A low VOC coating composition and its application

WO2024222727A1PCT designated stage expired Publication Date: 2024-10-31BASF COATINGS GMBH +1

Patent Information

Application Number
PCT/CN2024/089504
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-25
Filing Date
2024-04-24
Publication Date
2024-10-31

Smart Images

  • Figure PCTCN2024089504-FTAPPB-I100001
    Figure PCTCN2024089504-FTAPPB-I100001
  • Figure PCTCN2024089504-FTAPPB-I100002
    Figure PCTCN2024089504-FTAPPB-I100002
  • Figure PCTCN2024089504-FTAPPB-I100003
    Figure PCTCN2024089504-FTAPPB-I100003
Patent Text Reader

Abstract

The present invention provides a low VOC coating composition comprising Component (a) : at least one epoxy resin having an epoxy value in a range of from 0.1 to 1.0, preferably from 0.2 to 0.7 and more preferably from 0.3 to 0.6, Component (b) : at least one silicone-modified epoxy resin, Component (c) : at least one hydrocarbon resin, and a reactive diluent, wherein said Component (a) is at least one selected from a group consisting of glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, alicyclic epoxy compound and aliphatic epoxy compound, preferably glycidyl ether epoxy resin and more preferably bisphenol A glycidyl ether epoxy resin.
Need to check novelty before this filing date? Find Prior Art

Description

A LOW VOC COATING COMPOSITION AND ITS APPLICATIONTECHNICAL FIELD

[0001] The present invention relates to a low VOC coating composition and more specifically an epoxy resin based coating composition having low VOCs as well as its application in engineering ma-chineries.

[0002] BACKGROUN

[0003] At present, industrial coatings are still mainly solvent-based, and volatile organic compounds (VOCs) have caused pollutions to the environment and harm the health of people. Therefore, more strict regulations of VOC emissions are issued by the authority and coatings having low VOCs are developed including waterborne coatings, powder coatings and high content solid coatings, wherein high content solids coatings are most widely used.

[0004] In the field of engineering machinery, the coating composition is expected to dry fast to meet the requirement of high turnover rate of engineering machineries in production lines. And mean-while the coating films after curing need to have sufficient corrosion resistance such as salt re-sistance since the engineering machinery usually works under harsh conditions.

[0005] To achieve that, some measures were tried in the prior art. For example, CN109181486A dis-closed an epoxy primer with low VOCs comprising component A and component B in a ratio of 6: 1 by weight and said component A comprises bisphenol A epoxy resin, liquid hydrocarbon resin, dispersant, iron oxide black, zinc molybdate, aluminum tripolyphosphate, barium sulfate, mica powder, talc, organic bentonite, active diluent, xylene, and n-butanol; and said component B comprises modified polyamide curing agent, xylene, n-butanol, epoxy silane coupling agent, and epoxy curing accelerator. The obtained epoxy primer had high solid content and low VOCs and dried fast. However, the corrosion resistance especially salt resistance is not satisfying. Therefore, it is still required to provide a coating composition that could dry fast, and at the same time the coating films after curing could show good corrosion resistance especially salt resistance.SUMMARY OF THE INVENTION

[0006] In one aspect, the present invention provides a low VOC coating composition comprising Component (a) : at least one epoxy resin having an epoxy value in a range of from 0.1 to 1.0, preferably from 0.2 to 0.7 and more preferably from 0.3 to 0.6,

[0007] Component (b) : at least one silicone-modified epoxy resin,

[0008] Component (c) : at least one hydrocarbon resin, and a reactive diluent, wherein said Component (a) is at least one selected from a group consisting of glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, alicyclic epoxy compound and aliphatic epoxy com-pound, preferably glycidyl ether epoxy resin and more preferably bisphenol A glycidyl ether epoxy resin.

[0009] In another aspect, the present invention also provides a primer obtained from the invented coat-ing composition by curing.

[0010] Surprisingly, by combining epoxy resins and a silicone-modified epoxy resins, the obtained coating composition shows storage stability, good workability such as fast drying, anti-sagging and fillability and the coating films obtained from curing of the coating composition also have excellent mechanical properties and corrosion resistance especially salt resistance.

[0011] DETAILED DESCRIPTION OF THIS INVENTION

[0012] The present invention will be described in detail hereinafter. It is to be understood that the pre-sent invention can be embodied in many different ways and shall not be construed as limited to the embodiments set forth herein.

