Polylactic-acid-based composite material, and preparation method therefor and use thereof
By using polylactic acid-based composite materials, the problem of difficulty in degradation and rebound of existing nose bridge strips is solved, achieving good resilience and degradation performance of the nose bridge strips, reducing environmental pollution, and conforming to the concept of green environmental protection.
Patent Information
- Application Number
- PCT/CN2024/089726
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-26
- Filing Date
- 2024-04-25
- Publication Date
- 2024-10-31
AI Technical Summary
Existing mask nose bridge strips are mainly made of polyolefin resin, which is difficult to degrade, causing environmental pollution, lacks resilience and good degradation performance, and is difficult to comply with the concept of green and environmentally friendly development.
Using polylactic acid-based composite materials, polylactic acid, polybutylene adipate/butylene terephthalate and fillers are blended, and polyadipic acid/butylene terephthalate with intrinsic viscosity is prepared through an esterification reaction. Glycol esters to form biodegradable composite materials for use in the preparation of nose bridge strips.
It achieves good resilience, degradability and aging resistance of the nose bridge strip, meets the standards for plastic nose bridge strips for disposable masks, and reduces environmental pollution.
Smart Images

Figure CN2024089726_31102024_PF_FP_ABST
Abstract
Description
Polylactic acid-based composite material and its preparation method and application
[0001] Related applications
[0002] This application claims priority to Chinese patent application No. 2023104658137, filed on April 26, 2023, entitled “POLYLACTIC ACID-BASED COMPOSITE MATERIALS, PREPARATION METHODS AND APPLICATIONS THEREOF,” the entire text of which is incorporated herein by reference. Technical Field
[0003] The present application relates to the field of polymer composite materials, and in particular to a polylactic acid-based composite material and its preparation method and application. Background Art
[0004] The nose bridge strip, also known as the nose bridge muscle or nose bridge line, is a thin rubber strip inside the mask. It fixes the mask on the bridge of the nose and makes the mask fit well with the bridge of the nose and the skin on both sides, thereby reducing the leakage of pollutants from the gaps on both sides of the nose bridge when wearing the mask.
[0005] Current mask nose bridge strips are primarily made of polyolefin resin. Like wire, these strips bend and deform with external forces, retaining their shape without rebounding when external forces are removed. These strips secure the mask to the nose bridge. While inexpensive, polyolefin resins are difficult to degrade, contributing to environmental pollution and contradicting the concept of green development. Developing a nose bridge strip with both good resilience and degradation resistance is crucial.
[0006] Summary of the Invention
[0007] Based on this, according to various embodiments of the present application, a polylactic acid-based composite material, a preparation method and an application thereof are provided.
[0008] The technical solution is as follows:
[0009] A biodegradable polylactic acid-based composite material comprises the following components in parts by weight:
[0010] 15-55 parts of polylactic acid;
[0011] 30-70 parts of polybutylene adipate / terephthalate; and
[0012] 15-40 parts of filler;
[0013] In the polylactic acid, the mass content of residual monomers is ≤0.3%;
[0014] The polybutylene adipate / terephthalate has a structure shown in formula (I):
[0015] p is 0.44 to 0.54, p + q = 1;
[0016] At 25° C., the intrinsic viscosity of the polybutylene adipate / terephthalate is 0.9 dL / g to 1.9 dL / g.
[0017] In one embodiment, the biodegradable polylactic acid-based composite material comprises the following components in parts by weight:
[0018] 15-45 parts of polylactic acid;
[0019] 40-60 parts of polybutylene adipate / terephthalate; and
[0020] 15 to 35 parts of filler.
[0021] In one embodiment, the mass content of the polybutylene adipate / terephthalate in the biodegradable polylactic acid-based composite material is ≥20%.
[0022] In one embodiment, the filler has a D50 particle size of ≤10 μm.
[0023] In one embodiment, the filler is talc and calcium carbonate or a mixture of both.
[0024] In one embodiment, the biodegradable polylactic acid-based composite material further comprises 0.1 to 2 parts by weight of a lubricant.
[0025] The present application also provides a method for preparing the biodegradable polylactic acid-based composite material as described above, comprising the following steps:
[0026] The polylactic acid, polybutylene adipate / terephthalate and filler are blended and extruded.
[0027] In one embodiment, the extrusion temperature is 130°C to 220°C.
