Continuous production line and process for double-sided coating of current collector of lithium battery
By combining magnetron sputtering, evaporation and electroplating technologies in the lithium battery coating process, a high-quality electronic composite film is formed, which solves the problems of insufficient coating quality and low efficiency in the existing technology and achieves an efficient and environmentally friendly production process. .
Patent Information
- Application Number
- PCT/CN2024/075959
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-24
- Filing Date
- 2024-02-05
- Publication Date
- 2024-10-31
AI Technical Summary
The existing lithium battery coating process has problems such as insufficient coating quality, low efficiency, difficulty in one-time realization, incoherent processes, poor integrated molding effect, and environmental pollution, especially when thicker conductive films are plated on the surface of plastic substrates.
Use magnetron sputtering and/or evaporation to prepare nano-films on the surface of plastic substrates, and then thicken them into micron films through electroplating. Combined with activation cleaning devices to improve the preparation quality of composite films, and recycle industrial wastewater through electrolysis. of metal to reduce environmental pollution.
It achieves high bonding strength between the plastic substrate and the electroplated film layer, uniformity and density of the electronic composite film, improves production efficiency and quality, reduces pollution, and achieves resource recycling and zero emissions.
Smart Images

Figure CN2024075959_31102024_PF_FP_ABST
Abstract
Description
A continuous production line and process for double-sided coating of lithium battery current collectors Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and in particular to a continuous production line and process for double-sided coating of lithium battery current collectors. Background Art
[0002] The safety and energy density of lithium batteries are currently receiving significant attention. Regarding safety, the flammability of the electrolyte within lithium batteries and their high energy density can lead to thermal runaway during use, which can subsequently cause fires and spontaneous combustion in electric vehicles. Thermal runaway in lithium batteries occurs when high temperatures cause exothermic reactions in the active materials within the battery, releasing significant amounts of heat. This rapidly increases the battery temperature and causes changes in internal materials, including separator rupture and direct contact between the positive and negative electrodes, leading to internal short circuits. Regarding energy density, the battery's energy density, both in terms of volume and mass, determines the range of an electric vehicle. The positive and negative electrode materials are the active energy storage materials in lithium batteries. Copper foil, as a carrier and current collector for the negative electrode material, is crucial in increasing battery energy density. The "Made in China 2025" plan proposes that my country's power battery energy density reach 400 watt-hours / kg by 2025 and 500 watt-hours / kg by 2030. Lithium battery safety issues are becoming increasingly prominent. As lithium-ion batteries move towards higher energy densities, battery safety issues are becoming increasingly prominent, with explosions and leakage being among the most significant safety hazards.
[0003] With the rapid development of the new energy industry, the demand for various raw materials related to the research, development and production of lithium-ion batteries has grown rapidly. At the same time, the direction of battery research and development and improvement focuses on reducing battery size within the limited space of the vehicle, increasing battery capacity within the same space, and thus improving battery performance. In the batteries used in new energy vehicles, aluminum foil and copper foil are used as positive and negative electrode materials. These are thick and weak, resulting in heavy battery weight and prone to battery fluid leakage when impacted. Existing related technologies use electronic composite films to replace traditional aluminum foil and copper foil. The thickness can be reduced to 1 / 2, and the weight is lighter, which can increase the capacity of batteries of the same volume. The high tensile strength during later processing also significantly improves the safety of new energy vehicle batteries. Technical issues
[0004] The electronic composite film is formed by coating a metal conductive layer on the surface of a non-conductive plastic substrate. The existing technology generally uses magnetron sputtering, evaporation coating, electroplating or coating to coat the film. The electroplating method cannot directly coat plastic substrates. In the existing technology, low-concentration acidic solutions such as phosphoric acid, citric acid, hydrochloric acid, nitric acid, sulfuric acid, or mixed acid solutions thereof are generally used to activate the substrate before and after electroplating. The etching effect is poor, and the waste liquid after the activation of the substrate cannot be directly and effectively utilized, which will produce wastewater, waste gas, and waste residue that are harmful to human health and pollute the environment, which is not conducive to production and environmental protection. The coating method for preparing electronic composite thin films is formed by coating and then mechanical pressing, rather than metallurgical bonding. Therefore, the bonding force between the plastic substrate and the conductive layer is not strong, and the performance of the prepared electronic composite film is poor. The magnetron sputtering method and the evaporation coating method have thinner coatings, and the time and cost required to prepare micron-level thin films are high. Although the bonding force of the evaporation coating can meet the coating requirements, it is weaker than that of the magnetron coating. Its uniformity and density are both weaker than those of the magnetron coating, but the coating speed is faster than that of the magnetron coating. However, high-power excitation of high-melting-point metal targets can easily penetrate the plastic substrate due to the high energy. When a plastic substrate needs to be coated with a micron-sized metal conductive layer, the existing coating process is difficult to achieve in one go, and there are problems such as discontinuous processes, poor integrated molding effects, low production efficiency, and environmental pollution.
[0005] To solve the above problems, the present invention proposes a continuous production line and process for double-sided coating of lithium battery current collectors, which first prepares a nanofilm on the surface of a plastic substrate by magnetron sputtering and / or evaporation, and then thickens it into a micron film by electroplating to form an electronic composite film; the use of magnetron sputtering or evaporation to coat the surface of the substrate with a high-density nanofilm can improve the bonding strength between the substrate and the micron film during electroplating, and the time required for thickening into a micron film by electroplating is short and the cost is low; in addition, the production line is also provided with an activation and cleaning device to improve the preparation quality of the composite film, and recovers metals in industrial wastewater by electrolysis to reduce environmental pollution. Technical Solutions
[0006] The purpose of the present invention is to provide a continuous production line and process for double-sided coating of lithium battery current collectors, so as to solve the problems of insufficient coating quality and low efficiency existing in methods such as magnetron sputtering, evaporation or coating, and electroplating, as well as the problems of the existing coating process when coating a thicker conductive film on the surface of a plastic substrate, such as difficulty in one-time realization, discontinuous processes, poor integrated molding effect, low production efficiency, and environmental pollution.
[0007] To achieve the above object, the present invention adopts the following technical solutions:
[0008] A continuous production line for double-sided coating of a lithium battery current collector comprises an unwinding device, a pretreatment device, a first coating device, a first activation and cleaning device, a second coating device, a cleaning and drying device, and a winding device; a plastic substrate output by the unwinding device passes through the pretreatment device, the first coating device, the first activation and cleaning device, the second coating device, and the cleaning and drying device in sequence before entering the winding device; a first activation and cleaning liquid is contained in the first activation and cleaning device, and the first activation and cleaning liquid is a persulfate solution with a pH value of 2-6.
[0009] Preferably, the plastic substrate is driven by rollers arranged in the pretreatment device, the first coating device, the first activation and cleaning device, the second coating device, and the cleaning and drying device, and the linear speed of the rollers is 1m / min-15m / min.
[0010] Preferably, the first activation cleaning device includes a cleaning tank, a spraying device, a liquid storage tank, a first anode, a first cathode, a first circulation pipe, a second circulation pipe, a circulation pump, and a stop valve;
[0011] The output of the liquid storage tank is connected to the input of the spray device through a first circulation pipe, and the input of the liquid storage tank is connected to the output of the cleaning tank through a second circulation pipe. The first circulation pipe and the second circulation pipe are both provided with a circulation pump and a stop valve;
[0012] The bottom of the cleaning tank is also provided with a first anode and a first cathode for electrolytically recovering the waste liquid after etching and cleaning and the waste metals therein;
[0013] The first anode is an inert material selected from one of boron-doped diamond, graphite, Ti4O7, IrO2, RuO2, PbO or Pt, and the first cathode material is selected from one of Ag, Cu, Au, Al, W, Ni, Fe, Pt. The current density is 5-15ASD;
[0014] The spray device is provided with two groups of nozzles, which extend into the cleaning tank and are respectively located on the upper and lower sides of the front and back surfaces of the plastic substrate after surface coating, and spray the first activation cleaning liquid on the front and back surfaces of the plastic substrate to clean and etch the front and back surfaces of the plastic substrate.
