1:1, the accelerator is a mixture of accelerator D and accelerator TS in a weight ratio of 3:8, and the unsaturated fatty acid is oleic acid; the foaming agent is a mixture of ammonium bicarbonate, sodium bicarbonate, 4,4'-oxybisbenzenesulfonylhydrazine, dichloroethane and petroleum ether in a weight ratio of 1:2:3:1:4.
[0057] This embodiment also provides a method for preparing a foamed rubber shoe material, comprising the following steps:
[0058] (1) The rubber matrix, filler, oil, antioxidant, vulcanizing agent, n-butanol, triterpenoid saponin, and unsaturated fatty acid are mixed in an internal mixer at a speed of 60 r / min, the plug is pressed for 45 seconds, the plug is lifted for 10 seconds, the plug is pressed for 15 seconds, the plug is lifted for 15 seconds, and the plug is pressed until the rubber material stabilizes at 165° C., and then the rubber is discharged to obtain a masterbatch; 4,4′-oxybisbenzenesulfonylhydrazine, petroleum ether, dichloroethane, and bicarbonate are added to a stirring tank and homogenized at a rate of 2500 r / min for 10 minutes to obtain a foaming agent for standby use;
[0059] (2) mixing a masterbatch, an accelerator, sulfur, dicumyl peroxide, and a foaming agent to obtain a premixed rubber material, passing cooling water at 5° C. through the rollers of an open mill, and then thinly passing and plasticating the premixed rubber material in the open mill, and discharging the premixed rubber material at a roller distance of 2 mm to obtain a rubber sheet;
[0060] (3) Imitation N cloth is attached to the surface of the rubber sheet, and a sheet discharging machine is used to press the sheet with a roller distance of 2 mm to obtain a rubber shoe blank, which is then transferred to a vulcanizer for foaming and vulcanization. After the rubber shoe blank enters the vulcanizer, the temperature is raised to 60°C, then kept constant at this temperature for 20 minutes, then further raised to 90°C, kept constant at this temperature for 20 minutes, then raised to 115°C, kept constant at this temperature for 45 minutes, and finally raised to 150°C, kept constant at this temperature for 10 minutes to end the foaming and vulcanization and demold. After demolding, the rubber shoe blank is cut to obtain foamed rubber shoe material.
[0061] As shown in Table 2, the differences between Examples 1-5 are mainly due to the different raw material ratios of the premixed rubber.
[0062] Table 2 Ratio of raw materials of premixed rubber
[0063] Example 6
[0064] The difference between this embodiment and embodiment 5 is that the unsaturated fatty acid is linoleic acid.
[0065] Example 7
[0066] The difference between this embodiment and embodiment 5 is that the unsaturated fatty acid is linolenic acid.
[0067] Example 8
[0068] The difference between this embodiment and embodiment 5 is that the unsaturated fatty acid is arachidonic acid.
[0069] Example 9
[0070] The difference between this embodiment and embodiment 5 is that the unsaturated fatty acid is farnesic acid.
[0071] Example 10
[0072] The difference between this embodiment and embodiment 9 is that the rubber matrix is formed by mixing natural rubber and styrene-butadiene rubber in a weight ratio of 10:1.
[0073] Example 11
[0074] The difference between this embodiment and embodiment 10 is that the rubber matrix is formed by mixing natural rubber and pre-vulcanized rubber in a weight ratio of 10:1, and the pre-vulcanized rubber is prepared according to the method of preparation example 1.
[0075] As shown in Table 3, the difference between Examples 11-15 is that the preparation examples of the pre-vulcanized rubber are different.
[0076] Table 3 Preparation example of pre-vulcanized rubber
[0077] Example 16
[0078] The difference between this embodiment and Example 13 is that the filler components include 800 heavy calcium powder, 300 mesh white carbon black and modified glass fiber, the amount of modified glass fiber is 0.4% of the weight of the rubber matrix, and the balance is supplemented to 28 kg by heavy calcium powder and white carbon black in a weight ratio of 14:9.