[0013] Unless defined otherwise, all technical and scientific terms used herein have the meaning commonly understood by a person skilled in the art to which the invention belongs. As used herein, the following terms have the meanings ascribed to them below, unless specified other-wise.

[0014] As used herein, the terms “a” and “an” refer to one or to more than one (i.e., to at least one) of the grammatical object of the article or component.

[0015] As used herein, the terms “comprise” , “comprising” , etc. are used interchangeably with “contain” , “containing” , etc. and are to be interpreted in a non-limiting, open manner. That is, e.g., further components or elements can be present. The expressions “consists of” or “consists essentially of” or cognates can be embraced within “comprises” or cognates.

[0016] The Component (a) of the present invention, i.e. epoxy resin may be at least one selected from a group consisting of glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, alicyclic epoxy resin and aliphatic epoxy resin.

[0017] The glycidyl ether epoxy resin is obtained by condensation of polyphenol or polyol and epichlo-rohydrin. Examples of polyphenol include bisphenol A, bisphenol F, 4, 4'-dihydroxybenzophenone, 1, 1-bis- (4-hydroxyphenyl) -ethane, 1, 1-bis- (4-hydroxyphenyl) -isobu-tane, 2, 2-bis- (4-hydroxy-tert-butylphenyl) -propane, bis- (2-hydroxy-naphthyl) -methane, 1, 5-dihydroxynaphthalene and phenolic resin, etc., wherein bisphenol A and bisphenol F are partic-ularly preferred polyphenols. Examples of the polyol include ethylene glycol, diethylene glycol, triethylene glycol, 1, 2-propanediol, 1, 4-butanediol, 1, 5-pentanediol, 1, 2, 6-hexanetriol, pro-panetriol and 2, 2-bis (4-hydroxycyclohexyl) propane, pentaerythritol, dipentaerythritol, trime-thylolpropane, etc. Examples of the glycidyl ether epoxy resin include bisphenol A glycidyl ether (e.g., bisphenol A diglycidyl ether) , bisphenol F glycidyl ether (e.g. bisphenol F diglycidyl ether) , novolac polyglycidyl ether, 1, 4-butanediol diglycidyl ether, 1, 6-hexanediol diglycidyl ether, trime-thylolpropane triglycidyl ether, pentaerythritol diglycidyl ether, pentaerythritol triglycidyl ether, pentaerythritol tetraglycidyl ether, dipentaerythritol diglycidyl ether, dipentaerythritol triglycidyl ether, dipentaerythritol tetraglycidyl ether, trimethylolpropane diglycidyl ether, trimethylolpro-pane triglycidyl ether, neopentyl glycol diglycidyl ether, C12-14 alkyl glycidyl ether, butyl glycidyl ether, and 2-ethylhexyl glycidyl ether, and alicyclic glycidyl ether e.g. hydrogenated bisphenol A diglycidyl ether, dimethylol cyclohexane diglycidyl ether, and tricyclodecanedimethanol diglyc-idyl ether, etc.

[0018] Said glycidyl ester epoxy resins could be e polyglycidyl ester of polycarboxylic acid, e.g. oxalic acid, succinic acid, glutaric acid, neodecanedicarboxylic acid, cyclohexanedicarboxylic acid, terephthalic acid, 2, 6-naphthalenedicarboxylic acid, and dimeric linoleic acid, etc. Examples include adipic acid diglycidyl ester, phthalic acid diglycidyl ester, isophthalic acid diglycidyl ester and terephthalic acid diglycidyl ester etc. Preferably, the glycidyl ester epoxy resin is at least one selected from glycidyl ester of neodecanedicarboxylic acid, glycidyl ester of dimeric linoleic acid, and diglycidyl 1, 2-cyclohexanedicarboxylate.

[0019] The glycidyl amine epoxy resin is obtained by the condensation reaction of polyamine with epichlorohydrin, and examples include diamino diphenylmethane tetraglycidylamine, triglycidyl p-aminophenol and triglycidyl melamine etc.

[0020] Examples of the alicyclic epoxide include dicyclopentadiene dioxide, 3, 4-epoxy-6-methylcyclohexanecarboxylic acid-3', 4'-epoxy-6'-methylcyclohexane methyl ester.

[0021] One preferred example of the linear aliphatic epoxide is polybutadiene epoxide.