[0015] Preferably, the first activation cleaning solution is a mixed solution in which the pH value of a persulfate solution is adjusted to 2-6 by sulfuric acid; the persulfate is selected from one of sodium persulfate, potassium persulfate, and ammonium persulfate; the mass volume concentration of the persulfate solution is 50 g / L-300 g / L; and the molar concentration of sulfuric acid is 0.1 M-1 M.
[0016] Preferably, the first coating device is provided with a vacuum evaporation coating device and / or a magnetron sputtering coating device to coat the first film layer on both the front and back sides of the plastic substrate; the vacuum evaporation coating device includes a first evaporation device and a second evaporation device, and the plastic substrate is coated on one surface by the first evaporation device, and then reversed by a roller, and then enters the second evaporation device to coat the other side of the plastic substrate; the magnetron sputtering coating device includes two components of magnetron sputtering targets placed on the upper and lower sides of the front and back sides of the plastic substrate.
[0017] Preferably, tension sensors in contact with the surface of the plastic substrate are installed at the inlet and outlet of the magnetron sputtering coating device and the vacuum evaporation coating device to detect the surface tension of the plastic substrate.
[0018] Preferably, the second coating device is an electroplating device, which coats the second film layer on both sides of the plastic substrate. The electroplating device includes an electroplating tank, a second cathode, a second anode and an electroplating solution. The second anode is divided into two groups and is arranged in the electroplating tank. The plastic substrate is located between the two groups of second anodes. The first film layer coated on both sides of the plastic substrate serves as the second cathode. The electroplating solution is a mixed solution composed of a salt of the film metal and an acid with a pH value of 3-6; the salt of the film metal is selected from sulfate, nitrate or chloride of at least one metal selected from Cu, Al, Ag, Ni and Zn; the acid is hydrochloric acid or sulfuric acid.
[0019] Preferably, the target material in the magnetron sputtering coating device, the evaporation material in the vacuum evaporation coating device, and the second anode material in the electroplating device are all the same as the film metal or alloy plated on the front and back sides of the plastic substrate, and the metal is selected from one of Cu, Al, Ag, Ni, and Zn, and the alloy is selected from one of Cu-Zn, Al-Zn, Ag-Cu, Ag-Ni, Ag-Fe, Ni-Cu, Cu-Zn-Ni, and Cu-Ni-Sn.
[0020] Preferably, a continuous production process for double-sided coating of a lithium battery current collector adopts the above-mentioned continuous production line for double-sided coating of a lithium battery current collector, comprising the following steps:
[0021] S1, the unwinding device unwinds the plastic substrate, which is then alkali-washed, washed with water, and dried by the pretreatment device and then enters the first coating device;
[0022] S2. The first coating device performs evaporation or sputtering, or evaporation followed by sputtering, on the front and back surfaces of the plastic substrate under a protective atmosphere to coat the front and back surfaces of the plastic substrate with a first film layer, and then transports the plastic substrate to a first activation and cleaning device;
[0023] The protective atmosphere is argon, and the argon flow rate is 10-50sccm;
[0024] The evaporation process parameters are: power 50W-2200W, vacuum degree 10 -6 Pa~10 -3 Pa, evaporation rate is 0.1A / s-10A / s;
[0025] The sputtering coating process parameters are: sputtering power 50W-300W, sputtering temperature 25℃-120℃, vacuum degree 0.1Pa-10Pa;
[0026] S3, the first activation cleaning device sprays the first activation cleaning liquid onto the front and back surfaces of the plastic substrate through two sets of nozzles provided in the spray device, cleans and etches the first film layer plated on the front and back surfaces of the plastic substrate, and then transports it to the second coating device; at the same time, the first activation cleaning device electrolytically recovers the waste liquid and the waste metals therein after etching and cleaning through the first anode and the first cathode provided at the bottom of the cleaning tank;
[0027] The first activation cleaning solution is a mixed solution of a persulfate solution adjusted to a pH of 2-6 by sulfuric acid; the persulfate is selected from one of sodium persulfate, potassium persulfate, and ammonium persulfate; the mass volume concentration of the persulfate solution is 50g / L-300g / L; the molar concentration of the sulfuric acid is 0.1M-1M; the spraying speed is 10L / min-30L / min, the temperature is 40°C-60°C, and the distance between the nozzle and the first film layer is 5cm-10cm;
[0028] S4, the second coating device uses the first film layer coated on the front and back sides of the plastic substrate as the second cathode, and adopts a double-sided electroplating method to coat the second film layer on the surface of the second cathode to form an electronic composite film, which is then sent to the cleaning and drying device;
[0029] The electroplating process parameters are: the plating solution temperature is 40°C-60°C, the current density of the second cathode is 1A / dm 2 -6A / dm 2 The electroplating solution is a mixed solution of a sulfate, nitrate, chloride, hydrochloric acid, or sulfuric acid of at least one metal selected from Cu, Al, Ag, Ni, and Zn, with a pH value of 3-6, and a mass concentration of the metal salt solution of 50 mg / L-200 g / L;
[0030] S5. The cleaning and drying device cleans and dries the electronic composite film, and then sends it to the winding device for winding.
[0031] Preferably, a second activation cleaning device is provided between the second coating device and the cleaning and drying device to activate and clean the electronic composite film; the structure of the second activation cleaning device is the same as that of the first activation cleaning device, wherein a second activation cleaning liquid is contained therein to clean and etch the second film layer, and the cleaning waste liquid and the waste metal therein are electrolytically recovered, and the second activation cleaning liquid is a mixed solution obtained by adjusting the pH value of the persulfate solution to 2-6 by sulfuric acid; the persulfate is selected from one of sodium persulfate, potassium persulfate, and ammonium persulfate; the mass volume concentration of the persulfate solution is 50g / L-300g / L; the molar concentration of sulfuric acid is 0.1M-1M; the injection speed is 10L / min-30L / min, and the temperature is 40°C-60°C.
[0032] Preferably, in S4, after the electronic composite film is formed on the surface of the plastic substrate, it is sent to a second activation and cleaning device to activate and clean the electronic composite film; then, it is sent to a cleaning and drying device for cleaning and drying, and then sent to a winding device for winding;
[0033] The second activation cleaning solution is a mixed solution of a persulfate solution adjusted to a pH value of 2-6 by sulfuric acid; the persulfate is selected from one of sodium persulfate, potassium persulfate, and ammonium persulfate; the mass volume concentration of the persulfate solution is 50g / L-300g / L; the molar concentration of the sulfuric acid is 0.1M-1M; the injection speed is 10L / min-30L / min, the temperature is 40°C-60°C, and the distance between the nozzle and the first film layer is 5cm-10cm.
[0034] Preferably, the plastic substrate is one of plastic substrates including polyethylene terephthalate (PET), polybutylene naphthalate (PBN), polybutylene terephthalate (PBT), polypropylene (PT), polycyclohexylene dimethylene terephthalate resin (PCT), and polyimide (PI), and the thickness of the plastic substrate is 5um-200um.
[0035] Preferably, the magnetron sputtering coating time is 20s-600s, preferably 60s-200s, and the sputtering coating thickness is 20nm-500nm, preferably 50nm-150nm; the evaporation coating time is 20s-600s, preferably 40s-100s, and the evaporation coating thickness is 20nm-500nm, preferably 55nm-150nm; the electroplating time is 5min-60min, and the electroplating coating thickness is 1um-20um. Beneficial effects
[0036] Compared with the existing technology, the production line and process of the present invention have the following technical effects:
[0037] (1) The present invention innovatively proposes a continuous production line for double-sided coating of lithium battery current collectors, including a first coating device, a second coating device, a first activation cleaning device and other devices. The first coating device coats the first layer of metal nanofilm on both sides of the plastic substrate, thereby improving the bonding strength between the plastic substrate and the electroplated film layer. The second coating device coats the second layer of metal microfilm on both sides of the plastic substrate, thereby forming an electronic composite film with uniform thickness and a thicker conductive layer. The first activation cleaning device contains an acidic persulfate solution as a first activation cleaning liquid, which can clean away impurities and oxide films remaining on the surface of the first film layer on the plastic substrate, and micro-etch the first film layer, thereby further improving the bonding strength and production quality of the electronic composite film. The production line not only has a coherent process and a good integrated molding effect, but also significantly improves production efficiency and quality, and the electronic composite film can be molded in one step.