[0028] In one embodiment, the preparation method of polybutylene adipate / terephthalate comprises the following steps:
[0029] Terephthalic acid, 1,4-butanediol and a catalyst are mixed and an esterification reaction is performed to prepare an esterified product A1, wherein the molar ratio of terephthalic acid to 1,4-butanediol is (1.1-2.5):1;
[0030] Adipic acid and 1,4-butanediol are mixed in a molar ratio of (1 to 1.8):1, and an esterification reaction is performed to prepare an esterified product A2;
[0031] The esterified product A1 and the esterified product A2 are mixed and reacted at a temperature of 200° C. to 245° C. and a pressure of 1 KPa to 10 KPa for 0.5 h to 5 h to prepare a prepolymer;
[0032] The prepolymer is reacted for 1 to 5 hours at a temperature of 230° C. to 255° C. and a pressure of ≤150 Pa to prepare the polybutylene adipate / terephthalate.
[0033] In one embodiment, the process parameters for preparing the ester A1 include:
[0034] The temperature is 200℃~250℃, the pressure is 30KPa~110KPa, and the time is 1.5h~3.5h.
[0035] In one embodiment, the process parameters for preparing the ester A2 include:
[0036] The temperature is 100℃~250℃, the pressure is 30KPa~110KPa, and the time is 2h~4h.
[0037] The present application also provides a nose bridge strip, comprising the biodegradable polylactic acid-based composite material as described above, or the biodegradable polylactic acid-based composite material prepared according to the preparation method as described above.
[0038] The present application also provides a mask comprising the nose bridge strip as described above.
[0039] The details of one or more embodiments of the present application are set forth in the description below, and other features, objects, and advantages of the application will become apparent from the description and from the claims thereof. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the following is a brief introduction to the drawings required for use in the specific implementation methods or the description of the prior art. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.
[0041] FIG1 is a hydrogen nuclear magnetic resonance spectrum of PBAT prepared in a synthesis example of the present application. DETAILED DESCRIPTION
[0042] To make the above-mentioned objects, features, and advantages of the present application more clearly understood, the specific embodiments of the present application are described in detail below. The following description sets forth many specific details to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways than those described herein, and those skilled in the art can make similar modifications without violating the scope of the present application. Therefore, the present application is not limited to the specific embodiments disclosed below.
[0043] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application pertains. The terms used herein in the specification of this application are for the purpose of describing specific embodiments only and are not intended to limit this application. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0044] In this application, when referring to numerical ranges, unless otherwise specified, the numerical ranges are considered continuous and include the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe a feature or characteristic, the ranges can be combined. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges subsumed therein.
[0045] The temperature parameters in this application, unless otherwise specified, allow for both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows for temperature fluctuations within the precision range of instrument control.
[0046] In this application, when referring to a range of units, if only the right endpoint is followed by the unit, it means that the units of the left and right endpoints are the same. For example, 150-160°C means that the units of the left endpoint "150" and the right endpoint "160" are both degrees Celsius.
[0047] In this application, in the description of the application, "several" means at least two, such as two, three, etc., unless otherwise clearly and specifically defined. In the description of the application, "several" means at least one, such as one, two, etc., unless otherwise clearly and specifically defined.
[0048] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0049] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0050] It should be noted that, in the description of this application, directional words such as the terms "center", "horizontal", "longitudinal", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like indicate directions and positional relationships based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and should not be understood as limiting the specific scope of protection of this application.
[0051] Where “including,” “having,” and “comprising” are used herein, it is intended to cover a non-exclusive inclusion, and another component may also be added unless a clear limiting term such as “only,” “consisting of,” etc. is used.
[0052] Unless mentioned otherwise, terms in the singular may include plural forms and should not be construed as having one number.
[0053] In the present application, the ratio of polybutylene terephthalate in polybutylene adipate / terephthalate can be obtained by measuring the hydrogen nuclear magnetic resonance spectrum of polybutylene adipate / terephthalate and calculating the peak area of the corresponding peak.
[0054] In this application, the intrinsic viscosity is determined according to DIN 53728, Part 3, January 3, 1985. The solvent used includes a mixture of phenol and dichlorobenzene in a weight ratio of 50:50. The test temperature is 25°C.
[0055] The residual monomer content of polylactic acid in this application is tested as follows:
[0056] 1. Prepare standard solution
[0057] (1) Weigh 100 ± 10 mg of pentamethylbenzene and mix it with 100 mL of dichloromethane. Shake well. This is called the internal standard solution.
[0058] (2) Weigh 100 ± 10 mg of L-lactide standard, prepare a 100 mL dichloromethane solution, shake well, and record it as the standard solution;
[0059] (3) Take 1.0, 2.0, 5.0, 10.0, and 20.0 mL of the standard solution and transfer them to 25 mL volumetric flasks. Add 4.0 mL of the internal standard solution to each flask, fill it up with n-hexane, and shake at a constant temperature. These are referred to as calibration standard solutions.