[0022] In one embodiment, epoxy resin is bisphenol A glycidyl ether, such as bisphenol A diglycidyl ether and suitable bisphenol A glycidyl ether is commercially available, for example, BE501B75 from Changchun Chemical, BE188EL from Changchun Chemical and NPEL-128S from Nanya Chemical.

[0023] The epoxy value of said epoxy resin is in a range of from 0.1 to 1.0, preferably from 0.2 to 1.0, more preferably from 0.2 to 0.6, and most preferably from 0.2 to 0.5. Examples of suitable epoxy resin are E20, E40 and E51.

[0024] The content of said epoxy resin is from 10%to 70%, preferably from 15%to 50 %, more prefer-ably from 15%to 30%by weight, based on the total weight of the coating composition.

[0025] The silicone-modified epoxy resins are obtained by reaction of polysiloxane having at least one reactive end group and a compound having at least one epoxy group, and the reactive end group includes hydroxyl, amino and alkoxy group. The polysiloxane having at least one reactive end group may be polydimethylsiloxane having a terminal amino group, such as polydime-thylsiloxane having a terminal dimethylamino group, a terminal diethylamino group or a terminal dipropylamino group. The polysiloxane having a reactive end group may have a number aver-age molecular weight in a range of from 100 to 10,000g / mol, preferably from 200 to 8,000 g / mol and more preferably from 500 to 5,000g / mol. The compound having at least one epoxy group could be the same as Component (a) . The polysiloxane has reactive end group (s) per polymer chain in a range of from 1 to 20, preferably from 1 to 10 and more preferably from 1 to 5.

[0026] The content of the silicone-modified epoxy resin is in a range of from 1%to 40%, preferably from 2%to 30%, and more preferably from 5%to 15%by weight, based on the total weight of the coating composition.

[0027] Hydrocarbon resin is a thermoplastic resin obtained by polymerization of C5 aliphatic monomers, C9 aromatic monomers that are by-products of petroleum cracking. The polymerization reaction takes place with heating in presence of catalysts such as sulfuric acid, anhydrous aluminum trichloride, boron trifluoride, etc. Examples of the hydrocarbon resins include aliphatic resins e.g. C5 aliphatic resins, alicyclic resins e.g. dicyclopentadiene, aromatic resins e.g. C9 aromatic res-ins, copolymers of aliphatic and aromatic monomers e.g. copolymers of C5 aliphatic monomer and C9 aromatic monomer and hydrogenated hydrocarbon resins such as hydrogenated C5 hydrocarbon resin and hydrogenated C9 hydrocarbon resin. The hydrocarbon resin is commer-cially available, such as Novares LA300 from RüTGERS Group, Germany.

[0028] The content of the hydrocarbon resin is in a range of from 0.1%to 15%, preferably from 0.5%to 10%, and more preferably from 0.5%to 5%by weight, based on the total weight of the coating composition.

[0029] The coating composition of the present invention may further comprise a reactive diluent that can dramatically reduce the viscosity and at the same time increase the solid content of the coating system and meanwhile reduce the solvent emissions.

[0030] The reactive diluent has a low molecular weight at least one functional group reactive to epoxy groups of epoxy resins and / or functional group (s) e.g. epoxy group of curing agents. The reac-tive diluent can reduce the viscosity of the epoxy resin and therefore it does not evaporate dur-ing curing.

[0031] Examples of the monofunctional active diluent are glycidyl ether of a C2 to C20 aliphatic and alicyclic monohydroxyl compound such as C2-C20 alkyl glycidyl ether, in particular 2-ethylhexyl glycidyl ether, and glycidyl ester of a C2 to C20 aliphatic or alicyclic monocarboxylic acid. Pref-erably the reactive diluents are epoxy functional cashew phenols, such as Cardolite LITE 513 from Cardolite Corporation. It was surprisingly found that when epoxy functional cashew phenol is used, the solid content of the coating composition can be increased, and the toughness of the paint film is increased thereof, thus the salt resistance is improved.

