Fischer-tropsch synthesis iron-based catalyst and preparation method therefor

By uniformly distributing the Ba element in the Fischer-Tropsch synthesis iron-based catalyst, the problem of insufficient thermal stability of the catalyst is solved, the catalytic activity and thermal stability are improved, the preparation process is simplified and the cost is reduced, making it suitable for large-scale industrial applications.

WO2024221882A1PCT designated stage expired Publication Date: 2024-10-31CHINA ENERGY INVESTMENT CORP LTD +1

Patent Information

Application Number
PCT/CN2023/133691
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2023-11-23
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing iron-based catalysts for Fischer-Tropsch synthesis have insufficient thermal stability in high-temperature reactions and are prone to sintering, resulting in decreased activity. Existing methods such as adding SiO2 or structural additives cannot effectively improve thermal stability, and the preparation process is complex and costly.

Method used

0.3~3% Ba element is evenly distributed in the Fischer-Tropsch synthesis iron-based catalyst. The Ba element exists in the form of barium carbonate through a specific preparation method to avoid Fe grain sintering and is highly dispersed on the surface of Fe and SiO2 particles to form fine particles. , simplify the preparation process and reduce costs.

Benefits of technology

It significantly improves the thermal stability and catalytic activity of the catalyst, reduces the selectivity of CO2 and CH4, simplifies the preparation process, reduces production costs, and is suitable for large-scale industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2023133691-FTAPPB-I100001
    Figure PCTCN2023133691-FTAPPB-I100001
  • Figure PCTCN2023133691-FTAPPB-I100002
    Figure PCTCN2023133691-FTAPPB-I100002
  • Figure PCTCN2023133691-FTAPPB-I100003
    Figure PCTCN2023133691-FTAPPB-I100003
Patent Text Reader

Abstract

The present invention provides a Fischer-Tropsch synthesis iron-based catalyst, containing a Fe element, a Cu element, a K element, and SiO2, wherein the surface of the Fischer-Tropsch synthesis iron-based catalyst contains 0.3-3% by mole of a Ba element. The present invention further provides a preparation method for the Fischer-Tropsch synthesis iron-based catalyst. The Fischer-Tropsch synthesis iron-based catalyst provided by the present invention is simple and convenient to prepare, has excellent catalytic performance and good heat resistance, and is not prone to inactivation after being used for a long time, so that the use of said catalyst can significantly improve the production efficiency of a Fischer-Tropsch synthesis process, reduce production costs, and has very important economic and social value.
Need to check novelty before this filing date? Find Prior Art

Description

A Fischer-Tropsch synthesis iron-based catalyst and preparation method thereof Technical Field

[0001] The present invention relates to the field of Fischer-Tropsch synthesis, and in particular to an iron-based catalyst for Fischer-Tropsch synthesis and a preparation method thereof. Background Art

[0002] The Fischer-Tropsch synthesis (FTS) reaction, under appropriate temperature, pressure, and catalyst conditions, can synthesize hydrocarbons of varying carbon numbers from CO and H₂. These products can then be processed to produce fuels and chemicals. Therefore, FTS can be used to convert coal, natural gas, biomass, and other energy sources into syngas-to-liquids. FTS technology is divided into high-temperature and low-temperature technologies. High-temperature FTS operates at temperatures above 300°C, typically using a fluidized bed reactor and a molten iron catalyst. The products are primarily olefins and oxygenates. Low-temperature FTS operates at temperatures below 280°C, typically using a fixed bed or slurry bed reactor, using either a precipitated iron catalyst (suitable for reaction temperatures between 250-280°C) or a supported cobalt catalyst (suitable for reaction temperatures between 200-230°C). The products are primarily diesel and wax. Cobalt-based and iron-based catalysts differ in their active phase structures and primary and secondary reaction pathways, resulting in distinct formulations and preparation methods. Iron-based catalysts with iron as the active component are more suitable for large-scale industrial applications due to their low price, strong resistance to poisoning, and high content of linear α-olefins in the product.

[0003] Iron-based catalysts prepared by precipitation methods have small crystals and numerous active sites, but these small crystals are prone to sintering. Furthermore, Fischer-Tropsch synthesis is a highly exothermic reaction, with intense exothermic hot spots at the catalyst's active sites. Therefore, high thermal stability is required for the catalyst. Otherwise, the catalyst is prone to sintering or fragmentation due to the heat of reaction, resulting in a decrease in catalyst performance. Therefore, developing iron-based catalysts with both high activity and high thermal stability is a key research and development direction for slurry-bed Fischer-Tropsch synthesis technology.

[0004] Commonly used methods to improve catalyst stability include: (1) adding binders (such as SiO2) to disperse and bond iron grains, (2) improving the preparation process (such as through heat treatment) to improve particle strength and inhibit breakage; (3) adding structural additives (such as Ti, Zr) to improve particle strength. Among them, adding binders is the most effective method to improve the mechanical strength of catalysts. At present, almost all Fischer-Tropsch synthesis iron-based catalysts contain SiO2 binders. Although the addition of silicon plays a role in separating and bonding the active particles of the catalyst to avoid sintering of the active phase of the catalyst, it is not a good solution to the problem of thermal stability of the catalyst because silicon is a poor thermal conductor and silicon will also aggregate silicon balls under the action of heat and water vapor, which easily leads to a decrease in catalyst strength. Therefore, it cannot effectively solve the problem of thermal stability of the catalyst. Some researchers have also improved the mechanical strength of the catalyst by adding structural additives. For example, Chinese patents CN 1245255C, CN 101293206A and CN 101298046A respectively improve the wear resistance of the catalyst by adding zinc, zirconium and titanium additives. However, the above method of suppressing catalyst breakage by increasing catalyst particle strength cannot improve the catalyst's anti-sintering stability under the action of reaction heat, thereby preventing the decrease in catalyst activity caused by iron grain sintering. Therefore, how to improve the thermal stability of iron-based catalysts during the reaction remains an urgent problem to be solved for precipitated iron-based catalysts in Fischer-Tropsch synthesis.

[0005] Chinese patent CN 107684910B discloses a method for preparing an iron-based catalyst for Fischer-Tropsch synthesis. The catalyst components include Fe, Cu, K, Ca, and a metal promoter selected from at least one of barium, zinc, lanthanum, magnesium, aluminum, strontium, cerium, lawrencium, platinum, ytterbium, niobium, praseodymium, palladium, and cesium. The patent states that a precipitation reaction product containing iron, calcium, and the metal promoter is dispersed in a potassium salt solution in the presence of an organic carboxylic acid, impregnated, spray-dried, and calcined. The calcined product is then mixed with silica sol in the presence of an organic solvent, followed by a secondary spray drying and calcination, thereby obtaining a catalyst with high wear resistance. The catalyst preparation steps proposed in this patent are complex, generally requiring the addition of multiple promoters and a secondary calcination, resulting in high process costs.