[0060] 2. Sample testing
[0061] (1) Weigh 200 ± 20 mg of polylactic acid sample (W) in a 20 ml glass vial and add 4.0 ml of internal standard solution. Dissolve the sample at room temperature, stirring to aid dissolution. After the sample is completely dissolved, slowly add 10 ml of n-hexane to the inner wall of the flask. Stopper the vial and shake vigorously for 5-10 seconds. Let the sample stand for 10 minutes.
[0062] (2) After filtering with a membrane filter, transfer to a dedicated gas chromatography injection vial and perform the test according to the above-mentioned gas chromatography analysis conditions. Each sample solution should be injected at least 3 times.
[0063] 3. Calculation of residual monomer content of polylactic acid
[0064] Calculate the area ratio AR of lactide and pentamethylbenzene in the injected sample S and read the corresponding content ratio CR from the calibration curve S .
[0065] The lactide content of the sample during each GC run was calculated as follows:
[0066] CR S : The content ratio read in the calibration curve;
[0067] IS S : The mass of pentamethylbenzene in 100 mL of the internal standard solution for sample determination [mg / 100 mL];
[0068] W: weighed mass of PLA sample [mg].
[0069] In this application, the median particle size D50 test method is determined by referring to the method of GB / T 19077-2016 "Particle size distribution laser diffraction method".
[0070] The present application provides a polylactic acid-based composite material with good resilience, aging resistance and biodegradability by adopting a specific resin polymer formula, which can be used for nose bridge strips.
[0071] The technical solution is as follows:
[0072] A biodegradable polylactic acid-based composite material comprises the following components in parts by weight:
[0073] 15-55 parts of polylactic acid;
[0074] 30-70 parts of polybutylene adipate / terephthalate; and
[0075] 15-40 parts of filler;
[0076] The polybutylene adipate / terephthalate has a structure shown in formula (I):
[0077] p is 0.44 to 0.54, p + q = 1;
[0078] The intrinsic viscosity of the polybutylene adipate / terephthalate is 0.9 dL / g to 1.9 dL / g.
[0079] The applicant's research found that the content of polybutylene terephthalate segments in polybutylene adipate / terephthalate affects the degradation performance and strength of the composite material. The higher the polybutylene terephthalate content, the better the resilience and setting effects. In addition, the intrinsic viscosity of polybutylene adipate / terephthalate also affects the degradation performance of the composite material. The higher the intrinsic viscosity, the worse the degradation performance of the composite material, and the better the resilience and setting effects, especially the aging setting effect. In addition, the higher the residual monomer content in polylactic acid, the worse the aging setting effect of the composite material. The present application controls the molar fraction of the polybutylene terephthalate segment in polyadipate / terephthalate to be 0.44 to 0.54, and the intrinsic viscosity of the polybutylene adipate / terephthalate is 0.9 dL / g to 1.9 dL / g, and the mass content of the residual monomer in the polylactic acid is ≤0.3%. In combination with fillers, a biodegradable polylactic acid-based composite material with excellent resilience, degradability and aging resistance is prepared.
[0080] It can be understood that in the present application, in the polybutylene adipate / terephthalate, the mole fraction of the polybutylene terephthalate segment is 0.44 to 0.54, including but not limited to 0.44, 0.45, 0.46, 0.47, 0.48, 0.49, 0.50, 0.51, 0.52, 0.53 and 0.54.
[0081] It is to be understood that in the present application, the intrinsic viscosity of the polybutylene adipate / terephthalate is 0.9 dL / g to 1.9 dL / g, including but not limited to 0.9 dL / g, 1.0 dL / g, 1.1 dL / g, 1.2 dL / g, 1.3 dL / g, 1.4 dL / g, 1.5 dL / g, 1.6 dL / g, 1.7 dL / g, 1.8 dL / g and 1.9 dL / g. Preferably, the intrinsic viscosity of the polybutylene adipate / terephthalate is 1 dL / g to 1.9 dL / g. Further, the intrinsic viscosity of the polybutylene adipate / terephthalate is 1.1 dL / g to 1.6 dL / g.
[0082] It can be understood that in the present application, the biodegradable polylactic acid-based composite material contains 30 to 70 parts of poly(butylene adipate / terephthalate) in parts by weight, including but not limited to 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, 65 parts and 70 parts, preferably 40 to 60 parts.