[0079] The modified glass fiber was prepared as follows:
[0080] (1) adding a silane coupling agent to water to obtain a silane-modified solution, which is set aside; heating the glass fiber at 400° C. for 1 hour to remove oil, and then waiting for the glass fiber to cool to 20° C. and set aside; in this step, the silane coupling agent used includes γ-aminopropyltriethoxysilane, and the mass fraction of γ-aminopropyltriethoxysilane in the silane-modified solution is 0.5%;
[0081] (2) Adding glass fiber to the silane modification liquid, stirring under nitrogen protection, and heating to 70°C, then keeping the temperature for 2 hours. After the insulation is completed, filter out the glass fiber, wash and dry the taken out glass fiber to obtain modified glass fiber.
[0082] As shown in Table 4, the difference between Examples 16-20 is that the mass fraction of γ-aminopropyltriethoxysilane in the silane modification solution (hereinafter referred to as aminosilane content) is different.
[0083] Table 4 Aminosilane content
[0084] Example 21
[0085] The difference between this preparation example and Example 20 is that the silane coupling agent in the silane modification liquid further includes vinyltriethoxysilane, and the mass fraction of vinyltriethoxysilane in the silane modification liquid is 2.2%.
[0086] As shown in Table 5, the difference between Examples 21-25 is that the mass fraction of vinyltriethoxysilane in the silane-modified liquid (hereinafter referred to as vinylsilane content) is different.
[0087] Table 5 Alkenylsilane content
[0088] Examples 25-29
[0089] As shown in Table 6, Examples 25-29 differ in the percentage of modified glass fiber used relative to the weight of the styrene-butadiene rubber (hereinafter referred to as the fiber ratio, expressed as a percentage). In Examples 25-29, the total weight of filler remains constant, while the amounts of heavy calcium carbonate and silica decrease as the fiber ratio increases. Heavy calcium carbonate and silica are always compounded in a weight ratio of 14:9.
[0090] Table 6 Fiber ratio
[0091] Comparative Example
[0092] Comparative Example 1
[0093] This comparative example provides a foamed rubber shoe material obtained by foaming, vulcanizing, and cutting a rubber shoe base. The rubber shoe base comprises a rubber sheet and a fabric attached to the surface of the rubber sheet. The rubber sheet is formed by mixing a premixed rubber material in an open mill. The premixed rubber material comprises the following components: 44 kg of rubber matrix, 24 kg of filler, 5 kg of oil, 4 kg of vulcanizing agent, 1.8 kg of antioxidant, 0.5 kg of accelerator, 7 kg of sulfur, and 10 kg of foaming agent.
[0094] The rubber matrix is natural rubber (3L standard rubber), the filler is a mixture of 800 heavy calcium powder and 300 mesh white carbon black in a weight ratio of 14:9, the oil is 10# white mineral oil, the vulcanizing agent is a mixture of petroleum resin, PEG-4000, paraffin and zinc oxide in a weight ratio of 0.8:1.4:0.25:1.9, the antioxidant is a mixture of antioxidant SP-C and antioxidant SP-P in a weight ratio of 1:1, the accelerator is a mixture of accelerator D and accelerator TS in a weight ratio of 3:8, and the foaming agent is a mixture of ammonium bicarbonate, sodium bicarbonate, 4,4'-oxybisbenzenesulfonylhydrazine, dichloroethane and petroleum ether in a weight ratio of 1:2:3:1:4.
[0095] This comparative example also provides a method for preparing a foamed rubber shoe material, comprising the following steps:
[0096] (1) The rubber matrix, filler, oil, antioxidant, and vulcanizing agent are put into an internal mixer for mixing, the speed is set to 60 r / min, the plug is pressed for 45 seconds, the plug is lifted for 10 seconds, the plug is pressed for 15 seconds, the plug is lifted for 15 seconds, and the plug is pressed until the rubber material stabilizes at 165°C, and then the rubber is discharged to obtain a masterbatch; 4,4'-oxybisbenzenesulfonylhydrazine, petroleum ether, dichloroethane, and bicarbonate are put into a stirring tank and homogenized at a speed of 2500 r / min for 10 minutes to obtain a foaming agent for standby use;
[0097] (2) mixing a masterbatch, an accelerator, sulfur, and a foaming agent to obtain a premixed rubber material, passing cooling water at 5° C. through the rollers of an open mill, and then thinly passing and plasticating the premixed rubber material in the open mill, and discharging the sheet according to a roller distance of 2 mm to obtain a rubber sheet;
[0098] (3) Imitation N cloth is attached to the surface of the rubber sheet, and a sheet discharging machine is used to press the sheet with a roller distance of 2 mm to obtain a rubber shoe blank, which is then transferred to a vulcanizer for foaming and vulcanization. After the rubber shoe blank enters the vulcanizer, the temperature is raised to 60°C, then kept constant at this temperature for 20 minutes, then further raised to 90°C, kept constant at this temperature for 20 minutes, then raised to 115°C, kept constant at this temperature for 45 minutes, and finally raised to 150°C, kept constant at this temperature for 10 minutes to end the foaming and vulcanization and demold. After demolding, the rubber shoe blank is cut to obtain foamed rubber shoe material.