[0038] (2) The first activated cleaning device uses electrolysis to recycle the cleaning waste liquid and the waste metals therein, which facilitates the recycling of resources, reduces the cost of industrial water replacement, and reduces emission pollution; the persulfate in the cleaning waste liquid is regenerated by anodic oxidation, and the oxidation regeneration rate can reach 60-80%. The cleaning waste liquid is 100% recycled, truly achieving zero emissions. The first activated cleaning liquid is regenerated by electrolysis technology without adding any chemical additives or additives. The quality of the micro-etching liquid is guaranteed. The first activated cleaning liquid has a strong catalytic effect and can significantly accelerate the reaction rate; the waste metal ions are extracted through the cathode. The extracted metal is of good quality and has a purity of up to 99.99%, which can increase corporate profits. Inert materials are used as anodes, and the service life is long. Long life, high current efficiency, and electricity cost saving; after the first activation cleaning device micro-etches the first film layer on the surface of the plastic substrate, the bonding strength between the second film layer and the first film layer during electroplating will be greatly improved, so that the quality of the film layer is effectively improved; after being cleaned by the first activation cleaning device, a trace amount of acidic persulfate solution is attached to the surface of the plastic substrate, and the persulfate ions in the solution can effectively prevent the formation of oxide film or reduce the existing trace oxide film, thereby effectively ensuring the activation state of the surface of the first film layer, and then ensuring the bonding strength between the second conductive film and the first conductive film during plating. After the plastic substrate carrying persulfate ions and hydrogen ions on the surface enters the electroplating device, the cathode current density is reduced and the electroplating efficiency is improved.
[0039] (3) The production line includes a variety of combinations, one of which is "evaporation coating + sputtering coating + activation cleaning + electroplating + secondary activation cleaning". First, evaporation coating is used to quickly and gently form a film layer with moderate bonding strength. Under the protection of the evaporation coating layer, magnetron sputtering coating is used to effectively avoid the risk of the plastic substrate being punctured when sputtering a high-melting-point target material, and can effectively improve the uniformity and density of the film layer. Then, a thicker micron film is plated by electroplating. Compared with the existing technology, the coating speed, quality and efficiency are greatly improved, avoiding the defects of too long coating time when using evaporation coating and magnetron sputtering to plate micron films alone, and the defect that electroplating cannot achieve the bonding between the film metal and the plastic substrate.
[0040] (4) The production line is also optionally equipped with a second activation cleaning device after the electroplating device, which can not only clean the surface of the electronic composite film, but also micro-etch the surface of the electronic composite film. The second activation cleaning device can even adjust the cleaning and etching effects by controlling the concentration of persulfate, thereby meeting the needs of different electronic composite film products;
[0041] (5) A tension sensor is installed in the first coating device to monitor the surface tension of the plastic substrate in real time to prevent the plastic substrate from being stretched, deformed or even broken due to excessive tension, or wrinkled due to too low tension. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] FIG1 is a process flow chart of a continuous production line for double-sided coating of lithium battery current collectors.
[0043] FIG2 is a schematic diagram of a continuous coating production line according to Example 1 of the present invention.
[0044] FIG3 is a schematic diagram of a continuous coating production line according to Example 2 of the present invention.
[0045] FIG4 is a schematic diagram of a continuous coating production line according to Example 3 of the present invention.
[0046] FIG5 is a schematic structural diagram of the magnetron sputtering coating device of the present invention.
[0047] FIG6 is a schematic structural diagram of the vacuum evaporation coating device of the present invention.
[0048] FIG7 is a schematic structural diagram of the electroplating device of the present invention.
[0049] FIG8 is a schematic diagram of a first activation cleaning device according to the present invention, wherein FIG8( a ) is a top view of the first activation cleaning device according to the present invention, and FIG8( b ) is an AA cross-sectional view of FIG8( a ).
[0050] Figure 9 is a schematic diagram of the electronic composite membranes of Examples 1-6, wherein Figure 9(a) is a schematic diagram of the electronic composite membranes of Examples 1 and 4, Figure 9(b) is a schematic diagram of the electronic composite membranes of Examples 2 and 5, and Figure 9(c) is a schematic diagram of the electronic composite membranes of Examples 3 and 6.
[0051] Figure 10 is a schematic diagram of the activation principle of the first and second activation cleaning devices of Examples 1 and 4, wherein Figure 10 (a) is a schematic diagram of the activation principle of the first activation cleaning device of Examples 1 and 4, and Figure 10 (b) is a schematic diagram of the activation principle of the second activation cleaning device of Examples 1 and 4.
[0052] In the picture:
[0053] 1 unwinding device; 2 pretreatment device; 21 alkali washing device; 22 water washing device; 23 first drying device;
[0054] 3 first coating device; 31 magnetron sputtering coating device; 311 magnetron sputtering target; 312 vacuum chamber; 313 vacuum pump group; 314 gas mass flow controller; 315 vacuum sealing assembly; 316 partition; 317 water cooling roller; 318 water cooling plate;
[0055] 32 vacuum evaporation coating device; 32a first evaporation device; 32b second evaporation device; 321 evaporation boat; 322 wire unwinding device; 323 vacuum chamber; 324 vacuum pump assembly; 325 vacuum sealing assembly; 326 water-cooled roller; 33 tension sensor;
[0056] 4a first activation and cleaning device; 4b second activation and cleaning device; 41 cleaning tank; 42 spray device; 43 liquid storage tank; 44 first anode; 45 first cathode; 46a first circulation pipe; 46b second circulation pipe; 47 circulation pump; 48 stop valve; 49 partition;
[0057] 5 electroplating device; 51 electroplating tank; 52 second cathode; 53 second anode;
[0058] 6. Cleaning and drying device; 7. Winding device; 8. Plastic substrate; 9. Roller;
[0059] 8A The first film layer plated by the magnetron sputtering coating device; 8B The first film layer plated by the vacuum evaporation coating device; 8C The second film layer plated by the electroplating device. Modes for Carrying Out the Invention
[0060] The following is a clear and complete explanation of the technical solution of the present invention in conjunction with the embodiments and drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0061] In the description of the present invention, it should be noted that the terms "front," "back," "upper," "lower," "inner," "upper," "middle," "bottom," "one end," "other end," and the like, indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings and are intended solely to facilitate and simplify the description of the present invention. They are not intended to indicate or imply that the devices or components referred to must have, be constructed, or operate in a specific orientation, and therefore should not be construed as limiting the present invention. Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.
[0062] In the description of the present invention, it should be noted that, unless otherwise expressly specified or limited, the terms "provided with" and "connected" should be understood in a broad sense. For example, "connected" can mean a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium; it can also mean internal communication between two components. Those skilled in the art will be able to understand the specific meanings of the above terms in the present invention based on specific circumstances.