[0083] In one embodiment, the mass content of the polybutylene adipate / terephthalate in the biodegradable polylactic acid-based composite material is ≥ 20%, including but not limited to 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70% and 75%. Furthermore, the mass content of the polybutylene adipate / terephthalate in the biodegradable polylactic acid-based composite material is 25% to 65%.
[0084] It is understood that the weight content of residual monomers in the polylactic acid is ≤0.3%, which enables the composite material to have excellent degradability, resilience and aging stability. It is understood that the weight content of residual monomers in the polylactic acid includes but is not limited to 0, 0.1%, 0.2% and 0.3%.
[0085] It can be understood that in the present application, the biodegradable polylactic acid-based composite material contains 15 to 55 parts of polylactic acid (PLA) by weight, including but not limited to 15 parts, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts and 55 parts, preferably 15 to 55 parts.
[0086] It can be understood that in the present application, the biodegradable polylactic acid-based composite material contains 15 to 40 parts of filler in parts by weight, including but not limited to 15 parts, 20 parts, 25 parts, 30 parts, 35 parts and 40 parts, preferably 15 to 35 parts.
[0087] The applicant has found that the larger the D50 particle size of the filler, the worse the aging setting effect of the composite material. In one embodiment, the D50 particle size of the filler is ≤10μm, which enables the composite material to have excellent degradability, resilience and aging setting effects. It is understandable that the D50 particle size of the filler includes but is not limited to 0.1μm, 0.2μm, 0.3μm, 0.4μm, 0.5μm, 0.6μm, 0.7μm, 0.8μm, 0.9μm, 1μm, 1.5μm, 2μm, 2.5μm, 3μm, 3.5μm, 4μm, 4.5μm, 5μm, 5.5μm, 6μm, 6.5μm, 7μm, 7.5μm, 8μm, 8.5μm, 9μm, 9.5μm and 10μm. Preferably, the D50 particle size of the filler is ≤5μm.
[0088] In one embodiment, the filler is talc and / or calcium carbonate. Preferably, the filler is talc.
[0089] In one embodiment, the biodegradable polylactic acid-based composite material further comprises a lubricant.
[0090] In one embodiment, the lubricant is selected from one or a mixture of stearamide, oleamide, erucamide, zinc stearate, high molecular weight complex ester of metal soap, ethylene bisstearamide, polyethylene wax and silicone lubricants.
[0091] In one embodiment, the biodegradable polylactic acid-based composite material further includes 0.1 to 2 parts of a lubricant, in parts by weight, including but not limited to 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9 and 2 parts, preferably 0.1 to 1 part.
[0092] In some embodiments, the biodegradable polylactic acid-based composite material has a melt flow rate (melt index) of 2 g / 10 min to 15 g / 10 min and a flexural modulus greater than 1000 MPa. When the biodegradable polylactic acid-based composite material is used to prepare a nose bridge strip, the resulting nose bridge strip has a springback angle of less than 10° when folded at 180° and less than 15° when folded at 90°. After aging, the springback angle of the strip is less than 15° when folded at 180° and less than 20° when folded at 90°, meeting the standard for "Plastic Nose Bridge Strips for Disposable Masks."
[0093] In one embodiment, the biodegradable polylactic acid-based composite material comprises the following components in parts by weight:
[0094] In one embodiment, the biodegradable polylactic acid-based composite material comprises the following components in parts by weight:
[0095] The present application also provides a method for preparing the biodegradable polylactic acid-based composite material as described above, comprising the following steps:
[0096] The polylactic acid, polybutylene adipate / terephthalate and filler are blended and extruded.
[0097] In one embodiment, the extrusion temperature is 130° C. to 220° C. In one embodiment, after extrusion, the extruded product is cooled, shaped, and granulated.
[0098] In one embodiment, the preparation method of polybutylene adipate / terephthalate comprises the following steps:
[0099] Terephthalic acid, 1,4-butanediol, and a catalyst are mixed and subjected to an esterification reaction to prepare an esterified product A1; wherein, preferably, the molar ratio of terephthalic acid to 1,4-butanediol is (1.1-2.5):1; the catalyst accounts for 0.3% to 2.65% of the total mass of the raw materials, and the catalyst is one or a mixture of zinc-based, tin-based, and titanium-based catalysts;
[0100] Adipic acid and 1,4-butanediol are mixed in a molar ratio of (1 to 1.8):1, and an esterification reaction is performed to prepare an esterified product A2;
[0101] The esterified product A1 and the esterified product A2 are mixed and reacted at a temperature of 200° C. to 245° C. and a pressure of 1 KPa to 10 KPa for 0.5 h to 5 h (prepolymerization stage) to prepare a prepolymer;
[0102] The prepolymer is continued to react at a temperature of 230° C. to 255° C. and a pressure of ≤150 Pa (post-polymerization stage) for 1.0 h to 5 h to prepare the polybutylene adipate / terephthalate.