[0032] Examples of the multifunctional reactive diluent are glycidyl ether of a C2 to C20 multifunctional alcohols having average from 1.5 to 4 glycidyl groups, such as glycidyl ether of a saturated alkane polyol, in particular 1, 4-butanediol diglycidyl ether, 1, 6-hexanediol diglycidyl ether, di-or tri-glycidyl ether of trimethylolpropane, di-, tri-or tetra-glycidyl ether of pentaerythritol; or glycidyl ether of polyether alcohol, in particular diglycidyl ether of diethylene glycol, diglycidyl ether of triethylene glycol, diglycidyl ether of tetraethylene glycol, diglycidyl ether of polyethylene glycol or diglycidyl ether of polypropylene glycol; or glycidyl ether of an alicyclic alcohol, in particular cyclohexane-1, 4-diyl diglycidyl ether, diglycidyl ether of ring-hydrogenated bisphenol A or ring-hydrogenated bisphenol F.

[0033] The content of reactive diluent is in an amount of from 0.1%to 30%, preferably from 0.5%to 15%, and more preferably from 1%to 10%by weight, based on the total weight of the coating composition.

[0034] The coating composition of the present invention may also comprise at least one conventional solvent i.e. any organic solvent having a boiling point lower than 200℃ under 1 atm without  capacity of taking reaction with any other components of the coating composition. Examples of such conventional solvents are known to persons skilled in the art.

[0035] Preferably, the solvent in the coating composition of the present invention does not comprise any aromatic hydrocarbon solvent, especially toluene, ethylbenzene and xylenes to meet the requirements of environmental protection.

[0036] The solvent is added in amount that the viscosity of the obtained coating composition is suitable for applying. In some embodiments, the amount of solvent is in a range of from 1%to 20%and preferably from 2%to 15%and more preferably from 5%to 15%by weight, based on the total weight of the coating composition and consequently the viscosity of the coating composition is in a range of from 18 to 25 seconds (cup No. 4, 23℃) .

[0037] The curing agents could be amines, amides and anhydrides. The amine curing agent may in-clude: an aliphatic polyamine, such as ethylenediamine, propylenediamine, neopentyldiamine, hexamethylenediamine, octanediamine, 1, 10-diaminodecane, 1, 12-diaminododecane, diethy-lenetriamine, triethylenetetramine or tetraethylenepentamine; a cycloaliphatic polyamine, such as 1, 2-diaminocyclohexane, 1, 3-bis (aminomethyl) -cyclohexane, 1-methyl-2, 4-diaminocyclohexane, 4- (2-aminopropan-2-yl) -1-methylcyclohexane-1-amine, isophoronedia-mine, 4, 4'-diaminodicyclohexylmethane, 3, 3'-dimethyl-4, 4'-diaminodicyclohexylmethane or 4, 8-diaminotricyclo [5.2.1.0] decane; an aromatic polyamine, such as toluene diamine, xylene dia-mine, especially m-xylene diamine or bis (4-aminophenyl) methane; a cyclic polyamine, such as piperazine or aminoethylpiperazine; or an amino resin.

[0038] The amide curing agent may include, for example, a polyamide, which may be obtained by ami-dation of a dimeric or trimeric unsaturated fatty acid (e.g. dimeric linoleic acid) with a polyamine. Examples of the useful amide curing agent are, for example, Ancamide 2864 or Ancamine 2280 from Air Products Co., Ltd.

[0039] Examples of the anhydride curing agent may include maleic anhydride, phthalic anhydride, me-thyltetrahydrophthalic anhydride and hexahydrophthalic anhydride.

[0040] The curing agent is added into the coating composition immediately before applying the coating process. And after it is added, the ratio by molar of functional groups reactive to epoxy groups in the curing agent and epoxy groups in the coating composition is in a range of from 1: 2 to 2: 1, preferably from 1: 1.5 to 1.5: 1 and more preferably 1: 1.

[0041] In some embodiments, drying agent is added to the coating composition to accelerate the cur-ing process. Examples of drying agent are substituted imidazoles (e.g. 1-methylimidazole, 2-methylimidazole, 2, 4-ethylmethylimidazole, 2-phenylimidazole, 1-cyanoethylimidazole) , imidaz-olines (e.g. 2-phenylimidazoline) , tertiary amines (e.g. N, N-dimethylbenzylamine) , 1, 4-diazabicyclo [2, 2, 2] octane (DABCO) , 1, 8-diazabicyclo [5.4.0] undec-7-ene (DBU) , bis (2-dimethylaminoethyl) ether, pentamethyldiethylenetriamine, trimethylaminoethyl ethanolamine, tetramethyl-1, 6-hexamethylene diamine, aminoethyl morpholine, 2, 4, 6-tris (dimethylaminomethyl) phenol (e.g., DMP-30) , phenols and phenolic resins (e.g., bisphenol A, bisphenol F, nonylphe-nol, p-tert-butylphenol) , novolac type phenolic resins, salicylic acid, p-toluenesulfonic acid, ami-nopropylmorpholine, aminoethyethylidene urea, ketimines (for example, the reaction product of ethylenediamine and methyl isobutyl ketone) , etc.