[0063] Example 1;
[0064] 1, 2, 5, 7-9, this embodiment adopts the method of "magnetron sputtering + activation cleaning + electroplating + secondary activation cleaning" to coat the plastic substrate 8. The coating production line used includes an unwinding device 1, a pretreatment device 2 (alkali cleaning device 21, a water washing device 22, a first drying device 23), a magnetron sputtering coating device 31, a first activation cleaning device 4a, an electroplating device 5, a second activation cleaning device 4b, a cleaning and drying device 6, and a winding device 7, which are arranged in sequence:
[0065] The pretreatment device 2, magnetron sputtering coating device 31, first activation cleaning device 4a, electroplating device 5, second activation cleaning device 4b, and cleaning and drying device 6 on the production line are further provided with a plurality of rollers 9, and the plastic substrate 8 is driven by the rollers 9;
[0066] The first drying device 23 is provided with a hot air blower;
[0067] The magnetron sputtering coating device 31 is used to coat the plastic substrate 8 with a first film layer to metallize the rolled flexible plastic substrate 8. The device comprises eight magnetron sputtering targets 311, a vacuum chamber 312, a vacuum pump assembly 313, a gas mass flow controller 314 (MFC), a vacuum sealing assembly 315, a partition 316, a water-cooled roller 317, a water-cooled plate 318, and a tension sensor 33. Several partitions 316 are provided in the vacuum chamber 312 to divide the vacuum chamber 312 into two parts, an upper part and an lower part. The magnetron sputtering targets 311 are provided in the upper part of the vacuum chamber 312 and are provided on the upper and lower sides of the front and back surfaces of the plastic substrate 8, with four magnetron sputtering targets 311 on each side. One surface of the plastic substrate 8 is connected to the magnetron sputtering targets on the same side. A water-cooled plate 318 is located between the magnetron sputtering targets 311, opposite the magnetron sputtering target 311 on the other side. Water-cooled rollers 317 are located in front and behind the eight magnetron sputtering targets 311 to cool the plastic substrate 8. A vacuum pump assembly 313 and a gas mass flow controller (MFC) 314 are located below the vacuum chamber 312 to provide a vacuum environment for the magnetron sputtering coating device 31. The vacuum chamber 312 also has an inlet and outlet for the plastic substrate 8, which are sealed by a vacuum sealing assembly 315. A tension sensor 33 is also installed at the inlet and outlet of the magnetron sputtering coating device 31, contacting the surface of the plastic substrate 8 to detect the surface tension of the plastic substrate 8. The tension test value range of the tension sensor 33 is 5N-500N.
[0068] The first activation cleaning device 4a is used to clean the impurities and oxide film remaining on the surface of the first film layer plated on the plastic substrate 8 and to micro-etch the surface of the first film layer, and includes a cleaning tank 41, a spray device 42, a liquid storage tank 43, a first anode 44, a first cathode 45, a first circulation pipe 46a, a second circulation pipe 46b, a circulation pump 47, and a stop valve 48; the output of the liquid storage tank 43 is connected to the input of the spray device 42 through the first circulation pipe 46a, and the input of the liquid storage tank 43 is connected to the cleaning tank 41 through the second circulation pipe 46b. The first circulation pipe 46a and the second circulation pipe 46b are both provided with a circulation pump 47 and a stop valve 48; the cleaning tank 4 A first anode 44 and a first cathode 45 are also provided at the bottom of the cleaning tank 41 to electrolytically recover the waste liquid and the waste metals therein after etching and cleaning; the spray device 42 is provided above the cleaning tank 41 and is provided with two sets of nozzles. The two sets of nozzles extend into the cleaning tank 41 and are respectively located on the upper and lower sides of the front and back sides of the plastic substrate 8 after surface coating, and spray the first activation cleaning liquid on the front and back sides of the plastic substrate 8 for cleaning and etching; a horizontally arranged concave partition is provided in the middle of the cleaning tank 41, and a pipe is provided below the center of the partition 49. The pipe is provided with a solenoid valve switch, and the cleaning waste liquid flowing into the upper part of the cleaning tank 41 flows into the bottom of the cleaning tank 41 through the pipe;
[0069] The liquid storage tank 43 contains a first activated cleaning liquid. The first activated cleaning liquid flows through the first circulation pipe 46a and is sprayed from the output end of the spray device 42 onto the front and back surfaces of the plastic substrate 8 to clean it. The resulting cleaning waste liquid flows into the cleaning tank 41 as an electrolyte. After electrolysis, new first activated cleaning liquid is formed and flows through the second circulation pipe 46b into the liquid storage tank 43 for recycling. Impurities and residual metals on the surface of the first film layer plated on the plastic substrate 8 flow into the cleaning tank 41 along with the activated cleaning liquid and are electrolytically recovered at the first cathode 45.
[0070] The electroplating device 5 includes an electroplating tank 51, a second cathode 52, a second anode 53, and an electroplating solution. The second anode 53 is made of a metal copper sheet, and the first film layer on the surface of the plastic substrate 8 serves as the second cathode 52. There are two sets of second cathodes 52, and two sets of second anodes 53 are also provided. They are located on the upper and lower sides of the front and back surfaces of the plastic substrate 8 in the electroplating tank 51 to achieve double-sided coating. The electroplating device 5 is used to plate the plastic substrate 8 with a uniform second film layer.
[0071] The second activation cleaning device 4b is the same as the first activation cleaning device 4a, and contains a second activation cleaning liquid, which is used to clean the residual electrolyte and metal residue on the surface of the electronic composite film and perform micro-etching;
[0072] The cleaning and drying device 6 is provided with a water washing tank and a hot air blower.
[0073] Example 2;
[0074] 1, 3, 6-9, the difference from Example 1 is that this embodiment adopts the method of "evaporation coating + activation cleaning + electroplating + secondary activation cleaning" to coat the plastic substrate 8. The coating production line used includes an unwinding device 1, a pretreatment device 2 (alkali cleaning device 21, a water washing device 22, a first drying device 23), a vacuum evaporation coating device 32, an activation cleaning device 4a, an electroplating device 5, a second activation cleaning device 4b, a cleaning and drying device 6, and a winding device 7.
[0075] The vacuum evaporation coating device 32 coats the plastic substrate 8 with a first film layer to metallize the rolled flexible plastic substrate 8, and includes a first evaporation device 32a and a second evaporation device 32b. The two have exactly the same structure and both include a vacuum chamber 323, a vacuum pump group 324, a vacuum sealing component 325, a tension sensor 33, an evaporation system, and a water-cooled roller 326. The evaporation system and the vacuum pump group 324 are arranged in a corner of the lower part of the vacuum chamber 323 in an upper and lower position. The vacuum pump group 324 provides a vacuum environment for the vacuum chamber 323. The evaporation system includes an evaporation boat 321 and a wire-releasing device 322 located at an adjacent position. The evaporation boat 321 contains evaporation material, and the evaporation material is placed on the evaporation boat. Under the action of the evaporation boat 321, the liquid evaporates onto one surface of the plastic substrate 8; the plastic substrate 8 is first coated with a first film layer on one surface by the first evaporation device 32a, and then reversed by the roller 9, and then the first film layer is coated on the other side of the plastic substrate 8; the inlet and outlet of the plastic substrate 8 are provided at another set of diagonal positions of the vacuum chamber 323, and the inlet and outlet are sealed by the vacuum sealing assembly 325; there are two sets of tension sensors 33, which are respectively installed at the inlet and outlet of the first evaporation device 32a or the second evaporation device 32b, and are in contact with the surface of the plastic substrate 8 to detect the surface tension of the plastic substrate 8. The tension test value range of the tension sensor 33 is 5N-500N.
[0076] Example 3;
[0077] 1, 4-9, the difference from Examples 1 and 2 is that: this embodiment adopts the method of "evaporation coating + magnetron sputtering + activation cleaning + electroplating + secondary activation cleaning" to coat the plastic substrate 8, and the coating production line adopted includes an unwinding device 1, a pretreatment device 2 (alkaline washing device 21, a water washing device 22, a first drying device 23), a vacuum evaporation coating device 32, a magnetron sputtering coating device 31, a first activation cleaning device 4a, an electroplating device 5, a second activation cleaning device 4b, a cleaning and drying device 6, and a winding device 7 arranged in sequence.