[0103] The content of the polybutylene terephthalate segment in the PBAT and the intrinsic viscosity of the PBAT are controlled by adjusting the ratio of the raw materials and the reaction time of the polymerization process, so that the mole fraction of the polybutylene terephthalate segment in the PBAT having the structure represented by formula (I) is 0.44 to 0.54, and the intrinsic viscosity of the PBAT is 0.9 dL / g to 1.9 dL / g at 25°C.
[0104] In one embodiment, the process parameters for preparing the ester A1 include:
[0105] The temperature is 200℃~250℃, the pressure is 30KPa~110KPa, and the time is 1.5h~3.5h.
[0106] In one embodiment, the process parameters for preparing the ester A2 include:
[0107] The temperature is 100℃~250℃, the pressure is 30KPa~110KPa, and the time is 2h~4h.
[0108] The present application also provides a nose bridge strip, comprising the biodegradable polylactic acid-based composite material as described above, or the biodegradable polylactic acid-based composite material prepared according to the preparation method as described above.
[0109] The present application also provides a mask comprising the nose bridge strip as described above.
[0110] The following is a specific embodiment:
[0111] (1) Raw material description:
[0112] ① Polylactic acid:
[0113] PLA-1, purchased from Nature Works, with a residual monomer content of 0.1%;
[0114] PLA-2, purchased from Nature Works, with a residual monomer content of 0.3%;
[0115] PLA-3, purchased from Nature Works, with a residual monomer content of 0.5% by mass.
[0116] ②Packing:
[0117] Talc-1, commercially available, D50 particle size 5 μm;
[0118] Talc-2, commercially available, D50 particle size of 10 μm;
[0119] Calcium carbonate, commercially available, with a D50 particle size of 8 μm.
[0120] ③Lubricant: ethylene bisstearamide.
[0121] (2) Synthesis example:
[0122] Synthesis example 1:
[0123] This synthesis example provides a polybutylene adipate / terephthalate and a preparation method thereof, as follows:
[0124] 1) Terephthalic acid and 1,4-butanediol were added to an esterification reactor at a molar ratio of 1.1:1, and a catalyst of n-butyl titanate was added at 1% by weight of the total raw materials. The reaction was carried out at a temperature of 240° C. and a pressure of 40 kPa for 2.5 hours to obtain an esterified product A1;
[0125] 2) adding adipic acid and 1,4-butanediol in a molar ratio of 1.6:1 to an esterification reaction kettle, and reacting at a temperature of 200° C. and a pressure of 40 kPa for 2.5 hours to obtain an esterified product A2;
[0126] 3) The esters A1 and A2 were continuously fed into a mixer for mixing and reacted at a temperature of 240° C. and a pressure of 4 kPa for 2.5 hours to obtain a prepolymer, which was then further polymerized at a temperature of 240° C. and a pressure of 120 Pa for 2.5 hours to obtain biodegradable poly(butylene adipate / terephthalate) PBAT-1.
[0127] Synthesis example 2:
[0128] This synthesis example provides a polybutylene adipate / terephthalate and a preparation method thereof, as follows:
[0129] 1) Terephthalic acid and 1,4-butanediol were added to an esterification reactor at a molar ratio of 1.1:1, and a catalyst of n-butyl titanate was added at 1% by weight of the total raw materials. The reaction was carried out at a temperature of 240° C. and a pressure of 40 kPa for 2.5 hours to obtain an esterified product A1;
[0130] 2) adding adipic acid and 1,4-butanediol in a molar ratio of 1.5:1 to an esterification reaction kettle, and reacting at a temperature of 200° C. and a pressure of 40 kPa for 2.5 hours to obtain an esterified product A2;
[0131] 3) The esters A1 and A2 were continuously fed into a mixer for mixing and reacted at a temperature of 200° C. and a pressure of 4 kPa for 2.5 hours to obtain a prepolymer, which was then further polymerized at a temperature of 240° C. and a pressure of 120 Pa for 2.5 hours to obtain biodegradable poly(butylene adipate / terephthalate) PBAT-2.