[0006] Chinese patent CN 107913714B discloses an iron-based catalyst for Fischer-Tropsch synthesis, comprising Fe, Cu, Mn, K, SiO2, a first additive, and a second additive, wherein the first additive is selected from one or more of Ca, Sr, and Ba, and the second additive is one or more of La, Ce, Y, and Nd. The patent states that its technical solution provides a catalyst with high stability and low CO2 and CH4 selectivity, and emphasizes that the catalyst within the composition range of the invention can maintain low carbon dioxide selectivity and methane selectivity at high conversion rates under the synergistic effect of rare earth metals, alkaline earth metals, and other additives, and effectively inhibit catalyst deactivation; if only rare earth metals or alkaline earth metal additives are added alone, the above effects cannot be achieved simultaneously. In addition, from the perspective of its preparation method, when the first additive solution is added by impregnation, the precipitated catalyst slurry needs to be dried and calcined before impregnation. The impregnated catalyst needs to be dried and calcined a second time, which makes the preparation process long and costly.

[0007] Summary of the Invention

[0008] In order to make up for the deficiencies in the prior art, an object of the present invention is to provide an iron-based catalyst for Fischer-Tropsch synthesis, which has excellent catalytic performance and thermal stability, is very suitable for Fischer-Tropsch synthesis reaction, and can significantly improve the reaction efficiency.

[0009] Another object of the present invention is to provide a method for preparing the Fischer-Tropsch synthesis iron-based catalyst.

[0010] A first aspect of the present invention provides an iron-based catalyst for Fischer-Tropsch synthesis, comprising Fe, Cu, K and SiO2, wherein the surface of the iron-based catalyst for Fischer-Tropsch synthesis contains 0.3 to 3% of Ba in terms of molar percentage.

[0011] The Ba element has good heat resistance, stability and thermal conductivity. The present invention uniformly adds a specific amount of Ba element to the Fischer-Tropsch synthesis iron-based catalyst, so that it is highly dispersed on the surface of Fe grains and SiO2 particles and basically does not change the original form of the catalyst. The Ba element dispersed on the surface does not enter the crystal phase of Fe and Si, and can effectively protect the Fe grains in the catalyst, thereby avoiding the sintering of Fe grains and the combination of Fe grains and SiO2 particles to form difficult-to-reduced iron silicate species, thereby enabling the obtained catalyst to obtain excellent catalytic activity and thermal stability.

[0012] In some preferred embodiments, the surface of the Fischer-Tropsch synthesis iron-based catalyst may contain 0.5 to 2.8% of Ba element by mole percentage, for example, about 0.5%, about 0.8%, about 1%, about 1.2%, about 1.5%, about 1.8%, about 2%, about 2.2%, about 2.5%, about 2.8% or a mole percentage interval of any combination. In some more preferred embodiments, the surface of the Fischer-Tropsch synthesis iron-based catalyst may contain 1 to 2.5% of Ba element by mole percentage. In some further preferred embodiments, the surface of the Fischer-Tropsch synthesis iron-based catalyst may contain 1.5 to 2.5% of Ba element by mole percentage.

[0013] In the Fischer-Tropsch synthesis iron-based catalyst provided by the present invention, the Ba element exists in the form of barium carbonate (BaCO3). The Ba element itself has a certain alkalinity, which helps to suppress the generation of methane (CH4) by-products in the Fischer-Tropsch synthesis reaction, improve C5+ product selectivity and olefin selectivity, but also improves the selectivity of CO2. The inventors have found that when the Ba element exists in the form of barium carbonate, it can effectively play the role of Ba as an alkaline earth metal additive, while also being able to avoid the problem of CO2 selectivity increased by strongly basic additives (such as alkali metal additives K, Ba in the form of barium hydroxide, etc.), thereby enabling the resulting catalyst to have lower CO2 selectivity and CH4 selectivity at the same time, further improving its catalytic performance.

[0014] In some preferred embodiments, the specific surface area of ​​the Fischer-Tropsch synthesis iron-based catalyst provided by the present invention may be 100 to 250 m2 / g. In some more preferred embodiments, the specific surface area of ​​the Fischer-Tropsch synthesis iron-based catalyst provided by the present invention may be 120 to 210 m2 / g.

[0015] In some preferred embodiments, the Fischer-Tropsch synthesis iron-based catalyst provided by the present invention may comprise the following components in a mass ratio: Fe element: Cu element: K element: Ba element: SiO2 = 100: 0.2-5: 0.5-8: 1-10: 10-40. In some more preferred embodiments, the Fischer-Tropsch synthesis iron-based catalyst provided by the present invention may comprise the following components in a mass ratio: Fe element: Cu element: K promoter: Ba element: SiO2 = 100: 2-5: 4-8: 5-10: 20-40.

[0016] A second aspect of the present invention provides a method for preparing the Fischer-Tropsch synthesis iron-based catalyst, the preparation method comprising the following steps:

[0017] S1: forming a mixed aqueous solution of a water-soluble salt of Fe and a water-soluble salt of Cu, preparing a precipitant solution, and adding 0 to 100 wt % of a silicon source to the precipitant solution;

[0018] S2: contacting the mixed aqueous solution with the precipitant solution to perform a precipitation reaction, and separating the resulting precipitated product after the reaction is completed;

[0019] S3: mixing the precipitated product with the K promoter precursor aqueous solution and the remaining silicon source to form a mixed slurry and performing a slurry treatment to obtain a catalyst precursor slurry; and

[0020] S4: drying and calcining the catalyst precursor slurry;

[0021] The method of adding the Ba element includes: adding a water-soluble salt of Ba to the mixed aqueous solution of step S1, and making the concentration of Ba lower than 2.0g Ba / 100g water; or

[0022] The water-soluble salt of Ba is prepared into an aqueous solution with a concentration of less than 2.0 g Ba / 100 g water, and then added to the mixed slurry in step S3.

[0023] In the preparation method provided by the present invention, by controlling the concentration of Ba element when added, the Ba element can be uniformly distributed on the catalyst surface at a specific content and form very fine particles, without substantially changing the original catalyst morphology.

[0024] In the preparation method provided by the present invention, the silicon source can be added in whole or in part to the precipitant solution, or in whole or in part to the mixed slurry. For example, the silicon source added to the precipitant solution can be about 0 wt%, about 10 wt%, about 20 wt%, about 30 wt%, about 40 wt%, about 50 wt%, about 60 wt%, about 70 wt%, about 80 wt%, about 90 wt%, about 100 wt%, or any combination of weight ratios of the total mass of the silicon source, and the remaining silicon source is added to the mixed slurry.

[0025] In the preparation method provided by the present invention, the water-soluble salt of Fe may be a common type in the art, including but not limited to nitrate, hydrochloride or hydrate of each of Fe (wherein the number of crystal waters may be a common number in the art), such as Fe(NO3)3·9H2O. In some preferred embodiments, the concentration of Fe in the mixed aqueous solution may be 5 to 100 g / L, for example, about 5 g / L, about 10 g / L, about 20 g / L, about 30 g / L, about 40 g / L, about 50 g / L, about 60 g / L, about 70 g / L, about 80 g / L, about 90 g / L, about 100 g / L or any combination of concentration intervals.

[0026] In the preparation method provided by the present invention, the water-soluble salt of Cu can be a common type in the art, including but not limited to Cu nitrate, hydrochloride or their respective hydrates (wherein the number of crystal waters can be a common number in the art), such as Cu(NO3)2·3H2O.