[0099] Comparative Example 2
[0100] The difference between this comparative example and comparative example 1 is that the components of the premixed rubber material also include 8 kg of n-butanol, which is mixed with the masterbatch, accelerator, sulfur and foaming agent in step (2) of preparing the foamed rubber shoe material.
[0101] Comparative Example 3
[0102] The difference between this comparative example and Example 1 is that the components of the premixed rubber material do not include triterpenoid saponins.
[0103] Comparative Example 4
[0104] The difference between this comparative example and Example 1 is that the components of the premixed rubber material do not include unsaturated fatty acids.
[0105] Comparative Example 5
[0106] The difference between this comparative example and Example 1 is that the components of the premixed rubber material do not include dicumyl peroxide.
[0107] Comparative Example 6
[0108] The difference between this comparative example and Example 1 is that the components of the premixed rubber material do not include n-butanol.
[0109] Performance testing methods
[0110] Foaming effect evaluation
[0111] Sample: a rubber shoe blank cut from each embodiment and comparative example after foaming and vulcanization.
[0112] Test method: Referring to the description of GB / T 6343-2009 Foam plastics and rubber - Determination of apparent density, the apparent density of the sample was tested, and then the ratio between the apparent density of the sample of each embodiment and comparative example and the apparent density of the sample of comparative example 1 was calculated. The ratio was recorded as the relative density. The results are shown in Table 7.
[0113] Table 7 Relative density
[0114] Combining Example 1 and Comparative Example 1 and Table 7, it can be seen that the relative density measured in Example 1 is lower than that in Comparative Example 1, indicating that the foamed rubber shoe material of the present application has a lower apparent density after foaming and vulcanization, achieving a better foaming effect.
[0115] Combining Comparative Examples 1 and 2 with Table 7, it can be seen that even with the addition of n-butanol to Comparative Example 1, the measured relative density did not show a significant decrease, indicating that the cell wall collapse in Comparative Example 1 was more severe. Even if the added n-butanol could be vaporized during processing, the formed cells would be difficult to retain, resulting in poor foaming effect of the rubber compound.
[0116] Combining Example 1 and Comparative Example 3 with Table 7, it can be seen that the relative density measured in Example 1 is lower than that in Comparative Example 3, indicating that when the premixed rubber compound lacks triterpenoid saponins, hydrogen bonds cannot be formed on the inside of the pore wall by the glucose units of the triterpenoid saponins, and the strength of the pore wall cannot be fully improved by the participation of triterpenoid saponins in copolymerization. In addition, the bonding force between the bubbles and the natural rubber is poor, and it is difficult to fully limit the softening effect of the bubbles on the rubber compound. Therefore, the foaming effect of the rubber compound is poor.
[0117] Combining Example 1 and Comparative Example 4 with Table 7, it can be seen that the relative density measured in Example 1 is lower than that in Comparative Example 4, indicating that when the premixed rubber lacks unsaturated fatty acids, it is difficult to fully increase the pore wall strength by copolymerization between triterpenoid saponins and natural rubber alone, and thus it is difficult to prevent the collapse of bubbles. Therefore, the foaming effect of the rubber is poor and sufficient pores cannot be formed.
[0118] Combining Example 1 and Comparative Example 5 with Table 7, it can be seen that the relative density measured in Example 1 is lower than that in Comparative Example 5, indicating that in the absence of dicumyl peroxide, it is difficult for unsaturated fatty acids and triterpenoid saponins to form a copolymer to increase the pore wall strength. Therefore, the bubbles easily collapse, resulting in poor foaming effect of the rubber compound and inability to form sufficient pores.
[0119] Combining Example 1 and Comparative Example 6 with Table 7, it can be seen that the relative density measured in Example 1 is lower than that in Comparative Example 5, indicating that in the absence of n-butanol, the dispersion effect of triterpenoid saponins is relatively poor, affecting the foaming effect of the rubber compound.