[0042] The content of the drying agent is in a range of from 0.001%to 1.0%, preferably from 0.001%to 0.1%by weight, based on the total weight of the coating composition.

[0043] The coating composition of the present invention may further comprise additives such as dis-persant, leveling agent, defoamer, anti-settling agent, antirust pigment, effective pigments and fillers, etc., in proper amounts (e.g., from 0.01%to 10%by weight of the total amount of the coating composition) .

[0044] The antirust pigment plays the roles of both antirust agent and pigment and might be phos-phates or chromate. Examples of phosphate antirust pigment could be at least one selected from a group consisting of monometallic phosphate such as zinc phosphate, calcium phosphate, aluminium phosphate, titanium phosphate, zirconium phosphate and cerium phosphate; multi-metallic phosphate such as zinc molybdenum phosphate, zinc chromium phosphate, zinc iron phosphate, calcium strontium phosphosilicate, zinc strontium phosphosilicate, zinc calcium strontium phosphosilicate and preferably zinc strontium phosphosilicate; triphosphate such as aluminium triphosphate; ion-exchanging phosphate such as ion-exchanging zinc phosphate (e.g. Halox 430 from ICL Industry) . The antirust pigment may also be mica powder and preferably those one having a high ratio (e.g. ≥100) of diameter-to-thickness.

[0045] Surprisingly, it was found that when zinc strontium phosphosilicate is used as the antirust pig-ment, a very good antirust effect is achieved. And when tripolyphosphate (especially aluminum tripolyphosphate) is combined with mica powder, the obtained coating layers show better anti-corrosion effects. And particularly good anti-corrosion effect is reached when tripolyphosphate (especially aluminum tripolyphosphate) , ion-exchanging phosphate (especially ion-exchanging  zinc phosphate) , polymetallic phosphate (especially zinc strontium phosphosilicate) and mica are combining used.

[0046] The content of the antirust pigment could be in a range of from 1%to 60%, preferably from 5%to 30%and more preferably from 10%to 25%by weight, based on the total weight of the coat-ing composition.

[0047] The coating composition of the present invention is a two-component coating, wherein one component comprises binder resin and additives, and the other component comprises curing agent and optional drying agent and solvent.

[0048] The coating composition of the present invention can be prepared by mixing all components of the two-component coating composition.

[0049] In some embodiments, the coating composition of the present invention can be prepared by following steps:

[0050] 1) in one container mixing the epoxy resin, silicone-modified epoxy, hydrocarbon resin, reactive diluent, dispersant, coupling agent and solvent, then adding antirust pigment, effective pig-ments, filler and anti-settling agent in a dispersed state and dispersing the mixture at a speed of from 1000rpm to 1500rpm for 15 to 20 minutes, and then grinding it until the fine-ness is no more than 40μm.

[0051] 2) in another container mixing curing agent, drying agent and solvent.

[0052] 3) mixing the compositions obtained from steps 1) and 2) .

[0053] By grinding the mixture of anti-settling agent, antirust pigment, effective pigments and fillers, the evenly dispersed mixture could provide high thixotropy i.e. excellent applicability. And before applying onto substrates, the coating composition could be aged for a period of from 30 to 40 minutes.

[0054] Suitable application methods are known to persons skilled in the art, such as spraying, spin coating, dip coating, roller coating, knife coating and brush coating.

[0055] After application, the coating is cured at room temperature (5℃ to 25℃) or with heating to a temperature in a range of from 30℃ to 120℃, preferably from 40℃ to 80℃, for example at 60℃. The curing could be carried out in an oven and the curing time may be from 1 to 120 minutes, preferably from 20 to 100 minutes, and more preferably from 30 to 70 minutes.

[0056] The coating composition of the present invention could be applied onto substrates as primer and said substrates include metal, wood, plastic, glass, etc., and preferably metal.