[0027] In the preparation method provided by the present invention, the precipitant can be any common type in the art, including but not limited to one or more of sodium carbonate, ammonia water, ammonium carbonate, sodium hydroxide, potassium hydroxide, and potassium carbonate. In some preferred embodiments, the concentration of the precipitant in the precipitant solution can be 50 to 150 g / L, for example, about 50 g / L, about 60 g / L, about 70 g / L, about 80 g / L, about 90 g / L, about 100 g / L, about 110 g / L, about 120 g / L, about 130 g / L, about 140 g / L, about 150 g / L, or any combination of concentration ranges.

[0028] In the preparation method provided by the present invention, the silicon source can be any common type in the art, including but not limited to one or more of potassium silicate solution, sodium silicate solution, and silica sol solution, wherein the SiO2 concentration can be 10 to 50 wt%. In some preferred embodiments, the SiO2 concentration in the silicon source can be 10 to 30 wt%.

[0029] In the preparation method provided by the present invention, the water-soluble salt of Ba can be one or both of barium nitrate and barium hydroxide.

[0030] In the preparation method provided by the present invention, the K additive precursor can be any common type in the art, including but not limited to one or more of potassium nitrate, potassium carbonate, potassium bicarbonate, potassium silicate, and potassium chloride.

[0031] In the preparation method provided by the present invention, in step S2, the precipitation temperature of the precipitation reaction can be 5 to 95°C (for example, it can be about 5°C, about 20°C, about 40°C, about 60°C, about 80°C, about 95°C, or any combination of temperature intervals), the precipitation time can be 5 to 100 min (for example, it can be about 5 min, about 20 min, about 40 min, about 60 min, about 80 min, about 100 min, or any combination of time intervals), and the pH value during the precipitation process can be controlled at 5 to 10 (for example, it can be about 5, about 6, about 7, about 8, about 9, about 10, or any combination of pH value intervals).

[0032] In the preparation method provided by the present invention, in step S3, when forming a mixed slurry, the mixing temperature of each material can be 20-70°C (for example, it can be about 20°C, about 30°C, about 40°C, about 50°C, about 60°C, about 70°C, or any combination of temperature intervals), and the mixing time can be 1-60 min (for example, it can be about 5 min, about 10 min, about 20 min, about 30 min, about 40 min, about 50 min, about 60 min, or any combination of time intervals).

[0033] In the preparation method provided by the present invention, in the step S3, the slurrying temperature of the slurrying treatment can be 10 to 80°C (for example, it can be about 10°C, about 20°C, about 30°C, about 40°C, about 50°C, about 60°C, about 70°C, about 80°C or any combination of temperature intervals), and the slurrying time can be 10 to 80 min (for example, it can be about 10 min, about 20 min, about 30 min, about 40 min, about 50 min, about 60 min, about 70 min, about 80 min or any combination of time intervals), and the concentration of the slurry can be controlled to be 10 to 20 wt% during the slurrying treatment process.

[0034] In the preparation method provided by the present invention, the carbonate ions present in the preparation system, such as the carbonate ions in the precipitant and / or the K additive precursor, help the Ba element to form the form of BaCO3. However, when the system does not contain carbonate ions, or when the carbonate ions in the system cannot react with the Ba salt to form BaCO3, or when the amount of carbonate ions is insufficient to convert all the Ba elements into BaCO3, it is necessary to additionally introduce CO2 gas after the slurry treatment to ensure the formation of BaCO3. Even if the system contains carbonate ions, additional CO2 gas may be introduced to fully ensure the formation of BaCO3. In some preferred embodiments, the step S3 further includes: introducing CO2 gas for treatment for 0 to 180 minutes after the slurry treatment is completed. In some more preferred embodiments, the step S3 further includes: introducing CO2 gas for treatment for 30 to 180 minutes after the slurry treatment is completed. In other preferred embodiments, the temperature during the CO2 treatment may be the same as the temperature of the slurry treatment.

[0035] In the preparation method provided by the present invention, in step S4, the drying may include the following process: first, spray drying the catalyst precursor slurry, and drying the resulting powder in an air atmosphere at 110-300°C for 1-12 hours. In some preferred embodiments, the hot air inlet temperature of the spray drying may be 180-400°C, and the exhaust air outlet temperature may be 100-220°C.

[0036] In the preparation method provided by the present invention, in step S4, the calcination temperature can be 400-600°C and the calcination time can be 1-15 hours. In some preferred embodiments, the catalyst obtained after calcination can be stored in an atmosphere containing CO2 to prevent the catalyst from deteriorating.

[0037] The technical solution provided by the present invention has the following advantages:

[0038] (1) The surface of the iron-based catalyst for Fischer-Tropsch synthesis provided by the present invention is uniformly distributed with a specific content of Ba element, which can better exert the thermal stability and thermal conductivity of Ba element, thereby effectively avoiding the sintering of Fe and the combination of Fe and SiO2. Therefore, the catalyst has very excellent catalytic activity and thermal stability.

[0039] (2) In the Fischer-Tropsch synthesis iron-based catalyst provided by the present invention, the Ba element exists in the form of barium carbonate, which enables the catalyst to have lower CO2 selectivity and CH4 selectivity when used in the Fischer-Tropsch synthesis reaction.

[0040] (3) The preparation process of the iron-based catalyst for Fischer-Tropsch synthesis provided by the present invention is simple, only a small amount of barium salt needs to be added, the conditions are mild and easy to control, no secondary roasting is required, the process is highly operable, the cost is low, and it is suitable for large-scale industrial production.

[0041] In summary, the Fischer-Tropsch synthesis iron-based catalyst provided by the present invention is easy to manufacture, has excellent catalytic performance and good heat resistance, and is not easily deactivated after long-term use. Therefore, its application can significantly improve the production efficiency of the Fischer-Tropsch synthesis process and reduce production costs, and has very important economic and social value. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] FIG1 is the XRD spectra of the catalysts prepared in Example 1 and Comparative Example 1, wherein the upper portion is the XRD spectra of the catalyst prepared in Example 1, and the lower portion is the XRD spectra of the catalyst prepared in Comparative Example 1.

[0043] FIG2 is a TEM-EDS spectrum of the catalyst prepared in Example 1, wherein the left figure shows the distribution of Ba on the catalyst, and the right figure shows the distribution of Fe on the catalyst. DETAILED DESCRIPTION

[0044] The technical solution of the present invention is further described in detail below with reference to specific embodiments.

[0045] The testing method used in the present invention is as follows:

[0046] (1) Catalyst composition:

[0047] The components were determined by X-ray fluorescence analyzer (XRF).

[0048] (2) Catalyst specific surface area (BET)

[0049] The static low-temperature nitrogen adsorption method was used to measure the N2 adsorption isotherm at 77K, and the BET model equation was used to calculate the BET.

[0050] (3) Pore volume (PV)

[0051] The pore volume corresponds to P / P0=0.98~0.99 on the N2 adsorption isotherm measured at 77K.

[0052] (4) Average pore diameter (PD):

[0053] Calculated based on PD=4*PV / BET.

[0054] (5) Ba content on the catalyst surface:

[0055] The results were determined by X-ray photoelectron spectroscopy (XPS).