[0132] Synthesis example 3:
[0133] This synthesis example provides a polybutylene adipate / terephthalate and a preparation method thereof, as follows:
[0134] 1) Terephthalic acid and 1,4-butanediol were added to an esterification reactor at a molar ratio of 1.1:1, and a catalyst of n-butyl titanate was added at 1% by weight of the total raw materials. The reaction was carried out at a temperature of 240° C. and a pressure of 40 kPa for 2.5 hours to obtain an esterified product A1;
[0135] 2) adding adipic acid and 1,4-butanediol in a molar ratio of 1.3:1 to an esterification reaction kettle, and reacting at a temperature of 200° C. and a pressure of 40 kPa for 2.5 hours to obtain an esterified product A2;
[0136] 3) The esters A1 and A2 were continuously fed into a mixer for mixing and reacted at a temperature of 240° C. and a pressure of 4 kPa for 2.5 hours to obtain a prepolymer, which was then further polymerized at a temperature of 200° C. and a pressure of 120 Pa for 2.5 hours to obtain biodegradable poly(butylene adipate / terephthalate) PBAT-3.
[0137] Synthesis example 4:
[0138] This synthesis example provides a polybutylene adipate / terephthalate and a preparation method thereof, as follows:
[0139] 1) Terephthalic acid and 1,4-butanediol were added to an esterification reactor at a molar ratio of 1.1:1, and a catalyst of n-butyl titanate was added at 1% by weight of the total raw materials. The reaction was carried out at a temperature of 240° C. and a pressure of 40 kPa for 2.5 hours to obtain an esterified product A1;
[0140] 2) adding adipic acid and 1,4-butanediol in a molar ratio of 1.0:1 into an esterification reaction kettle, and reacting at a temperature of 200° C. and a pressure of 40 kPa for 2.5 hours to obtain an esterified product A2;
[0141] 3) The esters A1 and A2 were continuously fed into a mixer for mixing and reacted at a temperature of 240° C. and a pressure of 4 kPa for 2.5 hours to obtain a prepolymer, which was then further polymerized at a temperature of 240° C. and a pressure of 120 Pa for 2.5 hours to obtain biodegradable poly(butylene adipate / terephthalate) (PBAT-4).
[0142] Synthesis example 5:
[0143] This synthesis example provides a polybutylene adipate / terephthalate and a preparation method thereof, as follows:
[0144] 1) Terephthalic acid and 1,4-butanediol were added to an esterification reactor at a molar ratio of 1.5:1, and n-butyl titanate was added as a catalyst at a concentration of 1% by weight of the total raw materials. The reaction was carried out at a temperature of 240° C. and a pressure of 40 kPa for 2.5 hours to obtain an esterified product A1;
[0145] 2) adding adipic acid and 1,4-butanediol in a molar ratio of 1.67:1 to an esterification reaction kettle, and reacting at a temperature of 200° C. and a pressure of 40 kPa for 2.5 hours to obtain an esterified product A2;
[0146] 3) The esters A1 and A2 were continuously fed into a mixer for mixing and reacted at a temperature of 240° C. and a pressure of 4 kPa for 2.5 hours to obtain a prepolymer, which was then further polymerized at a temperature of 240° C. and a pressure of 120 Pa for 2.5 hours to obtain biodegradable poly(butylene adipate / terephthalate) PBAT-5.
[0147] Synthesis example 6:
[0148] This synthesis example provides a polybutylene adipate / terephthalate and a preparation method thereof, as follows:
[0149] 1) Terephthalic acid and 1,4-butanediol were added to an esterification reactor at a molar ratio of 1.1:1, and a catalyst of n-butyl titanate was added at 1% by weight of the total raw materials. The reaction was carried out at a temperature of 240° C. and a pressure of 40 kPa for 2.5 hours to obtain an esterified product A1;
[0150] 2) adding adipic acid and 1,4-butanediol in a molar ratio of 1.3:1 to an esterification reaction kettle, and reacting at a temperature of 200° C. and a pressure of 40 kPa for 2.5 hours to obtain an esterified product A2;
[0151] 3) The esters A1 and A2 were continuously fed into a mixer for mixing and reacted at a temperature of 240° C. and a pressure of 4 kPa for 2.5 hours to obtain a prepolymer, which was then further polymerized at a temperature of 240° C. and a pressure of 120 Pa for 0.5 hours to obtain biodegradable poly(butylene adipate / terephthalate) PBAT-6.