[0078] Example 4;
[0079] 1-2 , a continuous production process for double-sided coating of a lithium battery current collector according to this embodiment adopts the production line described in Example 1 and includes the following steps:
[0080] S1, the unwinding device 1 unwinds the plastic substrate 8, which is then alkali-washed, washed with water, and dried by the pretreatment device 2, and then enters the magnetron sputtering coating device 31;
[0081] The air-drying time was 5 min and the temperature was 50 °C;
[0082] The linear speed of roller 9 is 10 m / min;
[0083] The alkaline washing device 21 contains a 5 wt % NaOH solution, the alkaline washing temperature is 50° C., and the alkaline washing time is 10 min; the water washing device 22 contains ultrapure water with a resistivity of 18.25 MΩ·cm;
[0084] S2, the magnetron sputtering coating device 31 sputters the front and back surfaces of the plastic substrate 8 under a protective atmosphere, coating the front and back surfaces of the plastic substrate 8 with a first film layer, and then transports the plastic substrate 8 to the first activation and cleaning device 4a;
[0085] The protective atmosphere was argon with an argon flow rate of 20 sccm;
[0086] The sputtering coating process parameters are as follows: a copper target is used as the sputtering target, the coating temperature is 25°C, the vacuum degree of the vacuum chamber is 0.5 Pa, the power supply is 70 W, and the surface tension of the plastic substrate 8 measured during the coating process is 100 N.
[0087] S3, the first activation cleaning device 4a uses two sets of nozzles provided in the spray device 42 therein to simultaneously spray the first activation cleaning liquid on the front and back surfaces of the plastic substrate 8, cleaning and etching the first film layer plated on the front and back surfaces of the plastic substrate 8, and then transporting it to the electroplating device 5; at the same time, the first activation cleaning device 4a uses the first anode 44 and the first cathode 45 provided at the bottom of the cleaning tank 41 thereof to electrolyze and recover the waste liquid and the waste metals therein after the etching and cleaning;
[0088] The first activation cleaning solution is an acidic sodium persulfate solution mixed with 0.2M sulfuric acid and 100g / L Na2S2O8, with a spray rate of 15L / min, a temperature of 50°C, and a distance of 5cm between the nozzle and the first film layer;
[0089] The first anode 44 is made of graphite, the first cathode 45 is made of copper sheet, and the current density of the first cathode 45 is 5A / dm 2 ;
[0090] S4, the electroplating device 5 uses the first film layer plated on the front and back sides of the plastic substrate 8 as the second cathode 52, and adopts a double-sided electroplating method to plate the second film layer on the surface of the second cathode 52 to form an electronic composite film. Then, it is sent to the second activation and cleaning device 4b for secondary activation and cleaning, and then sent to the cleaning and drying device 6;
[0091] The electroplating process parameters are as follows: the second anode 53 is made of copper sheet, the electroplating solution is a mixed solution of 100g / L CuSO4, 50mg / L CuCl2, and 3M H2SO4 with a pH value of 4, the electroplating temperature is 50°C, and the current density of the second cathode 52 is 1A / dm 2 ;
[0092] The second activation cleaning solution is an acidic sodium persulfate solution mixed with 0.1M sulfuric acid and 50g / L Na2S2O8, with a spraying rate of 15L / min, a temperature of 50°C, and a distance of 5cm between the nozzle and the second film layer;
[0093] S5, the cleaning and drying device 6 cleans and dries the electronic composite film, and then sends it to the winding device 7 for winding;
[0094] The washing tank of the cleaning and drying device 6 is provided with ultrapure water with a resistivity of 18.25 MΩ·cm to clean the composite membrane; the air drying time of the hot air blower is 5 minutes and the temperature is 50°C.
[0095] In this embodiment, the process described in Example 1 is used to coat a PET plastic substrate 8. The plastic substrate 8 is polyethylene terephthalate (PET). The thickness of the PET plastic substrate 8 is 5 μm and the width is 600 mm. The magnetron sputtering coating time is 150 s, and the sputtering coating thickness is 120 nm×2. The electroplating time is 5 min, and the electroplating coating thickness is 1 μm×2. Finally, an electronic composite film with a thickness of 7 μm is formed. The electrical conductivity of the electronic composite film is 80% of that of copper, and the specific electrical conductivity is 45.712×10 6 S / m; compared with traditional copper foil, it is lighter, weighing about 30% of traditional copper foil, has high energy density, higher safety, and a good degree of bonding between the metal conductive layer and the plastic substrate 8. The production cycle is 2h; after using the first activation cleaning device 4a and the second activation cleaning device 4b, the recovery rate of waste metal in the cleaning solution reaches 100%.
[0096] Example 4-1;
[0097] The other conditions of this embodiment are the same as those of embodiment 4. The difference from embodiment 4 is that the only difference is that the magnetron sputtering power is 250W and the sputtering film thickness is 200nm×2 in the preparation process. Finally, an electronic composite film with a thickness of 7um is formed. The conductivity of the electronic composite film is about 85% of that of copper, and the specific conductivity is 48.569×10 6 S / m; compared with traditional copper foil, it is lighter, weighing about 30% of traditional copper foil, has high energy density, higher safety, and a good degree of bonding between the metal conductive layer and the plastic substrate 8. The production cycle is 2h; after using the first activation cleaning device 4a and the second activation cleaning device 4b, the recovery rate of waste metal in the cleaning solution reaches 100%.
[0098] Example 4-2;
[0099] The other conditions of this embodiment are the same as those of embodiment 4. The difference from embodiment 4 is that the current density of the second cathode 52 is 2A / dm 2The thickness of the electroplating film is 2um×2, and finally the thickness of the electronic composite film is 9um. The conductivity of the electronic composite film is about 78% of copper, and the specific conductivity is 44.5692×10 6 S / m; compared with traditional copper foil, it is lighter, weighing about 44% of traditional copper foil, has high energy density, higher safety, and a good degree of bonding between the metal conductive layer and the plastic substrate 8. The production cycle is 2h; after using the first activation cleaning device 4a and the second activation cleaning device 4b, the recovery rate of waste metal in the cleaning solution reaches 100%.
[0100] Example 5;
[0101] 1 and 3 , a continuous production process for double-sided coating of a lithium battery current collector described in this embodiment adopts the production line described in Example 2, including the following steps:
[0102] S1, the unwinding device 1 unwinds the plastic substrate 8, which is then alkali-washed, washed with water, and dried by the pretreatment device 2, and then enters the vacuum evaporation coating device 32;
[0103] The air drying time was 5 min and the temperature was 50 °C.
[0104] The linear speed of roller 9 is 10 m / min;
[0105] The alkaline washing device 21 contains a 5 wt % NaOH solution, the alkaline washing temperature is 50° C., and the alkaline washing time is 10 min; the water washing device 22 contains ultrapure water with a resistivity of 18.25 MΩ·cm;
[0106] S2, the vacuum evaporation coating device 32 performs evaporation coating on the front and back surfaces of the plastic substrate 8 under a protective atmosphere, coating the front and back surfaces of the plastic substrate 8 with a first film layer, and then transporting the plastic substrate 8 to the first activation and cleaning device 4a;
[0107] The protective atmosphere was argon with an argon flow rate of 20 sccm;
[0108] The evaporation process parameters are: the evaporation material is copper-zinc alloy wire, the evaporation power is 800W, the temperature is 80℃, the vacuum degree is 10 -3 Pa, evaporation rate is 3A / s;
[0109] The surface tension of the plastic substrate 8 was measured to be 80N during the coating process;
[0110] S3, the first activation cleaning device 4a uses two sets of nozzles provided in the spray device 42 therein to simultaneously spray the first activation cleaning liquid on the front and back surfaces of the plastic substrate 8, cleaning and etching the first film layer plated on the front and back surfaces of the plastic substrate 8, and then transporting it to the electroplating device 5; at the same time, the first activation cleaning device 4a uses the first anode 44 and the first cathode 45 provided at the bottom of the cleaning tank 41 thereof to electrolyze and recover the waste liquid and the waste metals therein after the etching and cleaning;
[0111] The first activation cleaning solution is an acidic sodium persulfate solution composed of a mixture of 0.5M sulfuric acid and 200g / L Na2S2O8, with a spray rate of 15L / min, a temperature of 50°C, and a distance of 5cm between the nozzle and the second membrane layer;
[0112] S4, the electroplating device 5 uses the first film layer plated on the front and back sides of the plastic substrate 8 as the second cathode 52, and adopts a double-sided electroplating method to plate the second film layer on the surface of the second cathode 52 to form an electronic composite film, which is then sent to the second activation and cleaning device 4b to perform secondary activation and cleaning on the electronic composite film, and then sent to the cleaning and drying device 6;
[0113] The electroplating process parameters are as follows: the second anode 53 is made of copper-zinc alloy sheet, the electroplating solution is a mixed solution of 100g / L CuSO4, 50mg / L CuCl2, 50g / L ZnSO4, and 3M H2SO4 with a pH value of 4, the electroplating temperature is 50°C, and the current density of the second cathode 52 is 1A / dm 2 ;
[0114] The second activation cleaning solution is an acidic sodium persulfate solution made by mixing 0.1M sulfuric acid and 50g / L Na2S2O8, the temperature is 50℃, and the distance between the nozzle and the second membrane layer is 5cm;
[0115] S5 , the cleaning and drying device 6 cleans and dries the electronic composite film, and then sends it to the winding device 7 for winding.