[0057] The coating composition of the present invention is drying fast. In some embodiments, it has a surface drying speed in a range of from 5 to 40 minutes, preferably from 10 to 25 minutes, un-der 25℃ and 70%humidity. With baking for 30 minutes at 60℃, the obtained warm coating layer leaves no mark after fingers press. This advantage of fast drying makes the invented coating composition is especially suitable for large engineering machinery and equipment of which the production line has a high turnover.

[0058] In conclusion, the coating composition of the present invention has low VOCs content in a range of less than 20%and preferably less than 10%by weight based on the total weight of the coat-ing composition, high solid content in a range of at least 80%and preferably at least 90%by weight based on the total weight of the coating composition, and easy for applying. The ob-tained coating layer (e.g. primer) is good at corrosion resistance especially salt resistance and also excellent mechanical properties. Moreover, the obtained coating layer could achieve good properties with low thickness of layers and therefore the cost is saved as well.

[0059] EMBODIMENT

[0060] Specific embodiments of the present invention are described below. These specific embodi-ments should not be interpreted as limitation on the scope of the present invention, which is only determined by the appended claims.

[0061] Embodiment 1

[0062] A low VOC coating composition comprising

[0063] Component (a) : at least one epoxy resin having an epoxy value in a range of from 0.1 to 1.0, preferably from 0.2 to 0.7 and more preferably from 0.3 to 0.6,

[0064] Component (b) : at least one silicone-modified epoxy resin,

[0065] Component (c) : at least one hydrocarbon resin, and a reactive diluent, wherein said Component (a) is at least one selected from a group consisting of glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, alicyclic epoxy compound and aliphatic epoxy com-pound, preferably glycidyl ether epoxy resin and more preferably bisphenol A glycidyl ether epoxy resin.

[0066] Embodiment 2

[0067] The coating composition according to Embodiment 1, wherein the content of said Component (a) is in a range of from 10%to 70%, preferably from 15%to 50%and more preferably from 15%to 30%by weight, based on the total weight of the coating composition.

[0068] Embodiment 3

[0069] The coating composition according to any one of Embodiments 1 to 2, wherein said Component (b) is a product obtained from reactions of an epoxy resin and a polysiloxane having at least one functional group reactive to epoxy groups, wherein said functional group is at least one se-lected from hydroxyl, amino and alkoxy groups.

[0070] Embodiment 4

[0071] The coating composition according to Embodiment 3, wherein said epoxy resin is Component (a).

[0072] Embodiment 5

[0073] The coating composition according to any one of Embodiments 1 to 4, wherein the content of said Component (b) is in a range of from 1%to 40%, preferably from 5%to 30%and more pref-erably from 5%to 20%by weight, based on the total weight of the coating composition.

[0074] Embodiment 6

[0075] The coating composition according to any one of Embodiments 1 to 5, wherein the content of said Component (c) is in a range of from 0.1%to 15%, preferably from 0.5%to 10%and more preferably from 0.5%to 5%by weight, based on the total weight of the coating composition. Embodiment 7

[0076] The coating composition according to any one of Embodiments 1 to 6, wherein said reactive diluent is epoxy-functional 3-pentadecylphenol.

[0077] Embodiment 8

[0078] The coating composition according to any one of Embodiments 1 to 7, wherein the content of said reactive diluent is in a range of from 0.1%to 30%, preferably from 0.5%to 15%, and more preferably from 1%to 10%by weight, based on the total weight of the coating composition.

[0079] Embodiment 9

[0080] The coating composition according to any one of Embodiments 1 to 8, wherein said antirust pigment is at least one selected from a group consisting of monometallic phosphate, multimetal-lic phosphate, triphosphate, ion-exchanging phosphate and mica powder.

[0081] Embodiment 10

[0082] The coating composition according to Embodiment 9, wherein said monometallic phosphate is at least one selected from a group consisting of zinc phosphate, calcium phosphate, aluminum phosphate, titanium phosphate, zirconium phosphate and cerium phosphate, and said multime-tallic phosphate is at least one selected from a group consisting of zinc molybdenum phosphate, zinc chromium phosphate, zinc iron phosphate, calcium strontium phosphosilicate, zinc stronti-um phosphosilicate and zinc calcium strontium phosphosilicate, and said triphosphate is alumi-num triphosphate, and said ion-exchanging phosphate is ion-exchanging zinc phosphate, and said mica powder is mica powder having a ratio of diameter to thickness of at least 100.