[0120] In combination with Example 1 and Comparative Examples 1-6 and Table 7, it can be seen that when the rubber material is foamed and vulcanized, the triterpenoid saponins and the unsaturated fatty acids migrate to the interface between the pore wall and the bubble, so that the hydrophilic end forms a hydrogen bond on the inside of the pore wall, and the sapogenin copolymerizes with the unsaturated fatty acids and the natural rubber on the outside of the pore wall, thereby improving the strength of the pore wall, reducing the possibility of bubbles breaking through the pore wall and causing the pore wall to collapse, overcoming the defect that the rubber material is easily densified due to the collapse of the pore wall, and helping to achieve sufficient foaming of the rubber material.
[0121] As can be seen from Examples 5-9 and Table 7, unsaturated fatty acids containing multiple carbon-carbon double bonds have more copolymerization sites than monoolefinic acids, which can better improve the copolymerization effect between the unsaturated fatty acids, triterpenoid saponins, and natural rubber, help increase cell wall strength, and fully promote the foaming of the rubber compound. Given the same number of carbon-carbon double bonds in the unsaturated fatty acids, the relative density measured in Example 9 is lower than that in Example 7, indicating that the farnesic acid used in Example 9 has good compatibility with the triterpenoid saponins and natural rubber, helps increase cell wall strength, and fully promotes the foaming of the rubber compound.
[0122] Combining Examples 9-15 and Table 7, it can be seen that although the addition of pre-vulcanized rubber can improve the foaming performance of the rubber compound in general, the improvement effect of the pre-vulcanized rubber on the foaming performance of the rubber compound tends to increase first and then decrease as the vulcanization time of the pre-vulcanized rubber increases. This indicates that when the vulcanization time of the pre-vulcanized rubber is too long, the improvement effect of the pre-vulcanized rubber on the foaming performance of the rubber compound will be subject to certain limitations. When the vulcanization time of the pre-vulcanized rubber is set between 28% and 52% of the theoretical positive vulcanization time, it helps to fully improve the foaming performance of the rubber compound.
[0123] Combining Example 13 with Examples 16-20 and Table 7, it can be seen that the relative density measured in Examples 16-20 is relatively low, indicating that the addition of modified glass fiber improves the matching between the vulcanization and foaming processes, reduces the possibility of bubbles breaking through the cell walls and causing cell wall collapse, and promotes sufficient foaming of the rubber compound. When the mass fraction of γ-aminopropyltriethoxysilane in the silane-modifying solution is 2.5-4.5%, the rubber compound has a better foaming effect.
[0124] Combining Example 20 with Examples 21-25 and Table 7, it can be seen that the relative density measured in Examples 21-25 is lower than that in Example 20, indicating that vinyltriethoxysilane helps limit the softening effect of bubbles on the rubber compound, thereby improving the rubber compound's foaming performance. When the mass fraction of vinyltriethoxysilane in the silane-modifying liquid is 3.8-5.4%, the rubber compound exhibits better foaming performance.
[0125] It can be seen from Examples 25-29 and Table 7 that when the amount of modified glass fiber is 0.8-1.2% of the weight of the rubber matrix, the foaming effect of the rubber compound is relatively good.
[0126] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make non-creative modifications to the present embodiment as needed, but as long as they are within the scope of the claims of the present application, they are protected by the patent law.
Claims
1. A foam rubber shoe material, It is characterized in that The foamed rubber shoe material is obtained by foaming, vulcanizing and cutting a rubber shoe blank, the rubber shoe blank comprises a rubber sheet and a cloth attached to the surface of the rubber sheet, the rubber sheet is processed by a premixed rubber in an open mill, the premixed rubber comprises the following components in parts by weight: 44-48 parts of a rubber matrix, 24-28 parts of a filler, 5-7 parts of an oil, 4-5 parts of a vulcanizing aid, 1.8-2.2 parts of an antioxidant, 0.5-0.7 parts of an accelerator, 4-6 parts of a triterpenoid saponin, 8-12 parts of n-butanol, 3-5 parts of an unsaturated fatty acid, 7-9 parts of sulfur, 1.6-2.4 parts of diisopropyl peroxide, and 10-14 parts of a foaming agent; the foaming agent comprises 4,4'-oxybisbenzenesulfonyl hydrazide, petroleum ether, ethylene dichloride and at least one bicarbonate, and the components of the rubber matrix comprise natural rubber.