[0056] Unless otherwise specified, the raw materials or reagents used in the examples and comparative examples of the present invention are commercially available products.

[0057] Unless otherwise specified, the percentages used in the examples and comparative examples of the present invention are all percentages by mass.

[0058] Example 1

[0059] Dissolve 10 kg of Fe(NO₃)₃·9H₂O, 140 g of Cu(NO₃)₂·3H₂O, and 260 g of Ba(NO₃)₂ in deionized water to prepare a 50 liter solution. Add 5 kg of ammonium carbonate and 1.84 kg of a 30% silica sol solution to the deionized water to prepare a 40 liter precipitant solution. A mixed solution containing iron, copper, and barium was co-precipitated with the precipitant solution at a temperature of 30°C, a precipitation time of 60 minutes, and a pH of 9.0. After the precipitation reaction was complete, the precipitated slurry was filtered and washed several times to obtain a catalyst precursor filter cake. Dissolve 195 g of potassium carbonate in 1.5 kg of deionized water to prepare a K promoter precursor aqueous solution. This K promoter precursor aqueous solution was added to the catalyst precursor filter cake and slurried at a concentration of 15% at a temperature of 25°C and a slurry time of 20 minutes to obtain a catalyst precursor slurry. The inlet temperature was controlled at 380°C and the outlet hot air temperature was controlled at 220°C for spray drying. The spray-dried product was collected and dried at 120°C in an air atmosphere for 12 hours, and then calcined at 450°C in an air atmosphere for 5 hours to obtain a finished catalyst, which was recorded as Catalyst 1.

[0060] As can be seen from Figure 1, compared with the catalyst without Ba component (i.e., the catalyst of Comparative Example 1), the XRD pattern of Catalyst 1 after adding Ba component still shows a conventional catalyst peak shape, indicating that the Ba component is highly dispersed in the catalyst and does not form a large crystal structure, thereby not significantly changing the morphology of the catalyst.

[0061] As can be seen from FIG2 , the Ba component is highly dispersed in the catalyst and does not form a large crystal structure.

[0062] Example 2

[0063] Dissolve 10 kg of Fe(NO₃)₃·9H₂O, 140 g of Cu(NO₃)₂·3H₂O, and 26 g of Ba(NO₃)₂ in deionized water to prepare a 50 liter solution. Add 4 kg of sodium carbonate and 30 g of a 20% silica sol solution to the deionized water to prepare a 40 liter precipitant solution. The mixed solution containing iron, copper, and barium is co-precipitated with the precipitant solution at 50°C for 50 minutes, with the pH controlled at 8.5. After the precipitation reaction is complete, the precipitate is filtered and washed several times to obtain a catalyst precursor filter cake. Prepare an aqueous solution of the K additive precursor by dissolving 12 g of potassium carbonate in 1.5 kg of deionized water. An aqueous solution of a K-promoter precursor and 660 g of a silica sol solution with a 20% silica concentration were sequentially added to the catalyst precursor filter cake for slurrying. The slurry concentration was controlled at 15%, the slurry temperature was maintained at 30°C, and the slurry time was 30 minutes to obtain a catalyst precursor slurry. Spray drying was then performed with the inlet temperature at 350°C and the outlet hot air temperature at 160°C. The spray-dried product was collected and dried at 150°C in air for 10 hours, followed by calcination at 400°C in air for 15 hours to obtain the finished catalyst, designated Catalyst 2.

[0064] Example 3

[0065] Dissolve 10 kg of Fe(NO₃)₃·9H₂O and 260 g of Cu(NO₃)₂·3H₂O in deionized water to prepare a 50 liter solution. Add 8 kg of 25% ammonia and 140 g of a potassium silicate solution with a modulus of 1 and a silica concentration of 20% to the deionized water to prepare a 40 liter precipitant solution. The iron-copper mixed solution and the precipitant solution are co-precipitated at 70°C for 30 minutes, with a pH of 5.0. After the precipitation reaction is complete, the precipitate slurry is filtered and washed several times to obtain a catalyst precursor filter cake. Dissolve 104 g of potassium carbonate and 28 g of Ba(OH)₂ in 1.5 kg of deionized water to prepare the K promoter precursor and Ba promoter aqueous solution. 2.63 kg of a silica sol solution with a silica mass concentration of 20% and aqueous solutions of Ba and K additive precursors were sequentially added to the catalyst precursor filter cake for slurrying. The slurry mass concentration was controlled at 15%, the slurrying temperature was 50°C, and the slurrying time was 40 minutes. After slurrying, CO2 gas was uniformly introduced into the slurry for 120 minutes to obtain a catalyst precursor slurry. Spray drying was performed with the inlet temperature controlled at 320°C and the outlet hot air temperature at 140°C. The spray-dried product was collected and dried at 180°C in an air atmosphere for 8 hours, followed by calcination at 600°C in an air atmosphere for 6 hours to obtain the finished catalyst, designated as Catalyst 3.

[0066] Example 4

[0067] Dissolve 10 kg of Fe(NO₃)₃·9H₂O and 10 g of Cu(NO₃)₂·3H₂O in deionized water to prepare a 50 liter solution. Add 12 kg of 25% ammonia water to the deionized water to prepare a 40 liter precipitant solution. Add the iron- and copper-containing mixed solution to the precipitant solution for precipitation. The precipitation temperature was maintained at 90°C, the precipitation time was 20 minutes, and the endpoint pH was controlled at 6.0. After the precipitation reaction was complete, the precipitate slurry was filtered and washed several times to obtain a catalyst precursor filter cake. The catalyst precursor filter cake was slurried in 1.5 kg of deionized water. A silicon additive precursor aqueous solution was prepared by dissolving 460 g of potassium silicate solution with a modulus of 1 and a silica content of 30% in 1.0 kg of deionized water. The silicon additive precursor aqueous solution was added to the catalyst precursor filter cake slurry and mixed thoroughly. A 5 wt% nitric acid solution was added to the slurry, controlling the endpoint pH to 7.0. The slurry was filtered to obtain a filter cake. 104g of potassium carbonate and 260g of Ba(NO3)2 were fully dissolved in 7kg of deionized water to prepare aqueous solutions of K and Ba additives. The aqueous solutions of K and Ba additives were added to the filter cake for slurrying. The mass concentration of the slurry was controlled to be 15%, the slurrying temperature was 70°C, and the slurrying time was 50 minutes. After the slurrying was completed, CO2 gas was evenly introduced into the slurry and treated for 150 minutes to obtain a catalyst precursor slurry. The inlet temperature was controlled at 290°C and the outlet hot air temperature was controlled at 120°C for spray drying. The spray-dried product was collected and dried at 200°C in an air atmosphere for 6 hours. It was then calcined at 600°C in an air atmosphere for 8 hours to obtain the finished catalyst, which was recorded as Catalyst 4.