[0116] The washing tank of the cleaning and drying device 6 is equipped with ultrapure water with a resistivity of 18.25 MΩ·cm to clean the composite membrane; the air drying time of the hot air blower is 5 minutes and the temperature is 50°C.
[0117] In this embodiment, the process described in Example 2 is used to coat the plastic substrate 8. The plastic substrate 8 is made of polybutylene naphthalate (PBN). The thickness of the PBN plastic substrate 8 is 5 μm and the width is 600 mm. The vacuum evaporation coating time is 80 seconds, and the evaporation coating thickness is 130 nm×2. The electroplating time is 15 minutes, and the electroplating coating thickness is 2 μm×2. Finally, an electronic composite film with a thickness of 9 μm is formed. The electrical conductivity of the electronic composite film is about 75% of that of copper, and the specific electrical conductivity is 42.855×10 6S / m; compared with traditional copper foil, it is lighter, weighing about 45% of traditional copper foil, has high energy density, higher safety, and a good degree of bonding between the metal conductive layer and the plastic substrate 8. The production cycle is 2.5h; after using the first activation cleaning device 4a and the second activation cleaning device 4b, the recovery rate of waste metal in the cleaning solution reaches 100%.
[0118] Example 5-1;
[0119] The difference between this embodiment and embodiment 5 is that the other conditions are the same as those in embodiment 5, except that the evaporation power is 1000W and the vacuum degree is 10 -4 Pa, the evaporation rate is 4.5A / s, and the evaporation coating thickness is 220nm×2; finally, an electronic composite film with a thickness of 9um is formed. The conductivity of the electronic composite film is about 70% of copper, and the specific conductivity is 40×10 6 S / m; compared with traditional copper foil, it is lighter, weighing about 45% of traditional copper foil, has high energy density, higher safety, and a good degree of bonding between the metal conductive layer and the plastic substrate 8. The production cycle is 2.5h; after using the first activation cleaning device 4a and the second activation cleaning device 4b, the recovery rate of waste metal in the cleaning solution reaches 100%.
[0120] Example 6;
[0121] 1 and 4 , a continuous production process for double-sided coating of a lithium battery current collector according to this embodiment adopts the production line described in Example 3, and includes the following steps:
[0122] S1, the unwinding device 1 unwinds the plastic substrate 8, which is then alkali-washed, washed with water, and dried by the pretreatment device 2, and then enters the first coating device 3;
[0123] The air drying time was 5 min and the temperature was 50 °C.
[0124] The linear speed of roller 9 is 6 m / min;
[0125] The alkaline washing device 21 contains a 5 wt % NaOH solution, the alkaline washing temperature is 50° C., and the alkaline washing time is 10 min; the water washing device 22 contains ultrapure water with a resistivity of 18.25 MΩ·cm;
[0126] S2, the first coating device 3 performs evaporation and then sputtering on the front and back surfaces of the plastic substrate under a protective atmosphere, coating the front and back surfaces of the plastic substrate 8 with a first film layer, and then transporting the plastic substrate 8 to the first activation and cleaning device 4a;
[0127] The protective atmosphere was argon with an argon flow rate of 20 sccm;
[0128] The evaporation process parameters are: the evaporation material is copper-nickel alloy, the evaporation power is 880W, the coating temperature is 100℃, and the vacuum degree is 10 -4 Pa, the evaporation material is deposited at a rate of 4 A / s;
[0129] The sputtering coating process parameters are as follows: the sputtering target material is copper-nickel alloy, the sputtering temperature is 100°C, the vacuum degree of the vacuum chamber is 0.5 Pa, and the power supply is 250W;
[0130] The surface tension of the plastic substrate 8 was measured to be 80N during the coating process;
[0131] S3, the first activation cleaning device 4a uses two sets of nozzles provided in the spray device 42 therein to simultaneously spray the first activation cleaning liquid on the front and back surfaces of the plastic substrate 8, cleaning and etching the first film layer plated on the front and back surfaces of the plastic substrate 8, and then transporting it to the electroplating device 5; at the same time, the first activation cleaning device 4a uses the first anode 44 and the first cathode 45 provided at the bottom of the cleaning tank 41 thereof to electrolyze and recover the waste liquid and the waste metals therein after the etching and cleaning;
[0132] The first activation cleaning solution is an acidic sodium persulfate solution composed of 0.5M sulfuric acid and 250g / L Na2S2O8, with a spraying rate of 15L / min, a temperature of 50°C, and a distance of 5cm between the nozzle and the first film layer;
[0133] S4, the electroplating device 5 uses the first film layer plated on the front and back sides of the plastic substrate 8 as the second cathode 52, and adopts a double-sided electroplating method to plate the second film layer on the surface of the second cathode 52 to form an electronic composite film, which is then sent to the second activation and cleaning device 4b to perform secondary activation and cleaning on the electronic composite film, and then sent to the cleaning and drying device 6;
[0134] The electroplating process parameters are as follows: the second anode 53 is made of a copper-nickel alloy plate, the electroplating solution is a solution composed of 150g / L CuSO4, 40g / L NiSO4·6H2O, 100mg / L NiCl2, 3M H2SO4 with a pH value of 4.5, the electroplating temperature is 50°C, and the current density of the second cathode 52 is 1.5A / dm 2 ;
[0135] The second activation cleaning solution is an acidic sodium persulfate solution composed of 0.1M sulfuric acid and 50g / L Na2S2O8, the temperature is 50°C, and the distance between the nozzle and the second membrane layer is 5cm;
[0136] S5 , the cleaning and drying device 6 cleans and dries the electronic composite film, and then sends it to the winding device 7 for winding.
[0137] The washing tank of the cleaning and drying device 6 is filled with ultrapure water with a resistivity of 18.25 MΩ·cm; the air drying time of the hot air blower is 5 minutes and the temperature is 50°C.
[0138] In this embodiment, the process described in Example 3 is used to coat the plastic substrate 8. The plastic substrate 8 is polypropylene (PT). The thickness of the PT plastic substrate 8 is 5 μm and the width is 600 mm. The evaporation coating time is 50 seconds, and the evaporation coating thickness is 100 nm×2. The magnetron sputtering coating time is 30 seconds, and the magnetron sputtering coating thickness is 55 nm×2. The electroplating time is 8 minutes, and the electroplating coating thickness is 1.5 μm. Finally, an electronic composite film with a thickness of 8 μm is formed. The electrical conductivity of the electronic composite film is about 70% of that of copper, specifically 39.998×10 6 S / m; compared with traditional copper foil, it is lighter, weighing about 38% of traditional copper foil, has high energy density, higher safety, and a good degree of bonding between the metal conductive layer and the plastic substrate 8. The production cycle is 3.5h; after using the first activation cleaning device 4a and the second activation cleaning device 4b, the recovery rate of waste metal in the cleaning solution reaches 100%.