2. The foamed rubber shoe material according to claim 1, It is characterized in that The unsaturated fatty acid molecules contain 2-4 carbon-carbon double bonds.
3. The foamed rubber shoe material according to claim 2, It is characterized in that The unsaturated fatty acid is farnesic acid.
4. The foamed rubber shoe material according to claim 1, It is characterized in that The rubber matrix also includes pre-vulcanized rubber, the weight ratio of the natural rubber to the pre-vulcanized rubber is 10:(1-2), and the pre-vulcanized rubber is prepared according to the following method: (1) mixing zinc oxide, stearic acid, an accelerator, an antioxidant and sulfur with styrene-butadiene rubber to obtain a styrene-butadiene rubber mixture; (2) taking a portion of the styrene-butadiene rubber mixture, selecting vulcanization process parameters and performing vulcanization processing, and determining the theoretical positive vulcanization time of the styrene-butadiene rubber mixture under the selected vulcanization process parameters; (3) According to the vulcanization process parameters selected in step (2), the remaining styrene-butadiene rubber is mixed The material is vulcanized, and the vulcanization time is set according to 20-70% of the theoretical positive vulcanization time measured in step (2). After the vulcanization process is completed, the pre-vulcanized rubber is obtained.
5. The foamed rubber shoe material according to claim 4, It is characterized in that In the step (3) of preparing the pre-vulcanized rubber, the vulcanization processing time is set according to 28-52% of the theoretical positive vulcanization time measured in the step (2).
6. The foamed rubber shoe material according to claim 1, It is characterized in that The filler comprises modified glass fiber, and the modified glass fiber is glass fiber with amino groups grafted on the surface.
7. The foamed rubber shoe material according to claim 6, It is characterized in that The modified glass fiber is prepared as follows: (1) adding a silane coupling agent to water to obtain a silane-modified liquid for standby use; heating and degreasing the glass fiber for standby use; the silane coupling agent comprises γ-aminopropyltriethoxysilane, and the mass fraction of the γ-aminopropyltriethoxysilane in the silane-modified liquid is 2.5-4.5%; (2) Adding glass fiber to the silane modification liquid, stirring under nitrogen protection, and heating to 70-75° C., then keeping the temperature for 2-3 hours. After the insulation is completed, filtering out the glass fiber, washing and drying the taken out glass fiber to obtain modified glass fiber.
8. The foamed rubber shoe material according to claim 7, It is characterized in that In the method for preparing the modified glass fiber, the silane coupling agent used also includes vinyl triethoxy silane, and the mass fraction of the vinyl triethoxy silane in the silane modification liquid is 3.8-5.4%.
9. The foamed rubber shoe material according to claim 8, It is characterized in that The modified glass fiber is used in an amount of 0.8-1.2% of the weight of the rubber matrix.
10. The method for preparing the foamed rubber shoe material according to claim 1, It is characterized in that The following steps are involved: (1) putting a rubber matrix, a filler, an oil, an antioxidant, a vulcanizing agent, n-butanol, a triterpenoid saponin, and an unsaturated fatty acid into an internal mixer for mixing, and after mixing, performing rubber removal to obtain a masterbatch; mixing 4,4'-oxybisbenzenesulfonylhydrazine, petroleum ether, ethylene dichloride, and bicarbonate, and then stirring, and then homogenizing to obtain a foaming agent for standby use; (2) mixing a masterbatch, an accelerator, sulfur, dicumyl peroxide and a foaming agent to obtain a premixed rubber material, and performing thin-pass plasticizing on the premixed rubber material in an open mixing mill to obtain a rubber sheet; (3) attaching cloth to the surface of the rubber sheet to obtain a rubber shoe blank, transferring the rubber shoe blank to a vulcanization device for foaming and vulcanization, and then cutting to obtain a foamed rubber shoe material.
Citation Information
Patent Citations
Rubber foamed shoe material and preparation method thereof
CN108912419A
Foamed shoe sole material and preparation method thereof
CN109134959A
Hard high-damping foamed rubber sole and preparation method thereof
CN109721772A
Integrated rubber foaming shoe and preparation method thereof