[0068] Example 5

[0069] Dissolve 10 kg of Fe(NO₃)₃·9H₂O, 260 g of Cu(NO₃)₂·3H₂O, and 260 g of Ba(NO₃)₂ in deionized water to prepare a 50 liter solution. Add 3.5 kg of sodium carbonate and 1.73 kg of a sodium silicate solution with a modulus of 1 and a silica concentration of 20% to the deionized water to prepare a 40 liter precipitant solution. Add a mixed solution containing iron, copper, and barium to the precipitant solution for precipitation. The precipitation temperature was maintained at 10°C, the precipitation time was 90 minutes, and the endpoint pH was controlled at 7.0. After the precipitation reaction was complete, the precipitated slurry was filtered and washed several times to obtain a catalyst precursor filter cake. Dissolve 12 g of potassium carbonate in 1.5 kg of deionized water to prepare a K promoter precursor aqueous solution. This K promoter precursor aqueous solution was added to the catalyst precursor filter cake for slurrying. The slurry concentration was controlled at 15% at a temperature of 10°C and a slurry time of 60 minutes to obtain a catalyst precursor slurry. The inlet temperature was controlled at 260°C and the outlet hot air temperature was controlled at 110°C for spray drying. The spray-dried product was collected and dried at 220°C in an air atmosphere for 4 h, and then calcined at 550°C in an air atmosphere for 10 h to obtain a finished catalyst, which was recorded as Catalyst 5.

[0070] Example 6

[0071] Dissolve 10 kg of Fe(NO₃)₃·9H₂O, 10 g of Cu(NO₃)₂·3H₂O, and 26 g of Ba(NO₃)₂ in deionized water to prepare a 50 liter solution. Add 4.5 kg of ammonium carbonate and 120 g of a sodium silicate solution with a modulus of 3.5 and a silica concentration of 30% by mass to the deionized water to prepare a 40 liter precipitant solution. Add a mixed solution containing iron, copper, and barium to the precipitant solution for precipitation. The precipitation temperature was maintained at 30°C, the precipitation time was 30 minutes, and the endpoint pH was controlled at 8.5. After the precipitation reaction, the precipitate was filtered and washed several times to obtain a catalyst precursor filter cake. Dissolve 195 g of potassium carbonate in 1.5 kg of deionized water to prepare an aqueous solution of the K additive precursor. An aqueous solution of a K-promoter precursor and 1.04 kg of a silica sol solution with a 30% silica concentration were added to the catalyst precursor filter cake for slurrying. The slurry concentration was controlled at 15%, the slurry temperature was maintained at 25°C, and the slurry time was 20 minutes to obtain a catalyst precursor slurry. Spray drying was performed with the inlet temperature controlled at 230°C and the outlet hot air temperature at 105°C. The spray-dried product was collected and dried at 250°C in air for 3 hours, followed by calcination at 400°C in air for 12 hours to obtain the finished catalyst, designated Catalyst 6.

[0072] Example 7

[0073] Dissolve 10 kg of Fe(NO₃)₃·9H₂O and 260 g of Cu(NO₃)₂·3H₂O in deionized water to prepare a 50 liter solution. Add 8 kg of 25% ammonia and 690 g of a potassium silicate solution with a modulus of 3.5 and a silica concentration of 20% to the deionized water to prepare a 40 liter precipitant solution. Add the iron- and copper-containing mixed solution to the precipitant solution for precipitation at a temperature of 50°C, a precipitation time of 60 minutes, and an endpoint pH of 5.0. After the precipitation reaction is complete, filter the precipitate slurry and wash several times to obtain a catalyst precursor filter cake. Dissolve 105 g of Ba(OH)₂ in 7 kg of deionized water to prepare a Ba additive aqueous solution. Dissolve 195 g of potassium carbonate in 1.0 kg of deionized water to prepare a K additive precursor aqueous solution. An aqueous solution of Ba and a precursor of K were sequentially added to the catalyst precursor filter cake for slurrying. The slurry concentration was controlled at 15%, the slurry temperature was 30°C, and the slurry time was 30 minutes. After slurrying, CO2 gas was uniformly introduced into the slurry for 180 minutes to obtain a catalyst precursor slurry. Spray drying was performed at an inlet temperature of 200°C and an outlet hot air temperature of 105°C. The spray-dried product was collected and dried at 280°C in air for 2 hours, followed by calcination at 500°C in air for 8 hours to obtain the finished catalyst, designated Catalyst 7.

[0074] Example 8

[0075] Dissolve 10 kg of Fe(NO₃)₃·9H₂O and 10 g of Cu(NO₃)₂·3H₂O in deionized water to prepare a 50 liter solution. Add 9 kg of 25% ammonia and 2.76 kg of a sodium silicate solution with a modulus of 1 and a silica concentration of 20% to the deionized water to prepare a 40 liter precipitant solution. Add the precipitant solution to the iron-copper mixed solution for precipitation at a temperature of 70°C, a precipitation time of 40 minutes, and an endpoint pH of 6.0. After the precipitation reaction is complete, filter the precipitate slurry and wash several times to obtain a catalyst precursor filter cake. Prepare a Ba additive aqueous solution by dissolving 160 g of Ba(NO₃)₂ in 7 kg of deionized water. Prepare a K additive precursor aqueous solution by dissolving 12 g of potassium carbonate in 1.0 kg of deionized water. An aqueous solution of Ba and a precursor of K were sequentially added to the catalyst precursor filter cake for slurrying. The slurry concentration was controlled at 15%, the slurry temperature was 50°C, and the slurry time was 40 minutes. After slurrying, CO2 gas was uniformly introduced into the slurry for 100 minutes to obtain a catalyst precursor slurry. Spray drying was performed with the inlet temperature controlled at 180°C and the outlet hot air temperature at 100°C. The spray-dried product was collected and dried at 300°C in air for 1 hour, followed by calcination at 550°C in air for 8 hours to obtain the finished catalyst, designated Catalyst 8.

[0076] Example 9

[0077] Dissolve 10 kg of Fe(NO₃)₃·9H₂O, 140 g of Cu(NO₃)₂·3H₂O, and 160 g of Ba(NO₃)₂ in deionized water to prepare a 50 liter solution. Add 3 kg of sodium carbonate and 1.73 kg of a sodium silicate solution with a modulus of 3.5 and a silica concentration of 20% to the deionized water to prepare a 40 liter precipitant solution. The mixed solution containing iron, copper, and barium was co-precipitated with the precipitant solution at a temperature of 30°C, a precipitation time of 80 minutes, and a pH of 7.0. After the precipitation reaction was complete, the precipitated slurry was filtered and washed several times to obtain a catalyst precursor filter cake. Dissolve 150 g of potassium nitrate in 1.5 kg of deionized water to prepare a K promoter precursor aqueous solution. This K promoter precursor aqueous solution was added to the catalyst precursor filter cake and slurried at a concentration of 15% at a temperature of 25°C and a slurry time of 50 minutes to obtain a catalyst precursor slurry. The inlet temperature was controlled at 380°C and the outlet hot air temperature was controlled at 220°C for spray drying. The spray-dried product was collected and dried at 120°C in an air atmosphere for 12 hours, and then calcined at 600°C in an air atmosphere for 10 hours to obtain a finished catalyst, which was recorded as Catalyst 9.