[0139] Example 6-1;
[0140] The difference between this embodiment and embodiment 6 is that other conditions are the same as those in embodiment 6, except that the evaporation power is 200W, the magnetron sputtering power is 300W, and the current density of the second cathode 52 is 5A / dm 2 The thickness of the electroplated film is 5um×2; finally, an electronic composite film with a thickness of 15um is formed. The conductivity of the electronic composite film is about 65% of copper, specifically 37.141×10 6 S / m; compared with traditional copper foil, it is lighter, weighing about 67% of traditional copper foil, has high energy density, higher safety, and a good degree of bonding between the metal conductive layer and the plastic substrate 8. The production cycle is 3.5h; after using the first activation cleaning device 4a and the second activation cleaning device 4b, the recovery rate of waste metal in the cleaning solution reaches 100%.
[0141] Comparative Example 1;
[0142] In this comparative example, the magnetron sputtering method is used alone to coat the plastic substrate 8. The plastic substrate 8 is made of polyethylene terephthalate (PET), the substrate thickness is 5um, the coating thickness is 1um, the coating cycle is 6h, and the coating efficiency is low. The electronic composite film is easily broken down, wrinkled and deformed under the sputtering high-energy coating environment for a long time. The quality of the prepared electronic composite film is worse than that of Example 1.
[0143] Comparative Example 2;
[0144] In this comparative example, the plastic substrate 8 is coated by the vapor deposition method alone. The plastic substrate 8 is made of polybutylene naphthalate (PBN). The substrate thickness is 5 μm, the coating thickness is 2 μm, and the coating cycle is 5 hours. The coating efficiency is low. The electronic composite film is prone to wrinkling and deformation under the high-temperature vapor deposition environment for a long time. The quality of the prepared electronic composite film is worse than that of Example 2.
[0145] Comparative Example 3;
[0146] In this comparative example, the existing electroplating method is used to perform a second coating on the plastic substrate 8 carrying a metal nanofilm on the surface. The plastic substrate 8 is made of polypropylene (PT), the substrate thickness is 5 μm, the original coating thickness is 100 nm, the electroplating cycle is 3 hours, and hydrochloric acid is used to activate and clean the electronic composite film. The prepared electronic composite film has poor bonding quality and is easy to fall off. The conductivity of the electronic composite film is worse than that of Example 3. The cleaning waste liquid cannot be reused, and will produce wastewater that is harmful to human health and pollutes the environment, which is not conducive to production and environmental protection.
[0147] The working principle of the first activation cleaning device 4a is:
[0148] Referring to FIG10 (a), taking Example 1 as an example, since there is a passivation film and impurities on the surface of the plastic substrate 8 after being coated by the first coating device 3, which will affect the quality of subsequent coating, the surface of the plastic substrate 8 needs to be cleaned and micro-etched by the acidic persulfate solution in the first activation cleaning device 4a to remove the impurities and oxide film on the surface of the first film layer coated on the plastic substrate 8, effectively improving the bonding strength between the first film layer and the second film layer. The chemical reaction equation for cleaning the metal oxide film remaining on the surface of the plastic substrate 8 is Na2S2O8+Cu Na2SO4+CuSO4+O2↑, then the waste metals in the cleaning solution are recovered by electrolysis. The chemical reaction equation for waste metal recovery is CuSO4+Na2SO4 Cu+Na2S2O8; since a trace amount of acidic persulfate solution is attached to the surface of the plastic substrate 8 after the first activation and cleaning, the persulfate ions in the solution have strong oxidizing properties and can effectively prevent the formation of an oxide film or reduce the existing trace oxide film, thereby effectively ensuring the activation state of the first film surface; in addition, since the surface of the plastic substrate 8 film carries persulfate ions and hydrogen ions, after entering the electroplating device 5, the presence of these two cations can reduce the current density of the second cathode 52 during electroplating, thereby improving the current efficiency, the electroplating efficiency, the film quality, and the bonding strength between the film and the plastic substrate 8; the first activation and cleaning device 4a can not only clean and etch the plastic substrate 8 or the electronic composite film with the first activation cleaning solution, but also electrolytically recover the first activation cleaning solution for recycling, and the residual metal will adhere to the surface of the first cathode 45 for recovery, thereby achieving high-quality and efficient plating, environmental protection and sustainable resource utilization.
[0149] The working principle of the second activation cleaning device 4b is:
[0150] Referring to FIG10 (b), taking Example 1 as an example, since there are residual electroplating solution and metal residues on the surface of the plastic substrate 8 after being plated by the electroplating device 5, the presence of the two will affect the quality of the electronic composite film, so the electronic composite film needs to be cleaned; the second activation cleaning device 4b is the same as the first activation cleaning device 4a, and both use an acidic persulfate solution to clean the surface of the plastic substrate 8, thereby ensuring the product quality of the electronic composite film. The chemical reaction equation for cleaning the metal residue on the surface of the electronic composite film is Na2S2O8+Cu Na2SO4+CuSO4, the chemical reaction equation for electrolytic recovery of metal residues is CuSO4+Na2SO4 Cu+Na2S2O8, the concentration of the second activation cleaning liquid and the first activation cleaning liquid can be different, and the effect of the secondary activation cleaning is adjusted by the second activation cleaning device 4b to meet the needs of different electronic composite film products.
[0151] In engineering applications, since the bonding force of magnetron sputtering coating is stronger than that of evaporation coating, the uniformity and density are higher than those of evaporation coating, but high-power excitation of high-melting-point metal targets is easy to penetrate the plastic substrate 8, and the evaporation coating speed is faster than that of magnetron sputtering coating. Therefore, it is necessary to reasonably select the coating method according to the following scheme according to the needs of the process, for example: "magnetron sputtering + activation cleaning + electroplating + secondary activation cleaning" in Examples 1 and 4, "evaporation coating + activation cleaning + electroplating + secondary activation cleaning" in Examples 2 and 5, and "evaporation coating + magnetron sputtering + activation cleaning" in Examples 3 and 6. "Cleaning + electroplating + secondary activation cleaning"; Examples 1-6 all adopt the first activation cleaning device 4a, which can greatly improve the electroplating efficiency, film quality and the bonding strength between the film and the plastic substrate 8; the coating methods described in Examples 3 and 6 are particularly suitable for high-melting-point targets. Since high-melting-point targets have high energy during magnetron sputtering coating and are easy to penetrate the plastic substrate 8, the nanofilm is coated by first evaporation and then magnetron sputtering, which can reduce the risk of the plastic substrate 8 being penetrated. Compared with the methods of Examples 2, 4 and 5, the coating strength, quality and efficiency can be further improved.
[0152] Matters not covered by the present invention are prior art.
[0153] The above embodiments are only for illustrating the technical concept and features of the present invention. Their purpose is to enable people familiar with this technology to understand the contents of the present invention and implement them accordingly. They are not intended to limit the scope of protection of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the scope of protection of the present invention.
Claims
1. A continuous production line for double-sided coating of a lithium battery current collector, comprising an unwinding device, a pretreatment device, a first coating device, a first activation and cleaning device, a second coating device, a cleaning and drying device, and a winding device; the plastic substrate output by the unwinding device is processed by the pretreatment device, the first coating device, the first activation and cleaning device, the second coating device, and the cleaning and drying device in sequence before entering the winding device; characterized in that: The first activation cleaning device contains a first activation cleaning liquid, which is a persulfate solution with a pH value of 2-6.
2. A continuous production line for double-sided coating of lithium battery current collectors according to claim 1, characterized in that: The plastic substrate is driven by rollers arranged in the pretreatment device, the first coating device, the first activation cleaning device, the second coating device, and the cleaning and drying device, and the linear speed of the rollers is 1m / min-15m / min.