[0083] Embodiment 11

[0084] The coating composition according to any one of Embodiments 9 to 10, wherein said antirust pigment is a mixture of triphosphate, ion-exchanging phosphate, mica and multimetallic phos-phate, and preferably a mixture of aluminum triphosphate, ion-exchanging zinc phosphate, zinc strontium phosphosilicate and mica powder having a ratio of diameter to thickness at least 100.

[0085] Embodiment 12

[0086] The coating composition according to any one of Embodiments 9 to 11, wherein the content of said antirust pigment is in a range of from 1%to 60%, preferably from 5%to 30%and more preferably from 10%to 25%by weight, based on the total weight of the coating composition.

[0087] Embodiment 13

[0088] The coating composition according to any one of Embodiments 1 to 12, wherein it further com-prises a dispersant and preferably an anionic dispersant.

[0089] Embodiment 14

[0090] The coating composition according to any one of Embodiments 1 to 13, wherein the solid con-tent of the coating composition is at least 80%, preferably at least 90%by weight, based on the total weight of the coating composition.

[0091] Embodiment 15

[0092] A primer obtained from the coating composition according to any one of Embodiments 1 to 14 by curing.

[0093] Embodiment 16

[0094] The primer according to Embodiment 15, wherein it is formed on the substrates of engineering machineries.

[0095] EXAMPLE

[0096] The present invention is further illustrated by below examples without limiting the protection scope.

[0097] Measurement methods

[0098] 1. Solid content is measured according to GB / T 1725-2007 under 120℃ for 1 hour.

[0099] 2. Viscosity is measured according to GB / T 1723-1993 under 23℃.

[0100] 3. Primer thickness is measured according to GB / T 13452.2.

[0101] 4. Primer surface drying speed is measured according to GR / T1728-79 (88) .

[0102] 5. Adhesion is measured according to GB / T9286-1998.

[0103] 6. Front impact strength is measured according to GB / T 1732-1993.

[0104] 7. Bending test is done according to GB / T 6742-2007.

[0105] 8. Water resistance is tested according to GB / T 1733-1993.

[0106] 9. Gasoline resistance is tested according to GB / T1734-1993.

[0107] 10. Machine oil resistance is tested according to GB / T 9274-1988.

[0108] 11. Acid resistance is tested according to GB / T 1763-1989.

[0109] 12. Alkali resistance is tested according to GB / T 1763-1989.

[0110] 13. Salt resistance is tested according to GB / T 1771-2007.

[0111] Example 1 and Comparative Examples C2 to C4: preparation of coating compositions

[0112] Example 1 and comparative examples C2 to C4 are prepared by mixing Component I (epoxy curing agent) , Component II (solvent) and Component III (binder) in a ratio of 6: 1: 0.5 by weight, and deionized water is added to adjust the viscosity to 35s (cup No. 4, 23℃) . The formulations of Components I, II and III are list in Table 1, 2 and 3 respectively. In Example 1 and compara-tive examples C2 to C4, the receipts of Components I and II are the same while certain compo-nents are adjusted in Component III.

[0113] Table 1: Formulation of Component I

[0114] Table 2: Formulation of Component II

[0115] Table 3: Formulation of Component III

[0116] * The silicone-modified epoxy resin is prepared by following steps: 140 parts of xylene and 60 parts of cyclohexanone as mixed solvents, 0.75 parts of organometallic salt catalyst zinc naph-thenate, 160 parts of epoxy resin E-20 and 200 parts of methyl phenyl silicone oligomer are reacted at 135℃ for 3h to obtain a light yellow transparent liquid, and then an appropriate amount of the mixed solvents is added to prepare a solution having a solid content of 50%.

[0117] Example 1#and Comparative Examples C2#to C4#: performance tests

[0118] The coating compositions of Example 1 and Comparative Examples C2 to C4 are sprayed onto sandblasted board respectively and baked at 80℃ for 60 minutes to get samples 1#and C2#to C4#respectively. The performance tests are carried out on samples 1#and C2#to C4#and the test results are list in Table 4.

[0119] Table 4:

[0120] As can be seen from Table 4, by combining epoxy resin and silicone-modified epoxy resin, the coating composition could reach a balanced performance in low VOC, fast drying and corrosion resistance.