[0078] Example 10

[0079] Dissolve 10 kg of Fe(NO₃)₃·9H₂O, 10 g of Cu(NO₃)₂·3H₂O, and 26 g of Ba(NO₃)₂ in deionized water to prepare a 50 liter solution. Add 4.5 kg of ammonium carbonate and 460 g of a sodium silicate solution with a modulus of 1 and a silica concentration of 30% by mass to the deionized water to prepare a 40 liter precipitant solution. The precipitant solution was added to a mixed solution containing iron, copper, and barium to precipitate at a temperature of 50°C, a precipitation time of 50 minutes, and an endpoint pH of 8.5. After the precipitation reaction was complete, the precipitate slurry was filtered and washed several times to obtain a catalyst precursor filter cake. Dissolve 20 g of potassium nitrate in 1.5 kg of deionized water to prepare a K promoter precursor aqueous solution. This K promoter precursor aqueous solution was added to the catalyst precursor filter cake for slurrying at a concentration of 15% by mass, a temperature of 30°C, and a slurry time of 60 minutes to obtain a catalyst precursor slurry. The inlet temperature was controlled at 350°C and the outlet hot air temperature was controlled at 150°C for spray drying. The spray-dried product was collected and dried at 150°C in an air atmosphere for 10 hours, and then calcined at 400°C in an air atmosphere for 9 hours to obtain a finished catalyst, which was recorded as Catalyst 10.

[0080] Example 11

[0081] Dissolve 10 kg of Fe(NO₃)₃·9H₂O and 260 g of Cu(NO₃)₂·3H₂O in deionized water to prepare a 50-liter solution. Add 8 kg of 25% ammonia water to the deionized water to prepare a 40-liter precipitant solution. Add the precipitant solution to the iron-copper mixed solution to precipitate. The precipitation temperature is controlled at 90°C, the precipitation time is 20 minutes, and the endpoint pH is controlled at 5.0. After the precipitation reaction is complete, filter the precipitated slurry and wash several times to obtain a catalyst precursor filter cake. Prepare a Ba additive aqueous solution by dissolving 170 g of Ba(OH)₂ in 7 kg of deionized water. Prepare a K additive precursor aqueous solution by dissolving 290 g of potassium nitrate in 0.5 kg of deionized water. An aqueous solution of Ba additive, an aqueous solution of K additive precursor, and 1.84 kg of a silica sol solution with a silica mass concentration of 30% were sequentially added to the catalyst precursor filter cake for slurrying. The slurry mass concentration was controlled at 15%, the slurry temperature was 70°C, and the slurry time was 20 minutes. After slurrying, CO2 gas was uniformly introduced into the slurry for 130 minutes to obtain a catalyst precursor slurry. Spray drying was performed with an inlet temperature of 320°C and an outlet hot air temperature of 130°C. The spray-dried product was collected and dried at 180°C in an air atmosphere for 8 hours, followed by calcination at 600°C in an air atmosphere for 4 hours to obtain the finished catalyst, designated as Catalyst 11.

[0082] Example 12

[0083] Dissolve 10 kg of Fe(NO₃)₃·9H₂O and 140 g of Cu(NO₃)₂·3H₂O in deionized water to prepare a 50 liter solution. Add 9 kg of 25% ammonia and 630 g of a potassium silicate solution with a modulus of 3.5 and a silica concentration of 30% to the deionized water to prepare a 40 liter precipitant solution. The iron-copper mixed solution and the precipitant solution are co-precipitated at 90°C for 20 minutes, with a pH of 6.0. After the precipitation reaction is complete, the precipitate slurry is filtered and washed several times to obtain a catalyst precursor filter cake. Prepare a Ba additive aqueous solution by dissolving 26 g of Ba(NO₃)₂ in 1.5 kg of deionized water. An aqueous solution of Ba additive and 530 g of potassium silicate solution with a modulus of 3.5 and a silica mass concentration of 30% were sequentially added to the catalyst precursor filter cake for slurrying. The slurry mass concentration was controlled at 15%, the slurry temperature was 70°C, and the slurry time was 30 minutes. After slurrying, CO2 gas was uniformly introduced into the slurry for 80 minutes to obtain a catalyst precursor slurry. Spray drying was performed with an inlet temperature of 290°C and an outlet hot air temperature of 120°C. The spray-dried product was collected and dried at 200°C in an air atmosphere for 6 hours, followed by calcination at 600°C in an air atmosphere for 4 hours to obtain the finished catalyst, designated as Catalyst 12.

[0084] Example 13

[0085] Dissolve 10 kg of Fe(NO₃)₃·9H₂O, 140 g of Cu(NO₃)₂·3H₂O, and 260 g of Ba(NO₃)₂ in deionized water to prepare a 50 liter solution. Add 3 kg of sodium carbonate and 750 g of a silica sol solution with a 25% silica concentration to the deionized water to prepare a 40 liter precipitant solution. Add the precipitant solution to a mixed solution containing iron, copper, and barium to precipitate. The precipitation temperature was controlled at 70°C, the precipitation time was 30 minutes, and the endpoint pH was controlled at 7.0. After the precipitation reaction was complete, the precipitated slurry was filtered and washed several times to obtain a catalyst precursor filter cake. A K additive precursor aqueous solution was prepared by dissolving 630 g of a potassium silicate solution with a modulus of 3.5 and a 25% silica concentration in 1.0 kg of deionized water. An aqueous solution of a K-promoter precursor was added to the catalyst precursor filter cake for slurrying. The slurry concentration was controlled at 15%, the slurry temperature was maintained at 50°C, and the slurry time was 40 minutes to obtain a catalyst precursor slurry. Spray drying was performed with the inlet temperature at 260°C and the outlet hot air temperature at 110°C. The spray-dried product was collected and dried at 220°C in air for 4 hours. It was then calcined at 450°C in air for 6 hours to obtain the finished catalyst, designated Catalyst 13.

[0086] Example 14

[0087] Dissolve 10 kg of Fe(NO₃)₃·9H₂O, 30 g of Cu(NO₃)₂·3H₂O, and 130 g of Ba(NO₃)₂ in deionized water to prepare a 50 liter solution. Add 4.5 kg of ammonium carbonate to the deionized water to prepare a 40 liter precipitant solution. A mixed solution containing iron, copper, and barium is co-precipitated with the precipitant solution at 30°C for 70 minutes, with a pH of 8.5. After the precipitation reaction is complete, the precipitated slurry is filtered and washed several times to obtain a catalyst precursor filter cake. A K additive precursor aqueous solution is prepared by dissolving 580 g of a potassium silicate solution with a modulus of 3.5 and a silica concentration of 25% in 0.5 kg of deionized water. An aqueous solution of a K-promoter precursor and 1.08 kg of a silica sol solution with a 25% silica concentration were sequentially added to the catalyst precursor filter cake for slurrying. The slurry concentration was controlled at 15%, the slurry temperature was maintained at 25°C, and the slurry time was 50 minutes to obtain a catalyst precursor slurry. Spray drying was performed with the inlet temperature controlled at 230°C and the outlet hot air temperature at 105°C. The spray-dried product was collected and dried at 250°C in air for 3 hours, followed by calcination at 550°C in air for 6 hours to obtain the finished catalyst, designated Catalyst 14.