[0152] Synthesis example 7:
[0153] This synthesis example provides a polybutylene adipate / terephthalate and a preparation method thereof, as follows:
[0154] 1) adding terephthalic acid and 1,4-butanediol in a molar ratio of 1:1 to an esterification reaction kettle, and adding 1% by weight of the total raw material as a catalyst, n-butyl titanate, and reacting at a temperature of 240° C. and a pressure of 40 kPa for 2.5 hours to obtain an esterified product A1;
[0155] 2) adding adipic acid and 1,4-butanediol in a molar ratio of 1.3:1 to an esterification reaction kettle, and reacting at a temperature of 200° C. and a pressure of 40 kPa for 2.5 hours to obtain an esterified product A2;
[0156] 3) The esters A1 and A2 were continuously fed into a mixer for mixing and reacted at a temperature of 240° C. and a pressure of 4 kPa for 2.5 hours to obtain a prepolymer, which was then further polymerized at a temperature of 240° C. and a pressure of 120 Pa for 5 hours to obtain biodegradable poly(butylene adipate / terephthalate) PBAT-7.
[0157] Synthesis example 8:
[0158] This synthesis example provides a polybutylene adipate / terephthalate and a preparation method thereof, as follows:
[0159] 1) adding terephthalic acid and 1,4-butanediol in a molar ratio of 1:1 to an esterification reaction kettle, and adding 1% by weight of the total raw material as a catalyst, n-butyl titanate, and reacting at a temperature of 240° C. and a pressure of 40 kPa for 2.5 hours to obtain an esterified product A1;
[0160] 2) adding adipic acid and 1,4-butanediol in a molar ratio of 1.3:1 to an esterification reaction kettle, and reacting at a temperature of 200° C. and a pressure of 40 kPa for 2.5 hours to obtain an esterified product A2;
[0161] 3) The esters A1 and A2 were continuously fed into a mixer for mixing and reacted at a temperature of 240° C. and a pressure of 4 kPa for 2.5 hours to obtain a prepolymer, which was then further polymerized at a temperature of 240° C. and a pressure of 120 Pa for 6 hours to obtain biodegradable polybutylene adipate / terephthalate (PBAT-8).
[0162] 1. By measuring the H NMR spectrum of the above-mentioned polybutylene adipate / terephthalate ester PBAT and calculating the peak area of the corresponding peak, the mole fraction of the polybutylene terephthalate segment in each PBAT is measured. The calculation method is as follows: T% = A 8.09 / (A 8.09 +A 2.33 )
[0163] Wherein, T% represents the mole fraction of polybutylene terephthalate in PBAT;
[0164] A 8.09 represents the peak area at 8.09 in the NMR spectrum;
[0165] A 2.33 It represents the peak area at 2.33 in the NMR spectrum.
[0166] Figure 1 is the hydrogen nuclear magnetic resonance spectrum of PBAT prepared in Synthesis Example 3.
[0167] (1) The results of the mole fraction of the polybutylene terephthalate segment in the PBAT prepared in each synthesis example are shown in Table 1 below.
[0168] (2) A mixed solvent of phenol and dichlorobenzene was prepared in a weight ratio of 50:50. The intrinsic viscosity of each PBAT at 25° C. was measured according to DIN 53728, Part 3, dated January 3, 1985. The results are shown in Table 1 below.
[0169] Table 1
[0170] 3. The above PBATs are used to prepare biodegradable polylactic acid-based composite materials and nose bridge strips:
[0171] Example 1:
[0172] This embodiment provides a biodegradable polylactic acid-based composite material, a preparation method thereof, and a nose bridge strip, as follows:
[0173] (1) 45 parts of PLA-1, 40 parts of PBAT-3, 15 parts of talc-1 and 0.4 parts of lubricant were mixed uniformly according to the above-mentioned feeding ratio, and then put into a twin-screw extruder, extruded at 200°C, granulated and dried to obtain a biodegradable polylactic acid-based composite material-1.
[0174] (2) The biodegradable polylactic acid-based composite material-1 is fed into an extruder, and the temperature of different sections of the body is adjusted to 150-180° C. for processing and molding, thereby obtaining a degradable nose bridge strip.
[0175] With reference to the operating steps shown in Example 1 and according to the formulations shown in Table 2, biodegradable polylactic acid-based composite materials of Examples 2 to 12 and Comparative Examples 1 to 7 were prepared.
[0176] Table 2 Note: Blank spaces in the table indicate that the substance was not added;
[0177] 4. The biodegradable polylactic acid-based composite materials prepared in Examples 1 to 12 and Comparative Examples 1 to 7 and a nose bridge strip with a width of 3.0 mm and a thickness of 0.8 mm were subjected to performance tests. The test method is as follows:
[0178] (1) Melt flow rate was measured according to GB / T 3682.1-2018, under the conditions of 190°C and 2.16 kg.
[0179] (2) Bending performance test: Use a specified mold to fold the finished nose bridge strip with a length of 8 cm, hold it for 10 seconds and then release it. After the finished nose bridge strip has been left to stand for 1 minute, use a protractor to test its forming angle; the experimental conditions are temperature (23±2)℃ and relative humidity (50±10)%.