3. A continuous production line for double-sided coating of lithium battery current collector according to claim 1, characterized in that: The first activated cleaning device comprises a cleaning tank, a spray device, a liquid storage tank, a first anode, a first cathode, a first circulation pipe, a second circulation pipe, a circulation pump, and a stop valve; The output of the liquid storage tank is connected to the input of the spray device through a first circulation pipe, and the input of the liquid storage tank is connected to the output of the cleaning tank through a second circulation pipe. The first circulation pipe and the second circulation pipe are both provided with a circulation pump and a stop valve; The bottom of the cleaning tank is also provided with a first anode and a first cathode to electrolyze and recover the waste liquid after etching and cleaning and the waste metals therein; The first anode is an inert material selected from one of boron-doped diamond, graphite, Ti4O7, IrO2, RuO2, PbO or Pt, the first cathode material is selected from one of Ag, Cu, Au, Al, W, Ni, Fe, Pt, and the current density is 5-15ASD; The spray device is provided with two groups of nozzles, which extend into the cleaning tank and are respectively located at the upper and lower sides of the front and back sides of the plastic substrate after surface coating, and spray the first activated cleaning liquid on the front and back sides of the plastic substrate to clean and etch the front and back sides of the plastic substrate.
4. A continuous production line for double-sided coating of lithium battery current collectors according to claim 3, characterized in that: The first activated cleaning solution is a mixed solution in which the pH value of a persulfate solution is adjusted to 2-6 by sulfuric acid; the persulfate is selected from one of sodium persulfate, potassium persulfate, and ammonium persulfate; the mass volume concentration of the persulfate solution is 50g / L-300g / L; and the molar concentration of sulfuric acid is 0.1M-1M.
5. A continuous production line for double-sided coating of lithium battery current collectors according to claim 1, characterized in that: The first coating device is provided with a vacuum evaporation coating device and / or a magnetron sputtering coating device to coat the first film layer on both sides of the plastic substrate; the vacuum evaporation coating device includes a first evaporation device and a second evaporation device. After the plastic substrate is coated on one surface by the first evaporation device, it is reversed by a roller and then enters the second evaporation device to coat the other side of the plastic substrate; the magnetron sputtering coating device includes two components of magnetron sputtering targets placed on the upper and lower sides of the front and back surfaces of the plastic substrate.
6. A continuous production line for double-sided coating of lithium battery current collectors according to claim 5, characterized in that: The inlet and outlet of the magnetron sputtering coating device and the vacuum evaporation coating device are both equipped with tension sensors in contact with the surface of the plastic substrate to detect the surface tension of the plastic substrate.
7. A continuous production line for double-sided coating of lithium battery current collectors according to any one of claims 1 to 6, characterized in that: The second coating device is an electroplating device, which is used to coat the second film layer on both sides of the plastic substrate. The electroplating device includes an electroplating tank, a second cathode, a second anode and an electroplating solution. The second anode is divided into two groups and arranged in the electroplating tank. The plastic substrate is located between the two groups of second anodes. The first film layer coated on both sides of the plastic substrate serves as the second cathode. The electroplating solution is a mixed solution composed of a salt of the film layer metal and an acid with a pH value of 3-6. The salt of the film layer metal is selected from the sulfate, nitrate or chloride of at least one metal selected from Cu, Al, Ag, Ni and Zn. The acid is hydrochloric acid or sulfuric acid.
8. A continuous production line for double-sided coating of lithium battery current collectors according to claim 7, characterized in that: The target material in the magnetron sputtering coating device, the evaporation material in the vacuum evaporation coating device, and the second anode material in the electroplating device are all the same as the film metal or alloy plated on the front and back sides of the plastic substrate. The metal is selected from one of Cu, Al, Ag, Ni, and Zn, and the alloy is selected from one of Cu-Zn, Al-Zn, Ag-Cu, Ag-Ni, Ag-Fe, Ni-Cu, Cu-Zn-Ni, and Cu-Ni-Sn.
9. A continuous production line for double-sided coating of lithium battery current collectors according to claim 8, characterized in that: A second activation cleaning device is also provided between the second coating device and the cleaning and drying device to activate and clean the electronic composite film; the structure of the second activation cleaning device is the same as that of the first activation cleaning device, wherein a second activation cleaning liquid is contained therein to clean and etch the second film layer, and the cleaning waste liquid and the waste metal therein are electrolytically recovered, and the second activation cleaning liquid is a mixed solution obtained by adjusting the pH value of the persulfate solution to 2-6 by sulfuric acid; the persulfate is selected from one of sodium persulfate, potassium persulfate, and ammonium persulfate; the mass volume concentration of the persulfate solution is 50g / L-300g / L; the molar concentration of sulfuric acid is 0.1M-1M; the injection speed is 10L / min-30L / min, and the temperature is 40℃-60℃.
10. A continuous production process for double-sided coating of a lithium battery current collector, using a continuous production line for double-sided coating of a lithium battery current collector as claimed in claim 8, comprising the following steps: S1, the unwinding device unwinds the plastic substrate, and after alkali washing, water washing and drying by the pretreatment device, enters the first coating device; S2, the first coating device performs evaporation or sputtering or evaporation followed by sputtering on the front and back surfaces of the plastic substrate under a protective atmosphere, coating the front and back surfaces of the plastic substrate with a first film layer, and then conveying the plastic substrate to a first activation and cleaning device; The protective atmosphere is argon gas, and the argon gas flow rate is 10-50sccm; The evaporation process parameters are: power 50W-2200W, vacuum degree 10 -6 Pa~10 -3 Pa, evaporation rate is 0.1A / s-10A / s; The process parameters of sputtering coating are: sputtering power 50W-300W, sputtering temperature 25℃-120℃, vacuum degree 0.1Pa-10Pa; S3, the first activation cleaning device sprays the first activation cleaning liquid on the front and back sides of the plastic substrate through two groups of nozzles arranged in the spray device, cleans and etches the first film layer plated on the front and back sides of the plastic substrate, and then transports it to the second coating device; at the same time, the first activation cleaning device electrolytically recovers the waste liquid after etching and cleaning and the waste metals therein through the first anode and the first cathode arranged at the bottom of the cleaning tank; The first activation cleaning solution is a mixed solution in which the pH value of a persulfate solution is adjusted to 2-6 by sulfuric acid; the persulfate is selected from one of sodium persulfate, potassium persulfate, and ammonium persulfate; the mass volume concentration of the persulfate solution is 50g / L-300g / L; the molar concentration of sulfuric acid is 0.1M-1M; the injection speed is 10L / min-30L / min, the temperature is 40°C-60°C, and the distance between the nozzle and the first film layer is 5cm-10cm; S4, the second coating device uses the first film layer coated on the front and back sides of the plastic substrate as the second cathode, and adopts a double-sided electroplating method to coat the second film layer on the surface of the second cathode to form an electronic composite film, which is then sent to a cleaning and drying device; The electroplating process parameters are: the plating solution temperature is 40°C-60°C, the current density of the second cathode is 1A / dm 2 -6A / dm 2 The electroplating solution is a mixed solution of sulfate, nitrate or chloride of at least one metal among Cu, Al, Ag, Ni and Zn, hydrochloric acid or sulfuric acid with a pH value of 3-6, and the mass concentration of the metal salt solution is 50mg / L-200g / L; S5. After the electronic composite film is cleaned and dried by the cleaning and drying device, it is sent to the winding device for winding.
11. A continuous production process for double-sided coating of lithium battery current collector according to claim 10, characterized in that: In S4, after the electronic composite film is formed on the surface of the plastic substrate, it is sent to the second activation and cleaning device to activate and clean the electronic composite film; then, it is sent to the cleaning and drying device for cleaning and drying, and then sent to the winding device for winding; The second activation cleaning solution is a mixed solution in which the pH value of a persulfate solution is adjusted to 2-6 by sulfuric acid; the persulfate is selected from one of sodium persulfate, potassium persulfate, and ammonium persulfate; the mass volume concentration of the persulfate solution is 50g / L-300g / L; the molar concentration of sulfuric acid is 0.1M-1M; the injection speed is 10L / min-30L / min, the temperature is 40°C-60°C, and the distance between the nozzle and the first film layer is 5cm-10cm.
Citation Information
Patent Citations
Preparation method and device of ultrathin flexible conductive composite film
CN114959626A
Negative current collector for lithium ion battery and preparation method of negative current collector
CN115911402A
Lithium battery current collector double-sided coating continuous production line and process
CN116145085A
Coiled material double-sided continuous electroplating system
CN211814695U
Pretreatment for electroless copper plating
JP1995278823A