[0088] Example 15

[0089] Dissolve 10 kg of Fe(NO₃)₃·9H₂O and 70 g of Cu(NO₃)₂·3H₂O in deionized water to prepare a 50 liter solution. Add 8 kg of 25% ammonia and 770 g of a sodium silicate solution with a modulus of 3.5 and a 25% silica concentration to the deionized water to prepare a 40 liter precipitant solution. The iron-copper mixed solution and the precipitant solution are co-precipitated at 50°C for 40 minutes, with a pH of 5.0. After the precipitation reaction is complete, the precipitate slurry is filtered and washed several times to obtain a catalyst precursor filter cake. Prepare a Ba additive aqueous solution by dissolving 85 g of Ba(OH)₂ in 7 kg of deionized water. Prepare a K additive precursor aqueous solution by dissolving 110 g of potassium nitrate in 0.5 kg of deionized water. An aqueous solution of Ba and a precursor of K were sequentially added to the catalyst precursor filter cake for slurrying. The slurry concentration was controlled at 15%, the slurry temperature was 30°C, and the slurry time was 60 minutes. After slurrying, CO2 gas was uniformly introduced into the slurry for 100 minutes to obtain a catalyst precursor slurry. Spray drying was performed with the inlet temperature controlled at 200°C and the outlet hot air temperature at 100°C. The spray-dried product was collected and dried at 280°C in air for 2 hours. It was then calcined at 550°C in air for 4 hours to obtain the finished catalyst, designated Catalyst 15.

[0090] Example 16

[0091] Dissolve 10 kg of Fe(NO₃)₃·9H₂O and 180 g of Cu(NO₃)₂·3H₂O in deionized water to prepare a 50 liter solution. Add 9 kg of 25% ammonia and 550 g of a sodium silicate solution with a modulus of 3.5 and a 25% silica concentration to the deionized water to prepare a 40 liter precipitant solution. The iron-copper mixed solution and the precipitant solution are co-precipitated at a temperature of 10°C for 90 minutes, with a pH of 6.0. After the precipitation reaction is complete, the precipitate slurry is filtered and washed several times to obtain a catalyst precursor filter cake. Prepare a Ba additive aqueous solution by dissolving 138 g of Ba(OH)₂ in 7 kg of deionized water. Prepare a K additive precursor aqueous solution by dissolving 210 g of potassium nitrate in 0.5 kg of deionized water. An aqueous solution of Ba additive, an aqueous solution of K additive precursor, and 550 g of a silica sol solution with a silica mass concentration of 25% were sequentially added to the catalyst precursor filter cake for slurrying. The slurry concentration was controlled at 15%, the slurry temperature was 10°C, and the slurry time was 60 minutes. After slurrying, CO2 gas was uniformly introduced into the slurry for 100 minutes to obtain a catalyst precursor slurry. Spray drying was performed with the inlet temperature controlled at 180°C and the outlet hot air temperature at 100°C. The spray-dried product was collected and dried at 300°C in air for 1 hour, followed by calcination at 600°C in air for 2 hours to obtain the finished catalyst, designated Catalyst 16.

[0092] Comparative Example 1

[0093] Except for not adding Ba(NO3)2, the remaining steps were the same as those in Example 1 to obtain a finished catalyst, which was recorded as comparative agent 1.

[0094] Comparative Example 2

[0095] Except for not adding Ba(NO3)2, the remaining steps were the same as those in Example 2 to obtain a finished catalyst, which was recorded as comparative agent 2.

[0096] Comparative Example 3

[0097] Except that Ba(NO3)2 was not added (only 104g potassium carbonate was fully dissolved in 1.0kg deionized water to prepare the K additive precursor aqueous solution) and CO2 treatment was not performed, the remaining steps were the same as in Example 3 to obtain a finished catalyst, which was recorded as comparative agent 3.

[0098] Comparative Example 4

[0099] Except for using 815g Ca(NO3)2·4H2O instead of 260g Ba(NO3)2, the remaining steps were the same as those in Example 4 to obtain a finished catalyst, which was recorded as comparative agent 4.

[0100] Comparative Example 5

[0101] Except for using 1458g Mg(NO3)2·6H2O instead of 260g Ba(NO3)2, the remaining steps were the same as those in Example 5 to obtain a finished catalyst, which was recorded as Comparative Agent 5.

[0102] Comparative Example 6

[0103] Except for using 33.5g Sr(NO3)2 instead of 26g Ba(NO3)2, the remaining steps are the same as those in Example 6 to obtain a finished catalyst, which is recorded as comparative agent 6.

[0104] Comparative Example 7

[0105] Except for using 300g Ba(NO3)2 to fully dissolve in 7kg deionized water to prepare the Ba auxiliary agent aqueous solution, the remaining steps are the same as Example 7 to obtain a finished catalyst, which is recorded as comparative agent 7.

[0106] Comparative Example 8

[0107] Except for using 13g Ba(NO3)2 to fully dissolve in 0.5kg deionized water to prepare the Ba auxiliary agent aqueous solution, the remaining steps are the same as Example 8 to obtain a finished catalyst, which is recorded as comparative agent 8.

[0108] Comparative Example 9

[0109] The catalyst was prepared according to the example of Chinese invention patent CN 107684910B, and the catalyst composition was 100Fe:6Cu:5K:2.1Ca:1.9Ba:20SiO2.

[0110] Comparative Example 10

[0111] The catalyst was prepared according to the example of Chinese invention patent CN 107913714B, and the catalyst composition was 100Fe:5.1Cu:2.9K:4.3Nd:1.5Ba:20.7SiO2.

[0112] Comparative Example 11

[0113] Except that CO2 gas was not introduced into the slurry for treatment after slurrying, the remaining steps were the same as those in Example 11, and a finished catalyst was obtained, which was recorded as comparative agent 11.

[0114] Test Case

[0115] Test equipment: 1L stirred tank.

[0116] Test conditions: 10 g of the catalysts prepared in Examples 1-16 and Comparative Examples 1-11 were mixed with 300 mL of liquid paraffin and placed in a 1 L stirred tank. After reduction activation, the reaction was switched to Fischer-Tropsch synthesis reaction conditions. The process conditions for reduction activation and Fischer-Tropsch synthesis reaction were as follows:

[0117] (1) Reduction activation: Use synthesis gas with a volume ratio of H2 / CO of 20:1 to reduce the reaction mixture by heating (4 h at 30-200 °C, 10 h at 200-265 °C, and 24 h at a constant temperature of 265 °C). The space velocity of the synthesis gas is 8000 h -1 , the reduction gauge pressure is 3.0MPa.

[0118] (2) Fischer-Tropsch synthesis: After the reduction is completed, the H2 / CO volume ratio of the synthesis gas is adjusted to 3:1 and stabilized for a period of time until the gas phase composition in the reaction tail gas basically does not change with time, which is recorded as the reaction zero point.

[0119] (3) Data calculation: The molar number of CO in the feed was measured and analyzed at the feed port of the stirred tank, and the molar number of CO, CO2, and CH4 in the discharge was measured and analyzed at the discharge port. The CO conversion rate (%), CO2 selectivity (%), and CH4 selectivity (%) were calculated using the following formulas:

[0120] CO conversion rate % = [(CO moles in feed - CO moles in discharge) / CO moles in feed] × 100%;

[0121] CO2 selectivity % = [CO2 moles in the discharge / (CO moles in the feed - CO moles in the discharge)] × 100%;

[0122] CH4 selectivity % = [mole number of CH4 in the discharge / (mole number of CO in the feed × CO conversion rate % × (1-CO2 selectivity %))] × 100%.