[0180] (3) The aging conditions are 60°C, 60% humidity, and the aging time is 72h.
[0181] The test results are shown in Table 3 below:
[0182] Table 3 Note: * indicates that the nose bridge sample has brittle fracture.
[0183] As can be seen from Table 3, the all-plastic nose bridge strip products of Examples 1 to 12 have a folded rebound angle of less than 10° and a 90° rebound angle of less than 15°; the biodegradable nose bridge strip products have a folded rebound angle of less than 15° and a 90° rebound angle of less than 20° after aging; they exhibit better bending performance than Comparative Examples 1 to 7, and are more suitable for use as plastic nose bridge strips for disposable masks.
[0184] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0185] The above-described embodiments merely represent several implementation methods of the present application. While the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent application. It should be noted that a person of ordinary skill in the art may make various modifications and improvements without departing from the spirit of the present application, and these modifications and improvements fall within the scope of protection of the present application. Therefore, the scope of protection of the present patent application shall be determined by the appended claims.
Claims
1. A biodegradable polylactic acid-based composite material, characterized in that: The composition comprises the following components in parts by weight: 15-55 parts of polylactic acid; 30-70 parts of polybutylene adipate / terephthalate; and 15-40 parts of filler; In the polylactic acid, the mass content of residual monomers is ≤0.3%; The polybutylene adipate / terephthalate has a structure shown in formula (I): p is 0.44 to 0.54, p+q=1; At 25° C., the intrinsic viscosity of the polybutylene adipate / terephthalate is 0.9 dL / g to 1.9 dL / g.
2. The biodegradable polylactic acid-based composite material according to claim 1, characterized in that: The composition comprises the following components in parts by weight: 15-45 parts of polylactic acid; 40-60 parts of polybutylene adipate / terephthalate; and 15 to 35 parts of filler.
3. The biodegradable polylactic acid-based composite material according to claim 1 or 2, characterized in that: The D50 particle size of the filler is ≤10 μm.
4. The biodegradable polylactic acid-based composite material according to any one of claims 1 to 3, characterized in that: The filler is one of talc and calcium carbonate or a mixture of the two.
5. The biodegradable polylactic acid-based composite material according to any one of claims 1 to 4, characterized in that: The biodegradable polylactic acid-based composite material further comprises 0.1 to 2 parts of lubricant in parts by weight.
6. A method for preparing the biodegradable polylactic acid-based composite material according to any one of claims 1 to 5, characterized in that: The steps include: The polylactic acid, polybutylene adipate / terephthalate and filler are blended and extruded.
7. The method for preparing the biodegradable polylactic acid-based composite material according to claim 6, characterized in that: The preparation method of polybutylene adipate / terephthalate comprises the following steps: Terephthalic acid, 1,4-butanediol and a catalyst are mixed to prepare an esterified product A1 through an esterification reaction, wherein the molar ratio of terephthalic acid to 1,4-butanediol is (1.1-2.5):1; Adipic acid and 1,4-butanediol are mixed in a molar ratio of (1 to 1.8):1, and an esterification reaction is performed to prepare an esterified product A2; The esterified product A1 and the esterified product A2 are mixed and reacted at a temperature of 200° C. to 245° C. and a pressure of 1 KPa to 10 KPa for 0.5 h to 5 h to prepare a prepolymer; The prepolymer is reacted for 1 h to 5 h at a temperature of 230° C. to 255° C. and a pressure of ≤150 Pa to obtain the polybutylene adipate / terephthalate.
8. The method for preparing the biodegradable polylactic acid-based composite material according to claim 7, characterized in that: The process parameters for preparing the esterification product A1 include: The temperature is 200℃~250℃, the pressure is 30KPa~110KPa, and the time is 1.5h~3.5h; and / or The process parameters for preparing the esterification product A2 include: The temperature is 100℃~250℃, the pressure is 30KPa~110KPa, and the time is 2h~4h.
9. A nose bridge strip, characterized in that: The invention comprises the biodegradable polylactic acid-based composite material according to any one of claims 1 to 5, or the biodegradable polylactic acid-based composite material prepared by the preparation method according to any one of claims 6 to 8.
10. A mask, characterized in that: The nose bridge strip comprising claim 9.
Citation Information
Patent Citations
Continuous production method for biodegradable aliphatic-aromatic copolyester
CN102443149A
Fully-biodegradable PLA / PBAT composite film and making method thereof
CN103589124A
Fully biodegradable material
CN111849177A
Full-biodegradable blending material