Claims

1.A low VOC coating composition comprisingComponent (a) : at least one epoxy resin having an epoxy value in a range of from 0.1 to 1.0, preferably from 0.2 to 0.7 and more preferably from 0.3 to 0.6,Component (b) : at least one silicone-modified epoxy resin,Component (c) : at least one hydrocarbon resin, and a reactive diluent, wherein said Com-ponent (a) is at least one selected from a group consisting of glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, alicyclic epoxy compound and ali-phatic epoxy compound, preferably glycidyl ether epoxy resin and more preferably bi-sphenol A glycidyl ether epoxy resin.2.The coating composition according to claim 1, wherein the content of said Component (a) is in a range of from 10%to 70%, preferably from 15%to 50%and more preferably from 15%to 30%by weight, based on the total weight of the coating composition.3.The coating composition according to any one of claims 1 to 2, wherein said Component (b) is a product obtained from reactions of an epoxy resin and a polysiloxane having at least one functional group reactive to epoxy groups, wherein said functional group is at least one selected from hydroxyl, amino and alkoxy groups.4.The coating composition according to claim 3, wherein said epoxy resin is Component (a) .5.The coating composition according to any one of claims 1 to 4, wherein the content of said Component (b) is in a range of from 1%to 40%, preferably from 5%to 30%and more pref-erably from 5%to 20%by weight, based on the total weight of the coating composition.6.The coating composition according to any one of claims 1 to 5, wherein the content of said Component (c) is in a range of from 0.1%to 15%, preferably from 0.5%to 10%and more preferably from 0.5%to 5%by weight, based on the total weight of the coating composition.7.The coating composition according to any one of claims 1 to 6, wherein said reactive diluent is epoxy-functional 3-pentadecylphenol.8.The coating composition according to any one of claims 1 to 7, wherein the content of said reactive diluent is in a range of from 0.1%to 30%, preferably from 0.5%to 15%, and more preferably from 1%to 10%by weight, based on the total weight of the coating composition.9.The coating composition according to any one of claims 1 to 8, wherein said antirust pig-ment is at least one selected from a group consisting of monometallic phosphate, multime-tallic phosphate, triphosphate, ion-exchanging phosphate and mica powder.10.The coating composition according to claim 9, wherein said monometallic phosphate is at least one selected from a group consisting of zinc phosphate, calcium phosphate, alumi-num phosphate, titanium phosphate, zirconium phosphate and cerium phosphate, and said multimetallic phosphate is at least one selected from a group consisting of zinc molyb-denum phosphate, zinc chromium phosphate, zinc iron phosphate, calcium strontium phos-phosilicate, zinc strontium phosphosilicate and zinc calcium strontium phosphosilicate, and said triphosphate is aluminum triphosphate, and said ion-exchanging phosphate is ion-exchanging zinc phosphate, and said mica powder is mica powder having a ratio of diame-ter to thickness of at least 100.11.The coating composition according to any one of claims 9 to 10, wherein said antirust pig-ment is a mixture of triphosphate, ion-exchanging phosphate, mica and multimetallic phos-phate, and preferably a mixture of aluminum triphosphate, ion-exchanging zinc phosphate, zinc strontium phosphosilicate and mica powder having a ratio of diameter to thickness at least 100.12.The coating composition according to any one of claims 9 to 11, wherein the content of said antirust pigment is in a range of from 1%to 60%, preferably from 5%to 30 %and more preferably from 10%to 25%by weight, based on the total weight of the coating composition.13.The coating composition according to any one of claims 1 to 12, wherein it further compris-es a dispersant and preferably an anionic dispersant.14.The coating composition according to any one of claims 1 to 13, wherein the solid content of the coating composition is at least 80%, preferably at least 90%by weight, based on the total weight of the coating composition.15.A primer obtained from the coating composition according to any one of claims 1 to 14 by curing.16.The primer according to Claim 15, wherein it is formed on the substrates of engineering ma-chineries.

Citation Information

Patent Citations

  • Low VOC epoxy priming paint, and preparation method thereof

    CN109181486A

  • Epoxy resin system for carbon fiber reinforced material

    CN107903587A

  • Solvent-free heavy anticorrosive coating, anticorrosive coating and ocean structure

    CN109971306A

Cited By

  • Epoxy resin-based woodware finish paint and production method thereof

    CN120137484A