[0123] The deactivation rate of the catalyst refers to the rate at which the catalyst activity (carbon monoxide conversion rate) decreases from the reaction plateau to the end of the reaction, and the unit is % / h.

[0124] The composition, properties and reaction performance results of the catalysts prepared in Examples 1-16 are shown in Table 1, and the composition, properties and reaction performance results of the catalysts prepared in Comparative Examples 1-11 are shown in Table 2.

[0125] Table 1

[0126] Table 2

[0127] It can be seen from the results in Table 1 and Table 2 that, compared with catalysts to which no Ba element is added (e.g., Comparative Examples 1-3), catalysts to which other types of alkaline earth metal elements are added (e.g., Comparative Examples 4-6), catalysts to which too much or too little Ba element is added (e.g., Comparative Examples 7-8), and existing catalysts to which two metal additives are added (e.g., Comparative Examples 9-10), the Fischer-Tropsch synthesis iron-based catalyst provided by the present invention has a higher CO conversion rate and lower CO2 selectivity and CH4 selectivity, indicating that it has excellent catalytic activity; the Fischer-Tropsch synthesis iron-based catalyst provided by the present invention also has a lower deactivation rate, indicating that it has good thermal stability, which is particularly important for highly exothermic Fischer-Tropsch synthesis reactions under high catalytic activity.

[0128] In addition, it can be seen from Comparative Example 11 that if the Ba element on the catalyst surface is not in the form of barium carbonate, the selectivity of CO2 will be significantly increased and the stability of the catalyst will be significantly reduced.

[0129] Unless otherwise defined, the terms used in the present invention have the same meanings as those commonly understood by those skilled in the art.

[0130] The embodiments described in the present invention are for illustrative purposes only and are not intended to limit the scope of protection of the present invention. Those skilled in the art may make various other substitutions, changes and improvements within the scope of the present invention. Therefore, the present invention is not limited to the above-mentioned embodiments, but is only limited by the claims.

Claims

1. A Fischer-Tropsch synthesis iron-based catalyst comprising Fe, Cu, K and SiO 2 , It is characterized in that The surface of the Fischer-Tropsch synthesis iron-based catalyst contains 0.3-3% of Ba element in terms of molar percentage.

2. The Fischer-Tropsch synthesis iron-based catalyst according to claim 1, It is characterized in that The Ba element on the surface of the Fischer-Tropsch synthesis iron-based catalyst exists in the form of barium carbonate; and / or The specific surface area of ​​the Fischer-Tropsch synthesis iron-based catalyst is 100 to 250 m 2 / g.

3. The Fischer-Tropsch synthesis iron-based catalyst according to claim 1 or 2, It is characterized in that The Fischer-Tropsch synthesis iron-based catalyst comprises the following components in mass ratio: Fe element: Cu element: K element: Ba element: SiO 2 =100:0.2~5:0.5~8:1~10:10~40.

4. The method for preparing the Fischer-Tropsch synthesis iron-based catalyst according to any one of claims 1 to 3, It is characterized in that The following steps are involved: S1: forming a mixed aqueous solution of a water-soluble salt of Fe and a water-soluble salt of Cu, preparing a precipitant solution, and adding 0 to 100 wt % of a silicon source to the precipitant solution; S2: contacting the mixed aqueous solution with the precipitant solution to perform a precipitation reaction, and separating the obtained precipitation product after the reaction is completed; S3: mixing the precipitated product with the K additive precursor aqueous solution and the remaining silicon source to form a mixed slurry and performing slurry treatment to obtain a catalyst precursor slurry; as well as S4: drying and calcining the catalyst precursor slurry; The method of adding the Ba element includes: adding a water-soluble salt of Ba to the mixed aqueous solution of step S1, and making the concentration of Ba lower than 2.0g Ba / 100g water; or The water-soluble salt of Ba is prepared into an aqueous solution with a concentration lower than 2.0 g Ba / 100 g water, and then added into the mixed slurry of step S3.

5. The preparation method according to claim 4, It is characterized in that The water-soluble salt of Fe is nitrate, hydrochloride or hydrate of Fe, and the water-soluble salt of Cu is nitrate, hydrochloride or hydrate of Cu; preferably, the concentration of Fe in the mixed aqueous solution is 5-100 g / L; and / or The precipitant is selected from one or more of sodium carbonate, ammonia water, ammonium carbonate, sodium hydroxide, potassium hydroxide, and potassium carbonate; preferably, its concentration is 50-150 g / L.

6. The preparation method according to claim 4 or 5, It is characterized in that The silicon source is selected from one or more of potassium silicate solution, sodium silicate solution and silica sol solution, wherein SiO 2 The concentration is 10 to 50 wt%; and / or The water-soluble salt of Ba is one or both of barium nitrate and barium hydroxide; and / or The K additive precursor is one or more of potassium nitrate, potassium carbonate, potassium bicarbonate, potassium silicate and potassium chloride.

7. The preparation method according to any one of claims 4 to 6, It is characterized in that In step S2, the precipitation temperature of the precipitation reaction is 5 to 95° C., the precipitation time is 5 to 100 min, and the pH value during the precipitation process is controlled at 5 to 10; and / or In the step S3, the slurrying temperature of the slurrying treatment is 10-80° C., the slurrying time is 10-80 min, and the concentration of the slurry is controlled to be 10-20 wt % during the slurrying treatment.

8. The preparation method according to any one of claims 4 to 7, It is characterized in that The step S3 also includes: after the slurry treatment is completed, CO 2 Gas treatment for 0 to 180 min, preferably with CO 2 Gas treatment takes 30 to 180 minutes.

9. The preparation method according to any one of claims 4 to 8, It is characterized in that In the step S4, the drying includes the following process: firstly, the catalyst precursor slurry is spray-dried, and the obtained powder is dried in an air atmosphere at 110-300° C. for 1-12 hours; Preferably, the hot air inlet temperature of the spray drying is 180-400°C, and the exhaust air outlet temperature is 100-220°C.

10. The preparation method according to any one of claims 4 to 9, It is characterized in that In the step S4, the calcination temperature is 400-600° C. and the calcination time is 1-15 hours.

Citation Information

Patent Citations

  • Iron base catalyst for fischer-tropsch synthesis and preparation method thereof

    CN101293206A

  • Iron catalyst containing titanium deposition for catalyzing Fischer-Tropsch synthesis reaction and method for producing the same

    CN101298046A

  • A Fischer-Tropsch synthesis iron-based catalyst and its preparation method

    CN107684910B

  • Iron-based catalysts for Fischer-Tropsch synthesis, their preparation methods, and Fischer-Tropsch synthesis methods

    CN107913714B

  • Iron base catalyzer through Fischer-Tropsch synthesis and preparation method

    CN1245255C

Cited By

  • Preparation method and application of iron-based catalyst constructed by multi-aid confinement

    CN121490772A

  • Preparation method and application of iron-based catalyst with multi-aid limited construction

    CN121490772B